AI Technical Summary
The internal resistance of existing ceramic-coated separators still needs to be further reduced, affecting the power performance and discharge efficiency of lithium-ion batteries.
Using low-sodium boehmite powder and ceramic slurry without sodium carboxymethyl cellulose (CMC), by adjusting the viscosity and solid content of the ceramic layer and adjusting the process parameters, a ceramic layer is formed to reduce the sodium content and internal resistance of the separator. , improve the breathability and peel strength of the separator.
It significantly reduces the internal resistance of the separator, improves the power performance and discharge efficiency of lithium-ion batteries, and ensures good adhesion and usability of the ceramic layer.
Smart Images

Figure PI2025002730_DRAWING_001
Abstract
Description
A low internal resistance ceramic coated diaphragm and preparation method thereof, and lithium ion battery
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This disclosure claims priority to the Chinese patent application with application number CN202211374693.1 filed with the Patent Office of China on November 4, 2022, entitled “A low internal resistance ceramic coated diaphragm and its preparation method, lithium-ion battery”, the entire contents of which are incorporated by reference into this disclosure. Technical Field
[0003] The present disclosure relates to the technical field of lithium-ion battery separators, and in particular to a low-internal-resistance ceramic-coated separator and a preparation method thereof, and a lithium-ion battery. Background Art
[0004] In recent years, new energy vehicles have placed increasing demands on high-rate charge and discharge performance in power batteries. Internal resistance is a key factor influencing battery power performance and discharge efficiency. Its initial value is primarily determined by the battery's structural design, raw material properties, and manufacturing process. Over time, lithium-ion batteries experience a gradual decline in performance, primarily manifested by capacity loss, increased internal resistance, and decreased power. Changes in internal resistance are affected by various operating conditions, including temperature and depth of discharge.
[0005] The main factors affecting the ionic impedance of the separator include electrolyte distribution within the separator, separator area, thickness, pore size, porosity, and tortuosity. Ionic conduction within the battery relies on the diffusion of lithium ions from the electrolyte through the porous structure of the separator. The separator's wettability is key to forming a good ion flow channel. When the separator has a higher liquid absorption rate and a more porous structure, it can improve conductivity, reduce battery impedance, and enhance the battery's rate performance.
[0006] Compared to conventional base membranes, ceramic and rubber-coated diaphragms significantly improve their high-temperature shrinkage resistance and enhance their liquid absorption and wetting capabilities. However, the internal resistance of existing ceramic-coated diaphragms still needs to be further reduced.
[0007] Current technology primarily controls the internal resistance of ceramic-coated diaphragms by adjusting their thickness and permeability. Generally, thinner diaphragms offer less resistance to the passage of solvated lithium ions, resulting in better ion conductivity and lower internal resistance. Higher permeability values increase internal resistance. However, less attention has been paid to the effect of the coating slurry composition on the internal resistance of the coating.
[0008] The conventional method for preparing boehmite is the Bayer process, which involves treating bauxite with sodium hydroxide to produce a sodium aluminate solution, which is then reprecipitated to produce boehmite. This process introduces a certain amount of sodium. When preparing boehmite ceramic slurry, CMC solution is often added to enhance adhesion between the boehmite and the base film and improve separator peel strength. CMC also acts as a suspending agent, improving particle settling after the slurry is prepared.
[0009] Summary of the Invention
[0010] The purpose of the present disclosure is to provide a low-internal-resistance ceramic-coated diaphragm and a preparation method thereof, as well as a lithium-ion battery equipped with the diaphragm, which can reduce the internal resistance of the battery cell and thereby improve the power performance and discharge efficiency of the battery.
[0011] The present disclosure is achieved as follows:
[0012] The present disclosure first provides a low internal resistance ceramic coated diaphragm, comprising: a polymer base film, and a ceramic layer coated on one or both sides of the polymer base film;
[0013] The ceramic layer has a sodium content of less than 1000 ppm and does not contain sodium carboxymethyl cellulose (CMC);
[0014] The peel strength between the ceramic layer and the polymer base film is above 20 N / m, optionally 20-70 N / m, optionally 30 N / m-70 N / m, optionally 40 N / m-70 N / m, for example 45 N / m, 50 N / m, 55 N / m, 60 N / m, 65 N / m.
[0015] The low internal resistance ceramic coated diaphragm disclosed herein can achieve an ion conductivity of 1.4 mS / cm or more, and can achieve an ion conductivity of 1.5 mS / cm or more, by adjusting the formula.
[0016] Optionally, the ceramic layer is formed by coating a ceramic slurry. Since CMC is omitted, the viscosity of the ceramic slurry is lower than that of conventional ceramic slurry, which is 10-40 mPa·S. -1 , such as 35mPa·S -1 Below, 30mPa·S -1 Below, 25mPa·S -1 Hereinafter, the solid content of the ceramic slurry is 25%-35%.
[0017] Optionally, the ceramic slurry comprises the following components:
[0018] Dispersant: 2-6 parts;
[0019] Low sodium boehmite powder: 292 parts;
[0020] Binder: 20-60 parts;
[0021] Wetting agent: 1-4 parts;
[0022] The low sodium boehmite powder has a sodium content of ≤100 ppm.
[0023] Optionally, the ceramic slurry further comprises 30-50 parts of a leveling agent; in an optional embodiment, the leveling agent is UNISAFE WHS-10.
[0024] Optionally, the thickness of the ceramic layer is 1-5 μm, and the surface density of the ceramic layer is 8-10 g / m 2 .
[0025] Optionally, the low internal resistance ceramic coated diaphragm has an air permeability of 75-175 sec / mL.
[0026] Optionally, the water content of the low internal resistance ceramic coated diaphragm is less than 1000 ppm, optionally less than 700 ppm, optionally less than 500 ppm.
[0027] Optionally, the polymer-based membrane is a polyolefin microporous membrane. Optionally, the polyolefin microporous membrane is a polyethylene microporous membrane, a polypropylene microporous membrane, or a two-layer or multi-layer composite membrane consisting of a polyethylene microporous membrane and a polypropylene microporous membrane.
[0028] The present disclosure also provides a method for preparing the low internal resistance ceramic coated diaphragm, comprising the following steps:
[0029] Step 1: Prepare ceramic slurry by adding 292 parts of low sodium boehmite powder, 2-6 parts of D-3019 dispersant, 20-60 parts of BM-900B binder, and 1-4 parts of 202E wetting agent into water, and stir and disperse the components evenly in water to obtain a stable ceramic slurry.
[0030] Step 2, coating slurry: Provide a polymer base film, use a gravure roller to coat the base film surface to form a ceramic layer, and adjust the operating parameters of the gravure roller according to the viscosity and solid content of the ceramic slurry to meet the requirements of the ceramic layer coating thickness and surface density.
[0031] Optionally, the line number of the gravure roller is 140-189, the line depth is 30-50 μm, the coating speed is 80-140 s / m, and the speed ratio is 90%-100%; wherein the speed ratio is the ratio of the gravure roller running speed to the coating machine running speed.
[0032] Step 3: Drying the ceramic layer to obtain the low internal resistance ceramic coated diaphragm.
[0033] Optionally, in step 2, before coating the base film, the ceramic slurry is continuously stirred at a low speed of 10-30 r / min to prevent the low-viscosity ceramic slurry from settling before coating.
[0034] Optionally, during the preparation process, the ambient humidity is controlled to be below 1% to reduce the water content of the low internal resistance ceramic coated diaphragm.
[0035] The present disclosure also provides a lithium battery comprising a positive electrode, a negative electrode, a non-aqueous electrolyte, and the above-mentioned low-internal-resistance ceramic-coated diaphragm or the low-internal-resistance ceramic-coated diaphragm obtained according to the above-mentioned preparation method.
[0036] The present disclosure has the following beneficial effects:
[0037] The low internal resistance ceramic coated diaphragm disclosed herein has a ceramic layer formed by coating one or both sides of a polymer base film with low-sodium boehmite and does not contain sodium carboxymethyl cellulose. The sodium content of the ceramic layer is less than 1000 ppm, which can significantly reduce the added value of the diaphragm's air permeability. When used in lithium-ion batteries, it can greatly reduce the internal resistance of the battery cell, thereby improving the battery's power performance and discharge efficiency. It can significantly reduce the internal resistance of the diaphragm, allowing the diaphragm to obtain good performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present disclosure and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without creative work.
[0039] FIG1 is a schematic structural diagram of a low internal resistance ceramic coated diaphragm disclosed in the present invention. DETAILED DESCRIPTION
[0040] To make the purpose, technical solutions, and advantages of the embodiments of the present disclosure more clear, the technical solutions in the embodiments of the present disclosure are described clearly and completely below. Where conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer were followed. Where the manufacturer of the reagents or instruments used is not specified, all are conventional products that can be purchased commercially.
[0041] As shown in Figure 1, the low internal resistance ceramic coated diaphragm disclosed in the present invention comprises: a polymer base film 1, and a ceramic layer 2 coated on one or both sides of the polymer base film 1. The present invention starts with the formulation of the ceramic layer, adopts a powder with a low sodium (Na) content to eliminate the influence of sodium on lithium batteries, and adopts a low sodium boehmite powder with a Na content of less than 100ppm; at the same time, the currently mainstream added sodium carboxymethyl cellulose (CMC) solution is removed from the ceramic slurry. On the one hand, since CMC contains Na, it will also affect the lithium-ion battery due to the introduction of Na, so CMC needs to be removed. On the other hand, since the main chain of CMC has a large number of carboxymethyl groups and hydroxyl groups that are hydrophilic groups, CMC is a highly hygroscopic substance, and its equilibrium moisture increases with the increase of ambient humidity and decreases with the increase of temperature. Not using CMC in the diaphragm will also greatly reduce the proportion of hygroscopic substances, thereby reducing the water content of the diaphragm and reducing the influence of moisture on the internal resistance of the diaphragm.
[0042] While meeting the other physical performance requirements of the ceramic coated diaphragm, the present invention reduces the sodium content in the slurry as much as possible, thereby reducing the internal resistance of the diaphragm and allowing the diaphragm to obtain good performance. The reason is that sodium and lithium belong to the same main group elements. A high sodium content in the slurry will affect the diffusion of lithium ions in the battery. The present invention controls the sodium content in the diaphragm to below 1000ppm, thereby suppressing the effect of sodium ions on the diffusion of lithium ions. In lithium-ion battery applications, the ceramic coated diaphragm of the present invention can achieve an ion conductivity of more than 1.4mS / cm and can achieve more than 1.5mS / cm.
[0043] Optionally, the present invention reduces the internal resistance of the ceramic coated diaphragm by adjusting the ceramic layer slurry formula and process, while ensuring that other physical properties of the ceramic coated diaphragm meet the use requirements. This is mainly reflected in: First, under the premise of removing CMC, by setting the ceramic slurry solid content gradient, the requirements of the ceramic layer coating thickness are met; second, by adjusting the content of adhesives and additives, the permeability increase value is reduced and the permeability is increased to an appropriate range; third, in the ceramic layer manufacturing process, the coating process parameters are adjusted, and the continuous stirring process of the slurry is added to prevent the precipitation of the slurry; fourth, by adjusting the additives, the problem of reduced peel strength caused by not adding CMC is solved, so that the peel strength meets the use requirements.
[0044] The features and performance of the present invention are further described in detail below with reference to the following embodiments and comparative examples.
[0045] Example 1
[0046] (1) Preparation of ceramic slurry: low sodium boehmite powder (BG-611D model), pure water and dispersant (D-3019 model) were added to a double planetary mixing tank and stirred and dispersed. Then, a binder (BM-900B model), a leveling agent (UNISAFE WHS-10) and a wetting agent (202E model) were added in sequence.
[0047] (2) Preparation of a low internal resistance ceramic coated diaphragm: Ceramic slurry was applied to both surfaces of a 12 μm thick PE microporous base membrane, and the coating thickness of each surface was 1.5 μm to form a ceramic layer, wherein the line number of the gravure roller was 150, the line depth was 40 μm, and the speed ratio was 90%; after drying, an ultra-low internal resistance ceramic coated diaphragm was obtained.
[0048] Example 2
[0049] (1) Preparation of ceramic slurry: low sodium boehmite powder (BG-611D model), pure water and dispersant (D-3019 model) were added to a double planetary mixing tank and stirred and dispersed. Then, a binder (BM-900B model), a leveling agent (UNISAFE WHS-10) and a wetting agent (202E model) were added in sequence.
[0050] (2) Preparation of low internal resistance ceramic coated diaphragm: ceramic slurry was coated on both surfaces of a 12 μm thick PE porous isolation membrane using a gravure roller, and the coating thickness on each surface was 1.5 μm to form a ceramic layer, wherein the number of lines of the gravure roller was 150, the line depth was 40 μm, and the speed ratio was 90%; after drying, an ultra-low internal resistance ceramic coated diaphragm was obtained.
[0051] Example 3
[0052] (1) Preparation of ceramic slurry: low sodium boehmite powder (BG-611D model), pure water and dispersant (D-3019 model) were added to a double planetary mixing tank and stirred and dispersed. Then, a binder (BM-900B model), a leveling agent (UNISAFE WHS-10) and a wetting agent (202E model) were added in sequence.
[0053] (2) Preparation of low internal resistance ceramic coated diaphragm: ceramic slurry was coated on both surfaces of a 12 μm thick PE porous isolation membrane using a gravure roller, and the coating thickness on each surface was 1.5 μm to form a ceramic layer, wherein the number of lines of the gravure roller was 150, the line depth was 40 μm, and the speed ratio was 90%; after drying, an ultra-low internal resistance ceramic coated diaphragm was obtained.
[0054] Example 4
[0055] (1) Preparation of ceramic slurry: low sodium boehmite powder (BG-611D model), pure water and dispersant (D-3019 model) were added to a double planetary mixing tank and stirred and dispersed. Then, a binder (BM-900B model), a leveling agent (UNISAFE WHS-10) and a wetting agent (202E model) were added in sequence.
[0056] (2) Preparation of low internal resistance ceramic coated diaphragm: ceramic slurry was coated on both surfaces of a 12 μm thick PE porous isolation membrane using a gravure roller, and the coating thickness on each surface was 1.5 μm to form a ceramic layer, wherein the number of lines of the gravure roller was 150, the line depth was 40 μm, and the speed ratio was 90%; after drying, an ultra-low internal resistance ceramic coated diaphragm was obtained.
[0057] Comparative Example 1
[0058] (1) Preparation of ceramic slurry: low sodium boehmite powder (BG-611D model), pure water and dispersant (D-3019 model) were added to a double planetary stirring tank and stirred and dispersed, and then a binder (BM-900B model), B1-CMC1220 solution and a wetting agent (202E model) were added in sequence.
[0059] (2) Preparation of a low internal resistance ceramic coated diaphragm: Ceramic slurry was applied to both surfaces of a 12 μm thick PE porous isolation membrane, and the coating thickness of each surface was 1.5 μm to form a ceramic layer, wherein the number of lines of the gravure roller was 180, the line depth was 30 μm, and the speed ratio was 90%; after drying, a ceramic coated diaphragm was obtained.
[0060] Comparative Example 2
[0061] (1) Preparation of ceramic slurry: Add boehmite powder (BG-611 model), pure water and dispersant (D-3019 model) into a double planetary stirring tank and stir and disperse them. Then add binder (BM-900B model) and wetting agent (202E model) in sequence.
[0062] (2) Preparation of a low internal resistance ceramic coated diaphragm: Ceramic slurry was applied to both surfaces of a 12 μm thick PE porous isolation membrane, and the coating thickness of each surface was 1.5 μm to form a ceramic layer, wherein the number of lines of the gravure roller was 180, the line depth was 30 μm, and the speed ratio was 90%; after drying, a ceramic coated diaphragm was obtained.
[0063] Comparative Example 3
[0064] (1) Preparation of ceramic slurry: Add boehmite powder (BG-611 model), pure water and dispersant (D-3019 model) into a double planetary stirring tank and stir and disperse them. Then add binder (BM-900B model), B1-CMC1220 solution and wetting agent (202E model) in sequence.
[0065] (2) Preparation of a low internal resistance ceramic coated diaphragm: Ceramic slurry was applied to both surfaces of a 12 μm thick PE porous isolation membrane, and the coating thickness of each surface was 1.5 μm to form a ceramic layer, wherein the number of lines of the gravure roller was 180, the line depth was 30 μm, and the speed ratio was 90%; after drying, a ceramic coated diaphragm was obtained.
[0066] The ceramic slurry formula and process parameters in the above examples and comparative examples are shown in Table 1 below:
[0067] Table 1 Summary of ceramic slurry formulations and process parameters in Examples and Comparative Examples
[0068]
[0069]
[0070] <Evaluation Method>
[0071] (1) Peel strength between ceramic layer and base film
[0072] A 12 mm wide, 15 cm long adhesive tape (Scotch, Model 550R-12) was applied to the ceramic layer surface of one side of the separator. The separator was cut so that its width and length matched those of the adhesive tape to prepare a measurement sample. The adhesive tape was applied to the separator so that its longitudinal direction aligned with the MD direction of the separator. It should be noted that the adhesive tape served as a support for peeling off one side of the ceramic layer.
[0073] The measurement sample was left in an atmosphere of a temperature of 23±1° C. and a relative humidity of 50±5% for 24 hours or more, and the following measurements were performed in the same atmosphere.
[0074] The adhesive tape is peeled off together with the ceramic layer immediately below it by about 10 cm, so that the laminate (1) of the adhesive tape and the ceramic layer is separated from the laminate (2) of the porous substrate and the ceramic layer of the other party by about 10 cm. The end of the laminate (1) is fixed to the upper chuck of TENSILON (RTC-1210A made by Orientec), and the end of the laminate (2) is fixed to the lower chuck of TENSILON. The measurement sample is suspended in the direction of gravity so that the tensile angle (the angle of the laminate (1) relative to the measurement sample) becomes 180 °. The laminate (1) is stretched at a tensile speed of 20 mm / min, and the load when the laminate (1) is peeled off from the porous substrate is measured. The load from 10 mm to 40 mm after the start of the measurement is obtained at intervals of 0.4 mm, and its average value is used as the peel strength.
[0075] (2) Diaphragm internal resistance and ionic conductivity
[0076] The electrochemical impedance spectroscopy (EIS) method was used to measure the ion exchange rate. The separator sample was assembled into a button cell in the order of positive electrode shell-separator-stainless steel sheet gasket-spring gasket-negative electrode shell. The electrochemical workstation was used to perform the ion exchange rate scan at a frequency of 0.01 Hz to 10 6 HZ, the voltage amplitude is 5mV, and the internal resistance Rb of the diaphragm is obtained. The ionic conductivity of the diaphragm is calculated as follows: K = d / (S*Rb), where K is the ionic conductivity of the diaphragm (mS / cm), d is the thickness of the diaphragm (cm), and S is the effective working area of the diaphragm (cm 2 ).
[0077] (3) Gurley air permeability
[0078] A composite membrane sample of 100 mm × 100 mm was cut and tested using a Gurley 4110N air permeability tester from the United States using a 100 cc test gas mode. The time it took for the test gas to completely pass through the composite membrane sample was recorded, which was the Gurley value.
[0079] Referring to Table 2, the performance test results of the diaphragms prepared in the above examples and comparative examples are compared as follows:
[0080] Table 2 Performance parameters of ceramic coated diaphragms prepared in Examples and Comparative Examples
[0081]
[0082] It can be seen from the results in Tables 1-2 above that the present disclosure reduces the added air permeability and sodium content of the diaphragm by using low-sodium boehmite and eliminating the addition of CMC solution, which can significantly reduce the internal resistance of the diaphragm and enable the diaphragm to obtain good performance. At the same time, the slurry sedimentation problem caused by eliminating the addition of CMC solution can be solved by adjusting the process parameters of the ceramic layer preparation process. After the preparation is completed, low-speed stirring can be performed to prevent sedimentation, and the operating parameters of the gravure roller can be adjusted to obtain the ideal ceramic layer thickness and surface density. In addition, due to the elimination of the addition of CMC solution, the bonding performance of the ceramic slurry is reduced, and the peel strength of the ceramic coating layer is also reduced. However, the present disclosure adjusts the ceramic layer slurry formula to ensure that the peel strength of the ceramic layer can still meet the use requirements of greater than 20N / m. By comparing Example 2 with Example 1, it can be seen that the ceramic peeling degree can be further improved by adding a leveling agent solution, so that the peel strength of the ceramic layer is increased to more than 40N / m.
[0083] The foregoing description is merely an optional embodiment of the present disclosure and is not intended to limit the present disclosure. Those skilled in the art will readily appreciate that the present disclosure is susceptible to various modifications and variations. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of the present disclosure shall be included within the scope of protection of the present disclosure.
Claims
1. A low internal resistance ceramic coated diaphragm, characterized in that: include: A polymer base film, and a ceramic layer coated on one or both sides of the polymer base film; The ceramic layer has a sodium content of less than 1000 ppm and does not contain sodium carboxymethyl cellulose; The peel strength between the ceramic layer and the polymer base film is greater than 20N / m; The ion conductivity of the low internal resistance ceramic coated diaphragm is greater than 1.4 mS / cm.
2. The low internal resistance ceramic coated diaphragm according to claim 1, characterized in that: The peeling strength between the ceramic layer and the polymer base film is 20-70 N / m.
3. The low internal resistance ceramic coated diaphragm according to claim 1, characterized in that: The ceramic layer is formed by coating a ceramic slurry, and the viscosity of the ceramic slurry is 10-40 mPa·S -1 , the solid content of the ceramic slurry is 25%-35%.
4. The low internal resistance ceramic coated diaphragm according to claim 3, characterized in that: The ceramic slurry comprises the following components: Dispersant: 2-6 parts; Low sodium boehmite powder: 292 parts; Binder: 20-60 parts; Wetting agent: 1-4 parts; The low sodium boehmite powder has a sodium content of ≤100 ppm.
5. The low internal resistance ceramic coated diaphragm according to claim 4, characterized in that: The ceramic slurry further comprises 30-50 parts of a leveling agent.
6. The low internal resistance ceramic coated diaphragm according to claim 1, characterized in that: The thickness of the ceramic layer is 1-5 μm, and the surface density of the ceramic layer is 8-10 g / m 2 .
7. The low internal resistance ceramic coated diaphragm according to claim 1, characterized in that: The low internal resistance ceramic coated diaphragm has an air permeability of 75-175 sec / mL.
8. The low internal resistance ceramic coated diaphragm according to claim 1, characterized in that: The water content of the low internal resistance ceramic coating diaphragm is less than 1000 ppm.
9. The method for preparing a low internal resistance ceramic coated diaphragm according to claim 1, characterized in that: The steps include: Step 1: Prepare ceramic slurry by stirring and dispersing the components in water to obtain a stable ceramic slurry; Step 2, coating slurry: providing a polymer base film, and using a gravure roller to coat the base film surface to form a ceramic layer; Step 3: Drying the ceramic layer to obtain the low internal resistance ceramic coated diaphragm.
10. The method for preparing a low internal resistance ceramic coated diaphragm according to claim 1, characterized in that: In step 2, before coating the base film, the ceramic slurry is continuously stirred at a speed of 10-30 r / min; the line number of the gravure roller is 140-189, the line depth is 30-50 μm, the coating speed is 80-140 s / m, and the speed ratio is 90%-100%.
11. The method for preparing a low internal resistance ceramic coated diaphragm according to claim 1, characterized in that: During the preparation process, the ambient humidity was controlled below 1%.
12. A lithium battery, characterized in that: The invention comprises a positive electrode, a negative electrode, a non-aqueous electrolyte and the low internal resistance ceramic coated diaphragm according to any one of claims 1 to 8 or the low internal resistance ceramic coated diaphragm obtained by the preparation method according to any one of claims 9 to 11.