Copper foil capable of preventing tear or wrinkle defects, electrode comprising same, secondary battery comprising same, and manufacturing method therefor
Patent Information
- Application Number
- MYPI2025002417
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-10-05
- Filing Date
- 2023-11-20
- Publication Date
- 2024-05-24
AI Technical Summary
The challenge is to prevent tearing or wrinkling defects in copper foil during manufacturing, which affects the performance and capacity of secondary batteries, particularly lithium secondary batteries, due to the curling of thin copper foil during winding, leading to reduced workability and increased defect rates.
A copper foil with specific properties is developed, including an R value between 2.0 and 3.5, a room temperature loss coefficient of 0.05 or less, and a high-temperature loss coefficient of 0.2 or less, achieved through a manufacturing process involving a copper film with a protective layer and precise control of electrolyte solution composition, including copper ions, sulfuric acid, chlorine, lead, tungsten, and organic additives, to prevent curling, wrinkling, and tearing.
The solution effectively prevents curling, wrinkling, and tearing of copper foil, enhancing the productivity and quality of secondary batteries by maintaining elastic energy storage and improving handling during high-temperature processes, thus reducing defect rates and maintaining charging and discharging efficiency.
Smart Images

Figure PI2025002417_DRAWING_001 
Figure PI2025002417_DRAWING_002
Abstract
Description
Copper foil capable of preventing tearing or wrinkle defects, electrode including the same, secondary battery including the same, and method for manufacturing the same
[0001] The present invention relates to a copper foil capable of preventing tearing or wrinkle defects, an electrode including the same, a secondary battery including the same, and a method for manufacturing the same.
[0002] Secondary batteries are a type of energy conversion device that converts electrical energy into chemical energy, stores it, and then generates electricity by converting the chemical energy back into electrical energy when needed. They are used as an energy source for portable appliances such as cell phones and laptops, as well as electric vehicles. Secondary batteries are also referred to as rechargeable batteries because they can be recharged.
[0003] Secondary batteries that have economic and environmental advantages over disposable primary batteries include lead-acid batteries, nickel-cadmium secondary batteries, nickel-hydrogen secondary batteries, and lithium secondary batteries.
[0004] In particular, lithium secondary batteries can store a relatively large amount of energy relative to their size and weight compared to other secondary batteries. Therefore, lithium secondary batteries are preferred in the information and communication device sector, where portability and mobility are crucial. Their application is also expanding to include energy storage devices for hybrid and electric vehicles.
[0005] Lithium secondary batteries are used repeatedly, with charging and discharging forming a single cycle. When operating a device with a fully charged lithium secondary battery, the lithium-ion secondary battery must possess high charge / discharge capacity to extend the device's operating time. Therefore, research is continually needed to meet consumers' ever-increasing expectations for the charge / discharge capacity of lithium secondary batteries.
[0006] These secondary batteries include anode current collectors made of copper foil. Among these copper foils, electrolytic copper foil is widely used as the anode current collector of secondary batteries. With the increasing acceptance of secondary batteries and the growing demand for high-capacity, high-efficiency, and high-quality secondary batteries, there is a growing demand for electrolytic copper foils that can enhance the characteristics of secondary batteries. In particular, there is a need for electrolytic copper foils that can ensure high capacity, stable capacity maintenance, and performance of secondary batteries.
[0007] Meanwhile, as the thickness of the copper foil becomes thinner, the amount of active material that can be contained in the same space increases, and the number of current collectors can increase, which can increase the capacity of the secondary battery. However, as the copper foil becomes thinner, curling occurs, and defects such as tearing or wrinkles in the copper foil due to edge curling during winding of the copper foil occur, making it difficult to manufacture copper foil in the form of a very thin film. Therefore, in order to manufacture copper foil with a very thin thickness, curling of the copper foil must be prevented.
[0008] Accordingly, the present invention relates to a copper foil, an electrode including the copper foil, a secondary battery including the copper foil, and a method for manufacturing the copper foil, which can prevent problems caused by the limitations and disadvantages of the above-mentioned related technologies.
[0009] One embodiment of the present invention provides a copper foil having an R value in the range of 2.0 to 3.5, thereby preventing curling, wrinkling or tearing during the manufacturing process.
[0010] One embodiment of the present invention is to provide a copper foil that does not curl, wrinkle, or tear during the manufacturing process by having a room temperature loss factor of 0.05 or less.
[0011] Another embodiment of the present invention is to provide a copper foil that does not curl, wrinkle, or tear during a high-temperature manufacturing process by having a high-temperature loss factor of 0.2 or less.
[0012] Another embodiment of the present invention provides an electrode for a secondary battery including such a copper foil, and a secondary battery including such a secondary battery electrode.
[0013] Another embodiment of the present invention is to provide a method for manufacturing a copper foil that prevents occurrence of drying, wrinkling or tearing.
[0014] In addition to the aspects of the present invention mentioned above, other features and advantages of the present invention will be described below or will be clearly understood by those skilled in the art to which the present invention pertains from such description.
[0015] One embodiment of the present invention provides a copper foil comprising a copper film comprising 99.9 wt% or more of copper and having an R value in the range of 2.0 to 3.5. The above R is calculated by the following formula 1, [Formula 1] R = log(WA / WB) / log(tA / tB) WA of the above formula 1 is calculated by the following formula 2, [Formula 2] WA = [XA0+(XA45)X2+XA90] / 4 WB of the above formula 1 is calculated by the following formula 3, [Formula 3] WB = [XB0+(XB45)X2+XB90] / 4 tA of the above formula 1 means the thickness of the test piece before the tensile test, tB of the above formula 1 means the thickness of the test piece after the tensile test, XA0, XA45, XA90 of the above formula 2 mean the width of the central part of the tensile direction before tensile testing of the test piece taken in the 0°, 45°, 90° directions, and XB0, XB45, XB90 of the above formula 3 mean the width of the central part of the tensile direction before tensile testing of the test piece taken in the 0°, 45°, 90° directions. It refers to the width of the central part of the tensile direction after tension of the test piece.
[0016] One embodiment of the present invention comprises a copper film comprising 99.9 wt% or more of copper, wherein the copper film has a room temperature loss coefficient of 0.05 or less, and the copper foil: the room temperature loss coefficient is calculated by the following equation 4. [Equation 4] Room temperature loss coefficient = Room temperature loss elastic modulus / Room temperature storage elastic modulus
[0017] Another embodiment of the present invention comprises the steps of preparing an electrolyte containing copper ions, forming a copper film, and forming a protective layer on the copper film, wherein the step of forming the copper film comprises the step of forming a copper film on the rotating cathode drum by energizing a positive electrode plate and a rotating cathode drum, which are spaced apart from each other in the electrolyte in an electrolytic cell, and the electrolyte comprises 70 to 100 g / L of copper ions, 70 to 150 g / L of sulfuric acid, 15 to 25 ppm of chlorine (Cl), 1 to 100 ppm of lead (Pb), 0.3 to 5 ppm of tungsten (W), 1 to 10 ml / L of hydrogen peroxide, and an organic additive, wherein the organic additive comprises at least one of a brightener (component A), a moderator (component B), and a leveling agent (component C), wherein the brightener (component A) comprises sulfonic acid or a metal salt thereof, and the moderator (component B) comprises: A method for manufacturing a copper foil is provided, wherein the copper foil comprises a nonionic water-soluble polymer, and the leveling agent (component C) comprises at least one of nitrogen (N) and sulfur (S).
[0018] According to another embodiment of the present invention, an electrode for a secondary battery is provided, comprising: copper foil; and an active material layer disposed on at least one surface of the copper foil.
[0019] According to another embodiment of the present invention, a secondary battery is provided, including: a cathode that provides lithium ions when charged; an anode that provides electrons and lithium ions when discharged; an electrolyte that is disposed between the cathode and the anode and provides an environment in which lithium ions can move; and a separator that electrically insulates the cathode and the anode.
[0020] According to the present invention, the occurrence of wrinkles or tears during the manufacturing process of copper foil is prevented, and by manufacturing intermediate parts and final products such as flexible printed circuit boards (FPCBs) and secondary batteries using the copper foil, the productivity of the intermediate parts as well as the final products can be improved.
[0021] Figure 1 is a cross-sectional view of a copper foil according to one embodiment of the present invention.
[0022] Figure 2 is a cross-sectional view of a copper foil according to another embodiment of the present invention.
[0023] Figure 3 is a cross-sectional view of an electrode for a secondary battery according to another embodiment of the present invention.
[0024] Figure 4 is a cross-sectional view of an electrode for a secondary battery according to another embodiment of the present invention.
[0025] Figure 5 is a schematic cross-sectional view of a secondary battery according to another embodiment of the present invention.
[0026] Figure 6 is a device for manufacturing copper foil according to another embodiment of the present invention.
[0027] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings. However, the embodiments described below are presented for illustrative purposes only to facilitate a clear understanding of the present invention and do not limit the scope of the present invention.
[0028] The shapes, sizes, ratios, angles, numbers, etc. disclosed in the drawings for explaining embodiments of the present invention are merely illustrative, and the present invention is not limited to the details depicted in the drawings. Throughout the specification, identical components may be designated by identical reference numerals. In describing the present invention, detailed descriptions of related known technologies will be omitted if they are deemed to unnecessarily obscure the gist of the present invention.
[0029] In this specification, where "includes," "has," and "consists of" are used, other parts may be added, unless the expression "only" is used. When a component is expressed in the singular, the plural is included unless otherwise explicitly stated. Furthermore, when interpreting a component, it is interpreted to include a margin of error even if there is no explicit indication otherwise.
[0030] When describing a positional relationship, for example, when the positional relationship between two parts is described as 'on top of', 'upper part of', 'lower part of', 'next to', etc., one or more other parts may be located between the two parts, unless the expression 'right' or 'directly' is used.
[0031] Spatially relative terms such as "below," "beneath," "lower," "above," and "upper" can be used to easily describe the relationship of one element or component to another, as illustrated in the drawings. Spatially relative terms should be understood to include different orientations of the elements during use or operation in addition to the orientations depicted in the drawings. For example, if an element depicted in the drawings were flipped over, an element described as "below" or "beneath" another element could instead be positioned "above" the other element. Thus, the exemplary term "below" can encompass both the above and below directions. Similarly, the exemplary term "above" or "above" can encompass both the above and below directions.
[0032] When describing a temporal relationship, for example, when the temporal relationship is described as 'after', 'following', 'next to', 'before', etc., it can also include cases where it is not continuous, as long as the expression 'immediately' or 'directly' is not used.
[0033] While terms like "first" and "second" are used to describe various components, these components are not limited by these terms. These terms are used merely to distinguish one component from another. Therefore, a "first" component referred to below may also be a "second" component within the technical scope of the present invention.
[0034] The term "at least one" should be understood to include all possible combinations of one or more associated items. For example, "at least one of the first, second, and third items" can mean not only the first, second, or third items, but also any combination of items that can be represented by two or more of the first, second, and third items.
[0035] The features of each of the various embodiments of the present invention can be partially or wholly combined or combined with each other, and various technical connections and operations are possible, and each embodiment can be implemented independently of each other or implemented together in a related relationship.
[0036] Figure 1 is a cross-sectional view of a copper foil (110) according to one embodiment of the present invention.
[0037] Referring to FIG. 1, the copper foil (110) of the present invention includes a copper film (111) containing 99.9 wt% or more of copper and a protective layer (112) on the copper film (111). In the copper foil (110) illustrated in FIG. 1, the protective layer (112) is formed on one surface of the copper film (111), but embodiments of the present invention are not limited thereto. Referring to FIG. 2, the protective layer (112) may be formed on both surfaces of the copper film (111).
[0038] A copper film (111) can be formed on a rotating cathode drum through electroplating, and has a shiny side that directly contacts the rotating cathode drum during the electroplating process and a matte side on the opposite side.
[0039] The protective layer (112) is formed by depositing an anticorrosion material on the copper film (111). The anticorrosion material may include at least one of a chromium compound, a silane compound, and a nitrogen compound. The protective layer (112) prevents oxidation and corrosion of the copper film (111) and improves heat resistance, thereby extending the lifespan of the copper foil (110) itself as well as the lifespan of the final product including it.
[0040] According to one embodiment of the present invention, the copper foil (110) has an R value in the range of 2.0 to 3.5. The R value can be obtained by measuring and calculating WA, WB, tA, and tB, respectively, and calculating the measured and calculated values of WA, WB, tA, and tB according to the following Equation 1.
[0041] [Formula 1]
[0042] R = log(WA / WB) / log(tA / tB)
[0043] In the above equation 1, tA means the thickness of the test piece before the tensile test, and tB in the above equation 1 means the thickness of the test piece after the tensile test.
[0044] The above WA and WB can be obtained by calculation according to the following Equations 2 and 3. First, copper foil (110) is sampled in three directions of 0°, 45°, and 90° from the MD direction, and an axial tensile test is performed on each sampled copper foil under the condition of a UTM tensile test speed of 5 mm / min. At this time, the tensile test is performed until the sampled copper foil grows 15% after tensile stretching compared to before tensile stretching by a universal testing machine (UTM). Then, the width of the central part in the tensile direction of the sampled copper foil before and after the tensile test is measured, respectively, and XA0, XA45, XA90, XB0, XB45, and XB90 of the following Equations 2 and 3 can be calculated and produced.
[0045] [Formula 2]
[0046] WA = [XA0+(XA45)X2+XA90] / 4
[0047] [Formula 3]
[0048] WB = [XB0+(XB45)X2+XB90] / 4
[0049] XA0, XA45, and XA90 in the above formula 2 represent the widths of the central portions of the tensile direction before tensile testing of the test specimens taken in the 0°, 45°, and 90° directions.
[0050] XB0, XB45, and XB90 in the above formula 3 represent the widths of the central portions of the tensile direction after tension of the test specimens taken in the 0°, 45°, and 90° directions.
[0051] According to one embodiment of the present invention, the copper foil (110) may have an R value in the range of 2.0 to 3.5.
[0052] If the R value of the copper foil (110) is less than 2.0, the change in the thickness of the copper foil (110) is large compared to the change in the width of the copper foil (110), and wrinkles or tears may occur during the manufacturing process of the copper foil (110), thereby reducing workability and increasing the defect rate of the secondary battery.
[0053] On the other hand, if the R value of the copper foil (110) exceeds 3.5, the change in the width of the copper foil (110) is large compared to the change in the thickness of the copper foil (110), so that wrinkles or tears may occur during the manufacturing process of the copper foil (110), and as a result, workability is reduced and the defect rate of the secondary battery increases.
[0054] According to one embodiment of the present invention, the copper film (111) has a room temperature loss coefficient of 0.05 or less. The room temperature loss coefficient can be obtained by calculating according to the following equation 4.
[0055] [Formula 4]
[0056] Room temperature loss modulus = Room temperature loss modulus / Room temperature storage modulus
[0057] The room temperature storage modulus of the above equation 4 refers to the elastic energy stored inside the copper film at room temperature, and the room temperature loss modulus of the above equation 4 refers to the energy lost due to viscosity from the elastic energy stored inside the copper film at room temperature. Specifically, room temperature refers to 25°C.
[0058] If the room temperature loss coefficient of the copper film (111) exceeds 0.05, the loss of elastic energy stored within the copper film (111) increases, and the elastic energy stored within the copper film may not be maintained against external impact. Therefore, wrinkles or tears may occur during the manufacturing process of the copper foil (110), which reduces workability and increases the failure rate of the secondary battery.
[0059] According to one embodiment of the present invention, the copper film (111) has a high temperature loss coefficient of 0.2 or less. The high temperature loss coefficient can be calculated and obtained according to the following equation 5.
[0060] [Formula 5]
[0061] High temperature loss modulus = High temperature loss modulus / High temperature storage modulus
[0062] The high-temperature storage elastic modulus of the above formula 5 refers to the elastic energy stored inside the copper film after heat treatment at 350°C for 1 hour, and the high-temperature loss elastic modulus of the above formula 5 refers to the energy lost due to viscosity from the elastic energy stored inside the copper film after heat treatment at 350°C for 1 hour.
[0063] If the high temperature loss coefficient of the copper film (111) exceeds 0.2, the loss of elastic energy stored inside the copper film (111) at high temperatures increases, and the elastic energy stored inside the copper film may not be maintained from external impact. In addition, due to the manufacturing process characteristics of the copper foil (110) that performs a high temperature process, softening may occur during the roll press process and / or drying process, and handling properties may deteriorate due to wrinkles.
[0064] According to one embodiment of the present invention, the copper film (111) may have a room temperature storage elastic modulus in the range of 30 to 80 GPa. The room temperature storage elastic modulus refers to the elastic energy stored inside the copper film at room temperature.
[0065] When the room temperature storage elastic modulus of the copper film (111) is less than 30 GPa, the elastic energy stored inside the copper film (111) is very small, and there is not enough elastic energy to withstand external impact. Therefore, wrinkles or tears may occur during the manufacturing process of the copper foil (110), which may reduce workability and increase the failure rate of the secondary battery.
[0066] If the room temperature storage elastic modulus of the copper film (111) exceeds 80 GPA, it may not be able to cope with the expansion and contraction of the active material during the manufacturing process of the negative electrode current collector of the secondary battery. As a result, the active material and the copper foil (110) may peel off or the copper foil (110) may break, thereby lowering the charge / discharge efficiency of the secondary battery.
[0067] According to one embodiment of the present invention, the copper film (111) has a room temperature loss modulus of elasticity of 5 GPa or less. The room temperature loss modulus refers to the energy lost due to viscosity from the elastic energy stored inside the copper film at room temperature.
[0068] If the room temperature loss modulus of elasticity of the copper film (111) exceeds 5 GPa, the loss of elastic energy stored within the copper film (111) increases, and the elastic energy stored within the copper film cannot be maintained against external impact. Therefore, wrinkles or tears may occur during the manufacturing process of the copper foil (110), which reduces workability and increases the failure rate of the secondary battery.
[0069] According to one embodiment of the present invention, the copper film (111) has a high-temperature storage modulus in the range of 20 to 60 GPa. The high-temperature storage modulus refers to the elastic energy stored within the copper film after heat treatment at 350°C for 1 hour.
[0070] When the high-temperature storage elastic modulus of the copper film (111) is less than 20 GPa, the elastic energy stored inside the copper film (111) at high temperatures is very small. Therefore, due to the manufacturing process characteristics of the copper foil (110) that performs a high-temperature process, the copper foil (110) does not have sufficient elastic energy to withstand external impact at high temperatures. Therefore, wrinkles or tears may occur during the manufacturing process of the copper foil (110), which may lower workability and increase the failure rate of the secondary battery.
[0071] When the high temperature storage elastic modulus of the copper film (111) exceeds 60 GPa, due to the manufacturing process characteristics of the copper foil (110) that performs a high temperature process, if the active material expands at a high temperature, the active material and the copper foil (110) may be separated, or the copper foil (110) may be broken, thereby lowering the charge / discharge efficiency of the secondary battery.
[0072] According to one embodiment of the present invention, the copper film (111) has a high-temperature loss modulus of elasticity of 10 GPa or less. The high-temperature loss modulus refers to the energy lost due to viscosity from the elastic energy stored within the copper film after heat treatment at 350°C for 1 hour.
[0073] When the high temperature loss modulus of elasticity of the copper film (111) exceeds 10 GPa, the loss of elastic energy stored inside the copper film (111) at high temperatures is large. Therefore, due to the manufacturing process characteristics of the copper foil (110) that performs a high temperature process, the copper foil (110) may not be able to maintain the elastic energy stored inside the copper film from external impact at high temperatures. In addition, due to the manufacturing process characteristics of the copper foil (110) that performs a high temperature process, softening may occur during the roll press process and / or the drying process, and handling properties may deteriorate due to wrinkles.
[0074] According to one embodiment of the present invention, the copper foil (110) may have a coefficient of thermal expansion in the range of 5 to 30 ppm / °C. Specifically, the copper foil (110) may have a coefficient of thermal expansion in the range of 10 to 25 ppm / °C. More specifically, the copper foil (110) may have a coefficient of thermal expansion in the range of 15 to 20 ppm / °C.
[0075] If the coefficient of thermal expansion of the copper foil (110) is less than 5 ppm / ℃, wrinkles or tears may occur in the copper foil (110) during the process of manufacturing the copper foil (110) through a roll-to-roll process.
[0076] On the other hand, when the coefficient of thermal expansion exceeds 30 ppm / ℃, the copper foil (110) is warped to a considerable extent during the process of manufacturing the copper foil (110) through a roll-to-roll process.
[0077] The copper foil (110) according to one embodiment of the present invention may have a thickness of 4 to 35 μm. When the copper foil (110) is used as a current collector of an electrode in a secondary battery, the thinner the copper foil (110), the more current collectors can be accommodated within the same space, which is advantageous for increasing the capacity of the secondary battery. However, the manufacture of a copper foil (110) having a thickness of less than 4 μm causes a decrease in workability.
[0078] On the other hand, when manufacturing a secondary battery with copper foil (110) exceeding 35 ㎛, it becomes difficult to achieve high capacity due to the thick copper foil (110).
[0079] According to one embodiment of the present invention, the copper foil (110) is 45 kg / mm 2 It can have a tensile strength of 45 kg / mm2 or more. In order to suppress wrinkles and tears of the copper foil (110), the copper foil (110) of the present invention has a high tensile strength of 45 kg / mm2 or more. If the tensile strength of the copper foil (110) is less than 45 kg / mm2, folding of the copper foil (110) occurs between two adjacent rolls during the roll-to-roll manufacturing process, or wrinkles occur at the left and right ends of the copper foil (110) during the roll-to-roll manufacturing process.
[0080] The copper foil (110) according to one embodiment of the present invention may have an elongation of 3 to 13%.
[0081] If the elongation of the copper foil (110) is less than 3%, when the copper foil (110) is used as a current collector of a secondary battery, there is a high risk that the copper foil (110) will not be sufficiently stretched to respond to the large volume expansion of the high-capacity active material and will tear.
[0082] On the other hand, if the elongation of the copper foil (110) exceeds 13%, the copper foil (110) may easily elongate during the secondary battery electrode manufacturing process, causing deformation of the electrode.
[0083] According to one embodiment of the present invention, the copper foil (110) may have a 10-point average roughness (Rz) of 0.7 to 0.9 μm.
[0084] As the charge and discharge of the secondary battery is repeated, the active material layer alternately contracts and expands, which causes separation of the active material layer and the copper foil (110), thereby reducing the charge and discharge efficiency of the secondary battery. Therefore, in order for the secondary electrode to secure a certain level of capacity retention rate and lifespan (i.e., to suppress the reduction in the charge and discharge efficiency of the secondary battery), the copper foil (110) must have excellent coating properties for the active material, thereby increasing the adhesive strength between the copper foil (110) and the active material layer.
[0085] Specifically, the smaller the 10-point average roughness (Rz) of the copper foil (110), the less the charge / discharge efficiency of the secondary battery including the copper foil (110) tends to deteriorate. Therefore, according to one embodiment of the present invention, the copper foil (110) has a 10-point average roughness (Rz) of 0.7 to 0.9 μm.
[0086] When the 10-point average roughness (Rz) of the copper foil (110) is less than 0.7, the surface area of the copper foil (110) is relatively small, so the active material is easily detached from the copper foil (110), and as a result, a rapid decrease in the lifespan of the secondary battery occurs due to repeated charging and discharging.
[0087] On the other hand, when the 10-point average roughness (Rz) of the copper foil (110) exceeds 0.9, the contact uniformity between the copper foil (110) and the active material layer does not reach a certain level, so that a large number of spaces exist between the copper foil (110) and the active material layer (i.e., the coating itself is not partially formed), and as a result, a rapid decrease in the lifespan of the secondary battery is caused due to repeated charge and discharge.
[0088] According to one embodiment of the present invention, the copper foil (110) may have an arithmetic mean roughness (Ra) of 0.2 to 0.3 μm.
[0089] As the charge and discharge of the secondary battery is repeated, the active material layer alternately contracts and expands, which causes separation of the active material layer and the copper foil (110), thereby reducing the charge and discharge efficiency of the secondary battery. Therefore, in order for the secondary electrode to secure a certain level of capacity retention rate and lifespan (i.e., to suppress the reduction in the charge and discharge efficiency of the secondary battery), the copper foil (110) must have excellent coating properties for the active material, thereby increasing the adhesive strength between the copper foil (110) and the active material layer.
[0090] Specifically, the smaller the arithmetic mean roughness (Ra) of the copper foil (110), the less the charge / discharge efficiency of the secondary battery including the copper foil (110) tends to deteriorate. Therefore, according to one embodiment of the present invention, the copper foil (110) has an arithmetic mean roughness (Ra) of 0.2 to 0.3 μm.
[0091] When the arithmetic mean roughness (Ra) of the copper foil (110) is less than 0.2, the surface area of the copper foil (110) is relatively small, so the active material is easily detached from the copper foil (110), and as a result, a rapid decrease in the lifespan of the secondary battery occurs due to repeated charging and discharging.
[0092] On the other hand, when the arithmetic mean roughness (Ra) of the copper foil (110) exceeds 0.3, the contact uniformity between the copper foil (110) and the active material layer does not reach a certain level, so that a large number of spaces exist between the copper foil (110) and the active material layer (i.e., the coating itself is not partially formed), and as a result, a rapid decrease in the lifespan of the secondary battery occurs due to repeated charge and discharge.
[0093] Hereinafter, an electrode (100) including a copper foil (110) of the present invention and a secondary battery including the electrode (100) will be described in detail.
[0094] Figure 3 is a cross-sectional view of an electrode for a secondary battery according to one embodiment of the present invention.
[0095] As illustrated in FIG. 3, an electrode (100) for a secondary battery according to one embodiment of the present invention includes a copper foil (110) and an active material layer (120) of any one of the embodiments of the present invention described above.
[0096] Figure 3 illustrates a configuration in which an active material layer (120) is formed on one side of a copper foil (110). However, one embodiment of the present invention is not limited thereto, and with reference to Figure 4, the active material layer (120) may be formed on both sides of the copper foil (110).
[0097] In lithium secondary batteries, aluminum foil is generally used as a positive electrode current collector combined with a positive electrode active material, and copper foil (110) is generally used as a negative electrode current collector combined with a negative electrode active material.
[0098] According to one embodiment of the present invention, the secondary battery electrode (100) is a negative electrode, the copper foil (110) is used as a negative electrode current collector, and the active material layer (120) includes a negative electrode active material.
[0099] In order to secure high capacity of the secondary battery, the active material layer (120) of the present invention may be formed of a composite of carbon and metal. The metal may include, for example, at least one of Si, Ge, Sn, Li, Zn, Mg, Cd, Ce, Ni, and Fe, preferably Si and / or Sn.
[0100] Figure 5 is a schematic cross-sectional view of a secondary battery according to one embodiment of the present invention.
[0101] Referring to FIG. 5, the secondary battery includes a cathode (370), an anode (340), an electrolyte (350) disposed between the anode (370) and the cathode (340) to provide an environment in which ions can move, and a separator (360) that electrically insulates the anode (370) and the cathode (340). Here, the ions that move between the anode (370) and the cathode (340) are, for example, lithium ions. The separator (360) separates the anode (370) and the cathode (340) to prevent charges generated at one electrode from being unnecessarily consumed by moving to the other electrode through the interior of the secondary battery (105). Referring to FIG. 5, the separator (360) is disposed within the electrolyte (350).
[0102] The positive electrode (370) includes a positive electrode current collector (371) and a positive electrode active material layer (372), and aluminum foil can be used as the positive electrode current collector (371).
[0103] The negative electrode (340) includes a negative electrode current collector (341) and a negative electrode active material layer (342), and copper foil (110) can be used as the negative electrode current collector (341).
[0104] According to one embodiment of the present invention, the copper foil (110) disclosed in FIG. 1 or FIG. 2 may be used as the negative electrode current collector (341). In addition, the secondary battery electrode (100) illustrated in FIG. 3 or FIG. 4 may be used as the negative electrode (340) of the secondary battery illustrated in FIG. 5.
[0105] Hereinafter, the method for manufacturing the copper foil (110) of the present invention will be specifically described with reference to FIG. 6.
[0106] The method for manufacturing copper foil (110) of the present invention includes a step of forming a copper film (111) and a step of forming a protective layer (112) on the copper film (111).
[0107] The method of the present invention includes a step of forming a copper film (111) on the rotating cathode drum (40) by energizing the anode plates (30) and the rotating cathode drum (40) which are spaced apart from each other in the electrolyte (20) in the electrolytic cell (10).
[0108] As illustrated in FIG. 6, the bipolar plate (30) may include first and second bipolar plates (31, 32) that are electrically insulated from each other.
[0109] The copper film (111) formation step can be performed by forming a seed layer by conducting current between the first positive electrode plate (31) and the rotating negative electrode drum (40), and then growing the seed layer by conducting current between the second positive electrode plate (32) and the rotating negative electrode drum (40).
[0110] The current density provided by the first and second bipolar plates (31, 32) may be 30 to 130 ASD, respectively.
[0111] When the current density provided by the first and second positive electrode plates (31, 32) is less than 30 ASD, the surface roughness of the copper foil (110) may be low, and the adhesion between the copper foil (110) and the active material layer (120) may not be sufficient.
[0112] On the other hand, if the current density provided by the first and second positive electrode plates (31, 32) exceeds 130 ASD, the surface of the copper foil (110) may be rough, so that the coating of the active material may not be performed smoothly.
[0113] The surface properties of the copper film (111) may vary depending on the degree of surface buffing or polishing of the rotating cathode drum (40). For example, the surface of the rotating cathode drum (40) may be polished with a polishing brush having a grit size of #800 to #3000.
[0114] During the copper film (111) formation process, the electrolyte (20) is maintained at a temperature of 48 to 60°C. More specifically, the temperature of the electrolyte (20) can be maintained at 50°C or higher. At this time, the physical, chemical, and electrical properties of the copper film (111) can be controlled by adjusting the composition of the electrolyte (20).
[0115] According to one embodiment of the present invention, the electrolyte (20) contains 70 to 100 g / L of copper ions, 70 to 150 g / L of sulfuric acid, 15 to 25 ppm of chlorine (Cl), 1 to 10 ml / L of hydrogen peroxide (H2O2), and an organic additive.
[0116] In order to facilitate the formation of a copper film (111) by copper electrodeposition, the concentration of copper ions and the concentration of sulfuric acid in the electrolyte (20) are adjusted to 70 to 100 g / L and 70 to 150 g / L, respectively.
[0117] In one embodiment of the present invention, chlorine (Cl) includes both chlorine ions (Cl-) and chlorine atoms present in the molecule. Chlorine (Cl) can be used, for example, to remove silver (Ag) ions introduced into the electrolyte (20) during the process of forming a copper film (111). Specifically, chlorine (Cl) can precipitate silver (Ag) ions in the form of silver chloride (AgCl). This silver chloride (AgCl) can be removed by filtration.
[0118] When the concentration of chlorine (Cl) is less than 15 ppm, the removal of silver (Ag) ions is not smoothly performed. On the other hand, when the concentration of chlorine (Cl) exceeds 25 ppm, an unnecessary reaction due to excessive chlorine (Cl) may occur. Therefore, the concentration of chlorine (Cl) in the electrolyte (20) is managed in the range of 15 to 25 ppm.
[0119] According to one embodiment of the present invention, the electrolyte (20) including an organic additive comprises lead ions (Pb 2+) may further include lead ions (Pb). Specifically, the electrolyte (20) may include 1 to 100 ppm of lead ions (Pb 2+ ) may contain lead ions (Pb 2+ ) is maintained at 1 to 100 ppm, the R value according to the present invention can be maintained in the range of 2.0 to 3.5.
[0120] Lead ion (Pb 2+ ) is maintained at 1 to 100 ppm, the copper film (111) according to the present invention can have a room temperature loss coefficient maintained at 0.05 or less and a high temperature loss coefficient maintained at 0.2 or less.
[0121] On the other hand, lead ion (Pb 2+ ) is less than 1 ppm, a problem of reduced effectiveness in maintaining the properties of the present invention may occur. As a result, a problem of the R value falling outside the range of 2.0 to 3.5 may occur.
[0122] Additionally, lead ions (Pb 2+ ) exceeds 100 ppm, copper is unevenly precipitated, which may cause rapid changes in the thickness and width of the copper foil before and after the tensile test, and thus, a problem may occur in which the R value falls outside the range of 2.0 to 3.5.
[0123] On the other hand, lead ion (Pb 2+ ) is less than 1 ppm, a problem of reduced effectiveness in maintaining the properties of the present invention may occur. As a result, rapid changes may occur in the values of the loss elastic modulus and storage elastic modulus of the copper film (111), so that the value of the room temperature loss coefficient exceeds 0.05 and the high temperature loss coefficient exceeds 0.2.
[0124] Additionally, lead ions (Pb 2+) exceeds 100 ppm, copper is unevenly precipitated, which may cause a rapid change in the values of the loss elastic modulus and storage elastic modulus of the copper film (111), so that the value of the room temperature loss coefficient exceeds 0.05 and the high temperature loss coefficient exceeds 0.2.
[0125] Additionally, according to one embodiment of the present invention, the electrolyte (20) including the organic additive may further include tungsten (W). Specifically, the electrolyte (20) may include 0.3 to 5 ppm of tungsten (W). When tungsten (W) is maintained at 0.3 to 5 ppm, the R value according to the present invention may be maintained in a range of 2.0 to 3.5.
[0126] According to one embodiment of the present invention, the electrolyte (20) including an organic additive may further include tungsten (W). When tungsten (W) is treated in the electrolyte (20), the average size of crystalline particles included in the copper film (111) may decrease, and the strength of the copper foil (110) may increase. The concentration of tungsten (W) in the electrolyte (20) may be 0.3 to 5 ppm. Specifically, it is preferable to add 1 to 4 ppm of tungsten (W).
[0127] On the other hand, when the concentration of tungsten (W) is less than 0.3 ppm, the average crystalline particle size of the copper film (111) becomes inconsistent, and as a result, rapid changes may occur in the thickness and width of the copper foil before and after the tensile test, and thus, a problem may occur in which the R value falls outside the range of 2.0 to 3.5.
[0128] In addition, when the concentration of tungsten (W) exceeds 5 ppm, the amount of impurities increases, which may cause rapid changes in the thickness and width of the copper foil before and after the tensile test, and thus, a problem may occur in which the R value falls outside the range of 2.0 to 3.5.
[0129] On the other hand, when the concentration of tungsten (W) is less than 0.3 ppm, the average crystalline particle size of the copper film (111) becomes inconsistent, and as a result, the values of the loss elastic modulus and the storage elastic modulus of the copper film (111) may change rapidly, so that the value of the room temperature loss coefficient exceeds 0.05 and the high temperature loss coefficient exceeds 0.2.
[0130] In addition, when the concentration of tungsten (W) exceeds 5 ppm, the amount of impurities increases, which may cause a rapid change in the values of the loss elastic modulus and storage elastic modulus of the copper film (111), so that the value of the room temperature loss coefficient exceeds 0.05 and the high temperature loss coefficient exceeds 0.2.
[0131] According to one embodiment of the present invention, the electrolyte (20) including an organic additive may further include hydrogen peroxide (H2O2). Organic impurities exist in the electrolyte (20) that is continuously plated due to the organic additive, and by treating with hydrogen peroxide (H2O2), the organic impurities are decomposed, so that the carbon (C) content inside the copper foil can be appropriately controlled. As the TOC concentration in the electrolyte (20) increases, the amount of carbon (C) element flowing into the copper film (111) increases, and accordingly, the total amount of elements released from the copper film (111) during heat treatment increases, which causes the strength of the copper foil (110) to decrease after the heat treatment.
[0132] The amount of hydrogen peroxide (H2O2) added is 1 to 10 ml per L of electrolyte. Specifically, it is preferable to add 2 to 8 ml per L of electrolyte. If the amount of hydrogen peroxide (H2O2) added is less than 1 ml / L, it is meaningless because the effect of decomposing organic impurities is almost nonexistent. If the amount of hydrogen peroxide (H2O2) added exceeds 10 ml / L, organic impurities are excessively decomposed, and the effect of organic additives such as brighteners, moderators, and leveling agents is also suppressed.
[0133] The organic additive contained in the electrolyte (20) includes at least one of a brightener (component A), a moderator (component B), and a leveling agent (component C). The organic additive has a concentration of 1 to 100 ppm in the electrolyte (20).
[0134] The organic additive may contain two or more of a brightener (component A), a moderator (component B), and a leveling agent (component C), or may contain all three. Even in such cases, the concentration of the organic additive is 100 ppm or less. When the organic additive contains all of a brightener (component A), a moderator (component B), and a leveling agent (component C), the concentration of the organic additive may be 10 to 100 ppm.
[0135] The polishing agent (component A) contains sulfonic acid or its metal salt. The polishing agent (component A) may have a concentration of 1 to 25 ppm in the electrolyte (20).
[0136] The brightener (component A) increases the charge of the electrolyte (20), thereby increasing the deposition speed of copper, improving the curling characteristics of the copper foil, and enhancing the gloss of the copper foil (110). If the concentration of the brightener (component A) is less than 1 ppm, the gloss of the copper foil (110) may decrease, and at the same time, surface defects of the copper foil (110) may occur, causing a problem in which the R value falls outside the range of 2.0 to 3.5. In addition, if the concentration of the brightener (component A) exceeds 25 ppm, the roughness of the copper foil (110) may increase and the strength may fall, and as a result, rapid changes may occur in the thickness and width of the copper foil before and after the tensile test, causing a problem in which the R value falls outside the range of 2.0 to 3.5.
[0137] The brightener (component A) increases the charge of the electrolyte (20), thereby increasing the deposition speed of copper, improving the curling characteristics of the copper foil, and enhancing the gloss of the copper foil (110). If the concentration of the brightener (component A) is less than 1 ppm, the gloss of the copper foil (110) may decrease, and if it exceeds 25 ppm, the roughness of the copper foil (110) may increase and the strength may decrease. As a result, curling, wrinkling, or tearing may occur during the manufacturing process of the copper foil (110). In addition, rapid changes may occur in the values of the loss modulus and the storage modulus, such that the value of the room temperature loss modulus exceeds 0.05, and the value of the high temperature loss modulus exceeds 0.2.
[0138] More specifically, the polishing agent (component A) may have a concentration of 5 to 20 ppm in the electrolyte (20).
[0139] The polishing agent may include, for example, at least one of bis-(3-sulfopropyl)-disulfide disodium salt, 3-mercapto-1-propanesulfonic acid, 3-(N,N-dimethylthiocarbamoyl)-thiopropanesulfonate sodium salt, 3-[(amino-iminomethyl)thio]-1-propanesulfonate sodium salt, o-ethyldithiocarbonato-S-(3-sulfopropyl)-ester sodium salt, 3-(benzothiazolyl-2-mercapto)-propyl-sulfonic acid sodium salt, and ethylenedithiodipropylsulfonic acid sodium salt.
[0140] The moderator (component B) includes a nonionic water-soluble polymer. The moderator (component B) may have a concentration of 1 to 10 ppm in the electrolyte (20).
[0141] The moderator (component B) reduces the deposition speed of copper, thereby preventing rapid increase in roughness and decrease in strength of the copper foil (110). This moderator (component B) is also called an inhibitor or suppressor.
[0142] If the concentration of the moderator (component B) is less than 1 ppm, the roughness of the copper foil (110) may increase rapidly, and the strength of the copper foil (110) may decrease. As a result, the thickness and width of the copper foil before and after the tensile test may change rapidly, and the R value may fall outside the range of 2.0 to 3.5. On the other hand, even if the concentration of the moderator (component B) exceeds 10 ppm, there is almost no change in the physical properties of the copper foil (110) such as appearance, gloss, roughness, strength, and elongation. Therefore, the concentration of the moderator (component B) can be adjusted to the range of 1 to 10 ppm without unnecessarily increasing the concentration of the moderator (component B) to increase the manufacturing cost and waste raw materials.
[0143] If the concentration of the moderator (component B) is less than 1 ppm, the roughness of the copper foil (110) may rapidly increase, and the strength of the copper foil (110) may decrease. In addition, the values of the loss modulus and the storage modulus may rapidly change, so that the value of the room temperature loss modulus exceeds 0.05, and the value of the high temperature loss modulus exceeds 0.2. As a result, wrinkles or tears may occur during the manufacturing process of the copper foil (110). On the other hand, even if the concentration of the moderator (component B) exceeds 10 ppm, there is almost no change in the physical properties of the copper foil (110) such as appearance, gloss, roughness, strength, and elongation. Therefore, the concentration of the moderator (component B) can be adjusted in the range of 1 to 10 ppm without unnecessarily increasing the concentration of the moderator (component B) to increase the manufacturing cost and waste raw materials.
[0144] The moderator (component B) may include at least one nonionic water-soluble polymer selected from, for example, polyethylene glycol (PEG), polypropylene glycol, polyethylene polypropylene copolymer, polyglycerin, polyethylene glycol dimethyl ether, hydroxyethylene cellulose, polyvinyl alcohol, stearic acid polyglycol ether, and stearyl alcohol polyglycol ether. However, the type of moderator is not limited thereto, and other nonionic water-soluble polymers that can be used in the production of high-strength copper foil (110) may be used as the moderator.
[0145] The leveling agent (component C) contains at least one of nitrogen (N) and sulfur (S). That is, the leveling agent (component C) may contain one or more nitrogen atoms (N) or one or more sulfur atoms (S) in one molecule, and may also contain one or more nitrogen atoms (N) and one or more sulfur atoms (S). For example, the leveling agent (component C) is an organic compound containing at least one of nitrogen (N) and sulfur (S).
[0146] The leveling agent (component C) prevents excessively high peaks or excessively large protrusions from being formed on the copper film (111), thereby making the copper film (111) macroscopically flat. The leveling agent (component C) may have a concentration of 1 to 10 ppm in the electrolyte (11).
[0147] When the concentration of the leveling agent (component C) is less than 1 ppm, the strength of the copper foil (110) is reduced, making it difficult to manufacture a high-strength copper foil (110). As a result, rapid changes may occur in the thickness and width of the copper foil before and after the tensile test, which may cause a problem in which the R value falls outside the range of 2.0 to 3.5. On the other hand, when the concentration of the leveling agent (component C) exceeds 10 ppm, the surface roughness of the copper foil (110) may excessively increase, which may cause a decrease in strength, and pinholes or curls may occur on the surface of the copper foil (110), which may cause difficulty in separating the copper foil (110) from the winder (WR) after its manufacture. As a result, rapid changes may occur in the thickness and width of the copper foil before and after the tensile test, which may cause a problem in which the R value falls outside the range of 2.0 to 3.5.
[0148] When the concentration of the leveling agent (component C) is less than 1 ppm, the strength of the copper foil (110) may be reduced, resulting in wrinkles or tears in the copper foil (110). In addition, rapid changes may occur in the values of the loss modulus and the storage modulus, resulting in the room temperature loss modulus exceeding 0.05 and the high temperature loss modulus exceeding 0.2. On the other hand, when the concentration of the leveling agent (component C) exceeds 10 ppm, the surface roughness of the copper foil (110) may excessively increase, resulting in a reduction in strength, and pinholes or curls may occur on the surface of the copper foil (110), making it difficult to separate the copper foil (110) from the winder (WR) after manufacturing it. In addition, rapid changes may occur in the values of the loss modulus and the storage modulus, resulting in the room temperature loss modulus exceeding 0.05 and the high temperature loss modulus exceeding 0.2.
[0149] Leveling agents (component C) include, for example, diethylthiourea, ethylenethiourea, acetylenethiourea, dipropylthiourea, dibutylthiourea, N-trifluoroacetylthiourea, N-ethylthiourea, N-cyanoacetylthiourea, N-allylthiourea, o-tolylthiourea, N,N'-butylene thiourea, thiazolidinethiol, 4-thiazolinethiol, 4-methyl-2-pyrimidinethiol, 2-thiouracil, 3-(benzotriazole-2-mercapto)-prosulfonic acid), 2-mercaptopyridine, 3(5-mercapto 1H-tetrazol)benzenesulfonate, 2-mercaptobenzothiazole, dimethylpyridine, 2,2'-bipyridine, 4.4'-bipyridine, pyrimidine, pyridazine, pyrimidine, pyrinoline, oxazole, thiazole, 1-methylimidazole, 1-benzylimidazole, 1-methyl-2methylimidazole, 1-benzyl-2-methylimidazole, 1-ethyl-4-methylimidazole, 1-ethyl-2-ethyl-4-methylol, N-methylpyrrole, N-ethylpyrrole, N-butylpyrrole, N-methylpyrroline, N-ethylpyrroline, It may include at least one of N-butylpyrroline, pyrimidine, purine, quinoline, isoquinoline, N-methylcarbazole, N-ethylcarbazole, and N-butylcarbazole.
[0150] When the copper film (111) is formed, the flow rate of the electrolyte (20) supplied into the electrolytic cell (10) is 41 to 45 m 3 It could be / hour.
[0151] The step of forming a copper film (111) may include at least one of a step of filtering the electrolyte (20) using activated carbon, a step of filtering the electrolyte (20) using diatomaceous earth, and a step of treating the electrolyte (20) with ozone (O3).
[0152] Specifically, for filtration of the electrolyte (20), the electrolyte (20) may be circulated at a flow rate of 35 to 45 m3 / hour. That is, in order to remove solid impurities present in the electrolyte (20) while electroplating for forming a copper film (111) is performed, filtration may be performed at a flow rate of 35 to 45 m3 / hour. At this time, activated carbon or diatomaceous earth may be used.
[0153] To maintain the cleanliness of the electrolyte (20), the electrolyte (20) may be treated with ozone (O3).
[0154] Additionally, to ensure the purity of the electrolyte (20), the copper wire (Cu wire), which is the raw material of the electrolyte (20), can be cleaned.
[0155] According to one embodiment of the present invention, the step of preparing an electrolyte (20) may include a step of heat-treating a copper wire, a step of acid-cleaning the heat-treated copper wire, a step of washing the acid-cleaned copper wire, and a step of putting the washed copper wire into sulfuric acid for an electrolyte.
[0156] More specifically, in order to maintain the purity of the electrolyte (20), a high-purity (99.9% or more) copper wire (Cu wire) is heat-treated in an electric furnace at 750°C to 850°C to burn off various organic impurities on the copper wire, and then the heat-treated copper wire is pickled for 10 to 20 minutes using a 10% sulfuric acid solution, and the pickled copper wire is washed using distilled water. Through these sequential processes, copper for preparing the electrolyte (20) can be manufactured. The washed copper wire can be mixed with sulfuric acid for the electrolyte to prepare the electrolyte (20).
[0157] According to one embodiment of the present invention, the concentration of total organic carbon (TOC) in the electrolyte (20) is managed to be 50 ppm or less in order to satisfy the characteristics of the copper foil (110). That is, the electrolyte (20) may have a total organic carbon (TOC) concentration of 50 ppm or less.
[0158] The copper film (111) manufactured in this way can be cleaned in a cleaning tank.
[0159] For example, acid cleaning to remove impurities, such as resin components or natural oxide, on the surface of the copper film (111) and water cleaning to remove the acid solution used in the acid cleaning may be performed sequentially. The cleaning process may be omitted.
[0160] Next, a protective layer (112) is formed on the copper film (111).
[0161] Referring to Fig. 6, a step of immersing the copper film (111) in an anticorrosion solution (60) may be further included. When the copper film (111) is immersed in the anticorrosion solution (60), it may be guided by a guide roll (70) placed within the anticorrosion solution (60).
[0162] As described above, the anti-rust solution (60) may include at least one of a chromium compound, a silane compound, and a nitrogen compound. For example, the copper film (111) may be immersed in a 1 to 10 g / L potassium dichromate solution at room temperature for 1 to 30 seconds.
[0163] Meanwhile, the protective layer (112) may include a silane compound through silane treatment or a nitrogen compound through nitrogen treatment.
[0164] Copper foil (110) is created by forming this protective layer (112).
[0165] An electrode for a secondary battery (i.e., an anode) of the present invention can be manufactured by coating one or more negative active materials selected from the group consisting of carbon; a metal (Me) of Si, Ge, Sn, Li, Zn, Mg, Cd, Ce, Ni or Fe; an alloy containing the metal (Me); an oxide (MeOx) of the metal (Me); and a complex of the metal (Me) and carbon on one or both sides of the copper foil (110) of the present invention manufactured through the above method.
[0166] For example, 100 parts by weight of carbon for negative electrode active material is mixed with 1 to 3 parts by weight of styrene butadiene rubber (SBR) and 1 to 3 parts by weight of carboxymethyl cellulose (CMC), and then a slurry is prepared using distilled water as a solvent. Then, the slurry is applied to the copper foil (110) to a thickness of 20 to 60 μm using a doctor blade, and pressed at a pressure of 0.5 to 1.5 ton / cm2 at 110 to 130°C.
[0167] A secondary battery can be manufactured using a conventional positive electrode, electrolyte, and separator together with the secondary battery electrode (negative electrode) of the present invention manufactured by the above method.
[0168] Below, the present invention is specifically described through examples and comparative examples. However, the following examples are provided solely to aid understanding of the present invention, and the scope of the present invention is not limited to these examples.
[0169] Example 1-4 and Comparative Example 1-7
[0170] Copper foil was manufactured using a foil maker including an electrolytic cell (10), a rotating cathode drum (40) placed in the electrolytic cell (10), and an anode plate (30) placed spaced apart from the rotating cathode drum (40). The electrolyte (20) is a copper sulfate solution. The concentration of copper ions in the electrolyte (20) was set to 87 g / L, the concentration of sulfuric acid was set to 110 g / L, the temperature of the electrolyte was set to 55°C, and the current density was set to 60 ASD.
[0171] In addition, chlorine (Cl) and lead (Pb) contained in the electrolyte (20) 2+ ), the concentration of tungsten (W) and the concentration of organic additives are as shown in Table 1 below.
[0172] Among the organic additives, bis-(3-sulfopropyl)-disulfide disodium salt (SPS) was used as a brightener (component A), polyethylene glycol (PEG) was used as a moderator (component B), and ethylene thiourea (ETU) was used as a leveling agent (component C).
[0173] A copper film (111) was manufactured by applying a current at a current density of 60 ASD between a rotating cathode drum (40) and an anode plate (30). Next, the copper film (111) was immersed in a rust-preventing solution for about 2 seconds to perform a chromate treatment on the surface of the copper film (111) to form a protective layer (112), thereby manufacturing a copper foil (110). A rust-preventing solution containing chromic acid as a main component was used, and the concentration of chromic acid was 5 g / L.
[0174] As a result, copper foils of Example 1-4 and Comparative Example 1-7 were manufactured.
[0175] SPS (Component A) (ppm) PEG (Component B) (ppm) ETU (Component C) (ppm) Chlorine (ppm) Lead (Pb) 2+ )(ppm)Tungsten(ppm)Hydrogen peroxide(ml / L)Current density(ASD)Example 152320301.0250Example 2104520301.5550Example 3156720501.5750Example 4208920702.0750Comparative Example 15555200.10.1950Comparative Example 210507200.10.1750Comparative Example 315755200.10.1550Comparative Example 40.5552013071550Comparative Example 5100.5720130100.150Comparative Example 61570.52015015550Comparative Example 70.5151520500.1550
[0176]
[0177] WAWBtAtBR tensile strength (kgf / mm) 2) Elongation (%) Rz Wrinkle / Tear Occurrence Example 1 12.7 12.3 8 7.9 2 3.1 8 5 6.2 10.2 0.8 None Example 2 12.7 12.5 8 7.9 5 2.5 3 5 1.3 7.5 0.8 None Example 3 12.7 12.5 8 7.9 4 2.1 0 5 8.5 8.6 0.8 None Example 4 12.7 12.4 8 7.9 4 3.1 7 5 7.6 11.2 0.8 None Comparative Example 1 12.7 12.1 8 7.8 0 1.9 1 3 5.2 10.5 2.7 Occurrence Comparative Example 2 12.7 12.1 8 7 .781.7345.610.50.75 Occurrence Comparison Example 312.712.287.841.9832.710.33.1 Occurrence Comparison Example 412.712.387.851.651.010.60.8 Occurrence Comparison Example 512.712.287.821.734.511.12.8 Occurrence Comparison Example 612.712.487.881.534.69.52.7 Occurrence Comparison Example 712.71287.894.050.615.00.8 Occurrence
[0178]
[0179] For the copper foils of Examples 1-4 and Comparative Examples 1-7 manufactured in this manner, i) WA, ii) WB, iii) tA, iv) tB, v) R value, vi) tensile strength, vii) elongation, and viii) Rz value were measured and calculated, and ix) whether wrinkles / tears occurred was confirmed. i) WA, ii) WB measurements
[0180] The WA and WB of copper foil (110) are calculated using the following equations 2 and 3.
[0181] [Formula 2]
[0182] WA = [XA0+(XA45)X2+XA90] / 4
[0183] [Formula 3]
[0184] WB = [XB0+(XB45)X2+XB90] / 4
[0185] Copper foil (110) is sampled in three directions of 0°, 45°, and 90° from the MD direction, and an axial tensile test is performed on each sampled copper foil under the condition of a UTM tensile test speed of 5 mm / min. At this time, the tensile test is performed until the sampled copper foil grows 15% after tensile stretching compared to before tensile stretching. Then, the width of the central part of the tensile direction of the sampled copper foil before and after the tensile test is measured, respectively, and XA0, XA45, XA90, XB0, XB45, and XB90 of the following equations 2 and 3 can be calculated and produced.
[0186] At this time, XA0, XA45, and XA90 of the above formula 2 mean the width of the central part in the tensile direction before tension of the test piece taken in the 0°, 45°, and 90° directions. XB0, XB45, and XB90 of the above formula 3 mean the width of the central part in the tensile direction after tension of the test piece taken in the 0°, 45°, and 90° directions.
[0187] iii) tA, iv) tB measurements
[0188] tA is the thickness of the specimen measured before the tensile test, and tB is the thickness of the specimen measured after the tensile test.
[0189] At this time, the tensile test was conducted using a universal testing machine (UTM).
[0190] v) Calculate R
[0191] The R value can be obtained by calculating the measured i) WA, ii) WB, iii) tA and iv) tB values according to the following equation 1.
[0192] [Formula 1]
[0193] R = log(WA / WB) / log(tA / tB)
[0194] vi) Tensile strength measurement
[0195] Tensile strength is measured using a universal testing machine (UTM). The sample width is 12.7 mm, the distance between grips is 50 mm, and the test speed is 50 mm / min.
[0196] vii) Measurement of elongation
[0197] Elongation was measured using a universal testing machine (UTM) according to the specifications of the IPC-TM-650 Test Method Manual. Specifically, elongation was measured using an Instron universal testing machine. The sample width for elongation measurement was 12.7 mm, the grip-to-grip distance was 50 mm, and the measurement speed was 50 mm / min.
[0198] viii) 10-point surface roughness (Rz) measurement
[0199] The 10-point surface roughness (Rz) of copper foil was measured using a surface roughness measuring device (M300, Mahr) according to the JIS B 0601-2001 standard.
[0200] ix) Whether wrinkles / tears occur
[0201] After 100 charge-discharge cycles, the secondary battery was disassembled and the copper foil was observed for wrinkles or tears. If wrinkles or tears occurred in the copper foil, they were marked as "occurrence," and if no wrinkles or tears occurred, they were marked as "none."
[0202] Referring to Table 1 and Table 2, the following results can be confirmed.
[0203] Contains an excessive amount of polishing agent (component A) and lead ions (Pb 2+ ) and tungsten (W) in small amounts, tearing / wrinkling occurred in the copper foil of Comparative Example 1 manufactured by the electrolyte.
[0204] Contains excessive amounts of moderator (component B) and lead ions (Pb 2+ ) and tungsten (W) in small amounts, tearing / wrinkling occurred in the copper foil of Comparative Example 2 manufactured by the electrolyte.
[0205] Contains an excessive amount of leveling agent (component C) and lead ions (Pb 2+) and tungsten (W) in small amounts, tearing / wrinkling occurred in the copper foil of Comparative Example 3 manufactured by the electrolyte.
[0206] Contains trace amounts of polishing agent (component A) and lead ions (Pb 2+ ) and tungsten (W) in excess, and tearing / wrinkling occurred in the copper foil of Comparative Example 4 manufactured by an electrolyte containing an excess of hydrogen peroxide.
[0207] Contains a trace amount of moderator (component B) and lead ions (Pb 2+ ), tearing / wrinkling occurred in the copper foil of Comparative Example 5 manufactured using an electrolyte containing an excess of tungsten (W) and a trace amount of hydrogen peroxide.
[0208] Contains trace amounts of leveling agent (component C) and lead ions (Pb 2+ ) and tungsten (W) in excess, tearing / wrinkling occurred in the copper foil of Comparative Example 6 manufactured by the electrolyte.
[0209] Tearing / wrinkling occurred in the copper foil of Comparative Example 7 manufactured using an electrolyte containing trace amounts of a brightener (component A) and tungsten (W) and excess amounts of a moderator (component B) and a leveling agent (component C).
[0210] Example 5-10 and Comparative Example 8-11
[0211] Copper foil was manufactured using a foil maker including an electrolytic cell (10), a rotating cathode drum (40) placed in the electrolytic cell (10), and an anode plate (30) placed spaced apart from the rotating cathode drum (40). The electrolyte (20) is a copper sulfate solution. The concentration of copper ions in the electrolyte (20) was set to 87 g / L, the concentration of sulfuric acid was set to 110 g / L, the temperature of the electrolyte was set to 55°C, and the current density was set to 60 ASD.
[0212] In addition, the concentrations of chlorine (Cl), lead (Pb), hydrogen peroxide (H2O2), tungsten (W) and organic additives contained in the electrolyte (20) are as shown in Table 1 below.
[0213] Among the organic additives, bis-(3-sulfopropyl)-disulfide disodium salt (SPS) was used as a brightener (component A), polyethylene glycol (PEG) was used as a moderator (component B), and ethylene thiourea (ETU) was used as a leveling agent (component C).
[0214] A copper film (111) was manufactured by applying a current at a current density of 60 ASD between a rotating cathode drum (40) and an anode plate (30). Next, the copper film (111) was immersed in a rust-preventing solution for about 2 seconds to perform a chromate treatment on the surface of the copper film (111) to form a protective layer (112), thereby manufacturing a copper foil (110). A rust-preventing solution containing chromic acid as a main component was used, and the concentration of chromic acid was 5 g / L.
[0215] As a result, copper foils of Examples 5-10 and Comparative Examples 8-11 were manufactured.
[0216] Electrolyte current density (ASD) Electrolyte temperature (℃) SPS (component A) (ppm) PEG (component B) (ppm) ETU (C Ingredients) (ppm) Chlorine (ppm) Lead (ppm) Hydrogen Peroxide (ml / L) Tungsten (ppm) Example 5 5 2 3 2 0 3 0 2 1.06 0 55 Example 6 1 0 4 5 2 0 5 0 5 1.56 0 55 Example 7 1 5 6 7 2 0 6 0 7 1.56 0 55 Example 8 2 0 8 9 2 0 7 0 7 2.06 0 55 Example 9 1 3 5 4 2 0 5 0 7 2.06 0 55 Example 1 0 8 7 6 2 0 5 0 7 2.26 0 55 Comparative Example 8 5 5 5 2 0 19 0.16 0 55 Comparative Example 9 1 0 5 0 7 2 0 15 0 7 0.16 0 55 Comparative Example 10 1 5 7 5 5 2 0 15 0 5 10 6 0 55 Comparative Example 1 1 1 0 5 5 2 0 5 2.06 0 55
[0217]
[0218] Room temperature storage modulus (E') (GPa) Room temperature loss modulus (E") (GPa) Room temperature loss modulus (E" / E') High temperature storage modulus (E') (GPa) High temperature loss modulus (E") (GPa) High temperature loss modulus (E" / E') Wrinkle / tear occurrence Whether or not Implementation Example 544.000.980.022332.154.580.142None Implementation Example 658.122.790.048027.965.570.199None Implementation Example 764.381.680.026140.865.250.128None Implementation Example 865.061.670.025751.836.300.122None Implementation Example 954.291.740.032135.636.790.191None Implementation Example 1070.703.020.042732.614.680.144NoneComparison Example 842.783.150.073653.2110.820.203OccurrenceComparison Example 971.824.250.059258.4012.480.214OccurrenceComparison Example 1040.283.140.078025.444.220.166OccurrenceComparison Example 1172.323.870.053560.2413.840.230Occurrence
[0219]
[0220] For the copper foils of Examples 5-10 and Comparative Examples 8-11 manufactured in this manner, i) room temperature storage elastic modulus (E'), ii) room temperature loss elastic modulus (E"), iii) room temperature loss modulus, iv) high temperature storage elastic modulus (E'), v) high temperature loss modulus (E"), vi) high temperature loss modulus, and vii) occurrence of wrinkles / tears were confirmed. i) Room temperature storage elastic modulus (E'), ii) Room temperature loss modulus (E") were measured.
[0221] After cooling the copper foil (110) to 20°C using Seiko Exstar 6000 (DMA / SS6100) manufactured by Seiko, the temperature was increased to 500°C at a heating rate of 5°C / min, and the viscoelasticity was measured at a vibration frequency of 1 Hz.
[0222] From the obtained viscoelastic curve, the room temperature storage elastic modulus (E') and room temperature loss elastic modulus (E") at 25°C were calculated.
[0223] iii) Calculation of room temperature loss coefficient (E" / E')
[0224] The room temperature loss modulus (E" / E') can be obtained by calculating the measured i) room temperature storage elastic modulus (E") and ii) room temperature loss elastic modulus (E') values according to the following Equation 4.
[0225] [Formula 4]
[0226] Room temperature loss modulus = Room temperature loss modulus / Room temperature storage modulus
[0227] iv) Measurement of high temperature storage modulus (E'), v) high temperature loss modulus (E")
[0228] The high-temperature storage modulus (E') and high-temperature loss modulus (E") were measured in the same manner as i) the room-temperature storage modulus (E') and ii) the room-temperature loss modulus (E"), except that the measurements were made after heating at 350°C for 1 hour.
[0229] vi) Calculation of high temperature loss coefficient (E" / E')
[0230] The high temperature loss modulus (E" / E') can be obtained by calculating the measured values of iv) high temperature storage elastic modulus (E') and v) high temperature loss elastic modulus (E") according to the following equation 5.
[0231] [Formula 5]
[0232] High temperature loss modulus = High temperature loss modulus / High temperature storage modulus
[0233] vii) Whether wrinkles / tears occur
[0234] After 100 charge-discharge cycles, the secondary battery was disassembled and the copper foil was observed for wrinkles or tears. If wrinkles or tears occurred in the copper foil, they were marked as "occurrence," and if no wrinkles or tears occurred, they were marked as "none."
[0235] Referring to Tables 3 and 4, the following results can be confirmed.
[0236] Tearing / wrinkling occurred in the copper foil of Comparative Example 8 manufactured using an electrolyte containing an excessive amount of a brightener (component A) and trace amounts of lead and tungsten.
[0237] Tearing / wrinkling occurred in the copper foil of Comparative Example 9 manufactured using an electrolyte containing an excess amount of moderator (component B) and lead, and a trace amount of tungsten.
[0238] Tearing / wrinkling occurred in the copper foil of Comparative Example 10 manufactured using an electrolyte containing an excessive amount of leveling agent (component C), lead, and tungsten.
[0239] Tearing / wrinkling occurred in the copper foil of Comparative Example 11 manufactured using an electrolyte containing an excessive amount of leveling agent (component C) and hydrogen peroxide.
[0240] On the other hand, in the copper foils of Examples 5 to 10 of the present invention, all values satisfied the standard, and as a result, no tearing / wrinkling occurred in the copper foil.
[0241] The present invention described above is not limited to the aforementioned embodiments and the attached drawings, and it will be apparent to those skilled in the art that various substitutions, modifications, and changes are possible without departing from the technical scope of the present invention. Therefore, the scope of the present invention is expressed by the following claims, and all changes or modifications derived from the meaning, scope, and equivalent concepts of the claims should be interpreted as being included within the scope of the present invention.
Claims
A copper film comprising 99.9 wt% or more of copper; Copper foil with an R value in the range of 2.0 to 3.5: The above R is calculated by the following equation 1, [Formula 1] R = log(WA / WB) / log(tA / tB) WA of the above equation 1 is calculated by the following equation 2, [Formula 2] WA = [XA0+(XA45)X2+XA90] / 4 The WB of the above equation 1 is calculated by the following equation 3, [Formula 3] WB = [XB0+(XB45)X2+XB90] / 4 tA in the above equation 1 means the thickness of the test piece before the tensile test, tB in the above equation 1 means the thickness of the test piece after the tensile test, XA0, XA45, and XA90 in the above formula 2 represent the widths of the central portions of the tensile direction before tensile testing of the test specimens taken in the 0°, 45°, and 90° directions. XB0, XB45, and XB90 in the above formula 3 represent the widths of the central portions in the tensile direction after tension of the test specimens taken in the 0°, 45°, and 90° directions.
2. In paragraph 1, 45kgf / mm 2 Copper foil having a tensile strength of the above.
3. In paragraph 1, Copper foil having an elongation of 3 to 13%.
4. In paragraph 1, Copper foil having a 10-point average roughness (Rz) of 0.7 to 0.9㎛.
5. In paragraph 1, Copper foil further comprising a protective layer on the copper film.
6. In paragraph 5, A copper foil wherein the protective layer comprises at least one of a chromium compound, a silane compound, and a nitrogen compound.
7. A step of preparing an electrolyte containing copper ions; Step of forming a copper film; and A step of forming a protective layer on the copper film; including: The step of forming the above copper film is: It includes a step of forming a copper film on the rotating cathode drum by energizing the positive electrode plates and the rotating cathode drum, which are arranged spaced apart from each other in the electrolyte in the electrolytic cell, The above electrolyte is, 70 to 100 g / L of copper ions; 70 to 150 g / L sulfuric acid; 15 to 25 ppm chlorine (Cl); 1 to 100 ppm of lead ion (Pb) 2+ ); 0.3 to 5 ppm of tungsten (W); 1 to 10 ml / L of hydrogen peroxide; and Contains organic additives; The above organic additive comprises at least one of a brightener (component A), a reducer (component B), and a leveling agent (component C). The above polishing agent (component A) contains sulfonic acid or its metal salt, The above-mentioned moderator (component B) contains a nonionic water-soluble polymer, The above leveling agent (component C) contains at least one of nitrogen (N) and sulfur (S). Method for manufacturing copper foil.
8. In paragraph 7, A method for manufacturing copper foil, wherein the above-mentioned polishing agent (component A) has a content of 1 to 25 ppm.
9. In paragraph 7, A method for manufacturing copper foil, wherein the above-mentioned moderator (component B) has a content of 1 to 10 ppm.
10. In paragraph 7, A method for manufacturing copper foil, wherein the leveling agent (component C) has a content of 1 to 10 ppm. A copper film comprising 99.9 wt% or more of copper; The copper film has a room temperature loss coefficient of 0.05 or less, copper foil: The above room temperature loss coefficient is calculated using the following equation 4. [Formula 4] Room temperature loss modulus = Room temperature loss modulus / Room temperature storage modulus 12. In paragraph 11, The copper film has a high temperature loss coefficient of 0.2 or less, copper foil: The above high temperature loss coefficient is calculated using the following equation 5. [Formula 5] High temperature loss modulus = High temperature loss modulus / High temperature storage modulus 13. In paragraph 11, Copper foil having a room temperature storage elastic modulus in the range of 30 to 80 GPa.
14. In paragraph 11, Copper foil having a room temperature loss modulus of elasticity of 5 GPa or less.
15. In paragraph 12, Copper foil having a high temperature storage modulus of elasticity in the range of 20 to 60 GPa.
16. In paragraph 12, Copper foil having a high temperature loss modulus of elasticity of 10 GPa or less.
17. In paragraph 11, Copper foil further comprising a protective layer on the copper film.
18. In paragraph 17, A copper foil wherein the protective layer comprises at least one of a chromium compound, a silane compound, and a nitrogen compound.