Solid catalyst component for olefin polymerization, and preparation method therefor and use thereof
Patent Information
- Application Number
- MYPI2025002609
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-10-26
- Filing Date
- 2023-10-25
- Publication Date
- 2024-04-26
AI Technical Summary
The polymerization activity of existing Ziegler-Natta type prepolymerized catalysts decays rapidly after extended storage time, resulting in high fine powder content in olefin polymerization products, affecting device stability and industrial application.
Provides a solid catalyst component containing magnesium element, titanium element, halogen and poly-α-olefin. The characteristic peak of the Ti2p spectrum is determined through the Gauss-Lorentz split peak fitting method of XPS analysis, combining alkyl aluminum and external electron donation. A catalyst with stable polymerization activity is prepared using a specific preparation method.
It prolongs the decay time of the catalyst's polymerization activity and reduces the fine powder content in the polymer. It is suitable for olefin polymerization units with or without prepolymerization operation units and meets the stability requirements of industrial applications.
Smart Images

Figure PI2025002609_DRAWING_001 
Figure PI2025002609_DRAWING_002
Abstract
Description
Solid catalyst component for olefin polymerization and preparation method and use thereof
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of Chinese patent applications 202211320920.2, 202211321506.3, 202211321006.X, 202211321023.3, and 202211321504.4 filed on October 26, 2022, the contents of which are incorporated herein by reference. Technical Field
[0003] The present invention relates to the field of catalysts for olefin polymerization, and in particular to a solid catalyst component for olefin polymerization, a preparation method thereof and an application thereof. Background Art
[0004] Ziegler-Natta spherical catalysts are widely used in loop polypropylene processes for the production of propylene homopolymer, propylene / ethylene (or butene) random copolymers, and impact copolymers. They feature high polymerization activity, high stereospecificity, and high polymer particle regularity. Spherical catalysts are also used in gas-phase polypropylene and polyethylene processes with prepolymerization units, such as the SHPERIZONE and SHPERILENE processes, for the production of these two processes. Despite these processes incorporating prepolymerization units, catalyst and polymer particle fragmentation can occur during resin production, leading to a certain amount of fines in the polymer. This is particularly true in the production of high-melt flow index (MFR) propylene homopolymers, where high fines content can affect plant stability and long-term operation. Polypropylene plants without prepolymerization units, such as the UNIPOL process, are not suitable for the use of Ziegler-Natta spherical catalysts because the catalyst or polymer particles often break apart during polymerization, generating large amounts of fines.
[0005] US9453088B2 discloses a prepolymerization catalyst for olefin polymerization. The prepolymerization catalyst comprises a catalyst component containing two electron donors, a 1,3-diether and an aromatic ester, and an average particle size of less than 30 μm, a prepolymerization multiple of less than 50 g polymer / g catalyst, and a preparation method comprising first preparing a spherical catalyst containing the two electron donors, the 1,3-diether and the aromatic ester, and then prepolymerizing the catalyst with an olefin having 2 to 10 carbon atoms. CN1421468A discloses a method for the polymerization or copolymerization of propylene, comprising prepolymerizing a Ziegler-Natta catalyst with ethylene or an α-olefin at a temperature between -10°C and 80°C, with the prepolymerization multiple controlled at 6 to 50,000, followed by polymerization of the propylene. US7329714B2 discloses a method for the production of prepolymerized polypropylene, comprising prepolymerizing a Ziegler-Zatta catalyst with propylene or 4-methyl-1-pentene at a temperature between 0 and 40°C, followed by polymerization of the propylene.
[0006] However, in the aforementioned methods for preparing prepolymerized catalysts, catalyst fragmentation is unavoidable when ethylene is used as the prepolymerized monomer, and the content of polymer fines is also high during olefin polymerization. Prepolymerized catalysts prepared using propylene or other α-olefins experience rapid decline in activity over extended storage time, resulting in lower commercial value. Regardless of whether the catalysts are prepared by ethylene or propylene prepolymerization, the polymerization activity declines with extended storage time, resulting in "instability" in the polymerization activity, which cannot meet the requirements of industrial applications.
[0007] Summary of the Invention
[0008] In view of this, the purpose of the present invention is to address the problem that the polymerization activity of existing Ziegler-Zatta type prepolymerization catalysts decays rapidly due to prolonged storage time, and to provide a solid catalyst component for olefin polymerization, a preparation method and use thereof.
[0009] First, the present invention provides a solid catalyst component for olefin polymerization, wherein the solid catalyst component comprises magnesium, titanium, halogen, poly-α-olefin and internal electron donor, wherein the Ti2p spectrum obtained by XPS analysis of the solid catalyst component is peak-split by Gauss-Lorentz peak fitting, and the peak-split results show that Ti2p 3 / 2 The spectrum peak of the orbital has at least three characteristic peaks at the electron binding energy of 459.9eV-454.9eV;
[0010] The Gaussian-Lorentz peak fitting method is as follows: set the ratio of Lorentz to Gaussian to 30%, Ti2p 1 / 2 The electron binding energy of the spectral peak of the orbital is related to the Ti2p 3 / 2The electron binding energy difference of the spectral peak of the orbital is 5.9eV, and the Ti2p 1 / 2 The half-maximum width of the spectrum peak of the orbital is Ti2p 3 / 2 1.7 times the half-maximum width of the spectrum peak of the orbital, Ti2p 1 / 2 The peak height of the orbital spectrum is Ti2p 3 / 2 The peak height of the spectrum of the orbital is 0.28 times, and Ti2p 3 / 2 The characteristic peaks of the spectrum of the orbital have the same half-maximum width.
[0011] Second, the present invention provides a method for preparing a solid catalyst component for olefin polymerization, the method comprising:
[0012] (1) in the presence of an inert solvent, a catalyst component A, an alkyl aluminum, and an external electron donor compound are contacted to react; the catalyst component A contains titanium, magnesium, a halogen, and an internal electron donor;
[0013] (2) mixing the reaction system obtained in step (1) with α-olefin to carry out polymerization reaction;
[0014] (3) removing the unreacted α-olefin in step (2), and adding hydrogen to the resulting reaction system to carry out the reaction.
[0015] Third, the present invention provides a solid catalyst component prepared by the method described above.
[0016] Fourthly, the present invention provides a catalyst system for olefin polymerization, which comprises the solid catalyst component described above and / or the solid catalyst component prepared by the method described above, an alkyl aluminum and an optional external electron donor compound or its reaction product.
[0017] Fifth, the present invention provides use of the solid catalyst component described above and / or the solid catalyst component prepared by the method described above and / or the catalyst system described above in olefin polymerization.
[0018] Sixth, the present invention provides a method for olefin polymerization, which comprises: polymerizing olefins in the presence of the solid catalyst component described above and / or the solid catalyst component prepared by the method described above and / or the catalyst system described above.
[0019] The present invention has the following advantages: the solid catalyst component provided by the present invention is a Ziegler-Zatta type prepolymerization catalyst, has the advantages that the polymerization activity decays slowly with the extension of storage time, and the solid catalyst component is used to polymerize the polymer with low fine powder content. The solid catalyst component is not only suitable for olefin polymerization devices with a prepolymerization operation unit, but also suitable for polyolefin devices without a prepolymerization operation unit. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] FIG1 is an XRD pattern of catalyst E1 of Example 1 (above) and catalyst CE1 of Comparative Example 1 (below);
[0021] FIG2 is an XPS peak fitting diagram of catalyst E1 of Example 1 (upper) and catalyst CE1 of Comparative Example 1 (lower). DETAILED DESCRIPTION
[0022] The present invention will be further described below with reference to specific examples, but they do not constitute any limitation to the present invention.
[0023] According to a first aspect of the present invention, the present invention provides a solid catalyst component for olefin polymerization, the solid catalyst component comprising magnesium, titanium, halogen, poly-α-olefin and an internal electron donor, wherein the Ti2p spectrum obtained by XPS analysis of the solid catalyst component is peak-split using a Gaussian-Lorentz peak-split fitting method, and the peak-split results show that Ti2p 3 / 2 The spectrum peak of the orbital has at least three characteristic peaks at the electron binding energy of 459.9eV-454.9eV;
[0024] The Gaussian-Lorentz peak fitting method is as follows: set the ratio of Lorentz to Gaussian to 30%, Ti2p 1 / 2 The electron binding energy of the spectral peak of the orbital is related to the Ti2p 3 / 2 The electron binding energy difference of the spectral peak of the orbital is 5.9eV, and the Ti2p 1 / 2 The half-maximum width of the spectrum peak of the orbital is Ti2p 3 / 2 1.7 times the half-maximum width of the spectrum peak of the orbital, Ti2p 1 / 2 The peak height of the orbital spectrum is Ti2p 3 / 2 The peak height of the spectrum of the orbital is 0.28 times, and Ti2p 3 / 2 The characteristic peaks of the spectrum of the orbital have the same half-maximum width.
[0025] As is well known in the art, the Ti2p spectrum obtained by XPS analysis of the solid catalyst component is subjected to peak separation using a Gaussian-Lorentz peak fitting method. 1 / 2 orbital peaks and Ti2p 3 / 2 The characteristic peaks in the spectrum of orbitals appear in pairs; among them, Ti2p 1 / 2 The electron binding energy of the spectral peak of the orbital is related to the Ti2p 3 / 2 The difference in electron binding energy of the peaks of the orbitals is called "Ti2p 1 / 2 The peak of the orbital is related to Ti2p 3 / 2 The difference in electron binding energy between the characteristic peaks that appear in pairs in the spectrum peak of the orbital. Similarly, Ti2p 1 / 2 The half-maximum width of the spectrum peak of the orbital is related to the Ti2p3 / 2 The half-width ratio of the spectrum peak of the orbital is referred to as "Ti2p 1 / 2 The peak of the orbital is related to Ti2p 3 / 2 The ratio of the half-width between the characteristic peaks that appear in pairs in the spectrum of the orbital"; Ti2p 1 / 2 The peak height of the orbital spectrum is Ti2p 3 / 2 The ratio of the peak heights of the orbital peaks is referred to as "Ti2p 1 / 2 The peak of the orbital is related to Ti2p 3 / 2 For example, according to the electron binding energy from high to low, the XPS spectrum of the solid catalyst component has the following characteristics: 3 / 2 The characteristic peaks of the spectrum of the orbital are named first characteristic peak, second characteristic peak, third characteristic peak, etc.; according to the electron binding energy from high to low, Ti2p 1 / 2 The characteristic peaks of the spectrum of the orbital are named as the first characteristic peak, the second characteristic peak, the third characteristic peak, etc. 1 / 2 The electron binding energy of the spectral peak of the orbital is related to the Ti2p 3 / 2 The difference in electron binding energy between the peaks of the orbital spectrum means that "the difference in electron binding energy between the first characteristic peak and the first characteristic peak, the difference in electron binding energy between the second characteristic peak and the second characteristic peak, and the difference in electron binding energy between the third characteristic peak and the third characteristic peak are all 5.9 eV." Similarly, Ti2p 1 / 2 The half-maximum width of the spectrum peak of the orbital is related to the Ti2p 3 / 2 The ratio of the half-maximum width of the spectrum peak of the orbital, Ti2p 1 / 2 The peak height of the orbital spectrum is Ti2p 3 / 2 The same is true for the ratio of the peak heights of the orbital spectral peaks.
[0026] According to the solid catalyst component provided by the present invention, the electron binding energies of Ti2p of titanium and C1s of carbon are measured using an X-ray photoelectron spectrometer (XPS). XPS uses a monochromatic Al Kα ray source and an electron neutralization gun for charge neutralization until the sample surface charge is completely neutralized. High-resolution spectra are obtained under conditions of a pass energy of 20 eV, a step size of 0.05 eV, and an analysis area of 500 μm. 2 .
[0027] XPS test sample preparation method: Use an infrared tablet press to press the sample onto a non-conductive double-sided tape in a glove box, transfer the pressed sample to an air-sensitive sample protection table for sealed storage, and then quickly transfer the sensitive sample protection table to the XPS sample preparation room for vacuuming. Wait until the pressure in the preparation room drops to 10 -6 After the pressure in the preparation room drops below 10 mbar, open the sealing cover of the sensitive sample protection table and wait for the pressure in the preparation room to drop to 10 -6After the temperature drops below 100 mbar, the sample is transferred to the analysis room for XPS testing. The charge of the prepolymerized catalyst (ie, the solid catalyst component as described above) is calibrated based on the C1s peak top binding energy value of 284.80 eV of the polypropylene or polyethylene contained in the catalyst.
[0028] In some preferred embodiments, the Ti2p 3 / 2 The electron binding energy has 3-5 characteristic peaks in the range of 459.9eV-454.9eV, for example, three characteristic peaks, four characteristic peaks, five characteristic peaks, etc. in the range of 459.9eV-454.9eV. According to the electron binding energy from high to low, the XPS spectrum of Ti2p 3 / 2 The characteristic peaks of the orbitals are named first characteristic peak, second characteristic peak, third characteristic peak, fourth characteristic peak, fifth characteristic peak, etc. In a particularly preferred embodiment, the XPS spectrum of the solid catalyst component contains Ti2p 3 / 2 The electron binding energy has three characteristic peaks in the range of 459.9eV-454.9eV.
[0029] In some preferred embodiments, the Ti2p 3 / 2 The spectrum peak of the orbital has three characteristic peaks at an electron binding energy of 459.9eV-454.9eV. The three characteristic peaks are named the first characteristic peak, the second characteristic peak, and the third characteristic peak, respectively, according to the electron binding energy from high to low. The electron binding energy of the first characteristic peak is 459.9eV-458.97eV, the electron binding energy of the second characteristic peak is 458eV-457.45eV, and the electron binding energy of the third characteristic peak is 456.2eV-454.9eV. The naming of the three characteristic peaks does not limit the technical solution of the present invention, but is only for distinguishing different characteristic peaks to facilitate better description.
[0030] In some embodiments, the Ti2p of the solid catalyst component 1 / 2 The electron binding energy of the spectrum peak of the orbital is 467eV-460eV. The Ti2p spectrum obtained by XPS analysis of the solid catalyst component is subjected to peak separation by Gauss-Lorentz peak fitting. 1 / 2 The peak of the orbital is related to Ti2p 3 / 2 The spectral peaks of the orbitals have the same number of characteristic peaks.
[0031] In some embodiments, the titanium element has a Ti2p value of 455.40 eV to 455.85 eV. 3 / 2Electron binding energy, for example, Ti2p of 455.42eV, 455.44eV, 455.45eV, 455.46eV, 455.47eV, 455.50eV, 455.54eV, 455.62eV, 455.63eV, 455.64eV, 455.65eV, 455.66eV, 455.67eV, 455.68eV, 455.69eV, 455.70eV, 455.71eV, 455.72eV, 455.79eV, 455.80eV, 455.81eV, 455.82eV, or 455.83eV 3 / 2 Electron binding energy.
[0032] In some embodiments, in addition to Ti2p having a wavelength of 456.20 eV-454.90 eV, preferably 455.40 eV-455.85 eV, 3 / 2 In addition to the electron binding energy, titanium also has a Ti2p energy of 458.97eV-459.25eV and / or 457.45eV-458.00eV. 3 / 2 Electron binding energy. For example, titanium has a Ti2p energy of 459.09eV-459.19eV and / or 457.60-457.75eV. 3 / 2 Electron binding energy, for example, titanium has a Ti2p binding energy of 459.05eV-459.15eV and / or 457.45eV-457.55eV. 3 / 2 Electron binding energy, for example, titanium has a Ti2p energy of 458.97eV-459.25eV and / or 457.53-458.00eV. 3 / 2 Electron binding energy.
[0033] In some preferred embodiments, the peak area of the third characteristic peak accounts for 5-20%, preferably 5-15%, of the total peak area of the first, second, and third characteristic peaks (e.g., 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, and any range consisting of any two of the foregoing). The peak areas of the first, second, and third characteristic peaks are denoted as S1, S2, and S3, respectively.
[0034] In some preferred embodiments, the solid catalyst component does not contain detectable amounts of Group IVB elements other than Ti. For example, the solid catalyst component does not contain detectable amounts of Zr and / or Hf.
[0035] According to the solid catalyst component provided by the present invention, wherein the poly α-olefin is selected from poly C2-C 10The olefin is preferably one or more of polyethylene, polypropylene, polybutene, polyoctene and polyisoprene, more preferably polypropylene.
[0036] According to the solid catalyst component provided by the present invention, the internal electron donor includes at least one of a glycol ester compound, a 1,3-diether compound and a carboxylic acid ester.
[0037] In some preferred embodiments, the diol ester compound has a chemical structure shown in formula (1):
[0038] In formula (1), R1-R6 are the same or different and are independently selected from hydrogen, amino, C1-C 10 Straight chain alkyl, C3-C 10 Branched alkyl, C3-C 10 Cycloalkyl, C6-C 10 Aryl, C7-C 10 Alkaryl and C7-C 10 Aralkyl; two or more groups in R1-R6 are optionally bonded to each other to form one or more condensed ring structures; R7 and R8 are the same or different and are independently selected from C1-C 10 Straight chain alkyl, C3-C 10 Branched alkyl, C3-C 20 Cycloalkyl, C6-C 20 Aryl, C7-C 20 Alkaryl and C7-C 20 of aralkyl.
[0039] According to the solid catalyst component provided by the present invention, wherein, in formula (1), R1-R6 are the same or different and are independently selected from hydrogen, amino, C1-C6 straight-chain alkyl, C3-C8 branched-chain alkyl, C3-C 10 Cycloalkyl, C6-C 10 Aryl, C7-C 10 Alkaryl and C7-C 10 Preferably, two or more groups in R1-R6 are optionally bonded to each other to form one or more fused ring structures.
[0040] According to the solid catalyst component provided by the present invention, wherein, in formula (1), R7 and R8 are the same or different, and are independently selected from C1-C6 straight chain alkyl, C3-C 10 Branched alkyl, C3-C 10 Cycloalkyl, C6-C 10 Aryl, C7-C 10 Alkaryl and C7-C 10 of aralkyl.
[0041] According to the solid catalyst component provided by the present invention, wherein the diol ester compound is selected from 1,3-propylene glycol dibenzoate, 2-methyl-1,3-propylene glycol dibenzoate, 2-ethyl-1,3-propylene glycol dibenzoate, 2,2-dimethyl-1,3-propylene glycol dibenzoate, 1,3-diphenyl-1,3-propylene glycol dibenzoate, 1,3-diphenyl-1,3-propylene glycol dipropionate, 1,3-Diphenyl-2-methyl-1,3-propanediol dipropionate, 1,3-diphenyl-2-methyl-1,3-propanediol diacetate, 1,3-diphenyl-2,2-dimethyl-1,3-propanediol dibenzoate, 1,3-diphenyl-2,2-dimethyl-1,3-propanediol dipropionate, 1,3-di-tert-butyl-2-ethyl-1,3-propanediol dibenzoate, 1,3-diphenyl-1,3-propanediol diacetate, 1,3-diisopropyl-1,3-propanol di(4-butylbenzoate), 1-phenyl-2-amino-1,3-propanediol dibenzoate, 1-phenyl-2- Methyl-1,3-butanediol dibenzoate, 2,4-pentanediol dibenzoate, 3-butyl-2,4-pentanediol dibenzoate, 3,3-dimethyl-2,4-pentanediol dibenzoate, 2,4-pentanediol di(p-methylbenzoate), 2,4-pentanediol di(p-tert-butylbenzoate), 2,4-pentanediol di(p-butylbenzoate), 2-methyl-1,3-pentanediol di(p-methylbenzoate), 2-butyl-1,3-pentanediol di(p-methylbenzoate), 2-methyl-1,3-pentanediol di(p-tert-butylbenzoate), 2-methyl-1,3-pentanediol pivalate, 2 ,2-dimethyl-1,3-pentanediol dibenzoate, 2-ethyl-1,3-pentanediol dibenzoate, 2-butyl-1,3-pentanediol dibenzoate, 2-methyl-1,3-pentanediol dibenzoate, 2-ethyl-1,3-pentanediol dibenzoate, 2-propyl-1,3-pentanediol dibenzoate, 2-butyl-1,3-pentanediol dibenzoate, 3-ethyl-3,5-heptanediol dibenzoate, 4-ethyl-3,5-heptanediol dibenzoate, 3-propyl-3,5-heptanediol dibenzoate, 4-propyl-3,5-heptanediol dibenzoate, 3-butyl-3,5-heptanediol dibenzoate dibenzoate, 2,3-dimethyl-3,5-heptanediol dibenzoate, 2,4-dimethyl-3,5-heptanediol dibenzoate, 2,5-dimethyl-3,5-heptanediol dibenzoate, 4,4-dimethyl-3,5-heptanediol dibenzoate, 4,5-dimethyl-3,5-heptanediol dibenzoate, 4,6-dimethyl-3,5-heptanediol dibenzoate, 6,6-dimethyl-3,5-heptanediol dibenzoate, 2-methyl-3-ethyl-3,5-heptanediol dibenzoate, 2-methyl-4-ethyl-3,5-heptanediol dibenzoate, 2-methyl-5-ethyl-3,At least one of 5-heptanediol dibenzoate, 3-methyl-4-ethyl-3,5-heptanediol dibenzoate, 3-methyl-5-ethyl-3,5-heptanediol dibenzoate, 4-methyl-3-ethyl-3,5-heptanediol dibenzoate and 4-methyl-4-ethyl-3,5-heptanediol dibenzoate.
[0042] In some preferred embodiments, the 1,3-diether compound has a chemical structure shown in formula (2):
[0043] In formula (2), R1 and R2 are the same or different and are independently selected from hydrogen, C1-C 20 Straight chain alkyl, C3-C 10 Branched alkyl, C3-C 20 Cycloalkyl, C6-C 20 Aryl, C7-C 20 Arylalkyl and C7-C 20 R3 and R4 are the same or different and are independently selected from C1-C 10 of alkyl.
[0044] According to the solid catalyst component provided by the present invention, wherein, in formula (2), R1 and R2 are the same or different and are independently selected from hydrogen, C1-C 10 Straight chain alkyl, C3-C 10 Branched alkyl, C3-C 10 Cycloalkyl, C6-C 10 Aryl, C7-C 20 Arylalkyl and C7-C 10 and / or R3 and R4 are each independently selected from a C1-C6 alkyl group.
[0045] According to the solid catalyst component provided by the present invention, the 1,3-diether compound is selected from 2-(2-ethylhexyl)-1,3-dimethoxypropane, 2-isopropyl-1,3-dimethoxypropane, 2-butyl-1,3-dimethoxypropane, 2-sec-butyl-1,3- Dimethoxypropane, 2-cyclohexyl-1,3-dimethoxypropane, 2-phenyl-1,3-dimethoxypropane, 2-(2-phenylethyl)-1,3-dimethoxypropane, 2-(2-cyclohexylethyl)-1,3-dimethoxypropane, 2-(p-chlorophenyl)-1,3-dimethoxypropane, 2-(diphenylmethyl)-1,3-dimethoxypropane, 2,2-dicyclohexyl-1,3-dimethoxypropane, 2,2-dicyclopentyl-1,3-dimethoxypropane, 2,2-diethyl-1,3-dimethoxypropane, 2,2-dipropyl-1,3-dimethoxypropane, 2 ,2-diisopropyl-1,3-dimethoxypropane, 2,2-dibutyl-1,3-dimethoxypropane, 2-methyl-2-propyl-1,3-dimethoxypropane, 2-methyl-2-benzyl-1,3-dimethoxypropane, 2-methyl-2-ethyl-1,3-dimethoxypropane, 2-methyl-2-isopropyl-1,3-dimethoxypropane, 2-methyl-2-phenyl-1,3-dimethoxypropane, 2-methyl-2-cyclohexyl-1,3-dimethoxypropane, 2,2-bis(2-cyclohexylethyl)-1,3-dimethoxypropane, 2-methyl-2-isobutyl-1,3- Dimethoxypropane, 2-methyl-2-(2-ethylhexyl)-1,3-dimethoxypropane, 2,2-diisobutyl-1,3-dimethoxypropane, 2,2-diphenyl-1,3-dimethoxypropane, 2,2-dibenzyl-1,3-dimethoxypropane, 2,2-bis(cyclohexylmethyl)-1,3-dimethoxypropane, 2-isobutyl-2-isopropyl-1,3-dimethoxypropane, 2-(1-methylbutyl)-2-isopropyl-1,3-dimethoxypropane, 2-isopropyl-2-isopentyl-1,3-dimethoxypropane, 2-phenyl-2-isopropyl-1,3-dimethoxypropane At least one of 2-phenyl-2-sec-butyl-1,3-dimethoxypropane, 2-benzyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclopentyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclopentyl-2-sec-butyl-1,3-dimethoxypropane, 2-cyclohexyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclohexyl-2-sec-butyl-1,3-dimethoxypropane, 2-isopropyl-2-sec-butyl-1,3-dimethoxypropane, 2-cyclohexyl-2-cyclohexylmethyl-1,3-dimethoxypropane and 9,9-dimethoxymethylfluorene.
[0046] According to the solid catalyst component provided by the present invention, in formula (1) and formula (2), the hydrogen on the benzene ring in the aryl, alkylaryl and / or aralkyl group may be optionally substituted by a halogen atom.
[0047] According to the solid catalyst component provided by the present invention, wherein, the carboxylate is aliphatic carboxylate and / or aromatic carboxylate. In some embodiments, the carboxylate is selected from at least one of monobasic aliphatic carboxylate, dibasic aliphatic carboxylate, monobasic aromatic carboxylate and dibasic aromatic carboxylate. Wherein, aliphatic carboxylate refers to the carboxylate prepared by monobasic (or dibasic) aliphatic carboxylic acid and aliphatic monohydric alcohol or aromatic monohydric alcohol, and aromatic carboxylate refers to the carboxylate prepared by monobasic (or dibasic) aromatic carboxylic acid and aliphatic monohydric alcohol or aromatic monohydric alcohol. Preferably, the carboxylate is selected from one or more of benzoic acid ester compounds, phthalic acid ester compounds and succinate compounds.
[0048] In the present invention, the benzoate compound can be selected from one or more of methyl benzoate, ethyl benzoate and n-butyl benzoate.
[0049] For example, the phthalate compound can be selected from one or more of diethyl phthalate, diisobutyl phthalate, di-n-butyl phthalate, diisooctyl phthalate and di-n-octyl phthalate.
[0050] For example, the succinate compound can be selected from one or more of diethyl 2,3-diisopropylsuccinate, diisobutyl 2,3-diisopropylsuccinate, di-n-butyl 2,3-diisopropylsuccinate, dimethyl 2,3-diisopropylsuccinate, diisobutyl 2,2-dimethylsuccinate, diisobutyl 2-ethyl-2-methylsuccinate and diethyl 2-ethyl-2-methylsuccinate.
[0051] According to the solid catalyst component provided by the present invention, the internal electron donor includes an internal electron donor a and an internal electron donor b, and the internal electron donor a and the internal electron donor b are:
[0052] Option I: The internal electron donor a is selected from the diol ester compound, and the internal electron donor b is selected from 1,3-diether compounds and optional carboxylic acid esters;
[0053] Option II: The internal electron donor a is selected from the 1,3-diether compound, and the internal electron donor b is selected from the phosphate compound shown in (3);
[0054] In formula (3), R5, R6 and R7 are the same or different and are independently selected from C1-C4 straight chain alkyl, C3-C4 branched chain alkyl, C3-C 20Cycloalkyl, C6-C 20 Aryl, C7-C 20 Alkaryl and C7-C 20 of aralkyl.
[0055] According to the solid catalyst component provided by the present invention, wherein, in formula (3), R5, R6 and R7 are the same or different and are independently selected from C1-C4 straight chain alkyl, C3-C4 branched chain alkyl, C3-C 10 Cycloalkyl, C6-C 10 Aryl, C7-C 10 Alkaryl and C7-C 10 of aralkyl.
[0056] According to the solid catalyst component provided by the present invention, the phosphate compound is selected from at least one of trimethyl phosphate, triethyl phosphate, tributyl phosphate, triphenyl phosphate, tricresyl phosphate, triisopropylphenyl phosphate, phenyl dimethyl phosphate, cresyl dibutyl phosphate, cumyl dimethyl phosphate, cumyl diethyl phosphate, cumyl dibutyl phosphate, phenyl ditolyl phosphate, phenyl diisopropylphenyl phosphate, p-cresyl dibutyl phosphate, m-cresyl dibutyl phosphate, p-cumyl dimethyl phosphate, p-cumyl diethyl phosphate, p-tert-butylphenyl dimethyl phosphate and o-cresyl p-di-tert-butylphenyl phosphate.
[0057] According to the solid catalyst component provided by the present invention, wherein the internal electron donor includes the internal electron donor a and the internal electron donor b, the mass ratio of the internal electron donor a to the internal electron donor b can be 0.1:1-1000:1. For example, the mass ratio of the internal electron donor a to the internal electron donor b can be 0.1:1, 0.2:1, 0.5:1, 0.8:1, 1:1, 2:1, 5:1, 10:1, 20:1, 30:1, 40:1, 50:1, 80:1, 100:1, 200:1, 500:1, 800:1, 1000:1, and ranges thereof.
[0058] According to the solid catalyst component provided by the present invention, the solid catalyst component is a spherical solid particle.
[0059] Preferably, the average particle size D of the solid catalyst component is 50 For example, the average particle size D of the solid catalyst component is 5-150 μm. 50 The average particle size D of the solid catalyst component may be 5 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 100 μm, 120 μm, 150 μm or a range consisting of the above. 50It can be 20-80μm.
[0060] In the present invention, the average particle size D 50 The particle size was measured using a Master Sizer 2000 laser particle size analyzer (manufactured by Malvern Instruments Ltd).
[0061] Preferably, the particle size distribution value (SPAN) of the solid catalyst component is 0.75-0.85.
[0062] In the present invention, the SPAN value is measured by using a Masters Sizer 2000 particle size analyzer from Malvern Instruments, UK, and n-hexane as the dispersion medium. The particle size distribution value Span = (D90-D10) / D50.
[0063] According to the solid catalyst component provided by the present invention, the content of the polyalphaolefin is 0.1-89 weight %, preferably 1-50 weight %, more preferably 9-35 weight %, the content of the titanium element is 0.1-3.5 weight %, preferably 0.5-2.5 weight %, more preferably 1.5-2.5 weight %, the content of the magnesium element is 1-18 weight %, preferably 11-17 weight %, the content of the halogen is 2-65 weight %, preferably 35-55 weight %, and the content of the internal electron donor is 0.6-15 weight %, preferably 1-10 weight %, more preferably 6-10 weight %.
[0064] In the present invention, the halogen is selected from one or more of fluorine, chlorine, bromine and iodine, preferably chlorine.
[0065] According to the solid catalyst component provided by the present invention, the magnesium element and / or halogen source can be a carrier, and the carrier is preferably an alkoxy magnesium carrier, a spherical magnesium chloride alcoholate carrier, or a spherical magnesium compound carrier. The type of the carrier is as described in the second aspect.
[0066] According to the solid catalyst component provided by the present invention, the titanium element and / or halogen source can be titanium halide (such as titanium tetrachloride), wherein the type of the titanium halide is as described in the second aspect.
[0067] According to the solid catalyst component provided by the present invention, the titanium content can be measured according to the colorimetric method. Specifically, 0.2-0.5g of the sample is dissolved in 50mL of 2N H2SO4, the upper floating matter is filtered, and the clear liquid is taken for colorimetry; a 2N H2SO4 solution is used as a blank, and the cuvette is 1cm thick. The absorbance E1 is measured at a wavelength of 410μm, and then one drop of 30% H2O2 is added, shaken, and the absorbance E2 is measured. The titanium content Ti (%) is calculated according to the following formula: Ti% = [(E2-E1)×100) / (K·L·W·100)]×100
[0068] Where: W is sample weight (g); L is cuvette thickness (cm); K is specific extinction coefficient; E1 is blank absorbance; E2 is sample absorbance.
[0069] The magnesium content can be measured according to the EDTA titration method. Specifically, take 0.2-0.5g of the sample into a 250mL conical flask, add 20-30mL of 2N H2SO4 solution to dissolve it, add 20mL of triethanolamine (1+2) standard solution, adjust the pH to 10 with 20% NaOH solution, shake, add 10mL of pH=10 buffer solution, add 6 drops of 30% H2O2 and 30-50mL of distilled water, add a small amount of chrome black T indicator, shake well, and titrate with 0.02N EDTA solution until the color changes from purple-red to blue (the purple light disappears) as the end point. The magnesium content Mg (%) is calculated according to the following formula: Mg (%) = [(VE·NE×24.31) / (G·1000)]×100
[0070] Where: G is the mass of the sample (g); VE is the amount of EDTA consumed (mL); NE is the equivalent number of EDTA solution; 24.31 is the atomic weight of magnesium.
[0071] Chloride content can be measured using silver nitrate titration. Specifically, weigh 0.04-0.1g of sample into a conical flask, add 20mL of 2N H2SO4 solution, and let it sit for 30 minutes. After rinsing with distilled water several times, add 20-30mL of 0.1N AgNO3 solution dropwise, add 3mL of 1:1 HNO3 solution, and titrate the excess AgNO3 solution with 0.1N NH4CNS standard solution until the brick-red color does not disappear for two seconds. Calculate the chlorine content (Cl) according to the following formula: Cl (%) = [(V1-V2×D)×N1×35.45 / G·1000)]×100
[0072] Where: V1—amount of AgNO3 solution (mL); V2—amount of NH4CNS solution consumed (mL); D—volume ratio of AgNO3 / NH4CNS solution; N1—equivalent concentration of AgNO3; G—mass of sample (g); 35.45—atomic weight of chlorine.
[0073] The test method for the polyα-olefin content in the solid catalyst component is as follows: a certain amount of sample (M1) is weighed and dissolved with ethanol and dilute hydrochloric acid, the insoluble matter is dried under vacuum at 80°C to obtain a solid (M2), 0.2g of the solid is pressed into a tablet, and the polyα-olefin content (C1) of the solid is measured using an infrared spectrometer. The mass percentage of the polyα-olefin in the solid catalyst component is calculated according to the following formula: C A =M2×C1 / M1
[0074] C A is the mass percentage of polyα-olefin in the solid catalyst component, M1 and M2 are the mass (g) of the sample and the dry solid, respectively, and C1 is the mass percentage of polyα-olefin in the dry solid.
[0075] The test method for the internal electron donor content in the solid catalyst component is: dissolve the sample with ethyl acetate and hydrochloric acid solution (concentration 2 mol / L), extract the internal electron donor, and analyze its content using a conventional liquid chromatograph.
[0076] The solid catalyst component provided by the present invention further comprises an aluminum alkyl and an external electron donor. The types and contents of the aluminum alkyl and external electron donor can be selected with reference to existing olefin prepolymerization catalysts. The polymerization process known in the art may result in a small amount of the aluminum alkyl and external electron donor remaining in the polyolefin, and the contents of the aluminum alkyl and external electron donor are generally the residual amounts in the polyolefin. The types of the aluminum alkyl and external electron donor are as described in the second aspect.
[0077] In addition, the solid catalyst component of the present invention may contain other components in addition to the above components, such as an inert solvent, such as the inert solvent added during the preparation of the solid catalyst component described in the second aspect.
[0078] According to a second aspect of the present invention, the present invention provides a method for preparing a solid catalyst component for olefin polymerization, the method comprising:
[0079] (1) in the presence of an inert solvent, a catalyst component A, an alkyl aluminum, and an external electron donor are contacted to react; the catalyst component A contains titanium, magnesium, a halogen, and an internal electron donor;
[0080] (2) mixing the reaction system obtained in step (1) with an α-olefin to carry out a polymerization reaction;
[0081] (3) removing the unreacted α-olefin in step (2), and adding hydrogen to the resulting reaction system to carry out the reaction.
[0082] In the present invention, catalyst component A represents a catalyst that has not been prepolymerized, and solid catalyst component represents a catalyst that has been prepolymerized.
[0083] According to the preparation method provided by the present invention, wherein, in step (1), the alkyl aluminum and the external electron donor compound can be selected with reference to existing olefin prepolymerization catalysts, and the present invention has no particular limitation on this. The number of alkyl groups in the alkyl aluminum can be 1-3, and the number of carbon atoms in the alkyl group can be C1-C8. Generally, the alkyl aluminum can be selected from one or more of triethyl aluminum, triisobutyl aluminum, tri-n-butyl aluminum, tri-n-hexyl aluminum and diethyl aluminum monochloride. The external electron donor compound can be selected from at least one of silicon-containing compounds, and the external electron donor compound can be selected from one or more of cyclohexylmethyldimethoxysilane, diisopropyldimethoxysilane, n-butyldimethoxysilane, diisobutyldimethoxysilane, diphenyldimethoxysilane, methyl-tert-butyldimethoxysilane and dicyclopentyldimethoxysilane.
[0084] Generally, the molar ratio of the aluminum alkyl, the external electron donor compound, and the amount of the catalyst component A calculated as titanium element can be 1-50:0.2-10:1. For example, the molar ratio of the aluminum alkyl, the external electron donor compound, and the amount of the catalyst component A calculated as titanium element can be 1:0.2:1, 5:0.2:1, 10:0.2:1, 15:0.2:1, 20:0.2:1, 30:0.2:1, 40:0.2:1, 50:0.2:1, 15:0.3:1, 15:0.5:1, 15:1:1, 15:2:1, 15:3:1, 15:4:1, 15:5:1, 15:20:1, or any range consisting of the above ratios of the aluminum alkyl and the external electron donor compound.
[0085] According to the preparation method provided by the present invention, in step (1), relative to 25g of catalyst component A, the amount of the alkyl aluminum is 1-30mmol, preferably 15-20mmol; the amount of the external electron donor compound is 0.01-10mmol, preferably 0.1-1mmol.
[0086] According to the preparation method provided by the present invention, the internal electron donor comprises at least one of a glycol ester compound, a 1,3-diether compound, and a carboxylic acid ester. The internal electron donor is as described in the first aspect and will not be described in detail here.
[0087] According to the preparation method provided by the present invention, wherein, in step (1), the inert solvent can be selected with reference to the prior art. Generally, the inert solvent can be selected from one or more of hexane, heptane and decane. The amount of the inert solvent added is such that the mass concentration of the catalyst component A in the inert solvent can be 5-50 g / L.
[0088] According to the preparation method provided by the present invention, wherein, in step (1), the reaction conditions include: the temperature can be 0-30°C, preferably 15-25°C; the time can be 1-30 min, preferably 10-20 min.
[0089] According to the preparation method provided by the present invention, wherein, in step (2), the conditions of the polymerization reaction include: the temperature can be 0-50°C, preferably 15-25°C; the time can be 5-30 minutes, preferably 10-20 minutes.
[0090] According to the preparation method provided by the present invention, wherein, in step (3), the reaction conditions include: the temperature can be 0-50°C, preferably 15-25°C; the time can be 5-30 min, preferably 10-20 min.
[0091] According to the preparation method provided by the present invention, the method for removing the unreacted α-olefin in step (2) can be a conventional method in the art, such as first venting the unreacted α-olefin and then replacing the remaining α-olefin with an inert gas. That is, step (3) includes: first venting the unreacted α-olefin in step (2), then replacing the remaining α-olefin with an inert gas, and then adding hydrogen to the resulting reaction system to carry out the reaction.
[0092] In the present invention, unless otherwise specified, before carrying out the prepolymerization reaction in the second aspect or the olefin polymerization reaction in the sixth aspect, the reactor is first purged with an inert gas to place the reactor in an inert atmosphere, and then the raw materials are added to the reactor. This is well known in the art.
[0093] In the present invention, the inert gas may be at least one of nitrogen, neon, argon, and krypton. The number of times the inert gas is replaced is not particularly limited and may be selected conventionally in the art, for example, 1 to 5 times.
[0094] According to the preparation method provided by the present invention, the amount of hydrogen added is controlled to maintain the reaction pressure at 0.01-1 MPa, preferably 0.1-0.5 MPa, more preferably 0.2-0.3 MPa. In the present invention, unless otherwise specified, pressure is generally gauge pressure.
[0095] According to the preparation method provided by the present invention, hydrogen can be added in the form of pure hydrogen or a hydrogen-containing gas mixture. The hydrogen-containing gas mixture can be composed of hydrogen and an inert gas, and the inert gas can be selected from at least one of nitrogen, helium, neon and argon. The present invention has no special requirements for the concentration of hydrogen in the hydrogen-containing gas mixture, as long as the defined reaction pressure can be achieved. Typically, the concentration of hydrogen in the hydrogen-containing gas mixture can be 0.1-100% by volume, for example, 20-100% by volume.
[0096] According to the preparation method provided by the present invention, step (3) further includes a post-processing step: performing solid-liquid separation and drying treatment on the system obtained in step (3) to obtain the solid catalyst component. The post-processing step generally includes: removing unreacted hydrogen, filtering to remove liquid or optionally washing with hexane 1-2 times to obtain a solid product; then drying the solid product under vacuum at 10-80°C to obtain the solid catalyst component. In the present invention, the vacuum drying can be carried out by a conventional vacuum pump, and the present invention has no special requirements for it.
[0097] According to the preparation method provided by the present invention, wherein the α-olefin is selected from C2-C 10 The olefin is preferably selected from one or more of ethylene, propylene, butene, octene and isopentene, and more preferably the α-olefin is propylene.
[0098] According to the preparation method provided by the present invention, the mass ratio of the α-olefin to the catalyst component A can be 0.04-10:1. For example, the mass ratio of the α-olefin to the catalyst component A can be 0.04:1, 0.05:1, 0.08:1, 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, or a range thereof.
[0099] According to the preparation method provided by the present invention, the catalyst component A can be prepared according to the conventional method of the main catalyst in the olefin polymerization catalyst in the art. The present invention is not particularly limited to this. For example, it can be prepared by referring to the methods disclosed in patent applications WO2012034357A1, WO2012097680A1 and patents ZL03153152.0, ZL200410062291.3, ZL201310491641.7, ZL201310491393.6 and ZL201310491648.9.
[0100] In the present invention, the catalyst component A may include or be the reaction product of titanium halide (such as titanium tetrachloride), a carrier and an internal electron donor. The carrier is preferably an alkoxy magnesium carrier, a magnesium chloride alcoholate spherical carrier or a spherical magnesium compound carrier.
[0101] In the present invention, the average particle size of the carrier is 5-150 μm, more preferably 20-80 μm, and even more preferably 30-60 μm.
[0102] In some embodiments, the catalyst component A can be prepared by referring to the methods disclosed in WO2012034357A1 and WO2012097680A1. More specifically, the support is an alkoxymagnesium support, and the catalyst component A is a reaction product of a titanium halide (e.g., titanium tetrachloride), an alkoxymagnesium support, and the internal electron donor in an inert solvent. The general formula of the alkoxymagnesium support is Mg(OEt) 2-k-l (OEH) k (OiPr) l , wherein Et is ethyl, EH is 2-ethylhexyl, iPr is isopropyl, and k and l are each independently 0-0.5.
[0103] The catalyst component A can be prepared by the following steps: reacting a magnesium alkoxide with a titanium halide (e.g., titanium tetrachloride) and an internal electron donor, such as a carboxylate, in the presence of an inert solvent. The reaction temperature is typically -40-200°C, preferably -20-150°C; and the reaction time is typically 1 minute to 20 hours, preferably 5 minutes to 8 hours. The solid obtained above is washed with an inert solvent, preferably toluene, to obtain a solid catalyst component. The washing period is typically 1-24 hours, preferably 6-10 hours.
[0104] The solid catalyst component may be stored in a dry state or in an inert solvent.
[0105] In other embodiments, the catalyst component A can be prepared by referring to the methods disclosed in patents ZL03153152.0 and ZL200410062291.3. More specifically, the support is a spherical magnesium chloride alcoholate support, and the catalyst component A is the reaction product of a titanium halide (e.g., titanium tetrachloride), a spherical magnesium chloride alcoholate, and the internal electron donor, e.g., a carboxylate.
[0106] The general formula of the spherical magnesium chloride alcoholate can be Mg(R'OH) i (H2O) j , wherein R′ is methyl, ethyl, n-propyl or isopropyl, i is 1.5-3.5, and j is 0-0.1.
[0107] The catalyst component A is prepared by a method comprising the following steps:
[0108] 1) reacting a titanium halide (e.g., titanium tetrachloride) with the magnesium chloride alcoholate spherical support at -20°C to 0°C for 20-120 minutes to obtain a mixture I;
[0109] 2) heating the mixture I to 100-120° C., adding the internal electron donor such as carboxylate during the heating process, and reacting at 100-120° C. for 20-200 minutes to obtain a solid product II;
[0110] 3) The solid product II is washed with titanium halide (such as titanium tetrachloride) and hexane respectively and then dried in vacuum.
[0111] In other embodiments, the catalyst component A can be prepared by referring to the methods disclosed in patents ZL201310491641.7, ZL201310491393.6, and ZL201310491648.9. More specifically, the support is a spherical magnesium compound support, and the catalyst component A is the reaction product of a titanium halide (e.g., titanium tetrachloride), a spherical magnesium compound support, and the internal electron donor, such as a carboxylic acid ester.
[0112] The spherical magnesium compound carrier is shown in formula (4):
[0113] In formula (4), R1 is C1-C 12 R2 and R3 are the same or different and are hydrogen or a C1-C5 straight chain or branched chain alkyl group, wherein the hydrogen on the alkyl group may be optionally substituted by a halogen atom; X is a halogen; m is 0.1-1.9; n is 0.1-1.9; m+n=2.
[0114] The catalyst component A is prepared by a method comprising the following steps:
[0115] 1) reacting a titanium halide (e.g., titanium tetrachloride) with the spherical magnesium compound support at -20°C to 0°C for 20-120 minutes to obtain a mixture I;
[0116] 2) heating the mixture I to 100-120° C., adding the internal electron donor such as carboxylate during the heating process, and reacting at 100-120° C. for 20-200 minutes to obtain a solid product II;
[0117] 3) The solid product II is washed with titanium halide (such as titanium tetrachloride) and hexane respectively and then dried in vacuum.
[0118] According to the preparation method provided by the present invention, the vacuum drying conditions in the above operation include: temperature of 40-50°C and time of 30-60 minutes. In the present invention, the vacuum drying can be carried out by a conventional vacuum pump, and the present invention has no special requirements for it.
[0119] According to a third aspect of the present invention, the present invention provides a solid catalyst component prepared by the method described in the second aspect of the present invention.
[0120] According to a fourth aspect of the present invention, the present invention provides a catalyst system for olefin polymerization, the catalyst system comprising the solid catalyst component of the present invention, an alkyl aluminum and an optional external electron donor compound or a reaction product thereof.
[0121] In the catalyst system provided by the present invention, the aluminum alkyl, external electron donor compound, and their respective contents can be selected according to existing techniques. In the present invention, the types of aluminum alkyl and external electron donor compound used in the catalyst system can be the same as or different from those used in the preparation of the solid catalyst component. For example, the types of aluminum alkyl and external electron donor compound described in the second aspect of the present invention can be used.
[0122] Generally, the alkylaluminum can be selected from one or more of triethylaluminum, triisobutylaluminum, tri-n-butylaluminum, tri-n-hexylaluminum and diethylaluminum monochloride.
[0123] The ratio of the molar amount of the aluminum alkyl calculated as aluminum element to the molar amount of the solid catalyst component calculated as titanium element can be 1 to 1000: 1. For example, the ratio of the molar amount of the aluminum alkyl calculated as aluminum element to the molar amount of the solid catalyst component calculated as titanium element can be 1:1, 2:1, 5:1, 10:1, 20:1, 50:1, 100:1, 200:1, 500:1, 1000:1, or a range thereof.
[0124] According to the catalyst system provided by the present invention, the content of the alkyl aluminum is 0.01-100 mmol, preferably 0.1-10 mmol, more preferably 1-5 mmol, per 15 mg of the solid catalyst component.
[0125] Generally, the external electron donor compound can be selected from at least one of cyclohexylmethyldimethoxysilane, diisopropyldimethoxysilane, di-n-butyldimethoxysilane, diisobutyldimethoxysilane, diphenyldimethoxysilane, methyl-tert-butyldimethoxysilane, dicyclopentyldimethoxysilane, cyclohexyltrimethoxysilane, tert-butyltrimethoxysilane and tert-hexyltrimethoxysilane.
[0126] The ratio of the molar amount of the aluminum alkyl calculated as aluminum element to the molar amount of the external electron donor compound calculated as silicon element is 2-1000:1. For example, the ratio of the molar amount of the aluminum alkyl calculated as aluminum element to the molar amount of the external electron donor compound calculated as silicon element can be 2:1, 5:1, 10:1, 20:1, 50:1, 100:1, 200:1, 500:1, 1000:1, or a range thereof.
[0127] Fifth, the present invention provides use of the solid catalyst component described above and / or the solid catalyst component prepared by the method described above and / or the catalyst system described above in olefin polymerization.
[0128] Sixth, the present invention provides a method for olefin polymerization, which comprises: polymerizing olefins in the presence of the solid catalyst component described above and / or the solid catalyst component prepared by the method described above and / or the catalyst system described above.
[0129] According to the method provided by the present invention, the general formula of the olefin is CH2=CHR, R is hydrogen, C1-C6 alkyl or C6-C 10 Preferably, the olefin is selected from one or more of ethylene, propylene, butene, pentene and hexene.
[0130] According to the method provided by the present invention, the polymerization reaction conditions can be conventionally selected in the art, for example, the reaction temperature is 0-150° C., preferably the reaction temperature is 60-90° C., and the reaction pressure is normal pressure or higher.
[0131] Seventh, the present invention provides a use of the solid catalyst component described above and / or the solid catalyst component prepared by the method described above in reducing olefin polymerization activity.
[0132] The advantages of the technical solution of the present invention will be described in detail below through specific embodiments.
[0133] In the following examples and comparative examples,
[0134] The isotactic index of a polymer (polypropylene) refers to the mass percentage of the polymer that is insoluble in boiling n-heptane under specified conditions. It is determined by the heptane extraction method (boiling heptane extraction for 6 hours), i.e., 2 g of a dried polymer sample is taken and placed in an extractor and extracted with boiling heptane for 6 hours. The residue is then dried to a constant weight, and the ratio of the mass (g) of the obtained polymer to 2 is the isotactic index.
[0135] The polymer melt index is measured according to the method of ASTM D1238-99.
[0136] The particle size distribution of the polymer was determined by sieving through a standard sieve and calculating the mass percentage of the fraction.
[0137] Determination methods of specific surface area, pore size, pore volume, etc.: The experiment used the AutoChem 2920 fully automatic chemisorption instrument produced by MICROMERITICS of the United States to test the carrier. The BET method was used to test the specific surface area, and the BJH method was used to test the pore volume.
[0138] The XRD spectrum test method is as follows: the carrier is tested using a Bruker AXS, D8 Advance X-ray diffractometer from Bruker, Switzerland. The test conditions of the instrument are: CuK α (λ=1.5406), tube voltage 40KV, tube current 40mA, slit system DS=SS=1°, receiving slit 0.3mm, monochromator is graphite monochromator, scintillation counter counting, scanning speed 2θ=3° / min, scanning range 2θ=5°-75°.
[0139] In the following embodiments, unless otherwise specified, the “vacuum” refers to the vacuum degree achieved by a conventional vacuum pump.
[0140] The following preparation example is used to illustrate the preparation method of catalyst component A.
[0141] In the following preparation examples, the structural formula of the spherical magnesium compound support is:
[0142] Preparation Example 1
[0143] To a 3L glass reaction bottle with stirring, add 1.2L titanium tetrachloride and cool to -20℃. Then, under stirring, add 100g of magnesium chloride alcoholate spherical carrier [Mg(C2H5OH) 2.6 ] (average particle size D50 = 45 μm), react at -20 ° C for 0.5 hour, then slowly heat up to 120 ° C, add 15 g of 2,4-pentanediol dibenzoate during the heating process, then react at 120 ° C for 0.5 hour, filter out the liquid, add 1 L of titanium tetrachloride, maintain at 120 ° C for 2 hours, filter out the liquid to obtain a solid product, wash the obtained solid product with hexane 5 times, and finally dry in vacuo at 45 ° C to obtain catalyst component A (average particle size D50 = 40 μm, SPAN value 0.79), recorded as A-1.
[0144] Preparation Example 2
[0145] To a 3L glass reaction bottle with stirring, add 1.2L titanium tetrachloride and cool to -20℃. Then, under stirring, add 100g of magnesium chloride alcoholate spherical carrier [Mg(C2H5OH) 2.6] (average particle size D50 = 45 μm), react at -20 ° C for 0.5 hour, then slowly heat up to 120 ° C, add 15 g of 2,4-pentanediol dibenzoate and 15 g of 2-isopropyl-2-isopentyl-1,3-dimethoxypropane during the heating process, then react at 120 ° C for 0.5 hour, filter out the liquid, add 1 L of titanium tetrachloride, maintain at 120 ° C for 1 hour, filter out the liquid to obtain a solid product, wash the obtained solid product with hexane 5 times, and finally dry in vacuo at 45 ° C to obtain catalyst component A (average particle size D50 = 41 μm, SPAN value 0.78), recorded as A-2.
[0146] Preparation Example 3
[0147] 100 g of diethoxymagnesium support (average particle size D50 = 47 μm), 500 ml of toluene, and 20.0 ml of 4-ethyl-3,5-heptanediol dibenzoate were prepared into a suspension. In a 3000 ml reactor that had been repeatedly purged with high-purity nitrogen, 100 ml of toluene and 900 ml of titanium tetrachloride were added. The temperature was raised to 80°C, and the prepared suspension was added to the reactor. After being kept at this temperature for 1 hour, the temperature was further raised to 115°C and kept at this temperature for 2 hours. The liquid was then filtered clean. A mixture of 1200 ml of toluene and 300 ml of titanium tetrachloride was then added, heated to 110°C, and stirred for 1 hour. This treatment was repeated three times, and the liquid was filtered off. The resulting solid was washed four times with 1500 ml of hexane, the liquid was filtered off, and the solid was dried to obtain a solid catalyst component (average particle size D50 = 42 μm, SPAN value 0.82), designated A-3.
[0148] Preparation Example 4
[0149] A suspension was prepared by mixing 100 g of a diethoxymagnesium support (average particle size D50 = 47 μm), 500 ml of toluene, 20.0 ml of 4-ethyl-3,5-heptanediol dibenzoate, and 20.0 ml of 2-isopropyl-2-isopentyl-1,3-dimethoxypropane. In a 3000 ml reactor that had been repeatedly purged with high-purity nitrogen, 100 ml of toluene and 900 ml of titanium tetrachloride were added. The reaction mixture was heated to 80°C and the suspension was added to the reactor. After maintaining the temperature for 1 hour, the temperature was raised to 115°C and maintained for 2 hours. The liquid was then filtered. Then, a mixture of 1200 ml of toluene and 300 ml of titanium tetrachloride was added, heated to 110° C., and stirred for 1 hour. This treatment was repeated three times, and the liquid was filtered off. The resulting solid was washed four times with 1500 ml of hexane, the liquid was filtered off, and the mixture was dried to obtain a solid catalyst component (average particle size D50 = 42 μm, SPAN value 0.82), which was recorded as A-4.
[0150] Preparation Example 5
[0151] To a stirred 3L glass reaction bottle, 1.2L of titanium tetrachloride was added and the temperature was lowered to -20°C. Then, 100g of a spherical magnesium compound carrier (average particle size D50 = 45μm) was added under stirring. The reaction was carried out at -20°C for 0.5 hour, and then the temperature was slowly raised to 120°C. During the heating process, 15g of 2,4-pentanediol dibenzoate was added. The reaction was then carried out at 120°C for 0.5 hour. The liquid was filtered off, and 1L of titanium tetrachloride was added. After maintaining the temperature at 120°C for 2 hours, the liquid was filtered off to obtain a solid product. The obtained solid product was washed 5 times with hexane and finally dried in vacuo to obtain catalyst component A (average particle size D50 = 40μm, SPAN value 0.76), which was recorded as A-5.
[0152] Preparation Example 6
[0153] To a stirred 3L glass reaction bottle, 1.2L of titanium tetrachloride was added and the temperature was lowered to -20°C. Then, 100g of a spherical magnesium compound carrier (average particle size D50 = 45μm) was added under stirring, and the reaction was carried out at -20°C for 0.5 hour. The temperature was then slowly raised to 120°C. During the heating process, 15g of 2,4-pentanediol dibenzoate and 15g of 2-isopropyl-2-isopentyl-1,3-dimethoxypropane were added. The reaction was then carried out at 120°C for 0.5 hour. The liquid was filtered off, and 1L of titanium tetrachloride was added. After maintaining at 120°C for 1 hour, the liquid was filtered off to obtain a solid product. The obtained solid product was washed 5 times with hexane and finally dried in vacuo at 45°C to obtain catalyst component A (average particle size D50 = 41μm, SPAN value 0.76), which was recorded as A-6.
[0154] Preparation Example 7
[0155] To a 3L glass reaction bottle with stirring, add 1.2L titanium tetrachloride and cool to -20℃. Then, under stirring, add 100g of magnesium chloride alcoholate spherical carrier [Mg(C2H5OH) 2.6 ] (average particle size D50 = 45 μm), react at -20 ° C for 0.5 hour, slowly heat up to 120 ° C, add 15 g 2-isopropyl-2-isopentyl-1,3-dimethoxypropane during the heating process, then react at 120 ° C for 0.5 hour, filter out the liquid, add 1 L titanium tetrachloride, maintain at 120 ° C for 2 hours, filter out the liquid to obtain a solid product, wash the obtained solid product with hexane 5 times, and finally dry in vacuo at 45 ° C to obtain catalyst component A (average particle size D50 = 40 μm, SPAN value 0.79), recorded as A-7.
[0156] Preparation Example 8
[0157] To a 3L glass reaction bottle with stirring, add 1.1L titanium tetrachloride and cool to -20℃. Then, under stirring, add 100g of magnesium chloride alcoholate spherical carrier [Mg(C2H5OH) 2.6 ] (average particle size D50 = 45 μm), react at -20 ° C for 0.5 hour, slowly heat up to 120 ° C, add 15 g 2-isopropyl-2-isopentyl-1,3-dimethoxypropane and 0.6 g tributyl phosphate during the heating process, then react at 120 ° C for 0.5 hour, filter out the liquid, add 1 L titanium tetrachloride, maintain at 120 ° C for 2 hours, filter out the liquid to obtain a solid product, wash the obtained solid product with hexane 5 times, and finally dry in vacuo at 45 ° C to obtain catalyst component A (average particle size D50 = 40 μm, SPAN value 0.79), recorded as A-8.
[0158] Preparation Example 9
[0159] A suspension of 100 g of diethoxymagnesium support (average particle size D50 = 47 μm) was prepared with 500 ml of toluene and 20.0 ml of 2-isopropyl-2-isopentyl-1,3-dimethoxypropane. In a 3000 ml reactor that had been repeatedly purged with high-purity nitrogen, 100 ml of toluene and 900 ml of titanium tetrachloride were added. The temperature was raised to 80°C, and the prepared suspension was added to the reactor. After maintaining the temperature for 1 hour, the temperature was further raised to 115°C and maintained for 2 hours. The liquid was then filtered. A mixture of 1200 ml of toluene and 300 ml of titanium tetrachloride was then added, heated to 110°C, and stirred for 1 hour. This process was repeated three times, and the liquid was filtered off. The resulting solid was washed four times with 1500 ml of hexane, filtered off, and dried to obtain a solid catalyst component (average particle size D50 = 42 μm, SPAN value 0.82), designated A-9.
[0160] Preparation Example 10
[0161] 100 g of diethoxymagnesium support (average particle size D50 = 47 μm), 500 ml of toluene, and 20.0 ml of 2-isopropyl-2-isopentyl-1,3-dimethoxypropane were prepared into a suspension. In a 3000 ml reactor that had been repeatedly purged with high-purity nitrogen, 100 ml of toluene and 900 ml of titanium tetrachloride were added. The temperature was raised to 80°C, and the prepared suspension was added to the reactor. After incubation for 1 hour, the temperature was further raised to 115°C and maintained for 2 hours. The liquid was then filtered. A mixture of 1200 ml of toluene and 300 ml of titanium tetrachloride was then added, heated to 110°C, and stirred for 1 hour. This process was repeated three times, and the liquid was filtered off. The resulting solid was washed four times with 1500 ml of hexane, filtered off, and dried to obtain a solid catalyst component (average particle size D50 = 42 μm, SPAN value 0.82), designated A-10.
[0162] Preparation Example 11
[0163] To a stirred 3L glass reaction bottle, 1.2L of titanium tetrachloride was added and the temperature was lowered to -20°C. Then, 100g of a spherical magnesium compound carrier (average particle size D50 = 45μm) was added under stirring. After reacting at -20°C for 0.5 hour, the temperature was slowly raised to 120°C. During the heating process, 15g of 2-isopropyl-2-isopentyl-1,3-dimethoxypropane was added. Then, the reaction was continued at 120°C for 0.5 hour. The liquid was filtered off, and 1L of titanium tetrachloride was added. After maintaining the temperature at 120°C for 2 hours, the liquid was filtered off to obtain a solid product. The obtained solid product was washed 5 times with hexane and finally dried in vacuo at 45°C to obtain catalyst component A (average particle size D50 = 40μm, SPAN value 0.76), which was recorded as A-11.
[0164] Preparation Example 12
[0165] To a stirred 3L glass reaction bottle, 1.1L of titanium tetrachloride was added and the temperature was lowered to -20°C. Then, 100g of a spherical magnesium compound carrier (average particle size D50 = 45μm) was added under stirring. After reacting at -20°C for 0.5 hour, the temperature was slowly raised to 120°C. During the heating process, 15g of 2-isopropyl-2-isopentyl-1,3-dimethoxypropane and 0.6g of tributyl phosphate were added. The mixture was then reacted at 120°C for 0.5 hour. The liquid was filtered off, and 1L of titanium tetrachloride was added. After maintaining the temperature at 120°C for 2 hours, the liquid was filtered off to obtain a solid product. The obtained solid product was washed 5 times with hexane and finally dried in vacuo at 45°C to obtain catalyst component A (average particle size D50 = 40μm, SPAN value 0.76), which was recorded as A-12.
[0166] Preparation Example 13
[0167] To a 3L glass reaction bottle with stirring, add 1.2L titanium tetrachloride and cool to -20℃. Then, under stirring, add 100g of magnesium chloride alcoholate spherical carrier [Mg(C2H5OH) 2.6 ] (average particle size D50 = 45 μm), react at -20 ° C for 0.5 hour, slowly heat up to 120 ° C, add 15 g of diisobutyl phthalate during the heating process, then react at 120 ° C for 0.5 hour, filter out the liquid, add 1 L of titanium tetrachloride, maintain at 120 ° C for 2 hours, filter out the liquid to obtain a solid product, wash the obtained solid product with hexane 5 times, and finally dry in vacuum to obtain catalyst component A (average particle size D50 = 40 μm, SPAN value 0.79), recorded as A-13.
[0168] Preparation Example 14
[0169] To a 3L glass reaction bottle with stirring, add 1.2L titanium tetrachloride and cool to -20℃. Then, under stirring, add 100g of magnesium chloride alcoholate spherical carrier [Mg(C2H5OH) 2.6 ] (average particle size D50 = 45 μm), react at -20 ° C for 0.5 hour, slowly heat up to 120 ° C, add 15 g of 2,3-diisopropyl succinic acid diethyl ester during the heating process, then react at 120 ° C for 0.5 hour, filter out the liquid, add 1 L of titanium tetrachloride, maintain at 120 ° C for 2 hours, filter out the liquid to obtain a solid product, wash the obtained solid product with hexane 5 times, and finally dry in vacuum to obtain catalyst component A (average particle size D50 = 41 μm, SPAN value 0.80), recorded as A-14.
[0170] Preparation Example 15
[0171] Get 650g diethoxy magnesium support (average particle size D50=47 μ m), 3250ml toluene and 65ml di-n-butyl phthalate (DNBP), be mixed with suspension.In the 16L pressure-resistant reactor that repeats replacement through high-purity nitrogen, add 2600ml toluene and 3900ml titanium tetrachloride, be cooled to-5 ℃, then the suspension for preparing is added in the still, constant temperature after 1 hour, slowly be warming up to 110 ℃, add 65ml DNBP when rising to 80 ℃, constant temperature 2 hours, then the liquid press filtration is clean.Then add the mixed solution of 5070ml toluene and 3380ml titanium tetrachloride and be warming up to 110 ℃ of stirring treatments 1 hour, so handle 3 times, elimination liquid, the solid of gained is washed 4 times with 150ml hexane, elimination liquid and drying, promptly get solid catalyst component (average particle size D50=42 μ m, SPAN value 0.82), be designated as A-15.
[0172] Preparation Example 16
[0173] A suspension was prepared by combining 650 g of a diethoxymagnesium support (average particle size D50 = 47 μm), 3250 mL of toluene, and 65 mL of diethyl 2,3-diisopropylsuccinate. In a 16-L pressure-resistant reactor that had been repeatedly purged with high-purity nitrogen, 2600 mL of toluene and 3900 mL of titanium tetrachloride were added. The reaction mixture was cooled to -5°C and the prepared suspension was added to the reactor. After maintaining the temperature for 1 hour, the temperature was slowly raised to 110°C. When the temperature reached 80°C, 65 mL of diethyl 2,3-diisopropylsuccinate was added. The temperature was maintained for 2 hours, and the liquid was then filtered. Then, a mixture of 5070 mL of toluene and 3380 mL of titanium tetrachloride was added, heated to 110° C., and stirred for 1 hour. This treatment was repeated three times, and the liquid was filtered off. The resulting solid was washed four times with 150 mL of hexane, the liquid was filtered off, and the mixture was dried to obtain a solid catalyst component (average particle size D50 = 42 μm, SPAN value 0.82), which was recorded as A-16.
[0174] Preparation Example 17
[0175] To a stirred 3L glass reaction flask, 1.2L of titanium tetrachloride was added and the temperature was lowered to -20°C. Then, under stirring, 100g of a spherical magnesium compound carrier (average particle size D50=46μm) was added. After reacting at -20°C for 0.5 hour, the temperature was slowly raised to 120°C. 15g of diisobutyl phthalate was added during the temperature rise, and then the reaction was carried out at 120°C for 0.5 hour. The liquid was filtered off, and 1L of titanium tetrachloride was added. After maintaining at 120°C for 2 hours, the liquid was filtered off to obtain a solid product. The obtained solid product was washed 5 times with hexane and finally dried in vacuo to obtain catalyst component A (average particle size D50=41μm, SPAN value 0.76), which was recorded as A-17.
[0176] Preparation Example 18
[0177] To a stirred 3L glass reaction bottle, 1.2L of titanium tetrachloride was added and the temperature was lowered to -20°C. Then, 100g of a spherical magnesium compound carrier (average particle size D50 = 46μm) was added under stirring. After reacting at -20°C for 0.5 hour, the temperature was slowly raised to 120°C. 15g of diethyl 2,3-diisopropylsuccinate was added during the heating process. Then, the reaction was continued at 120°C for 0.5 hour, the liquid was filtered off, and 1L of titanium tetrachloride was added. After maintaining at 120°C for 2 hours, the liquid was filtered off to obtain a solid product. The obtained solid product was washed 5 times with hexane and finally dried in vacuo to obtain catalyst component A (average particle size D50 = 42μm, SPAN value 0.78), which was recorded as A-18.
[0178] The following examples are used to illustrate the solid catalyst component and its preparation method and the method for olefin polymerization of the present invention.
[0179] Example 1
[0180] (1) Preparation of solid catalyst component
[0181] In a 5L autoclave, 1.1L of hexane, 15mmol of triethylaluminum, 0.3mmol of cyclohexylmethyldimethoxysilane, and 25.0g of catalyst component A-1 were added and reacted at 22°C for 10 minutes. Then, 10g of propylene was added and reacted at 23°C for 10 minutes, with the unreacted propylene vented. The reactor was purged with nitrogen, and hydrogen was added to a reaction pressure of 0.2MPa. The reaction was continued at 15°C for 10 minutes, with the unreacted hydrogen vented. The liquid in the reaction product was filtered off and then dried under vacuum (temperature 45°C, time 40 minutes) to obtain a solid catalyst component (average particle size D50 = 41μm, SPAN value 0.80), designated E-1. The composition of catalyst component E-1 is as follows: 2.2% by weight of titanium, 15.3% by weight of magnesium, 54.1% by weight of chlorine, 9.0% by weight of 2,4-pentanediol dibenzoate, and 9.5% by weight of polyolefin.
[0182] (2) Propylene polymerization A
[0183] In a 5 L autoclave, 1.3 mmol of triethylaluminum, 0.05 mmol of cyclohexylmethyldimethoxysilane, 10 mL of hexane, and 15 mg of solid catalyst component E-1 were added. After 1.5 NL of hydrogen was introduced, 2.0 kg of liquid propylene was added. The temperature was raised to 70°C while stirring and polymerization was carried out at 70°C for 1 hour. Stirring was stopped and unpolymerized propylene monomer was removed to obtain polypropylene, which was recorded as P-1A.
[0184] Propylene Polymerization B
[0185] After the solid catalyst component E-1 was stored in nitrogen for one year, propylene was polymerized according to the method of propylene polymerization A, and was recorded as P-1B.
[0186] Example 2
[0187] (1) Preparation of solid catalyst component
[0188] In a 5 L autoclave, 1.0 L of hexane, 15 mmol of triethylaluminum, 0.3 mmol of cyclohexylmethyldimethoxysilane, and 25.0 g of catalyst component A-2 were added and reacted at 15°C for 10 minutes. Then, 12 g of propylene was added and reacted at 22°C for 10 minutes, after which the unreacted propylene was vented. The reactor was then purged with nitrogen, and hydrogen was added to a reaction pressure of 0.2 MPa. The reaction was continued at 15°C for 10 minutes, after which the unreacted hydrogen was vented. The liquid in the reaction product was filtered off and dried under vacuum to obtain a solid catalyst component (average particle size D50 = 42 μm, SPAN value 0.79), designated E-2. The composition of catalyst component E-2 is as follows: 2.1 wt% titanium, 14.2 wt% magnesium, 50.2 wt% chlorine, 4.6 wt% 2,4-pentanediol dibenzoate, 5.1 wt% 2-isopropyl-2-isopentyl-1,3-dimethoxypropane, and 17.1 wt% polyolefin.
[0189] (2) Propylene polymerization A
[0190] Polypropylene was obtained by polymerization according to the method of propylene polymerization A in Example 1, using E-2 instead of E-1, and recorded as P-2A.
[0191] Propylene Polymerization B
[0192] After the solid catalyst component E-2 was stored in nitrogen for one year, propylene was polymerized according to the method of propylene polymerization A and recorded as P-2B.
[0193] Example 3
[0194] (1) Preparation of solid catalyst component
[0195] In a 5 L autoclave, 1.0 L of hexane, 15 mmol of triethylaluminum, 0.3 mmol of cyclohexylmethyldimethoxysilane, and 25.0 g of catalyst component A-2 were added and reacted at 15°C for 10 minutes. Then, 12 g of ethylene was added, and the reaction was carried out at 22°C for 10 minutes, after which unreacted propylene was vented. The reaction vessel was purged with nitrogen, and hydrogen was added to a reaction pressure of 0.2 MPa. The reaction was continued at 15°C for 10 minutes, after which unreacted hydrogen was vented. The liquid in the reaction product was filtered off and dried under vacuum to obtain a solid catalyst component (average particle size D50 = 42 μm, SPAN value 0.80), designated E-3. The composition of catalyst component E-3 is as follows: 2.1 wt% titanium, 14.4 wt% magnesium, 50.6 wt% chlorine, 4.7 wt% 2,4-pentanediol dibenzoate, 5.0 wt% 2-isopropyl-2-isopentyl-1,3-dimethoxypropane, and 17.3 wt% polyolefin.
[0196] (2) Propylene polymerization A
[0197] Polypropylene was obtained by polymerization according to the method of propylene polymerization A in Example 1, except that E-3 was used instead of E-1, and the obtained polypropylene was designated as P-3A.
[0198] Propylene Polymerization B
[0199] After the solid catalyst component E-3 was stored in nitrogen for one year, propylene was polymerized according to the method of propylene polymerization A and recorded as P-3B.
[0200] Example 4
[0201] (1) Preparation of solid catalyst component
[0202] In a 5 L autoclave, 1.0 L of hexane, 15 mmol of triethylaluminum, 0.3 mmol of cyclohexylmethyldimethoxysilane, and 25.0 g of catalyst component A-2 were added and reacted at 15° C. for 10 minutes. Then, 15 g of propylene was added and reacted at 22° C. for 10 minutes, with the unreacted propylene vented. The reactor was purged with nitrogen, and a mixture of hydrogen and nitrogen with a hydrogen content of 20% by volume was added to a reaction pressure of 0.2 MPa. The reaction was continued at 15° C. for 10 minutes, with the unreacted hydrogen vented. The liquid in the reaction product was filtered off and dried under vacuum to obtain a solid catalyst component (average particle size D50 = 43 μm, SPAN value 0.81), designated E-4. The composition of catalyst component E-4 is as follows: 1.7 wt% titanium, 11.6 wt% magnesium, 40.3 wt% chlorine, 3.9 wt% 2,4-pentanediol dibenzoate, 4.2 wt% 2-isopropyl-2-isopentyl-1,3-dimethoxypropane, and 33.2 wt% polyolefin.
[0203] (2) Propylene polymerization A
[0204] Polypropylene was obtained by polymerization according to the method of propylene polymerization A in Example 1, except that E-4 was used instead of E-1, and the obtained polypropylene was designated as P-4A.
[0205] Propylene Polymerization B
[0206] After the solid catalyst component E-4 was stored in nitrogen for one year, propylene was polymerized according to the method of propylene polymerization A and recorded as P-4B.
[0207] Example 5
[0208] (1) Preparation of solid catalyst component
[0209] In a 5 L autoclave, 1.1 L of hexane, 15 mmol of triethylaluminum, 0.3 mmol of cyclohexylmethyldimethoxysilane, and 25.0 g of catalyst component A-3 were added and reacted at 22°C for 10 minutes. Then, 10 g of propylene was added and reacted at 23°C for 10 minutes, with the unreacted propylene vented. The reactor was purged with nitrogen, and hydrogen was added to a reaction pressure of 0.2 MPa. The reaction was continued at 15°C for 10 minutes, with the unreacted hydrogen vented. The liquid in the reaction product was filtered off and dried under vacuum to obtain a solid catalyst component (average particle size D50 = 43 μm, SPAN value 0.83), designated E-5.
[0210] (2) Propylene polymerization A
[0211] In a 5 L autoclave, 1.3 mmol of triethylaluminum, 0.05 mmol of cyclohexylmethyldimethoxysilane, 10 mL of hexane, and 15 mg of solid catalyst component E-5 were added. After 1.5 NL of hydrogen was introduced, 2.0 kg of liquid propylene was added. The temperature was raised to 70°C while stirring and polymerization was carried out at 70°C for 1 hour. Stirring was stopped and unpolymerized propylene monomer was removed to obtain polypropylene, which was recorded as P-5A.
[0212] Propylene Polymerization B
[0213] After the solid catalyst component E-5 was stored in nitrogen for one year, propylene was polymerized according to the method of propylene polymerization A and recorded as P-5B.
[0214] Example 6
[0215] (1) Preparation of solid catalyst component
[0216] In a 5 L autoclave, 1.0 L of hexane, 15 mmol of triethylaluminum, 0.3 mmol of cyclohexylmethyldimethoxysilane, and 25.0 g of catalyst component A-4 were added and reacted at 15°C for 10 minutes. Then, 10 g of propylene was added and reacted at 22°C for 10 minutes, after which the unreacted propylene was vented. The reaction vessel was purged with nitrogen, and hydrogen was added to a reaction pressure of 0.2 MPa. The reaction was continued at 15°C for 10 minutes, after which the unreacted hydrogen was vented. The liquid in the reaction product was filtered off and dried under vacuum to obtain a solid catalyst component (average particle size D50 = 43 μm, SPAN value 0.83), designated E-6.
[0217] (2) Propylene polymerization A
[0218] Polypropylene was obtained by polymerization according to the method of propylene polymerization A in Example 5, except that E-6 was used instead of E-5, and the obtained polypropylene was designated as P-6A.
[0219] Propylene Polymerization B
[0220] After the solid catalyst component E-6 was stored in nitrogen for one year, propylene was polymerized according to the method of propylene polymerization A and recorded as P-6B.
[0221] Example 7
[0222] (1) Preparation of solid catalyst component
[0223] In a 5 L autoclave, 1.0 L of hexane, 15 mmol of triethylaluminum, 0.3 mmol of cyclohexylmethyldimethoxysilane, and 25.0 g of catalyst component A-4 were added and reacted at 15°C for 10 minutes. Then, 10 g of ethylene was added, and the reaction was continued at 22°C for 10 minutes, with unreacted propylene vented. The reaction vessel was purged with nitrogen, and hydrogen was added to a reaction pressure of 0.2 MPa. The reaction was continued at 15°C for 10 minutes, with unreacted hydrogen vented. The liquid in the reaction product was filtered off and dried under vacuum to obtain a solid catalyst component (average particle size D50 = 42 μm, SPAN value 0.82), designated E-7.
[0224] (2) Propylene polymerization A
[0225] Polypropylene was obtained by polymerization according to the method of propylene polymerization A in Example 5, using E-7 instead of E-5, and recorded as P-7A.
[0226] Propylene Polymerization B
[0227] After the solid catalyst component E-7 was stored in nitrogen for one year, propylene was polymerized according to the method of propylene polymerization A and recorded as P-7B.
[0228] Example 8
[0229] (1) Preparation of solid catalyst component
[0230] In a 5 L autoclave, 1.1 L of hexane, 15 mmol of triethylaluminum, 0.3 mmol of cyclohexylmethyldimethoxysilane, and 25.0 g of catalyst component A-5 were added and reacted at 22°C for 10 minutes. Then, 10 g of propylene was added and reacted at 23°C for 10 minutes, after which the unreacted propylene was vented. The reaction vessel was purged with nitrogen, and hydrogen was added to a reaction pressure of 0.2 MPa. The reaction was continued at 15°C for 10 minutes, after which the unreacted hydrogen was vented. The liquid in the reaction product was filtered off and dried under vacuum to obtain a solid catalyst component (average particle size D50 = 41 μm, SPAN value 0.77), designated E-8.
[0231] (2) Propylene polymerization A
[0232] In a 5 L autoclave, 1.3 mmol of triethylaluminum, 0.05 mmol of cyclohexylmethyldimethoxysilane, 10 mL of hexane, and 15 mg of solid catalyst component E-5 were added. After 1.5 NL of hydrogen was introduced, 2.0 kg of liquid propylene was added. The temperature was raised to 70°C while stirring, and polymerization was carried out at 70°C for 1 hour. Stirring was stopped, and the unpolymerized propylene monomer was removed to obtain polypropylene, which was recorded as P-8A.
[0233] Propylene Polymerization B
[0234] After the solid catalyst component E-8 was stored in nitrogen for one year, propylene was polymerized according to the method of propylene polymerization A and recorded as P-8B.
[0235] Example 9
[0236] (1) Preparation of solid catalyst component
[0237] In a 5 L autoclave, 1.0 L of hexane, 15 mmol of triethylaluminum, 0.3 mmol of cyclohexylmethyldimethoxysilane, and 25.0 g of catalyst component A-6 were added and reacted at 15°C for 10 minutes. Then, 10 g of propylene was added and reacted at 22°C for 10 minutes, after which the unreacted propylene was vented. The reaction vessel was purged with nitrogen, and hydrogen was added to a reaction pressure of 0.2 MPa. The reaction was continued at 15°C for 10 minutes, after which the unreacted hydrogen was vented. The liquid in the reaction product was filtered off and dried under vacuum to obtain a solid catalyst component (average particle size D50 = 42 μm, SPAN value 0.77), designated E-9.
[0238] (2) Propylene polymerization A
[0239] Polypropylene was obtained by polymerization according to the method of propylene polymerization A in Example 8, except that E-9 was used instead of E-8, and the obtained polypropylene was designated as P-9A.
[0240] Propylene Polymerization B
[0241] After the solid catalyst component E-9 was stored in nitrogen for one year, propylene was polymerized according to the method of propylene polymerization A and recorded as P-9B.
[0242] Example 10
[0243] (1) Preparation of solid catalyst component
[0244] In a 5 L autoclave, 1.0 L of hexane, 15 mmol of triethylaluminum, 0.3 mmol of cyclohexylmethyldimethoxysilane, and 25.0 g of catalyst component A-6 were added and reacted at 15°C for 10 minutes. Then, 10 g of ethylene was added, and the reaction was carried out at 22°C for 10 minutes, after which unreacted propylene was vented. The reaction vessel was purged with nitrogen, and hydrogen was added to a reaction pressure of 0.2 MPa. The reaction was continued at 15°C for 10 minutes, after which unreacted hydrogen was vented. The liquid in the reaction product was filtered off and dried under vacuum to obtain a solid catalyst component (average particle size D50 = 42 μm, SPAN value 0.77), designated E-10.
[0245] (2) Propylene polymerization A
[0246] Polypropylene was obtained by polymerization according to the method of propylene polymerization A in Example 8, except that E-10 was used instead of E-8, and the obtained polypropylene was designated as P-10A.
[0247] Propylene Polymerization B
[0248] After the solid catalyst component E-10 was stored in nitrogen for one year, propylene was polymerized according to the method of propylene polymerization A, and was recorded as P-10B.
[0249] Example 11
[0250] (1) Preparation of solid catalyst component
[0251] In a 5-liter autoclave, 1.0 liter of hexane, 20 mmol of triethylaluminum, 0.3 mmol of cyclohexylmethyldimethoxysilane, and 25.0 g of catalyst component A-7 were added and reacted at 22°C for 10 minutes. Then, 6 g of propylene was added and reacted at 23°C for 10 minutes, with the unreacted propylene vented. The reactor was purged with nitrogen, and hydrogen was added to a pressure of 0.2 MPa. The reaction was continued at 15°C for 10 minutes, with the unreacted hydrogen vented. The liquid in the reaction product was filtered off and dried under vacuum to obtain a solid catalyst component (average particle size D50 = 41 μm, SPAN value 0.80), designated E-11. The composition of catalyst component E-11 was as follows: 2.2 wt% titanium, 16.3 wt% magnesium, 53.1 wt% chlorine, 9.1 wt% 2-isopropyl-2-isopentyl-1,3-dimethoxypropane, and 13.0 wt% polyolefin.
[0252] (2) Propylene polymerization A
[0253] In a 5 L autoclave, 1.3 mmol of triethylaluminum, 0.05 mmol of cyclohexylmethyldimethoxysilane, 10 mL of hexane, and 15 mg of solid catalyst component E-11 were added. After 1.5 NL of hydrogen was introduced, 2.0 kg of liquid propylene was added. The temperature was raised to 70°C while stirring and polymerization was carried out at 70°C for 1 hour. Stirring was stopped and unpolymerized propylene monomer was removed to obtain polypropylene, which was recorded as P-11A.
[0254] Propylene Polymerization B
[0255] After the solid catalyst component E-11 was stored for one year, propylene polymerization was carried out in the same manner as propylene polymerization A. The resulting polypropylene was designated P-11B.
[0256] Example 12
[0257] (1) Preparation of solid catalyst component
[0258] The solid catalyst component was prepared in the same manner as in Example 11, except that A-8 was used instead of A-7. A solid catalyst component (average particle size D50 = 41 μm, SPAN value 0.80) was obtained, designated E-12. The composition of catalyst component E-12 was as follows: 2.3 wt% titanium, 16.1 wt% magnesium, 52.8 wt% chlorine, 8.9 wt% 2-isopropyl-2-isopentyl-1,3-dimethoxypropane, and 13.2 wt% polyolefin.
[0259] (2) Propylene polymerization A
[0260] The same propylene polymerization A as in Example 11 was carried out except that E-12 was used instead of E-11 to obtain polypropylene, which was designated as P-12A.
[0261] Propylene Polymerization B
[0262] The same propylene polymerization B as in Example 11 was carried out except that E-12 was used instead of E-11 to obtain polypropylene, which was designated as P-12B.
[0263] Example 13
[0264] (1) Preparation of solid catalyst component
[0265] A solid catalyst component was prepared according to the method of Example 11, except that ethylene was used instead of propylene, resulting in a solid catalyst component (average particle size D50 = 41 μm, SPAN value 0.80), designated E-13. The composition of catalyst component E-13 was as follows: 2.2 wt% titanium, 16.2 wt% magnesium, 52.9 wt% chlorine, 9.0 wt% 2-isopropyl-2-isopentyl-1,3-dimethoxypropane, and 13.5 wt% polyolefin.
[0266] (2) Propylene polymerization A
[0267] The same propylene polymerization process as in Example 11 was carried out except that E-13 was used instead of E-11 to obtain polypropylene, which was designated as P-13A.
[0268] Propylene Polymerization B
[0269] The same propylene polymerization B as in Example 11 was carried out except that E-13 was used instead of E-11 to obtain polypropylene, which was designated as P-13B.
[0270] Example 14
[0271] (1) Preparation of solid catalyst component
[0272] A solid catalyst component was prepared according to the method of Example 11, except that 5 g of propylene and 0.2 g of ethylene were used in place of 6 g of propylene. This resulted in a solid catalyst component (average particle size D50 = 41 μm, SPAN value 0.80), designated E-14. The composition of catalyst component E-14 was as follows: 2.2 wt% titanium, 16.6 wt% magnesium, 53.8 wt% chlorine, 9.0 wt% 2-isopropyl-2-isopentyl-1,3-dimethoxypropane, and 13.1 wt% polyolefin.
[0273] (2) Propylene polymerization A
[0274] The method of propylene polymerization A in Example 11 was followed, except that the solid catalyst component was replaced by E-14 from E-11, to obtain polypropylene, which was designated as P-14A.
[0275] Propylene Polymerization B
[0276] The same propylene polymerization B as in Example 11 was carried out except that E-14 was used instead of E-11 to obtain polypropylene, which was designated as P-14B.
[0277] Example 15
[0278] (1) Preparation of solid catalyst component
[0279] In a 5-L autoclave, 1.0 L of hexane, 20 mmol of triethylaluminum, 0.3 mmol of cyclohexylmethyldimethoxysilane, and 25.0 g of catalyst component A-7 were added and reacted at 22°C for 10 minutes. Then, 15 g of propylene was added and reacted at 23°C for 10 minutes, with the unreacted propylene vented. The reactor was purged with nitrogen, and hydrogen was added to a pressure of 0.2 MPa. The reaction was continued at 15°C for 10 minutes, with the unreacted hydrogen vented. The liquid in the reaction product was filtered off and dried under vacuum to obtain a solid catalyst component (average particle size D50 = 41 μm, SPAN value 0.81), designated E-15. The composition of catalyst component E-15 was as follows: 1.7 wt% titanium, 12.6 wt% magnesium, 40.2 wt% chlorine, 7.0 wt% 2-isopropyl-2-isopentyl-1,3-dimethoxypropane, and 33.8 wt% polyolefin.
[0280] (2) Propylene polymerization A
[0281] Polypropylene was obtained by polymerization according to the method of propylene polymerization A in Example 11, using E-15 instead of E-11, and recorded as P-5A.
[0282] Propylene Polymerization B
[0283] After the solid catalyst component E-15 was stored in nitrogen for one year, propylene was polymerized according to the method of propylene polymerization A, and was recorded as P-15B.
[0284] Example 16
[0285] (1) Preparation of solid catalyst component
[0286] In a 5 L autoclave, 1.0 L of hexane, 20 mmol of triethylaluminum, 0.3 mmol of cyclohexylmethyldimethoxysilane, and 25.0 g of catalyst component A-9 were added and reacted at 22° C. for 10 minutes. Then, 6 g of propylene was added and reacted at 23° C. for 10 minutes, after which the unreacted propylene was vented. The reactor was then purged with nitrogen, and hydrogen was added to a pressure of 0.2 MPa. The reaction was continued at 15° C. for 10 minutes, after which the unreacted hydrogen was vented. The liquid in the reaction product was filtered off and dried under vacuum to obtain a solid catalyst component (average particle size D50 = 43 μm, SPAN value 0.83), designated E-16.
[0287] (2) Propylene polymerization A
[0288] In a 5 L autoclave, 1.3 mmol of triethylaluminum, 0.05 mmol of cyclohexylmethyldimethoxysilane, 10 mL of hexane, and 15 mg of the solid catalyst component E-16 were added. After 1.5 NL of hydrogen was introduced, 2.0 kg of liquid propylene was added. The temperature was raised to 70°C while stirring and polymerization was carried out at 70°C for 1 hour. Stirring was stopped and the unpolymerized propylene monomer was removed to obtain polypropylene, which was recorded as P-16A.
[0289] Propylene Polymerization B
[0290] After the solid catalyst component E-16 was stored for one year, propylene polymerization was carried out in the same manner as propylene polymerization A. The resulting polypropylene was designated P-16B.
[0291] Example 17
[0292] (1) Preparation of solid catalyst component
[0293] The solid catalyst component was prepared in the same manner as in Example 16 except that A10 was used instead of A9. A solid catalyst component (average particle size D50 = 43 μm, SPAN value 0.83) was obtained and designated as E-17.
[0294] (2) Propylene polymerization A
[0295] The same propylene polymerization process as in Example 16 was carried out except that E-17 was used instead of E-16 to obtain polypropylene, which was designated as P-17A.
[0296] Propylene Polymerization B
[0297] The same propylene polymerization B as in Example 16 was carried out except that E-17 was used instead of E-16 to obtain polypropylene, which was designated as P-17B.
[0298] Example 18
[0299] (1) Preparation of solid catalyst component
[0300] A solid catalyst component was prepared according to the method of Example 16, except that ethylene was used instead of propylene, thereby obtaining a solid catalyst component (average particle size D50 = 43 μm, SPAN value 0.83), which was recorded as E-18.
[0301] (2) Propylene polymerization A
[0302] The same propylene polymerization process as in Example 16 was carried out except that E-18 was used instead of E-16 to obtain polypropylene, which was designated as P-18A.
[0303] Propylene Polymerization B
[0304] The same propylene polymerization B as in Example 16 was carried out except that E-18 was used instead of E-16 to obtain polypropylene, which was designated as P-18B.
[0305] Example 19
[0306] (1) Preparation of solid catalyst component
[0307] A solid catalyst component was prepared according to the method of Example 16, except that 5 g of propylene and 0.2 g of ethylene were used instead of 6 g of propylene, thereby obtaining a solid catalyst component (average particle size D50 = 43 μm, SPAN value 0.83), which was recorded as E-19.
[0308] (2) Propylene polymerization A
[0309] The method of propylene polymerization A in Example 16 was followed, except that the solid catalyst component was replaced by E-16 from E-19, to obtain polypropylene, which was designated as P-19A.
[0310] Propylene Polymerization B
[0311] The same propylene polymerization B as in Example 16 was carried out except that E-19 was used instead of E-16 to obtain polypropylene, which was designated as P-19B.
[0312] Example 20
[0313] (1) Preparation of solid catalyst component
[0314] In a 5 L autoclave, 1.0 L of hexane, 20 mmol of triethylaluminum, 0.3 mmol of cyclohexylmethyldimethoxysilane, and 25.0 g of catalyst component A-11 were added and reacted at 22°C for 10 minutes. Then, 6 g of propylene was added and reacted at 23°C for 10 minutes, after which the unreacted propylene was vented. The reaction vessel was purged with nitrogen, and hydrogen was added to a pressure of 0.2 MPa. The reaction was continued at 15°C for 10 minutes, after which the unreacted hydrogen was vented. The liquid in the reaction product was filtered off and dried under vacuum to obtain a solid catalyst component (average particle size D50 = 41 μm, SPAN value 0.77), designated E-20.
[0315] (2) Propylene polymerization A
[0316] In a 5 L autoclave, 1.3 mmol of triethylaluminum, 0.05 mmol of cyclohexylmethyldimethoxysilane, 10 mL of hexane, and 15 mg of the solid catalyst component E-20 were added. After 1.5 NL of hydrogen was introduced, 2.0 kg of liquid propylene was added. The temperature was raised to 70°C while stirring and polymerization was carried out at 70°C for 1 hour. Stirring was stopped and the unpolymerized propylene monomer was removed to obtain polypropylene, which was recorded as P-20A.
[0317] Propylene Polymerization B
[0318] After the solid catalyst component E-20 was stored for one year, propylene polymerization was carried out in the same manner as propylene polymerization A. The resulting polypropylene was designated P-20B.
[0319] Example 21
[0320] (1) Preparation of solid catalyst component
[0321] The solid catalyst component was prepared in the same manner as in Example 20 except that A12 was used instead of A11. A solid catalyst component (average particle size D50 = 41 μm, SPAN value 0.77) was obtained and designated as E-21.
[0322] (2) Propylene polymerization A
[0323] The same propylene polymerization process as in Example 20 was carried out except that E-21 was used instead of E-20 to obtain polypropylene, which was designated as P-21A.
[0324] Propylene Polymerization B
[0325] The same propylene polymerization B as in Example 20 was carried out except that E-21 was used instead of E-20 to obtain polypropylene, which was designated as P-21B.
[0326] Example 22
[0327] (1) Preparation of solid catalyst component
[0328] A solid catalyst component was prepared according to the method of Example 20, except that ethylene was used instead of propylene, thereby obtaining a solid catalyst component (average particle size D50 = 41 μm, SPAN value 0.77), which was recorded as E-22.
[0329] (2) Propylene polymerization A
[0330] The same propylene polymerization process as in Example 20 was carried out except that E-22 was used instead of E-20 to obtain polypropylene, which was designated as P-22A.
[0331] Propylene Polymerization B
[0332] The same propylene polymerization B as in Example 20 was carried out except that E-22 was used instead of E-20 to obtain polypropylene, which was designated as P-22B.
[0333] Example 23
[0334] (1) Preparation of solid catalyst component
[0335] A solid catalyst component was prepared according to the method of Example 20, except that 5 g of propylene and 0.2 g of ethylene were used instead of 6 g of propylene, thereby obtaining a solid catalyst component (average particle size D50 = 41 μm, SPAN value 0.77), which was recorded as E-23.
[0336] (2) Propylene polymerization A
[0337] The method of propylene polymerization A in Example 20 was followed, except that the solid catalyst component was replaced by E-20 from E-23, to obtain polypropylene, which was designated as P-23A.
[0338] Propylene Polymerization B
[0339] The same propylene polymerization B as in Example 20 was carried out except that E-23 was used instead of E-20 to obtain polypropylene, which was designated as P-23B.
[0340] Example 24
[0341] (1) Preparation of solid catalyst component
[0342] In a 5 L autoclave, 1.0 L of hexane, 16 mmol of triethylaluminum, 0.3 mmol of cyclohexylmethyldimethoxysilane, and 25.0 g of catalyst component A-13 were added and reacted at 22°C for 10 minutes. Then, 10 g of propylene was added and reacted at 15°C for 10 minutes, with the unreacted propylene vented. The reactor was purged with nitrogen, and hydrogen was added to a pressure of 0.3 MPa. The reaction was continued at 15°C for 10 minutes, with the unreacted hydrogen vented. The liquid in the reaction product was filtered off and dried under vacuum to obtain a solid catalyst component (average particle size D50 = 41 μm, SPAN value 0.80), designated E-24. The composition of catalyst component E-24 was as follows: 2.3 wt% titanium, 15.5 wt% magnesium, 54.3 wt% chlorine, 8.7 wt% diisobutyl phthalate, and 9.5% polyolefin.
[0343] (2) Propylene polymerization A
[0344] In a 5 L autoclave, 5.0 mmol of triethylaluminum, 0.2 mmol of cyclohexylmethyldimethoxysilane, 10 mL of hexane, and 15 mg of the solid catalyst component E-24 were added. After 1.5 NL of hydrogen was introduced, 2.0 kg of liquid propylene was added. The temperature was raised to 70°C while stirring, and polymerization was carried out at 70°C for 1 hour. Stirring was stopped, and the unpolymerized propylene monomer was removed to obtain polypropylene, which was recorded as P-24A.
[0345] Propylene Polymerization B
[0346] After the solid catalyst component E-24 was stored under nitrogen for one year, propylene polymerization was carried out according to the propylene polymerization method A, and was recorded as P-24B.
[0347] Example 25
[0348] (1) Preparation of solid catalyst component
[0349] A solid catalyst component was prepared according to the method of Example 24, except that ethylene was used instead of propylene, resulting in a solid catalyst component (average particle size D50 = 42 μm, SPAN value 0.82), designated E-25. The composition of catalyst component E-25 was as follows: 2.3 wt% titanium, 15.1 wt% magnesium, 54.9 wt% chlorine, 8.5 wt% diisobutyl phthalate, and 9.4 wt% polyolefin.
[0350] (2) Propylene polymerization A
[0351] Propylene polymerization was carried out according to the propylene polymerization method A of Example 24, except that the solid catalyst component E-24 was replaced by E-25, thereby producing polypropylene, which was recorded as P-25A.
[0352] Propylene Polymerization B
[0353] After the solid catalyst component E-25 was stored under nitrogen for one year, propylene polymerization was carried out according to the propylene polymerization method A of Example 24, and the result was recorded as P-25B.
[0354] Example 26
[0355] (1) Preparation of solid catalyst component
[0356] A solid catalyst component was prepared according to the method of Example 24, except that catalyst component A14 was used instead of A13, resulting in a solid catalyst component (average particle size D50 = 42 μm, SPAN value 0.81), designated E-26. Catalyst component E-26 had the following composition: 2.2 wt% titanium, 15.2 wt% magnesium, 55.0 wt% chlorine, 9.0 wt% diethyl 2,3-diisopropylsuccinate, and 9.1 wt% polyolefin.
[0357] (2) Propylene polymerization A
[0358] Propylene polymerization was carried out according to the propylene polymerization method A of Example 24, except that the solid catalyst component was replaced by E-26 from E-24 to obtain polypropylene, which was recorded as P-26A.
[0359] Propylene Polymerization B
[0360] After the solid catalyst component E-26 was stored under nitrogen for one year, propylene polymerization was carried out according to the propylene polymerization method A of Example 24, and was recorded as P-26B.
[0361] Example 27
[0362] (1) Preparation of solid catalyst component
[0363] In a 5L autoclave, 1.0L of hexane, 15mmol of triethylaluminum, 0.3mmol of cyclohexylmethyldimethoxysilane, and 25.0g of catalyst component A-14 were added and reacted at 15°C for 10 minutes. Then, 15g of propylene was added and reacted at 22°C for 10 minutes, with the unreacted propylene vented. The reactor was purged with nitrogen, and a mixed gas containing 20% hydrogen was added to a reaction pressure of 0.2MPa. The reaction was continued at 15°C for 10 minutes, with the unreacted hydrogen vented. The liquid in the reaction product was filtered off and dried under vacuum to obtain a solid catalyst component (average particle size D50 = 42μm, SPAN value 0.82), designated E-27. The composition of catalyst component E-27 is as follows: 1.6wt% titanium, 11.9wt% magnesium, 39.3wt% chlorine, 6.0wt% diethyl 2,3-diisopropylsuccinate, and 32.5wt% polyolefin.
[0364] (2) Propylene polymerization A
[0365] Polypropylene was obtained by polymerization according to the method of propylene polymerization A in Example 24, using E-27 instead of E-24, and recorded as P-27A.
[0366] Propylene Polymerization B
[0367] After the solid catalyst component E-27 was stored in nitrogen for one year, propylene was polymerized according to the method of propylene polymerization A and recorded as P-27B.
[0368] Example 28
[0369] (1) Preparation of solid catalyst component
[0370] In a 5 L autoclave, 1.0 L of hexane, 16 mmol of triethylaluminum, 0.3 mmol of cyclohexylmethyldimethoxysilane, and 25.0 g of catalyst component A-15 were added and reacted at 22° C. for 10 minutes. Then, 10 g of propylene was added and reacted at 15° C. for 10 minutes, after which the unreacted propylene was vented. The reactor was then purged with nitrogen, and hydrogen was added to a pressure of 0.3 MPa. The reaction was continued at 15° C. for 10 minutes, after which the unreacted hydrogen was vented. The liquid in the reaction product was filtered off and dried under vacuum to obtain a solid catalyst component (average particle size D50 = 43 μm, SPAN value 0.83), designated E-28.
[0371] (2) Propylene polymerization A
[0372] In a 5 L autoclave, 5.0 mmol of triethylaluminum, 0.2 mmol of cyclohexylmethyldimethoxysilane, 10 mL of hexane, and 15 mg of the solid catalyst component E-28 were added. After 1.5 NL of hydrogen was introduced, 2.0 kg of liquid propylene was added. The temperature was raised to 70°C while stirring and polymerization was carried out at 70°C for 1 hour. Stirring was stopped and the unpolymerized propylene monomer was removed to obtain polypropylene, which was recorded as P-28A.
[0373] Propylene Polymerization B
[0374] After the solid catalyst component E-28 was stored under nitrogen for one year, propylene polymerization was carried out according to the propylene polymerization method A, and was recorded as P-28B.
[0375] Example 29
[0376] (1) Preparation of solid catalyst component
[0377] A solid catalyst component was prepared according to the method of Example 28, except that ethylene was used instead of propylene, thereby obtaining a solid catalyst component (average particle size D50 = 43 μm, SPAN value 0.83), which was recorded as E-29.
[0378] (2) Propylene polymerization A
[0379] Propylene polymerization was carried out according to the propylene polymerization method A of Example 28, except that the solid catalyst component E-28 was replaced by E-29, thereby producing polypropylene, which was recorded as P-29A.
[0380] Propylene Polymerization B
[0381] After the solid catalyst component E-29 was stored under nitrogen for one year, propylene polymerization was carried out according to the propylene polymerization method A in Example 28, and the result was recorded as P-29B.
[0382] Example 30
[0383] (1) Preparation of solid catalyst component
[0384] A solid catalyst component was prepared according to the method of Example 28, except that catalyst component A16 was used instead of A15, thereby obtaining a solid catalyst component (average particle size D50 = 43 μm, SPAN value 0.83), which was recorded as E-30.
[0385] (2) Propylene polymerization A
[0386] Propylene polymerization was carried out according to the propylene polymerization method A of Example 28, except that the solid catalyst component was replaced by E-30 from E-28 to obtain polypropylene, which was recorded as P-30A.
[0387] Propylene Polymerization B
[0388] After the solid catalyst component E-30 was stored under nitrogen for one year, propylene polymerization was carried out according to the propylene polymerization method A in Example 28, and the result was recorded as P-30B.
[0389] Example 31
[0390] (1) Preparation of solid catalyst component
[0391] In a 5 L autoclave, 1.0 L of hexane, 16 mmol of triethylaluminum, 0.3 mmol of cyclohexylmethyldimethoxysilane, and 25.0 g of catalyst component A-17 were added and reacted at 22°C for 10 minutes. Then, 10 g of propylene was added and reacted at 15°C for 10 minutes, after which the unreacted propylene was vented. The reactor was then purged with nitrogen, and hydrogen was added to a pressure of 0.3 MPa. The reaction was continued at 15°C for 10 minutes, after which the unreacted hydrogen was vented. The liquid in the reaction product was filtered off and dried under vacuum to obtain a solid catalyst component (average particle size D50 = 42 μm, SPAN value 0.77), designated E-31.
[0392] (2) Propylene polymerization A
[0393] In a 5 L autoclave, 5.0 mmol of triethylaluminum, 0.2 mmol of cyclohexylmethyldimethoxysilane, 10 mL of hexane, and 15 mg of the solid catalyst component E-31 were added. After 1.5 NL of hydrogen was introduced, 2.0 kg of liquid propylene was added. The temperature was raised to 70°C while stirring, and polymerization was carried out at 70°C for 1 hour. Stirring was stopped, and the unpolymerized propylene monomer was removed to obtain polypropylene, which was recorded as P-31A.
[0394] Propylene Polymerization B
[0395] After the solid catalyst component E-31 was stored under nitrogen for one year, propylene polymerization was carried out according to the propylene polymerization method A, and was recorded as P-31B.
[0396] Example 32
[0397] (1) Preparation of solid catalyst component
[0398] A solid catalyst component was prepared according to the method of Example 31, except that ethylene was used instead of propylene, thereby obtaining a solid catalyst component (average particle size D50 = 42 μm, SPAN value 0.77), which was recorded as E-32.
[0399] (2) Propylene polymerization A
[0400] Propylene polymerization was carried out according to the propylene polymerization method A of Example 31, except that the solid catalyst component E-31 was replaced by E-32, thereby producing polypropylene, which was recorded as P-32A.
[0401] Propylene Polymerization B
[0402] After the solid catalyst component E-32 was stored under nitrogen for one year, propylene polymerization was carried out according to the propylene polymerization method A in Example 31, and the result was recorded as P-32B.
[0403] Example 33
[0404] (1) Preparation of solid catalyst component
[0405] A solid catalyst component was prepared according to the method of Example 31, except that catalyst component A-18 was used instead of A-17, thereby obtaining a solid catalyst component (average particle size D50 = 43 μm, SPAN value 0.79), which was recorded as E-33.
[0406] (2) Propylene polymerization A
[0407] Propylene polymerization was carried out according to the propylene polymerization method A of Example 31, except that the solid catalyst component was replaced by E-33 from E-31 to obtain polypropylene, which was recorded as P-33A.
[0408] Propylene Polymerization B
[0409] After the solid catalyst component E-33 was stored under nitrogen for one year, propylene polymerization was carried out according to the propylene polymerization method A in Example 31, and the result was recorded as P-33B.
[0410] Comparative Example 1
[0411] (1) Preparation of solid catalyst component
[0412] In a 5 L autoclave, 1.0 L of hexane, 15 mmol of triethylaluminum, 0.3 mmol of cyclohexylmethyldimethoxysilane, and 25.0 g of catalyst component A-1 were added and reacted at 22°C for 10 minutes. Then, 10 g of propylene and 2 g of hydrogen were added and reacted at 23°C for 10 minutes. Unreacted propylene was vented and the reactor was replaced with nitrogen. The liquid in the reaction product was filtered off and dried under vacuum to obtain a solid catalyst component, designated CE-1.
[0413] (2) Propylene polymerization A
[0414] Propylene polymerization was carried out according to the propylene polymerization method A of Example 1, except that the solid catalyst component was replaced by CE-1 in place of E-1, thereby producing polypropylene, which was designated as CP-1A.
[0415] Propylene Polymerization B
[0416] Propylene polymerization was carried out according to the propylene polymerization method B of Example 1, except that the solid catalyst component was replaced by CE-1, thereby producing polypropylene, which was recorded as CP-1B.
[0417] Comparative Example 2
[0418] (1) Preparation of solid catalyst component
[0419] In a 5 L autoclave, 1.0 L of hexane, 15 mmol of triethylaluminum, 0.3 mmol of cyclohexylmethyldimethoxysilane, and 25.0 g of catalyst component A-4 were added and reacted at 15°C for 10 minutes. Then, 10 g of ethylene was added and reacted at 22°C for 10 minutes. Unreacted ethylene was vented and the atmosphere in the autoclave was replaced with nitrogen. The liquid in the reaction product was filtered off and dried under vacuum to obtain a solid catalyst component, designated CE-2.
[0420] (2) Propylene polymerization A
[0421] Propylene polymerization was carried out according to the propylene polymerization method A of Example 6, except that the solid catalyst component was replaced by CE-2 in place of E-6, thereby producing polypropylene, which was designated as CP-2A.
[0422] Propylene Polymerization B
[0423] Propylene polymerization was carried out according to the propylene polymerization method B of Example 6, except that the solid catalyst component was replaced by CE-2 in place of E-6, thereby producing polypropylene, which was designated as CP-2B.
[0424] Comparative Example 3
[0425] (1) Preparation of solid catalyst component
[0426] In a 5 L autoclave, 1.0 L of hexane, 20 mmol of triethylaluminum, 0.3 mmol of cyclohexylmethyldimethoxysilane and 25.0 g of catalyst component A-7 were added and reacted at 22°C for 10 minutes. Then, 6 g of propylene was added and reacted at 23°C for 10 minutes. The unreacted propylene was vented. The liquid in the reaction product was filtered off and dried under vacuum to obtain a solid catalyst component, which was recorded as CE-3.
[0427] (2) Propylene polymerization A
[0428] The same propylene polymerization process as in Example 10 was carried out except that CE-3 was used instead of E-10 to obtain polypropylene, which was designated as CP-3A.
[0429] Propylene Polymerization B
[0430] The same propylene polymerization B as in Example 10 was carried out except that CE-3 was used instead of E-10 to obtain polypropylene, which was designated as CP-3B.
[0431] Comparative Example 4
[0432] (1) Preparation of solid catalyst component
[0433] A solid catalyst component was prepared according to the method of Comparative Example 3, except that 6 g of ethylene was used instead of 6 g of propylene, thereby preparing a solid catalyst component, which was recorded as CE-4.
[0434] (2) Propylene polymerization A
[0435] The same propylene polymerization process as in Example 10 was carried out except that CE-4 was used instead of E-100 to obtain polypropylene, which was designated as CP-4A.
[0436] Propylene Polymerization B
[0437] The same propylene polymerization B as in Example 10 was carried out except that CE-4 was used instead of E-10 to obtain polypropylene, which was designated as CP-4B.
[0438] Comparative Example 5
[0439] (1) Preparation of solid catalyst component
[0440] In a 5-liter autoclave, 1.0 liter of hexane, 20 mmol of triethylaluminum, 0.3 mmol of cyclohexylmethyldimethoxysilane, and 25.0 g of catalyst component A-7 were added, and the mixture was reacted at 22°C for 10 minutes. Then, 6 g of ethylene and 2 g of hydrogen were added, and the mixture was reacted at 23°C for 10 minutes. The unreacted gas was vented. The liquid in the reaction product was filtered off and dried under vacuum to obtain a solid catalyst component, which was designated as CE-5.
[0441] (2) Propylene polymerization A
[0442] The same propylene polymerization A as in Example 10 was carried out except that CE-5 was used instead of E-10 to obtain polypropylene, which was designated as CP-5A.
[0443] Propylene Polymerization B
[0444] The same propylene polymerization B as in Example 10 was carried out except that CE-5 was used instead of E-10 to obtain polypropylene, which was designated as CP-5B.
[0445] Comparative Example 6
[0446] (1) Preparation of solid catalyst component
[0447] In a 5 L autoclave, 1.0 L of hexane, 16 mmol of triethylaluminum, 0.3 mmol of cyclohexylmethyldimethoxysilane, and 25.0 g of catalyst component A-13 were added and reacted at 22° C. for 10 minutes. Then, 10 g of propylene was added and reacted at 15° C. for 10 minutes. The unreacted propylene was vented. The reactor was replaced with nitrogen, the liquid in the reaction product was filtered off, and then dried under vacuum to obtain a solid catalyst component, which was recorded as CE-6.
[0448] (2) Propylene polymerization A
[0449] Propylene polymerization was carried out according to the propylene polymerization method A of Example 24, except that the solid catalyst component was replaced by CE-6 in place of E-24, thereby producing polypropylene, which was designated as CP-6A.
[0450] Propylene Polymerization B
[0451] Propylene polymerization was carried out according to the propylene polymerization method B of Example 24, except that the solid catalyst component was replaced by CE-6 in place of E-24, thereby producing polypropylene, which was designated as CP-6B.
[0452] Comparative Example 7
[0453] (1) Preparation of solid catalyst component
[0454] In a 5-liter autoclave, 1.0 liter of hexane, 16 mmol of triethylaluminum, 0.3 mmol of cyclohexylmethyldimethoxysilane, and 25.0 g of catalyst component A-13 were added, and the mixture was reacted at 22°C for 10 minutes. Then, 10 g of ethylene and 2 g of hydrogen were added, and the mixture was reacted at 15°C for 10 minutes. The unreacted gas was vented. The liquid in the reaction product was filtered off and dried under vacuum to obtain a solid catalyst component, which was designated as CE-7.
[0455] (2) Propylene polymerization A
[0456] The same propylene polymerization A as in Example 24 was carried out except that CE-7 was used instead of E-24 to obtain polypropylene, which was designated as CP-7A.
[0457] Propylene Polymerization B
[0458] The same propylene polymerization B as in Example 24 was carried out except that CE-7 was used instead of E-24 to obtain polypropylene, which was designated as CP-7B.
[0459] Comparative Example 8
[0460] (1) Preparation of solid catalyst component
[0461] In a 5 L autoclave, 1.0 L of hexane, 16 mmol of triethylaluminum, 0.3 mmol of cyclohexylmethyldimethoxysilane and 25.0 g of catalyst component A-13 were added and reacted at 22°C for 10 minutes. Then, 10 g of propylene and 2 g of hydrogen were added and reacted at 15°C for 10 minutes. The unreacted gas was vented. The liquid in the reaction product was filtered off and dried under vacuum to obtain a solid catalyst component, which was recorded as CE-8.
[0462] (2) Propylene polymerization A
[0463] The same propylene polymerization A as in Example 24 was carried out except that CE-8 was used instead of E-24 to obtain polypropylene, which was designated as CP-8A.
[0464] Propylene Polymerization B
[0465] The same propylene polymerization B as in Example 24 was carried out except that CE-8 was used instead of E-24 to obtain polypropylene, which was designated as CP-8B.
[0466] Table 1 Titanium Ti2p of solid catalyst component 3 / 2 Electron binding energy Note: The “-” in Table 1-3 does not have the third characteristic peak.
[0467] Table 2 Ti2p of titanium in catalyst components and solid catalyst components 3 / 2 Electron binding energy
[0468] Table 3 Ti2p of titanium in catalyst components and solid catalyst components 3 / 2 Electron binding energy
[0469] Table 4 Propylene polymerization results
[0470] Table 5 Propylene polymerization properties
[0471] Table 6 Propylene polymerization results
[0472] It can be seen from Table 1-3 that the titanium component Ti2p in the solid catalyst component prepared by the preparation method of the present invention is3 / 2 The electron binding energy has changed, with unique characteristic peaks, which will lead to changes in its olefin polymerization properties.
[0473] As can be seen from Tables 4-6, the solid catalyst component of the present invention exhibits high polymerization activity for olefin polymerization, meeting the requirements of industrial application. Compared with existing prepolymerized catalyst technologies, as shown in Comparative Examples 1-8, the attenuation of polymerization activity after one year of storage is significantly reduced, providing a prepolymerized catalyst with stable polymerization activity for the industrial production of polypropylene. The solid catalyst component of the present invention exhibits the advantage of low polymer fines content for olefin polymerization.
[0474] The specific surface area of catalyst E1 of Example 1 is 20.2 m 2 / g, pore volume 0.026cm 3 / g, the pore diameter is 5.1nm, and the specific surface area of the catalyst CE1 of comparative example 1 is 24.3m 2 / g, pore volume 0.022cm 3 / g, pore size is 5.5nm.
[0475] The specific surface area of catalyst E11 of Example 11 is 31.5 m 2 / g, pore volume 0.035cm 3 / g, the pore diameter is 4.4nm, and the specific surface area of the catalyst CE3 of comparative example 3 is 32.1m 2 / g, pore volume 0.034cm 3 / g, and the pore size is 4.9nm.
[0476] A comparison shows that the specific surface area, pore volume, and pore diameter of the catalysts in the two groups of Examples and Comparative Examples are not significantly different and can be considered to be approximately the same. The specific surface area, pore volume, and pore diameter of the catalyst prepared by the method of the present invention using catalyst component A in the preparation examples of the present invention and the catalyst prepared by the method of the Comparative Example are also similar. Therefore, the slow activity decay of the catalyst of the present invention is not significantly correlated with the specific surface area, pore volume, and pore diameter of the catalyst.
[0477] The XRD patterns of solid catalyst component E-1 (top) of Example 1 and solid catalyst component CE-1 (bottom) of Comparative Example 1 are shown in Figure 1. As can be seen from the figure, the XRD patterns of the catalysts are almost identical. The XRD patterns of catalyst component A in the preparation examples of the present invention, prepared according to the method of the present embodiment, and the catalyst prepared according to the method of the comparative example are also almost identical. Therefore, the slow activity decay of the catalyst of the present invention is not significantly correlated with the characteristic XRD peaks of the catalyst.
[0478] Meanwhile, the composition of the solid catalyst component of the example was tested and no detectable amount of Group IVB elements other than Ti was found.
[0479] The XPS peak fitting diagrams of the solid catalyst component E-1 (above) of Example 1 and the solid catalyst component CE-1 (below) of Comparative Example 1 are shown in FIG2 , wherein the dotted line is the fitted peak shape. As can be seen from the figure, the catalyst CE1 of Comparative Example 1 has a high peak at Ti2p 3 / 2 There are two fitting peaks in the solid catalyst component E-1 of Example 1. 3 / 2 There are three characteristic peaks in the solid catalyst component of the embodiment of the present invention. 3 / 2 There are three characteristic peaks in the solid catalyst component of the comparative example. 3 / 2 There are only two characteristic peaks in the XPS spectrum, as shown in Tables 1-3. Therefore, the slow activity decay of the catalyst of the present invention is correlated with the three characteristic peaks in the XPS spectrum of the catalyst.
[0480] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation of the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein. On the contrary, the present invention can be extended to all other methods and applications with the same function.
Claims
1. A solid catalyst component for olefin polymerization, characterized in that The solid catalyst component includes magnesium, titanium, halogen, poly-α-olefin and internal electron donor, wherein the Ti2p spectrum obtained by XPS analysis of the solid catalyst component is peak separated by Gauss-Lorentz peak fitting, and the peak separation results show that Ti2p 3 / 2 The spectrum peak of the orbital has at least three characteristic peaks at the electron binding energy of 459.9eV-454.9eV; The Gaussian-Lorentz peak fitting method is as follows: set the ratio of Lorentz to Gaussian to 30%, Ti2p 1 / 2 The electron binding energy of the spectral peak of the orbital is related to the Ti2p 3 / 2 The electron binding energy difference of the spectral peak of the orbital is 5.9eV, and the Ti2p 1 / 2 The half-maximum width of the spectrum peak of the orbital is Ti2p 3 / 2 1.7 times the half-maximum width of the spectrum peak of the orbital, Ti2p 1 / 2 The peak height of the orbital spectrum is Ti2p 3 / 2 The peak height of the spectrum of the orbital is 0.28 times, and Ti2p 3 / 2 The characteristic peaks of the spectrum of the orbital have the same half-maximum width.
2. The solid catalyst component according to claim 1, wherein The Ti2p 3 / 2 The spectrum peak of the orbital has three characteristic peaks at the electron binding energy of 459.9eV-454.9eV. According to the electron binding energy from high to low, the three characteristic peaks are named the first characteristic peak, the second characteristic peak, and the third characteristic peak. The electron binding energy of the first characteristic peak is 459.9eV-458.97eV, the electron binding energy of the second characteristic peak is 458eV-457.45eV, and the electron binding energy of the third characteristic peak is 456.2eV-454.9eV. And / or, the Ti2p of the solid catalyst component 1 / 2 The electron binding energy of the orbital peak is 467eV-462eV.
3. The solid catalyst component according to claim 2, wherein The ratio of the peak area of the third characteristic peak to the sum of the peak areas of the first characteristic peak, the second characteristic peak and the third characteristic peak is 5-20%, preferably 5-15%.
4. The solid catalyst component according to any one of claims 1 to 3, wherein The solid catalyst component does not contain detectable amounts of Group IVB elements other than Ti.
5. The solid catalyst component according to any one of claims 1 to 4, wherein The poly α-olefin is selected from poly C2-C 10 The olefin is preferably one or more of polyethylene, polypropylene, polybutene, polyoctene and polyisoprene, more preferably polypropylene.
6. The solid catalyst component according to any one of claims 1 to 4, wherein The internal electron donor is at least one of a glycol ester compound, a 1,3-diether compound, and a carboxylic acid ester; Preferably, the diol ester compound has a chemical structure shown in formula (1): In formula (1), R1-R6 are the same or different and are independently selected from hydrogen, amino, C1-C 10 Straight chain alkyl, C3-C 10 Branched alkyl, C3-C 10 Cycloalkyl, C6-C 10 Aryl, C7-C 10 Alkaryl and C7-C 10 Aralkyl; two or more groups in R1-R6 are optionally bonded to each other to form one or more condensed ring structures; R7 and R8 are the same or different and are independently selected from C1-C 10 Straight chain alkyl, C3-C 10 Branched alkyl, C3-C 20 Cycloalkyl, C6-C 20 Aryl, C7-C 20 Alkaryl and C7-C 20 Aralkyl; Preferably, the 1,3-diether compound has a chemical structure shown in formula (2): In formula (2), R1 and R2 are the same or different and are independently selected from hydrogen, C1-C 20 Straight chain alkyl, C3-C 10 Branched alkyl, C3-C 20 Cycloalkyl, C6-C 20 Aryl, C7-C 20 Arylalkyl and C7-C 20 R1 and R2 are optionally bonded to each other to form a fused ring structure, R3 and R4 are the same or different and are independently selected from C1-C 10 of alkyl.
7. The solid catalyst component according to claim 6, wherein The diol ester compound is selected from 1,3-propylene glycol dibenzoate, 2-methyl-1,3-propylene glycol dibenzoate, 2-ethyl-1,3-propylene glycol dibenzoate, 2,2-dimethyl-1,3-propylene glycol dibenzoate, 1,3-diphenyl-1,3-propylene glycol dibenzoate, 1,3-diphenyl-1,3-propylene glycol dipropionate, 1,3-diphenyl-2-methyl-1,3-propylene glycol dipropionate, 1,3-diphenyl-2-methyl-1,3-propylene glycol diacetate, 1,3-diphenyl-2,2-dimethyl-1,3-propylene glycol dibenzoate, 1,3-diphenyl-2,2-dimethyl-1,3-propylene glycol dipropionate, 1,3-di-tert-butyl-2-ethyl-1,3 -propylene glycol dibenzoate, 1,3-diphenyl-1,3-propanediol diacetate, 1,3-diisopropyl-1,3-propanediol di(4-butylbenzoate), 1-phenyl-2-amino-1,3-propanediol dibenzoate, 1-phenyl-2-methyl-1,3-butanediol dibenzoate, 2,4-pentanediol dibenzoate, 3-butyl-2,4-pentanediol dibenzoate, 3,3-dimethyl-2,4-pentanediol dibenzoate, 2,4-pentanediol di(p-toluic acid) ester, 2,4-pentanediol di(p-tert-butylbenzoic acid) ester, 2,4-pentanediol di(p-butylbenzoic acid) ester, 2-methyl-1,3-pentanediol di(p-toluic acid) ester, 2-butyl-1,3-pentanediol di(p- benzoate, 2-methyl-1,3-pentanediol di(p-tert-butylbenzoate), 2-methyl-1,3-pentanediol pivalate, 2,2-dimethyl-1,3-pentanediol dibenzoate, 2-ethyl-1,3-pentanediol dibenzoate, 2-butyl-1,3-pentanediol dibenzoate, 2-methyl-1,3-pentanediol dibenzoate, 2-ethyl-1,3-pentanediol dibenzoate, 2-propyl-1,3-pentanediol dibenzoate, 2-butyl-1,3-pentanediol dibenzoate, 3-ethyl-3,5-heptanediol dibenzoate, 4-ethyl-3,5-heptanediol dibenzoate, 3-propyl-3,5-heptanediol dibenzoate, 4-propyl-3,5-heptanediol dibenzoate Ester, 3-butyl-3,5-heptanediol dibenzoate, 2,3-dimethyl-3,5-heptanediol dibenzoate, 2,4-dimethyl-3,5-heptanediol dibenzoate, 2,5-dimethyl-3,5-heptanediol dibenzoate, 4,4-dimethyl-3,5-heptanediol dibenzoate, 4,5-dimethyl-3,5-heptanediol dibenzoate, 4,6-dimethyl-3,5-heptanediol dibenzoate, 6,6-dimethyl-3,5-heptanediol dibenzoate, 2-methyl-3-ethyl-3,5-heptanediol dibenzoate, 2-methyl-4-ethyl-3,5-heptanediol dibenzoate, 2-methyl-5-ethyl-3,5-heptanediol dibenzoate, 3-methyl-4-ethyl-3,At least one of 5-heptanediol dibenzoate, 3-methyl-5-ethyl-3,5-heptanediol dibenzoate, 4-methyl-3-ethyl-3,5-heptanediol dibenzoate and 4-methyl-4-ethyl-3,5-heptanediol dibenzoate; And / or, the 1,3-diether compound is selected from 2-(2-ethylhexyl)-1,3-dimethoxypropane, 2-isopropyl-1,3-dimethoxypropane, 2-butyl-1,3-dimethoxypropane, 2-sec-butyl-1,3-dimethoxypropane, 2-cyclohexyl-1,3-dimethoxypropane, 2-phenyl-1,3-dimethoxypropane, 2-(2-phenylethyl)-1,3-dimethoxypropane, 2-(2-cyclohexylethyl)-1,3-dimethoxypropane, 2-(p-chlorophenyl)-1,3-dimethoxypropane, 2-(diphenylmethyl)-1,3-dimethoxypropane, 2,2-dicyclohexyl-1,3-dimethoxy Propane, 2,2-dicyclopentyl-1,3-dimethoxypropane, 2,2-diethyl-1,3-dimethoxypropane, 2,2-dipropyl-1,3-dimethoxypropane, 2,2-diisopropyl-1,3-dimethoxypropane, 2,2-dibutyl-1,3-dimethoxypropane, 2-methyl-2-propyl-1,3-dimethoxypropane, 2-methyl-2-benzyl-1,3-dimethoxypropane, 2-methyl-2-ethyl-1,3-dimethoxypropane, 2-methyl-2-isopropyl-1,3-dimethoxypropane, 2-methyl-2-phenyl-1,3-dimethoxypropane, 2-methyl-2-cyclohexyl-1,3-dimethoxypropane, 2,2-bis(2-cyclohexylethyl)-1,3-dimethoxypropane, 2-methyl-2-isobutyl-1,3-dimethoxypropane, 2-methyl-2-(2-ethylhexyl)-1,3-dimethoxypropane, 2,2-diisobutyl-1,3-dimethoxypropane, 2,2-diphenyl-1,3-dimethoxypropane, 2,2-dibenzyl-1,3-dimethoxypropane, 2,2-bis(cyclohexylmethyl)-1,3-dimethoxypropane, 2-isobutyl-2-isopropyl-1,3-dimethoxypropane, 2-(1-methylbutyl)-2-isopropyl-1,3-dimethoxypropane, 2-isopropyl-2-isopentyl-1,3-dimethoxypropane At least one of 2-phenyl-2-isopropyl-1,3-dimethoxypropane, 2-phenyl-2-sec-butyl-1,3-dimethoxypropane, 2-benzyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclopentyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclopentyl-2-sec-butyl-1,3-dimethoxypropane, 2-cyclohexyl-2-isopropyl-1,3-dimethoxypropane, 2-cyclohexyl-2-sec-butyl-1,3-dimethoxypropane, 2-isopropyl-2-sec-butyl-1,3-dimethoxypropane, 2-cyclohexyl-2-cyclohexylmethyl-1,3-dimethoxypropane and 9,9-dimethoxymethylfluorene.
8. The solid catalyst component according to claim 6, wherein The carboxylate is an aliphatic carboxylate and / or an aromatic carboxylate; preferably, the carboxylate is one or more of a benzoate compound, a phthalate compound, and a succinate compound; Preferably, the benzoate compound is selected from one or more of methyl benzoate, ethyl benzoate and n-butyl benzoate; Preferably, the phthalate compound is selected from one or more of diethyl phthalate, diisobutyl phthalate, di-n-butyl phthalate, diisooctyl phthalate and di-n-octyl phthalate; Preferably, the succinate compound is selected from one or more of diethyl 2,3-diisopropylsuccinate, diisobutyl 2,3-diisopropylsuccinate, di-n-butyl 2,3-diisopropylsuccinate, dimethyl 2,3-diisopropylsuccinate, diisobutyl 2,2-dimethylsuccinate, diisobutyl 2-ethyl-2-methylsuccinate and diethyl 2-ethyl-2-methylsuccinate.
9. The solid catalyst component according to any one of claims 1 to 8, wherein The internal electron donor includes an internal electron donor a and an internal electron donor b, and the internal electron donor a and the internal electron donor b are: Option I: The internal electron donor a is selected from the diol ester compound, and the internal electron donor b is selected from 1,3-diether compounds and optional carboxylic acid esters; Option II: The internal electron donor a is selected from the 1,3-diether compound, and the internal electron donor b is selected from the phosphate compound represented by formula (3); In formula (3), R5, R6 and R7 are the same or different and are independently selected from C1-C4 straight chain alkyl, C3-C4 branched chain alkyl, C3-C 20 Cycloalkyl, C6-C 20 Aryl, C7-C 20 Alkaryl and C7-C 20 Aralkyl; Preferably, the phosphate compound is selected from at least one of trimethyl phosphate, triethyl phosphate, tributyl phosphate, triphenyl phosphate, tricresyl phosphate, triisopropylphenyl phosphate, phenyl dimethyl phosphate, cresyl dibutyl phosphate, isopropylphenyl dimethyl phosphate, isopropylphenyl diethyl phosphate, isopropylphenyl dibutyl phosphate, phenyl ditolyl phosphate, phenyl diisopropylphenyl phosphate, p-cresyl dibutyl phosphate, m-cresyl dibutyl phosphate, p-cumyl dimethyl phosphate, p-cumyl diethyl phosphate, p-tert-butylphenyl dimethyl phosphate and o-cresyl p-di-tert-butylphenyl phosphate.
10. The solid catalyst component according to claim 9, wherein The mass ratio of the internal electron donor a to the internal electron donor b is 0.1:1-1000:
1.
11. The solid catalyst component according to any one of claims 1 to 10, wherein Based on the total weight of the solid catalyst component, the content of magnesium in the solid catalyst component is 1-18 weight percent; the content of titanium is 0.1-3.5 weight percent; the content of halogen is 2-65 weight percent; the content of polyalphaolefin is 0.1-89 weight percent; and the content of internal electron donor is 0.6-15 weight percent.
12. A method for preparing a solid catalyst component for olefin polymerization, characterized in that: The method includes: (1) in the presence of an inert solvent, a catalyst component A, an alkyl aluminum, and an external electron donor are contacted to react; the catalyst component A contains titanium, magnesium, a halogen, and an internal electron donor; (2) mixing the reaction system obtained in step (1) with an α-olefin to carry out a polymerization reaction; (3) removing the unreacted α-olefin in step (2), and adding hydrogen to the resulting reaction system to carry out the reaction.
13. The method according to claim 12, wherein: The molar ratio of the alkyl aluminum, the external electron donor compound and the catalyst component A calculated as titanium element is 1-50:0.2-10:1; and / or, the number of alkyl groups in the alkylaluminum is 1-3, and the number of carbon atoms in the alkyl group is C1-C8, more preferably, the alkylaluminum is selected from one or more of triethylaluminum, triisobutylaluminum, tri-n-butylaluminum, tri-n-hexylaluminum and diethylaluminum monochloride; and / or, the external electron donor compound is selected from at least one silicon-containing compound, preferably one or more selected from cyclohexylmethyldimethoxysilane, diisopropyldimethoxysilane, n-butyldimethoxysilane, diisobutyldimethoxysilane, diphenyldimethoxysilane, methyl-tert-butyldimethoxysilane and dicyclopentyldimethoxysilane; and / or, the internal electron donor comprises at least one of a glycol ester compound, a 1,3-diether compound, and a carboxylic acid ester; And / or, the α-olefin is selected from C2-C 10 The olefin is preferably one or more of ethylene, propylene, butene, octene and isopentene, more preferably propylene.
14. The method according to claim 12 or 13, wherein: In step (1), the reaction conditions include: temperature of 0-30°C, preferably 15-25°C; time of 1-30 min, preferably 10-20 min; And / or, in step (2), the polymerization reaction conditions include: temperature of 0-50°C, preferably 15-25°C; time of 5-30 min, preferably 10-20 min; And / or, in step (3), the reaction conditions include: temperature of 0-50°C, preferably 15-25°C; time of 5-30 min, preferably 10-20 min; and / or, in step (3), controlling the amount of hydrogen added to maintain the reaction pressure at 0.01-1 MPa; And / or, in step (2), the mass ratio of the α-olefin to the catalyst component A is 0.04-10:
1.
15. A solid catalyst component prepared by the method according to any one of claims 12 to 14.
16. A catalyst system for olefin polymerization, characterized in that: The catalyst system comprises the solid catalyst component according to any one of claims 1 to 11 and / or the solid catalyst component prepared by the method according to any one of claims 12 to 14, an alkyl aluminum and an optional external electron donor compound or a reaction product thereof.
17. Use of the solid catalyst component according to any one of claims 1 to 11 and / or the solid catalyst component prepared by the method according to any one of claims 12 to 14 and / or the catalyst system according to claim 16 in olefin polymerization.
18. A method for olefin polymerization, characterized in that: The method comprises: polymerizing olefins in the presence of the solid catalyst component according to any one of claims 1 to 11 and / or the solid catalyst component prepared by the method according to any one of claims 12 to 14 and / or the catalyst system according to claim 16; Preferably, the general formula of the olefin is CH2=CHR, R is hydrogen or C1-C6 alkyl or C6-C 10 aryl; Preferably, the polymerization temperature is 0-150°C, more preferably 60-90°C.