Method for producing polyacetal copolymer
Patent Information
- Application Number
- MYPI2025002733
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-11-07
- Filing Date
- 2023-09-19
- Publication Date
- 2024-05-07
AI Technical Summary
Existing methods for producing polyacetal copolymers face challenges in deactivating catalysts efficiently, leading to residual catalysts and formaldehyde generation, which affects polymer stability and quality, especially during mass production, and result in poor appearance and fluidity of molded products.
A method involving the use of a combination of heteropolyacid and its salt as a polymerization catalyst, specifically phosphotungstovanadate and sodium phosphotungstate, to reduce formaldehyde generation and enhance polymerization stability, fluidity, and appearance of molded products, while maintaining low catalyst amounts.
This approach allows for stable production of polyacetal copolymers with reduced formaldehyde generation, improved fluidity during molding, and excellent appearance of molded products, even in mass production, by effectively deactivating catalysts and optimizing polymerization conditions.
Abstract
Description
Method for producing polyacetal copolymer
[0001] The present invention relates to a method for producing a polyacetal copolymer.
[0002] A known method for producing polyacetal copolymers involves cationic polymerization of a main monomer (trioxane) and a comonomer copolymerizable with the main monomer in the presence of a cationic polymerization catalyst. Lewis acids such as boron trifluoride, tin tetrachloride, titanium tetrachloride, phosphorus pentafluoride, phosphorus pentachloride, and antimony pentafluoride, as well as complex compounds or salts thereof, are widely used as the cationic polymerization catalyst.
[0003] However, polymerization catalysts such as boron trifluoride must be added in relatively large amounts (e.g., 40 ppm or more relative to the total monomers) during polymerization. Therefore, there is a problem in the production process in that it is difficult to sufficiently deactivate the catalyst remaining in the polyacetal copolymer after polymerization. Even if the catalyst can be deactivated, catalyst-derived substances remaining in the copolymer can sometimes cause problems such as accelerated copolymer decomposition. Furthermore, because the catalyst deactivation step is performed in a large amount of aqueous solution (treatment liquid) containing a basic compound such as triethylamine, additional complicated steps are required after the step, such as a step of separating the copolymer from the treatment liquid and drying it, and a step of recovering unreacted monomers dissolved in the treatment liquid.
[0004] In recent years, there has been a demand for high-quality polyacetal copolymers that have excellent thermal stability and emit very little formaldehyde. To this end, studies have been conducted on efficient catalyst deactivation and stabilization of the crude polyacetal copolymers after catalyst deactivation by decomposition of unstable terminals.
[0005] For example, Patent Document 1 describes a method for producing a polyacetal copolymer, which includes a step of copolymerizing a copolymer using a predetermined heteropolyacid as a polymerization catalyst, and a step of adding a predetermined salt or a hydrate thereof to the obtained reaction product and melt-kneading the mixture to deactivate the polymerization catalyst. Patent Document 2 also describes that the use of a polymerization catalyst comprising a mixture of a predetermined heteropolyacid and a predetermined metal salt of a heteropolyacid can provide stable polymerization in industrial production.
[0006] JP 2014-105278 A JP 2019-178187 A
[0007] According to Patent Document 1, by using a predetermined highly active heteropolyacid as a polymerization catalyst and melt-kneading it together with a deactivator, polymerization becomes possible with a small amount of catalyst, complicated steps can be eliminated, the amount of formaldehyde generated is extremely small, and a high-quality polyacetal copolymer can be obtained. However, when the production amount of polyacetal resin was increased with a small amount of polymerization catalyst, a decrease in the polymerization yield of the polyacetal copolymer and variations in the quality of the polyacetal resin began to be observed.
[0008] According to Patent Document 2, the use of a polymerization catalyst containing a mixture of a specific heteropolyacid and a specific heteropolyacid metal salt stabilizes the polymerization reaction and improves the resin quality by reducing the amount of formaldehyde generated. However, molded articles made from the obtained polyacetal resin may have poor appearance, and an improvement in this regard has been desired.
[0009] The present invention has been made in view of the above points, and aims to provide a method for producing a polyacetal copolymer that can not only reduce the amount of formaldehyde generated but also has excellent flowability during molding and can be used to produce molded articles with excellent appearance, in a stable manner even in mass production.
[0010] As a result of extensive research, the present inventors have completed the inventions relating to the following [1] to [6].
[0011] [1] A method for producing a polyacetal copolymer, comprising copolymerizing trioxane and a comonomer copolymerizable with the trioxane in the presence of a polymerization catalyst, wherein the polymerization catalyst is a heteropolyacid (A) represented by the following general formula (1) and a heteropolyacid salt (B) represented by the following general formula (2), and the heteropolyacid (A) and the heteropolyacid salt (B) are used in combination:
[0012]
[0013] (In formulas (1) and (2), L is an alkali metal element, and M 1 and N 1 are each independently a central element of P or Si, and M 2 and M 3 are coordination elements of W, Mo or V which may be the same or different from each other, and N 2 and N 3 are coordination elements of W, Mo or V, which may be the same or different from each other, provided that M 2 and M 3 , and N 2 and N 3 At least one of the elements is a different coordination element. Here, p is an integer of 1 or more and 10 or less, q and r are positive integers, s is an integer of 10 or more and 100 or less, h is an integer of 1 or more, and i is an integer of 0 or more and 50 or less. v is an integer of 1 or more and 10 or less, w and x are positive integers, y is an integer of 10 or more and 100 or less, j is an integer of 1 or more, and k is an integer of 0 or more and 50 or less. However, M 2 and M 3 are the same coordination elements, q+r is an integer of 6 to 40, and N 2 and N 3 When the coordinate elements are the same, w+x is an integer of 6 or more and 40 or less.)
[0014] [2] The method for producing a polyacetal copolymer according to [1] above, wherein a mass ratio (B / A) of the heteropolyacid salt (B) to the heteropolyacid (A) is 0.2 to 10.
[0015] [3] The method for producing a polyacetal copolymer according to [1] or [2] above, wherein the heteropolyacid (A) is at least one selected from the group consisting of phosphomolybdic acid, phosphotungstic acid, phosphomolybdotungstic acid, phosphomolybdovanadic acid, phosphomolybdotungstovanadic acid, phosphotungstovanadic acid, silicotungstic acid, silicomolybdic acid, silicomolybdotungstic acid, and silicomolybdotungstovanadic acid.
[0016] [4] The method for producing a polyacetal copolymer according to [1] or [2] above, wherein the heteropolyacid salt (B) is at least one selected from the group consisting of lithium tungstophosphoric acid salt, sodium tungstophosphoric acid salt, potassium tungstophosphoric acid salt, sodium silicotungstate, sodium phosphomolybdate, and sodium tungstovanadate.
[0017] [5] The method for producing a polyacetal copolymer according to any one of [1] to [4] above, wherein the comonomer is at least one selected from the group consisting of 1,3-dioxolane, diethylene glycol formal, 1,4-butanediol formal, 1,3-dioxane, and ethylene oxide.
[0018] [6] A polyacetal copolymer produced by the production method according to any one of [1] to [5] above.
[0019] According to the present invention, it is possible to provide a production method that can stably produce, even in mass production, a polyacetal copolymer that not only can reduce the amount of formaldehyde generated but also has excellent flowability during molding and can be used to produce molded articles with excellent appearance.
[0020] Hereinafter, embodiments of the present invention will be described in detail, but the present invention is not limited to the following embodiments.
[0021] 1. Method for Producing Polyacetal Copolymer A method for producing a polyacetal copolymer according to one embodiment of the present invention is a method for producing a polyacetal copolymer by copolymerizing trioxane and a comonomer copolymerizable with trioxane in the presence of a polymerization catalyst. Each of the constituent components will be described below.
[0022] (Trioxane) Trioxane is a cyclic trimer of formaldehyde. Trioxane according to one embodiment of the present invention is used as a main monomer. Here, the main monomer refers to the monomer that is contained in the largest amount among all the monomers. Trioxane is generally obtained by reacting an aqueous formaldehyde solution in the presence of an acid catalyst, and is used after being purified by a method such as distillation.
[0023] (Comonomer) The comonomer according to one embodiment of the present invention is not particularly limited as long as it is copolymerizable with trioxane. The comonomer is preferably selected from the group consisting of cyclic ethers and cyclic formals having at least one carbon-carbon bond.
[0024] Examples of the comonomer include 1,3-dioxolane, diethylene glycol formal, 1,4-butanediol formal, 1,3-dioxane, ethylene oxide, propylene oxide, epichlorohydrin, etc. Among these, 1,3-dioxolane, diethylene glycol formal, 1,4-butanediol formal, 1,3-dioxane, and ethylene oxide are preferred from the viewpoint of polymerization stability.
[0025] Comonomers that can be used include compounds having two polymerizable cyclic ether groups or cyclic formal groups, such as diglycidyl ethers of alkylene glycols (e.g., butanediol diglycidyl ether) and diformals, and compounds having three or more polymerizable cyclic ether groups or cyclic formal groups, such as glycerin triglycidyl ether, trimethylolpropane triglycidyl ether, and pentaerythritol tetraglycidyl ether. By using these comonomers, polyacetal copolymers having a branched structure or a crosslinked structure can be obtained.
[0026] The content of the comonomer according to one embodiment of the present invention is preferably 0.01 to 20 parts by mass, and more preferably 0.05 to 5 parts by mass, relative to 100 parts by mass of trioxane. When the content of the comonomer is 0.01 to 20 parts by mass relative to 100 parts by mass of trioxane, polymerization can proceed stably, and a decrease in the crystallization rate and the degree of crystallization of the polymer chain can be suppressed.
[0027] (Polymerization catalyst) A polymerization catalyst according to one embodiment of the present invention is a heteropolyacid (A) represented by the following general formula (1) and a heteropolyacid salt (B) represented by the following general formula (2). In one embodiment of the present invention, the heteropolyacid (A) and the heteropolyacid salt (B) are used in combination.
[0028]
[0029] In the formulas (1) and (2), L is an alkali metal element, and the alkali metal element is preferably any one of lithium, sodium, and potassium. 1 and N 1 are each independently a central element of P or Si, and M 2 and M 3 are coordination elements of W, Mo or V which may be the same or different from each other, and N 2 and N 3 are coordination elements of W, Mo or V, which may be the same or different from each other, provided that M 2 and M 3 , and N 2 and N 3At least one of them is composed of a different coordination element. Here, p is an integer of 1 or more and 10 or less. q and r are positive integers. s is an integer of 10 or more and 100 or less, and preferably an integer of 30 or more and 80 or less. h is an integer of 1 or more and preferably an integer of 1 or more and 10 or less. i is an integer of 0 or more and 50 or less, and preferably an integer of 30 to 50 or less. Furthermore, v is an integer of 1 or more and 10 or less. w and x are positive integers. y is an integer of 10 or more and 100 or less, and preferably an integer of 30 to 80 or less. j is an integer of 1 or more and preferably an integer of 1 to 10 or less. k is an integer of 0 or more and 50 or less, and preferably an integer of 30 to 50 or less. However, M 2 and M 3 When N is the same coordination element, q+r is an integer of 6 or more and 40 or less, and preferably an integer of 10 or more and 20 or less. 2 and N 3 When the coordinate elements are the same, w+x is an integer of 6 or more and 40 or less, and preferably an integer of 10 or more and 20 or less.
[0030] Examples of the heteropolyacid (A) include phosphomolybdic acid, phosphotungstic acid, phosphomolybdotungstic acid, phosphomolybdovanadic acid, phosphomolybdotungstovanadic acid, phosphotungstovanadic acid, silicotungstic acid, silicomolybdic acid, silicomolybdotungstic acid, silicomolybdotungstovanadic acid, etc. Among these, from the viewpoints of polymerization stability and the stability of the heteropolyacid itself, phosphotungstic acid, phosphomolybdotungstovanadic acid, and phosphotungstovanadic acid are preferred, and phosphotungstovanadic acid is more preferred.
[0031] From the viewpoint of solubility in a solvent, the heteropolyacid salt (B) is preferably a salt of an alkali metal. Examples of such heteropolyacid salt (B) include lithium phosphotungstate, sodium phosphotungstate, potassium phosphotungstate, sodium silicotungstate, sodium phosphomolybdate, sodium phosphotungstovanadate, sodium silicotungstovanadate, etc. Among these, sodium phosphotungstate, sodium silicotungstate, sodium phosphomolybdate, and sodium phosphotungstovanadate are preferred.
[0032] The heteropolyacid (A) and the heteropolyacid salt (B) according to one embodiment of the present invention are used in combination. Examples of combinations of the heteropolyacid (A) and the heteropolyacid salt (B) include phosphotungstovanadic acid and sodium phosphotungstate, phosphotungstovanadic acid and lithium phosphotungstate, phosphotungstovanadic acid and potassium phosphotungstate, phosphomolybdotungstovanadic acid and sodium phosphotungstate, phosphotungstovanadic acid and sodium silicotungstate, phosphotungstovanadic acid and sodium phosphomolybdate, and phosphotungstic acid and sodium phosphotungstovanadate.
[0033] Among these, phosphotungstovanadic acid and sodium phosphotungstate, phosphomolybdotungstovanadic acid and sodium phosphotungstate, phosphotungstovanadic acid and sodium silicotungstate, phosphotungstovanadic acid and sodium phosphomolybdate, and phosphotungstic acid and sodium phosphotungstovanadate are preferred.
[0034] By using a mixture of the heteropolyacid (A) and the heteropolyacid salt (B), it is possible to reduce the amount of formaldehyde generated and also to obtain a polyacetal copolymer that has excellent flowability during molding and can be used to produce molded articles with excellent appearance.
[0035] The mass ratio (B / A) of the heteropolyacid salt (B) to the heteropolyacid (A) is preferably 0.2 to 10, more preferably 0.5 to 10. When the mass ratio (B / A) is 0.2 to 10, the flowability during molding is improved, and the appearance of the molded product is also improved.
[0036] The content of the polymerization catalyst according to one embodiment of the present invention is preferably 0.05 to 100 ppm, more preferably 0.1 to 50 ppm, relative to the total amount of the above-mentioned monomers (trioxane and comonomer). The content of the polymerization catalyst may be appropriately changed depending on the type of catalyst. Here, "ppm" represents "mass / mass ppm."
[0037] The polymerization catalyst is preferably used after diluting with a solvent inert to the polymerization reaction (hereinafter also referred to as "solvent"). The concentration of the polymerization catalyst diluted with the solvent is preferably 0.05 to 30% by mass, more preferably 0.1 to 20% by mass, and even more preferably 0.5 to 10% by mass. When the concentration of the diluted polymerization catalyst is 0.05 to 30% by mass, the polymerization catalyst can be sufficiently diffused in the monomer, allowing the polymerization reaction to be carried out uniformly.
[0038] Examples of the solvent include esters such as methyl formate, ethyl formate, methyl acetate, ethyl acetate, and butyl acetate, and ketones such as acetone, 2-butanone, 2-pentanone, 3-pentanone, 2-hexanone, 3-hexanone, methyl isobutyl ketone, and methyl t-butyl ketone. Of these, methyl formate, ethyl formate, methyl acetate, ethyl acetate, butyl acetate, acetone, 2-butanone, and methyl isobutyl ketone are preferred.
[0039] (Other Additives) In the method for producing a polyacetal copolymer according to one embodiment of the present invention, in addition to the above-mentioned components, it is preferable to use a known chain transfer agent for adjusting the degree of polymerization (molecular weight), such as methylal or butyral, and a hindered phenol-based antioxidant, such as triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate] or pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate].
[0040] (Method for Producing Polyacetal Copolymer) A method for producing a polyacetal copolymer according to one embodiment of the present invention is a method for copolymerizing trioxane with the above-described comonomer in the presence of the above-described polymerization catalyst (heteropolyacid (A) and heteropolyacid salt (B)).
[0041] The polyacetal copolymer according to one embodiment of the present invention can be produced using a known method and polymerization apparatus, such as a batch method or a continuous method.
[0042] In the batch polymerization apparatus, a reaction vessel equipped with a commonly used stirrer can be used. In addition, in the continuous polymerization apparatus, a co-kneader, a twin-screw continuous extrusion mixer, a twin-screw paddle screw extruder, a vented twin-screw extruder, etc. can be used. The continuous method is industrially preferred.
[0043] The polyacetal copolymer according to one embodiment of the present invention can be obtained, for example, by continuously supplying a mixed liquid containing trioxane, the comonomer described above, any additives for polymerization reaction, and a polymerization catalyst (heteropolyacid (A) and heteropolyacid salt (B)) to a continuous twin-screw paddle screw extruder-type polymerization reactor having a jacket for passing a heating or cooling medium, and polymerizing the mixed liquid for a predetermined period of time.
[0044] Furthermore, a basic compound such as an alkali metal compound, a quaternary amine compound, or a triazine compound having an amino group can be added to the polyacetal copolymer obtained by the above-mentioned method, and the mixture can be melt-kneaded and subjected to a catalyst deactivation treatment or the like to obtain a desired polyacetal copolymer.
[0045] In addition, during catalyst deactivation treatment, other components may be added as appropriate depending on the required performance, such as other polymers, other fillers, nitrogen compounds, stabilizers such as ultraviolet absorbers, anti-acid agents such as metal salts, antistatic agents, flame retardants, colorants such as dyes and pigments, lubricants, mold release agents, crystallization accelerators, crystal nucleating agents, etc. One type of other component may be used alone, or two or more types may be used in combination.
[0046] A method for producing a polyacetal copolymer according to one embodiment of the present invention uses a mixture of a heteropolyacid (A) and a heteropolyacid salt (B) as a polymerization catalyst, thereby making it possible to not only reduce the amount of formaldehyde generated but also stably mass-produce a polyacetal copolymer that has excellent flowability during molding and can be used to produce molded articles with excellent appearance.
[0047] 2. Polyacetal Copolymer A polyacetal copolymer according to one embodiment of the present invention is a copolymer produced by the production method of the present invention. That is, the polyacetal copolymer is obtained by copolymerizing trioxane and the above-described comonomer in the presence of a polymerization catalyst (heteropolyacid (A) and heteropolyacid salt (B)).
[0048] The polyacetal copolymer obtained by the production method according to one embodiment of the present invention has excellent flowability during molding. Furthermore, molded articles produced from the polyacetal copolymer can reduce the amount of formaldehyde emitted and have excellent appearance.
[0049] The present invention will be specifically explained below with reference to examples, but the present invention is not limited to these examples.
[0050] 1. Production of Polyacetal Copolymers 1 to 22 [Polyacetal Copolymer 1] (Polymerization Apparatus) A continuous twin-screw paddle screw extruder (hereinafter also referred to as "polymerization apparatus") was used as the polymerization apparatus. The extruder has a jacket on the outside of the body for passing a heating or cooling medium. The body is divided into upper and lower parts, and the upper part can be opened. Inside the extruder, two rotating shafts equipped with numerous paddles for stirring and propulsion are provided in the longitudinal direction.
[0051] (Production Method) A mixed liquid containing 100 parts by mass of trioxane (TOX), 4.0 parts by mass of 1,3-dioxolane (DO), and a predetermined amount of methylal was continuously supplied per unit time to a polymerization apparatus heated by passing a medium at 80°C through the jacket, and a mixture of 2.5 ppm of tungstovanadic phosphonate (A1) as the heteropolyacid (A) and 0.6 ppm of sodium tungstophosphoric acid salt (B1) as the heteropolyacid salt (B) was added as a methyl formate solution to carry out a polymerization reaction.
[0052] To the crude polymer obtained from the discharge outlet of the polymerization apparatus, 0.1 mass % of melamine and 0.3 mass % of IRGANOX 1010 (manufactured by BASF Japan, "IRGANOX" is a registered trademark of BASF) were added, and the mixture was continuously melt-kneaded and extruded using a vented twin-screw extruder under conditions of a cylinder temperature of 220°C and a vacuum degree of 5 mmHg in the vent section, to obtain pellets of polyacetal copolymer 1.
[0053] The amount of methylal added was adjusted so that the melt flow rate (MFR) of the resulting copolymer was 9 g / 10 min. Here, "9 g" refers to the range of "9 g ± 0.3". The MFR was measured in accordance with ISO 1133 using a Melt Indexer L220 (manufactured by Tateyama Scientific High-Technologies Co., Ltd.) under conditions of a load of 2.16 kg, a temperature of 190 °C, and a discharged resin acquisition time of 7 minutes.
[0054] [Polyacetal Copolymers 2 to 8] Pellets of polyacetal copolymers 2 to 8 were obtained by the same production method as for polyacetal copolymer 1, except that the amount of heteropolyacid (A) and / or heteropolyacid salt (B) added and the amount of methylal added were changed so that the MFR of the resulting copolymer would be 9 g / 10 min, as shown in Table 1.
[0055] [Polyacetal Copolymer 9] Pellets of polyacetal copolymer 9 were obtained by the same production method as for polyacetal copolymer 1, except that the type of comonomer, the amount of heteropolyacid salt (B) added, and the amount of methylal added were changed so that the MFR of the resulting copolymer would be 9 g / 10 min, as shown in Table 1.
[0056] [Polyacetal Copolymers 10 to 14] Pellets of polyacetal copolymers 10 to 14 were obtained by the same production method as for polyacetal copolymer 1, except that the type of heteropolyacid salt (B) and the amount of methylal added were changed so that the MFR of the resulting copolymer would be 9 g / 10 min, as shown in Table 1.
[0057] [Polyacetal Copolymers 15 to 17, 19, and 20] Pellets of polyacetal copolymers 15 to 17, 19, and 20 were obtained by the same production method as for polyacetal copolymer 1, except that the type of heteropolyacid salt (A), the amount of heteropolyacid salt (B) added, and the amount of methylal added so that the MFR of the resulting copolymer would be 9 g / 10 min were changed as shown in Table 1.
[0058] [Polyacetal Copolymer 18] Pellets of polyacetal copolymer 18 were obtained by the same production method as for polyacetal copolymer 1, except that the type of heteropolyacid salt (A), the type of heteropolyacid salt (B), and the amount of methylal added were changed so that the MFR of the resulting copolymer would be 9 g / 10 min, as shown in Table 1.
[0059] [Polyacetal Copolymer 21] A mixed liquid containing 100 parts by mass of trioxane (TOX), 4.0 parts by mass of 1,3-dioxolane (DO), and a predetermined amount of methylal was continuously supplied to the above-mentioned polymerization apparatus per unit time, and 3.3 ppm of phosphotungstic acid (A5) was added as a heteropolyacid (A) in the form of a methyl formate solution, to carry out a polymerization reaction.
[0060] To the crude polymer obtained from the discharge port of the polymerization apparatus, 0.1 mass % of melamine and 0.3 mass % of IRGANOX 1010 were added, and the mixture was continuously melt-kneaded and extruded using a vented twin-screw extruder under conditions of 220°C and a vacuum degree of 5 mmHg at the vent section, to obtain pellets of polyacetal copolymer 21.
[0061] The amount of methylal added was adjusted in the same manner as in the case of polyacetal copolymer 1.
[0062] [Polyacetal Copolymer 22] A mixed solution containing 100 parts by mass of trioxane (TOX), 4.0 parts by mass of 1,3-dioxolane (DO), and a predetermined amount of methylal was continuously supplied to the above-mentioned polymerization apparatus per unit time, and 30 ppm of boron trifluoride (C) was added to carry out a polymerization reaction. Next, the crude polymer obtained from the discharge port of the polymerization apparatus was added to an aqueous solution containing 0.1% triethylamine to terminate the polymerization reaction, and the copolymer was then dried. Note that boron trifluoride (C) was added as a 0.3 wt % cyclohexane solution of a dibutyl ether complex.
[0063] To the dried copolymer, 0.1% by mass of melamine and 0.3% by mass of IRGANOX 1010 were added, and the mixture was continuously melt-kneaded and extruded using a vented twin-screw extruder under conditions of 220°C and a vacuum degree of 5 mmHg at the vent section, to obtain pellets of polyacetal copolymer 22.
[0064] The amount of methylal added was adjusted in the same manner as in the case of polyacetal copolymer 1.
[0065] The heteropolyacid (A), heteropolyacid salt (B) and Lewis acid (C) used in the above-described production method are compounds shown in Table 1.
[0066] 2. Evaluation Polyacetal copolymers 1 to 22 obtained by the above-mentioned production method were evaluated for the polymerization yield of the polyacetal copolymer, the appearance of molded articles using the polyacetal copolymer, the amount of formaldehyde generated, and bar flow (BF).
[0067] [Polymerization Yield of Polyacetal Copolymer] (Evaluation Method) The reaction product discharged from the discharge port of the polymerization apparatus was continuously collected for a certain period of time, and each sample was added to an aqueous solution containing 0.1% triethylamine. The mixture was stirred for a predetermined period of time to deactivate the catalyst and wash away unreacted monomers. The aqueous solution was then filtered, and the resulting crude polymer was washed with acetone and dried. The polyacetal copolymer yield, which is the ratio of the copolymer obtained to the total monomers, was calculated from the weight of the dried polyacetal copolymer. A polymerization yield of 70% or more is practically preferred for the polyacetal copolymer.
[0068] [Formaldehyde Emission Amount from Melt] (Evaluation Method) 5 g of each of polyacetal copolymers 1 to 22 was filled into a cylinder maintained at 200°C and held in a molten state for 5 minutes. The polyacetal copolymer melts were then extruded into sealed containers. Nitrogen gas was passed through the sealed containers, and the formaldehyde contained in the nitrogen gas was dissolved in water and collected. The formaldehyde concentration in the water was measured in accordance with JIS K0102 (2013), to determine the mass of formaldehyde from the melt. The mass of formaldehyde was divided by the mass of the polyacetal copolymer used to determine the amount of formaldehyde emitted (unit: ppm). A formaldehyde emission amount of 70 ppm or less is practically preferred.
[0069] [Evaluation of Appearance of Molded Articles] (Evaluation Method) Polyacetal copolymers 1 to 22 were each injection molded into a 50mm square, 3t flat plate with a φ1.5mm center single pin gate under the following conditions using a molding machine (FANUC injection molding machine "S100iA (φ36)") After that, the size of the flow marks near the gate of the molded article was measured, and the appearance was evaluated on a 5-point scale.
[0070] (Molding conditions) Cylinder temperature (nozzle head temperature: 200°C) Mold temperature: 90°C Holding pressure: 75 MPa Injection time: 4.5 seconds Injection conditions: Metering position: 20 mm, Suck back: 5 mm, VP switching position: 8 mm
[0071] (Evaluation) 5: The size of the flow mark is less than 6 mm. 4: The size of the flow mark is 6 mm or more and less than 8 mm. 3: The size of the flow mark is 8 mm or more and less than 10 mm. 2: The size of the flow mark is 10 mm or more and less than 12 mm. 1: The size of the flow mark is 12 mm or more.
[0072] [Bar Flow Evaluation] (Evaluation Method) Using an injection molding machine (ES3000, manufactured by Nissei Plastic Industrial Co., Ltd.), each of the polyacetal copolymers 1 to 22 was injected into an evaluation mold having a thickness of 2 mmt, and the flow length was measured. The flow length (unit: mm) at each injection pressure was evaluated on a 5-point scale.
[0073] (Molding conditions) Cylinder temperature (nozzle head temperature: 195°C) Mold temperature: 80°C Injection speed: 70 mm / s Injection pressure: 100 MPa
[0074] (Evaluation) 5: The flow length is 450 mm or more at an injection pressure of 100 MPa. 4: The flow length is 440 mm or more and less than 450 mm at an injection pressure of 100 MPa. 3: The flow length is 430 mm or more and less than 440 mm at an injection pressure of 100 MPa. 2: The flow length is 420 mm or more and less than 430 mm at an injection pressure of 100 MPa. 1: The flow length is less than 420 mm at an injection pressure of 100 MPa.
[0075] [Measurement of MFR] In the production of polyacetal copolymers 1 to 22, the MFR, which is an index of the fluidity of the resulting crude polymer when melted, was determined as follows: (Measurement method) Using a Melt Indexer L220 manufactured by Tateyama Scientific High-Technologies Co., Ltd., measurement was performed under conditions in accordance with ISO 1133, with a load of 2.16 kg, a temperature of 190°C, and a discharged resin collection time of 7 minutes.
[0076] The main constituent components of polyacetal copolymers 1 to 22 and the evaluation results are shown in Table 1. The abbreviations and names of the heteropolyacid (A), heteropolyacid salt (B), and Lewis acid (C) in Table 1 are as follows:
[0077] (Main monomer) TOX: Trioxane (Comonomer) DO: 1,3-dioxolane BDF: 1,4-butanediol formal
[0078] [Polymerization catalyst] (heteropolyacid (A)) A1:H 5 PV 2 W 10 O 40 (phosphotungstovanadic acid) A2:H 4 PV 1 W 11 O 40 (phosphotungstovanadic acid) A3:H 6 PV 3 W 9 O 40 (phosphotungstovanadic acid) A4:H 3 PMo 2 W 10 O 4 (phosphomolybdotungstic acid) A5:H 3 P.W. 12 O 40 (phosphotungstic acid)
[0079] (Heteropolyacid salt (B)) B1: Na 3 P.W. 12 O 40 (Sodium phosphotungstate) B2: Li 3 P.W. 12 O 40 (lithium phosphotungstate) B3:K 3 P.W. 12 O 40 (Potassium phosphotungstate) B4: NaSiW 12 O 40 (Sodium silicotungstate) B5: Na 3 PMo 12 O 40 (Sodium phosphomolybdate) B6: Na 3 PV 2 W 10 O 40 (Sodium phosphotungstovanadate)
[0080] (Lewis acid (C)) C: BF 3 (boron trifluoride)
[0081] (Evaluation items) HCHO: Formaldehyde BF: Bar flow
[0082]
[0083] From Table 1, it was found that by using a mixture of heteropolyacid (A) and heteropolyacid salt (B) as a polymerization catalyst, not only the amount of formaldehyde generated can be reduced, but also a polyacetal copolymer can be produced with stable polymerization yield and quality even in mass production. 5 PV 2 W 10 O 40 (phosphotungstovanadic acid), heteropolyacid salt (B) containing Na 3 P.W. 12 O 40 It was found that the best results were obtained in all evaluation items when sodium phosphotungstate was used.
[0084] The method of the present invention not only reduces the amount of formaldehyde generated but also enables stable mass production of polyacetal copolymers that have excellent flowability during molding and excellent appearance in molded products, and is therefore expected to contribute to the advancement and spread of technology in this field.
Claims
1. A method for producing a polyacetal copolymer, comprising copolymerizing trioxane and a comonomer copolymerizable with said trioxane in the presence of a polymerization catalyst, wherein the polymerization catalyst is a heteropolyacid (A) represented by the following general formula (1) and a heteropolyacid salt (B) represented by the following general formula (2), and the heteropolyacid (A) and the heteropolyacid salt (B) are used in combination: (In formulas (1) and (2), L is an alkali metal element, and M 1 and N 1 are each independently a central element of P or Si, and M 2 and M 3 are coordination elements of W, Mo or V which may be the same or different from each other, and N 2 and N 3 are coordination elements of W, Mo or V, which may be the same or different from each other, provided that M 2 and M 3 , and N 2 and N 3 At least one of the elements is a different coordination element. Here, p is an integer of 1 or more and 10 or less, q and r are positive integers, s is an integer of 10 or more and 100 or less, h is an integer of 1 or more, and i is an integer of 0 or more and 50 or less. v is an integer of 1 or more and 10 or less, w and x are positive integers, y is an integer of 10 or more and 100 or less, j is an integer of 1 or more, and k is an integer of 0 or more and 50 or less. However, M 2 and M 3 are the same coordination elements, q+r is an integer of 6 to 40, and N 2 and N 3 When the coordinate elements are the same, w+x is an integer of 6 or more and 40 or less.) 2. The method for producing a polyacetal copolymer according to claim 1, wherein the mass ratio (B / A) of the heteropolyacid salt (B) to the heteropolyacid (A) is 0.2 to 10.
3. The method for producing a polyacetal copolymer according to claim 1 or 2, wherein the heteropolyacid (A) is at least one selected from the group consisting of phosphomolybdic acid, phosphotungstic acid, phosphomolybdotungstic acid, phosphomolybdovanadic acid, phosphomolybdotungstovanadic acid, phosphotungstovanadic acid, silicotungstic acid, silicomolybdic acid, silicomolybdotungstic acid and silicomolybdotungstovanadic acid.
4. The method for producing a polyacetal copolymer according to claim 1 or 2, wherein the heteropolyacid salt (B) is at least one selected from the group consisting of lithium phosphotungstate, sodium phosphotungstate, potassium phosphotungstate, sodium silicotungstate, sodium phosphomolybdate, and sodium phosphotungstovanadate.
5. The method for producing a polyacetal copolymer according to claim 1, wherein the comonomer is at least one selected from the group consisting of 1,3-dioxolane, diethylene glycol formal, 1,4-butanediol formal, 1,3-dioxane, and ethylene oxide.
6. A polyacetal copolymer produced by the method of claim 1.