Catalyst component for olefin polymerization, preparation method therefor and use thereof
Patent Information
- Application Number
- MYPI2025002505
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-10-27
- Filing Date
- 2023-10-24
- Publication Date
- 2024-04-24
AI Technical Summary
Existing olefin polymerization catalysts have problems such as low Z+1 average molecular weight and poor rigidity-toughness balance performance.
Use a combination of phosphate ester and α-cyanosuccinate or its substitutes as the internal electron donor, and control the molar ratio of phosphate ester to magnesium element, combined with titanium halide and magnesium carrier to form a catalyst component to improve olefin polymerization Z+1 average molecular weight and polymerization activity of the substance.
It improves the formation of tie/intercrystalline bridge chains in the polymer, improves creep resistance and stiffness-toughness balance properties, and at the same time enhances polymerization activity and bulk density.
Abstract
Description
Catalyst component for olefin polymerization, preparation method and use thereof
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of Chinese patent application No. 202211302325.6 filed on October 24, 2022, and Chinese patent application No. 202211322445.2 filed on October 27, 2022, the contents of which are incorporated herein by reference. Technical Field
[0003] The present invention belongs to the field of olefin polymerization catalysts, and in particular relates to a catalyst component for olefin polymerization, a preparation method thereof and an application thereof. Background Art
[0004] The discovery and use of internal electron donors marked a significant milestone in the development of polypropylene catalysts, and internal electron donor technology is one of the core technologies in polypropylene catalyst technology. Different electron donor compounds have a significant impact on the performance of both the catalyst and the polymer. Benzoate compounds, initially used, had low activity and isotacticity. The subsequent development of phthalate compounds as internal electron donors significantly improved the activity and stereospecificity of the catalysts. However, these catalysts exhibited low sensitivity to hydrogen regulation, leading to the development of diether compounds as internal electron donors in propylene polymerization catalysts. However, the polypropylene resin produced using these catalysts exhibited a narrow molecular weight distribution, which can affect the performance of polypropylene resins.
[0005] The glycol ester compounds used in CN1453298A and CN1313869A and 2,3 Dialkyl succinate compounds are used as internal electron donors. Although the molecular weight distribution of polypropylene resins produced by these catalysts is wider than that of o-phthalates, the range is relatively limited. CN102146146A further modifies the molecular weight distribution of the polymer product by compounding this internal electron donor with other types of internal electron donors, such as diethers and o-anisyl benzoates. However, the resulting polyolefins have a low Z+1 average molecular weight and poor stiffness-toughness balance.
[0006] Summary of the Invention
[0007] The purpose of the present invention is to overcome the problems of low Z+1 average molecular weight and poor rigidity-toughness balance of polyolefins in the prior art, and to provide a catalyst component for olefin polymerization, a preparation method and use thereof.
[0008] Among existing olefin polymerization catalysts, phosphates are typically used as solvents during the preparation process and are used in large quantities. The inventors of the present invention unexpectedly discovered that by using a combination of phosphates and α-cyanosuccinates and / or substituted α-cyanosuccinates as internal electron donors and controlling the molar ratio of phosphate to magnesium, the Z+1 average molecular weight (hereinafter referred to as Mz+1) of the olefin polymer can be increased, which is conducive to the formation of more ligaments / intercrystalline bridging chains in the polymer, and imparting to the product excellent properties such as better creep resistance and stiffness-toughness balance. To achieve the above objectives, the first aspect of the present invention provides a catalyst component for olefin polymerization, the catalyst component comprising magnesium, titanium, and an internal electron donor; wherein the internal electron donor comprises phosphate and α-cyanosuccinates and / or substituted α-cyanosuccinates, and the molar ratio of phosphate to magnesium is 0.0002-0.002:1.
[0009] A second aspect of the present invention provides a method for preparing a catalyst component for olefin polymerization, the method comprising: mixing a magnesium-containing support, a titanium halide, and an internal electron donor to obtain the catalyst component, wherein the internal electron donor comprises a phosphate and an α-cyanosuccinate and / or a substituted α-cyanosuccinate, and the amounts of the phosphate and the magnesium-containing support are such that the molar ratio of the phosphate to the magnesium-containing support, calculated as magnesium element, in the obtained catalyst component is 0.0002-0.002:1.
[0010] A third aspect of the present invention provides a catalyst system for olefin polymerization, the catalyst system comprising:
[0011] (1) the catalyst component described above and / or the catalyst component prepared by the method described above;
[0012] (2) aluminum alkyls; and
[0013] (3) Optional external electron donor.
[0014] The fourth aspect of the present invention provides use of the above-mentioned catalyst component and / or the catalyst component prepared by the above-mentioned method and / or the above-mentioned catalyst system in olefin polymerization.
[0015] A fifth aspect of the present invention provides an olefin polymerization method, which comprises: conducting an olefin polymerization reaction in the presence of the above-mentioned catalyst component and / or the catalyst component prepared by the above-mentioned method and / or the above-mentioned catalyst system.
[0016] Through the above technical solution, the present invention achieves the following beneficial effects:
[0017] (1) The catalyst component of the present invention adopts an internal electron donor composed of a phosphate and α-cyanosuccinate and / or a substituted α-cyanosuccinate, and controls the molar ratio of the phosphate to the magnesium element, which can increase the Mz+1 and Mz+1 / Mn of the polymer, increase the content of the high molecular weight portion in the polymer, and is conducive to forming more ligaments / intercrystalline bridging chains in the polymer, thereby giving the product better creep resistance, rigidity-toughness balance and other good properties.
[0018] (2) Further preferably, the present invention introduces a dialkoxy-substituted alkane internal electron donor on the basis of the internal electron donor compounded with phosphate and α-cyanosuccinate and / or substituted α-cyanosuccinate, which can further improve the polymerization activity while ensuring Mz+1 and Mz+1 / Mn. DETAILED DESCRIPTION
[0019] The endpoints of the ranges and any values disclosed herein are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoints of each range, the endpoints of each range and individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered to be specifically disclosed herein.
[0020] A first aspect of the present invention provides a catalyst component for olefin polymerization, comprising magnesium, titanium, and an internal electron donor; wherein the internal electron donor comprises a phosphate and an α-cyanosuccinate and / or a substituted α-cyanosuccinate, and the molar ratio of the phosphate to the magnesium is 0.0002-0.002:1.
[0021] The molar ratio of the phosphate to the magnesium element can be 0.0002:1, 0.0003:1, 0.0004:1, 0.0006:1, 0.0008:1, 0.001:1, 0.0012:1, 0.0014:1, 0.0016:1, 0.0018:1, 0.002:1, or a range consisting of any two of the above. Preferably, the molar ratio of the phosphate to the magnesium element is 0.0003-0.002:1.
[0022] The inventors of the present invention unexpectedly discovered that compounding a small amount of phosphate with α-cyanosuccinate and / or substituted α-cyanosuccinate as an internal electron donor can improve the rigidity-toughness balance of a polymer, increasing the Mz+1 and Mz+1 / Mn values of the polymer. However, when the phosphate content exceeds the above range, the catalyst morphology is significantly damaged, and when the catalyst is used in a polymerization reaction, the Mz+1 and Mz+1 / Mn values of the resulting polymer are low. In the present invention, unless otherwise specified, the units of Mz+1 and Mn are g / mol.
[0023] According to the present invention, preferably, the molar ratio of the phosphate to α-cyanosuccinate and / or substituted α-cyanosuccinate is 1:15-500 (1:15, 1:20, 1:30, 1:40, 1:50, 1:60, 1:70, 1:80, 1:90, 1:100, 1:200, 1:300, 1:400, 1:500, and ranges consisting of any two of the above), more preferably 1:40-400.
[0024] According to the present invention, preferably, the phosphate ester includes at least one of a hydrocarbyl ester of phosphoric acid, a halogenated hydrocarbyl ester of phosphoric acid, a hydrocarbyl ester of phosphorous acid, and a halogenated hydrocarbyl ester of phosphorous acid; the number of carbon atoms of the hydrocarbyl group in the phosphate ester may be C1-C 10 Preferably, the hydrocarbyl ester of phosphoric acid includes at least one of monohydrocarbyl phosphate, dihydrocarbyl phosphate and trihydrocarbyl phosphate, more preferably trihydrocarbyl phosphate. 10 Alkyl ester; more preferably tri-C1-C5 alkyl phosphate.
[0025] According to a preferred embodiment of the present invention, the tri-C1-C 10 The alkyl ester includes at least one of tributyl phosphate, trimethyl phosphate, triethyl phosphate, and tripropyl phosphate.
[0026] According to the present invention, the substituent in the substituted α-cyanosuccinate may be at the α position or the β position. Preferably, the α-cyanosuccinate and / or substituted α-cyanosuccinate is selected from at least one compound represented by formula (III):
[0027] In formula (III), R a 、R b Each independently selected from C1-C 14 Straight chain alkyl, C3-C 14 Branched alkyl, C3-C 10 Cycloalkyl, C6-C 10 Aryl, C7-C 10 Alkaryl or C7-C 10 Aralkyl; R c and R d Each independently selected from H, C1-C 14 Straight chain alkyl, C3-C 14 Branched alkyl, C3-C 10 Cycloalkyl, C6-C 10 Aryl, C7-C 10 Alkaryl or C7-C 10 Aralkyl; R c and R dThey are optionally bonded to each other to form one or more fused ring structures.
[0028] According to the present invention, preferably, in formula (III), R a 、R b Each independently selected from C1-C 10 Straight chain alkyl, C3-C 10 Branched alkyl, C3-C 10 Cycloalkyl, C6-C 10 Aryl, C7-C 10 Alkaryl or C7-C 10 Aralkyl; R c and R d Each independently selected from C1-C 10 Straight chain alkyl, C3-C 10 Branched alkyl, C3-C 10 Cycloalkyl, C6-C 20 Aryl, C7-C 20 Alkaryl or C7-C 20 Aromatic hydrocarbon group.
[0029] According to the present invention, preferably, in formula (III), R a 、R b Each is independently selected from C1-C5 straight chain alkyl, C3-C5 branched chain alkyl, C3-C5 cycloalkyl; R c and R d Each is independently selected from C1-C5 straight chain alkyl, C3-C5 branched chain alkyl, C3-C6 cycloalkyl, and C6-C8 aryl.
[0030] The hydrogen atoms on the aromatic ring (such as the benzene ring) in the aryl, alkylaryl or aromatic hydrocarbon group of the present invention may be optionally replaced by other atoms.
[0031] According to the present invention, preferably, the α-cyanosuccinate and / or substituted α-cyanosuccinate include: diethyl 2,3-diisopropyl-2-cyanosuccinate, diethyl 3-methyl-2-isopropyl-2-cyanosuccinate, diethyl 3-ethyl-2-isopropyl-2-cyanosuccinate, diethyl 3-propyl-2-isopropyl-2-cyanosuccinate, diethyl 3-butyl-2-isopropyl-2-cyanosuccinate, diethyl 3-phenyl-2-isopropyl-2-cyanosuccinate, diethyl 2,3-dicyclohexyl-2-cyanosuccinate, dibutyl 2,3-diisopropyl-2-cyanosuccinate and diethyl 2-diisopropyl 3-cyclopentyl-2-cyanosuccinate.
[0032] According to the present invention, preferably, the molar ratio of the α-cyanosuccinate and / or substituted α-cyanosuccinate to the magnesium element is 0.01-0.2:1 (for example, 0.01:1, 0.02:1, 0.03:1, 0.04:1, 0.05:1, 0.06:1, 0.07:1, 0.08:1, 0.09:1, 0.1:1, 0.11:1, 0.12:1, 0.15:1, 0.2:1, and ranges consisting of any two of the above), more preferably 0.03-0.15:1, and even more preferably 0.04-0.11:1.
[0033] According to the present invention, the inventors of the present invention have further discovered that the use of phosphate and α-cyanosuccinate and / or substituted α-cyanosuccinate in combination with dialkoxy-substituted alkanes as internal electron donors can not only improve the Mz+1 and Mz+1 / Mn of the polymer, but also further improve the polymerization activity. Therefore, preferably, the internal electron donor further includes a dialkoxy-substituted alkane, and more preferably, the dialkoxy-substituted alkane is selected from (R 7 )(R 8 )C(OR 9 )(OR 10 ), wherein R 7 and R 8 Each independently selected from hydrogen, C1-C 20 Alkyl (straight chain alkyl or branched chain alkyl), C3-C 20 Cycloalkyl, C6-C 20 Aryl, C7-C 20 Arylalkyl or C7-C 10 The alkylaryl group, R 7 and R 8 They may be optionally linked to form a ring; R 9 and R 10 Each independently selected from C1-C 20 of an alkyl group (a straight-chain alkyl group or a branched-chain alkyl group).
[0034] According to the present invention, preferably, the dialkoxy-substituted alkane is selected from (R 7 )(R 8 )C(OR 9 )(OR 10 ), wherein R 7 and R 8 Each independently selected from hydrogen, C1-C 10 Alkyl, C3-C 10 Cycloalkyl, C6-C 10 Aryl, C7-C 10 Arylalkyl or C7-C 10 The alkylaryl group, R 7and R 8 They may be optionally linked to form a ring; R 9 and R 10 Each independently selected from C1-C 10 of an alkyl group (a straight-chain alkyl group or a branched-chain alkyl group).
[0035] In a further preferred embodiment, the dialkoxy-substituted alkane is selected from 2-(2-ethylhexyl)-1,3-dimethoxypropane, 2-isopropyl-1,3-dimethoxypropane, 2-butyl-1,3-dimethoxypropane, 2-sec-butyl-1,3-dimethoxypropane, 2-cyclohexyl-1,3-dimethoxypropane, 2-phenyl-1,3-dimethoxypropane, 2-(2-phenylethyl)-1,3-dimethoxypropane, 2-(2-cyclohexylethyl)-1,3-dimethoxypropane, 2-(p-chlorophenyl)-1,3-dimethoxypropane, 2-(diphenylmethyl)-1,3-dimethoxypropane, 2,2-dicyclohexyl-1,3-dimethoxypropane, 2, 2-Dicyclopentyl-1,3-dimethoxypropane, 2,2-diethyl-1,3-dimethoxypropane, 2,2-dipropyl-1,3-dimethoxypropane, 2,2-diisopropyl-1,3-dimethoxypropane, 2,2-dibutyl-1,3-dimethoxypropane, 2-methyl-2-propyl-1,3-dimethoxypropane, 2-methyl-2-benzyl-1,3-dimethoxypropane, 2-methyl-2-ethyl-1,3-dimethoxypropane, 2-methyl-2-isopropyl-1,3-dimethoxypropane, 2-methyl-2-phenyl-1,3-dimethoxypropane, 2-methyl-2-cyclohexyl-1,3-dimethoxypropane, 2,2-bis(2-cyclohexylethyl)-1,3 -dimethoxypropane, 2-methyl-2-isobutyl-1,3-dimethoxypropane, 2-methyl-2-(2-ethylhexyl)-1,3-dimethoxypropane, 2,2-diisobutyl-1,3-dimethoxypropane, 2,2-diphenyl-1,3-dimethoxypropane, 2,2-dibenzyl-1,3-dimethoxypropane, 2,2-bis(cyclohexylmethyl)-1,3-dimethoxypropane, 2-isobutyl-2-isopropyl-1,3-dimethoxypropane, 2-(1-methylbutyl)-2-isopropyl-1,3-dimethoxypropane, 2-isopropyl-2-isopentyl-1,3-dimethoxypropane, 2-phenyl-2-isopropyl-1,3-dimethoxypropane, 2-phenyl-2 - at least one of sec-butyl-1,3-dimethoxypropane, 2-benzyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclopentyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclopentyl-2-sec-butyl-1,3-dimethoxypropane, 2-cyclohexyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclohexyl-2-sec-butyl-1,3-dimethoxypropane, 2-isopropyl-2-sec-butyl-1,3-dimethoxypropane, 2-cyclohexyl-2-cyclohexylmethyl-1,3-dimethoxypropane, and 9,9-dimethoxymethylfluorene, for example, 2-isopropyl-2-isopentyl-1,3-dimethoxypropane and / or 9,9-dimethoxymethylfluorene.
[0036] According to the present invention, the content of the dialkoxy-substituted alkane may be a partial replacement of α-cyanosuccinate and / or a replacement of α-cyanosuccinate, or a certain amount of dialkoxy-substituted alkane may be added to the content of the above-mentioned α-cyanosuccinate and / or the replacement of α-cyanosuccinate. Preferably, the molar ratio of the dialkoxy-substituted alkane to the magnesium element is 0.001-0.15:1 (0.001:1, 0.005:1, 0.01:1, 0.02:1, 0.03:1, 0.04:1, 0.05:1, 0.06:1, 0.07:1, 0.08:1, 0.09:1, 0.1:1, 0.15:1, and a range consisting of any two of the above), more preferably 0.01-0.1:1, and even more preferably 0.02-0.1:1.
[0037] According to the present invention, preferably, the molar ratio of the phosphate ester to the dialkoxy-substituted alkane is 1:10-400 (1:30, 1:40, 1:50, 1:60, 1:70, 1:80, 1:90, 1:100, 1:200, 1:300, 1:400, and ranges consisting of any two of the foregoing), more preferably 1:50-350, and even more preferably 1:50-120.
[0038] According to a particularly preferred embodiment of the present invention, when phosphate, α-cyanosuccinate and / or substituted α-cyanosuccinate, and dialkoxy-substituted alkane are used as internal electron donors, the molar ratio of the phosphate, α-cyanosuccinate and / or substituted α-cyanosuccinate, and dialkoxy-substituted alkane is 1:10-250:20-100, more preferably 1:200-250:50-100.
[0039] According to the present invention, preferably, the magnesium source is a magnesium-containing carrier, and the magnesium-containing carrier includes a magnesium chloride alcoholate carrier and / or an alkoxy magnesium carrier. More preferably, the carrier is spherical.
[0040] According to the present invention, preferably, the magnesium chloride alcoholate carrier comprises a component represented by formula (I), MgY 1 Y 2 ·mR'OH Formula (I)
[0041] In formula (I), Y 1 is selected from halogen, preferably chlorine or bromine; Y 2 Selected from halogen, alkyl or alkoxy, more preferably selected from chlorine, bromine, C1-C 14 Alkyl, C1-C 14 Alkoxy, C6-C 14 Aryl, C6-C 14R' is selected from one of halogen-substituted or unsubstituted alkyl, halogen-substituted or unsubstituted cycloalkyl, halogen-substituted or unsubstituted aralkyl, more preferably from halogen-substituted or unsubstituted C1-C 12 Alkyl, halogen substituted or unsubstituted C3-C 10 Cycloalkyl, halogen substituted or unsubstituted C7-C 10 One of the aralkyl groups; m is 1-5 (for example, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, and ranges consisting of any two of the foregoing).
[0042] In a further preferred embodiment, in formula (I), Y 1 is chlorine, Y 2 Chlorine, bromine, C1-C5 alkyl, C1-C5 alkoxy, C6-C 10 Aryl or C6-C 10 The aryloxy group is R', which is selected from a halogen-substituted or unsubstituted C1-C8 alkyl group, a halogen-substituted or unsubstituted C3-C8 cycloalkyl group, and is preferably selected from a halogen-substituted or unsubstituted C1-C6 alkyl group (for example, a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, an isobutyl group or a n-hexyl group), and m is 1.2-3.5 (for example, 1.5-2.8).
[0043] More preferably, MgY in formula (I) 1 Y 2 It is magnesium dichloride.
[0044] In the present invention, the preparation of the magnesium chloride alcoholate carrier is not particularly limited and can be carried out by any method disclosed in the prior art.
[0045] According to the present invention, preferably, the magnesium chloride alcoholate carrier does not contain a detectable amount of P, preferably does not contain a detectable amount of phosphate.
[0046] According to the present invention, preferably, the alkoxy magnesium support comprises a component represented by formula (II): [R1O] m’ Mg[OCH(CHXR2)(R3)] n Formula (II);
[0047] In formula (II), R1 is selected from one of a straight-chain alkyl group or a halogen-substituted straight-chain alkyl group, a branched-chain alkyl group or a halogen-substituted branched-chain alkyl group, a cycloalkyl group or a halogen-substituted cycloalkyl group; R2 and R3 are each independently one of hydrogen, a straight-chain alkyl group or a halogen-substituted straight-chain alkyl group, a branched-chain alkyl group or a halogen-substituted branched-chain alkyl group; X is a halogen; m' is 0.1-1.9, n is 0.1-1.9, and m'+n=2.
[0048] In a further preferred embodiment, in formula (II), R1 is selected from one of C1-C8 straight-chain alkyl or halogen-substituted straight-chain alkyl, C3-C8 branched-chain alkyl or halogen-substituted branched-chain alkyl, C3-C8 cycloalkyl or halogen-substituted cycloalkyl; R2 and R3 are each independently one of hydrogen, C1-C5 straight-chain alkyl or halogen-substituted straight-chain alkyl, C3-C5 branched-chain alkyl or halogen-substituted branched-chain alkyl; X is chlorine or bromine; m' is 0.8-1.2, n is 0.8-1.2, and m'+n=2.
[0049] According to the present invention, preferably, the alkoxymagnesium carrier does not contain a detectable amount of P, preferably does not contain a detectable amount of phosphate.
[0050] In a preferred embodiment, the alkoxymagnesium support is a mixture or reaction product of components including magnesium halide, organic alcohol, and epoxy compound.
[0051] In a further preferred embodiment, the magnesium halide is selected from at least one of the compounds represented by MgX2, the organic alcohol is selected from at least one of the compounds represented by R1OH, and the epoxy compound is selected from at least one of the compounds represented by formula (II').
[0052] Wherein, X in MgX2, R1 in R1OH, R2 and R3 in formula (II') have the same definitions as the corresponding groups in formula (II), which are not repeated here.
[0053] The preparation of the alkoxy magnesium support represented by formula (II) of the present invention is not particularly limited and can be carried out by any method disclosed in the prior art.
[0054] According to the present invention, preferably, the titanium source is titanium halide, and the titanium halide is selected from Ti(OR 4 ) 4-n X' n At least one of the compounds shown, wherein R 4 Selected from C1-C 20 The hydrocarbon group is preferably selected from C1-C 14 The repeated X's are the same or different and are independently selected from F, Cl or Br, and n is an integer of 0-4.
[0055] According to the present invention, preferably, the titanium halide is selected from one of titanium tetrachloride, titanium tetrabromide, titanium tetraiodide, titanium tetrabutoxide, titanium tetraethoxide, titanium trichloride, titanium tributoxide, titanium dichloride, titanium trichloride, titanium trichloride or a mixture thereof, preferably titanium tetrachloride.
[0056] According to the present invention, preferably, the molar ratio of the titanium element to the magnesium element is 0.01-0.3:1 (for example, 0.01:1, 0.02:1, 0.03:1, 0.04:1, 0.05:1, 0.06:1, 0.07:1, 0.08:1, 0.09:1, 0.1:1, 0.11:1, 0.12:1, 0.15:1, 0.2:1, 0.24:1, 0.28:1, 0.3:1, and ranges consisting of any two of the above points), and more preferably 0.06-0.15:1.
[0057] The bulk density of polymers produced using the olefin polymerization catalysts of the present invention is also an important catalyst property. Generally speaking, a higher bulk density of a polymer means a higher production capacity can be achieved, thereby leading to higher production efficiency, cost savings, and improved economic efficiency. The inventors have discovered that propylene polymers produced using the catalysts of the present invention for olefin polymerization exhibit relatively high bulk density.
[0058] A second aspect of the present invention provides a method for preparing a catalyst component for olefin polymerization, comprising: mixing a magnesium-containing support, a titanium halide, and an internal electron donor, wherein the internal electron donor comprises a phosphate and an α-cyanosuccinate and / or a substituted α-cyanosuccinate, and the amounts of the phosphate and the magnesium-containing support are such that the molar ratio of the phosphate to the magnesium-containing support, calculated as magnesium, in the resulting catalyst component is 0.0002-0.002:1. In the prior art, however, phosphate is used as a solvent to dissolve the magnesium halide, and the amount used is relatively large; typically, the molar amount of phosphate is approximately 1 times the amount of magnesium, or even higher.
[0059] According to the present invention, preferably, the method of mixing the magnesium-containing support, titanium halide, and internal electron donor includes: (1) mixing the magnesium-containing support with the titanium halide; (2) mixing the system of step (1) with the internal electron donor.
[0060] According to the present invention, preferably, the mixing in step (1) is carried out at -30°C to 0°C, preferably -25°C to -15°C. For example, the mixing in step (1) can be carried out at -30°C, -20°C, -10°C, 0°C or 5°C. The mixing method in step (1) is not particularly limited, and can be, for example, stirring. The mixing time in step (1) can be 1-600 minutes.
[0061] According to the present invention, preferably, in step (2), the temperature is first increased, and the internal electron donor is added during the temperature increase; more preferably, the temperature is increased to 80°C-130°C, preferably 90°C-120°C. For example, the temperature is increased to 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, or 130°C. The mixing time in step (2) can be 30-900 minutes.
[0062] According to the present invention, preferably, after mixing in step (2), filtration and optionally washing and drying are performed. The mixing method in step (2) is not particularly limited, and can be, for example, stirring. In a further preferred embodiment, washing is first performed with the titanium halide and then with an alkane solvent (e.g., hexane).
[0063] According to a particularly preferred embodiment of the present invention, the method comprises:
[0064] (1) adding titanium halide to a reaction vessel, cooling to -30°C to 0°C, then adding a magnesium-containing support to the reaction vessel, and stirring at -30°C to 0°C for 1-600 min (preferably 10-60 min);
[0065] (2) The reaction vessel is heated to 0-130°C (preferably 80-130°C), and the internal electron donor is added during the heating process. The temperature is then maintained for 30-900 minutes (preferably 10-60 minutes), and the liquid is filtered off. Then, titanium tetrachloride is added for washing, and finally washed with hexane, and the catalyst component is obtained after drying.
[0066] According to the present invention, preferably, the amounts of the α-cyanosuccinate and / or substituted α-cyanosuccinate and the magnesium-containing support are such that the molar ratio of the α-cyanosuccinate and / or substituted α-cyanosuccinate to the magnesium-containing support in the obtained catalyst component, calculated as magnesium element, is 0.01-0.2:1, more preferably 0.03-0.15:1, and even more preferably 0.04-0.11:1.
[0067] According to the present invention, preferably, the amount of the phosphoric acid ester and α-cyanosuccinate and / or substituted α-cyanosuccinate is such that the molar ratio of the phosphoric acid ester to α-cyanosuccinate and / or substituted α-cyanosuccinate in the obtained catalyst component is 1:15-500, more preferably 1:40-400.
[0068] According to the present invention, preferably, the internal electron donor further comprises a dialkoxy-substituted alkane.
[0069] According to the present invention, the amount of the dialkoxy-substituted alkane can be to partially replace the α-cyanosuccinate and / or replace the α-cyanosuccinate, or to add a certain amount of the dialkoxy-substituted alkane on the basis of the amount of the above-mentioned α-cyanosuccinate and / or substituted α-cyanosuccinate. Preferably, the amount of the dialkoxy-substituted alkane and the magnesium-containing support is such that the molar ratio of the dialkoxy-substituted alkane to the magnesium-containing support calculated as magnesium in the obtained catalyst component is 0.001-0.15:1, more preferably 0.01-0.1:1, and even more preferably 0.02-0.1:1.
[0070] According to the present invention, preferably, the amounts of the phosphate and the dialkoxy-substituted alkane are such that the molar ratio of the phosphate to the dialkoxy-substituted alkane in the obtained catalyst component is 1:10-400, more preferably 1:50-350.
[0071] According to a particularly preferred embodiment of the present invention, when a phosphate, an α-cyanosuccinate and / or a substituted α-cyanosuccinate, or a dialkoxy-substituted alkane is used as the internal electron donor, the amounts of the phosphate, the α-cyanosuccinate and / or the substituted α-cyanosuccinate, and the dialkoxy-substituted alkane are such that the molar ratio of the phosphate, the α-cyanosuccinate and / or the substituted α-cyanosuccinate, and the dialkoxy-substituted alkane in the resulting catalyst component is 1:10-250:20-100, more preferably 1:200-250:50-100.
[0072] According to the present invention, preferably, the amounts of the titanium halide and the magnesium-containing support are such that the molar ratio of the titanium halide to the magnesium-containing support in the obtained catalyst component calculated as magnesium element is 0.01-0.3:1, more preferably 0.06-0.15:1.
[0073] In the present invention, the magnesium-containing support and titanium halide are as described in the first aspect and will not be described in detail here.
[0074] In a preferred embodiment, the magnesium chloride alcoholate carrier can be prepared by conventional methods in the art (e.g., CN1718595A); preferably, but not limited to, the following method:
[0075] 1) MgY 1 Y 2 Mix with R'OH and react at 110-130℃ for 1-3h to obtain MgY 1 Y 2 / R'OH adduct melt;
[0076] 2) The MgY 1 Y 2The MgY / R'OH adduct melt is emulsified, and the emulsified product is rapidly cooled and formed, and then dried to obtain the MgY 1 Y 2 ·m'R'OH; wherein an inert liquid medium is added in step 1) and / or step 2).
[0077] Among them, R'OH and MgY 1 Y 2 The molar ratio is 1-5, preferably 1.2-3.5 (for example, 1.5-2.8).
[0078] In step 2), the inert liquid medium can be any liquid medium commonly used in the art that does not chemically interact with the magnesium halide adduct, such as silicone oil and / or hydrocarbon solvents. Specifically, the inert liquid medium can be one or more of kerosene, paraffin oil, vaseline oil, white oil, methyl silicone oil, ethyl silicone oil, methylethyl silicone oil, phenyl silicone oil, and methylphenyl silicone oil. The amount of the inert liquid medium can be adjusted according to the amount of MgY 1 Y 2 The specific dosage is selected. 1 Y 2 The amount of inert liquid medium used is 0.2-13 L, preferably 0.6-6.5 L, for example 0.2 L, 0.5 L, 1 L, 2 L, 4 L, 6 L, 8 L, 10 L, 12 L or 13 L per mole of magnesium.
[0079] In a preferred embodiment, the inert liquid medium is added in step 1) and / or step 2).
[0080] For example, in method (A), the MgY 1 Y 2 The m'R'OH adduct melt is mixed with an inert liquid medium and the resulting mixture is emulsified to achieve the MgY 1 Y 2 ·Emulsification of the m'R'OH adduct melt.
[0081] For example, in method (B), an inert liquid medium is added in both step 1) and step 2), that is, in step 1) an inert liquid medium is added as the medium for preparing the MgY 1 Y 2 / R'OH adduct melt reaction medium, thereby obtaining MgY 1 Y 2 / R'OH adduct melt, and then the mixture is mixed with an inert liquid medium and emulsified to achieve the MgY 1 Y 2The inert liquid medium in step 1) and step 2) can be the same or different. For example, the inert liquid medium in step 1) can be white oil, and the inert liquid medium in step 2) can be methyl silicone oil. When mixing in step 2), the inert liquid medium needs to be preheated to a temperature that is compatible with MgY 1 Y 2 / R'OH adduct melt at the same temperature.
[0082] For example, in method (C), in step 1), an inert liquid medium is added as the preparation medium of MgY 1 Y 2 / R'OH adduct melt reaction medium, thereby obtaining MgY 1 Y 2 / R'OH adduct melt, emulsifying the mixture to achieve the MgY 1 Y 2 / R'OH adduct melt emulsification.
[0083] According to the present invention, if necessary, a surfactant such as fatty acid glyceride, fatty acid sorbitan, polysorbate, polyoxyethylene ether or polyoxyethylene-polyoxypropylene copolymer can be added to the inert liquid medium. The amount of the surfactant can be the conventional amount in the art, for example: 1 Y 2 The amount of the surfactant used can be 0.001-1 mol, for example, 0.001 mol, 0.005 mol, 0.01 mol, 0.05 mol, 0.1 mol, 0.2 mol, 0.4 mol, 0.6 mol, 0.8 mol or 1 mol per mol of magnesium.
[0084] In the present invention, various methods known to those skilled in the art can be used to convert MgY 1 Y 2 / R'OH adduct melt emulsification, for example: in the presence of an inert liquid medium, MgY 1 Y 2 The high-speed shearing method is well known to those skilled in the art, for example, the high-speed stirring method disclosed in CN1151183C (i.e., MgY 1 Y 2 / R'OH adduct melt in an inert liquid medium at a speed of 2000-5000 rpm is stirred); CN1267508C discloses the method of mixing MgY 1 Y 2The mixture of the molten R'OH adduct and the inert liquid medium is rotated in a supergravity bed (the rotation speed can be 100-3000 rpm) to disperse; CN1463990A discloses the method of dispersing MgY 1 Y 2 The mixture of the molten R'OH adduct, silicone oil and white oil is output in an emulsifier at a speed of 1500-8000 rpm; US6020279 discloses a method of spraying the MgY 1 Y 2 The mixture of the R'OH adduct melt is emulsified.
[0085] According to the present invention, the emulsified product can be rapidly cooled and formed by a method known to those skilled in the art to obtain spherical MgY 1 Y 2 ·m'R'OH. For example, the emulsified product may be rapidly cooled to form the emulsified product by transferring the emulsified product to a liquid cooling medium.
[0086] The liquid cooling medium can be any of various commonly used liquid media in the art that do not chemically interact with the magnesium halide adduct. For example, the liquid cooling medium can be an inert hydrocarbon solvent. Specific examples of the liquid cooling medium can include, but are not limited to, at least one of n-pentane, n-hexane, n-heptane, gasoline, and petroleum.
[0087] In the present invention, the water in the liquid cooling medium can participate in the reaction or be subjected to a dehydration treatment to control the moisture content of the liquid cooling medium used to a range that does not affect the test results. Generally, the water content of the liquid cooling medium is controlled to be no more than 5 ppm (by weight). Methods for controlling or reducing the water content in the liquid cooling medium are well known in the art, for example, the liquid material can be distilled and / or contacted with a water absorbent (such as a molecular sieve), and a high-purity inert gas flow, such as a high-purity nitrogen flow, can be continuously introduced into the heated liquid material.
[0088] The temperature of the liquid cooling medium is determined to enable the emulsified product to be cooled and formed. Generally, the temperature of the liquid cooling medium can be between -50°C and 0°C, preferably between -40°C and -20°C. There is no particular limitation on the amount of the liquid cooling medium used, as long as the amount of the liquid cooling medium is sufficient to cool and form the emulsified product. Specifically, the volume ratio of the liquid cooling medium to the emulsified product is (1-15):1, preferably (2-9):1.
[0089] MgY obtained by rapid cooling 1 Y 2The m'R'OH particles can be washed and dried. The present invention can use an inert hydrocarbon solvent known to those skilled in the art (such as n-pentane, n-hexane, n-heptane, petroleum ether and gasoline) to wash the obtained MgY 1 Y 2 The drying temperature may be no higher than 35°C, preferably 25-30°C; the drying time may be 0.5-3 hours, preferably 1-2 hours. The drying may be carried out under normal pressure or reduced pressure.
[0090] Other parameters not limited in the preparation method of the present invention can be conventionally selected according to the prior art.
[0091] In a preferred embodiment, the alkoxy magnesium support can be prepared by conventional methods in the art; preferably, but not limited to, by the following method:
[0092] S1: mixing a magnesium halide of the general formula MgX2, a compound of the general formula R5OH, a surfactant, and an optional inert liquid medium and heating to obtain a liquid mixture;
[0093] S2: contacting the liquid mixture obtained in step S1 with an epoxy compound for reaction.
[0094] In a preferred embodiment, in step S1, the inert liquid medium is selected from at least one of kerosene, paraffin oil, vaseline oil, white oil, methyl silicone oil, ethyl silicone oil, methylethyl silicone oil, phenyl silicone oil and methylphenyl silicone oil; preferably white oil.
[0095] In a further preferred embodiment, the amount of the inert liquid medium is 0.8-10 L, preferably 2-8 L, based on 1 mol of magnesium halide with the general formula MgX2.
[0096] In a preferred embodiment, the surfactant is selected from at least one of polyvinyl pyrrolidone (PVP), polyethylene glycol (PEG), polyvinyl alcohol, polyacrylic acid, polyacrylate, polyacrylamide, polystyrene sulfonate, naphthalenesulfonic acid formaldehyde condensate, condensed alkyl phenyl ether sulfate, condensed alkylphenol polyoxyethylene ether phosphate, oxyalkyl acrylate copolymer modified polyethyleneimine, 1-dodecan-4-vinylpyridinium bromide polymer, polyvinylbenzyltrimethylamine salt, polyethylene oxide propylene oxide block copolymer, polyvinylpyrrolidone vinyl acetate copolymer, alkylphenyl polyoxyethylene ether and polyalkyl methacrylate; preferably selected from at least one of polyvinyl pyrrolidone, polyvinylpyrrolidone vinyl acetate copolymer and polyethylene glycol.
[0097] In a further preferred embodiment, the amount of the surfactant is 1-20g, for example, 1g, 2g, 4g, 6g, 8g, 10g, 12g, 14g, 16g, 18g or 20g, based on 1mol MgX2.
[0098] In a preferred embodiment, the heating temperature in step S1 is 80-120° C., and the reaction time is 0.5-5 hours; preferably, the temperature is 80-100° C., and the reaction time is 0.5-3 hours.
[0099] In a preferred embodiment, in step S2, the contact reaction temperature is 40-120°C, and the reaction time is 15-60 minutes; preferably, the contact reaction temperature is 60-100°C, and the reaction time is 20-50 minutes.
[0100] In a preferred embodiment, the preparation method of the alkoxymagnesium carrier further optionally comprises S3: performing solid-liquid separation, washing and drying the separated solid phase product.
[0101] Wherein, the solid-liquid separation can be various existing methods capable of achieving separation of the solid phase and the liquid phase, such as suction filtration, filter press or centrifugal separation. Preferably, the method of the solid-liquid separation is filter press. The present invention does not particularly limit the conditions for filter press, so as to achieve the separation of the solid phase and the liquid phase as fully as possible. The washing can be performed by methods well known to those skilled in the art to wash the obtained solid-phase product, for example, an inert hydrocarbon solvent (for example: pentane, hexane, heptane, petroleum ether and gasoline) can be used to wash the obtained solid-phase product. The present invention does not particularly limit the conditions for the drying, for example: the drying temperature can be 20-70°C, and the drying time can be 0.5-10 hours. According to the present invention, the drying can be carried out under normal pressure or reduced pressure.
[0102] As a specific embodiment of the present invention, the content of the above-mentioned components in the spherical support of the olefin polymerization catalyst can be selected and varied within a wide range. Preferably, based on 1 mol of the magnesium halide of the general formula MgX2, the amount of the compound of the general formula R5OH is 4-30 mol, and the amount of the epoxy compound is 1-10 mol. Further preferably, based on 1 mol of the magnesium halide of the general formula MgX2, the amount of the compound of the general formula R5OH is 6-20 mol, and the amount of the epoxy compound is 2-6 mol.
[0103] In a preferred embodiment, the compound of the general formula R5OH may be a C1-C5 monohydric alcohol, for example, at least one of methanol, ethanol, propanol, butanol and pentanol, and is particularly preferably ethanol.
[0104] The third aspect of the present invention provides a catalyst system for olefin polymerization, the catalyst system comprising:
[0105] (1) the catalyst component described above and / or the catalyst component prepared by the method described above;
[0106] (2) aluminum alkyls; and
[0107] (3) Optional external electron donor.
[0108] According to the present invention, the alkyl aluminum can be an alkyl aluminum with an activation effect commonly used in the art. Preferably, the number of alkyl groups in the alkyl aluminum is 1-3, and the number of carbon atoms in the alkyl group is C1-C8. More preferably, the alkyl aluminum is selected from at least one of triethyl aluminum, tripropyl aluminum, tri-n-butyl aluminum, triisobutyl aluminum, tri-n-octylaluminum, diethyl aluminum monohydrogenate, diisobutyl aluminum monohydrogenate, diethyl aluminum monochloride, diisobutyl aluminum monochloride, sesquiethyl aluminum chloride and ethyl aluminum dichloride.
[0109] According to the present invention, the external electron donor can be any commonly used external electron donor in the art. Preferably, the external electron donor is selected from at least one silicon-containing compound, especially C4-C 20 At least one of the silanes, in particular a silane containing two alkoxy groups, the alkoxy group is, for example, a C1-C5 alkoxy group, more preferably at least one selected from cyclohexylmethyldimethoxysilane, diisopropyldimethoxysilane, di-n-butyldimethoxysilane, diisobutyldimethoxysilane, diphenyldimethoxysilane, methyl-tert-butyldimethoxysilane, dicyclopentyldimethoxysilane, 2-ethylpiperidinyl-2-tert-butyldimethoxysilane, (1,1,1-trifluoro-2-propyl)-2-ethylpiperidinyldimethoxysilane, and (1,1,1-trifluoro-2-propyl)-methyldimethoxysilane.
[0110] According to the present invention, preferably, the molar ratio of the catalyst component to the alkyl aluminum is 1:15-718 (for example, 1:15, 1:50, 1:100, 1:150, 1:200, 1:250, 1:300, 1:350, 1:400, 1:450, 1:500, 1:550, 1:600, 1:650, 1:700 or 1:718, and ranges consisting of any two of the above points), wherein the moles of the catalyst component are calculated based on the moles of the Ti element therein.
[0111] According to the present invention, preferably, the molar ratio of the catalyst component and the external electron donor is 1:1-111 (for example, 1:1, 1:5, 1:6, 1:7, 1:10, 1:20, 1:30, 1:40, 1:50, 1:60, 1:70, 1:80, 1:90, 1:100 or 1:110, and ranges consisting of any two of the above points), wherein the moles of the catalyst component are calculated based on the moles of the Ti element therein.
[0112] The fourth aspect of the present invention provides use of the above-mentioned catalyst component and / or the catalyst component prepared by the above-mentioned method and / or the above-mentioned catalyst system in olefin polymerization.
[0113] The fifth aspect of the present invention provides an olefin polymerization method, which comprises: conducting an olefin polymerization reaction in the presence of the above-mentioned catalyst component and / or the catalyst component prepared by the above-mentioned method and / or the above-mentioned catalyst system.
[0114] According to the present invention, preferably, the olefin is selected from at least one compound represented by the formula CH2=CHR, wherein R is hydrogen or a C1-C6 straight chain or C3-C6 branched alkyl group.
[0115] In a further preferred embodiment, the olefin is selected from at least one of ethylene, propylene, 1-n-butene, 1-n-pentene, 1-n-hexene, 1-n-octene, and 4-methyl-1-pentene, preferably at least one of ethylene, propylene, 1-n-butene, 1-n-hexene, and 4-methyl-1-pentene, for example, propylene.
[0116] Wherein, the polymerization is the homopolymerization of a single olefin or the copolymerization of two or more olefins.
[0117] According to the present invention, preferably, the polymerization temperature is 0-150°C, for example, the temperature is 0°C, 20°C, 50°C, 80°C, 100°C, 120°C or 150°C.
[0118] According to the present invention, preferably, the polymerization time is 0.1-8 hours, for example, the time is 0.1, 0.5, 1, 2, 3, 4, 5, 6, 7 or 8 hours.
[0119] According to the present invention, preferably, the polymerization pressure is 0.01-10 MPa. For example, the pressure is 0.01 MPa, 0.05 MPa, 0.1 MPa, 0.5 MPa, 1 MPa, 2 MPa, 4 MPa, 6 MPa, 8 MPa or 10 MPa. The polymerization pressure in the present invention refers to the gauge pressure.
[0120] In a further preferred embodiment, the polymerization conditions include: temperature of 50-100° C. and time of 0.5-3 hours.
[0121] In a further preferred embodiment, the polymerization conditions include: a pressure of 0.5-5 MPa.
[0122] The amount of the catalyst used can be any conventional amount of olefin catalysts in the prior art.
[0123] In the present invention, the polymerization process may further include a step of using hydrogen. The amount of hydrogen used may be 0-15 L (standard volume) or 0.5-10 L (standard volume) per 1 L of liquid propylene.
[0124] The present invention will be described in detail below through examples.
[0125] Unless otherwise specified, the raw materials used in the examples and comparative examples are all disclosed in the prior art, for example, they can be directly purchased or prepared according to the preparation methods disclosed in the prior art.
[0126] In the various examples and comparative examples of the present invention, the average particle diameter and particle size distribution of the olefin polymerization catalyst support were measured using a Masters Sizer 2000 particle size analyzer (manufactured by Malvern Instruments Ltd).
[0127] In the various embodiments and comparative examples of the present invention, the test method for the content of each component in the catalyst is as follows:
[0128] The catalyst component provided by the present invention can be measured for titanium content by colorimetry. Specifically, 0.2-0.5 g of a sample is dissolved in 50 mL of 2N H2SO4, the supernatant is filtered, and the clear solution is used for colorimetry. A 2N H2SO4 solution is used as a blank in a 1 cm thick cuvette at a wavelength of 410 μm, and the absorbance E1 is measured. Then, one drop of 30 wt% H2O2 is added, shaken, and the absorbance E2 is measured. The titanium content (%) is calculated according to the following formula:
[0129] Ti%=[(E2-E1)×100) / (K·L·W·100)]×100%
[0130] Where: W is sample weight (g); L is cuvette thickness (cm); K is specific extinction coefficient; E1 is blank absorbance; E2 is sample absorbance.
[0131] The magnesium content can be measured according to the EDTA titration method. Specifically, take 0.2-0.5g of sample into a 250mL conical flask, add 20-30mL 2N H2SO4 solution to dissolve, add 20mL triethanolamine (1+2) standard solution, adjust the pH to 10 with 20% by weight NaOH solution, shake, add 10mL pH=10 buffer solution, add 6 drops of 30% H2O2 and 30-50mL distilled water, add a small amount of chrome black T indicator, shake well, and titrate with 0.02N EDTA solution until the color changes from purple-red to blue (the purple light disappears) as the end point. The magnesium content Mg (%) is calculated according to the following formula:
[0132] Mg(%)=[(VE·NE×24.31) / (G·1000)]×100%
[0133] Where: G is the mass of the sample (g); VE is the amount of EDTA consumed (mL); NE is the equivalent number of EDTA solution; 24.31 is the atomic weight of magnesium.
[0134] The phosphorus content was analyzed using an Axios-Advanced X-ray fluorescence spectrometer from Panalytical BV of the Netherlands.
[0135] Bulk density: Place the polymer powder in a funnel from a height of 10 cm and allow it to fall freely into a 100 mL container. When the container is full, weigh the mass of the polymer powder in the container as X (in g). The bulk density of the polymer is calculated as X ÷ 100. The unit of bulk density is g / cm 3 .
[0136] The contents of α-cyanosuccinate and / or substituted α-cyanosuccinate and dialkoxy-substituted alkanes were determined by gas chromatography using diamyl phthalate as an internal standard.
[0137] In the embodiments and comparative examples of the present invention, the molecular weights Mw, Mn, and Mz+1 of the polymer (polypropylene) were measured using a PL-GPC 220 gel permeation chromatograph coupled with an IR5 infrared detector from Polymer Laboratories, UK, at 150°C. The chromatographic columns consisted of three PLgel 13 μm Olexis columns, the mobile phase consisted of 1,2,4-trichlorobenzene (with 0.025% by mass of the antioxidant 2,6-dibutyl-p-cresol added), the flow rate was 1.0 mL / min, the sample mass concentration was approximately 1 mg / mL, and universal calibration was performed using PL's EasiCal PS-1 narrow distribution polystyrene standard.
[0138] In various examples and comparative examples of the present invention, the melt flow rate (MFR) of the polymer (polypropylene) is measured according to ISO 1133 at 230° C. and a load of 2.16 kg.
[0139] The isotactic index of a polymer (polypropylene) refers to the mass percentage of the polymer that is insoluble in boiling n-heptane under specified conditions. It is determined by the heptane extraction method (boiling heptane extraction for 6 hours), i.e., 2 g of a dried polymer sample is taken and placed in an extractor and extracted with boiling heptane for 6 hours. The residue is then dried to a constant weight, and the ratio of the mass (g) of the obtained polymer to 2 is the isotactic index.
[0140] In each of the examples and comparative examples of the present invention, the surface morphology of the olefin polymerization catalyst support was observed using an optical microscope, model Eclipse E200, purchased from Nikon Corporation.
[0141] The α-cyanosuccinates and / or substituted α-cyanosuccinates in the examples were synthesized according to the methods disclosed in CN101811983A, CN102372651A, CN102603931A, WO 2010 / 094211A1, etc.
[0142] The triethylaluminum used was a hexane solution of triethylaluminum, wherein the concentration of triethylaluminum was 0.5 mmol / mL.
[0143] The test method of the repose angle of the catalyst is as follows: a rotary table repose angle measuring instrument is used for testing. A certain amount of sample is dropped on a circular plate, and the measuring rod is aligned with the stacking angle. The angle is measured, which is the repose angle.
[0144] The following Example A is used to illustrate the preparation method of the catalyst component using phosphate and α-cyanosuccinate and / or substituted α-cyanosuccinate as internal electron donors and the process of preparing the polymer.
[0145] Example A1
[0146] (1) Magnesium chloride alcoholate carrier MgY 1 Y 2mR'OH was prepared as follows: In a 150-L stirred reactor, 10 kg of anhydrous magnesium chloride and 12.6 kg of ethanol were added to 60 L of white oil with a viscosity of 30 centipoise (20°C) and reacted at 125°C for 2 hours. The resulting mixture of the molten adduct and white oil was then transferred to 120 L of methyl silicone oil preheated to 125°C (with a viscosity of 300 centipoise (20°C)). The mixture was stirred at 200 rpm for 30 minutes to obtain a mixture. The mixture was then introduced into a high-gravity rotating bed for dispersion. The dispersed mixture was then introduced into 1200 L of hexane precooled to -35°C under stirring. The magnesium chloride / alcohol adduct melt, dispersed into small droplets, cooled and solidified to form spherical solid particles. Solid particles were filtered out from the suspension obtained after rapid cooling, and washed with hexane at room temperature. The amount of hexane used was 100 L / time, and the washing was performed 5 times in total. The solid was then vacuumed at 60°C to obtain a solid.
[0147] The magnesium chloride alcoholate carrier had an average particle diameter (D50) of 52 microns and a particle size distribution ((D90-D10) / D50) of 1.1. Observation of the particle morphology using an optical microscope revealed that the magnesium chloride alcoholate carrier had a relatively regular particle morphology, a relatively smooth surface, and a relatively concentrated particle size distribution.
[0148] Gas chromatography-mass spectrometry, nuclear magnetic resonance and elemental analysis confirmed that the magnesium chloride alcoholate carrier contained the following components: MgCl2·2.5C2H5OH.
[0149] (2) Preparation of olefin polymerization catalyst components
[0150] In a 300mL glass reaction bottle, add 100mL of titanium tetrachloride, cool to -20°C, add 0.04mol of magnesium chloride alcoholate support, and stir at -20°C for 30 minutes. Then, slowly raise the temperature to 110°C. During this heating process, add 0.38mmol of tributyl phosphate and 6mmol of diethyl 2,3-diisopropyl-2-cyanosuccinate. Maintain the temperature at 110°C for 30 minutes, then filter and remove the liquid. Then, wash twice with titanium tetrachloride, and finally wash three times with hexane. After drying, obtain catalyst a.
[0151] (3) Propylene polymerization
[0152] A 5-liter stainless steel autoclave was purged with nitrogen. Then, 1 mmol of triethylaluminum, 0.05 mmol of methylcyclohexyldimethoxysilane, 10 mL of anhydrous hexane, 10 mg of the above-prepared catalyst a (containing 0.008 mmol of titanium), 1.5 L (standard volume) of hydrogen, and 2.5 L of liquid propylene were introduced into the nitrogen stream. The reaction was heated to 70°C and allowed to react at this temperature for 1 hour. The temperature was then lowered, the pressure released, and the product was discharged and dried to obtain polypropylene powder.
[0153] Example A2
[0154] The amount of phosphate was changed to 0.76 mmol of tributyl phosphate, and the other steps were the same as those in Example A1.
[0155] Example A3
[0156] The amount of phosphate used was changed, and the reaction was the same as in Example A1 except that 1.14 mmol of tributyl phosphate was used.
[0157] Example A4
[0158] The amount of phosphate used was changed, and the reaction was the same as in Example A1 except that 1.9 mmol of tributyl phosphate was used.
[0159] Example A5
[0160] The amount of phosphate used was changed, and the reaction was the same as in Example A1 except that 3.04 mmol of tributyl phosphate was used.
[0161] Example A6
[0162] (1) An alkoxy magnesium support was obtained as follows: 0.08 mol of magnesium chloride, 1.2 mol of ethanol, and 1 g of PVP (polyvinyl pyrrolidone) as a surfactant were added to a 0.6 L reactor. The temperature was raised to 90°C with stirring, and the mixture was kept at this temperature for 2 hours. 38 mL (0.48 mol) of epichlorohydrin was then added. The mixture was kept at this temperature for half an hour, and then filtered. The filtered product was washed five times with hexane, and finally dried under vacuum to obtain a catalyst support for olefin polymerization. Gas chromatography-mass spectrometry, nuclear magnetic resonance, and elemental analysis confirmed that the alkoxy magnesium support contained the following components: (C2H5O)Mg[(OCH(CH2Cl)(CH2Cl)].
[0163] The average particle diameter (D50) of the catalyst carrier is 61 micrometers, and the particle size distribution ((D90-D10) / D50) is 1.3.
[0164] (2) Preparation of olefin polymerization catalyst components
[0165] In a 300 mL glass reaction bottle, add 100 mL of titanium tetrachloride, cool to -20°C, add 0.04 mol of the catalyst support obtained above, and stir at -20°C for 30 minutes. Then, slowly raise the temperature to 110°C. During this heating process, add 1.9 mmol of tributyl phosphate and 6 mmol of diethyl 2,3-diisopropyl-2-cyanosuccinate. Maintain the temperature at 110°C for 30 minutes, then filter and remove the liquid. Then, wash twice with titanium tetrachloride, and finally wash three times with hexane. After drying, obtain olefin polymerization catalyst b.
[0166] (3) Propylene polymerization
[0167] A 5 L stainless steel autoclave was purged with nitrogen. Then, 1 mmol of triethylaluminum, 0.05 mmol of methylcyclohexyldimethoxysilane, 10 mL of anhydrous hexane, 10 mg of the olefin polymerization catalyst b (containing 0.0069 mol of titanium) prepared above, 1.5 L (standard volume) of hydrogen, and 2.5 L of liquid propylene were introduced into the nitrogen stream. The reaction was heated to 70°C and allowed to react at this temperature for 1 hour. The temperature was then lowered, the pressure released, and the product was discharged and dried to obtain polypropylene powder.
[0168] Example A7
[0169] (1) Repeat the process of Example A1 for the magnesium chloride alcoholate carrier;
[0170] (2) Preparation of olefin polymerization catalyst components
[0171] In a 300 mL glass reaction bottle, add 50 mL of titanium tetrachloride, cool to 0°C, add 0.04 mol of magnesium halide adduct, and stir at 0°C for 30 minutes. Then, slowly raise the temperature to 115°C. During this heating process, add 0.76 mmol of tributyl phosphate and 6 mmol of diethyl 2,3-dicyclohexyl-2-cyanosuccinate. Maintain the temperature at 115°C for 30 minutes, then filter and remove the liquid. Then, wash twice with titanium tetrachloride, and finally wash three times with hexane. After drying, obtain Catalyst C.
[0172] (3) The process of Example A1 was repeated to carry out propylene polymerization using catalyst c.
[0173] Example A8
[0174] (1) Repeat the process of Example A1 for the magnesium chloride alcoholate carrier;
[0175] (2) Preparation of olefin polymerization catalyst components
[0176] In a 300 mL glass reaction bottle, add 120 mL of titanium tetrachloride, cool to -15°C, add 0.04 mol of magnesium halide adduct, and stir at -15°C for 30 minutes. Then, slowly raise the temperature to 90°C. During this heating process, add 0.76 mmol of tributyl phosphate and 6 mmol of dibutyl 2,3-diisopropyl-2-cyanosuccinate. Maintain the temperature at 90°C for 30 minutes, then filter and remove the liquid. Then, wash twice with titanium tetrachloride, and finally wash three times with hexane. After drying, obtain catalyst d.
[0177] (3) The process of Example A1 was repeated to carry out propylene polymerization using catalyst d.
[0178] Example A9
[0179] (1) Repeat the process of Example A1 for the magnesium chloride alcoholate carrier;
[0180] (2) Preparation of olefin polymerization catalyst components
[0181] In a 300 mL glass reaction bottle, add 115 mL of titanium tetrachloride, cool to 0°C, add 0.04 mol of magnesium halide adduct, and stir at 0°C for 30 minutes. Then, slowly raise the temperature to 95°C. During this heating process, add 0.76 mmol of tributyl phosphate and 6 mmol of diethyl 2-isopropyl 3-phenyl-2-cyanosuccinate. Maintain the temperature at 95°C for 30 minutes, then filter and remove the liquid. Then, wash twice with titanium tetrachloride, and finally wash three times with hexane. After drying, obtain Catalyst e.
[0182] (3) Repeat the process of Example A1 and use catalyst e to carry out propylene polymerization.
[0183] Example A10
[0184] (1) Repeat the process of Example A1 for the magnesium chloride alcoholate carrier;
[0185] (2) Preparation of olefin polymerization catalyst components
[0186] In a 300 mL glass reaction bottle, add 110 mL of titanium tetrachloride, cool to 0°C, add 0.04 mol of magnesium halide adduct, and stir at 0°C for 30 minutes. Then, slowly raise the temperature to 112°C. During this heating process, add 0.76 mmol of tributyl phosphate and 6 mmol of diethyl 2-isopropyl 3-cyclopentyl-2-cyanosuccinate. Maintain the temperature at 112°C for 30 minutes, then filter and remove the liquid. Then, wash twice with titanium tetrachloride, and finally wash three times with hexane. After drying, obtain Catalyst f.
[0187] (3) Repeat the process of Example A1 and use catalyst f to carry out propylene polymerization.
[0188] Example A11
[0189] The type of phosphate was changed, and the process was the same as in Example A3 except that tributyl phosphate was replaced by an equimolar amount of trioctyl phosphate.
[0190] Comparative Example A1
[0191] Except for not adding tributyl phosphate, the other procedures are the same as those in Example A1.
[0192] Comparative Example A2
[0193] The process was the same as in Example A1 except that diisobutyl phthalate was used in an equimolar amount instead of diethyl 2,3-diisopropyl-2-cyanosuccinate.
[0194] Comparative Example A3
[0195] The process was the same as in Example A5 except that diisobutyl phthalate was used in an equimolar amount instead of diethyl 2,3-diisopropyl-2-cyanosuccinate.
[0196] Comparative Example A4
[0197] In a reactor that has been repeatedly replaced with high-purity nitrogen, 4.8 g of anhydrous magnesium chloride (0.05 mol), 100 ml of toluene, 4.0 ml of epichlorohydrin (0.05 mol), and 6 ml of tributyl phosphate (0.022 mol) were added in sequence, and the reaction was carried out at a temperature of 60°C for 3 hours. 1.4 g of phthalic anhydride was added, and the reaction was continued for one hour. The temperature was lowered to -29°C, 56 ml of titanium tetrachloride was added dropwise, and the temperature was gradually raised to 85°C. During the heating process, 7.5 mmol of diethyl 2,3-diisopropyl-2-cyanosuccinate was added, and the temperature was kept constant at 85°C for one hour. The mother liquor was filtered off, washed twice with toluene, and then 48 ml of titanium tetrachloride and 72 ml of toluene solution were added. The temperature was kept constant at 110°C for 0.5 hour. After filtration, the treatment was repeated twice, and then washed 5 times with hexane. The remaining solid product was vacuum dried to obtain a solid titanium catalyst component DC4.
[0198] Propylene was polymerized according to step (3) of Example A1 using the solid titanium catalyst component DC4.
[0199] Comparative Example A5
[0200] Except for not adding tributyl phosphate, the other procedures are the same as those of Comparative Example A2.
[0201] The molar ratios of the components in the catalyst components of Example A and Comparative Example A and the angles of repose of the catalyst components, as well as the Mz+1, Mz+1 / Mn, MFR, isotacticity, and (dw / dlogM) / peak height when logMW=3 of the polymers prepared by polymerization of Example A and Comparative Example A for 1 h are shown in Table 1-2.
[0202] Table 1 n p:Mg represents the molar ratio of phosphate to magnesium, n CN:Mg represents the molar ratio of α-cyanosuccinate and / or substituted α-cyanosuccinate to magnesium, n Ti:Mg It represents the molar ratio of titanium to magnesium.
[0203] Table 2 In the above table, MW refers to the molecular weight of the polymer, logMW is used as the abscissa of the GPC curve, dw / dlogM is used as the ordinate of the GPC curve, and the peak height mentioned above refers to the maximum value of dw / dlogM.
[0204] As can be seen from Table 1-2:
[0205] (1) The polypropylene obtained by polymerization of the catalyst components of the present invention for 1 hour has a high Mz+1 and Mz+1 / Mn, indicating a high content of high molecular weight fractions, which is conducive to the formation of more ligaments / intercrystalline bridging chains in the polymer, thus imparting the product with good properties such as better creep resistance and a good balance of stiffness and toughness. Furthermore, the polymer of the present invention also has a low MFR.
[0206] (2) When the polypropylene obtained by polymerization of the catalyst components of the present invention for 1 hour is tested by GPC and logMW=3, the (dw / dlogM) / peak height is less than that without adding phosphate ester. This indicates that the content of the low molecular weight part of the polymer obtained after adding phosphate ester is lower, which is beneficial to its use in the medical and health field (when used as a food medical device, its precipitates are less).
[0207] (3) Compared with Comparative Examples 2-3 (compounds of phosphate and phthalate as internal electron donors), the phosphate of the present invention and the cyanosuccinate diester compound as internal electron donors have excellent synergistic effects, can significantly improve the Mz+1 and Mz+1 / Mn of the polymer, and reduce the MFR of the polymer. The products prepared from the polymer have excellent creep resistance and toughness balance, which broadens the application field of polypropylene.
[0208] (4) The catalyst components of Examples A1-A11 exhibited favorable morphologies, with virtually no cracking. The catalyst components of the present invention exhibited a smaller angle of repose, indicating that the resulting catalysts possessed improved fluidity and were less susceptible to bridging, ensuring smooth catalyst deployment and transport during the production process and contributing to smoother production.
[0209] The following Example B is used to illustrate the preparation method of the catalyst component using phosphate / α-cyanosuccinate and / or substituted α-cyanosuccinate and dialkoxy-substituted alkane as internal electron donors and the process of preparing the polymer.
[0210] Example B1
[0211] (1) A magnesium chloride alcoholate support was prepared according to step (1) of Example A1.
[0212] (2) Preparation of olefin polymerization catalyst components
[0213] In a 300mL glass reaction bottle, add 50ml of titanium tetrachloride, cool to -20°C, add 0.04mol of the magnesium chloride alcoholate carrier prepared above, and stir at 0°C for 60min. Then, slowly raise the temperature to 100°C. During the heating process, add 0.76mmol of tributyl phosphate, 1mmol of 2-isopropyl-2-isopentyl-1,3-dimethoxypropane, and 4.5mmol of 2,3-diisopropyl-2-cyanosuccinic acid diethyl ester. Maintain at 100°C for 60min and filter out the liquid. Then, add titanium tetrachloride and wash twice, and finally wash three times with hexane. After drying, the catalyst is obtained.
[0214] The catalyst has a molar ratio of phosphate to magnesium of 0.00035, a molar ratio of α-cyanosuccinate and / or substituted α-cyanosuccinate to magnesium of 0.07197, a molar ratio of dialkoxy-substituted alkane to magnesium of 0.02044, and a molar ratio of titanium to magnesium of 0.1051. The catalyst has an angle of repose of 33.2°.
[0215] (3) Propylene polymerization
[0216] A 5-liter stainless steel autoclave was purged with nitrogen. Then, 1 mmol of triethylaluminum, 0.05 mmol of methylcyclohexyldimethoxysilane, 10 mL of anhydrous hexane, 10 mg of the above-prepared catalyst (containing 0.0073 mmol of Ti), 1.5 L (standard volume) of hydrogen, and 2.5 L of liquid propylene were introduced into the nitrogen stream. The reaction was heated to 70°C and allowed to react for 1 hour. The temperature was then lowered, the pressure released, and the product was discharged and dried to obtain polypropylene powder.
[0217] The polymerization activity in 1h is 45.6kgPP / g·Cat, the Mz+1 of the polypropylene powder is 6294397, Mz+1 / Mn is 128.39, MFR is 1.1g / 10min, and the bulk density is 0.48g / cm 3 When logMW=3, dw / dlogM is equal to peak height×(10 -3 ) ratio is 4.6; wherein, MW refers to the molecular weight of the polymer, logMW is used as the abscissa of the GPC curve, dw / dlogM is used as the ordinate of the GPC curve, and the above-mentioned peak height refers to the maximum value of dw / dlogM.
[0218] Example B2
[0219] The method of Example B1 was followed, except that the amounts of tributyl phosphate, 2-isopropyl-2-isopentyl-1,3-dimethoxypropane and diethyl 2,3-diisopropyl-2-cyanosuccinate were 1.9 mmol, 4 mmol and 2 mmol, respectively.
[0220] The catalyst has a molar ratio of phosphate to magnesium of 0.00186, a molar ratio of α-cyanosuccinate and / or substituted α-cyanosuccinate to magnesium of 0.03172, a molar ratio of dialkoxy-substituted alkane to magnesium of 0.06569, and a molar ratio of titanium to magnesium of 0.0838. The catalyst has an angle of repose of 33.6°.
[0221] The polymerization activity in 1h is 55.8kgPP / g·Cat, the Mz+1 of the polypropylene powder is 5069700, Mz+1 / Mn is 81.58, MFR is 3.1g / 10min, and the bulk density is 0.48g / cm 3 When logMW=3, dw / dlogM is equal to peak height×(10 -3 ) ratio is 4.9; wherein, MW refers to the molecular weight of the polymer, logMW is used as the abscissa of the GPC curve, dw / dlogM is used as the ordinate of the GPC curve, and the peak height refers to the maximum value of dw / dlogM.
[0222] By adopting the method of Example B of the present invention, using phosphate / α-cyanosuccinate and / or substituted α-cyanosuccinate and dialkoxy-substituted alkane as internal electron donors, not only can the prepared polymer have higher Mz+1 and Mz+1 / Mn, but also the polymerization activity can be further improved.
[0223] Compared to Example A, the polymer prepared in Example B of the present invention has a lower dw / dlogM to GPC curve peak height ratio when logMW=3 in the GPC test, indicating a lower content of the low molecular weight portion of the polymer, which is beneficial for its application in the medical and health fields (less precipitates when used as food and medical devices). Furthermore, the polymer prepared in the present invention has a higher bulk density and has great industrial application prospects.
[0224] By comparing Example B1 and Example B2, it can be found that Example B1 within the preferred dosage range can take into account both the Mz+1 and Mz+1 / Mn of the polymer and the polymerization activity.
[0225] The preferred embodiments of the present invention have been described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, various simple variations of the technical solution of the present invention may be made, including combining the various technical features in any other appropriate manner. These simple variations and combinations should also be regarded as disclosed in the present invention and fall within the scope of protection of the present invention.
Claims
1. A catalyst component for olefin polymerization, characterized in that The catalyst component comprises magnesium, titanium and an internal electron donor; wherein the internal electron donor comprises phosphate and α-cyanosuccinate and / or substituted α-cyanosuccinate, and the molar ratio of phosphate to magnesium is 0.0002-0.002:
1.
2. The catalyst component according to claim 1, wherein The molar ratio of the phosphate to α-cyanosuccinate and / or substituted α-cyanosuccinate is 1:15-500, preferably 1:40-400.
3. The catalyst component according to claim 1 or 2, wherein The phosphate ester includes at least one of a hydrocarbon ester of phosphoric acid, a halogenated hydrocarbon ester of phosphoric acid, a hydrocarbon ester of phosphorous acid, and a halogenated hydrocarbon ester of phosphorous acid; preferably, the hydrocarbon ester of phosphoric acid includes at least one of a mono-hydrocarbon ester of phosphoric acid, a di-hydrocarbon ester of phosphoric acid, and a tri-hydrocarbon ester of phosphoric acid, more preferably a tri-C1-C1 10 Alkyl ester; Further preferably, the phosphate tris-C1-C 10 The alkyl ester includes at least one of tributyl phosphate, trimethyl phosphate, triethyl phosphate, and tripropyl phosphate.
4. The catalyst component according to any one of claims 1 to 3, wherein The α-cyanosuccinate and / or substituted α-cyanosuccinate is selected from at least one compound represented by formula (III): In formula (III), R a 、R b Each independently selected from C1-C 14 Straight chain alkyl, C3-C 14 Branched alkyl, C3-C 10 Cycloalkyl, C6-C 10 Aryl, C7-C 10 Alkaryl or C7-C 10 Aralkyl; R c and R d Each independently selected from H, C1-C 14 Straight chain alkyl, C3-C 14 Branched alkyl, C3-C 10 Cycloalkyl, C6-C 10 Aryl, C7-C 10 Alkaryl or C7-C 10 Aralkyl; R c and R d optionally bonded to each other to form one or more fused ring structures; Preferably, in formula (III), R a 、R b Each independently selected from C1-C 10 Straight chain alkyl, C3-C 10 Branched alkyl, C3-C 10 Cycloalkyl, C6-C 10 Aryl, C7-C 10 Alkaryl or C7-C 10 Aralkyl; R c and R d Each independently selected from C1-C 10 Straight chain alkyl, C3-C 10 Branched alkyl, C3-C 10 Cycloalkyl, C6-C 20 Aryl, C7-C 20 Alkaryl or C7-C 20 Aromatic hydrocarbon group.
5. The catalyst component according to any one of claims 1 to 4, wherein The molar ratio of the α-cyanosuccinate and / or substituted α-cyanosuccinate to the magnesium element is 0.01-0.2:1, preferably 0.03-0.15:1, and more preferably 0.04-0.11:
1.
6. The catalyst component according to any one of claims 1 to 5, wherein The internal electron donor further comprises a dialkoxy substituted alkane, preferably, the dialkoxy substituted alkane is selected from (R 7 )(R 8 )C(OR 9 )(OR 10 ), wherein R 7 and R 8 Each independently selected from hydrogen, C1-C 20 Alkyl, C3-C 20 Cycloalkyl, C6-C 20 Aryl, C7-C 20 Arylalkyl or C7-C 10 The alkylaryl group, R 7 and R 8 They may be optionally linked to form a ring; R 9 and R 10 Each independently selected from C1-C 20 Alkyl; Preferably, the dialkoxy-substituted alkane is selected from (R 7 )(R 8 )C(OR 9 )(OR 10 ) is at least one, wherein R 7 and R 8 Each independently selected from hydrogen, C1-C 10 Alkyl, C3-C 10 Cycloalkyl, C6-C 10 Aryl, C7-C 10 Arylalkyl or C7-C 10 The alkylaryl group, R 7 and R 8 They may be optionally linked to form a ring; R 9 and R 10 Each independently selected from C1-C 10 of alkyl.
7. The catalyst component according to claim 6, wherein The molar ratio of the dialkoxy-substituted alkane to the magnesium element is 0.001-0.15:1, preferably 0.01-0.1:1; And / or, the molar ratio of the phosphate ester to the dialkoxy-substituted alkane is 1:30-400, preferably 1:50-350.
8. The catalyst component according to any one of claims 1 to 7, wherein The magnesium source is a magnesium-containing carrier, and the magnesium-containing carrier includes a magnesium chloride alcoholate carrier and / or an alkoxy magnesium carrier; Preferably, the magnesium chloride alcoholate carrier comprises a component represented by formula (I), MgY 1 Y 2 ·mR’OH of formula (I) In formula (I), Y 1 is selected from halogen, preferably chlorine or bromine; Y 2 is selected from halogen, alkyl or alkoxy; R' is selected from one of halogen-substituted or unsubstituted alkyl, halogen-substituted or unsubstituted cycloalkyl, and halogen-substituted or unsubstituted aralkyl; m is 1-5; Preferably, the alkoxy magnesium support comprises a component represented by formula (II): [R1O] m’ Mg[OCH(CHXR2)(R3)] n Formula (II); In formula (II), R1 is selected from one of a linear alkyl group or a halogen-substituted linear alkyl group, a branched alkyl group or a halogen-substituted branched alkyl group, a cycloalkyl group or a halogen-substituted cycloalkyl group; R2 and R3 are each independently hydrogen, a linear alkyl group or a halogen-substituted linear alkyl group, a branched alkyl group or a halogen-substituted branched alkyl group; X is a halogen; m' is 0.1-1.9, n is 0.1-1.9, and m'+n=2; And / or, the titanium source is titanium halide, and the titanium halide is selected from Ti(OR 4 ) 4-n X' n At least one of the compounds shown, wherein R 4 Selected from C1-C 20 The hydrocarbon group is preferably selected from C1-C 14 The repeated X's are the same or different and are independently selected from F, Cl or Br, and n is an integer from 0 to 4; Preferably, the titanium halide is selected from titanium tetrachloride, titanium tetrabromide, titanium tetraiodide, titanium tetrabutoxide, titanium tetraethoxide, titanium trichloride, titanium tributoxide, titanium dichloride, titanium trichloride, titanium trichloride, titanium trichloride, titanium trichloride, titanium trichloride, titanium tetrachloride, titanium trichloride, titanium trichloride, titanium trichloride, titanium tetrachloride, titanium tetrachloride, titanium tetrachloride, titanium tetrachloride, titanium trichloride, titanium trichloride, titanium trichloride, titanium trichloride, titanium trichloride, titanium tetrachloride, titanium tetrachloride, titanium tetrachloride, titanium tetrachloride, titanium tetrachloride, titanium tetrachloride, titanium trichloride, titanium trichloride, titanium trichloride, titanium trichloride, titanium trichloride, titanium trichloride, titanium trichloride, titanium trichloride, titanium tetra ... trichloride And / or, the molar ratio of the titanium element to the magnesium element is 0.01-0.3:1, preferably 0.06-0.15:
1.
9. A method for preparing a catalyst component for olefin polymerization, characterized in that The method comprises: mixing a magnesium-containing carrier, a titanium halide, and an internal electron donor, wherein the internal electron donor comprises a phosphate and an α-cyanosuccinate and / or a substituted α-cyanosuccinate, and the amounts of the phosphate and the magnesium-containing carrier are such that the molar ratio of the phosphate to the magnesium-containing carrier calculated as magnesium element in the obtained catalyst component is 0.0002-0.002:
1.
10. The method according to claim 9, wherein: The method of mixing the magnesium-containing support, titanium halide, and internal electron donor includes: (1) mixing the magnesium-containing support with the titanium halide; (2) mixing the system of step (1) with the internal electron donor; Preferably, the internal electron donor further comprises a dialkoxy-substituted alkane.
11. The method according to claim 10, wherein: The mixing in step (1) is carried out at -30°C to 0°C, preferably at -25°C to -15°C; and / or, In step (2), the temperature is first raised, and the internal electron donor is added during the heating process; preferably, the temperature is raised to 80°C-120°C, more preferably 90°C-115°C.
12. The method according to claim 10, wherein: The α-cyanosuccinate and / or substituted α-cyanosuccinate and the magnesium-containing support are used in such an amount that the molar ratio of the α-cyanosuccinate and / or substituted α-cyanosuccinate to the magnesium-containing support in the obtained catalyst component, calculated as magnesium element, is 0.01-0.2:1, preferably 0.03-0.15:1, and more preferably 0.04-0.11:1; and / or, the amounts of the phosphoric acid ester and α-cyanosuccinate and / or substituted α-cyanosuccinate are such that the molar ratio of the phosphoric acid ester to α-cyanosuccinate and / or substituted α-cyanosuccinate in the resulting catalyst component is 1:15-500, preferably 1:40-300; and / or, the amounts of the dialkoxy-substituted alkane and the magnesium-containing support are such that the molar ratio of the dialkoxy-substituted alkane to the magnesium-containing support in the obtained catalyst component, calculated as magnesium element, is 0.001-0.15:1, preferably 0.01-0.1:1; And / or, the amounts of the phosphate and the dialkoxy-substituted alkane are such that the molar ratio of the phosphate to the dialkoxy-substituted alkane in the obtained catalyst component is 1:30-400, preferably 1:50-350.
13. A catalyst system for olefin polymerization, characterized in that: The catalyst system comprises: (1) The catalyst component according to any one of claims 1 to 8 and / or the catalyst component prepared by the method according to any one of claims 9 to 12; (2) aluminum alkyls; and (3) Optional external electron donor.
14. The catalyst system according to claim 13, wherein The number of alkyl groups in the alkylaluminum is 1-3, and the number of carbon atoms in the alkyl group is C1-C8. More preferably, the alkylaluminum is selected from at least one of triethylaluminum, tripropylaluminum, tri-n-butylaluminum, triisobutylaluminum, tri-n-octylaluminum, diethylaluminum monohydrogenate, diisobutylaluminum monohydrogenate, diethylaluminum monochloride, diisobutylaluminum monochloride, sesquiethylaluminum chloride, and ethylaluminum dichloride; And / or, the external electron donor is selected from at least one silicon-containing compound, preferably at least one selected from cyclohexylmethyldimethoxysilane, diisopropyldimethoxysilane, di-n-butyldimethoxysilane, diisobutyldimethoxysilane, diphenyldimethoxysilane, methyl-tert-butyldimethoxysilane, dicyclopentyldimethoxysilane, 2-ethylpiperidinyl-2-tert-butyldimethoxysilane, (1,1,1-trifluoro-2-propyl)-2-ethylpiperidinyldimethoxysilane, and (1,1,1-trifluoro-2-propyl)-methyldimethoxysilane; Preferably, the molar ratio of the catalyst component to the alkyl aluminum is 1:15-718, and / or the molar ratio of the catalyst component to the external electron donor is 1:1-111, wherein the mole of the catalyst component is calculated based on the mole of the Ti element therein.
15. Use of the catalyst component according to any one of claims 1 to 8 and / or the catalyst component prepared by the method according to any one of claims 9 to 12 and / or the catalyst system according to claim 13 or 14 in olefin polymerization.
16. A method for olefin polymerization, characterized in that: The olefin polymerization method comprises: conducting an olefin polymerization reaction in the presence of the catalyst component according to any one of claims 1 to 8 and / or the catalyst component prepared by the method according to any one of claims 9 to 12 and / or the catalyst system according to claim 13 or 14; Preferably, the olefin is selected from at least one compound represented by the formula CH2=CHR, wherein R is hydrogen or a C1-C6 straight chain or C3-C6 branched chain alkyl group; Preferably, the polymerization conditions include: temperature of 0-150° C., time of 0.1-8 hours, and pressure of 0.01-10 MPa.