Aluminum alloy material, and preparation method therefor and use thereof

MYPI2025002719A0Undetermined Publication Date: 2024-05-09BEIJING CHEHEJIA AUTOMOBILE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025002719
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-11-09
Filing Date
2023-11-08
Publication Date
2024-05-09

AI Technical Summary

Technical Problem

While existing aluminum alloy materials improve strength and conductive properties, they are relatively expensive, and too much Ni and Fe content affects material properties, making it difficult to maintain high strength and high conductivity while reducing costs.

Method used

By forming NiAl3, FeNiAl9 and Fe4Al13 phases in aluminum alloys, controlling their content and α-Al grain size, and combining Ti, Nb, V, Zr and B elements, the microstructure of the material is optimized to improve strength and conductivity, while utilizing Scrap aluminum with high iron content reduces costs.

Benefits of technology

It achieves the high strength, low cost and good electrical conductivity of aluminum alloy materials, and is suitable for the production of automobile parts. The electrical conductivity is ≥48% IACS, the room temperature yield strength is ≥75MPa, the tensile strength is ≥160MPa, and the elongation is ≥10%. And the liquidity is good.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025002719_DRAWING_001
    Figure PI2025002719_DRAWING_001
Patent Text Reader

Abstract

An aluminum alloy material, and a preparation method therefor and a use thereof. In addition to an aluminum matrix, the as-cast structure of the aluminum alloy material also contains an eutectic phase NiAl3, and primary solidification phases FeNiAl9 and Fe4Al13. The aluminum alloy material is obtained by means of smelting, refining, degassing, slag removal and casting of raw materials containing elements. The aluminum alloy material can be cast in the manner of low pressure, differential pressure, extrusion or high pressure, and is suitable for manufacturing automobile parts such as motor rotors, wires, and inverters. FIG. 1
Need to check novelty before this filing date? Find Prior Art

Description

Aluminum alloy material, preparation method and application thereof

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This disclosure is based on and claims the priority of the Chinese patent application with application number 202211398488.9 and application date of November 9, 2022. The entire content of the Chinese patent application is hereby incorporated into this disclosure as a reference. Technical Field

[0003] The present disclosure belongs to the technical field of aluminum alloys, and particularly relates to an aluminum alloy material, a preparation method thereof, and applications thereof. Background Art

[0004] Drive induction motors are evolving toward higher integration, higher voltage, and higher power density. As speeds continue to increase, so too are the performance requirements for rotor materials. Aluminum alloys, with their high specific strength, low cost, and high recyclability, are gradually replacing copper alloys as the primary material for automotive motor rotors. To meet these performance requirements, aluminum alloys must possess both high strength and high electrical conductivity.

[0005] In order to obtain high-strength and high-conductivity cast aluminum alloy materials, alloying is required. US20210332461A1 discloses a cast aluminum rotor material suitable for high-pressure casting, containing 4-6% Ni, 0.2-0.8% Fe, and 0.01-0.1% Ti. Ni is mainly added to form a NiAl3 eutectic phase to improve the castability of the alloy. CN 113981278A discloses a high-conductivity, heat-resistant pressure casting aluminum alloy and its preparation method. The aluminum alloy contains 1.8-3.8% Ni, 0.25-0.30% Fe, 0.006-0.15% Zr, 0.0015-0.025% Cr, and 0.001-0.02% V. High strength and high conductivity are achieved by combining the NiAl3 eutectic phase and trace elements Fe, Zr, Cr, and V to form a high-temperature stable fine and dispersed intermetallic compound. US20220090234A1 discloses a high vacuum die-cast aluminum alloy rotor material, the aluminum alloy contains 1.5-6.5% Ni, 0.1-1.5% Si, 0.1-3% Mg, Fe<0.2%, Mn<0.65%, Ti<0.12%, V<0.15%, Zr<0.15%, Mo<0.15%, Cr<0.01, Sr<0.02, combined with NiAl3 eutectic phase and Mg2Si heat treatment strengthening to improve performance.

[0006] All of the above technologies improve casting properties by adding and regulating the alloying element Ni, while minimizing the impact on electrical conductivity, by forming a NiAl3 eutectic phase. Secondly, trace elements Fe, Zr, Cr, and V are added to form intermetallic compounds or Mg2Si is heat-treated to improve yield strength. However, all of the above technologies have the problem of excessive addition of the main element Ni and too low Fe content, resulting in high material costs. However, changing the Ni and Fe content may affect the strength and electrical conductivity of the aluminum alloy material.

[0007] Therefore, it is necessary to develop an aluminum alloy material that has high strength and high conductivity while reducing costs.

[0008] Summary of the Invention

[0009] The present disclosure aims to provide an aluminum alloy material and its preparation method and application. The aluminum alloy material has the advantages of high strength, high conductivity and low cost.

[0010] To achieve this goal, the present disclosure adopts the following technical solutions:

[0011] In a first aspect, the present disclosure provides an aluminum alloy material, wherein the cast structure of the aluminum alloy material contains, in addition to the aluminum matrix, a eutectic phase NiAl3, a primary solidification phase FeNiAl9 and a primary solidification phase Fe4Al 13 .

[0012] The present invention has found that under low Ni / Fe ratio conditions, in addition to NiAl3 phase and FeNiAl9 phase, Fe4Al 13 phase, which has good thermal stability, helps to inhibit the slip of defects such as high-temperature dislocations, stabilize the performance of aluminum alloy materials, and improve strength. 13 phase, which also indicates that the Ni / Fe ratio in the aluminum alloy is low, which further indicates that the Ni content is small and the Fe content is high, which is beneficial to reduce the cost. 13 The combination of the two phases makes the obtained aluminum alloy material have the advantages of high strength, high conductivity and low cost.

[0013] In some embodiments of the present disclosure, the mass content of the eutectic phase NiAl3 is 0.2-2.2%, the mass content of the primary solidified phase FeNiAl9 is 0.1-1.1%, and the mass content of the primary solidified phase Fe4Al 13 The mass content is 1-6%;

[0014] Furthermore, the α-Al grain size in the aluminum alloy material is less than 100 μm.

[0015] The mass content of the eutectic phase NiAl3 is 0.2-2.2% (for example, it can be 0.2%, 0.5%, 0.8%, 1%, 1.1%, 1.4%, 1.5%, 1.7%, 2% or 2.2%, etc.);

[0016] The mass content of the primary solidified phase FeNiAl9 is 0.1-1.1% (for example, it can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0% or 1.1%, etc.);

[0017] The primary solidification phase Fe4Al 13 The mass content of α-Al is 1-6% (for example, it can be 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5% or 6%, etc.); and the α-Al grain size in the aluminum alloy material is below 100 μm (for example, it can be 100 μm, 95 μm, 90 μm, 85 μm, 80 μm, 75 μm, 70 μm, 65 μm, 60 μm, 50 μm, 40 μm, 30 μm, 20 μm or 10 μm, etc.).

[0018] The eutectic phase NiAl3 helps to improve the fluidity of aluminum alloy materials and make them easier to cast. The NiAl3 content is positively correlated with the amount of Ni added. An increase in NiAl3 content means an increase in Ni content, which means an increase in cost. 13 It can effectively inhibit the dissolution of Fe in the mold. 13 The increase in Fe content means the increase in Fe content, which allows the aluminum alloy provided by the present disclosure to use scrap aluminum with high iron content as raw material, which helps to reduce costs. 13 The thermal stability is good, which helps to inhibit the slip of defects such as high temperature dislocations and stabilize the performance of the material. Therefore, FeNiAl9 and Fe4Al 13 It helps to improve the strength of aluminum alloy materials, but too high a content will split the matrix and reduce the elongation of the material. Refining α-Al grains helps to improve the strength and elongation of the material.

[0019] The present invention discloses a method for rationally regulating the eutectic phase NiAl3, the primary solidification phase FeNiAl9 and Fe4Al 13 Increasing the content of α-Al and refining the α-Al grain size can further optimize the electrical conductivity and strength of the aluminum alloy material while reducing costs.

[0020] In some embodiments of the present disclosure, the aluminum alloy material contains the eutectic phase NiAl3, the primary solidification phase FeNiAl9 and Fe4Al 13In addition, it does not contain any other second phase.

[0021] It should be noted that the other crystalline phases in the aluminum alloy material except the main Al crystalline phase are collectively referred to as "second phases". 13 In the case of other second phases besides aluminum, it may lead to enhanced impurity scattering or matrix fragmentation, thereby affecting the conductivity, strength and other properties of the aluminum alloy material.

[0022] In some embodiments of the present disclosure, the aluminum alloy material includes the following components in mass percentage:

[0023] Ni 0.5%-1.5%, Fe 0.8%-2.5%, one or more of Ti, Nb, V and Zr, and the total mass percentage of Ti, Nb, V and Zr is ≥0.02%, and the balance is Al.

[0024] The mass percentage of Ni may be 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4% or 1.5%, etc.

[0025] The mass percentage of Fe may be 0.8%, 0.9%, 1%, 1.2%, 1.3%, 1.5%, 1.6%, 1.8%, 2%, 2.2%, 2.3% or 2.5%, etc.

[0026] The total mass percentage of Ti, Nb, V and Zr may be 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.11%, 0.12%, 0.13%, 0.14% or 0.15%, etc.

[0027] The present disclosure has found through research that under the Ni / Fe ratio conditions of the present disclosure, in addition to the NiAl3 phase and FeNiAl9 phase, Fe4Al 13 phase, which has good thermal stability, helps to inhibit the slip of defects such as high-temperature dislocations, stabilize the performance of aluminum alloy materials, and improve strength.

[0028] The present invention reduces the Ni content, increases the Fe content, reduces the Ni / Fe ratio, and regulates the eutectic phase NiAl3, the primary solidification phase FeNiAl9 and Fe4Al 13 content; on the other hand, by regulating the grain refining elements (Ti, V, Nb, Zr and B), the α-Al grains can be refined, thereby further optimizing the electrical conductivity and strength of the aluminum alloy material while reducing costs.

[0029] In some embodiments of the present disclosure, the mass ratio of Ni to Fe in the aluminum alloy material is 0.2-1.5; for example, it can be 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4 or 1.5, etc.

[0030] In some embodiments of the present disclosure, the total mass percentage of Ti, Nb, V and Zr is ≤0.15%, preferably 0.02-0.07%.

[0031] In some embodiments of the present disclosure, the mass percentage of Ti is ≤0.1%, for example, it can be 0.1%, 0.09%, 0.08%, 0.07%, 0.06%, 0.05%, 0.04%, 0.03%, 0.02%, 0.01%, 0.005% or 0%, etc.;

[0032] The mass percentage of Nb is ≤0.1%, for example, it can be 0.1%, 0.09%, 0.08%, 0.07%, 0.06%, 0.05%, 0.04%, 0.03%, 0.02%, 0.01%, 0.005% or 0%;

[0033] The mass percentage of V is ≤0.1%, for example, it can be 0.1%, 0.09%, 0.08%, 0.07%, 0.06%, 0.05%, 0.04%, 0.03%, 0.02%, 0.01%, 0.005% or 0%;

[0034] The mass percentage of Zr is ≤0.1%, for example, it can be 0.1%, 0.09%, 0.08%, 0.07%, 0.06%, 0.05%, 0.04%, 0.03%, 0.02%, 0.01%, 0.005% or 0%.

[0035] In some embodiments of the present disclosure, the aluminum alloy material further contains B.

[0036] In some embodiments of the present disclosure, the ratio of the mass of the B to the total mass of the Ti, Nb, V and Zr is ≤2 (for example, it can be 2, 1.8, 1.5, 1.2, 1, 0.8, 0.5, 0.3, 0.2, 0.1 or 0, etc.); preferably ≤0.5.

[0037] In some embodiments of the present disclosure, the mass percentage of B is ≤0.05%; for example, it can be 0.05%, 0.04%, 0.03%, 0.02%, 0.01%, 0.008%, 0.006%, 0.005%, 0.003%, 0.001% or 0%, etc.

[0038] In the present disclosure, Ti, V, Nb, Zr, and B are grain-refining elements that help improve melt cleanliness, reduce hydrogen absorption, and improve fluidity. They also refine α-Al grains, ultimately increasing the strength and elongation of the material. Controlling the combined content of Ti, Nb, V, and Zr to ≥ 0.02% and the ratio of the mass of B to the total mass of Ti, Nb, V, and Zr to ≤ 2 contributes to sufficient α-Al grain refinement and improved aluminum alloy performance. However, when the mass percentage of Ti exceeds 0.1%, or the mass percentage of Nb exceeds 0.1%, or the mass percentage of V exceeds 0.1%, or the mass percentage of Zr exceeds 0.1%, or the mass percentage of B exceeds 0.05%, or the total mass percentage of Ti, Nb, V, and Zr exceeds 0.15%, or the ratio of the mass of B to the total mass of Ti, Nb, V, and Zr exceeds 2, the formation of a second phase containing Ti, Nb, V, Zr, and / or B is easily induced, reducing the material's strength and electrical conductivity. Therefore, the contents of Ti, V, Nb, Zr, and B in the present disclosure preferably meet the content or proportion requirements described in the present disclosure, respectively, and preferably meet the following requirements: the total mass percentage of Ti, Nb, V, and Zr is 0.02-0.15%, the mass percentage of Ti is ≤0.1%, the mass percentage of Nb is ≤0.1%, the mass percentage of V is ≤0.1%, the mass percentage of Zr is ≤0.1%, the mass percentage of B is ≤0.05%, and the ratio of the mass of B to the total mass of Ti, Nb, V, and Zr is ≤2.

[0039] In some embodiments of the present disclosure, the total mass percentage of Mn, Cr and Si in the aluminum alloy material is ≤0.25%; for example, it can be 0.25%, 0.23%, 0.22%, 0.2%, 0.18%, 0.16%, 0.15%, 0.13%, 0.12%, 0.1%, 0.08%, 0.05%, 0.02% or 0%, etc.

[0040] In some embodiments of the present disclosure, the mass percentage of Mn in the aluminum alloy material is ≤0.1%, for example, it can be 0.1%, 0.09%, 0.08%, 0.07%, 0.06%, 0.05%, 0.04%, 0.03%, 0.02%, 0.01%, 0.005% or 0%;

[0041] The mass percentage of Cr is ≤ 0.05%, for example, it can be 0.05%, 0.04%, 0.03%, 0.02%, 0.01%, 0.008%, 0.005%, 0.002% or 0%;

[0042] The mass percentage of Si is ≤0.1%, for example, it can be 0.1%, 0.09%, 0.08%, 0.07%, 0.06%, 0.05%, 0.04%, 0.03%, 0.02%, 0.01%, 0.005% or 0%.

[0043] In some embodiments of the present disclosure, the ratio of the total mass of Mn and Cr to the mass of Si in the aluminum alloy material is ≤0.5; for example, it can be 0.5, 0.4, 0.3, 0.2, 0.1, 0.05 or 0, etc.

[0044] It should be noted that Mn, Cr and Si are impurities in the present disclosure and the less their content, the better. However, these elements are often inevitably contained in existing aluminum raw materials. When the mass percentage of Mn in the aluminum alloy material is greater than 0.1%, or the mass percentage of Cr is greater than 0.05%, or the mass percentage of Si is greater than 0.1%, or the total mass percentage of Mn, Cr and Si is greater than 0.25%, or the ratio of the total mass of Mn and Cr to the mass of Si is greater than 0.5, it is easy to produce NiAl3, FeNiAl9 and Fe4Al9 phases in addition to the eutectic phase. 13 Other secondary phases besides Mn affect the electrical conductivity, strength and other properties of the aluminum alloy material. Therefore, for the present disclosure, when the aluminum alloy material contains Mn, Cr and Si, their contents must meet the content or ratio requirements described in the present disclosure, and preferably, they must simultaneously meet the requirements that the total mass percentage of Mn, Cr and Si is ≤ 0.25%, the mass percentage of Mn is ≤ 0.1%, the mass percentage of Cr is ≤ 0.05%, the mass percentage of Si is ≤ 0.1%, and the ratio of the total mass of Mn and Cr to the mass of Si is ≤ 0.5.

[0045] In the aluminum alloy material disclosed herein, the content of other impurities except Mn, Cr and Si is ≤0.1 wt %.

[0046] In a second aspect, the present disclosure provides a method for preparing the aluminum alloy material according to the first aspect, the preparation method comprising the following steps:

[0047] (1) mixing raw materials containing the elements according to the ratio of the elements in the aluminum alloy material and smelting them to obtain a first aluminum alloy liquid;

[0048] (2) refining, degassing, and deslagging the first aluminum alloy liquid to obtain a second aluminum alloy liquid;

[0049] (3) The second aluminum alloy liquid is kept warm and then cast to obtain the aluminum alloy material.

[0050] Since the aluminum alloy material provided by the present invention has a high Fe content, the raw materials of each element, especially the aluminum material, can be either electrolytic aluminum with a low iron content or scrap aluminum with a high iron content. The aluminum alloy material prepared using the latter as the raw material not only has a lower cost, but also maintains or even exceeds the performance of the former.

[0051] In some embodiments of the present disclosure, the smelting temperature is 680-800°C (for example, 680°C, 690°C, 700°C, 710, 720°C, 730°C, 740°C, 750°C, 760°C, 770°C, 780°C, 790°C or 800°C, etc.), and the smelting time is 120-180 min (for example, 120 min, 130 min, 140 min, 150 min, 160 min, 170 min or 180 min, etc.).

[0052] In some embodiments of the present disclosure, the refining temperature is 680-800°C (for example, 680°C, 690°C, 700°C, 710, 720°C, 730°C, 740°C, 750°C, 760°C, 770°C, 780°C, 790°C or 800°C, etc.), and the refining time is 15-30 min (for example, 15 min, 18 min, 20 min, 22 min, 25 min, 28 min or 30 min, etc.).

[0053] In some embodiments of the present disclosure, the insulation temperature is 680-800°C (for example, it can be 680°C, 690°C, 700°C, 710, 720°C, 730°C, 740°C, 750°C, 760°C, 770°C, 780°C, 790°C or 800°C, etc.), and the time is 30-120min (for example, it can be 30min, 40min, 50min, 60min, 70min, 80min, 90min, 100min, 110min or 120min, etc.).

[0054] In some embodiments of the present disclosure, the casting is low-pressure casting, differential pressure casting, squeeze casting or high-pressure casting.

[0055] In a third aspect, the present disclosure provides an application of the aluminum alloy material as described in the first aspect, wherein the aluminum alloy material is used to manufacture automotive parts.

[0056] In some embodiments, the automotive component is a motor rotor, a wire, or an inverter.

[0057] The present invention discloses a method for utilizing NiAl3 phase, FeNiAl9 phase and Fe4Al 13 The obtained aluminum alloy material has the advantages of high strength, high conductivity and low cost.

[0058] In addition, through further optimization, the electrical conductivity of the obtained aluminum alloy material is ≥48% IACS, the yield strength at room temperature is ≥75MPa, the tensile strength is ≥160MPa, the elongation is ≥10%, and the yield strength decay rate after 100h of insulation at 180°C is ≤10%. It has the advantages of high strength, good conductivity and low cost, and has good fluidity. It can be cast by low pressure, differential pressure, extrusion or high pressure, and is suitable for the production of motor rotors, wires, inverters and other automotive parts. BRIEF DESCRIPTION OF THE DRAWINGS

[0059] Figure 1 shows the phase composition and phase relationship of the Al-rich corner of the Al-xFe-yNi system under non-equilibrium solidification of aluminum alloy materials. DETAILED DESCRIPTION

[0060] The technical solution of the present disclosure will be further described below with reference to the accompanying drawings and through specific embodiments. Those skilled in the art should understand that the specific embodiments are only to help understand the present disclosure and should not be regarded as specific limitations of the present disclosure.

[0061] Examples 1-11 and Comparative Examples 1-5

[0062] Examples 1-11 and Comparative Examples 1-5 each provide an aluminum alloy material, which is prepared according to the following method:

[0063] (1) adding industrial pure aluminum, AlNi alloy, Al-Fe alloy, Al-Ti alloy, Al-Nb alloy, Al-V alloy, Al-Zr alloy and / or Al-B alloy raw materials into a melting furnace according to the ratio of each element in the aluminum alloy material, and melting at 740° C. for 120 minutes to obtain a first aluminum alloy liquid;

[0064] (2) adding 0.5 wt % of a refining agent to the first aluminum alloy liquid, refining at 740° C. for 15 min, degassing with high-purity argon, and removing slag after standing for 15 min to obtain a second aluminum alloy liquid;

[0065] (3) The second aluminum alloy liquid was held at 740°C for 30 minutes and the aluminum alloy material was obtained by low-pressure casting (pressure 0.01 MPa, holding pressure 120 seconds), differential pressure casting (pressure difference between upper and lower cavities 0.1 MPa, holding pressure 80 seconds), squeeze casting (pressure 15 MPa, holding pressure 25 seconds), or high-pressure casting (slow pressure to fast pressure switching point 240 mm, injection speed 3 m / s, pressure 35 MPa, holding pressure 20 seconds). Casting parameters: The mold was pre-sprayed with a release agent and preheated to 180°C. The casting temperature was controlled at 720°C and the ejection temperature was 370°C.

[0066] The contents of the elements and the casting methods of the aluminum alloy materials provided in Examples 1-11 and Comparative Examples 1-5 are shown in Table 1 below:

[0067] Table 1 Element content (wt%) and casting method

[0068] The proportions and structural information of the elements in the aluminum alloy materials provided by Examples 1-11 and Comparative Examples 1-5 are shown in Table 2 below:

[0069] Table 2 Element ratio and organization information

[0070] The Mn, Cr, and Si content was determined by inductively coupled plasma spectroscopy (ICP) with an analytical error of 3-5%. Powder was sawn from different areas of the alloy sample and mixed thoroughly, with 1g of powder sampled for analysis. Each batch of samples was tested twice independently, and the average value was calculated.

[0071] NiAl3, FeNiAl9 and Fe4Al 13 The content was determined by X-ray diffraction analysis of powdered alloy samples. The test conditions were: Cu target, Kα radiation; 2θ angle range of 10-90°; scan step size of 0.02°; and scan speed of 0.33° / s. The results were refined using Topas.

[0072] The α-Al grain size was determined by observing the metallographic sample under an optical microscope to obtain polarized photographs, and using the line intercept method (ASTM standard E112-10) to calculate the grain size.

[0073] Performance testing:

[0074] The electrical conductivity, yield strength, tensile strength, elongation and high temperature resistance of the aluminum alloy materials provided in Examples 1-11 and Comparative Examples 1-5 were tested using the following test methods:

[0075] Conductivity: Tested according to GB / T 12966-2022 Aluminum and aluminum alloy electrical conductivity eddy current test method;

[0076] Room temperature yield strength: tested according to GB / T 228.1-2021 Metallic materials tensile tests part 1: Room temperature test methods;

[0077] Room temperature tensile strength: tested according to GB / T 228.1-2021 Metallic materials tensile tests Part 1: Room temperature test methods;

[0078] Room temperature elongation: tested according to GB / T 228.1-2021 Metallic materials tensile tests part 1: Room temperature test methods;

[0079] High temperature resistance: Keep the aluminum alloy material at 180℃ for 100h, test its yield strength, and calculate the strength decay rate.

[0080] The results of the above tests are shown in Table 3 below:

[0081] Table 3

[0082] From the performance data of the above embodiments, it can be seen that the aluminum alloy material provided by the present disclosure has an electrical conductivity of ≥48% IACS, a yield strength of ≥75 MPa at room temperature, a tensile strength of ≥160 MPa, an elongation of ≥10%, a yield strength decay rate of ≤10% after insulation at 180°C for 100 hours, a low Ni / Fe ratio, and the advantages of high strength and high conductivity with low cost. It also has good fluidity and can be cast by low pressure, differential pressure, extrusion, or high pressure.

[0083] Among them, compared with Example 7, the Ni content of Comparative Example 1 is too little and the Ni / Fe ratio is too low, resulting in too low contents of the eutectic phase NiAl3 and the primary solidification phase FeNiAl9, which leads to a decrease in the electrical conductivity of the aluminum alloy material.

[0084] Compared with Example 8, the Fe content of Comparative Example 2 is too low and the Ni / Fe ratio is too high, resulting in the primary solidification phase Fe4Al 13 If the content is too low, the yield and tensile strength of the aluminum alloy material will decrease.

[0085] Compared with Example 9, the respective contents, total contents and (Mn+Cr) / Si mass ratio of Mn, Cr and Si in Comparative Example 3 are too high, resulting in the generation of NiAl3, FeNiAl9 and Fe4Al3 phases in the aluminum alloy material. 13 In addition to the second phase rich in Mn, Cr, and Si elements, the electrical conductivity and elongation of the aluminum alloy material decrease.

[0086] Compared with Example 10, the total content of Ti, Nb, V and Zr in Comparative Example 4 is too high, resulting in the generation of NiAl3 eutectic phase, FeNiAl9 primary solidification phase and Fe4Al 13 If there are other second phases rich in Ti, Nb, V and Zr elements besides the Al alloy, the strength and elongation of the aluminum alloy material will decrease.

[0087] Compared with Example 11, the B / (Ti+Nb+V+Zr) mass ratio in Comparative Example 5 is too large, resulting in the production of other B-rich second phases in the aluminum alloy material in addition to the eutectic phase NiAl3 and the primary solidification phase FeNiAl9, and the α-Al grain size is larger, and the electrical conductivity, strength and elongation of the aluminum alloy material are reduced.

[0088] The phase composition and phase relationship of the Al-rich corner of the Al-xFe-yNi system (0≤x / y≤7) under non-equilibrium solidification were respectively calculated by Calphad thermodynamics for the aluminum alloy materials provided by the present invention and the aluminum alloy materials of Rio Tinto (US20220090234A1), Tesla (US20210332461A1), and Shenzhen Xinshen (CN 113981278A), and the results are shown in Figure 1.

[0089] As can be seen from FIG1 , the aluminum alloy of the prior art is mainly composed of aluminum matrix (Fcc), NiAl3 and FeNiAl9 in the range of Ni and Fe; while the aluminum alloy provided by the present disclosure is mainly composed of aluminum matrix (Fcc), NiAl3, FeNiAl9, Fe4Al9 in the range of Ni and Fe. 13 Composition. Different phase compositions can result in different alloy properties.

[0090] The foregoing description is intended only to provide specific embodiments of the present disclosure, intended to enable those skilled in the art to understand and implement the present disclosure. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present disclosure. Therefore, the present disclosure is not intended to be limited to the embodiments described herein, but rather to be construed in the broadest manner consistent with the principles and novel features disclosed herein.

Claims

1. An aluminum alloy material, wherein: The cast structure of the aluminum alloy material contains, in addition to the aluminum matrix, eutectic phase NiAl3, primary solidification phase FeNiAl9 and primary solidification phase Fe4Al 13 .

2. The aluminum alloy material according to claim 1, wherein The mass content of the eutectic phase NiAl3 is 0.2-2.2%, the mass content of the primary solidification phase FeNiAl9 is 0.1-1.1%, and the mass content of the primary solidification phase Fe4Al 13 The mass content is 1-6%; Furthermore, the α-Al grain size in the aluminum alloy material is less than 100 μm.

3. The aluminum alloy material according to claim 1 or 2, wherein: The aluminum alloy material contains the eutectic phase NiAl3, the primary solidification phase FeNiAl9 and Fe4Al 13 In addition, it does not contain any other second phase.

4. The aluminum alloy material according to any one of claims 1 to 3, wherein: The aluminum alloy material includes the following components in percentage by mass: Ni 0.5%-1.5%, Fe 0.8%-2.5%, one or more of Ti, Nb, V and Zr, and the total mass percentage of Ti, Nb, V and Zr is ≥0.02%, and the balance is Al.

5. The aluminum alloy material according to claim 4, wherein: The mass ratio of Ni to Fe is 0.2-1.5; Preferably, the total mass percentage of Ti, Nb, V and Zr is ≤0.15%, preferably 0.02-0.07%; Preferably, the mass percentage of Ti is ≤0.1%, the mass percentage of Nb is ≤0.1%, the mass percentage of V is ≤0.1%, and the mass percentage of Zr is ≤0.1%.

6. The aluminum alloy material according to any one of claims 3 to 5, wherein: The aluminum alloy material further contains B; Preferably, the ratio of the mass of B to the total mass of Ti, Nb, V and Zr is ≤2, preferably ≤0.5; Preferably, the mass percentage of B is ≤0.05%.

7. The aluminum alloy material according to any one of claims 1 to 6, wherein: The total mass percentage of Mn, Cr and Si in the aluminum alloy material is ≤0.25%; Preferably, the mass percentage of Mn in the aluminum alloy material is ≤0.1%, the mass percentage of Cr is ≤0.05%, and the mass percentage of Si is ≤0.1%; Preferably, the ratio of the total mass of Mn and Cr to the mass of Si in the aluminum alloy material is ≤0.

5.

8. A method for preparing the aluminum alloy material according to any one of claims 1 to 7, wherein: The preparation method comprises the following steps: (1) mixing raw materials containing the elements according to the ratio of the elements in the aluminum alloy material and smelting them to obtain a first aluminum alloy liquid; (2) refining, degassing, and deslagging the first aluminum alloy liquid to obtain a second aluminum alloy liquid; (3) The second aluminum alloy liquid is kept warm and then cast to obtain the aluminum alloy material.

9. The preparation method according to claim 8, wherein The smelting temperature is 680-800°C and the smelting time is 120-180 minutes; Preferably, the refining temperature is 680-800°C and the refining time is 15-30 minutes; Preferably, the temperature of the insulation is 680-800°C and the time is 30-120 minutes; Preferably, the casting is low-pressure casting, differential pressure casting, squeeze casting or high-pressure casting.

10. Use of the aluminum alloy material according to any one of claims 1 to 7, wherein: The aluminum alloy material is used to make automobile parts; Preferably, the automotive component is a motor rotor, a wire or an inverter.