Copper foil capable of preventing tear or wrinkle defects, electrode comprising same, secondary battery comprising same, and manufacturing method therefor
Patent Information
- Application Number
- MYPI2025002464
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-10-05
- Filing Date
- 2023-11-20
- Publication Date
- 2024-06-22
AI Technical Summary
The challenge is to develop a copper foil with high strength characteristics that prevents tearing and wrinkling during manufacturing, particularly for use in secondary batteries where thin copper foils are prone to curling and defects, affecting the battery's capacity and performance.
A copper foil with specific stress coefficient values (1.1 to 1.6, 2.8 to 3.2, and 2.5 to 3.0) and a protective layer is formed using an electrolyte solution containing copper ions, sulfuric acid, chlorine, nickel, and organic additives, ensuring high tensile strength and preventing curling, wrinkling, and tearing.
The solution results in a high-strength copper foil that prevents defects during manufacturing, enhancing the productivity and quality of secondary batteries by maintaining stable capacity and performance.
Smart Images

Figure PI2025002464_DRAWING_001 
Figure PI2025002464_DRAWING_002
Abstract
Description
Copper foil capable of preventing tearing or wrinkle defects, electrode including the same, secondary battery including the same, and method for manufacturing the same
[0001] The present invention relates to a copper foil capable of preventing tearing or wrinkle defects, an electrode including the same, a secondary battery including the same, and a method for manufacturing the same.
[0002] Secondary batteries are a type of energy conversion device that converts electrical energy into chemical energy, stores it, and then generates electricity by converting the chemical energy back into electrical energy when needed. They are used as an energy source for portable appliances such as cell phones and laptops, as well as electric vehicles. Secondary batteries are also referred to as rechargeable batteries because they can be recharged.
[0003] Secondary batteries that have economic and environmental advantages over disposable primary batteries include lead-acid batteries, nickel-cadmium secondary batteries, nickel-hydrogen secondary batteries, and lithium secondary batteries.
[0004] In particular, lithium secondary batteries can store a relatively large amount of energy relative to their size and weight compared to other secondary batteries. Therefore, lithium secondary batteries are preferred in the information and communication device sector, where portability and mobility are crucial. Their application is also expanding to include energy storage devices for hybrid and electric vehicles.
[0005] Lithium secondary batteries are used repeatedly, with charging and discharging forming a single cycle. When operating a device with a fully charged lithium secondary battery, the lithium-ion secondary battery must possess high charge / discharge capacity to extend the device's operating time. Therefore, research is continually needed to meet consumers' ever-increasing expectations for the charge / discharge capacity of lithium secondary batteries.
[0006] These secondary batteries include anode current collectors made of copper foil. Among these copper foils, electrolytic copper foil is widely used as the anode current collector of secondary batteries. With the increasing acceptance of secondary batteries and the growing demand for high-capacity, high-efficiency, and high-quality secondary batteries, there is a growing demand for electrolytic copper foils that can enhance the characteristics of secondary batteries. In particular, there is a need for electrolytic copper foils that can ensure high capacity, stable capacity maintenance, and performance of secondary batteries.
[0007] Electrolytic copper foil, used as the negative current collector of secondary batteries, can accommodate a larger amount of active material as it becomes thinner, increasing the capacity of the secondary battery. However, thinner copper foil also reduces strength, making handling difficult and increasing the risk of fracture. Therefore, tensile strength becomes even more important in ultra-thin copper foils. Furthermore, metal-based and composite-based active materials, which have recently gained popularity for high-capacity applications, exhibit significant volume expansion, necessitating the development of high-strength electrolytic copper foils capable of handling this phenomenon.
[0008] Meanwhile, as the thickness of the copper foil becomes thinner, the amount of active material that can be contained in the same space increases, and the number of current collectors can increase, which can increase the capacity of the secondary battery. However, as the copper foil becomes thinner, curling occurs, and defects such as tearing or wrinkles in the copper foil due to edge curling during winding of the copper foil occur, making it difficult to manufacture copper foil in the form of a very thin film. Therefore, in order to manufacture copper foil with a very thin thickness, curling of the copper foil must be prevented.
[0009] Accordingly, the present invention relates to a copper foil, an electrode including the copper foil, a secondary battery including the copper foil, and a method for manufacturing the copper foil, which can prevent problems caused by the limitations and disadvantages of the above-mentioned related technologies.
[0010] One embodiment of the present invention seeks to provide a copper foil having high strength characteristics by having an A value in the range of 1.1 to 1.6.
[0011] One embodiment of the present invention is to provide a copper foil having an A value in the range of 1.1 to 1.6, which does not cause curling, wrinkling or tearing during the manufacturing process.
[0012] One embodiment of the present invention seeks to provide a copper foil that does not wrinkle or tear by having a first stress coefficient value in the range of 2.8 to 3.2.
[0013] One embodiment of the present invention seeks to provide a copper foil that does not wrinkle or tear by having a second stress coefficient value in the range of 2.5 to 3.0.
[0014] One embodiment of the present invention seeks to provide a copper foil that does not wrinkle or tear by having a third stress coefficient value in the range of 3.5 to 4.5.
[0015] Another embodiment of the present invention provides an electrode for a secondary battery including such a copper foil, and a secondary battery including such a secondary battery electrode.
[0016] Another embodiment of the present invention is to provide a method for manufacturing a copper foil that prevents occurrence of drying, wrinkling or tearing.
[0017] In addition to the aspects of the present invention mentioned above, other features and advantages of the present invention will be described below or will be clearly understood by those skilled in the art to which the present invention pertains from such description.
[0018] One embodiment of the present invention provides a copper foil comprising a copper film comprising 99.9 wt% or more of copper, wherein the copper film has an A value in a range of 1.1 to 1.6. The A is calculated by the following Equation 1, [Equation 1] A = P / Q, where P in Equation 1 is the peak intensity of the copper film at 1650 cm-1, and Q in Equation 1 is the peak intensity of the copper film at 1460 cm-1, and the peak intensity is measured by FT-IR.
[0019] One embodiment of the present invention provides a copper foil comprising a copper film comprising 99.9 wt% or more of copper, having a first stress factor in a range of 2.8 to 3.2, a second stress factor in a range of 2.5 to 3.0, and a third stress factor in a range of 3.5 to 4.5. At this time, the first stress coefficient is calculated by the following equation 2, [Equation 2] First stress coefficient = A / A' + B / B'+C / C' The second stress coefficient is calculated by the following equation 3, [Equation 3] Second stress coefficient = A / B + A' / B' The third stress coefficient is calculated by the following equation 4, [Equation 4] Third stress coefficient = A / C + A' / C' A in the equation 1 is the stress at 50% elongation in the MD direction, A' in the equation 2 is the stress at 50% elongation in the TD direction, B in the equation 2 is the stress at 10% elongation in the MD direction, B' in the equation 2 is the stress at 10% elongation in the TD direction, C in the equation 2 is the stress at 5% elongation in the MD direction, and C' in the equation 2 is the stress at 5% elongation in the TD direction.
[0020] Another embodiment of the present invention comprises the steps of: preparing an electrolyte containing copper ions; forming a copper film; and forming a protective layer on the copper film, wherein the step of forming the copper film comprises the step of forming a copper film on the rotating cathode drum by conducting current between a positive electrode plate and a rotating cathode drum, which are spaced apart from each other in an electrolyte in an electrolytic cell, and the electrolyte comprises: 70 to 100 g / L of copper ions; 70 to 150 g / L of sulfuric acid; 15 to 25 ppm of chlorine (Cl); 15 to 150 ppm of nickel (Ni); and 1 to 20 ppm of lead ions (Pb). 2+ ); 1 to 10 ml / L of hydrogen peroxide; 0.3 to 5 ppm of tungsten (W); and an organic additive; wherein the organic additive comprises at least one of a brightener (component A), a moderator (component B), a leveling agent (component C), and a softener (component D), wherein the brightener (component A) comprises sulfonic acid or a metal salt thereof, the moderator (component B) comprises a nonionic water-soluble polymer, the leveling agent (component C) comprises at least one of nitrogen (N) and sulfur (S), and the softener (component D) comprises citric acid.
[0021] According to another embodiment of the present invention, an electrode for a secondary battery is provided, comprising: copper foil; and an active material layer disposed on at least one surface of the copper foil.
[0022] According to another embodiment of the present invention, a secondary battery is provided, including: a cathode that provides lithium ions when charged; an anode that provides electrons and lithium ions when discharged; an electrolyte that is disposed between the cathode and the anode and provides an environment in which lithium ions can move; and a separator that electrically insulates the cathode and the anode.
[0023] According to the present invention, it is possible to produce a high-strength copper foil that can prevent the occurrence of wrinkles or tears during the manufacturing process of copper foil, and by using this high-strength copper foil to manufacture intermediate parts and final products such as flexible printed circuit boards (FPCBs) and secondary batteries, it is possible to improve the productivity of the intermediate parts as well as the final products.
[0024] Figure 1 is a cross-sectional view of a copper foil according to one embodiment of the present invention.
[0025] Figure 2 is a cross-sectional view of a copper foil according to another embodiment of the present invention.
[0026] Figure 3 is a cross-sectional view of an electrode for a secondary battery according to another embodiment of the present invention.
[0027] Figure 4 is a cross-sectional view of an electrode for a secondary battery according to another embodiment of the present invention.
[0028] Figure 5 is a schematic cross-sectional view of a secondary battery according to another embodiment of the present invention.
[0029] Figure 6 is a device for manufacturing copper foil according to another embodiment of the present invention.
[0030] Figure 7 is a drawing for explaining MD and TD of the copper foil of the present invention.
[0031] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings. However, the embodiments described below are presented for illustrative purposes only to facilitate a clear understanding of the present invention and do not limit the scope of the present invention.
[0032] The shapes, sizes, ratios, angles, numbers, etc. disclosed in the drawings for explaining embodiments of the present invention are merely illustrative, and the present invention is not limited to the details depicted in the drawings. Throughout the specification, identical components may be designated by identical reference numerals. In describing the present invention, detailed descriptions of related known technologies will be omitted if they are deemed to unnecessarily obscure the gist of the present invention.
[0033] In this specification, where "includes," "has," and "consists of" are used, other parts may be added, unless the expression "only" is used. When a component is expressed in the singular, the plural is included unless otherwise explicitly stated. Furthermore, when interpreting a component, it is interpreted to include a margin of error even if there is no explicit indication otherwise.
[0034] When describing a positional relationship, for example, when the positional relationship between two parts is described as 'on top of', 'upper part of', 'lower part of', 'next to', etc., one or more other parts may be located between the two parts, unless the expression 'right' or 'directly' is used.
[0035] Spatially relative terms such as "below," "beneath," "lower," "above," and "upper" can be used to easily describe the relationship of one element or component to another, as illustrated in the drawings. Spatially relative terms should be understood to include different orientations of the elements during use or operation in addition to the orientations depicted in the drawings. For example, if an element depicted in the drawings were flipped over, an element described as "below" or "beneath" another element could instead be positioned "above" the other element. Thus, the exemplary term "below" can encompass both the above and below directions. Similarly, the exemplary term "above" or "above" can encompass both the above and below directions.
[0036] When describing a temporal relationship, for example, when the temporal relationship is described as 'after', 'following', 'next to', 'before', etc., it can also include cases where it is not continuous, as long as the expression 'immediately' or 'directly' is not used.
[0037] While terms like "first" and "second" are used to describe various components, these components are not limited by these terms. These terms are used merely to distinguish one component from another. Therefore, a "first" component referred to below may also be a "second" component within the technical scope of the present invention.
[0038] The term "at least one" should be understood to include all possible combinations of one or more associated items. For example, "at least one of the first, second, and third items" can mean not only the first, second, or third items, but also any combination of items that can be represented by two or more of the first, second, and third items.
[0039] The features of each of the various embodiments of the present invention can be partially or wholly combined or combined with each other, and various technical connections and operations are possible, and each embodiment can be implemented independently of each other or implemented together in a related relationship.
[0040] Figure 1 is a cross-sectional view of a copper foil (110) according to one embodiment of the present invention.
[0041] Referring to FIG. 1, the copper foil (110) of the present invention includes a copper film (111) containing 99.9 wt% or more of copper and a protective layer (112) on the copper film (111). In the copper foil (110) illustrated in FIG. 1, the protective layer (112) is formed on one surface of the copper film (111), but embodiments of the present invention are not limited thereto. Referring to FIG. 2, the protective layer (112) may be formed on both surfaces of the copper film (111).
[0042] A copper film (111) can be formed on a rotating cathode drum through electroplating, and has a shiny side that directly contacts the rotating cathode drum during the electroplating process and a matte side on the opposite side.
[0043] The protective layer (112) is formed by depositing an anticorrosion material on the copper film (111). The anticorrosion material may include at least one of a chromium compound, a silane compound, and a nitrogen compound. The protective layer (112) prevents oxidation and corrosion of the copper film (111) and improves heat resistance, thereby extending the lifespan of the copper foil (110) itself as well as the lifespan of the final product including it.
[0044] According to one embodiment of the present invention, the copper film (111) has an A value in the range of 1.1 to 1.6. The A value can be obtained by measuring and calculating P and Q, respectively, and calculating the measured and calculated values of P and Q according to the following Equation 1.
[0045] [Formula 1]
[0046] A = P / Q
[0047] P in the above formula 1 is 1650 cm of copper film (111). -1 It means the peak intensity at , and Q in the above equation 1 is 1460 cm of the copper film (111). -1 It means the peak intensity in . At this time, the peak intensity is measured by FT-IR.
[0048] 1650cm -1 The peak intensity at 1460 cm represents the intensity due to C=O stretching vibration within the copper film (111). -1 The peak intensity in refers to the intensity due to the bending vibration of CH within the copper film (111).
[0049] According to one embodiment of the present invention, the copper film (111) may have an A value in the range of 1.1 to 1.6.
[0050] When the A value of the copper film (111) is less than 1.1, the Q value of the copper film (111) (1460 cm -1 P value (1650 cm) vs. peak intensity -1 Peak intensity) is small, and the P value (1650 cm -1When the peak strength) is small, the proportion of C=O bonds within the copper film (111) may be small. The C=0 bonds within the copper film (111) are functional groups that enable hydrogen bonding. Therefore, when the proportion of C=0 bonds that enable hydrogen bonding is small, the proportion of hydrogen bonds within the copper film (111) may be small, making it difficult to obtain a copper foil with high strength characteristics. In addition, folding of the copper foil (110) may occur, or wrinkles may form at the left and right ends of the copper foil (110) during the roll-to-roll manufacturing process.
[0051] On the other hand, when the A value of the copper film (111) exceeds 1.6, the Q value of the copper film (111) (1460 cm -1 P value (1650 cm) vs. peak intensity -1 Peak intensity) is very large, and the P value (1650 cm -1 When the peak intensity) is very large, the proportion of C=O bonds within the copper film (111) may be very large. When the proportion of C=O bonds that enable hydrogen bonding within the copper film (111) is very large, the copper foil (110) has low elongation, which may cause breakage of the copper foil (110) during the manufacturing process of final products such as a negative electrode current collector of a secondary battery and a flexible printed circuit board (FPCB).
[0052] Therefore, in order to have high strength characteristics, the A value of the copper film (111) needs to be in the range of 1.1 to 1.6.
[0053] According to one embodiment of the present invention, the copper foil (110) has a first stress coefficient value in the range of 2.8 to 3.2. The first stress coefficient value can be obtained by measuring and calculating A, A', B, B', C, and C', respectively, and calculating the measured values of A, A', B, B', C, and C' according to the following equation 2.
[0054] [Formula 2]
[0055] First stress factor = A / A' + B / B' + C / C'
[0056] In the above equation 2, A represents the stress at 50% elongation in the MD direction of the copper foil (110), A' represents the stress at 50% elongation in the TD direction of the copper foil (110), B represents the stress at 10% elongation in the MD direction of the copper foil (110), B' represents the stress at 10% elongation in the TD direction of the copper foil (110), C represents the stress at 5% elongation in the MD direction, and C' represents the stress at 5% elongation in the TD direction. At this time, A, A', B, B', C, and C' are measured using a universal tensile tester (UTM).
[0057] Referring to Fig. 7, there are MD (Machine direction: machine direction or length direction) and TD (Transverse direction: width direction), and the surface properties of the machine direction and the transverse direction are different from each other. The copper foil (110) according to one embodiment of the present invention is characterized by minimizing the difference between the surface properties of the machine direction (MD) and the transverse direction (TD).
[0058] According to one embodiment of the present invention, the copper foil (110) may have a first stress coefficient value of 2.8 or more.
[0059] When the first stress coefficient value of the copper foil (110) is less than 2.8, the stress difference in the MD direction and the TD direction during elongation of the copper foil (110) may increase. As a result, wrinkles or tears may occur during the manufacturing process of the copper foil (110), and pinholes or curls may occur on the surface of the copper foil (110). As a result, workability may deteriorate, and the failure rate of the secondary battery may increase.
[0060] Therefore, in order to prevent wrinkles or tears from occurring during the manufacturing process of the copper foil (110), the first stress coefficient value of the copper foil (110) needs to be 2.8 or more.
[0061] According to one embodiment of the present invention, the copper foil (110) may have a second stress coefficient value of 2.5 or more.
[0062] The second stress coefficient value can be obtained by measuring and calculating A, A', B, and B', respectively, and calculating the measured values of A, A', B, and B' according to the following equation 3.
[0063] [Formula 3]
[0064] Second stress factor = A / B + A' / B'
[0065] When the second stress coefficient value of the copper foil (110) is less than 2.5, a stress difference may occur in the MD direction and the TD direction when the copper foil (110) is stretched by 10% and 50%. As a result, wrinkles or tears may occur during the manufacturing process of the copper foil (110), and pinholes or curls may occur on the surface of the copper foil (110). As a result, the charge / discharge efficiency of the negative electrode material may decrease, or workability may decrease, which may increase the failure rate of the secondary battery.
[0066] Therefore, in order to prevent wrinkles or tears from occurring during the manufacturing process of the copper foil (110), the second stress coefficient value of the copper foil (110) needs to be 2.5 or more.
[0067] According to one embodiment of the present invention, the copper foil (110) may have a third stress coefficient of 3.5 or more.
[0068] The third stress coefficient value can be obtained by measuring and calculating A, A', C and C', respectively, and calculating the measured values of A, A', C and C' according to the following equation 4.
[0069] [Formula 4]
[0070] Third stress factor = A / C + A' / C'
[0071] When the third stress coefficient value of the copper foil (110) is less than 3.5, a stress difference may occur in the MD direction and the TD direction when the copper foil (110) is stretched by 5% and 10%. As a result, wrinkles or tears may occur during the manufacturing process of the copper foil (110), and pinholes or curls may occur on the surface of the copper foil (110). Accordingly, the charge / discharge efficiency of the negative electrode material may decrease, or workability may decrease, and the failure rate of the secondary battery may increase.
[0072] Therefore, in order to prevent wrinkles or tears from occurring during the manufacturing process of the copper foil (110), the third stress coefficient value of the copper foil (110) needs to be 3.5 or more.
[0073] According to one embodiment of the present invention, the copper foil (110) may have a Vickers hardness in the range of 1.3 to 1.9 Hv.
[0074] When the Vickers hardness of the copper foil is less than 1.3 Hv, the copper foil (110) may be folded between two adjacent rolls during the roll-to-roll manufacturing process, or wrinkles may be formed at the left and right ends of the copper foil (110) during the roll-to-roll manufacturing process.
[0075] On the other hand, if the Vickers hardness of the copper foil (110) exceeds 1.9 Hv, the copper foil (110) has low elongation, which may cause breakage of the copper foil (110) during the manufacturing process of final products such as a negative electrode current collector of a secondary battery or a flexible printed circuit board (FPCB). Therefore, it is preferable to have a Vickers hardness of 1.5 to 1.7 Hv.
[0076] According to one embodiment of the present invention, the copper foil (110) has a thickness of 4 to 35 μm. When the copper foil (110) is used as a current collector of an electrode in a secondary battery, the thinner the copper foil (110), the more current collectors can be accommodated within the same space, which is advantageous for increasing the capacity of the secondary battery. However, the manufacture of a copper foil (110) having a thickness of less than 4 μm causes a decrease in workability.
[0077] On the other hand, when manufacturing a secondary battery with copper foil (110) exceeding 35 ㎛, it becomes difficult to achieve high capacity due to the thick copper foil (110).
[0078] According to one embodiment of the present invention, the copper foil (110) is 45 kg / mm 2 It can have a tensile strength of 45 kg / mm. In order to suppress wrinkles and tearing of the copper foil (110), the copper foil (110) of the present invention has a tensile strength of 45 kg / mm. 2 It has a high tensile strength of 45 kg / mm. The tensile strength of copper foil (110) is 45 kg / mm. 2 If it is less than this, folding of the copper foil (110) occurs between two adjacent rolls during the roll-to-roll manufacturing process, or wrinkles occur at the left and right ends of the copper foil (110) during the roll-to-roll manufacturing process.
[0079] The copper foil (110) according to one embodiment of the present invention may have an elongation of 3 to 13%.
[0080] If the elongation of the copper foil (110) is less than 3%, when the copper foil (110) is used as a current collector of a secondary battery, there is a high risk that the copper foil (110) will not be sufficiently stretched to respond to the large volume expansion of the high-capacity active material and will tear.
[0081] On the other hand, if the elongation of the copper foil (110) exceeds 13%, the copper foil (110) may easily elongate during the secondary battery electrode manufacturing process, causing deformation of the electrode.
[0082] According to one embodiment of the present invention, the copper foil (110) may have a 10-point average roughness (Rz) of 0.7 to 0.9 μm.
[0083] As the charge and discharge of the secondary battery is repeated, the active material layer alternately contracts and expands, which causes separation of the active material layer and the copper foil (110), thereby reducing the charge and discharge efficiency of the secondary battery. Therefore, in order for the secondary electrode to secure a certain level of capacity retention rate and lifespan (i.e., to suppress the reduction in the charge and discharge efficiency of the secondary battery), the copper foil (110) must have excellent coating properties for the active material, thereby increasing the adhesive strength between the copper foil (110) and the active material layer.
[0084] Specifically, the smaller the 10-point average roughness (Rz) of the copper foil (110), the less the charge / discharge efficiency of the secondary battery including the copper foil (110) tends to deteriorate. Therefore, according to one embodiment of the present invention, the copper foil (110) has a 10-point average roughness (Rz) of 0.7 to 0.9 μm.
[0085] When the 10-point average roughness (Rz) of the copper foil (110) is less than 0.7, the surface area of the copper foil (110) is relatively small, so the active material is easily detached from the copper foil (110), and as a result, a rapid decrease in the lifespan of the secondary battery occurs due to repeated charging and discharging.
[0086] On the other hand, when the 10-point average roughness (Rz) of the copper foil (110) exceeds 0.9, the contact uniformity between the copper foil (110) and the active material layer does not reach a certain level, so that a large number of spaces exist between the copper foil (110) and the active material layer (i.e., the coating itself is not partially formed), and as a result, a rapid decrease in the lifespan of the secondary battery is caused due to repeated charge and discharge.
[0087] Hereinafter, an electrode (100) including a copper foil (110) of the present invention and a secondary battery including the electrode (100) will be described in detail.
[0088] Figure 3 is a cross-sectional view of an electrode for a secondary battery according to one embodiment of the present invention.
[0089] As illustrated in FIG. 3, an electrode (100) for a secondary battery according to one embodiment of the present invention includes a copper foil (110) and an active material layer (120) of any one of the embodiments of the present invention described above.
[0090] Figure 3 illustrates a configuration in which an active material layer (120) is formed on one side of a copper foil (110). However, one embodiment of the present invention is not limited thereto, and with reference to Figure 4, the active material layer (120) may be formed on both sides of the copper foil (110).
[0091] In lithium secondary batteries, aluminum foil is generally used as a positive electrode current collector combined with a positive electrode active material, and copper foil (110) is generally used as a negative electrode current collector combined with a negative electrode active material.
[0092] According to one embodiment of the present invention, the secondary battery electrode (100) is a negative electrode, the copper foil (110) is used as a negative electrode current collector, and the active material layer (120) includes a negative electrode active material.
[0093] In order to secure high capacity of the secondary battery, the active material layer (120) of the present invention may be formed of a composite of carbon and metal. The metal may include, for example, at least one of Si, Ge, Sn, Li, Zn, Mg, Cd, Ce, Ni, and Fe, preferably Si and / or Sn.
[0094] Figure 5 is a schematic cross-sectional view of a secondary battery according to one embodiment of the present invention.
[0095] Referring to FIG. 5, the secondary battery includes a cathode (370), an anode (340), an electrolyte (350) disposed between the anode (370) and the cathode (340) to provide an environment in which ions can move, and a separator (360) that electrically insulates the anode (370) and the cathode (340). Here, the ions that move between the anode (370) and the cathode (340) are, for example, lithium ions. The separator (360) separates the cathode (370) and the anode (340) to prevent charges generated at one electrode from being unnecessarily consumed by moving to the other electrode through the interior of the secondary battery (105). Referring to FIG. 5, the separator (360) is disposed within the electrolyte (350).
[0096] The positive electrode (370) includes a positive electrode current collector (371) and a positive electrode active material layer (372), and aluminum foil can be used as the positive electrode current collector (371).
[0097] The negative electrode (340) includes a negative electrode current collector (341) and a negative electrode active material layer (342), and copper foil (110) can be used as the negative electrode current collector (341).
[0098] According to one embodiment of the present invention, the copper foil (110) disclosed in FIG. 1 or FIG. 2 may be used as the negative electrode current collector (341). In addition, the secondary battery electrode (100) illustrated in FIG. 3 or FIG. 4 may be used as the negative electrode (340) of the secondary battery illustrated in FIG. 5.
[0099] Hereinafter, the method for manufacturing the copper foil (110) of the present invention will be specifically described with reference to FIG. 6.
[0100] The method for manufacturing copper foil (110) of the present invention includes a step of forming a copper film (111) and a step of forming a protective layer (112) on the copper film (111).
[0101] The method of the present invention includes a step of forming a copper film (111) on the rotating cathode drum (40) by energizing the anode plates (30) and the rotating cathode drum (40) which are spaced apart from each other in the electrolyte (20) in the electrolytic cell (10).
[0102] As illustrated in FIG. 6, the bipolar plate (30) may include first and second bipolar plates (31, 32) that are electrically insulated from each other.
[0103] The copper film (111) formation step can be performed by forming a seed layer by conducting current between the first positive electrode plate (31) and the rotating negative electrode drum (40), and then growing the seed layer by conducting current between the second positive electrode plate (32) and the rotating negative electrode drum (40).
[0104] The current density provided by the first and second bipolar plates (31, 32) may be 30 to 130 ASD, respectively.
[0105] When the current density provided by the first and second positive electrode plates (31, 32) is less than 30 ASD, the surface roughness of the copper foil (110) may be low, and the adhesion between the copper foil (110) and the active material layer (120) may not be sufficient.
[0106] On the other hand, if the current density provided by the first and second positive electrode plates (31, 32) exceeds 130 ASD, the surface of the copper foil (110) may be rough, so that the coating of the active material may not be performed smoothly.
[0107] The surface properties of the copper film (111) may vary depending on the degree of surface buffing or polishing of the rotating cathode drum (40). For example, the surface of the rotating cathode drum (40) may be polished with a polishing brush having a grit size of #800 to #3000.
[0108] During the copper film (111) formation process, the electrolyte (20) is maintained at a temperature of 48 to 60°C. More specifically, the temperature of the electrolyte (20) can be maintained at 50°C or higher. At this time, the physical, chemical, and electrical properties of the copper film (111) can be controlled by adjusting the composition of the electrolyte (20).
[0109] According to one embodiment of the present invention, the electrolyte (20) contains 70 to 100 g / L of copper ions, 70 to 150 g / L of sulfuric acid, 15 to 25 ppm of chlorine (Cl), 15 to 150 ppm of nickel (Ni), and 1 to 20 ppm of lead ions (Pb). 2+ ), 1 to 10 ml / L of hydrogen peroxide (H2O2), 0.3 to 5 ppm of tungsten (W) and organic additives.
[0110] In order to facilitate the formation of a copper film (111) by copper electrodeposition, the concentration of copper ions and the concentration of sulfuric acid in the electrolyte (20) are adjusted to 70 to 100 g / L and 70 to 150 g / L, respectively.
[0111] In one embodiment of the present invention, chlorine (Cl) includes both chlorine ions (Cl-) and chlorine atoms present in the molecule. Chlorine (Cl) can be used, for example, to remove silver (Ag) ions introduced into the electrolyte (20) during the process of forming a copper film (111). Specifically, chlorine (Cl) can precipitate silver (Ag) ions in the form of silver chloride (AgCl). This silver chloride (AgCl) can be removed by filtration.
[0112] When the concentration of chlorine (Cl) is less than 15 ppm, the removal of silver (Ag) ions is not smoothly performed. On the other hand, when the concentration of chlorine (Cl) exceeds 25 ppm, an unnecessary reaction due to excessive chlorine (Cl) may occur. Therefore, the concentration of chlorine (Cl) in the electrolyte (20) is managed in the range of 15 to 25 ppm.
[0113] According to one embodiment of the present invention, the electrolyte (20) including an organic additive may further include hydrogen peroxide (H2O2). Organic impurities exist in the electrolyte (20) that is continuously plated due to the organic additive, and by treating with hydrogen peroxide (H2O2), the organic impurities are decomposed, so that the carbon (C) content inside the copper foil can be appropriately controlled. As the TOC concentration in the electrolyte (20) increases, the amount of carbon (C) element flowing into the copper film (111) increases, and accordingly, the total amount of elements released from the copper film (111) during heat treatment increases, which causes the strength of the copper foil (110) to decrease after the heat treatment.
[0114] According to one embodiment of the present invention, the electrolyte (20) including an organic additive may further include hydrogen peroxide (H2O2). Organic impurities exist in the electrolyte (20) that is continuously plated due to the organic additive, and by treating with hydrogen peroxide (H2O2), the organic impurities are decomposed, so that the carbon (C) content inside the copper foil can be appropriately controlled. As the TOC concentration in the electrolyte (20) increases, the amount of carbon (C) element flowing into the copper film (111) increases, and accordingly, the total amount of elements released from the copper film (111) during heat treatment may increase. As a result, the first stress coefficient, second stress coefficient, and third stress coefficient values to be obtained may not be obtained, and as a result, wrinkles or tears may occur, and pinholes or curls may occur on the surface of the copper foil (110).
[0115] The amount of hydrogen peroxide (H2O2) added is 1 to 10 ml per L of electrolyte. Specifically, it is preferable to add 2 to 8 ml per L of electrolyte. If the amount of hydrogen peroxide (H2O2) added is less than 1 ml / L, it is meaningless because the effect of decomposing organic impurities is almost nonexistent. If the amount of hydrogen peroxide (H2O2) added exceeds 10 ml / L, organic impurities are excessively decomposed, and the effect of organic additives such as brighteners, moderators, and leveling agents is also suppressed.
[0116] The amount of hydrogen peroxide (H2O2) to be added is 1 to 10 ml per L of electrolyte. Specifically, it is preferable to add 2 to 8 ml of hydrogen peroxide (H2O2) per L of electrolyte. When the amount of hydrogen peroxide (H2O2) added is less than 1 ml / L, the effect of decomposing organic impurities is almost absent, so that the amount of carbon (C) elements introduced into the copper film (111) increases, and accordingly, the amount of the total elements released from the copper film (111) during heat treatment may increase. As a result, the desired first stress coefficient, second stress coefficient, and third stress coefficient values may not be obtained, and as a result, wrinkles or tears may occur, and pinholes or curls may occur on the surface of the copper foil (110).
[0117] According to one embodiment of the present invention, the electrolyte (20) including an organic additive may further include tungsten (W). When tungsten (W) is treated in the electrolyte (20), the average size of crystalline particles included in the copper film (111) may decrease, and the strength of the copper foil (110) may increase. The concentration of tungsten (W) in the electrolyte (20) may be 0.3 to 5 ppm. Specifically, it is preferable to add 1 to 4 ppm of tungsten (W).
[0118] When the amount of tungsten (W) added is less than 0.3 ppm, the average crystalline particle size of the copper film (111) may not be sufficiently small, and the A value of the copper film (111) may become lower than 1.1. As a result, the strength of the copper foil (110) may be reduced. In addition, folding of the copper foil (110) may occur, or wrinkles may form at the left and right ends of the copper foil (110) during the roll-to-roll manufacturing process.
[0119] On the other hand, if the amount of tungsten (W) added exceeds 5 ppm, the amount of impurities increases, which may suppress the effect of the organic additive. As a result, a problem may arise in which the A value of the copper film (111) falls outside the range of 1.1 to 1.6.
[0120] When the amount of tungsten (W) added is less than 0.3 ppm, the average crystalline grain size of the copper film (111) is not sufficiently small, and the strength of the copper foil (110) is reduced. In addition, the average crystalline grain size of the copper film (111) becomes non-uniform, and the desired first stress coefficient, second stress coefficient, and third stress coefficient values may not be obtained, and as a result, wrinkles or tears may occur, and pinholes or curls may occur on the surface of the copper foil (110).
[0121] On the other hand, if the amount of tungsten (W) added exceeds 5 ppm, the amount of impurities increases, which may inhibit the effect of the organic additive. In addition, due to the excessive amount of impurities, the stress value of the copper foil (110) may fluctuate rapidly. As a result, the desired first stress coefficient, second stress coefficient, and third stress coefficient values may not be obtained, and as a result, wrinkles or tears may occur, and pinholes or curls may occur on the surface of the copper foil (110).
[0122] According to one embodiment of the present invention, the electrolyte (20) including an organic additive contains 1 to 20 ppm of lead ions (Pb 2+) may further include lead ions (Pb) in the electrolyte (20). 2+ ) is managed at a concentration of 00 to 20 ppm. Lead ion (Pb 2+ ) A material that does not contain lead (Pb) can be used as a raw material added to the electrolyte (20) to maintain the concentration.
[0123] Lead ion (Pb 2+ ) is less than 1 ppm, a problem of reduced effectiveness in maintaining the properties of the present invention may occur. As a result, the 1460 cm of the copper film (111) -1 and 1650cm -1 A fluctuation in peak intensity may occur, causing a problem in which the A value of the copper film (111) falls outside the range of 1.1 to 1.6.
[0124] Lead ion (Pb 2+ ) exceeds 20 ppm, use an ion exchange filter to remove lead ions (Pb 2+ ) must be removed from the electrolyte (20), and copper is deposited unevenly, thereby causing a 1460 cm thick copper film (111). -1 and 1650cm -1 A fluctuation in peak intensity may occur, causing a problem in which the A value of the copper film (111) falls outside the range of 1.1 to 1.6.
[0125] Lead ion (Pb 2+ ) is less than 1 ppm, a problem of reduced effectiveness in maintaining the properties of the present invention may occur. As a result, the desired first stress coefficient, second stress coefficient, and third stress coefficient values may not be obtained, and as a result, wrinkles or tears may occur, and pinholes or curls may occur on the surface of the copper foil (110).
[0126] Lead ion (Pb 2+ ) exceeds 20 ppm, use an ion exchange filter to remove lead ions (Pb 2+) must be removed from the electrolyte (20), and copper may be unevenly deposited, causing wrinkles or tears, and pinholes or curls may occur on the surface of the copper foil (110). In addition, due to the uneven deposition of copper, a rapid change may occur in the stress value of the copper foil (110). As a result, the desired first stress coefficient, second stress coefficient, and third stress coefficient values may not be obtained, and as a result, wrinkles or tears may occur, and pinholes or curls may occur on the surface of the copper foil (110).
[0127] According to one embodiment of the present invention, the electrolyte (20) including the organic additive may further include nickel (Ni) in a range of 15 to 150 ppm. Nickel (Ni) in the electrolyte (20) is managed at a concentration in a range of 15 to 150 ppm.
[0128] When the concentration of nickel (Ni) exceeds 150 ppm, a problem may occur in which the A value of the copper film (111) becomes lower than 1.1, and as a result, the strength of the copper foil (110) is reduced, making it difficult to manufacture a high-strength copper foil (110).
[0129] On the other hand, when the concentration of nickel (Ni) is less than 15 ppm, a problem may occur in which the A value of the copper film (111) becomes lower than 1.1, and as a result, the strength of the copper foil (110) may be reduced, and curls may occur on the surface of the copper foil (110).
[0130] When the concentration of nickel (Ni) exceeds 150 ppm, the strength of the copper foil (110) is reduced, making it difficult to manufacture a high-strength copper foil (110). In addition, the stress value of the copper foil (110) may fluctuate rapidly. As a result, the desired first stress coefficient, second stress coefficient, and third stress coefficient values may not be obtained, and as a result, wrinkles or tears may occur, and pinholes or curls may occur on the surface of the copper foil (110).
[0131] On the other hand, when the concentration of nickel (Ni) is less than 15 ppm, the surface roughness of the copper foil (110) may increase excessively, resulting in a decrease in strength, and curls may occur on the surface of the copper foil (110). In addition, a rapid change may occur in the stress value of the copper foil (110). As a result, the desired first stress coefficient, second stress coefficient, and third stress coefficient values may not be obtained, and as a result, wrinkles or tears may occur, and pinholes or curls may occur on the surface of the copper foil (110).
[0132] The organic additive contained in the electrolyte (20) includes at least one of a brightener (component A), a moderator (component B), a leveling agent (component C), and a softener (component D). The organic additive has a concentration of 1 to 100 ppm in the electrolyte (20).
[0133] The organic additive may contain two or more of a brightener (component A), a moderator (component B), a leveling agent (component C), and an emollient (component D), or may contain all four components. Even in such cases, the concentration of the organic additive is 100 ppm or less. When the organic additive contains all of a brightener (component A), a moderator (component B), a leveling agent (component C), and an emollient (component D), the concentration of the organic additive may be 10 to 100 ppm.
[0134] The polishing agent (component A) contains sulfonic acid or its metal salt. The polishing agent (component A) may have a concentration of 1 to 25 ppm in the electrolyte (20).
[0135] The polishing agent (component A) can increase the charge of the electrolyte (20), thereby increasing the deposition speed of copper, improving the curling characteristics of the copper foil, and enhancing the gloss of the copper foil (110).
[0136] If the concentration of the polishing agent (component A) is less than 1 ppm, the gloss of the copper foil (110) may decrease, and if it exceeds 25 ppm, the roughness of the copper foil (110) may increase, and the A value of the copper film (111) may become lower than 1.1. As a result, the strength of the copper foil (110) may decrease, and folding of the copper foil (110) may occur, or wrinkles may form on the left and right ends of the copper foil (110) during the roll-to-roll manufacturing process.
[0137] The brightener (component A) increases the charge of the electrolyte (20), thereby increasing the deposition speed of copper, improving the curling characteristics of the copper foil, and enhancing the gloss of the copper foil (110). If the concentration of the brightener (component A) is less than 1 ppm, the gloss of the copper foil (110) is reduced, and if it exceeds 25 ppm, wrinkles or tears may occur in the copper foil (110), pinholes or curls may occur on the surface of the copper foil (110), and a rapid change may occur in the stress value of the copper foil (110). As a result, the first stress coefficient, second stress coefficient, and third stress coefficient values to be obtained may not be obtained, and as a result, wrinkles or tears may occur, and pinholes or curls may occur on the surface of the copper foil (110).
[0138] More specifically, the polishing agent (component A) may have a concentration of 5 to 20 ppm in the electrolyte (20).
[0139] The polishing agent may include, for example, at least one of bis-(3-sulfopropyl)-disulfide disodium salt, 3-mercapto-1-propanesulfonic acid, 3-(N,N-dimethylthiocarbamoyl)-thiopropanesulfonate sodium salt, 3-[(amino-iminomethyl)thio]-1-propanesulfonate sodium salt, o-ethyldithiocarbonato-S-(3-sulfopropyl)-ester sodium salt, 3-(benzothiazolyl-2-mercapto)-propyl-sulfonic acid sodium salt, and ethylenedithiodipropylsulfonic acid sodium salt.
[0140] The moderator (component B) includes a nonionic water-soluble polymer. The moderator (component B) may have a concentration of 1 to 15 ppm in the electrolyte (20).
[0141] The moderator (component B) reduces the deposition speed of copper, thereby preventing rapid increase in roughness and decrease in strength of the copper foil (110). This moderator (component B) is also called an inhibitor or suppressor.
[0142] If the concentration of the moderator (component B) is less than 1 ppm, the roughness of the copper foil (110) may rapidly increase, and the A value of the copper film (111) may become lower than 1.1. As a result, the strength of the copper foil (110) may be reduced, and folding of the copper foil (110) may occur, or wrinkles may form on the left and right ends of the copper foil (110) during the roll-to-roll manufacturing process.
[0143] If the concentration of the moderator (component B) is less than 1 ppm, the roughness of the copper foil (110) may rapidly increase, and the strength of the copper foil (110) may decrease. In addition, wrinkles or tears may occur in the copper foil (110), and pinholes or curls may occur on the surface of the copper foil (110). In addition, a rapid change may occur in the stress value of the copper foil (110). As a result, the desired first stress coefficient, second stress coefficient, and third stress coefficient values may not be obtained, and as a result, wrinkles or tears may occur, and pinholes or curls may occur on the surface of the copper foil (110).
[0144] On the other hand, even if the concentration of the moderator (component B) exceeds 15 ppm, there is almost no change in the physical properties of the copper foil (110), such as appearance, gloss, roughness, strength, and elongation. Therefore, the concentration of the moderator (component B) can be adjusted to the range of 1 to 10 ppm without unnecessarily increasing the concentration of the moderator (component B), thereby increasing manufacturing costs and wasting raw materials.
[0145] The moderator (component B) may include at least one nonionic water-soluble polymer selected from, for example, polyethylene glycol (PEG), polypropylene glycol, polyethylene polypropylene copolymer, polyglycerin, polyethylene glycol dimethyl ether, hydroxyethylene cellulose, polyvinyl alcohol, stearic acid polyglycol ether, and stearyl alcohol polyglycol ether. However, the type of moderator is not limited thereto, and other nonionic water-soluble polymers that can be used in the production of high-strength copper foil (110) may be used as the moderator.
[0146] The leveling agent (component C) contains at least one of nitrogen (N) and sulfur (S). That is, the leveling agent (component C) may contain one or more nitrogen atoms (N) or one or more sulfur atoms (S) in one molecule, and may also contain one or more nitrogen atoms (N) and one or more sulfur atoms (S). For example, the leveling agent (component C) is an organic compound containing at least one of nitrogen (N) and sulfur (S).
[0147] The leveling agent (component C) prevents excessively high peaks or excessively large protrusions from being formed on the copper film (111), thereby making the copper film (111) macroscopically flat. The leveling agent (component C) may have a concentration of 1 to 15 ppm in the electrolyte (11).
[0148] If the concentration of the leveling agent (component C) is less than 1 ppm, a problem may arise where the A value of the copper film (111) becomes lower than 1.1. As a result, the strength of the copper foil (110) may be reduced, folding of the copper foil (110) may occur, or wrinkles may form at the left and right ends of the copper foil (110) during the roll-to-roll manufacturing process.
[0149] On the other hand, if the concentration of the leveling agent (component C) exceeds 15 ppm, the surface roughness of the copper foil (110) may increase excessively, resulting in a decrease in strength, and pinholes or curls may occur on the surface of the copper foil (110), making it difficult to separate the copper foil (110) from the winder (WR) after manufacturing it.
[0150] When the concentration of the leveling agent (component C) is less than 1 ppm, the strength of the copper foil (110) is reduced, making it difficult to manufacture a high-strength copper foil (110). In addition, a rapid change may occur in the stress value of the copper foil (110). As a result, the desired first stress coefficient, second stress coefficient, and third stress coefficient values may not be obtained, and as a result, wrinkles or tears may occur, and pinholes or curls may occur on the surface of the copper foil (110).
[0151] On the other hand, if the concentration of the leveling agent (component C) exceeds 15 ppm, the surface roughness of the copper foil (110) may increase excessively, resulting in a decrease in strength, and pinholes or curls may occur on the surface of the copper foil (110), making it difficult to separate the copper foil (110) from the winder (WR) after manufacturing it. In addition, if the concentration of the leveling agent (component C) exceeds 15 ppm, a rapid change may occur in the stress value of the copper foil (110). As a result, the desired first stress coefficient, second stress coefficient, and third stress coefficient values may not be obtained.
[0152] Leveling agents (component C) include, for example, diethylthiourea, ethylenethiourea, acetylenethiourea, dipropylthiourea, dibutylthiourea, N-trifluoroacetylthiourea, N-ethylthiourea, N-cyanoacetylthiourea, N-allylthiourea, o-tolylthiourea, N,N'-butylene thiourea, thiazolidinethiol, 4-thiazolinethiol, 4-methyl-2-pyrimidinethiol, 2-thiouracil, 3-(benzotriazole-2-mercapto)-prosulfonic acid), 2-mercaptopyridine, 3(5-mercapto 1H-tetrazol)benzenesulfonate, 2-mercaptobenzothiazole, dimethylpyridine, 2,2'-bipyridine, 4.4'-bipyridine, pyrimidine, pyridazine, pyrimidine, pyrinoline, oxazole, thiazole, 1-methylimidazole, 1-benzylimidazole, 1-methyl-2methylimidazole, 1-benzyl-2-methylimidazole, 1-ethyl-4-methylimidazole, 1-ethyl-2-ethyl-4-methylol, N-methylpyrrole, N-ethylpyrrole, N-butylpyrrole, N-methylpyrroline, N-ethylpyrroline, It may include at least one of N-butylpyrroline, pyrimidine, purine, quinoline, isoquinoline, N-methylcarbazole, N-ethylcarbazole, and N-butylcarbazole.
[0153] The emollient (component D) may include citric acid (CA). Specifically, the electrolyte (20) may include 1 to 5 ppm of citric acid (CA).
[0154] When the concentration of citric acid (CA) in the electrolyte (20) exceeds 5 ppm, the surface roughness of the copper foil (110) may excessively increase, causing a problem in which the A value of the copper film (111) becomes lower than 1.1. In addition, a problem in which the Vickers hardness and tensile strength of the copper foil (110) become lower may occur.
[0155] On the other hand, if the concentration of citric acid (CA) in the electrolyte (20) is less than 1 ppm, a problem may arise where the A value of the copper film (111) becomes lower than 1.1. As a result, the strength of the copper foil (110) may be reduced, making it difficult to manufacture a high-strength copper foil (110).
[0156] If the concentration of citric acid (CA) in the electrolyte (20) exceeds 5 ppm, the surface roughness of the copper foil (110) may increase excessively, resulting in a decrease in strength, and curls may also occur on the surface of the copper foil (110). In addition, a rapid change may occur in the stress value of the copper foil (110). As a result, the desired first stress coefficient, second stress coefficient, and third stress coefficient values may not be obtained.
[0157] On the other hand, when the concentration of citric acid (CA) in the electrolyte (20) is less than 1 ppm, the strength of the copper foil (110) is reduced, making it difficult to manufacture a high-strength copper foil (110). In addition, a rapid change may occur in the stress value of the copper foil (110). As a result, the desired first stress coefficient, second stress coefficient, and third stress coefficient values may not be obtained, and as a result, wrinkles or tears may occur, and pinholes or curls may occur on the surface of the copper foil (110).
[0158] When the copper film (111) is formed, the flow rate of the electrolyte (20) supplied into the electrolytic cell (10) is 41 to 45 m 3 It could be / hour.
[0159] The step of forming a copper film (111) may include at least one of a step of filtering the electrolyte (20) using activated carbon, a step of filtering the electrolyte (20) using diatomaceous earth, and a step of treating the electrolyte (20) with ozone (O3).
[0160] Specifically, for filtration of the electrolyte (20), the electrolyte (20) is 35 to 45 m 3 / hour. That is, in order to remove solid impurities present in the electrolyte (20) while electroplating for forming a copper film (111) is performed, 35 to 45 m 3 Filtration can be performed at a flow rate of / hour. At this time, activated carbon or diatomaceous earth can be used.
[0161] To maintain the cleanliness of the electrolyte (20), the electrolyte (20) may be treated with ozone (O3).
[0162] Additionally, to ensure the purity of the electrolyte (20), the copper wire (Cu wire), which is the raw material of the electrolyte (20), can be cleaned.
[0163] According to one embodiment of the present invention, the step of preparing an electrolyte (20) may include a step of heat-treating a copper wire, a step of acid-cleaning the heat-treated copper wire, a step of washing the acid-cleaned copper wire, and a step of putting the washed copper wire into sulfuric acid for an electrolyte.
[0164] More specifically, in order to maintain the purity of the electrolyte (20), a high-purity (99.9% or more) copper wire (Cu wire) is heat-treated in an electric furnace at 750°C to 850°C to burn off various organic impurities on the copper wire, and then the heat-treated copper wire is pickled for 10 to 20 minutes using a 10% sulfuric acid solution, and the pickled copper wire is washed using distilled water. Through these sequential processes, copper for preparing the electrolyte (20) can be manufactured. The washed copper wire can be mixed with sulfuric acid for the electrolyte to prepare the electrolyte (20).
[0165] According to one embodiment of the present invention, the concentration of total organic carbon (TOC) in the electrolyte (20) is managed to be 50 ppm or less in order to satisfy the characteristics of the copper foil (110). That is, the electrolyte (20) may have a total organic carbon (TOC) concentration of 50 ppm or less.
[0166] The copper film (111) manufactured in this way can be cleaned in a cleaning tank.
[0167] For example, acid cleaning to remove impurities, such as resin components or natural oxide, on the surface of the copper film (111) and water cleaning to remove the acid solution used in the acid cleaning may be performed sequentially. The cleaning process may be omitted.
[0168] Next, a protective layer (112) is formed on the copper film (111).
[0169] Referring to Fig. 6, a step of immersing the copper film (111) in an anticorrosion solution (60) may be further included. When the copper film (111) is immersed in the anticorrosion solution (60), it may be guided by a guide roll placed within the anticorrosion solution (60).
[0170] As described above, the anti-rust solution (60) may include at least one of a chromium compound, a silane compound, and a nitrogen compound. For example, the copper film (111) may be immersed in a 1 to 10 g / L potassium dichromate solution at room temperature for 1 to 30 seconds.
[0171] Meanwhile, the protective layer (112) may include a silane compound through silane treatment or a nitrogen compound through nitrogen treatment.
[0172] Copper foil (110) is created by forming this protective layer (112).
[0173] An electrode for a secondary battery (i.e., an anode) of the present invention can be manufactured by coating one or more negative active materials selected from the group consisting of carbon; a metal (Me) of Si, Ge, Sn, Li, Zn, Mg, Cd, Ce, Ni or Fe; an alloy containing the metal (Me); an oxide (MeOx) of the metal (Me); and a complex of the metal (Me) and carbon on one or both sides of the copper foil (110) of the present invention manufactured through the above method.
[0174] For example, 100 parts by weight of carbon for negative electrode active material is mixed with 1 to 3 parts by weight of styrene butadiene rubber (SBR) and 1 to 3 parts by weight of carboxymethyl cellulose (CMC), and then a slurry is prepared using distilled water as a solvent. Then, the slurry is applied to the copper foil (110) to a thickness of 20 to 60 μm using a doctor blade, and pressed at a pressure of 0.5 to 1.5 ton / cm2 at 110 to 130°C.
[0175] A secondary battery can be manufactured using a conventional positive electrode, electrolyte, and separator together with the secondary battery electrode (negative electrode) of the present invention manufactured by the above method.
[0176] Below, the present invention is specifically described through examples and comparative examples. However, the following examples are provided solely to aid understanding of the present invention, and the scope of the present invention is not limited to these examples.
[0177] Example 1-5 and Comparative Example 1-5
[0178] Copper foil was manufactured using a foil maker including an electrolytic cell (10), a rotating cathode drum (40) placed in the electrolytic cell (10), and an anode plate (30) placed spaced apart from the rotating cathode drum (40). The electrolyte (20) is a copper sulfate solution. The concentration of copper ions in the electrolyte (20) was set to 87 g / L, the concentration of sulfuric acid was set to 110 g / L, the temperature of the electrolyte was set to 55°C, and the current density was set to 60 ASD.
[0179] In addition, the concentrations of chlorine (Cl), nickel (Ni), lead (Pb), hydrogen peroxide, and tungsten contained in the electrolyte (20) and the concentrations of organic additives are as shown in Table 1 below.
[0180] Among the organic additives, bis-(3-sulfopropyl)-disulfide disodium salt (SPS) was used as a brightener (component A), polyethylene glycol (PEG) was used as a moderator (component B), and ethylene thiourea (ETU) was used as a leveling agent (component C).
[0181] A copper film (111) was manufactured by applying a current at a current density of 60 ASD between a rotating cathode drum (40) and an anode plate (30). Next, the copper film (111) was immersed in a rust-preventing solution for about 2 seconds to perform a chromate treatment on the surface of the copper film (111) to form a protective layer (112), thereby manufacturing a copper foil (110). A rust-preventing solution containing chromic acid as a main component was used, and the concentration of chromic acid was 5 g / L.
[0182] As a result, copper foils of Example 1-5 and Comparative Example 1-5 were manufactured.
[0183] SPS (Component A) (ppm) PEG (Component B) (ppm) ETU (Component C) (ppm) CA (D) Ingredients) (ppm) Chlorine (ppm) Nickel (ppm) Lead (ppm) Hydrogen peroxide (ml / L) Tungsten (ppm) Example 1523120501021 Example 21045320601553 Example 31567520801875 Example 42089220100871 Example 5151010420120553 Comparative Example 1555552050.193 Comparative Example 210507520505070.1 Comparative Example 3157103203010510 Comparative Example 4105755202001050.1 Comparative Example 510520520301053
[0184]
[0185] Peak strength (P) Peak strength (Q) A (P / Q) Vickers hardness (Hv) Whether wrinkles / tears occurred Whether fracture occurred Example 10.000940.000641.471.52 None None Example 20.001000.000841.191.85 None None Example 30.000970.000741.311.54 None None Example 40.001020.000701.461.60 None None Example 50.000890.000571.561.41 None None Comparison Example 10.000860.000880.981.21 No occurrence Comparison Example 20.000990.000610.981.21 No occurrence Comparison Example 30.001270.000791.611.55 No occurrence Comparison Example 40.000880.000920.961.23 No occurrence Comparison Example 50.000920.001000.921.18 No occurrence
[0186]
[0187] For the copper foils of Example 1-5 and Comparative Example 1-5 manufactured in this manner, i) peak strength (P), ii) peak strength (Q), iii) A(P / Q), iv) Vickers hardness, v) occurrence of wrinkles / tears, and vi) occurrence of fracture were confirmed. i) Peak strength (P), ii) Peak strength (Q) measurement
[0188] Peak intensity (P) is the peak intensity of the copper film (111) at 1650 cm-1, and peak intensity (Q) is the peak intensity of the copper film (111) at 1460 cm-1.
[0189] At this time, peak intensities (P, Q) are measured by FT-IR.
[0190] iii) A(P / Q) measurement
[0191] The A value can be obtained by calculating the above measured i) peak intensity (P) and ii) peak intensity (Q) values according to the following equation 1.
[0192] [Formula 1]
[0193] A = P / Q
[0194] iv) Vickers hardness (Hv)
[0195] Vickers hardness (Hv) was measured using a nanoindenter (HM 2000, Helmut Fischer).
[0196] Environment: (23±2)℃, (45±5)% RH
[0197] Indenter Type: Vickers Indenter (Correction Factor: 0.75)
[0198] Load Increase Time: 10s
[0199] Unload Increase Time: 10s
[0200] Creep Time: 3s
[0201] Load: 0.5mN
[0202] The Vickers Hardness in Table 2 above means the average of the values of Vickers Hardness measured three times using the above method.
[0203] v) Whether wrinkles / tears occur
[0204] After 100 charge-discharge cycles, the secondary battery was disassembled and the presence or absence of wrinkles or tears in the copper foil was observed. If wrinkles or tears occurred in the copper foil, they were marked as "occurrence," and if no wrinkles or tears occurred, they were marked as "none."
[0205] vi) Whether or not a break has occurred
[0206] After 100 charge-discharge cycles, the secondary battery was disassembled and the presence or absence of copper foil fractures was observed. If the copper foil fractured, it was marked as "occurred," while if it did not, it was marked as "none."
[0207] Referring to Table 1 and Table 2, the following results can be confirmed.
[0208] Tearing / wrinkling occurred in the copper foil of Comparative Example 1 manufactured using an electrolyte containing an excessive amount of a brightener (component A) and trace amounts of nickel and lead.
[0209] Tearing / wrinkling occurred in the copper foil of Comparative Example 2 manufactured using an electrolyte containing an excess amount of moderator (component B) and lead, and a trace amount of tungsten.
[0210] A fracture occurred in the copper foil of Comparative Example 3 manufactured using an electrolyte containing an excessive amount of tungsten.
[0211] Tearing / wrinkling occurred in the copper foil of Comparative Example 4 manufactured using an electrolyte containing an excess amount of a softener (component D) and nickel, and a trace amount of tungsten.
[0212] Tearing / wrinkling occurred in the copper foil of Comparative Example 5 manufactured using an electrolyte containing an excessive amount of leveling agent (component C).
[0213] On the other hand, in the copper foils of Examples 1 to 5 according to the present invention, all values satisfied the standard, and as a result, no wrinkles / tears occurred and no fractures occurred.
[0214] Example 6-10 and Comparative Example 6-9
[0215] Copper foil was manufactured using a foil maker including an electrolytic cell (10), a rotating cathode drum (40) placed in the electrolytic cell (10), and an anode plate (30) placed spaced apart from the rotating cathode drum (40). The electrolyte (20) is a copper sulfate solution. The concentration of copper ions in the electrolyte (20) was set to 87 g / L, the concentration of sulfuric acid was set to 110 g / L, the temperature of the electrolyte was set to 55°C, and the current density was set to 60 ASD.
[0216] Additionally, the concentrations of chlorine (Cl), nickel (Ni), lead (Pb), hydrogen peroxide, tungsten (W), and organic additives contained in the electrolyte (20) are as shown in Table 3 below.
[0217] Among the organic additives, bis-(3-sulfopropyl)-disulfide disodium salt (SPS) was used as a brightener (component A), polyethylene glycol (PEG) was used as a moderator (component B), and ethylene thiourea (ETU) was used as a leveling agent (component C).
[0218] A copper film (111) was manufactured by applying a current at a current density of 60 ASD between a rotating cathode drum (40) and an anode plate (30). Next, the copper film (111) was immersed in a rust-preventing solution for about 2 seconds to perform a chromate treatment on the surface of the copper film (111) to form a protective layer (112), thereby manufacturing a copper foil (110). A rust-preventing solution containing chromic acid as a main component was used, and the concentration of chromic acid was 5 g / L.
[0219] As a result, copper foils of Example 6-10 and Comparative Example 6-9 were manufactured.
[0220] SPS (Component A) (ppm) PEG (Component B) (ppm) ETU (Component C) (ppm) CA (Component D) (ppm) Chlorine (ppm) Nickel (ppm) Lead (ppm) Hydrogen Peroxide (ppm) Tungsten (ppm) Example 6 5 2 3 1 2 0 5 0 1 0 1 Example 7 1 0 4 5 3 2 0 6 0 1 5 3 Example 8 1 5 6 7 5 2 0 8 0 1 5 7 5 Example 9 2 0 8 9 2 0 1 0 1 8 7 1 Example 1 0 1 5 1 0 1 8 5 3 Comparative Example 6 5 5 5 5 2 0 5 0 1 Comparative Example 7 1 0 5 0 7 5 2 0 5 0 0 1 1 Comparative Example 8 1 5 7 5 5 3 2 0 3 0 1 5 1 5 1 0 Comparative Example 9 1 0 5 7 5 5 2 0 0 5 0 5 3
[0221]
[0222] Distinction MD direction TD direction 1st stress factor (A / A'+B / B'+C / C') 2nd stress factor (A / B+A' / B') 3rd stress factor (A / C+A' / C') Occurrence of tearing / wrinkling Whether A(Pa)B(Pa)C(Pa)A'(Pa)B'(Pa)C'(Pa)Example 648.737.223.248.337.924.12.952.584.10NoneExample 755.342.126.255.244.224.13.042.564.40NoneExample 845.332.123.946.936.823.42.862.693.90NoneExample 952.239.224.850.441.225.42.962.554.09NoneExample 1 049.337.424.148.838.223.43.022.604.13NoneComparison Example653.244.832.157.246.833.62.842.413.36OccurrenceComparison Example736.229.921.138.331.925.72.832.413.44OccurrenceComparison Example841.833.221.146.936.825.72.612.533.81OccurrenceExample648.737.223.248.337.924.12.952.584.10None
[0223]
[0224] For the copper foils of Example 6-10 and Comparative Example 6-9 manufactured in this manner, i) A, A', B, B', C and C' ii) first stress factor, iii) second stress factor, iv) third stress factor and v) occurrence of wrinkles / tears were confirmed. i) Measurement of A, A', B, B', C and C'
[0225] A is the stress at 50% elongation in the MD direction of the copper foil, A' is the stress at 50% elongation in the TD direction of the copper foil, B is the stress at 10% elongation in the MD direction of the copper foil, B' is the stress at 10% elongation in the TD direction of the copper foil, C is the stress at 5% elongation in the MD direction of the copper foil, and C' is the stress at 5% elongation in the TD direction of the copper foil.
[0226] A, A', B, B', C, and C' are measured by a universal testing machine (UTM, Instron) according to the specifications of the IPC-TM-650 Test Method Manual. The sample width is 12.7 mm, the distance between grips is 50 mm, and the measuring speed is 50 mm / min.
[0227] A measured stress after 50% elongation in MD direction under the same conditions as above for copper foil, A' measured stress after 50% elongation in TD direction under the same conditions as above for copper foil, B measured stress after 10% elongation in MD direction under the same conditions as above for copper foil, B' measured stress after 10% elongation in TD direction, C measured stress after 5% elongation in MD direction under the same conditions as above for copper foil, and C' measured stress after 5% elongation in TD direction under the same conditions as above for copper foil.
[0228] ii) Calculation of the first stress coefficient
[0229] The first stress coefficient value can be obtained by calculating the measured i) A, A', B, B', C and C' values according to the following equation 2.
[0230] [Formula 2]
[0231] First stress factor = A / A' + B / B' + C / C'
[0232] iii) Calculation of the second stress factor
[0233] The second stress coefficient value can be obtained by calculating the measured i) A, A', B and B' values according to the following equation 3.
[0234] [Formula 3]
[0235] Second stress factor = A / B + A' / B'
[0236] iv) Calculation of the third stress factor
[0237] The third stress coefficient value can be obtained by calculating the measured i) A, A', C and C' values according to the following equation 4.
[0238] [Formula 4]
[0239] Third stress factor = A / C + A' / C'
[0240] v) Whether wrinkles / tears occur
[0241] After 100 charge-discharge cycles, the secondary battery was disassembled and the copper foil was observed for wrinkles or tears. If wrinkles or tears occurred in the copper foil, they were marked as "occurrence," and if no wrinkles or tears occurred, they were marked as "none."
[0242] Referring to Tables 3 and 4, the following results can be confirmed.
[0243] Tearing / wrinkling occurred in the copper foil of Comparative Example 6 manufactured using an electrolyte containing an excessive amount of a brightener (component A) and trace amounts of nickel, lead and tungsten.
[0244] Tearing / wrinkling occurred in the copper foil of Comparative Example 7 manufactured using an electrolyte containing an excessive amount of a moderator (component B) and trace amounts of lead and hydrogen peroxide.
[0245] Tearing / wrinkling occurred in the copper foil of Comparative Example 8 manufactured using an electrolyte containing an excess of leveling agent (component C), hydrogen peroxide, and tungsten.
[0246] Tearing / wrinkling occurred in the copper foil of Comparative Example 9 manufactured using an electrolyte containing an excessive amount of a softener (component D), nickel, and lead.
[0247] On the other hand, in the copper foils of Examples 6 to 10 according to the present invention, all values satisfied the standard, and as a result, no tearing / wrinkling occurred.
[0248] The present invention described above is not limited to the aforementioned embodiments and the attached drawings, and it will be apparent to those skilled in the art that various substitutions, modifications, and changes are possible without departing from the technical scope of the present invention. Therefore, the scope of the present invention is expressed by the following claims, and all changes or modifications derived from the meaning, scope, and equivalent concepts of the claims should be interpreted as being included within the scope of the present invention.
Claims
A copper film comprising 99.9 wt% or more of copper; The copper film has an A value in the range of 1.1 to 1.6, copper foil: The above A is calculated by the following equation 1, [Formula 1] A = P / Q P in the above formula 1 is 1650 cm of the copper film. -1 is the peak intensity at , Q in the above formula 1 is 1460 cm of the copper film. -1 is the peak intensity at , The above peak intensity is measured by FT-IR.
2. In paragraph 1, Copper foil having a Vickers hardness in the range of 1.3 to 1.9 Hv.
3. In paragraph 1, 45kgf / mm 2 Copper foil having a tensile strength of the above.
4. In paragraph 1, Copper foil having an elongation of 3 to 13%.
5. In paragraph 1, Copper foil further comprising a protective layer on the copper film.
6. In paragraph 5, A copper foil wherein the protective layer comprises at least one of a chromium compound, a silane compound, and a nitrogen compound.
7. A step of preparing an electrolyte containing copper ions; Step of forming a copper film; and A step of forming a protective layer on the copper film; including: The step of forming the above copper film is: It includes a step of forming a copper film on the rotating cathode drum by conducting current between the anode plates and the rotating cathode drum, which are arranged spaced apart from each other in the electrolyte in the electrolytic cell. The above electrolyte is, 70 to 100 g / L of copper ions; 70 to 150 g / L sulfuric acid; 15 to 25 ppm chlorine (Cl); 15 to 150 ppm nickel (Ni); 1 to 20 ppm of lead ion (Pb) 2+ ); 1 to 10 ml / L of hydrogen peroxide; 0.3 to 5 ppm of tungsten (W); and Contains organic additives; The above organic additive comprises at least one of a brightener (component A), a reducer (component B), a leveling agent (component C), and an emollient (component D). The above polishing agent (component A) contains sulfonic acid or its metal salt, The above-mentioned moderator (component B) contains a nonionic water-soluble polymer, The above leveling agent (component C) contains at least one of nitrogen (N) and sulfur (S), The above emollient (component D) contains citric acid. Method for manufacturing copper foil.
8. In paragraph 7, A method for manufacturing copper foil, wherein the above-mentioned polishing agent (component A) has a content of 1 to 25 ppm.
9. In paragraph 7, A method for manufacturing copper foil, wherein the above-mentioned moderator (component B) has a content of 1 to 15 ppm.
10. In paragraph 7, A method for manufacturing copper foil, wherein the leveling agent (component C) has a content of 1 to 15 ppm.
11. In paragraph 7, A method for manufacturing copper foil, wherein the above-mentioned emollient (component D) has a content of 1 to 5 ppm. A copper film comprising 99.9 wt% or more of copper; Having a first stress factor of 2.8 or more, Having a second stress factor of 2.5 or more, Copper foil having a third stress factor of 3.5 or greater: The above first stress coefficient is calculated by the following equation 2: [Formula 2] First stress factor = A / A' + B / B' + C / C' The above second stress coefficient is calculated by the following equation 3: [Formula 3] Second stress factor = A / B + A' / B' The above third stress coefficient is calculated by the following equation 4: [Formula 4] Third stress factor = A / C + A' / C' A in the above equation 2 is the stress at 50% elongation in the MD direction, A' in the above equation 2 is the stress at 50% elongation in the TD direction, B in the above equation 2 is the stress at 10% elongation in the MD direction, B' in the above equation 2 is the stress at 10% elongation in the TD direction, C in the above equation 2 is the stress at 5% elongation in the MD direction, C' in the above equation 2 is the stress at 5% elongation in the TD direction.
13. In paragraph 12, Copper foil further comprising a protective layer on the copper film.
14. In paragraph 13, A copper foil wherein the protective layer comprises at least one of a chromium compound, a silane compound, and a nitrogen compound.