Method for manufacturing acidic gas adsorbent
Patent Information
- Application Number
- MYPI2025002699
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-11-16
- Filing Date
- 2023-11-14
- Publication Date
- 2024-05-16
AI Technical Summary
Existing acidic gas adsorbents fail to meet practical requirements for ventilation differential pressure, crushing strength, water resistance, and open porosity, making them unsuitable for efficient and continuous treatment of acidic exhaust gases in thermal power plants and waste incineration facilities.
A method involving granulation of layered double hydroxide (LDH) with a silicic acid binder and water to form pellet-like or spherical granules, followed by heat treatment, which includes the use of a foaming agent like perlite or obsidian to enhance porosity and strength, ensuring the adsorbent maintains crushing strength and water resistance while achieving required dynamic adsorption.
The method produces an acidic gas adsorbent with improved ventilation differential pressure, crushing strength, and open porosity, enabling effective and continuous adsorption of acidic gases without disintegration, even under water exposure, thus addressing the limitations of previous technologies.
Smart Images

Figure PI2025002699_DRAWING_001
Abstract
Description
Method for manufacturing acid gas adsorbent
[0001] The present invention relates to a method for producing an acidic gas adsorbent, and more particularly to a method for producing an acidic gas adsorbent that efficiently removes acidic exhaust gases generated from thermal power plants, waste incineration facilities, and the like.
[0002] Combustion exhaust gases generated in thermal power plants, waste incineration, etc. contain harmful acidic substances such as hydrogen chloride, sulfur oxides, nitrogen oxides, etc. Therefore, various methods are used to treat acidic exhaust gases containing the acidic substances in order to remove the acidic substances.
[0003] In relation to such methods for removing acidic substances, the present applicant has proposed an efficient treatment technology capable of simultaneously treating and removing multiple types of acidic substances, and has proposed a method and treatment agent for treating acidic exhaust gases that utilizes a carbonate-type Mg—Al-based layered double hydroxide (hereinafter, layered double hydroxide is also referred to as LDH (Layered Double Hydroxide)) as an acidic gas adsorbent (Patent Document 1).
[0004] A carbonate-type Mg—Al-based LDH is an acidic gas adsorbent that can be regenerated and reused. Patent Document 1 relates to a method for regenerating a carbonate-type Mg—Al-based LDH, and discloses a technique for converting an anionic Mg—Al-based LDH that has been used in acidic exhaust gas treatment into an anionic Mg—Al-based LDH by mixing it with an aqueous carbonate solution.
[0005] The present applicant has disclosed another regeneration technology in which anionic Mg-A-based LDH is regenerated into carbonate Mg-Al-based LDH by utilizing gas obtained by treating acidic exhaust gas and removing acidic gases other than carbon dioxide (Patent Document 2).
[0006] Patent Document 2 describes a technology for efficiently performing the removal of acidic exhaust gases using an acidic gas adsorbent and the regeneration treatment of the acidic gas adsorbent within the same reaction tower. Specifically, the technology involves packing a carbonate Mg-Al-based LDH into a reaction tower, passing acidic exhaust gas through it to adsorb and remove the acidic gases, and when the carbonate Mg-Al-based LDH changes to an anionic Mg-A-based LDH and the acidic exhaust gas treatment capacity decreases, operating a selector valve to switch the destination of the acidic exhaust gas to another reaction tower, and introducing the treated gas into a reaction tower packed with anionic Mg-A-based LDH for regeneration treatment.
[0007] Patent No. 6954569 Patent No. 6898627
[0008] As in the regeneration treatment method of Patent Document 2, an acid gas adsorbent that is packed into a reaction tower and regenerated in the reaction tower by contact with water containing a specified gas must satisfy the following requirements, but no method for producing an acid gas adsorbent that satisfies all of the following requirements has been put into practical use. (Requirement 1) The adsorbent has a shape that ensures a practical level of differential pressure when acidic exhaust gas or regeneration gas is passed through the reaction tower. (Requirement 2) The adsorbent has a crushing strength that prevents it from collapsing even when packed into a reaction tower and compacted. (Requirement 3) The adsorbent has water resistance that prevents it from collapsing even when contacted with water during regeneration treatment. (Requirement 4) The adsorbent has an open porosity that allows it to achieve the dynamic adsorption amount required when continuously passing acidic exhaust gas through the reaction tower.
[0009] For example, there is a trade-off between the open porosity (requirement 4) and the crushing strength (requirement 2) or the water resistance (requirement 3), and it has been thought that it would be difficult to develop an acidic gas adsorbent that satisfies all of the above requirements.
[0010] An object of the present invention is to provide a method for producing an acidic gas adsorbent that satisfies the above requirements.
[0011] As a result of extensive research, the present inventors have found that the above-mentioned problems can be solved by granulating the powder into a specific shape and then hardening it by heat treatment. The present invention is based on this finding.
[0012] The present invention provides the following [1] to [5]. [1] A method for producing an acidic gas adsorbent, comprising a granulation step of adding a silicic acid binder and water to a layered double hydroxide to form pellet-shaped or spherical granules having a particle size of 1 to 10 mm, and a heat treatment step of heat-treating the granules to harden them. [2] The method for producing an acidic gas adsorbent according to [1], wherein the granules are granulated by further adding a blowing agent in the granulation step. [3] The method for producing an acidic gas adsorbent according to [1] or [2], wherein the blowing agent is perlite or obsidian. [4] The method for producing an acidic gas adsorbent according to any of [1] to [3], wherein the silicic acid binder is sodium metasilicate. [5] The method for producing an acidic gas adsorbent according to any of [1] to [4], wherein the heat treatment temperature in the heat treatment step is 150 to 600°C. [6] The method for producing an acidic gas adsorbent according to [1], wherein the silicic acid binder is an aqueous solution of sodium metasilicate. [7] The method for producing an acidic gas adsorbent according to [6], wherein the concentration of the aqueous sodium metasilicate solution is 1 to 12 mass%. [8] The method for producing an acidic gas adsorbent according to [1], wherein the granulation is carried out by at least one granulation method selected from the group consisting of a tumbling granulation method, a mixing and stirring granulation method, an extrusion granulation method, a compression granulation method, and a fluidized bed granulation method. [9] The method for producing an acidic gas adsorbent according to [1], wherein the pellet-shaped granules are granulated by an extrusion granulation method.
[10] The method for producing an acidic gas adsorbent according to [1], wherein the spherical granules are granulated by an extrusion granulation method.
[0013] According to the present invention, a method for producing an acidic gas adsorbent can be provided, which has a shape that allows the aeration differential pressure when acidic exhaust gas or regeneration gas is passed through a reaction tower to be at a practical level, has a crushing strength that prevents collapse even when packed into a reaction tower and compacted, has water resistance that prevents collapse even when contacted with water during regeneration treatment, and has an open porosity that allows the dynamic adsorption amount required for continuous aeration of acidic exhaust gas to be achieved.
[0014] According to the invention of claim 2, LDH is mixed with a silicate binder, a blowing agent, and water, and then granulated to obtain pellet-shaped or spherical granules having a particle size of 1 to 10 mm. Heat-treating the pellet-shaped or spherical granules hardens the silicate binder, improving water resistance, and causes the blowing agent to foam, improving open porosity. This promotes intragranular diffusion of acidic gases, thereby increasing the dynamic adsorption amount of acidic gases. An acidic gas adsorbent made of granulated LDH obtained by the method of claim 2 maintains a crushing strength of 4N or more despite the improved open porosity. In this specification, granulated LDH refers to the granules obtained in the granulation step that have been heat-treated and hardened, and is synonymous with acidic gas adsorbent. Assuming the packed height of the actual reactor is 3 m and the particle size of the granulated LDH is 5 mm, the load on the granulated LDH below the packed bed is 0.34 N. With a safety factor of 10, a crushing strength of 4N or more of granulated LDH can be considered sufficient for practical use. In this specification, the open porosity means the volume / mass % of the volume of the voids (pores) inside the granulated LDH that are connected to the outside air relative to the mass of the granulated LDH.
[0015] 1 is a photograph showing the results of evaluating water resistance in Example 1, Example 2, and Comparative Example 1.
[0016] An embodiment of the present invention will be described in detail below. In the following description, the expression "A to B" indicating a range of numerical values means "A or more and B or less", including the endpoints.
[0017] The present invention includes a granulation step in which a layered double hydroxide (LDH) is added with a silicic acid binder and water to form pellet-shaped or spherical granules having a particle size of 1 to 10 mm, and a heat treatment step in which the granules are heat-treated to harden them.
[0018] <Granulation Step> [LDH] The LDH is preferably a powdered carbonate Mg—Al-based layered double hydroxide. The particle size of the powdered carbonate Mg—Al-based layered double hydroxide is preferably in the range of 0.004 to 0.1 mm. A particle size within this range allows for uniform mixing with the blowing agent described below.
[0019] [Silicate Binder] The silicic acid binder is preferably sodium metasilicate. Monosilicic acid is known to have a strong interaction with Mg and Al. Sodium metasilicate readily dissolves in water to form highly reactive monosilicic acid. Adding sodium metasilicate and water causes the Mg-Al layered double hydroxide to react with the monosilicic acid, which then polymerizes to form polysilicic acid. As the polymerization progresses, crushing strength and water resistance can be imparted, resulting in granulated LDH that does not collapse when packed into a reaction column and compacted, and does not crack or collapse when immersed in water. While sodium metasilicate and water may be added separately, from the viewpoint of uniform mixing and dispersion, it is preferable to add sodium metasilicate as an aqueous solution dissolved in water. The concentration of the sodium metasilicate aqueous solution is not particularly limited, but is preferably 1 to 12 mass%.
[0020] [Foaming Agent] In the granulation step, it is preferable to further add a foaming agent to granulate the granules. The foaming agent is preferably perlite or obsidian. Perlite and obsidian are minerals that are used as raw materials for perlite and have the property of foaming when heated at high temperatures. By heating granules granulated by mixing perlite or obsidian with LDH, the foaming action of the perlite or obsidian increases the open porosity of the granulated LDH. The dynamic adsorption amount when acidic exhaust gas is continuously passed through the granulated LDH depends on the intragranular open porosity of the granulated LDH. Increasing the open porosity of the granulated LDH increases the diffusibility of acidic gases within the granulated LDH, allowing for effective adsorption of acidic gases.
[0021] [Granulation Method] The method for granulating the pellet-shaped or spherical granules is not particularly limited, and examples thereof include a rolling granulation method using a drum granulator, a dish granulator, etc.; a mixing and stirring granulation method using a Flexomix, a vertical granulator, etc.; an extrusion granulation method using a screw extrusion granulator, a roll extrusion granulator, a blade extrusion granulator, a self-molding extrusion granulator, etc.; a compression granulation method using a tableting granulator, a briquette granulator, etc.; and a fluidized bed granulation method in which a titanate powder and a binder are kept suspended in a blown-up fluid (mainly air) while a binder such as water or alcohol is sprayed onto the powder to form granules. Of these, extrusion granulation is preferred when forming pellets, and rolling granulation or mixing and stirring granulation is preferred when forming spherical powders.
[0022] [Particle size] The size of the granules granulated in the granulation step is 1 to 10 mm. By setting the particle size to 1 mm or more, the ventilation differential pressure when venting acidic exhaust gas or regeneration gas into the reaction tower can be kept at a practical level. Specifically, excessive pressure loss when venting the reaction tower can be avoided, and blower power consumption can be reduced. By setting the particle size to 10 mm or less, a decrease in adsorption capacity due to a small surface area can be avoided, and the adsorption capacity for acidic gases can be maintained at a good level. Here, the particle size of the granules corresponds to the diameter if the granules are spherical, and in the case of pellets, it means the length of the part where the gap between the plates is the widest when the granules are sandwiched between two parallel plates (the gap between the two plates). Granules with a particle size of 1 to 10 mm are granules that do not pass through a sieve with a 1 mm mesh size but pass through a 10 mm mesh size sieve.
[0023] <Heat Treatment Step> By adding a silicate binder and water to LDH, mixing the mixture, granulating the mixture, and then heat-treating the mixture, the binder hardens to form granulated LDH with a crushing strength that does not collapse even when contacted with water during regeneration, and does not collapse even when a load is applied when the LDH is filled into a reaction tower. Furthermore, by adding a silicate binder, a blowing agent, and water to LDH, mixing the mixture, granulating the mixture, and then heat-treating the mixture, the blowing agent foams, increasing the open porosity of the granulated LDH and increasing the dynamic adsorption amount of acidic gases.
[0024] The heat treatment temperature in the heat treatment step is preferably 150 to 600°C. The heat treatment atmosphere may be either an air atmosphere or a nitrogen atmosphere. The foaming of perlite or obsidian is due to the volatilization of water contained in the perlite or obsidian. By setting the heat treatment temperature to 150°C or higher, sufficient water volatilization occurs to promote foaming. By setting the heat treatment temperature to 600°C or lower, the phenomenon in which the LDH crystals change from a layered structure to a spinel structure is suppressed, the deactivation of ion exchange ability due to the change in the crystal structure is avoided, and the function of adsorbing acidic gases can be well maintained.
[0025] Next, specific examples of the present invention will be described, but the present invention is not limited to these examples.
[0026] Example 1: LDH + Sodium Metasilicate + Perlite 200 g of powdered carbonate-type LDH (Kyowa Chemical Industry Co., Ltd., Kyoward 1000) and 30 g of perlite (Mikata, Hyogo Prefecture) were mixed in a mixing and stirring granulator (trade name "VG-01", manufactured by Powrex) at a rotation speed of 400 rpm, and 220 g of a 12% by weight aqueous solution of sodium metasilicate was slowly added, followed by tumbling granulation to grow particles in a snowball-like manner. The obtained coarse granules were further added to a wet extrusion granulator (trade name "Multigran MG-55", manufactured by Dalton) equipped with a 2.5 mm diameter die to produce granulated pellets. The obtained granulated pellets were spheronized using a spheronizer (trade name "Marmerizer QJ-230T", manufactured by Dalton), and the spheroidized bodies were dried at 200 ° C. for 4 hours to obtain granulated LDH1 having a particle size of 2.0 to 3.0 mm.
[0027] Example 2: LDH + Sodium Metasilicate 200 g of powdered carbonate-type LDH (Kyowa Chemical Industry Co., Ltd., Kyoward 1000) was placed in a mixing and stirring granulator (trade name "VG-01", manufactured by Powrex) and stirred at 400 rpm. 200 g of a 12% by mass aqueous solution of sodium metasilicate was slowly added, followed by the addition of 20 g of pure water, followed by tumbling granulation to grow particles in a snowball-like fashion. The resulting coarse granules were further added to a wet extrusion granulator (trade name "Multigran MG-55", manufactured by Dalton) equipped with a 2.5 mm diameter die to produce granulated pellets. The resulting granulated pellets were spheronized using a spheronizer (trade name "Marmerizer QJ-230T", manufactured by Dalton), and the spheroidized bodies were dried at 200°C for 4 hours to obtain granulated LDH2 having a particle size of 2.0 to 3.0 mm.
[0028] Comparative Example 1: LDH 200 g of powdered carbonate-type LDH (Kyowa Chemical Industry Co., Ltd., Kyoward 1000) was placed in a mixing and stirring granulator (trade name "VG-01", manufactured by Powrex), and 175 g of pure water was added while stirring at a rotation speed of 400 rpm, and the particles were grown in a snowball-like manner by rolling granulation. The obtained coarse granules were further granulated using a wet extrusion granulator (trade name "Multigran MG-55", manufactured by Dalton) using a 2.5 mm die to produce granulated pellets. Next, the granulated pellets were spheronized using a spherical spheronizer (trade name "Marumerizer QJ-230T", manufactured by Dalton), and the spheroidized molded bodies were dried at 200 ° C. for 4 hours to obtain granulated LDH3 having a particle size of 2.0 to 3.0 mm.
[0029] <Evaluation 1 - Water Resistance> Granulated LDH1 to 3 were each immersed in pure water, and the presence or absence of disintegration was visually confirmed. Granulated LDH1 (Example 1), which contained sodium metasilicate and perlite, and granulated LDH2 (Example 2), which contained only sodium metasilicate, did not disintegrate even after 9 days of immersion in pure water. On the other hand, granulated LDH3 (Comparative Example 1), which contained neither sodium metasilicate nor perlite, disintegrated immediately upon immersion in water, emitting a noise (see Figure 1). The above evaluation results confirm that the addition of sodium metasilicate improves water resistance.
[0030] <Evaluation 2 - Open Porosity> Open porosity was measured using the following procedure, with reference to "JIS R 1634:1998 - Measuring Methods for Sintered Density and Open Porosity of Fine Ceramics." Three measurements were taken and the average was used for comparison. Step 1. Weigh the empty pycnometer (A). Step 2. Place the sample dried at 110°C into the empty pycnometer and weigh (B). Step 3. Fill the pycnometer with the 110°C dried sample with pure water and weigh (C). Step 4. Transfer the sample to a beaker and boil for at least three hours, then allow to cool. Step 5. After boiling, place the sample in the pycnometer, fill with pure water, and weigh (D). Step 6. Calculate the open porosity using the following formula: Open porosity (%) = (D - C) / (B - A) x 100
[0031] The open porosity of granulated LDH1 (Example 1) and granulated LDH2 (Example 2) was measured, and the results are shown in Table 1. Note that, as shown in the section <Water resistance>, granulated LDH3 (Comparative Example 1) could not be measured because it disintegrated when immersed in pure water and could not be boiled.
[0032]
[0033] From the above evaluation results, it can be confirmed that the open porosity of the granulated LDH increases by using a silicate binder and a foaming agent (perlite) in combination (Example 1).
[0034] <Evaluation 3 - Crushing Strength> The crushing strength of granulated LDH1 (Example 1), granulated LDH2 (Example 2), and granulated LDH3 (Comparative Example 1) was measured using a Kiya hardness tester. The crushing strength of 10 granules was measured and the average was calculated, and the results are shown in Table 2.
[0035]
[0036] The measurement results for all of granulated LDH1 (Example 1), granulated LDH2 (Example 2), and granulated LDH3 (Comparative Example 1) were a crushing strength of 4N or more. As confirmed in the above-mentioned Evaluation 2, it can be confirmed that granulated LDH1 (Example 1) does not experience a decrease in crushing strength despite having a high open porosity. The compatibility of a high open porosity and a crushing strength of 4N or more is thought to be the effect of sodium metasilicate.
[0037] <Evaluation 4 - Dynamic Adsorption Amount> 60 g of each of granulated LDH1 (Example 1) and granulated LDH3 (Comparative Example 1) was packed into a column having an inner diameter of 57 mm and a length of 250 mm, and a simulated acidic gas having a hydrogen chloride concentration of 400 ppm and a temperature of 150° C. was passed through the column at a superficial velocity of 0.4 m / sec. The dynamic adsorption amount was calculated from the time to reach 50% breakthrough using the following formula (1). The results are shown in Table 3.
[0038] q e = 3600 VTC 1 x10 -6 ×273 / (273+t)×M i / 22.4 / Z i ρ (1) In the above formula (1), q e : Dynamic adsorption amount [g-gas / g-granulation LDH], V: superficial velocity [m / s], T: time to reach 50% breakthrough [h], C i : Acid gas concentration [ppm], t: Gas temperature [°C], M i : molecular weight of gas component, Z i : Filled bed height [m], ρ: Granulated LDH packing density [kg / m 3 ].
[0039]
[0040] The dynamic adsorption amount of granulated LDH1 (Example 1) was larger than that of granulated LDH3 (Comparative Example 1). In granulated LDH1 (Example 1), the LDH content was lower by the amount of sodium metasilicate and perlite blended, but as confirmed in Evaluation 2, this is thought to be due to the large open porosity, allowing utilization of the interior of the granulated LDH.
Claims
1. A method for producing an acidic gas adsorbent, comprising a granulation step of adding a silicate binder and water to a layered double hydroxide to form pellet-shaped or spherical granules with a particle size of 1 to 10 mm, and a heat treatment step of heat-treating the granules to harden them.
2. The method for producing an acidic gas adsorbent according to claim 1, wherein in the granulation step, a foaming agent is further added to granulate the granules.
3. The method for producing an acid gas adsorbent according to claim 2, wherein the foaming agent is perlite or obsidian.
4. The method for producing an acid gas adsorbent according to claim 1, wherein the silicate binder is sodium metasilicate.
5. The method for producing an acidic gas adsorbent according to claim 1, wherein the heat treatment temperature in the heat treatment step is 150 to 600°C.
6. The method for producing an acidic gas adsorbent according to claim 1, wherein the silicate binder is an aqueous solution of sodium metasilicate.
7. The method for producing an acidic gas adsorbent according to claim 6, wherein the concentration of the aqueous sodium metasilicate solution is 1 to 12 mass %.
8. The method for producing an acidic gas adsorbent according to claim 1, wherein the granulation is carried out by at least one granulation method selected from the group consisting of rolling granulation, mixing and stirring granulation, extrusion granulation, compression granulation, and fluidized bed granulation.
9. The method for producing an acidic gas adsorbent according to claim 1, wherein the pellet granulation is carried out by extrusion granulation.