Polycarbonate oligomer, manufacturing method therefor, curable composition, epoxy crosslinked product, and method for degrading epoxy crosslinked product by aminolysis
Patent Information
- Application Number
- MYPI2025002577
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2022-12-09
- Publication Date
- 2024-06-09
AI Technical Summary
Existing polycarbonate recycling technology mainly relies on mechanical processing or physical mixing, which results in the material being easily damaged, and the re-solidification process requires the participation of solvents, which is inconvenient to operate and harmful to the environment. Moreover, chemical recycling methods require a large amount of solvents and cumbersome separation and purification. Industrialization is difficult to achieve.
Polycarbonate oligomers are prepared through alcoholysis and used as hardeners for epoxy resins. They are cured with epoxy resins to form epoxy cured products with excellent properties. They are also recyclable through aminolysis and degradation to avoid solvents. use.
It realizes the reusability and environmental protection benefits of polycarbonate, reduces the use of solvents, improves the processability and high-temperature resistance of the cured product, and realizes the recycling of high-purity phenoxy resin through aminolysis degradation.
Smart Images

Figure PI2025002577_DRAWING_001 
Figure PI2025002577_DRAWING_002 
Figure PI2025002577_DRAWING_003
Abstract
Description
Polycarbonate oligomer, preparation method thereof, curable composition, epoxy cured product and method for aminolysis degradation of epoxy cured product Technical Field
[0001] The present invention relates to an oligomer and a preparation method thereof, and in particular to a polycarbonate oligomer, a preparation method thereof, a curable composition, an epoxy cured product and a method for aminolysis degradation of the epoxy cured product. Background Art
[0002] Polycarbonate (PC) is currently produced industrially by transesterifying bisphenol A with diphenyl carbonate at high temperatures. It is a polymer material with excellent optical and mechanical properties and is widely used in consumer products such as drinking water bottles, optical discs, data storage devices, and automotive parts.
[0003] Currently, polycarbonate recycling is still primarily performed physically through mechanical processing or physical blending, where new materials are added to compensate for the physical defects of the recycled material. Although this operation is relatively simple, the physical properties of polycarbonate are easily destroyed during the recycling process, which still greatly limits its application. In addition, when the recycled polycarbonate is mixed with epoxy resin for re-curing, it is often still necessary to dissolve the polycarbonate and epoxy resin in a solvent before the subsequent curing operation can be carried out. Therefore, the re-curing and reuse of existing recycled polycarbonate still requires the participation of a solution, which is inconvenient and environmentally unfriendly.
[0004] To address future recycling issues, many academic articles have begun discussing chemical recycling methods, which involve degrading bisphenol A monomer (BPA) to obtain it, which is then used in polycarbonate synthesis. However, obtaining high-purity BPA monomer using this method requires large amounts of solvents and cumbersome separation and purification steps, making it difficult to commercialize.
[0005] In view of this, how to use waste polycarbonate as a hardener for epoxy resin and solidify it with epoxy resin so that the solidified product has the characteristics of recyclability and decomposition to achieve the sustainable utilization of waste polycarbonate has become the goal of relevant industries.
[0006] Summary of the Invention
[0007] An object of the present invention is to provide a polycarbonate oligomer and a preparation method thereof, wherein waste polycarbonate is prepared into the polycarbonate oligomer by utilizing the principle of alcoholysis, so that the polycarbonate oligomer has better processability and can be used as an epoxy resin hardener.
[0008] Another object of the present invention is to provide a curable composition, an epoxy cured product, and a method for degrading the epoxy cured product by aminolysis, wherein a polycarbonate oligomer is cured with an epoxy resin, and the resulting cured product retains excellent physical properties and is recyclable.
[0009] One embodiment of the present invention provides a polycarbonate oligomer having a structure as shown in formula (I):
[0010]
[0011] wherein R1 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an alkoxy group having 1 to 6 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a halogen atom; and R2 is an alkyl group having 1 to 10 carbon atoms, an ether group having 1 to 10 carbon atoms, a cycloalkyl group having 3 to 6 carbon atoms, or a structure represented by formula (1), formula (2), formula (3), formula (4), formula (5), formula (6), or formula (7):
[0012]
[0013] Wherein, X is a single bond, a structure represented by formula (8), formula (9), formula (10), formula (11), formula (12), formula (13), formula (14), formula (15), formula (16), formula (17) or formula (18):
[0014]
[0015] wherein R3 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an alkoxy group having 1 to 6 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a halogen atom; R4 is a hydrogen atom or a methyl group; a is an integer from 0 to 4; b is an integer from 0 to 5; n is any number from 0 to 60; and m and p are each independently any number from 0 to 50. X1 and X2 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an aromatic group having 6 to 12 carbon atoms.
[0016] Another embodiment of the present invention provides a method for preparing the aforementioned polycarbonate oligomer, comprising a dissolution step, an addition step, a washing step, and a filtration step. The dissolution step involves dissolving a polycarbonate in a solvent, heating the mixture to a heated temperature, and stirring to form a first mixture. The addition step involves adding a compound represented by formula (II) to the first mixture and maintaining the mixture at the heated temperature to react, thereby forming a second mixture:
[0017]
[0018] The washing step is to cool the second mixture and to precipitate and wash it with an alcohol solvent to form a third mixture. The filtering step is to filter and dry the third mixture to obtain a polycarbonate oligomer.
[0019] According to the preparation method of the polycarbonate oligomer described above, the solvent can be selected from the group consisting of N,N-dimethylacetamide, N-methylpyrrolidone, dimethylformamide, anisole, dimethyl sulfoxide, propylene glycol methyl ether acetate, and propylene glycol methyl ether propionate.
[0020] According to the method for preparing the polycarbonate oligomer described in the preceding paragraph, the heating temperature may be 100°C to 180°C.
[0021] According to the method for preparing the polycarbonate oligomer described in the preceding paragraph, the molar ratio of the polycarbonate to the compound represented by formula (II) can be 1:10 to 1:90.
[0022] Another embodiment of the present invention provides a curable composition comprising the aforementioned polycarbonate oligomer, an epoxy resin, and a catalyst, which are mixed at a mixing temperature to prepare a sample, wherein the equivalent ratio of the carbonate group of the polycarbonate oligomer to the epoxy group of the epoxy resin is 0.5 to 3.0.
[0023] According to the curable composition described in the preceding paragraph, the catalyst may be selected from the group consisting of 4-dimethylaminopyridine, imidazole, 2-methylimidazole, 2-phenylimidazole, and 2-ethyl-4-methylimidazole.
[0024] According to the curable composition described in the preceding paragraph, the amount of the catalyst added may be 0.05 weight percent to 5.0 weight percent of the epoxy resin content.
[0025] According to the curable composition described in the preceding paragraph, the mixing temperature may be 90°C to 170°C.
[0026] Another embodiment of the present invention provides an epoxy cured product obtained by subjecting the curable composition to a curing reaction.
[0027] According to the epoxy cured material described in the previous paragraph, the curing reaction is completed by heating the curable composition, and a curing temperature of the curing reaction can be 150° C. to 240° C.
[0028] Another embodiment of the present invention provides a method for aminolysis degradation of epoxy curing material, comprising providing the aforementioned epoxy curing material and performing a degradation step, wherein the degradation step is to react a compound containing an aliphatic amine group with the epoxy curing material to aminolysis degrade the epoxy curing material.
[0029] According to the method for aminolysis degradation of epoxy cured material described in the preceding paragraph, the epoxy cured material is degraded to form a phenoxy resin represented by formula (III):
[0030]
[0031] Wherein, Y is a single bond, a structure represented by formula (8), formula (9), formula (10), formula (11), formula (12), formula (13), formula (14), formula (15), formula (16), formula (17), formula (18), or a structure represented by formula (19):
[0032]
[0033] The polycarbonate oligomer of the present invention reuses polycarbonate as an epoxy resin hardener. The mixture of the two requires no solvent and can be applied to epoxy molding compound (EMC) encapsulation. The resulting epoxy cured product, catalyzed by a catalyst, exhibits excellent properties and can be degraded for recycling, achieving environmental benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] To make the above and other objects, features, advantages and embodiments of the present invention more apparent, the following descriptions of the accompanying drawings are given:
[0035] FIG1 is a flow chart showing the steps of a method for preparing a polycarbonate oligomer according to one embodiment of the present invention;
[0036] FIG2 is a flow chart showing the steps of a method for preparing an epoxy cured product according to another embodiment of the present invention;
[0037] FIG3 is a flow chart showing the steps of a method for aminolysis degradation of epoxy cured materials according to another embodiment of the present invention;
[0038] FIG4 shows the 1H-NMR spectrum of Example 1;
[0039] FIG5 shows the 1H-NMR spectrum of Comparative Example 1;
[0040] FIG6 shows a Fourier transform infrared spectrum of Example 1;
[0041] FIG7 shows a Fourier transform infrared spectrum of Example 4; and
[0042] FIG8 shows the 1H-NMR spectrum of Example 7.
[0043]
Explanation of symbols
[0044] 100: Preparation method of polycarbonate oligomer
[0045] 200: Preparation method of epoxy cured product
[0046] 300: Method for aminolysis degradation of epoxy cured products
[0047] 110,120,130,140,210,220,310,320: Steps DETAILED DESCRIPTION
[0048] The following will discuss various embodiments of the present invention in more detail. However, this embodiment can be applied to various inventive concepts and can be specifically implemented in various specific scopes. The specific embodiments are for illustrative purposes only and are not intended to limit the scope of the disclosure.
[0049] In this invention, compound structures are sometimes represented using skeleton formulas. This representation may omit carbon atoms, hydrogen atoms, and carbon-hydrogen bonds. If a functional group is explicitly depicted in a structural formula, the depicted group shall prevail.
[0050] In the present invention, "a polycarbonate oligomer having a structure as shown in formula (I)" may sometimes be expressed as a polycarbonate oligomer represented by formula (I) or polycarbonate oligomer (I) for the sake of brevity and fluency, and the representation of other compounds or groups may be deduced similarly.
[0051] <Polycarbonate oligomer>
[0052] The present invention provides a polycarbonate oligomer having a structure as shown in formula (I):
[0053]
[0054] wherein R1 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an alkoxy group having 1 to 6 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a halogen atom; and R2 is an alkyl group having 1 to 10 carbon atoms, an ether group having 1 to 10 carbon atoms, a cycloalkyl group having 3 to 6 carbon atoms, or a structure represented by formula (1), formula (2), formula (3), formula (4), formula (5), formula (6), or formula (7):
[0055]
[0056] Wherein, X is a single bond, a structure represented by formula (8), formula (9), formula (10), formula (11), formula (12), formula (13), formula (14), formula (15), formula (16), formula (17) or formula (18):
[0057]
[0058] wherein R3 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an alkoxy group having 1 to 6 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a halogen atom; R4 is a hydrogen atom or a methyl group; a is an integer from 0 to 4; b is an integer from 0 to 5; n is any number from 0 to 60; and m and p are each independently any number from 0 to 50. X1 and X2 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an aromatic group having 6 to 12 carbon atoms.
[0059] Therefore, the polycarbonate oligomer of the present invention has better processability than high molecular weight polycarbonate and better compatibility with epoxy resin, and can be used as an epoxy resin hardener.
[0060] <Method for Preparing Polycarbonate Oligomer>
[0061] 1 , which illustrates a flow chart of a method 100 for preparing a polycarbonate oligomer according to one embodiment of the present invention. In FIG1 , the method 100 for preparing a polycarbonate oligomer includes steps 110 , 120 , 130 , and 140 .
[0062] Step 110 is a dissolution step in which a polycarbonate is dissolved in a solvent, and the mixture is heated to a heating temperature and stirred to form a first mixture. Specifically, the solvent is preferably a non-alcoholic or non-amine solvent having a boiling point above 110°C and capable of dissolving the polycarbonate. Thus, the solvent of the present invention can be selected from the group consisting of N,N-dimethylacetamide (DMAc), N-methylpyrrolidone (NMP), dimethylformamide (DMF), anisole, dimethyl sulfoxide (DMSO), propylene glycol methyl ether acetate, and propylene glycol methyl ether propionate. The heating temperature can be between 100°C and 180°C, preferably between 130°C and 170°C.
[0063] Step 120 is an adding step, wherein a compound represented by formula (II) is added to the first mixture and maintained at a heated temperature to react to form a second mixture:
[0064]
[0065] The definition of R2 is as described above and is not further elaborated here. In addition, the molar ratio of the polycarbonate to the compound represented by formula (II) can be 1:10 to 1:90, preferably 1:40 to 1:70.
[0066] Step 130 is a cleaning step in which the second mixture is cooled and precipitated and cleaned with an alcohol solvent to form a third mixture. Specifically, the alcohol solvent may be methanol, ethanol, or isopropanol, but is not limited thereto.
[0067] Step 140 is to perform a filtration step, in which the third mixture is filtered and dried to obtain polycarbonate oligomer, which is a powder product.
[0068] <Curable Composition>
[0069] The present invention provides a curable composition comprising the aforementioned polycarbonate oligomer, an epoxy resin and a catalyst, wherein the equivalent ratio of the carbonate groups of the polycarbonate oligomer to the epoxy groups of the epoxy resin can be 0.5 to 3.0.
[0070] The epoxy resin can be bisphenol A epoxy resin (DGEBA), phenol novolac epoxy resin (PNE), cresol novolac epoxy resin (CNE), dicyclopentadiene-phenol epoxy resin (DNE), naphthalene-containing epoxy resin, phosphorus-based epoxy resin, or a mixture thereof. In other words, the epoxy resins can be used alone or in combination. When two or more epoxy resins are used, they can be mixed in any proportion. By selecting the appropriate epoxy resin, the desired properties can be imparted to the subsequent cured product.
[0071] The catalyst can be selected from the group consisting of 4-dimethylaminopyridine (DMAP), imidazole, 2-methylimidazole, 2-phenylimidazole, and 2-ethyl-4-methylimidazole. The catalyst can react with the epoxy groups of the epoxy resin, facilitating the subsequent curing reaction. Specifically, the catalyst can be added in an amount of 0.05 to 5.0 weight percent, preferably 0.1 to 0.5 weight percent, based on the epoxy resin content.
[0072] Specifically, the curable composition is prepared by mixing a polycarbonate oligomer represented by formula (I), an epoxy resin, and a catalyst at a mixing temperature, wherein the mixing temperature may be 90°C to 170°C, preferably 110°C to 140°C. Too low a temperature will result in uneven mixing, while too high a temperature will result in gelation due to the curing reaction, making it impossible to prepare a sample smoothly.
[0073] <Epoxy Cured Material>
[0074] The present invention further provides a cured epoxy material obtained by subjecting the curable composition to a curing reaction. The curing reaction is briefly described below with reference to FIG2 , which illustrates a flow chart of a method 200 for preparing a cured epoxy material according to another embodiment of the present invention. In FIG2 , the method 200 includes steps 210 and 220.
[0075] Step 210 is a mixing step in which a polycarbonate oligomer, an epoxy resin, and a catalyst are mixed to form a curable composition. Specifically, step 210 forms a solid prepolymer containing the curable composition from the polycarbonate oligomer, epoxy resin, and catalyst. Details regarding the polycarbonate oligomer, epoxy resin, and catalyst are described above and are not further elaborated here.
[0076] Step 220 is a curing step to crosslink the polycarbonate oligomer and the epoxy resin under the catalysis of a catalyst to form an epoxy cured product. The curing reaction is completed by heating the curable composition, and the curing temperature of the curing reaction can be 150° C. to 240° C., preferably 170° C. to 200° C.
[0077] <Method for Degrading Epoxy Cured Material by Amine Decomposition>
[0078] 3 , which illustrates a flow chart of a method 300 for degrading epoxy cured materials by aminolysis according to another embodiment of the present invention. In FIG3 , the method 300 for degrading epoxy cured materials by aminolysis includes steps 310 and 320 .
[0079] Step 310 is to provide the aforementioned epoxy curing material. Step 320 is to perform a degradation step, wherein a compound containing an aliphatic amine group reacts with the epoxy curing material to degrade the epoxy curing material by aminolysis.
[0080] In addition, the aforementioned epoxy cured product can be degraded and washed with alcohol to obtain a phenoxy resin as shown in formula (III):
[0081]
[0082] Wherein, the definition of X is as described above and is not repeated here, and Y is a single bond, a structure represented by formula (8), formula (9), formula (10), formula (11), formula (12), formula (13), formula (14), formula (15), formula (16), formula (17), formula (18), or a structure represented by formula (19):
[0083]
[0084] Furthermore, the phenoxy resin represented by formula (III) is advantageously reusable as an auxiliary agent.
[0085] The present invention is further illustrated by the following specific examples, which are intended to facilitate those skilled in the art to which the present invention relates, so that they can fully utilize and practice the present invention without excessive interpretation. These examples should not be construed as limiting the scope of the present invention, but are intended to illustrate how to implement the materials and methods of the present invention.
[0086] <Examples / Comparative Examples>
[0087] <Preparation of Polycarbonate Oligomer>
[0088] Example 1: Take 100 g (4×10 -3 150 g of N,N-dimethylacetamide solvent was added to 0.17 mole of polycarbonate pellets (purchased from Chi Mei Industrial, product code PC-122). The mixture was heated to 150°C and maintained at that temperature with stirring to dissolve the polycarbonate pellets in the solvent to form a first mixture. 18.3 g (0.17 mole) of benzyl alcohol was then added and reacted for 9 hours to form a second mixture. The second mixture was then cooled and poured into methanol for washing and precipitation to form a third mixture. The third mixture was then filtered by vacuum filtration to obtain a white powder, which was then dried in a vacuum oven at 110°C to obtain the polycarbonate oligomer powder of Example 1 with a yield of 75%. Specifically, the number average molecular weight (Mn) of the polycarbonate PC-122 was 24,400, and the weight average molecular weight (Mw) was 45,488. The polycarbonate oligomer of Example 1, as measured by gel permeameter chromatography (GPC), had a number average molecular weight (Mn) of 2,391 and a weight average molecular weight (Mw) of 3,532.
[0089] Example 2: Take 100 g (4.1×10 -3 150 g of N,N-dimethylacetamide solvent was added to 0.25 mole of polycarbonate pellets (purchased from Chi Mei Industrial, product code PC-122). The mixture was heated to 150°C and maintained at that temperature with stirring to dissolve the polycarbonate pellets in the solvent to form a first mixture. 27.41 g (0.25 mole) of benzyl alcohol was then added and reacted for 9 hours to form a second mixture. The second mixture was then cooled and poured into methanol for washing and precipitation to form a third mixture. The third mixture was then filtered by vacuum filtration to obtain a white powder, which was then dried in a vacuum oven at 110°C to obtain the polycarbonate oligomer powder of Example 2 with a yield of 45%. Specifically, the number average molecular weight (Mn) of the polycarbonate PC-122 was 24,400, and the weight average molecular weight (Mw) was 45,488. The polycarbonate oligomer of Example 2 was measured by gel permeameter (GPC) to have a number average molecular weight (Mn) of 2,163 and a weight average molecular weight (Mw) of 2,747.
[0090] Example 3: Take 100 g (4.3×10 -3150 g (0.17 mole) of waste polycarbonate was added to 150°C of N,N-dimethylacetamide solvent. The mixture was heated to 150°C and maintained at this temperature with stirring to dissolve the waste polycarbonate in the solvent, forming a first mixture. 18.3 g (0.17 mole) of benzyl alcohol was then added and allowed to react for 9 hours to form a second mixture. The second mixture was then cooled and poured into methanol for washing and precipitation to form a third mixture. The third mixture was then filtered by vacuum filtration to obtain a white powder, which was then dried in a vacuum oven at 110°C to obtain the polycarbonate oligomer powder of Example 3 with a yield of 78%. Specifically, gel permeameter chromatography (GPC) showed that the number average molecular weight (Mn) of the waste polycarbonate was 23,512 and the weight average molecular weight (Mw) was 44,758, while the number average molecular weight (Mn) of the polycarbonate oligomer of Example 3 was 3,561 and the weight average molecular weight (Mw) was 5,707.
[0091] Comparative Example 1: Take 100 g (4.1×10 -3 150 g (0.04 mole) of polycarbonate pellets (purchased from Chi Mei Industrial, product code PC-122) were added to a mixture of 150 g (150°C) of N,N-dimethylacetamide solvent. The mixture was heated to 150°C and maintained at that temperature with stirring to dissolve the polycarbonate pellets in the solvent, forming a first mixture. 4.58 g (0.04 mole) of benzyl alcohol was then added and reacted for 9 hours to form a second mixture. The second mixture was then cooled and poured into methanol for washing and precipitation to form a third mixture. The third mixture was then filtered by vacuum filtration to obtain a white powder, which was then dried in a vacuum oven at 110°C to obtain the polycarbonate oligomer powder of Comparative Example 1 with a yield of 88%. Specifically, the number average molecular weight (Mn) of the polycarbonate PC-122 is 24,400, and the weight average molecular weight (Mw) is 45,488. The polycarbonate oligomer of Comparative Example 1, as measured by gel permeameter chromatography (GPC), has a number average molecular weight (Mn) of 8,798 and a weight average molecular weight (Mw) of 10,777.
[0092] The reaction equations for Examples 1 to 3 and Comparative Example 1 are shown in Table 1 below.
[0093]
[0094] Examples 1 to 3 and Comparative Example 1 were 1 H-NMR analysis was performed to confirm the structures of Examples 1 to 3 and Comparative Example 1. 1 H-NMR spectrum, FIG5 shows the comparative example 1 1 H-NMR spectra, and the 1The H-NMR spectrum is similar to that of Example 1 and is not shown here. As shown in Figures 4 and 5 , the products of Examples 1 to 3 are all polycarbonate oligomers, and the molecular weight of Comparative Example 1 is larger than that of Examples 1 to 3.
[0095] <Preparation of Epoxy Cured Material>
[0096] Example 4: 2 g of Example 1 (127.14 g / eq) and 2.91 g of bisphenol A epoxy resin (purchased from Changchun Resins, product code BE188) were melt-stirred at 110° C. in a ratio such that the equivalent ratio of the two was 1. After mixing, 0.006 g of 2-phenylimidazole (0.2 wt % of BE188) was added as a catalyst at 90° C. and melt-stirred to obtain a mixed prepolymer. The mixture was then cured in an oven at 175° C. for 30 minutes to obtain the epoxy cured product of Example 4.
[0097] Example 5: 2 g of Example 2 (127.14 g / eq) and 2.91 g of bisphenol A epoxy resin (purchased from Changchun Resins, product code BE188) were melted and stirred at 110° C. at an equivalent ratio of 1. After mixing, 0.006 g of 2-phenylimidazole (0.2 wt % of BE188) was added as a catalyst at 90° C. The remaining steps were the same as in Example 4 to obtain the epoxy cured product of Example 5.
[0098] Example 6: 2 g of Example 3 (127.14 g / eq) and 2.91 g of bisphenol A epoxy resin (purchased from Changchun Resins, product code BE188) were melted and stirred at 110° C. at an equivalent ratio of 1. After mixing, 0.006 g of 2-phenylimidazole (0.2 wt % of BE188) was added as a catalyst at 90° C. The remaining steps were the same as in Example 4 to obtain the epoxy cured product of Example 6.
[0099] Comparative Example 2: 2 g of polycarbonate (available from Chi Mei Industrial, product code PC-122, 127.14 g / eq) and 2.91 g of bisphenol A epoxy resin (available from Chang Chun Resins, product code BE188) were melt-stirred at 140°C at an equivalent ratio of 1. However, complete melt mixing failed. Furthermore, 0.006 g of 2-phenylimidazole (0.2 wt% of BE188) was added as a catalyst at 140°C, but the mixture immediately gelled and could not be mixed smoothly to obtain a prepolymer.
[0100] Comparative Example 3: 2 g of polycarbonate (purchased from Chi Mei Industrial, product code PC-122, 127.14 g / eq) and 2.91 g of bisphenol A epoxy resin (purchased from Chang Chun Resins, product code BE188) were melt-stirred at 140°C to achieve an equivalent ratio of 1. After mixing, 0.006 g of 4-dimethylaminopyridine (0.2 wt% of BE188) was added as a catalyst at 140°C. However, the mixture immediately gelled, preventing smooth mixing to produce a prepolymer.
[0101] Comparative Example 4: 2 g of waste polycarbonate (127.14 g / eq) and 2.91 g of bisphenol A epoxy resin (purchased from Chang Chun Resins, product code BE188) were melt-stirred at 140°C in an equivalent ratio of 1. After mixing, 0.006 g of 2-phenylimidazole (0.2 wt% of BE188) was added as a catalyst at 140°C. However, the mixture immediately gelled and could not be smoothly mixed to obtain a prepolymer.
[0102] Comparative Example 5: 2 g of the polycarbonate oligomer (127.14 g / eq) of Comparative Example 1 and 2.91 g of bisphenol A epoxy resin (purchased from Chang Chun Resins, product code BE188) were melt-stirred at 140°C in a ratio of 1. After mixing, 0.006 g of 2-phenylimidazole (0.2 wt% of BE188) was added as a catalyst at 140°C. However, the mixture immediately gelled and could not be smoothly mixed to obtain a prepolymer.
[0103] Comparative Example 6: 2 g of phenolic resin (purchased from Chang Chun Resins, product code PF8110, 127.14 g / eq) and 2.91 g of bisphenol A epoxy resin (purchased from Chang Chun Resins, product code BE188) were melted and stirred at 140° C. at an equivalent ratio of 1. After mixing, 0.006 g of 2-phenylimidazole (0.2 wt % of BE188) was added as a catalyst at 90° C. The remaining steps were the same as in Example 4 to obtain the epoxy cured product of Comparative Example 6.
[0104] Please refer to Figures 6 and 7, wherein Figure 6 shows the Fourier transform infrared spectrum (FTIR) of Example 1, and Figure 7 shows the Fourier transform infrared spectrum (FTIR) of Example 4. As can be seen from the results of Figure 6, the characteristic peak of C=O on the carbonyl group in the polycarbonate oligomer of Example 1 is located at 1764 cm -1 7 , it can be seen that after Example 1 and the epoxy resin are cured, the characteristic peak of C=O on the carbonyl group in the epoxy cured product of Example 4 shifts to 1748 cm -1, indicating that the carbonyl group is converted from an aromatic carbonate structure to an aliphatic carbonate structure. The reaction is shown in Table 2 below.
[0105]
[0106] According to the above results, when using Comparative Example 1 and polycarbonate as epoxy hardeners, heating to 140°C is required for melt mixing. Cooling causes the sample to solidify, forcing the catalyst to be added only at high temperatures. Adding the catalyst at high temperatures triggers the reaction during mixing, which can easily cause the sample to gel during the process, preventing smooth sample preparation. The polycarbonate oligomers of Examples 1 to 3 of the present invention have lower molecular weights than Comparative Example 1 and polycarbonate, resulting in better miscibility during melt mixing. They can be melt mixed with epoxy resin at 110°C and remain molten after cooling to 90°C, facilitating catalyst addition and providing a good processing window. The curable composition can be fully reacted upon curing at 175°C, confirming good reactivity with epoxy resin and confirming its suitability for use as an epoxy hardener. Furthermore, they can be uniformly mixed at high temperatures and are readily operable after the addition of the catalyst, preventing immediate gelation, resulting in a long processing time.
[0107] <Thermal Property Evaluation>
[0108] Thermal properties of the epoxy cured products of Examples 4 to 6 and Comparative Example 6 were evaluated using a differential scanning calorimeter (DSC) at a heating rate of 10°C / min to measure the glass transition temperature (T g ) and T g The measurement results are listed in Table 3 below.
[0109]
[0110] As can be seen from the results in Table 3 above, the glass transition temperatures of Examples 4 to 6 fluctuate with the molecular weight of the oligomer. Although their performance is slightly inferior to that of epoxy cured with a phenolic hardener, they still exhibit heat resistance exceeding 120°C, which is sufficient for many applications.
[0111] <Degradable Epoxy Cured Material>
[0112] To investigate the degradation properties of epoxy curing agents cured with the polycarbonate oligomers of the present invention, 0.2 g of each of the epoxy curing agents from Examples 4 to 6 and Comparative Example 6 was placed in a reactor with 4 g of ethanolamine (MEA) and heated in an oven. After the reaction, the ethanolamine was removed to yield fully degraded epoxy curing agents from Examples 7 to 9 and Comparative Example 7. Examples 7 to 9 represent the degradation results of the epoxy curing agents from Examples 4 to 6, while Comparative Example 7 represents the degradation results of the epoxy curing agent from Comparative Example 6. Table 4 below shows the epoxy curing agent type, reaction temperature (°C), reaction time (hrs), and residual weight (%) used in Examples 7 to 9 and Comparative Example 7.
[0113]
[0114] The results in Table 4 show that Examples 4 through 6 all use the polycarbonate oligomer of the present invention as the epoxy curing agent. When the epoxy curing agent, formed by reacting with the epoxy resin, is degraded, it only requires the addition of an aliphatic amine and heating to initiate an aminolysis reaction. Ultimately, the epoxy curing agent is completely decomposed, with a residual weight of 0%. In contrast, Comparative Example 6 uses a phenolic resin as the curing agent, which lacks the ability to decompose, and thus ultimately retains its original epoxy curing state.
[0115] In addition, please refer to FIG8, which shows the embodiment 7. 1 H-NMR spectrum. Example 7 The epoxy cured product of Example 4 of the present invention was subjected to degradation reaction with ethanolamine. After the reaction was completed, the excess ethanolamine was removed, and then washed with ethanol and filtered and dried to obtain a light yellow solid product. The light yellow solid product was 1 H-NMR analysis, as shown in Figure 8 , shows that the degradation product of the epoxy curing material of Example 4 after reacting with ethanolamine is a high-purity phenoxy resin. The reaction equation is shown in Table 5 below. Gel permeameter chromatography (GPC) analysis revealed a number average molecular weight (Mn) of 8,391 and a weight average molecular weight (Mw) of 10,612. This product can be used as a polyol oligomer for modification or as a coating additive, achieving complete recycling.
[0116]
[0117] In summary, the present invention can produce polycarbonate oligomers through alcoholysis of waste polycarbonate, which can be used as epoxy resin hardeners. Furthermore, the polycarbonate oligomers of the present invention can be directly mixed with epoxy resin for curing, reducing the use of solvents compared to prior art and representing a significant breakthrough in epoxy resin melt processing. Curing at high temperatures can produce a high-temperature-resistant cured product, which can then be completely aminolyzed after being soaked in aliphatic amines and heated, ultimately yielding a high-purity phenoxy resin. This resin can potentially be recycled as an additive into the product cycle, thereby achieving waste recycling.
[0118] Although the present invention has been disclosed above in terms of embodiments, this is not intended to limit the present invention. Anyone skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be determined by the appended claims.
Claims
1. A polycarbonate oligomer, characterized in that Having a structure as shown in formula (I): wherein R1 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an alkoxy group having 1 to 6 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a halogen atom; and R2 is an alkyl group having 1 to 10 carbon atoms, an ether group having 1 to 10 carbon atoms, a cycloalkyl group having 3 to 6 carbon atoms, or a structure represented by formula (1), formula (2), formula (3), formula (4), formula (5), formula (6), or formula (7): Wherein, X is a single bond, a structure represented by formula (8), formula (9), formula (10), formula (11), formula (12), formula (13), formula (14), formula (15), formula (16), formula (17) or formula (18): wherein R3 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an alkoxy group having 1 to 6 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a halogen atom; R4 is a hydrogen atom or a methyl group; a is an integer from 0 to 4; b is an integer from 0 to 5; n is any number from 0 to 60; and m and p are each independently any number from 0 to 50; wherein X1 and X2 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an aromatic group having 6 to 12 carbon atoms.
2. A method for preparing a polycarbonate oligomer according to claim 1, characterized in that: Include: Performing a dissolving step, wherein a polycarbonate is dissolved in a solvent, and the mixture is heated to a heating temperature and stirred to form a first mixture; An adding step is performed, wherein a compound represented by formula (II) is added to the first mixture and the mixture is reacted at the heating temperature to form a second mixture: performing a washing step, wherein the second mixture is cooled and precipitated and washed with an alcohol solvent to form a third mixture; and A filtration step is performed to filter and dry the third mixture to obtain the polycarbonate oligomer.
3. The method for preparing a polycarbonate oligomer according to claim 2, wherein: The solvent is selected from the group consisting of N,N-dimethylacetamide, N-methylpyrrolidone, dimethylformamide, anisole, dimethyl sulfoxide, propylene glycol methyl ether acetate, and propylene glycol methyl ether propionate.
4. The method for preparing a polycarbonate oligomer according to claim 2, wherein: The heating temperature is 100°C to 180°C.
5. The method for preparing a polycarbonate oligomer according to claim 2, wherein: The molar ratio of the polycarbonate to the compound represented by formula (II) is 1:10 to 1:
90.
6. A curable composition, characterized in that The method comprises the polycarbonate oligomer as claimed in claim 1, an epoxy resin and a catalyst, and the mixture is mixed at a mixing temperature, wherein the equivalent ratio of the carbonate group of the polycarbonate oligomer to the epoxy group of the epoxy resin is 0.5 to 3.
0.
7. The curable composition according to claim 6, wherein The catalyst is selected from the group consisting of 4-dimethylaminopyridine, imidazole, 2-methylimidazole, 2-phenylimidazole, and 2-ethyl-4-methylimidazole.
8. The curable composition according to claim 6, wherein The added amount of the catalyst is 0.05 weight percent to 5.0 weight percent of the epoxy resin content.
9. The curable composition according to claim 6, wherein The mixing temperature is from 90°C to 170°C.
10. An epoxy cured product, characterized in that: The invention is obtained by subjecting the curable composition according to any one of claims 6 to 9 to a curing reaction.
11. The epoxy cured product according to claim 10, wherein The curing reaction is completed by heating the curable composition, and a curing temperature of the curing reaction is 150° C. to 240° C.
12. A method for degrading epoxy cured products by aminolysis, characterized in that: Include: Providing the epoxy cured product according to claim 10; and A degradation step is performed in which a compound containing an aliphatic amine group reacts with the epoxy curing material to degrade the epoxy curing material by aminolysis.
13. The method for degrading epoxy cured material by aminolysis according to claim 12, wherein: The epoxy cured product is degraded to form a phenoxy resin as shown in formula (III): Wherein, Y is a single bond, the structure represented by formula (8), formula (9), formula (10), formula (11), formula (12), formula (13), formula (14), formula (15), formula (16), formula (17), formula (18), or a structure represented by formula (19):