Polyalkyl p-phenylenediamine Anti-aging agent, and intermediate thereof and preparation method therefor
Patent Information
- Application Number
- MYPI2025002481
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-11-10
- Filing Date
- 2022-11-21
- Publication Date
- 2024-05-10
AI Technical Summary
The existing preparation method of p-phenylenediamine antioxidants requires expensive bromide and precious metal catalysts, the conversion rate and yield are not high, and wastewater containing metal bromide salts is produced, which is not conducive to industrial production, and lacks novel structure and green environmental protection. of anti-aging agents.
The structure of a polyalkyl p-phenylenediamine compound is used to carry out condensation and reduction reactions through catalysts such as alkali metal hydroxides to prepare an antioxidant with good thermal oxygen aging resistance and ultraviolet light aging resistance. The green and environmentally friendly preparation method avoids the emission of three wastes.
It achieves more efficient thermal oxygen aging resistance and ultraviolet light aging resistance, and the preparation method is environmentally friendly and waste-free. The catalyst is recyclable and is suitable for industrial production.
Abstract
Description
Polyalkyl p-phenylenediamine antioxidant, intermediates thereof and preparation method Technical Field
[0001] The invention belongs to the field of p-phenylenediamine antioxidants, and particularly relates to polyalkyl p-phenylenediamine antioxidants, intermediates thereof and a preparation method. Background Art
[0002] Currently, p-phenylenediamine antioxidants are widely used in rubber products such as rubber tires. They offer highly effective ozone protection, excellent protection against flexural aging, general aging effects such as oxygen and heat, and excellent protection against harmful metals such as copper and manganese. For example, the antioxidant 6PPD, chemically known as N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, is a highly effective rubber antioxidant.
[0003] Chinese patent application CN113072741A discloses an environmentally friendly p-phenylenediamine antioxidant and its preparation method. The structure of the environmentally friendly p-phenylenediamine antioxidant disclosed in the patent application is:
[0004]
[0005] The antioxidant will not convert into a quinone compound after aging of the rubber material if the following specific conditions are met: at least one of x and w is 1, at least one of y and z is 1, and if x and z are both 1, y and w are not both 0. The preparation process provided in this patent application involves first subjecting aniline to a CN coupling reaction with p-bromonitrobenzene having corresponding substituents. The resulting coupling product is then subjected to a reduction reaction in a hydrogen atmosphere under catalytic conditions to obtain a reaction intermediate. The reaction intermediate is then subjected to a reductive amination reaction with an aldehyde or ketone under catalytic conditions to obtain the p-phenylenediamine antioxidant. This method requires the use of expensive bromides and precious metal organophosphorus complex catalysts, resulting in low reaction conversion and yield, complex separation and purification, and the generation of wastewater containing metal bromide salts, making it unsuitable for industrial production.
[0006] 4-Aminodiphenylamine is an important intermediate of p-phenylenediamine antioxidants. It is produced by condensing aniline or its derivatives with nitrobenzene under alkaline conditions and then reducing them. Alternatively, anilinonitrobenzene can be prepared by a CN coupling reaction between aniline and p-halogenated nitrobenzene in the presence of a triphenylphosphine-coordinated palladium catalyst, followed by hydrogenation and reduction.
[0007] Therefore, the present invention requires novel p-phenylenediamine antioxidants and green and environmentally friendly preparation methods.
[0008] Summary of the Invention
[0009] To address the problems existing in the prior art, the present invention provides a novel p-phenylenediamine antioxidant with excellent resistance to heat-oxidative aging and UV-light aging. The present invention also provides a method for preparing the p-phenylenediamine antioxidant, which is environmentally friendly and eliminates the discharge of three wastes. The present invention also provides an intermediate for preparing the p-phenylenediamine antioxidant.
[0010] Specifically, one aspect of the present invention provides a compound represented by formula I:
[0011]
[0012] In formula I, each R1 is independently selected from H, C1-C18 chain hydrocarbon group and C3-C18 alicyclic hydrocarbon group, and a is an integer from 1 to 5;
[0013] R2, R3, R4, and R5 are each independently selected from H, a C1-C18 chain hydrocarbon group, and a C3-C18 alicyclic hydrocarbon group, and at least one of R2, R3, R4, and R5 is not H;
[0014] R6 and R7 are each independently selected from a C1-C18 chain hydrocarbon group and a C3-C18 alicyclic hydrocarbon group, or R6 and R7 form a C3-C18 aliphatic ring.
[0015] In one or more embodiments, in Formula I, each R1 is independently selected from H and C1-C8 alkyl.
[0016] In one or more embodiments, in Formula I, a is an integer of 1-2.
[0017] In one or more embodiments, in Formula I, R2, R3, R4, and R5 are each independently selected from H and C1-C8 alkyl.
[0018] In one or more embodiments, in Formula I, 2 to 3 of R2, R3, R4, and R5 are H.
[0019] In one or more embodiments, in Formula I, R6 and R7 are each independently selected from C1-C8 alkyl and C3-C8 cycloalkyl, or R6 and R7 form a C3-C8 aliphatic ring.
[0020] Another aspect of the present invention provides a method for preparing the compound represented by Formula I, comprising the following steps:
[0021] (1) subjecting the compound represented by Formula A and the compound represented by Formula B to a condensation reaction under the action of a first catalyst to obtain a condensate comprising the compound represented by Formula C and / or the compound represented by Formula C′, and then subjecting the condensate to a reduction reaction under the action of H2 and a second catalyst to obtain the compound represented by Formula II;
[0022]
[0023] (2) subjecting the compound represented by Formula II to a reductive alkylation reaction with the compound represented by Formula D in the presence of H2 and a third catalyst to obtain the compound represented by Formula I;
[0024]
[0025] R1, R2, R3, R4, R5, R6, and R7 in Formula A, Formula B, Formula C, Formula C′, Formula D, Formula II, and Formula I are as defined in any embodiment herein.
[0026] In one or more embodiments, the first catalyst is selected from one or more of an alkali metal hydroxide, an alkali metal alkoxide, a quaternary ammonium base, and a combination of an alkali metal hydroxide and a tetraalkylammonium halide.
[0027] In one or more embodiments, the second catalyst is a porous metal catalyst or a supported metal catalyst; the porous metal catalyst is preferably selected from one or more of Raney nickel, Raney cobalt and Raney copper, the metal in the supported metal catalyst is preferably selected from one or more of nickel, cobalt, copper, platinum, palladium, ruthenium and rhodium, and the carrier in the supported metal catalyst is preferably selected from one or more of carbon, alumina, silica gel and molecular sieve.
[0028] In one or more embodiments, the third catalyst is a supported metal catalyst; the metal in the supported metal catalyst is preferably selected from one or more of nickel, cobalt, copper, platinum, palladium, ruthenium and rhodium, and the carrier in the supported metal catalyst is preferably selected from one or more of carbon, alumina, silica gel and molecular sieves.
[0029] In one or more embodiments, in step (1), the molar ratio of the compound represented by formula A to the compound represented by formula B is 2:1 to 15:1, preferably 4:1 to 10:1.
[0030] In one or more embodiments, in step (1), the temperature of the condensation reaction is 40 to 90° C., preferably 65 to 85° C., and the vacuum degree is -0.09 to -0.99 MPa.
[0031] In one or more embodiments, in step (1), the temperature for reacting the condensate with H2 is 40-120°C, preferably 60-90°C, and the hydrogen pressure is 0.5-5 MPa, preferably 0.5-2.5 MPa.
[0032] In one or more embodiments, in step (2), the molar ratio of the compound represented by formula D to the compound represented by formula II is 1:1 to 15:1.
[0033] In one or more embodiments, in step (2), the reaction temperature is 40 to 150° C., and the reaction pressure is 0.5 to 5 MPa.
[0034] Another aspect of the present invention provides a compound shown in formula II:
[0035]
[0036] In formula II, each R1 is independently selected from H, C1-C18 chain hydrocarbon group and C3-C18 alicyclic hydrocarbon group, and a is an integer from 1 to 5;
[0037] R2, R3, R4, and R5 are each independently selected from H, a C1-C18 chain hydrocarbon group, and a C3-C18 alicyclic hydrocarbon group, and at least one of R2, R3, R4, and R5 is not H.
[0038] In one or more embodiments, in Formula II, each R1 is independently selected from H and C1-C8 alkyl.
[0039] In one or more embodiments, in Formula II, a is an integer from 1 to 2.
[0040] In one or more embodiments, in Formula II, R2, R3, R4, and R5 are each independently selected from H and C1-C8 alkyl.
[0041] In one or more embodiments, in Formula II, 2 to 3 of R2, R3, R4, and R5 are H.
[0042] Another aspect of the present invention provides a method for preparing a compound of Formula II, comprising: subjecting a compound of Formula A to a condensation reaction with a compound of Formula B in the presence of a first catalyst to obtain a condensate comprising a compound of Formula C and / or a compound of Formula C′, and then subjecting the condensate to a reduction reaction in the presence of H2 and a second catalyst to obtain a compound of Formula II.
[0043]
[0044] R1, R2, R3, R4, and R5 in Formula A, Formula B, Formula C, Formula C', and Formula II are as defined in any embodiment herein.
[0045] In one or more embodiments, the first catalyst is selected from one or more of an alkali metal hydroxide, an alkali metal alkoxide, a quaternary ammonium base, and a combination of an alkali metal hydroxide and a tetraalkylammonium halide.
[0046] In one or more embodiments, the second catalyst is a porous metal catalyst or a supported metal catalyst; the porous metal catalyst is preferably selected from one or more of Raney nickel, Raney cobalt and Raney copper, the metal in the supported metal catalyst is preferably selected from one or more of nickel, cobalt, copper, platinum, palladium, ruthenium and rhodium, and the carrier in the supported metal catalyst is preferably selected from one or more of carbon, alumina, silica gel and molecular sieve.
[0047] In one or more embodiments, in step (1), the molar ratio of the compound represented by formula A to the compound represented by formula B is 2:1 to 15:1, preferably 4:1 to 10:1.
[0048] In one or more embodiments, in step (1), the temperature of the condensation reaction is 40 to 90° C., preferably 65 to 85° C., and the vacuum degree is -0.09 to -0.99 MPa.
[0049] In one or more embodiments, in step (1), the temperature for reacting the condensate with H2 is 40-120°C, preferably 60-90°C, and the hydrogen pressure is 0.5-5 MPa, preferably 0.5-2.5 MPa.
[0050] Another aspect of the present invention provides a rubber composition, comprising the compound of formula I described in any embodiment herein.
[0051] Another aspect of the present invention provides a rubber product, comprising the rubber composition according to any one of the embodiments herein; preferably, the rubber product is a tire.
[0052] Another aspect of the present invention provides a method for improving the heat-oxidative aging resistance and / or ultraviolet aging resistance of rubber or rubber products, the method comprising adding a compound of formula I as described in any embodiment of the present invention to the rubber or rubber product. DETAILED DESCRIPTION
[0053] To facilitate understanding of the features and effects of the present invention by those skilled in the art, the following provides a general description and definition of terms and expressions used in the specification and claims. Unless otherwise indicated, all technical and scientific terms used herein have the ordinary meanings as understood by those skilled in the art regarding the present invention. In the event of conflict, the definitions in this specification shall prevail.
[0054] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0055] Herein, “comprising,” “including,” “containing” and similar terms encompass the meanings of “consisting essentially of” and “consisting of,” for example, when “A comprises B and C” is disclosed herein, “A consists essentially of B and C” and “A consists of B and C” should be deemed to have been disclosed herein.
[0056] Herein, all features such as values, amounts, amounts, and concentrations defined in numerical ranges or percentage ranges are for brevity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to include and specifically disclose all possible subranges and individual values within the range (including integers and fractions).
[0057] In this document, unless otherwise specified, percentage refers to mass percentage and ratio refers to mass ratio.
[0058] Herein, when describing embodiments or examples, it should be understood that they are not intended to limit the present invention to these embodiments or examples. On the contrary, all alternatives, modifications and equivalents of the methods and materials described herein are encompassed within the scope defined by the claims.
[0059] In this document, for the sake of brevity, not all possible combinations of the various technical features in each embodiment or example are described. Therefore, as long as there are no contradictions in the combination of these technical features, the various technical features in each embodiment or example can be combined in any way, and all possible combinations should be considered to be within the scope of this specification.
[0060] As used herein, chain hydrocarbon groups refer to straight or branched saturated or unsaturated hydrocarbon groups, typically containing 1 to 18 carbon atoms (C1-C18 chain hydrocarbon groups). Examples of chain hydrocarbon groups include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-hexyl, isohexyl, 1,3-dimethylbutyl, 1,4-dimethylpentyl, tert-octyl, vinyl, propenyl, and ethynyl.
[0061] As used herein, an alicyclic hydrocarbon group refers to a group in which carbon atoms are bonded in a ring, typically containing 3 to 18 carbon atoms (C3-C18 alicyclic hydrocarbon groups). Examples of alicyclic hydrocarbon groups include, but are not limited to, isobornyl, cyclohexyl, norbornyl, norbornenyl, dicyclopentadienyl, ethynylcyclohexyl, and ethynylcyclohexenyl.
[0062] As used herein, an alkyl group refers to a linear or branched monovalent saturated hydrocarbon group, typically containing 1 to 18 carbon atoms (C1-C18 alkyl), for example, 1 to 8 carbon atoms (C1-C8 alkyl). Examples of alkyl groups include, but are not limited to, methyl, ethyl, propyl, 1-methylpropyl, isobutyl, and 1,3-dimethylbutyl.
[0063] Herein, cycloalkyl refers to a monovalent saturated hydrocarbon ring containing 3 to 18 carbon atoms, preferably 3 to 8 carbon atoms. Examples of cycloalkyl include, but are not limited to, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, and adamantyl.
[0064] Compounds of formula I
[0065] The present invention has discovered that a polyalkyl p-phenylenediamine compound having a structure shown in Formula I (referred to as the compound of Formula I) can be used as a rubber antioxidant and can impart better resistance to heat-oxidative aging and UV-aging than the antioxidant 6PPD:
[0066]
[0067] In Formula I, each R1 is independently selected from H, C1-C18 chain hydrocarbon group and C3-C18 alicyclic hydrocarbon group, and a is an integer of 1-5;
[0068] R2, R3, R4, and R5 are each independently selected from H, a C1-C18 chain hydrocarbon group, and a C3-C18 alicyclic hydrocarbon group, and at least one of R2, R3, R4, and R5 is not H;
[0069] R6 and R7 are each independently selected from a C1-C18 chain hydrocarbon group and a C3-C18 alicyclic hydrocarbon group, or R6 and R7 form a C3-C18 aliphatic ring.
[0070] In some preferred embodiments, each R1 is independently selected from H and C1-C8 alkyl. In some embodiments, each R1 is independently selected from H, methyl, and ethyl. In some embodiments, each R1 is independently selected from H and methyl. In some embodiments, a is 1 or 2. When a is 1, R1 is preferably located in the ortho or para position relative to the -NH- group. When a is 2, preferably, the two R1s are located in the ortho and meta positions relative to the -NH- group, respectively, and the two R1s are adjacent.
[0071] In some preferred embodiments, each R1 is independently selected from a C1-C8 alkyl group. In some embodiments, each R1 is independently selected from a C1-C4 alkyl group. In some embodiments, each R1 is methyl. In some embodiments, a is 1 or 2. When a is 1, R1 is preferably located in the ortho or para position relative to the -NH- group. When a is 2, preferably, the two R1s are located in the ortho and meta positions relative to the -NH- group, respectively, and the two R1s are adjacent.
[0072] In some preferred embodiments, R2, R3, R4, and R5 are each independently selected from H and C1-C8 alkyl, and preferably, two to three of R2, R3, R4, and R5 are H. In some embodiments, R2, R3, R4, and R5 are each independently selected from H and C1-C4 alkyl. In some embodiments, R2, R3, R4, and R5 are each independently selected from H and methyl. When three of R2, R3, R4, and R5 are H, preferably, R2 is not H. When two of R2, R3, R4, and R5 are H, preferably, R2 and R4 are not H, or R2 and R3 are not H.
[0073] In some preferred embodiments, R6 and R7 are each independently selected from a C1-C8 alkyl group and a C3-C8 cycloalkyl group, or R6 and R7 form a C3-C8 aliphatic ring. In some embodiments, R6 and R7 are each independently selected from a C1-C6 alkyl group, such as a C1-C4 alkyl group, or R6 and R7 form a C5-C7 aliphatic ring, such as a C6 aliphatic ring. In some embodiments, R6 is selected from a C1-C2 alkyl group, such as a methyl group, and R7 is selected from a C1-C6 alkyl group, such as a C1-C4 alkyl group, or R6 and R7 form a C5-C7 aliphatic ring, such as a C6 aliphatic ring. Preferably, the aliphatic ring formed by R6 and R7 is a saturated aliphatic ring.
[0074] In some embodiments, each R1 is independently selected from H and C1-C4 alkyl, or each R1 is independently selected from C1-C4 alkyl, a is 1 or 2; R2, R3, R4, R5 are independently selected from H and C1-C4 alkyl, and preferably, 2 to 3 groups among R2, R3, R4, R5 are H; R6 and R7 are independently selected from C1-C6 alkyl, for example, C1-C4 alkyl, or R6 and R7 form a C5-C7 aliphatic ring, for example, a C6 aliphatic ring.
[0075] In some embodiments, each R1 is independently selected from H and C1-C4 alkyl, preferably H and methyl, or each R1 is independently selected from C1-C4 alkyl, such as methyl, a is 1, and R1 is preferably located in the ortho position of the -NH- group; R2, R3, R4, and R5 are independently selected from H and C1-C4 alkyl, preferably H and methyl, and preferably, 2 to 3 groups among R2, R3, R4, and R5 are H, wherein preferably, R2 is not H, or R2 and R3 are not H; R6 and R7 are independently selected from C1-C6 alkyl, such as C1-C4 alkyl, or R6 and R7 form a C5-C7 aliphatic ring, such as a C6 aliphatic ring.
[0076] In some embodiments, the compound of Formula I is selected from:
[0077]
[0078] Compound of formula II
[0079] The present invention also provides compounds of formula II which can be used as intermediates in the preparation of compounds of formula I:
[0080]
[0081] In Formula II, R1, a, R2, R3, R4 and R5 are as defined above for R1, a, R2, R3, R4 and R5 in any embodiment of the compound of Formula I.
[0082] In some embodiments, the compound of Formula II is selected from:
[0083]
[0084] Preparation methods of compounds of formula I and formula II
[0085] The preparation method of the compound of formula I and the compound of formula II provided by the present invention comprises the following steps:
[0086] (1) subjecting the compound represented by Formula A and the compound represented by Formula B to a condensation reaction under the action of a first catalyst to obtain a condensate comprising the compound represented by Formula C and / or the compound represented by Formula C′, and then subjecting the condensate to a reduction reaction under the action of H2 and a second catalyst to obtain the compound represented by Formula II;
[0087]
[0088] (2) subjecting the compound represented by Formula II to a reductive alkylation reaction with the compound represented by Formula D in the presence of H2 and a third catalyst to obtain the compound represented by Formula I;
[0089]
[0090] R1, R2, R3, R4, R5, R6, and R7 in Formula A, Formula B, Formula C, Formula C′, Formula D, Formula II, and Formula I are as defined in any embodiment herein.
[0091] The first catalyst used in step (1) can be one or more selected from alkali metal hydroxides, alkali metal alkoxides, quaternary ammonium bases, and combinations of alkali metal hydroxides and tetraalkylammonium halides. Suitable alkali metal hydroxides for use in the present invention include sodium hydroxide, potassium hydroxide, lithium hydroxide, etc. Suitable alkali metal alkoxides for use in the present invention include sodium methoxide, potassium methoxide, sodium ethoxide, potassium ethoxide, sodium tert-butoxide, potassium tert-butoxide, sodium tert-amyl alcoholate, potassium tert-amyl alcoholate, etc. Quaternary ammonium bases are compounds of the general formula R4NOH, wherein R is four identical or different aliphatic groups (e.g., alkyl) or aromatic groups. In some embodiments, each R group in the quaternary ammonium base is an alkyl group, for example, each R group can be independently selected from methyl, ethyl, propyl, and butyl. Examples of quaternary ammonium bases suitable for use in the present invention include tetraalkylammonium hydroxides, such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrabutylammonium hydroxide, etc. The first catalyst can also be a combination of alkali metal hydroxides and tetraalkylammonium halides. The general formula of tetraalkylammonium chloride is R4NX, where R is four identical or different aliphatic or aromatic groups, such as methyl, ethyl, propyl, butyl, etc., and X is a halogen atom, such as fluorine, chlorine, bromine, or iodine. Examples of combinations of alkali metal hydroxides and tetraalkylammonium halides include sodium hydroxide and tetrabutylammonium bromide. In some embodiments, the first catalyst is a quaternary ammonium base, such as tetraalkylammonium hydroxide. The molar ratio of the first catalyst to the compound of formula A can be 0.1:1 to 2:1, preferably 0.1:1 to 0.5:1, such as 0.2:1, 0.3:1, or 0.4:1.
[0092] In some embodiments, in step (1), the compound of formula A is first salted with the first catalyst, and then the compound of formula B is added dropwise to carry out a condensation reaction.
[0093] In step (1), the condensation product obtained by the condensation reaction of the compound of formula A and the compound of formula B under the action of the first catalyst may be one or both of the nitro compound represented by formula C and the nitroso compound represented by formula C', and may also contain an azobenzene compound. The molar ratio of the compound of formula A to the compound of formula B may be 2:1 to 15:1, preferably 4:1 to 10:1, more preferably 5:1 to 8:1, for example 6:1 or 7:1.
[0094] In step (1), the condensation reaction can be carried out at 40-90° C., preferably 65-85° C., for example, the reaction temperature can be 60° C., 70° C., 75° C., or 80° C. The condensation reaction needs to be carried out under vacuum conditions, with a vacuum degree range of -0.09 to -0.99 MPa.
[0095] The second catalyst used in step (1) can be a porous metal catalyst or a supported metal catalyst. Porous metal catalysts are also called sponge metal catalysts. Porous metal catalysts suitable for the present invention include Raney nickel (also known as skeleton nickel), Raney cobalt, Raney copper, etc. Supported metal catalysts include a metal as a catalytic active center and a carrier for supporting the metal. The metal in the supported metal catalyst suitable for the present invention can be nickel, cobalt, copper, platinum, palladium, ruthenium, rhodium, etc., and the carrier can be carbon, alumina, silica gel, molecular sieve, etc. The carbon as a carrier can be activated carbon. In some embodiments, the second catalyst is a porous metal catalyst, such as Raney nickel. The ratio of the amount of metal in the second catalyst to the amount of the condensate can be 0.0001:1 to 0.2:1.
[0096] In step (1), the condensate generated by the condensation reaction is subjected to a hydrogenation reduction reaction in the presence of a second catalyst to produce a compound of formula II. In step (1), the reduction reaction can be carried out at 40 to 120° C., preferably 60 to 90° C., for example, the reaction temperature can be 70° C., 75° C., or 80° C. The hydrogen pressure during the reduction reaction can be 0.5 to 5 MPa, preferably 0.5 to 2.5 MPa, for example, 1 MPa, 1.5 MPa, 2 MPa, or 2.5 MPa.
[0097] In step (1), compound C itself can be used as a solvent, or solvents such as toluene and xylene can be used. After the reaction in step (1) is completed, the reaction solution is filtered to recover the second catalyst, the oil-water phase is separated to recover the first catalyst, and the organic phase is distilled to remove light components to obtain the compound of formula II.
[0098] The third catalyst used in step (2) can be the aforementioned supported metal catalyst, such as Pt / C. The molar ratio of the metal in the third catalyst to the compound of formula II can be 0.0001:1 to 0.2:1.
[0099] In step (2), the compound of formula II and the compound of formula D are subjected to a hydrogenation reduction alkylation reaction under the action of a third catalyst to produce a compound of formula I. After the reaction, the carbonyl carbon atom in the compound of formula D is connected to the amino nitrogen atom in the compound of formula II. Therefore, a suitable compound of formula D can be selected for reaction based on the R6 and R7 groups contained in the compound of formula I to be prepared. The molar ratio of the compound of formula D to the compound of formula II can be 1:1 to 15:1, for example, 2:1, 3:1, 5:1, 8:1, 10:1, 14:1. The reaction temperature of step (2) can be 40 to 150°C, preferably 50 to 120°C, for example, 50°C, 70°C, 80°C, 100°C, 120°C. The hydrogen pressure in step (2) can be 0.5 to 5 MPa, preferably 0.5 to 2.5 MPa, for example, 1 MPa, 1.5 MPa, 2 MPa, 2.5 MPa.
[0100] In step (2), the compound of formula D, which is a reaction raw material, can be used as a solvent. After the reaction in step (2) is completed, the reaction solution is filtered to recover the third catalyst, and the light components are removed by vacuum distillation to obtain the compound of formula I.
[0101] In the present invention, liquid chromatography (LC) or gas chromatography (GC) can be used to determine whether each step of the reaction has reached the endpoint, thereby determining the appropriate reaction time.
[0102] The preparation methods of the compounds of formula I and formula II of the present invention are green and environmentally friendly. The preparation process of the intermediate compound of formula II does not produce wastewater, does not require the use of expensive bromides, and the catalysts can be recycled and reused.
[0103] Rubber composition and rubber product
[0104] The present invention also provides a rubber composition, wherein the rubber composition contains the compound of formula I of the present invention as an antioxidant. The compound of formula I of the present invention is hereinafter referred to as the antioxidant of the present invention.
[0105] The raw materials of the rubber composition generally include a diene elastomer, a reinforcing filler, an antioxidant, and a cross-linking agent. Herein, the rubber composition includes unvulcanized rubber and vulcanized rubber. The unvulcanized rubber can be vulcanized (cured) to produce vulcanized rubber.
[0106] The raw materials of the rubber composition of the present invention include, based on 100 parts by weight of the diene elastomer, 30-70 parts by weight of the reinforcing filler, 0.1-8 parts by weight of the antioxidant, and 0.5-3 parts by weight of the crosslinking agent. Unless otherwise specified herein, parts by weight are based on 100 parts by weight of the diene elastomer contained in the raw materials of the rubber composition.
[0107] Herein, diene elastomer refers to an elastomer whose monomers contain dienes (such as butadiene, isoprene). Diene elastomers suitable for the present invention can be various diene elastomers known in the art, including but not limited to one or more selected from natural rubber (NR), butadiene rubber (BR), isoprene rubber, styrene-butadiene rubber (SBR), chloroprene rubber (CR), acrylonitrile-butadiene rubber (NBR), isoprene / butadiene copolymer, isoprene / styrene copolymer and isoprene / butadiene / styrene copolymer. In some embodiments, in the raw materials of the rubber composition of the present invention, the diene elastomer contains natural rubber and butadiene rubber, or is composed of natural rubber and butadiene rubber; the mass ratio of natural rubber to butadiene rubber can be 1:9 to 9:1, 2:8 to 8:2, 3:7 to 7:3, 4:6 to 6:4, 4.5:5.5 to 5.5:4.5 or 1:1. In some embodiments, the diene elastomer is natural rubber.
[0108] The raw materials of the rubber composition of the present invention generally include 0.1-8 parts by weight, preferably 1-5 parts by weight, and more preferably 2±0.5 parts by weight of an antioxidant. The rubber composition of the present invention is characterized in that the antioxidant includes the antioxidant of the present invention. In the present invention, the antioxidant of the present invention can account for more than 50%, more than 60%, more than 80%, more than 90% or 100% of the total weight of the antioxidant contained in the rubber composition.
[0109] The reinforcing filler applicable to the present invention can be the reinforcing filler conventionally used for rubber composition, includes but not limited to one or more selected from carbon black, titanium oxide, magnesium oxide, calcium carbonate, magnesium carbonate, aluminum hydroxide, magnesium hydroxide, clay and talc. In some embodiments, in the rubber composition of the present invention, the reinforcing filler is carbon black. The raw material of rubber composition generally includes 30-70 weight parts, preferably 40-60 weight parts, more preferably 45-55 weight parts of reinforcing filler. In some embodiments, the raw material of rubber composition of the present invention includes 30-70 weight parts, preferably 40-60 weight parts, more preferably 45-55 weight parts, for example 50 ± 2 weight parts of carbon black.
[0110] The cross-linking agent may be sulfur. The raw materials of the rubber composition generally contain 0.5-3 parts by weight, preferably 1-3 parts by weight of a cross-linking agent. In some embodiments, the raw materials of the rubber composition of the present invention contain 0.5-3 parts by weight, preferably 1-3 parts by weight, for example 2.5±0.5 parts by weight, 2.5±0.2 parts by weight of a cross-linking agent, such as sulfur.
[0111] The raw materials of the rubber composition of the present invention may further include other ingredients commonly used in rubber compositions, including but not limited to one or more of auxiliary agents and accelerators. The amounts of the auxiliary agents and accelerators used may be conventional amounts in the art.
[0112] Auxiliary agent can include the softening agent used in order to improve the performances such as processability.Softening agent can include petroleum softening agent (process oil), such as naphthenic oil, aromatic oil, process oil, lubricating oil, paraffin, liquid paraffin, petroleum asphalt and vaseline etc., and can also include fatty oil softening agent, such as stearic acid, castor oil, linseed oil, rapeseed oil, coconut oil, wax (such as beeswax, carnauba wax and lanolin), tall oil, linoleic acid, palmitic acid and lauric acid etc. Auxiliary agent can also include activating agent, such as zinc oxide, can play the effects such as accelerating vulcanization speed, improving rubber thermal conductivity, wear resistance, tear resistance. Usually, the diene elastomer of every 100 weight parts uses the auxiliary agent of 2-20 mass parts in total. In some embodiments, the raw material of rubber combination of the present invention includes fatty oil softening agent, such as stearic acid. The raw materials of the rubber composition of the present invention may include 0-5 parts by weight, preferably 0.5-4 parts by weight, more preferably 1-3 parts by weight, for example 2±0.5 parts by weight, 2±0.2 parts by weight of a fat oil softener, such as stearic acid. In some embodiments, the raw materials of the rubber composition of the present invention include an activating agent, such as zinc oxide. The raw materials of the rubber composition of the present invention may include 0-10 parts by weight, preferably 2-8 parts by weight, more preferably 3-7 parts by weight, for example 5±1 parts by weight of an activating agent, such as zinc oxide. In some embodiments, the raw materials of the rubber composition of the present invention include a fat oil softener and an activating agent, and the respective amounts of the fat oil softener and the activating agent may be as described above.
[0113] Accelerator is generally a vulcanization accelerator, and can be selected from one or more of sulfonamide vulcanization accelerator, thiazole vulcanization accelerator, thiuram vulcanization accelerator, thiourea vulcanization accelerator, guanidine vulcanization accelerator, dithiocarbamate vulcanization accelerator, aldehyde amine vulcanization accelerator, aldehyde ammonia vulcanization accelerator, imidazoline vulcanization accelerator and xanthate vulcanization accelerator.For example, accelerator can be accelerator CBS (N- cyclohexyl -2- benzothiazole sulfenamide).In some embodiments, the raw material of rubber combination of the present invention includes accelerator, such as accelerator CBS.The raw material of rubber combination of the present invention can include 0-1.5 weight portion, preferably 0.2-1 weight portion, such as 0.6 ± 0.2 weight portion, 0.6 ± 0.1 weight portion accelerator, such as accelerator CBS.
[0114] In addition, when necessary, the rubber composition may further include plasticizers such as DMP (dimethyl phthalate), DEP (diethyl phthalate), DBP (dibutyl phthalate), DHP (diheptyl phthalate), DOP (dioctyl phthalate), DINP (diisononyl phthalate), DIDP (diisodecyl phthalate), BBP (butyl benzyl phthalate), DWP (dilauryl phthalate), and DCHP (dicyclohexyl phthalate). The amount of the plasticizer used may be a conventional amount in the art.
[0115] The unvulcanized rubber of the present invention can be prepared by conventional rubber mixing methods, for example, by a two-stage mixing method: a first stage of mixing in an internal mixer to mix the diene elastomer, reinforcing filler, additives and antioxidant to obtain a masterbatch; a second stage of mixing in an open mixer to mix the masterbatch obtained in the first stage with a crosslinking agent and an accelerator to obtain the unvulcanized rubber.
[0116] The unvulcanized rubber of the present invention can be vulcanized using conventional vulcanization methods to obtain vulcanized rubber. The vulcanization temperature is generally 130°C to 200°C, for example, 140°C to 160°C, or 150±5°C. The vulcanization time depends on the vulcanization temperature, the vulcanization system, and the vulcanization kinetics, and is generally 10-60 minutes, for example, 15±5 minutes or 15±2 minutes. Prior to vulcanization, the kneaded unvulcanized rubber can be subjected to conventional sheeting.
[0117] The present invention also provides a rubber product comprising the rubber composition of any embodiment of the present invention. The rubber product may include a tire, rubber shoes, sealing strips, sound insulation panels, vibration damping pads, and the like. In certain embodiments, the rubber product is a tire, such as a tire tread, belt, and sidewall. The tire belt may contain, in addition to the rubber composition of the present invention, a reinforcing material commonly used in the art.
[0118] The present invention also provides a use of a compound of formula I of the present invention for improving the heat-oxidative aging resistance and / or ultraviolet aging resistance of rubber or rubber products. Preferably, the rubber product is a tire. The use comprises adding the compound of formula I of the present invention to the rubber or rubber product as an antioxidant.
[0119] The present invention will be described below by way of specific examples. It should be understood that these examples are merely illustrative and are not intended to limit the scope of the present invention. The methods, reagents, and materials used in the examples are, unless otherwise stated, conventional methods, reagents, and materials in the art. The starting compounds in the examples can all be purchased from commercial sources.
[0120] Example 1: Synthesis of Compound I-1 (N-isopropyl-N′-phenyl-2-methyl-1,4-phenylenediamine)
[0121] (1) Synthesis of Compound II-1
[0122] In a 500 mL four-necked flask, 139.7 g (1.5 mol) of aniline and 91 g (0.25 mol) of a 25% aqueous solution of tetramethylammonium hydroxide (TMAOH) were added. The mixture was stirred and heated to 40-55° C., and dehydrated by vacuum distillation to form a salt between TMAOH and aniline. During this process, the reaction solution gradually changed from yellow to deep red. The temperature was gradually raised to 72° C. When the fraction reached approximately 46 mL, 34.3 g (0.25 mol) of 3-methylnitrobenzene was added dropwise by vacuum distillation at 72° C. (−0.098 MPa) for approximately 3 h. After the addition was complete, the mixture was incubated for 1 h. LC monitoring was performed to determine the complete reaction of 3-methylnitrobenzene to obtain a condensation solution.
[0123] The condensation solution was transferred to a 500 mL stainless steel reactor, and 50 g of deionized water and 40 g of skeletal nickel catalyst were added. The reaction was then hydrogenated three times, heated to 75°C, and hydrogen was introduced to 1.5 MPa for a hydrogenation reduction reaction. LC monitoring was performed until the nitro and nitroso compounds were completely reduced. The reaction was then filtered and phase separated. The organic phase was washed with water and distilled under reduced pressure (-0.1 MPa, 160°C) to remove aniline and light by-products. Finally, 42.6 g of the reduction product (Compound II-1) was distilled off, which solidified on cooling to form a yellow solid. The yield was approximately 86%, and the content was >99% as determined by GC.
[0124]
[0125] 1 H NMR (400MHz, CDCl3) δ7.22-7.15 (m, 2H), 7.03 (d, J=8.3Hz, 1H), 6.79-6.74 (m, 1H), 6.68 (dt, J=8.8, 1 .7Hz, 2H), 6.61 (d, J=2.6Hz, 1H), 6.54 (dd, J=8.3, 2.7Hz, 1H), 5.15 (s, 1H), 3.56 (s, 2H), 2.17 (s, 3H).
[0126] (2) Synthesis of Compound I-1
[0127] 40 g (0.2 mol) of compound II-1, 162.4 g (2.8 mol) of acetone, and 0.5 g of Pt / C catalyst were placed in a reactor. The atmosphere was replaced with hydrogen three times, and the temperature was raised to 70°C. Hydrogen was introduced to 1.5 MPa and the reaction was stopped when the content of compound II-1 was less than 0.1%. The temperature was lowered, the catalyst was removed by filtration, and light components were removed by distillation at -0.1 MPa and 180°C to obtain 48.3 g of compound I-1 (yield approximately 99.4%). The content was >98% as determined by GC. The solidified product cooled and solidified to a light pink solid.
[0128]
[0129] 1 H NMR (400MHz, CDCl3) δ7.20-7.11 (m, 2H), 7.03 (d, J=8.4Hz, 1H), 6.77-6.70 (m, 1H), 6.65 (dt, J=8.8, 1. 7Hz, 2H), 6.50 (d, J=2.7Hz, 1H), 6.44 (dd, J=8.4, 2.7Hz, 1H), 5.13 (s, 1H), 3.71-3.43 (m, 1H), 3.34 (br s, 1H), 2.17 (s, 3H), 1.23 (d, J=6.3Hz, 6H).
[0130] Example 2: Synthesis of Compound I-2 (N-1,3-dimethylbutyl-N′-phenyl-2,6-dimethyl-1,4-phenylenediamine)
[0131] (1) Synthesis of Compound II-2
[0132] In a 500 mL four-necked flask, 186.2 g (2 mol) of aniline and 91 g (0.25 mol) of a 25% aqueous solution of tetramethylammonium hydroxide (TMAOH) were added. The mixture was stirred and heated to 40-55° C., and dehydrated by vacuum distillation to form a salt between TMAOH and aniline. During this process, the reaction solution gradually changed from yellow to deep red. The temperature was gradually raised to 72° C. When the fraction reached approximately 46 mL, 37.8 g (0.25 mol) of 3,5-dimethylnitrobenzene was added dropwise by vacuum distillation at 72° C. (−0.098 MPa) for approximately 3 h. After the addition was complete, the mixture was incubated for 1 h. LC monitoring was performed to determine the complete reaction of 3,5-dimethylnitrobenzene to obtain a condensation solution.
[0133] The condensation solution was transferred to a 500 mL stainless steel reactor, and 50 g of deionized water and 50 g of skeletal nickel catalyst were added. The reaction was then hydrogenated three times, heated to 75°C, and hydrogen was introduced to 1.5 MPa for a hydrogenation reduction reaction. LC monitoring was performed until the nitro and nitroso compounds were completely reduced. The reaction was then filtered and phase separated. The organic phase was washed with water and distilled under reduced pressure (-0.1 MPa, 160°C) to remove aniline and light by-products. Finally, 44.3 g of the reduction product (Compound II-2) was distilled off, which solidified on cooling to form a light green solid. The yield was approximately 82%, and the content was >98% as determined by GC.
[0134]
[0135] H NMR (400MHz, CDCl3) δ7.15 (dd, J=17.7, 10.1Hz, 2H), 6.70 (t, J=7.3Hz, 1H), 6.49 (s, 2H), 6.47 (d, J=5.7Hz, 2H), 4.98 (s, 1H), 3.55 (s, 2H), 2.14 (s, 6H).
[0136] 13 C NMR (101MHz, CDCl3) δ147.62, 144.52, 138.11, 129.47, 129.33, 117.47, 115.09, 112.85, 18.44.
[0137] (2) Synthesis of Compound I-2
[0138] 43.2 g (0.2 mol) of compound II-2, 160.3 g (1.6 mol) of 4-methyl-2-pentanone, and 0.5 g of Pt / C catalyst were placed in a reactor. The atmosphere was replaced with hydrogen three times, and the temperature was raised to 90°C. Hydrogen was introduced to 1.5 MPa and the reaction was stopped when the content of compound II-2 was less than 0.1%. The temperature was lowered, the catalyst was removed by filtration, and light components were removed by distillation at -0.1 MPa and 180°C to obtain 59.5 g of compound I-2 (yield: approximately 99.5%). The content was greater than 98.2% as determined by GC. It was a dark red liquid at room temperature.
[0139]
[0140] 1 H NMR (400MHz, CDCl3) δ7.13 (dd, J=8.4, 7.4Hz, 2H), 6.68 (t, J=7.3Hz, 1H), 6.48 (d, J=7.6Hz, 2H), 6.36 (s, 2H), 4.97 (s, 1H), 3.62-3.39 (m, 1H), 3.28 (s, 1H), 2.14 (s, 6H), 1.87-1.71 (m, 1H), 1.45-1.52 (m, 1H), 1.35-1.23 (m , 1H), 1.18 (d, J=6.2Hz, 3H), 0.97 (d, J=6.6Hz, 3H), 0.95 (d, J=6.6Hz, 3H).
[0141] 13 C NMR (101MHz, CDCl3) δ147.86, 145.96, 138.07, 129.25, 127.83, 117.21, 112.81, 112.73, 47.15, 46.71, 25.21, 23.07, 22.71, 21.28, 18.61.
[0142] Example 3: Synthesis of Compound I-3 (N-cyclohexyl-N′-phenyl-2,6-dimethyl-1,4-phenylenediamine)
[0143] (1) Synthesis of Compound II-2
[0144] The synthesis of compound II-2 is the same as in Example 2.
[0145] (2) Synthesis of Compound I-3
[0146] 43.2 g (0.2 mol) of compound II-2, 156.8 g (1.6 mol) of cyclohexanone, and 0.5 g of Pt / C catalyst were placed in a reactor. The atmosphere was replaced with hydrogen three times, and the temperature was raised to 100°C. Hydrogen was introduced to 1.5 MPa and the reaction was continued. GC analysis was performed. When the content of compound II-2 was <0.1%, the reaction was stopped. The temperature was lowered, the catalyst was removed by filtration, and light components were removed by distillation at -0.1 MPa and 180°C to obtain 59.6 g of compound I-3 (yield: approximately 99.5%). The content was >98.2% as determined by GC analysis. It was a dark red liquid at room temperature.
[0147]
[0148] 1 H NMR (400MHz, CDCl3) δ7.16 (dd, J=8.4, 7.4Hz, 2H), 6.71 (t, J=7.3Hz, 1H), 6.50 (d, J=7.6Hz, 2H), 6.41 (s, 2H), 4.99 (s, 1H), 3.50 (s, 1 H), 3.38-3.18(m, 1H), 2.17(s, 6H), 2.16-2.06(m, 2H), 1.89-1.76(m, 2H), 1.76-1.64(m, 1H), 1.51-1.36(m, 2H), 1.35-1.09(m, 3H).
[0149] 13 C NMR (101MHz, CDCl3) δ147.83, 145.62, 138.02, 129.21, 127.87, 117.18, 112.87, 112.69, 51.86, 33.69, 26.01, 25.11, 18.56.
[0150] Example 4: Synthesis of Compound I-4 (N-cyclohexyl-N′-2-methylphenyl-2-methyl-1,4-phenylenediamine)
[0151] (1) Synthesis of Compound II-4
[0152] In a 500 mL four-necked flask, 160.5 g (1.5 mol) of 2-methylaniline and 91 g (0.25 mol) of a 25% aqueous solution of tetramethylammonium hydroxide (TMAOH) were added, the temperature was raised to 40-50° C. with stirring, and dehydration was carried out by distillation under reduced pressure to form a salt between TMAOH and 2-methylaniline. During this process, the reaction solution gradually changed from yellow to deep red. The temperature was gradually raised to 72° C. When the fraction was approximately 50% of the amount of the 25% tetramethylammonium hydroxide solution of the catalyst charged, 34.3 g (0.25 mol) of 3-methylnitrobenzene was added dropwise under reduced pressure (−0.098 MPa) at 72° C. The addition time was about 3 h. After the addition was complete, the temperature was kept for 1 h. LC monitoring was performed to obtain a condensation solution.
[0153] The condensation solution was transferred to a 500 mL stainless steel reactor, and 50 g of deionized water and 40 g of skeletal nickel catalyst were added. The reaction was replaced with hydrogen three times, and the temperature was raised to 75°C and the pressure was increased to 1.5 MPa. LC monitoring was performed until the nitro and nitroso compounds were completely reduced. The reaction was then filtered, washed with water, and the phases were separated. The organic phase was distilled under reduced pressure (-0.1 MPa, 170°C) to remove light components to obtain 42.8 g of compound II-4 (yield approximately 80%). The GC assay showed a content of >98%, and the product was a light yellow solid at room temperature.
[0154]
[0155] 1 H NMR (400MHz, CDCl3) δ7.09 (d, J=7.3Hz, 1H), 6.99 (t, J=7.7Hz, 1H), 6.91 (d, J=8.2Hz, 1H) , 6.69 (t, J=7.3Hz, 1H), 6.55 (s, 1H), 6.49 (dd, J=14.3, 5.2Hz, 2H), 4.91 (s, 1H), 3.48 (br s, 2H), 2.23 (s, 3H), 2.11 (s, 3H).
[0156] 13 C NMR (101MHz, CDCl3) δ144.96, 143.28, 134.47, 131.88, 130.36, 126.83, 126.36, 123.02, 118.25, 117.60, 113.65, 113.07, 17.90, 17.62.
[0157] (2) Synthesis of Compound I-4
[0158] 42.8 g (0.2 mol) of compound II-4, 156.8 g (1.6 mol) of cyclohexanone, and 0.5 g of Pt / C catalyst were placed in a reactor. The atmosphere was replaced with hydrogen three times, and the temperature was raised to 100°C. Hydrogen was introduced to 1.5 MPa and the reaction was continued. GC was used to detect the content of compound II-4. The reaction was stopped when the content of compound II-4 was less than 0.1%. The temperature was lowered, the catalyst was removed by filtration, and light components were removed by distillation at -0.1 MPa and 180°C to obtain 59.6 g of compound I-4 (yield: approximately 99.5%). The content of the compound I-4 was greater than 98.2% as determined by GC. The compound I-4 was a dark brown liquid at room temperature.
[0159]
[0160] 1 H NMR (400MHz, CDCl3) δ7.17 (d, J=7.3Hz, 1H), 7.10-7.04 (m, 1H), 7.02 (d, J=8.4Hz, 1 H), 6.76 (td, J=7.3, 0.9Hz, 1H), 6.60-6.56 (m, 2H), 6.51 (dd, J=8.4, 2.7Hz, 1H), 4. 99(s, 1H), 3.51(s, 1H), 3.37-3.23(m, 1H), 2.33(s, 3H), 2.21(s, 3H), 2.18-2.10(m , 2H), 1.90-1.80(m, 2H), 1.78-1.69(m, 1H), 1.52-1.39(m, 2H), 1.37-1.16(m, 3H).
[0161] 13 C NMR (101MHz, CDCl3) δ145.36, 144.83, 134.97, 130.30, 130.26, 127.05, 126.85, 12 2.56, 117.88, 115.60, 112.70, 111.64, 52.10, 33.64, 26.00, 25.10.18.12.17.63.
[0162] Example 5: Synthesis of Compound I-5 (N-1,3-dimethylbutyl-N′-2-methylphenyl-2-methyl-1,4-phenylenediamine)
[0163] (1) Synthesis of Compound II-4
[0164] The synthesis of compound II-4 is the same as that of Example 4.
[0165] (2) Synthesis of Compound I-5
[0166] 43.2 g (0.2 mol) of compound II-4, 160.3 g (1.6 mol) of 4-methyl-2-pentanone, and 0.5 g of Pt / C catalyst were placed in a reactor. The atmosphere was replaced with hydrogen three times, and the temperature was raised to 100°C. Hydrogen was introduced to 1.5 MPa and the reaction was stopped when the content of compound II-2 was <0.1%. The temperature was lowered, the catalyst was removed by filtration, and light components were removed by distillation at -0.1 MPa and 180°C to obtain 59.6 g of compound I-3 (yield: approximately 99.5%). The content was >98.2% as determined by GC. It was a dark red liquid at room temperature.
[0167]
[0168] 1 H NMR (400MHz, CDCl3) δ7.15 (d, J=7.3Hz, 1H), 7.08-7.03 (m, 1H), 7.01 (d, J=8.4Hz, 1H), 6.74 (td, J=7.3 , 1.0Hz, 1H), 6.59-6.53 (m, 2H), 6.49 (dd, J=8.4, 2.7Hz, 1H), 4.97 (s, 1H), 3.65-3.51 (m, 1H), 3.21 (br s, 1H), 2.31 (s, 3H), 2.19 (s, 3H), 1.90-1.75 (m, 1H), 1.59-1.47 (m, 1H), 1.38-1 .28 (m, 1H), 1.22 (d, J = 6.2Hz, 3H), 1.01 (d, J = 6.6Hz, 3H), 0.99 (d, J = 6.6Hz, 3H).
[0169] 13 C NMR (101MHz, CDCl3) δ145.40, 145.20, 135.03, 130.35, 130.23, 127.11, 126.90, 122.60, 1 17.92, 115.55, 112.76, 111.53, 47.09, 46.93, 25.19, 23.08, 22.68, 21.23, 18.18, 17.67.
[0170] Example 6: Synthesis of Compound I-6 (N-cyclohexyl-N′-4-methylphenyl-2-methyl-1,4-phenylenediamine)
[0171] (1) Synthesis of Compound II-6
[0172] In a 500mL four-necked flask, 160.5g (1.5mol) of 4-methylaniline and 100.1g (0.275mol) of a 25% aqueous solution of tetramethylammonium hydroxide (TMAOH) were added, and the mixture was stirred and heated to 40-50°C. The mixture was dehydrated by distillation under reduced pressure to form a salt between TMAOH and 4-methylaniline. During this process, the reaction solution gradually changed from yellow to dark red. The temperature was gradually increased to 72°C. When the fraction was approximately 50% of the amount of the 25% tetramethylammonium hydroxide solution of the catalyst, 34.3g (0.25mol) of 3-methylnitrobenzene was added dropwise under reduced pressure (-0.098MPa) at 72°C. The addition time was about 3h. After the addition was complete, the mixture was kept warm for 1h. The reaction was monitored by LC to obtain a condensation solution.
[0173] The condensation solution was transferred to a 500 mL stainless steel reactor, and 50 g of deionized water and 40 g of skeletal nickel catalyst were added. The reaction was replaced with hydrogen three times, and the temperature was raised to 75°C and the pressure was increased to 1.5 MPa. LC monitoring was performed until the nitro and nitroso compounds were completely reduced. The reaction was then filtered, washed with water, and the phases were separated. The organic phase was distilled under reduced pressure (-0.1 MPa, 170°C) to remove light components to obtain 46.1 g of compound II-6 (yield approximately 86%). The GC assay showed a content of >98%, and the product was a light yellow solid at room temperature.
[0174]
[0175] 1 H NMR (400MHz, CDCl3) δ7.01 (t, J=6.6Hz, 3H), 6.67-6.63 (m, 2H), 6.62 (d, J=2.5Hz, 1H ), 6.55 (dd, J=8.3, 2.6Hz, 1H), 5.02 (s, 1H), 3.38 (s, 2H), 2.29 (s, 3H), 2.19 (s, 3H).
[0176] 13 C NMR (101MHz, CDCl3) δ144.36, 142.87, 133.94, 132.41, 129.72, 127.73, 125.32, 117.69, 114.90, 113.67, 20.47, 17.99.
[0177] (2) Synthesis of Compound I-6
[0178] 42.8 g (0.2 mol) of compound II-6, 156.8 g (1.6 mol) of cyclohexanone, and 0.5 g of Pt / C catalyst were placed in a reactor, replaced with hydrogen three times, and then heated to 100°C. Hydrogen was introduced to 1.5 MPa for reaction, and the reaction was stopped when the content of compound II-6 was <0.1%. The temperature was lowered, the catalyst was removed by filtration, and light components were removed by distillation at -0.1 MPa and 180°C to obtain 59.6 g of compound I-6 (yield of approximately 99.5%). The content was >98.2% as determined by GC. It was a dark brown liquid at room temperature.
[0179]
[0180] 1 H NMR (400MHz, CDCl3) δ6.99 (t, J=8.2Hz, 3H), 6.60 (d, J=8.4Hz, 2H), 6.51 (d, J=2.5Hz, 1H), 6.45 (dd, J=8.4, 2.7Hz, 1H), 5.04 (s, 1H), 3.40 (s, 1H ), 3.29-3.17(m, 1H), 2.26(s, 3H), 2.17(s, 3H), 2.12-2.04(m, 2H), 1.83 -1.75(m, 2H), 1.72-1.61(m, 1H), 1.51-1.31(m, 2H), 1.28-1.13(m, 3H).
[0181] 13 C NMR (101MHz, CDCl3) δ144.85, 144.56, 134.52, 130.81, 129.71, 127.39, 12 6.12, 115.71, 114.54, 111.69, 52.22, 33.70, 26.03, 25.12, 20.48, 18.22.
[0182] Example 7: Synthesis of Compound I-7 (N-1,3-dimethylbutyl-N′-4-methylphenyl-2-methyl-1,4-phenylenediamine)
[0183] (1) Synthesis of Compound II-6
[0184] The synthesis of compound II-6 is the same as that of Example 6
[0185] (2) Synthesis of Compound I-7
[0186] 43.2 g (0.2 mol) of compound II-6, 160.3 g (1.6 mol) of 4-methyl-2-pentanone, and 0.5 g of Pt / C catalyst were placed in a reactor. The atmosphere was replaced with hydrogen three times, and the temperature was raised to 100°C. Hydrogen was introduced to 1.5 MPa and the reaction was stopped when the content of compound II-6 was <0.1%. The temperature was lowered, the catalyst was removed by filtration, and light components were removed by distillation at -0.1 MPa and 180°C to obtain 59.6 g of compound I-3 (yield: approximately 99.5%). The content was >98.2% as determined by GC. It was a dark red liquid at room temperature.
[0187]
[0188] 1 H NMR (400MHz, CDCl3) δ6.96 (dd, J=9.8, 8.6Hz, 3H), 6.57 (d, J=8.4Hz, 2H), 6.46 (d, J =2.3Hz, 1H), 6.40 (dd, J = 8.4, 2.5Hz, 1H), 4.98 (s, 1H), 3.58-3.40 (m, 1H), 3.25 (br s, 1H), 2.22 (s, 3H), 2.14 (s, 3H), 1.82-1.68 (m, 1H), 1.52-1.36 (m, 1H), 1.31-1 .19 (m, 1H), 1.15 (d, J = 6.2Hz, 3H), 0.94 (d, J = 6.6Hz, 3H), 0.92 (d, J = 6.6Hz, 3H).
[0189] 13 C NMR (101MHz, CDCl3) δ144.92, 134.61, 130.72, 129.74, 127.34, 126.24, 115. 60, 114.55, 111.51, 47.13, 46.99, 25.21, 23.10, 22.71, 21.26, 20.52, 18.27.
[0190] Example 8: Synthesis of Compound I-8 (N-cyclohexyl-N′-2,3-dimethylphenyl-2-methyl-1,4-phenylenediamine)
[0191] (1) Synthesis of Compound II-8
[0192] In a 500 mL four-necked flask, 181.5 g (1.5 mol) of 2,3-dimethylaniline and 100.1 g (0.275 mol) of a 25% aqueous solution of tetramethylammonium hydroxide (TMAOH) were added dropwise. The mixture was stirred and heated to 40-50° C., and dehydrated by vacuum distillation to form a salt between TMAOH and 2,3-dimethylaniline. During this process, the reaction solution gradually changed from yellow to deep red. The temperature was gradually raised to 72° C. When the fraction was approximately 50% of the amount of the 25% tetramethylammonium hydroxide solution of the catalyst charged, 34.3 g (0.25 mol) of 3-methylnitrobenzene was added dropwise at 72° C. under reduced pressure (−0.098 MPa) for approximately 3 h. After the addition was complete, the mixture was incubated for 1 h. LC monitoring was performed to obtain a condensation solution.
[0193] The condensation solution was transferred to a 500 mL stainless steel reactor, and 50 g of deionized water and 40 g of skeletal nickel catalyst were added. The reaction was replaced with hydrogen three times, and the temperature was raised to 75°C and the pressure was increased to 1.5 MPa. LC monitoring was performed until the nitro and nitroso compounds were completely reduced. The reaction was then filtered, washed with water, and the phases were separated. The organic phase was distilled under reduced pressure (-0.1 MPa, 180°C) to remove light components to obtain 46.6 g of compound II-8 (yield approximately 80%). The GC assay showed a content of >97%. After cooling, the product was a light yellow solid.
[0194]
[0195] 1 H NMR (400MHz, CDCl3) δ6.93 (t, J=7.8Hz, 1H), 6.88 (d, J=8.3Hz, 1H), 6.68 (d, J=7.4Hz, 1H), 6.62 (d, J=2.1Hz, 1H ), 6.58-6.50 (m, 1H), 6.46 (d, J=8.1Hz, 1H), 4.95 (s, 1H), 3.53 (s, 2H), 2.33 (s, 3H), 2.19 (s, 3H), 2.16 (s, 3H).
[0196] 13 C NMR (101MHz, CDCl3) δ144.73, 142.86, 137.04, 133.81, 132.84, 125.97, 125.55, 122.39, 120.95, 117.73, 113.75, 112.33, 20.72, 17.98, 12.99.
[0197] (2) Synthesis of Compound I-8
[0198] 46.6 g (0.2 mol) of compound II-8, 156.8 g (1.6 mol) of cyclohexanone, and 0.5 g of Pt / C catalyst were placed in a reactor, replaced with hydrogen three times, and then heated to 100°C. Hydrogen was introduced to 1.5 MPa for reaction, and the reaction was stopped when the content of compound II-8 was <0.1%. The temperature was lowered, the catalyst was removed by filtration, and light components were removed by distillation at -0.1 MPa and 180°C to obtain 65.9 g of compound I-8 (yield: approximately 99.5%). The content was >97.6% as determined by GC. It was a red liquid at room temperature.
[0199]
[0200] 1 H NMR (400MHz, CDCl3) δ7.02-6.86 (m, 2H), 6.68 (d, J=7.4Hz, 1H), 6.54 (d, J=2.6Hz, 1H), 6.51-6.41 (m, 2H), 4.96 (s, 1H), 3.51 (br s, 1H), 3.39 -3.07(m,1H),2.35(s,3H),2.22(s,3H),2.18(s,3H),2.16-2.05(m,2H),1 .88-1.76(m, 2H), 1.75-1.64(m, 1H), 1.49-1.34(m, 2H), 1.34-1.11(m, 3H).
[0201] 13 C NMR (101MHz, CDCl3) δ145.18, 144.54, 136.88, 134.42, 131.08, 126.40, 125.95, 1 21.69, 120.48, 115.72, 111.74, 52.21, 33.70, 26.04, 25.13, 20.71.18.16.12.90.
[0202] Example 9: Synthesis of Compound I-9 (N-isopropyl-N′-4-methylphenyl-2-methyl-1,4-phenylenediamine)
[0203] (1) Synthesis of Compound II-8
[0204] The synthesis of compound II-8 is the same as that of Example 8
[0205] (2) Synthesis of Compound I-9
[0206] 46.6 g (0.2 mol) of compound II-8, 162.4 g (2.8 mol) of acetone, and 0.5 g of Pt / C catalyst were placed in a reactor. The atmosphere was replaced with hydrogen three times, and the temperature was raised to 70°C. Hydrogen was passed through the reactor to 1.5 MPa. The reaction was detected by GC. When the content of compound II-8 was less than 0.1%, the reaction was stopped. The temperature was lowered, the catalyst was removed by filtration, and light components were removed by distillation at -0.1 MPa and 180°C to obtain 54.9 g of compound I-9 (yield: approximately 99.5%). The content was greater than 97% as determined by GC. It was an off-white solid at room temperature.
[0207]
[0208] 1 H NMR (400MHz, CDCl3) δ7.01-6.93 (m, 2H), 6.71 (d, J=7.4Hz, 1H), 6.57 (d, J=2.6Hz, 1H), 6.50 (dd, J=8.3, 2.8Hz, 2H), 4.99 (br s, 1H), 3.78-3.56 (m, 1H), 3.13 (br s, 1H), 2.38 (s, 3H), 2.24 (s, 3H), 2.21 (s, 3H), 1.28 (d, J=6.3Hz, 6H).
[0209] 13 C NMR (101MHz, CDCl3) δ145.10, 144.59, 136.85, 134.30, 131.20, 126.28, 125.92 , 121.71, 120.29, 115.81, 111.81, 111.78, 44.66, 23.15, 20.68, 18.13.12.88.
[0210] Example 10: Synthesis of Compound I-10 (N-isopropyl-N′-2,3-dimethylphenyl-2,3-dimethyl-1,4-phenylenediamine)
[0211] (1) Synthesis of Compound II-10
[0212] In a 500 mL four-necked flask, 181.5 g (1.5 mol) of 2,3-dimethylaniline and 100.1 g (0.275 mol) of a 25% aqueous solution of tetramethylammonium hydroxide (TMAOH) were added dropwise. The mixture was stirred and heated to 40-50° C., and dehydrated by vacuum distillation to form a salt between TMAOH and 2,3-dimethylaniline. During this process, the reaction solution gradually changed from yellow to deep red. The temperature was gradually increased to 72° C. When the fraction was approximately 50% of the amount of the 25% tetramethylammonium hydroxide solution of the catalyst charged, 37.8 g (0.25 mol) of 2,3-dimethylnitrobenzene was added dropwise at 72° C. under reduced pressure (−0.098 MPa) for about 3 hours. After the addition was complete, the mixture was kept warm for 2 hours. LC monitoring was performed to obtain a condensation solution.
[0213] The condensation solution was transferred to a 500 mL stainless steel reactor, and 50 g of deionized water and 40 g of skeletal nickel catalyst were added. The reaction was replaced with hydrogen three times, and the temperature was raised to 75°C and the pressure was increased to 1.5 MPa. LC monitoring was performed until the nitro and nitroso compounds were completely reduced. The reaction was then filtered, washed with water, and the phases were separated. The organic phase was distilled under reduced pressure (-0.1 MPa, 180°C) to remove light components to obtain 47.5 g of compound II-10 (yield approximately 76%). The GC assay showed a content of >96%. After cooling, the product was a light yellow liquid.
[0214]
[0215] 1 H NMR (400MHz, CDCl3) δ6.91 (t, J=7.9Hz, 1H), 6.87 (d, J=8.3Hz, 1H), 6.67 (d, J=7.5Hz, 1H), 6.58 (d, J=8.2Hz , 1H), 6.27 (d, J=8.2Hz, 1H), 4.93 (s, 1H), 3.52 (s, 2H), 2.35 (s, 3H), 2.21 (s, 3H), 2.18 (s, 3H), 2.16 (s, 3H).
[0216] (2) Synthesis of Compound I-10
[0217] 37.5 g (0.15 mol) of compound II-10, 162.4 g (2.8 mol) of acetone, and 0.5 g of Pt / C catalyst were placed in a reactor. The atmosphere was replaced with hydrogen three times, and the temperature was raised to 70°C. Hydrogen was passed through the reactor to 1.5 MPa, and the reaction was stopped when the content of compound II-10 was <0.1%. The temperature was lowered, the catalyst was removed by filtration, and light components were removed by distillation at -0.1 MPa and 180°C to obtain 43.7 g of compound I-10 (yield: approximately 99.4%). The content was >96% as determined by GC. It was an off-white solid at room temperature.
[0218]
[0219] 1 H NMR (400MHz, CDCl3) δ6.90 (t, J=7.7Hz, 1H), 6.84 (d, J=8.0Hz, 1H), 6.57 (d, J=7.5Hz, 1H), 6.55 (d, J=8.1Hz, 1H), 6.23 (d, J=8.1Hz, 1H), 4.95 (s, 1H), 3.76-3.53 (m, 1H), 3.12 (s, 1H), 2.35 (s, 3H), 2.21 (s, 3H), 2.17 (s, 6H), 1.29 (d, J=6.2Hz, 6H).
[0220] Test Case
[0221] According to the formulation shown in Table 1, the following steps were used to prepare compounds 1-4:
[0222] 1. Add natural rubber SCR5 to an internal mixer and knead for a period of time, then add carbon black N330, aromatic oil, zinc oxide, stearic acid and antioxidant (6PPD, compound I-1, compound I-2 or compound I-4), and continue kneading until the mixture is uniform; during the kneading period, the temperature is controlled between 150°C and 160°C;
[0223] 2. Cool the entire mixture to below 100°C, then add the crosslinking system (sulfur S and accelerator CBS) and knead the entire mixture; control the temperature not to exceed 110°C during kneading;
[0224] 3. The obtained rubber composition was rolled into a sheet (thickness of 2-3 mm) and vulcanized at a temperature of 150° C. for 15 minutes.
[0225] The sources of the materials in Table 1 are as follows:
[0226] SCR5: natural rubber SCR5 from Xishuangbanna Sinochem Rubber Co., Ltd.
[0227] N330: Cabot Corporation carbon black N330;
[0228] Stearic acid: general reagent stearic acid (AR) from Shanghai Titan Technology Co., Ltd.;
[0229] Zinc oxide: general reagent zinc oxide (AR) from Shanghai Titan Technology Co., Ltd.;
[0230] CBS: CBS vulcanization accelerator from Senao Chemical Technology Co., Ltd.
[0231] S: Sublimed sulfur (AR) from Sinopharm Chemical Reagent Company;
[0232] 6PPD: antioxidant SIRANTOX 6PPD from Sennics Technology Co., Ltd.;
[0233] Compound I-1: the compound synthesized in Example 1;
[0234] Compound I-2: the compound synthesized in Example 2;
[0235] Compound I-4: the compound synthesized in Example 4.
[0236] Table 1: Rubber compound formula (unit: mass parts)
[0237] Formula Rubber compound 1 Rubber compound 2 Rubber compound 3 Rubber compound 4SCR5100.0100.0100.0100.0N33050.050.050.050.0
[0238] Zinc oxide 5.05.05.05.0 Stearic acid 2.02.02.02.06 PPD 2.5 Compound I-1 2.5 Compound I-2 2.5 Compound I-4 2.5 CBS 0.60.60.60.6 S 2.52.52.52.5 Total 162.6162.6162.6162.6
[0239] According to GB / T 16585 Test method for artificial weathering of vulcanized rubber (fluorescent ultraviolet lamp), the anti-ultraviolet light aging test was carried out on the rubber materials 1-4. The test conditions, parameters and steps are shown in Table 2, and the test results are shown in Table 3.
[0240] According to GB / T 528-2009, Determination of tensile stress-strain properties of vulcanized or thermoplastic rubber, the physical properties (tensile strength, elongation at break) of compounds 1-4 were measured. The results are shown in Table 3.
[0241] Thermal oxidative aging tests were conducted on compounds 1-4 in accordance with GB / T 3512-2014 Vulcanized rubber or thermoplastic rubber - Hot air accelerated aging and heat resistance tests. The test conditions were: 100°C for 48 hours. The test results are shown in Table 3.
[0242] Table 2: Anti-UV aging test parameters and test steps
[0243]
[0244] Table 3: Original physical properties and physical properties of vulcanized rubber after aging
[0245]
[0246] The test results in Table 3 demonstrate that compounds 2-4 containing the antioxidant of the present invention exhibit superior thermal oxygen aging resistance and UV aging resistance compared to compound 1 containing 6PPD. Regarding thermal oxygen aging resistance, after aging at 100°C for 48 hours, the property retention of compounds 2-4 was approximately 10% higher than that of compound 1. Regarding UV aging resistance, after aging for 168 hours according to the test parameters in Table 2, the property retention of compounds 2-4 was over 5% higher than that of compound 1.
Claims
1. The compound represented by formula I: In formula I, each R1 is independently selected from H, C1-C18 chain hydrocarbon group and C3-C18 alicyclic hydrocarbon group, and a is an integer from 1 to 5; R2, R3, R4, and R5 are each independently selected from H, a C1-C18 chain hydrocarbon group, and a C3-C18 alicyclic hydrocarbon group, and at least one of R2, R3, R4, and R5 is not H; R6 and R7 are each independently selected from a C1-C18 chain hydrocarbon group and a C3-C18 alicyclic hydrocarbon group, or R6 and R7 form a C3-C18 aliphatic ring.
2. The compound according to claim 1, wherein Each R1 is independently selected from H and C1-C8 alkyl, and a is an integer from 1 to 2; R2, R3, R4, and R5 are each independently selected from H and C1-C8 alkyl, and 2 to 3 of R2, R3, R4, and R5 are H; R6 and R7 are each independently selected from C1-C8 alkyl and C3-C8 cycloalkyl, or R6 and R7 form a C3-C8 aliphatic ring.
3. The method for preparing the compound according to claim 1, characterized in that The preparation method comprises the following steps: (1) subjecting the compound represented by Formula A and the compound represented by Formula B to a condensation reaction under the action of a first catalyst to obtain a condensate comprising the compound represented by Formula C and / or the compound represented by Formula C′, and then subjecting the condensate to a reduction reaction under the action of H2 and a second catalyst to obtain the compound represented by Formula II; (2) subjecting the compound represented by Formula II to a reductive alkylation reaction with the compound represented by Formula D in the presence of H2 and a third catalyst to obtain the compound represented by Formula I; R1, R2, R3, R4, R5, R6, and R7 in Formula A, Formula B, Formula C, Formula C′, Formula D, Formula II, and Formula I are as defined in claim 1.
4. The preparation method according to claim 3, wherein The preparation method has one or more of the following characteristics: The first catalyst is selected from one or more of an alkali metal hydroxide, an alkali metal alkoxide, a quaternary ammonium base, and a combination of an alkali metal hydroxide and a tetraalkylammonium halide; The second catalyst is a porous metal catalyst or a supported metal catalyst; the porous metal catalyst is preferably selected from one or more of Raney nickel, Raney cobalt and Raney copper, the metal in the supported metal catalyst is preferably selected from one or more of nickel, cobalt, copper, platinum, palladium, ruthenium and rhodium, and the carrier in the supported metal catalyst is preferably selected from one or more of carbon, alumina, silica gel and molecular sieve; The third catalyst is a supported metal catalyst; the metal in the supported metal catalyst is preferably selected from one or more of nickel, cobalt, copper, platinum, palladium, ruthenium and rhodium, and the carrier in the supported metal catalyst is preferably selected from one or more of carbon, alumina, silica gel and molecular sieve; In step (1), the molar ratio of the compound represented by formula A to the compound represented by formula B is 2:1 to 15:1, preferably 4:1 to 10:1; In step (1), the condensation reaction temperature is 40 to 90° C., preferably 65 to 85° C., and the vacuum degree is -0.09 to -0.99 MPa; In step (1), the temperature of the reaction between the condensate and H2 is 40 to 120°C, preferably 60 to 90°C, and the hydrogen pressure is 0.5 to 5 MPa, preferably 0.5 to 2.5 MPa; In step (2), the molar ratio of the compound represented by formula D to the compound represented by formula II is 1:1 to 15:1; In step (2), the reaction temperature is 40-150° C., and the reaction pressure is 0.5-5 MPa.
5. Compound represented by formula II: In formula II, each R1 is independently selected from H, C1-C18 chain hydrocarbon group and C3-C18 alicyclic hydrocarbon group, and a is an integer from 1 to 5; R2, R3, R4, and R5 are each independently selected from H, a C1-C18 chain hydrocarbon group, and a C3-C18 alicyclic hydrocarbon group, and at least one of R2, R3, R4, and R5 is not H.
6. The compound according to claim 5, wherein Each R1 is independently selected from H and C1-C8 alkyl, and a is an integer from 1 to 2; R2, R3, R4, and R5 are each independently selected from H and C1-C8 alkyl, and 2 to 3 groups among R2, R3, R4, and R5 are H.
7. The method for preparing the compound according to claim 5, characterized in that: The preparation method comprises: subjecting a compound represented by formula A and a compound represented by formula B to a condensation reaction under the action of a first catalyst to obtain a condensate comprising a compound represented by formula C and / or a compound represented by formula C′; and then subjecting the condensate to a reduction reaction under the action of H2 and a second catalyst to obtain a compound represented by formula II; R1, R2, R3, R4 and R5 in Formula A, Formula B, Formula C, Formula C′ and Formula II are as defined in claim 5.
8. The preparation method according to claim 7, wherein The preparation method has one or more of the following characteristics: The first catalyst is selected from one or more of an alkali metal hydroxide, an alkali metal alkoxide, a quaternary ammonium base, and a combination of an alkali metal hydroxide and a tetraalkylammonium halide; The second catalyst is a porous metal catalyst or a supported metal catalyst; the porous metal catalyst is preferably selected from one or more of Raney nickel, Raney cobalt and Raney copper, the metal in the supported metal catalyst is preferably selected from one or more of nickel, cobalt, copper, platinum, palladium, ruthenium and rhodium, and the carrier in the supported metal catalyst is preferably selected from one or more of carbon, alumina, silica gel and molecular sieve; In step (1), the molar ratio of the compound represented by formula A to the compound represented by formula B is 2:1 to 15:1, preferably 4:1 to 10:1; In step (1), the condensation reaction temperature is 40 to 90° C., preferably 65 to 85° C., and the vacuum degree is -0.09 to -0.99 MPa; In step (1), the temperature for the reaction of the condensate and H2 is 40-120°C, preferably 60-90°C, and the hydrogen pressure is 0.5-5 MPa, preferably 0.5-2.5 MPa.
9. A rubber composition, characterized in that The rubber composition contains the compound according to claim 1 or 2.
10. A rubber product, characterized in that: The rubber product comprises the rubber composition according to claim 9; preferably, the rubber product is a tire.
11. A method for improving the heat-oxidative aging resistance and / or ultraviolet aging resistance of rubber or rubber products, characterized in that: The method comprises adding the compound of claim 1 or 2 to rubber or a rubber product.