Lift method and receiving substrate

MYPI2025002386A0Undetermined Publication Date: 2024-04-21SHIN ETSU CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025002386
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-10-21
Filing Date
2023-10-10
Publication Date
2024-04-21

Smart Images

  • Figure PI2025002386_DRAWING_001
    Figure PI2025002386_DRAWING_001
  • Figure PI2025002386_DRAWING_002
    Figure PI2025002386_DRAWING_002
  • Figure PI2025002386_DRAWING_003
    Figure PI2025002386_DRAWING_003
Patent Text Reader

Abstract

The present invention is a LIFT method for transferring a microstructure formed on a supply substrate to a receiving substrate by laser lift-off. A face of the microstructure facing the receiving substrate has a recess so that an outer region of the face is higher than an inner region of the face. A face of the receiving substrate to which the microstructure is to be transferred has a resin layer. The laser lift-off is performed with the resin layer in contact with or in proximity to a bottom face of the recess of the microstructure. This can provide a LIFT method that allows for transfer of microstructures with recesses to a receiving substrate by laser lift-off without causing damages on the microstructures. Fig. 3
Need to check novelty before this filing date? Find Prior Art

Description

Lifting method and receiving substrate

[0001] The present invention relates to a laser-induced forward transfer (LIFT) method for transferring relatively fragile microstructures, such as mini light-emitting diodes (hereinafter also referred to as mini LEDs) and micro light-emitting diodes (hereinafter also referred to as micro LEDs) having uneven portions such as solder particles, from a supply substrate to a receiving substrate by laser lift-off (hereinafter also referred to as LLO) without damaging the microstructures, and to a receiving substrate that can receive the microstructures by laser lift-off without damaging them.

[0002] In recent years, with the miniaturization of semiconductor elements, microstructure transfer technology using adhesive resins has attracted attention as a means of assembling electrical and electronic products using semiconductor elements. In particular, there has been active development of technology for manufacturing LED displays for applications such as signage, TVs, medical devices, in-vehicle displays, and smartphones by transferring tens of thousands of mini-LEDs (LED elements with short sides of 100 μm to several hundred μm) or micro-LEDs (LED elements with short sides of 100 μm or less, or even 50 μm or less) at once.

[0003] We have previously developed a method for transferring microstructures such as microLEDs onto circuit boards using silicone adhesive cured materials as donor substrates or transfer stamp materials (Patent Document 1).

[0004] On the other hand, semiconductor elements generally have electrodes formed on both ends of the MESA region, resulting in a shape with minute irregularities. Figure 9 shows a schematic diagram of a supply substrate equipped with an example of a typical semiconductor element. In the supply substrate 20 shown in Figure 9, a semiconductor element 100 is bonded onto a sapphire wafer 21 with a benzocyclobutene (BCB) adhesive layer 22. A surface 100A of the semiconductor element 100 opposite the surface in contact with the BCB adhesive layer 22 has a recess 110 such that an outer region 102 of the surface 100A is higher than an inner region 101.

[0005] As a result, mini LED elements, which are larger than micro LED elements, have been known to crack during the LLO process when transferring them from a supply substrate to a receiving substrate. Red LED elements, which are made up of elements different from blue or green LED elements, are relatively brittle and prone to cracking. Therefore, similar cracking has also occurred during the LLO process.

[0006] Another known technique involves using conductive adhesives to electrically connect transferred microstructures, such as LED elements, to circuit boards. However, this connection method requires high positional accuracy when mounting the microstructures and has limitations on the miniaturization of conductive fillers, making it difficult to keep up with the ever-increasing miniaturization of semiconductor elements. Furthermore, heat generation or light emission from microstructures, such as semiconductor elements, can degrade the adhesive resin components, making it difficult to achieve long-term reliability. Against this backdrop, attention is now being paid to soldering processes. This technique uses bump-equipped semiconductor elements with solder particles (also referred to as bumps) pre-mounted on the electrodes of the element. After mounting on a circuit board, reflow is performed to melt the solder particles and implement circuit integration. Adjusting the amount of solder allows for a more agile approach to miniaturization, while the self-alignment effect, which corrects misalignment when the solder particles melt, allows for greater flexibility in mounting position accuracy. Furthermore, because the molten solder itself acts as an adhesive, degradation over time is relatively minimized.

[0007] However, since the formation of the bump results in the bump portion being raised in a convex shape, in order to transfer such an element, the resin layer of the donor substrate needs to receive the convex element surface, but there was a phenomenon in which the element was broken by the impact of the LLO.

[0008] Japanese Patent Application Laid-Open No. 2021-34610

[0009] In addition to microstructures such as blue or green LEDs that have been studied in the past, there was a need for a method for transferring microstructures that have steps such as bumps or that are fragile and easily damaged, such as red LEDs, from a supply substrate to a receiving substrate using LLO without damaging them.

[0010] The present invention has been made to solve the above problems, and aims to provide a lifting method that can transfer a microstructure having a recess to a receiving substrate by laser lift-off without damaging it, and a receiving substrate that can receive the microstructure by laser lift-off without damaging it.

[0011] In order to solve the above problems, the present invention provides a lifting method for transferring a microstructure formed on a supply substrate to a receiving substrate by laser lift-off, wherein the surface of the microstructure facing the receiving substrate has a recess such that the outer region of the surface is higher than the inner region, the surface of the receiving substrate onto which the microstructure is transferred has a resin layer, and laser lift-off is performed with the resin layer in contact with or close to the bottom surface of the recess of the microstructure.

[0012] With this type of lifting method, by performing laser lift-off with the resin layer in contact with or close to the bottom surface of the recess in the microstructure, the impact applied to the microstructure during laser lift-off is dispersed and absorbed by the resin layer, thereby mitigating the impact. This allows the microstructure to be transferred from the supply substrate to the receiving substrate without damage. Therefore, with the lifting method of the present invention, even microstructures that are easily damaged, such as red LED elements that are brittle and easily cracked, or LED elements with an uneven surface such as a bump, can be transferred by laser lift-off without damage.

[0013] The outer region of the microstructure may have an electrode or a bump.

[0014] According to the lifting method of the present invention, even a microstructure having, for example, electrodes or bumps in its outer region can be transferred without being damaged.

[0015] The inner region of the microstructure may be a MESA region.

[0016] The inner region of the minute structure is not particularly limited, but may be a MESA region.

[0017] For example, the minute structure may be one or more LED elements selected from a red LED, a blue LED, and a green LED.

[0018] The microstructure to be transferred in the present invention is not limited as long as it has a recess, but may be, for example, an LED element such as a red LED, a blue LED, or a green LED.

[0019] The resin layer may be prepared by forming it through at least one curing reaction selected from the group consisting of a radical curing reaction, a cationic curing reaction, an anionic curing reaction, an addition curing reaction, and a condensation curing reaction.

[0020] The resin layer can be formed by, for example, at least one curing reaction selected from the group consisting of a radical curing reaction, a cationic curing reaction, an anionic curing reaction, an addition curing reaction, and a condensation curing reaction.

[0021] For example, the supply substrate and the receiving substrate can be bonded together and pressure can be applied to deform the resin layer so that the resin layer is in contact with or close to the bottom surface of the recess of the minute structure.

[0022] For example, by applying pressure, the resin layer can be brought into contact with or close to the bottom surface of the recess of the minute structure.

[0023] It is preferable to use a resin layer having flexibility or fluidity as the resin layer.

[0024] By using such a resin layer, it is possible to easily bring the resin layer into contact with or close to the bottom surface of the recess of the minute structure.

[0025] In this case, it is more preferable to use a resin layer having a storage modulus at 25° C. of 1 to 300 kPa as the resin layer.

[0026] If such a resin layer is used, it can be more easily brought into contact with or close to the bottom surface of the recess of the minute structure.

[0027] The present invention also provides a receiving substrate for transferring and receiving a microstructure formed on a supply substrate by laser lift-off, the receiving substrate having a resin layer on the surface onto which the microstructure is transferred, the surface of the microstructure facing the receiving substrate having a recess so that the outer region of the surface is higher than the inner region, and the resin layer is deformed by bonding the supply substrate and the receiving substrate together and applying pressure.

[0028] In such a receiving substrate, the resin layer is deformed by bonding the supply substrate and the receiving substrate together and applying pressure, so that the impact applied to the microstructure during laser lift-off is dispersed and absorbed by the resin layer, thereby mitigating the impact. As a result, the microstructure can be received from the supply substrate without being damaged. Therefore, with the receiving substrate of the present invention, even if the microstructure is a fragile red LED element that is easily broken, or an LED element with an uneven surface such as a bump, it can be transferred and received by laser lift-off without being damaged.

[0029] The resin layer is preferably deformed to an extent sufficient to bring it into contact with or close to the bottom surface of the recess of the minute structure.

[0030] If the receiving substrate has such a resin layer, damage to the minute structure can be prevented more reliably.

[0031] In this case, the resin layer is more preferably a resin layer having a storage modulus at 25°C of 1 to 300 kPa.

[0032] If the receiving substrate has such a resin layer, damage to the minute structure can be prevented more reliably.

[0033] As described above, the lift-off method of the present invention allows microstructures with recesses to be transferred to a receiving substrate by laser lift-off without damaging them. This method is particularly applicable to the manufacturing process of LED displays for use in signage, TVs, medical devices, in-vehicle displays, smartphones, etc.

[0034] Furthermore, the receiving substrate of the present invention can receive a microstructure having a recess by transferring it using laser lift-off without damaging it.

[0035] FIG. 1 is a schematic diagram showing an example of a receiving substrate of the present invention; FIG. 2 is a schematic diagram showing another side of an example of a receiving substrate of the present invention; FIG. 3 is a schematic diagram showing an example of a lifting method of the present invention; FIG. 4 is a schematic diagram showing an example of a supply substrate that can be used in the lifting method of the present invention; FIG. 5 is a schematic diagram showing another example of a supply substrate that can be used in the lifting method of the present invention; FIG. 6 is a schematic diagram showing one step of an embodiment of the lifting method of the present invention; FIG. 7 is a schematic diagram showing another step of an embodiment of the lifting method of the present invention; FIG. 8 is a schematic diagram showing a lifting method of a comparative example; FIG. 9 is a schematic diagram showing a supply substrate provided with an example of a general semiconductor element.

[0036] As described above, there was a need to develop a lifting method that can transfer a microstructure having a recess to a receiving substrate by laser lift-off without damaging it, and a receiving substrate that can receive the microstructure by laser lift-off without damaging it.

[0037] After extensive research into the above-mentioned problems, the inventors discovered that by providing a resin layer on the surface of the receiving substrate onto which the microstructure is to be transferred, and performing laser lift-off with the resin layer in contact with or close to the bottom surface of the recess in the microstructure, it is possible to transfer the microstructure having a recess onto the receiving substrate without damaging it, and thus completed the present invention.

[0038] In other words, the present invention is a lifting method for transferring a microstructure formed on a supply substrate to a receiving substrate by laser lift-off, wherein the surface of the microstructure facing the receiving substrate has a recess such that the outer region of the surface is higher than the inner region, the surface of the receiving substrate onto which the microstructure is transferred has a resin layer, and laser lift-off is performed with the resin layer in contact with or close to the bottom surface of the recess of the microstructure.

[0039] The present invention also provides a receiving substrate for transferring and receiving a microstructure formed on a supply substrate by laser lift-off, the receiving substrate having a resin layer on the surface onto which the microstructure is transferred, the surface of the microstructure facing the receiving substrate having a recess so that the outer region of the surface is higher than the inner region, and the resin layer is deformed by bonding the substrate and the receiving substrate together and applying pressure.

[0040] The present invention will be described in detail below, but the present invention is not limited thereto.

[0041] [Receiving Substrate] An example of the receiving substrate of the present invention is schematically shown in Fig. 1. However, the receiving substrate of the present invention is not limited to the example shown in Fig. 1.

[0042] 1 includes a resin layer 12 on a support substrate 11. A surface 10A of the receiving substrate 10 on which the resin layer 12 is provided is a surface onto which a microstructure, which will be described below, is transferred.

[0043] As shown in FIG. 2, the resin layer 12 is deformed by bonding the supply substrate 20 and the receiving substrate 10 together and applying pressure.

[0044] 2 is the same as the supply substrate 20 described with reference to Fig. 9. Specifically, the supply substrate 20 includes a support substrate 21 and a microstructure 100 supported by the support substrate 21. A surface 100A of the microstructure 100 opposite to the surface facing the support substrate 21 has a recess 110 such that an outer region 102 of the surface 100A is higher than an inner region 101. The configuration of the supply substrate 20 will be described later.

[0045] With such a receiving substrate 10, the resin layer 12 is deformed by bonding the supply substrate 20 and the receiving substrate 10 together and applying pressure, so that the impact applied to the microstructure 100 during laser lift-off is dispersed and absorbed by the resin layer 12, thereby mitigating the impact. As a result, the microstructure 100 can be received from the supply substrate 20 without being damaged. Therefore, with the receiving substrate 10 of the present invention, even if the microstructure 100 is a fragile red LED element that is easily broken, or an LED element with an uneven surface such as a bump, it can be received by transfer using laser lift-off without being damaged.

[0046] The resin layer 12 of the receiving substrate 10 is preferably deformed to an extent sufficient to come into contact with or be close to the bottom surface 110A of the recess 110 of the minute structure 100, as shown in FIG. 2(B), for example.

[0047] If the receiving substrate 10 has such a resin layer 12, damage to the minute structure 100 can be prevented more reliably.

[0048] The receiving substrate 10 can be formed, for example, by applying a precursor of the resin layer 12 (for example, a silicone-based gel composition) onto the supporting substrate 11 and curing it.

[0049] Examples of the support substrate 11 used for the receiving substrate 10 include a synthetic quartz glass substrate, float glass, etc., and from the standpoint of flatness and transferring a microstructure 100 having uneven portions (depressions 110) such as bumps, a synthetic quartz glass substrate is preferred, as transparency is required for the support substrate 11 in order to confirm whether the resin layer 12 is in contact with or close to the bottom 110A of the depression 110 after the bonding process described below.

[0050] Furthermore, the size of the support substrate 11 used for the receiving substrate 10 is preferably the same as or larger than the diameter of the supply substrate 20. Specifically, when a sapphire substrate with an outer diameter of 10.16 cm (4 inches) is used as the supply substrate 20, a receiving substrate 10 with an outer diameter of 10.16 to 20.32 cm (4 to 8 inches) can be used.

[0051] In order to reliably transfer some or all of the multiple microstructures 100 from the supply substrate 20 to the receiving substrate 10, it is preferable that when the multiple microstructures 100 formed on one side of the supply substrate 20 are bonded to the receiving substrate 10 having a resin layer 12 on a support substrate 11, each microstructure 100 is temporarily and uniformly fixed to the resin layer 12 of the receiving substrate 10.

[0052] In order to temporarily fix the microstructure 100 with high precision, the support substrate 11 used for the receiving substrate 10 has a spatial frequency of 1 mm obtained by measuring an area of ​​6.01 mm x 6.01 mm with a pixel number of 1240 x 1240 using a white light interferometer. -1 The power spectral density above is 10 12 nm 4 It is preferable that the spatial frequency is 10 mm or less, and in particular, when the minute structure 100 is a micro LED, taking into consideration the distance between the minute structures 100, the spatial frequency is 10 mm or less, which is obtained by measuring an area of ​​6.01 mm x 6.01 mm with a white light interferometer at a pixel count of 1240 x 1240. -1 More than 50 mm -1 The power spectral density at 9 nm 4 It is preferable that:

[0053] Furthermore, since the receiving substrate 10 temporarily fixes the microstructure 100 with high precision, it is preferable that the support substrate 11 used for the receiving substrate 10 has a small thickness variation. For example, the thickness variation (TTV) measured with a wavelength conversion Fizeau flatness tester manufactured by Mizojiri Optical Industries Co., Ltd. is preferably 2 μm or less, more preferably 1 μm or less, and even more preferably 0.5 μm or less.

[0054] The resin layer 12 is preferably flexible or fluid, and more preferably has a storage modulus of 1 to 300 kPa at 25° C. Such a resin layer 12 may be, for example, a silicone-based gel layer, but is not limited to this.

[0055] The silicone gel layer is provided, for example, by curing a silicone gel composition, and the curing mode is preferably at least one selected from addition curing reactions, radical curing reactions such as photoradical polymerization reactions and thermal radical polymerization reactions, cationic curing reactions, anionic curing reactions, and condensation curing reactions, and among these, addition curing reactions, photoradical polymerization reactions, and thermal radical polymerization reactions are preferred in terms of ease of resin design or ease of curing. The silicone gel layer may be, for example, a curable resin layer that can be further cured, and in this case, the silicone gel composition may be a two-stage curing type silicone gel composition.

[0056] The silicone gel composition can be coated onto the support substrate 11, for example, by spin coating the silicone gel composition onto the support substrate 11 to a thickness of preferably 1 to 500 μm, more preferably 5 to 200 μm, and even more preferably 10 to 10 μm. The thickness may be determined arbitrarily, taking into consideration the shape and thickness of the microstructure 100 to be transferred. In this case, the entire surface of the support substrate 11 may be coated, or, for reasons such as ensuring ease of handling, excess silicone gel composition may be washed away using edge rinsing, leaving part of the outer periphery of the support substrate 11 exposed. Alternatively, the composition may be applied to any thickness and shape using slit coating, screen printing, or the like.

[0057] In order to improve the adhesion or bonding strength at the interface between the support substrate 11 and the resin layer 12, the support substrate 11 may be pre-treated with a primer.

[0058] After the coating step, for example, when curing by an addition curing reaction, the composition is placed in a heating furnace in an environment of preferably 20 to 200°C for 5 to 90 minutes, or when curing by a photoradical polymerization reaction, the composition is preferably placed in a nitrogen environment with 365 nm light as an index, at an intensity of 50 to 3000 mW / cm. 2 and 100 to 20,000 mJ / cm 2 The resin layer 12 can be formed under curing conditions suitable for the silicone composition used, such as by irradiating the composition with ultraviolet light at an integrated light amount of 1000 kJ / cm 2 or more.

[0059] [Lifting Method] Next, the lifting method of the present invention will be described with reference to Fig. 3 and again with reference to Fig. 1 and Fig. 2. However, the present invention is not limited to the embodiment shown in the drawings.

[0060] FIG. 3 shows a schematic diagram of an example of the lifting method of the present invention.

[0061] The lifting method of the present invention is a lifting method in which a microstructure 100 formed on a supply substrate 20 is transferred to a receiving substrate 10 by laser lift-off.

[0062] 2, the surface 100A of the microstructure 100 formed on the supply substrate 20, which faces the receiving substrate 10, has a recess 110 such that the outer region 102 of the surface 100A is higher than the inner region 101. Also, as in FIG. 1, the surface 10A of the receiving substrate 10 onto which the microstructure is transferred has a resin layer 12.

[0063] 3, in the lift-off method of the present invention, laser lift-off is performed by irradiating a laser L onto the back surface of the support substrate 21 of the supply substrate 20 with the resin layer 12 in contact with or in proximity to the bottom surface 110A of the recess 110 of the microstructure 100. Details of the laser lift-off will be described later.

[0064] The state in which the resin layer 12 is in contact with the bottom surface 110A of the recess 110 of the microstructure 100 is not limited to the state in which the entire bottom surface 110A is in contact with the resin layer 12, but may also be the state in which only a portion of the bottom surface 110A is in contact with the resin layer 12, as shown in Fig. 3. When the resin layer 12 is in contact with the bottom surface 110A of the recess 110 of the microstructure 100, the distance (shortest distance) between the bottom surface 110A of the recess 110 of the microstructure 100 and the resin layer 12 is 0 µm.

[0065] The state in which the resin layer 12 is close to the bottom surface 110A of the recess 110 of the microstructure 100 means that a minute gap exists between the bottom surface 110A and the resin layer 12 that can absorb the impact applied to the microstructure 100 during laser lift-off. Specifically, the close state can be, for example, a state in which the gap between the bottom surface 110A and the resin layer 12 is greater than 0 μm and not greater than 1 μm, and preferably greater than 0 μm and not greater than 0.5 μm. In another aspect, when the depth of the recess 110 of the microstructure 100 is defined as "1," the gap between the bottom surface 110A and the resin layer 12 can be said to be greater than "0" and not greater than "0.1," and preferably greater than "0" and not greater than "0.05."

[0066] The state in which resin layer 12 is in contact with or close to bottom surface 110A of recess 110 of microstructure 100 can also be referred to as a "state of approximate contact." The state of approximate contact can be referred to as a state in which the distance between bottom surface 110A and resin layer 12 is 0 μm or more and 1 μm or less, and in another aspect, can be referred to as a state in which, when the depth of recess 110 of microstructure 100 is "1," the distance between bottom surface 110A and resin layer 12 is "0" or more and "0.1" or less.

[0067] With this type of lifting method, laser lift-off is performed with the resin layer 12 in contact with or close to the bottom surface 110A of the recess 110 of the microstructure 100, and the impact applied to the microstructure 100 during laser lift-off is dispersed and absorbed by the resin layer 12, thereby mitigating the impact. This allows the microstructure 100 to be transferred from the supply substrate 20 to the receiving substrate 10 without being damaged. Therefore, with the lifting method of the present invention, even if the microstructure 100 is a fragile red LED element that is prone to cracking, or an LED element having an uneven surface such as a bump, it is possible to transfer the microstructure 100 by laser lift-off without damaging it.

[0068] The receiving substrate and the supply substrate used in the lifting method of the present invention will be described below.

[0069] [Receiving Substrate] As the receiving substrate 10, for example, the receiving substrate 10 of the present invention described above can be used.

[0070] In preparing the receiving substrate 10, the resin layer 12 can be prepared by forming it through at least one curing reaction selected from the group consisting of, for example, a radical curing reaction, a cationic curing reaction, an anionic curing reaction, an addition curing reaction, and a condensation curing reaction.

[0071] The resin layer 12 is preferably flexible or fluid, and more preferably has a storage modulus of elasticity at 25° C. of 1 to 300 kPa.

[0072] For further details about the receiving substrate 10, please refer to the previous description of the receiving substrate 10 of the present invention.

[0073] [Supply Substrate and Microstructure] The supply substrate 20 used in the lifting method of the present invention has a microstructure 100 formed thereon, as described with reference to Fig. 2. The surface 100A of the microstructure 100 facing the receiving substrate 10 has a recess 110 such that an outer region 102 of the surface 100A is higher than an inner region 101.

[0074] For example, as shown in Fig. 4, the supply substrate 20 may be one in which a plurality of microstructures 100 are formed on one surface of a support substrate 21, and the microstructures 100 have electrodes 130 formed on an element body 120. The region corresponding to the electrodes 130 is an outer region 102, which is higher than the inner region 101. As a result, recesses 110 are formed between the electrodes 130.

[0075] When a bump is mounted, a bump 140 is further formed on the electrode 130 as shown in FIG.

[0076] The inner region 101 of the minute structure 100 may be a MESA region.

[0077] The support substrate 21 used in the supply substrate 20 may be, for example, a sapphire substrate, a GaAs substrate (gallium arsenide substrate), a Si substrate, or a SiC substrate, and may have any diameter.

[0078] Furthermore, examples of the microstructure 100 include elements obtained by providing the basic structure of a device on a supply substrate 20 through processes carried out in typical semiconductor pre-processing steps such as epitaxial growth, ion implantation, wet etching, dry etching, vapor deposition, and electrode formation, and then separating the element by conventional methods such as blade dicing, dry etching, and laser dicing to a depth required to separate the element.

[0079] For example, if the microstructure 100 is an LED element, the supply substrate 20 can be prepared by the following procedure. A buffer layer is formed on a 4-inch sapphire substrate serving as the support substrate 21. A 3 μm thick N-type GaN layer is then formed on the 4-inch sapphire substrate. This is followed by a known light-emitting layer structure and P-type GaN, resulting in an LED epitaxial substrate with a total epitaxial thickness of 4 μm. After that, the N-type layer is locally exposed by dry etching, and a P-type electrode is formed on the P-type layer by a known process. The N-type electrode is then formed in contact with the exposed N-type layer, and a bump is formed on the electrode by plating, vapor deposition, sputtering, or another method. Then, to separate LED elements of a predetermined size, laser dicing is performed until it reaches at least the sapphire substrate and the elements are completely separated. This results in a supply substrate 20 on which LED elements are formed as the microstructure 100.

[0080] The size of the microstructure 100 used in the present invention is arbitrary, but for example, in the case of a power LED, it is about 1 mm square. In addition, in the case of an LED element, it is about 300 μm square, in the case of a mini LED, it is about 100 μm square, in the case of a micro LED, it is about 60 μm square or less, and in the case of an extremely small micro LED, it is 30 μm square or less.

[0081] Although the shape of the microstructure 100 described above is an example of a substantially square, the present invention is not limited to this. For example, in the case of a micro LED, the shape may be a rectangle with one side measuring 30 to 60 μm and the other side measuring 10 to 30 μm.

[0082] The thickness of the main body of the microstructure 100 depends on the thickness of epitaxial growth of the supply substrate 20 on the support substrate 21, and is not particularly limited, but is preferably about 3 to 10 μm. The thickness of the electrodes is not particularly limited, but is preferably 2 μm or less, and the thickness of the bump is not particularly limited, but is preferably about 1 to 10 μm.

[0083] [Embodiment] Next, one embodiment of the lifting method of the present invention will be described with reference to Figures 6 and 7. However, the present invention is not limited to the embodiment described below.

[0084] The lifting method of the embodiment described here includes a bonding step, a transfer step by laser lift-off, and a peeling step.

[0085] [Bonding Process] The bonding of the plurality of microstructures 100 formed on one surface of the supply substrate 20 to the resin layer 12 of the receiving substrate 10 can be carried out, for example, as shown in Fig. 6. Specifically, the bonding is as follows. In the embodiment described below, a silicone-based gel layer is used as the resin layer 12 of the receiving substrate 10, and the supply substrate 20 has the microstructures 100 shown in Fig. 4 formed thereon.

[0086] First, as shown in FIG. 6A, the supply substrate 20 and the receiving substrate 10 are aligned. Next, the silicone-based gel layer 12 of the receiving substrate 10 is bonded to the electrodes 130 and element body 120 of the microstructure 100. Next, as shown in FIG. 6B, the receiving substrate 10 is pressed against the supply substrate 20, thereby deforming the silicone-based gel layer 12 and bringing the silicone gel layer 12 into contact with or close to the bottom surface 110A of the recess 110 of the microstructure 100, as shown in FIG. 2B. In FIG. 6B, the gel of the silicone-based gel layer 12 covers the microstructure 100. When using the supply substrate 20 on which the microstructure 100 with bumps 140 shown in FIG. 5 is formed, bonding is performed using a similar process.

[0087] The pressure load during lamination is not particularly limited as long as the plurality of microstructures 100 can be transferred onto the silicone-based gel layer 12, but it is preferable to perform lamination by applying a load of, for example, preferably 0.05 to 1.0 MPa, more preferably 0.10 to 0.5 MPa. At this time, in order to make it easier to follow the shape of the microstructure 100, vacuum decompression or heat may be applied simultaneously with the mechanical pressurization.

[0088] By this lamination process including the application of pressure, a laminated substrate 30 including the supply substrate 20 and the receiving substrate 10 laminated to the supply substrate 20 is obtained as shown in FIG. 6(B).

[0089] After the lamination step, the silicone-based gel layer 12 conforms to and deforms to the uneven shape caused by the presence of the electrodes 130 and bumps 140 on the microstructure 100, so that it is in approximate contact with the bottom surface 110A of the recess 110 of the microstructure 100, and it is also possible to confirm through the substrate using a laser microscope or the like that there is no gap of more than 1 μm between the silicone-based gel layer 12 and the microstructure 100. Because a cured gel is generally soft and adhesive, if the silicone-based gel layer 12 is in contact with or in close proximity to the bottom surface 110A of the recess 110 of the microstructure 100 after the lamination step, that state can be maintained in the LLO step described below, and as a result, damage to the microstructure 100 can be prevented.

[0090] [Transfer Process by Laser Lift-Off and Peeling-Off Process] The transfer process by LLO (Laser Lift-Off) is shown in FIG.

[0091] As shown in Fig. 7(A), the laminated substrate 30 obtained in the bonding step is irradiated with pulsed laser light L from the surface of the supply substrate 20 opposite to the surface on which the microstructure 100 is formed, thereby peeling off the microstructure 100 from the support substrate 21. After similar laser irradiation is performed on all of the microstructures 100 to be transferred, a jig is used to peel off the support substrate 11 of the receiving substrate 10 and the support substrate 21 of the supply substrate 20, resulting in the state shown in Fig. 7(B), whereby the microstructure 100 can be transferred to the silicone-based gel layer 12 on the receiving substrate 10.

[0092] In the LLO process, for example, when lifting off a gallium nitride microstructure 100 fixed to a support substrate 21 such as a sapphire substrate, the gallium nitride in the irradiated portion is melted by irradiation with laser light from an excimer laser, a YAG laser, or the like, and the gallium nitride microstructure 100 can be peeled off from the supply substrate 20. In this case, KrF excimer laser light is preferred, particularly for microLEDs, from the viewpoint of the reliability of the microstructure 100.

[0093] Specifically, laser light is selectively irradiated to cause laser ablation at the interface between the microstructure 100 to be selected and the support substrate 21 of the supply substrate 20. As a result, in the case of a gallium nitride microstructure 100, for example, gallium nitride decomposes into metallic gallium and nitrogen between the microstructure 100 to be selected and the support substrate 21 of the supply substrate 20, generating gas, and the microstructure 100 can be peeled off relatively easily.

[0094] On the other hand, since gel materials are generally soft and have a high degree of tackiness, they can easily adsorb and receive the microstructure 100 after it has been peeled off from the supply substrate 20, thereby allowing the microstructure 100 to be transferred.

[0095] This transfer method can also be used for microstructures 100 that are easily damaged, such as red LED elements that are brittle and easily cracked, or LED elements with uneven surfaces such as bumps.By applying pressure to and bonding the silicone-based gel layer 12 on the receiving substrate 10, the gel deforms to conform to the shape of the microstructure 100, and the silicone-based gel layer 12 comes into contact with or close to the bottom surface 110A of the recess 110 in the microstructure 100.By performing LLO in this state, the silicone-based gel disperses and absorbs the impact applied to the microstructure 100 during LLO, so the microstructure 100 can be transferred onto the receiving substrate 10 without being damaged.

[0096] The microstructure 100 transferred onto the receiving substrate 10 through this process can then be surface cleaned, for example with an acidic or alkaline cleaning solution or plasma treatment, and then mounted onto a circuit board through the desired process, such as using the transfer stamp material described in Patent Document 1 or transferring the microstructure again onto a polyimide layer.

[0097] That is, the receiving substrate 10 that has received the minute structures 100 transferred by the lifting method of the present invention can also be used as a supply substrate (donor substrate) in another process.

[0098] EXAMPLES The present invention will be specifically explained below using examples and comparative examples, but the present invention is not limited to these.

[0099] Supply substrates equipped with the following microstructures were prepared: <Supply substrate A and microstructure A> A sapphire substrate cut into 1.5 cm squares and equipped with blue mini LED elements measuring 90 × 140 μm and a total thickness of 19 μm, with a bump height of 7 μm <Supply substrate B and microstructure B> A sapphire substrate cut into 1.5 cm squares and equipped with blue mini LED elements measuring 90 × 140 μm and a total thickness of 12 μm <Supply substrate C and microstructure C> A sapphire substrate cut into 1.5 cm squares and equipped with red micro LED elements measuring 18 × 36 μm and a total thickness of 5 μm

[0100] The following was prepared as a support substrate for the receiving substrate: <Support substrate used for receiving substrate> A synthetic quartz substrate having an outer diameter of 15.24 cm (6 inches), a thickness of 1 mm, and a total thickness variation (TTV) of 0.8 μm.

[0101] Examples 1 to 5 Preparation of Receiving Substrates Three grams of the following heat-curable or photo-curable silicone gel composition was dropped onto a supporting substrate and uniformly coated onto the supporting substrate using a spin coater to a film thickness of 30 μm. The silicone-coated supporting substrate was cured into a gel under the curing conditions described below to prepare a receiving substrate having a silicone gel layer as a resin layer.

[0102] [Lamination] The supply substrate and the receiving substrate were bonded together under pressure of 0.5 MPa so that the microstructures on the supply substrate and the silicone gel on the receiving substrate, respectively, shown in Table 1 below, were in contact with each other. After that, it was confirmed using a laser microscope that there was no gap larger than 1 μm between the bottom surface of the recess of the microstructure and the silicone gel layer.

[0103] [LLO] LLO was performed by irradiating the microstructure with KrF excimer laser light from the backside of the supply substrate. The supply substrate was then peeled off from the receiving substrate, and the transfer rate and damage rate of the microstructure from the supply substrate to the receiving substrate were evaluated. The results are summarized in Table 1.

[0104] [Measurement of Elastic Modulus] The dynamic viscoelastic properties of the silicone gel cured product of the present invention are defined by a characteristic frequency and a storage modulus G' at a specific temperature, and measurements were performed using an ARES G-II viscoelasticity measuring device manufactured by TA Instruments. A silicone resin cured and molded to a size of 3 cm square and 500 μm thick was sandwiched between the circular measuring part of the testing device and a parallel plate with a diameter of 20 mm, taking care not to trap air bubbles, and was measured for 10 minutes at a strain value of 4% and a frequency of 1 Hz while maintaining a temperature of 25°C. The value 10 minutes after the start of measurement was read as the storage modulus G'.

[0105] [Silicone gel compositions and curing conditions] Silicone 1: A silicone gel composition that is heat-cured at 120°C for 1 hour and has a storage modulus of 0.2 kPa at 25°C Silicone 2: 365 nm UV-LED 3000 mJ / cm under nitrogen 2 (Illuminance: 100mW / cm 2 Silicone gel composition that undergoes photoradical curing by irradiation with UV-LED 3000 mJ / cm at 365 nm under nitrogen and has a storage modulus of 0.2 kPa at 25°C. 2 (Illuminance: 100mW / cm 2 ) and undergoes photoradical curing, and has a storage modulus of 5.3 kPa at 25°C.

[0106] <Comparative Examples 1 to 4> In Comparative Examples 1 to 4, transfer was performed in the same manner as in the Examples, except that the silicone gel composition used in the receiving substrate was changed to Silicone 4 or 5 below, and the supply substrate shown in Table 1 below was used.

[0107] Silicone 4: A silicone rubber composition that is heat-cured at 120°C for 1 hour and has a storage modulus of 500 kPa at 25°C. Silicone 5: A silicone rubber composition that is heat-cured at 120°C for 1 hour and has a storage modulus of 3 MPa at 25°C.

[0108] In the comparative example, as shown in FIG. 8, LLO was performed in a state where the silicone was not deformed and was not in contact with or close to the surface of the recess of the minute structure.

[0109]

[0110] As is clear from the results shown in Table 1, in Examples 1 to 5, laser lift-off was performed with the silicone gel layer in contact with or close to the bottom surface of the recess of the microstructure, so that even when the transfer rate exceeded 99%, damage during transfer by laser lift-off could be kept to less than 1%.

[0111] On the other hand, in Comparative Examples 1 to 4, laser lift-off was performed when the silicone gel layer was not in contact with or close to the bottom surface of the recess of the microstructure, and therefore, damage during transfer by laser lift-off was 5% or more.

[0112] This specification includes the following aspects. [1] A lifting method for transferring a microstructure formed on a supply substrate to a receiving substrate by laser lift-off, wherein the surface of the microstructure facing the receiving substrate has a recess such that the outer region of the surface is higher than the inner region, and the surface of the receiving substrate onto which the microstructure is transferred has a resin layer, and the laser lift-off is performed with the resin layer in contact with or in close proximity to the bottom of the recess of the microstructure. [2] The lifting method according to [1], wherein the outer region of the microstructure has an electrode or a bump. [3] The lifting method according to [1] or [2], wherein the inner region is a MESA region. [4] The lifting method according to any one of [1] to [3], wherein the microstructure is an LED element selected from one or more of a red LED, a blue LED, and a green LED. [5] The lifting method according to any one of [1] to [4], wherein the resin layer is prepared by forming it through at least one curing reaction selected from the group consisting of a radical curing reaction, a cationic curing reaction, an anionic curing reaction, an addition curing reaction, and a condensation curing reaction. [6] The lifting method according to any one of [1] to [5], wherein the supply substrate and the receiving substrate are bonded together and pressurized to deform the resin layer so that the resin layer is in contact with or close to the bottom surface of the recess of the microstructure. [7] The lifting method according to any one of [1] to [6], wherein the resin layer is a flexible or fluid resin layer. [8] The lifting method according to any one of [1] to [7], wherein the resin layer is a resin layer having a storage modulus of 1 to 300 kPa at 25°C. [9] A receiving substrate for transferring and receiving a microstructure formed on a supply substrate by laser lift-off, the receiving substrate having a resin layer on the surface onto which the microstructure is transferred, the surface of the microstructure facing the receiving substrate having a recess so that the outer region of the surface is higher than the inner region, the resin layer deforms when the supply substrate and the receiving substrate are bonded together and pressure is applied.

[10] The receiving substrate described in [9], wherein the amount of deformation of the resin layer is sufficient to bring the resin layer into contact with or close to the bottom surface of the recess of the microstructure.

[11] The receiving substrate according to [9] or

[10] , wherein the resin layer has a storage modulus of 1 to 300 kPa at 25°C.

[0113] The present invention is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and that exhibits similar effects is included within the technical scope of the present invention.

Claims

1. A lifting method for transferring a microstructure formed on a supply substrate to a receiving substrate by laser lift-off, wherein the surface of the microstructure facing the receiving substrate has a recess such that the outer region of the surface is higher than the inner region, the surface of the receiving substrate onto which the microstructure is transferred has a resin layer, and laser lift-off is performed with the resin layer in contact with or close to the bottom surface of the recess of the microstructure.

2. The lifting method according to claim 1, wherein the outer region of the microstructure has an electrode or a bump.

3. The lifting method according to claim 2, wherein the inner region is a MESA region.

4. The lifting method according to claim 1, wherein the minute structure is an LED element selected from one or more of a red LED, a blue LED, and a green LED.

5. The lifting method of claim 1, wherein the resin layer is prepared by forming it through at least one curing reaction selected from the group consisting of a radical curing reaction, a cationic curing reaction, an anionic curing reaction, an addition curing reaction, and a condensation curing reaction.

6. A lifting method according to any one of claims 1 to 5, wherein the supply substrate and the receiving substrate are bonded together and pressurized to deform the resin layer so that the resin layer is in contact with or in close proximity to the bottom surface of the recess of the microstructure.

7. A lifting method according to any one of claims 1 to 5, wherein a flexible or fluid resin layer is used as the resin layer.

8. The lifting method according to claim 7, wherein the resin layer has a storage modulus of 1 to 300 kPa at 25°C.

9. A receiving substrate for transferring and receiving a microstructure formed on a supply substrate by laser lift-off, the receiving substrate having a resin layer on the surface onto which the microstructure is transferred, the surface of the microstructure facing the receiving substrate having a recess so that the outer region of the surface is higher than the inner region, and the resin layer is deformed by bonding the supply substrate and the receiving substrate together and applying pressure.

10. The receiving substrate according to claim 9, wherein the amount of deformation of the resin layer is sufficient to bring the resin layer into contact with or close to the bottom surface of the recess of the microstructure.

11. The receiving substrate according to claim 9 or 10, wherein the resin layer has a storage modulus of 1 to 300 kPa at 25°C.