Polishing liquid composition for magnetic disk substrate

MYPI2025002780A0Undetermined Publication Date: 2024-05-08KAO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025002780
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-11-08
Filing Date
2023-11-01
Publication Date
2024-05-08

AI Technical Summary

Technical Problem

The increasing demand for higher recording densities in magnetic disk drives requires more stringent surface quality of magnetic disk substrates, with a trade-off between polishing rate and scratches, and existing polishing liquids lack excellent dispersion stability.

Method used

A polishing liquid composition containing silica particles with a specific silicon atom concentration range, measured by X-ray photoelectron spectroscopy, combined with an acid and water, which improves polishing rate and reduces scratches while maintaining excellent dispersion stability.

Benefits of technology

The composition enhances polishing efficiency by increasing the frequency of silica particle contact with the substrate, reducing scratches, and ensuring stable dispersion, thereby producing high-quality magnetic disk substrates with improved yield and productivity.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

One aspect of the present disclosure provides a polishing liquid composition that is capable of achieving both the improvement in polishing speed and reduction of scratches on polished substrate surfaces and also excellent in dispersion stability. Viewed from one aspect, the present disclosure relates to a polishing liquid composition for a magnetic disk substrate, containing silica particles (component A), an acid (component B), and water, wherein a silicon atom concentration in the component A as measured by X-ray photoelectron spectroscopy (XPS) at a detection angle of 15° is 28 atom% or more and 38 atom% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Polishing composition for magnetic disk substrates

[0001] The present disclosure relates to a polishing composition for magnetic disk substrates, and a method for manufacturing and polishing magnetic disk substrates using the same.

[0002] In recent years, magnetic disk drives have become smaller and their capacities have increased, resulting in a demand for higher recording densities. To achieve higher recording densities, technological developments are underway to reduce the unit recording area and lower the flying height of the magnetic head to improve the detection sensitivity of weakened magnetic signals. To accommodate the lower flying height of the magnetic head and ensure a sufficient recording area, magnetic disk substrates are increasingly being required to improve smoothness and flatness, such as reducing surface roughness, waviness, and edge sagging (roll-off), as well as to reduce defects, such as scratches, protrusions, and pits.

[0003] For example, Japanese Patent Laid-Open No. 2012-11869 (Patent Document 1) describes a silica sol having a solid content concentration of 10 to 60 mass %, which is obtained by dispersing non-spherical silica fine particles having an average particle diameter in the range of 5 to 300 nm as measured by a dynamic light scattering method in a dispersion medium, 29 A polishing silica sol has been proposed in which the area of ​​Q4 in the peak area of ​​the chemical shift of -73 to -120 ppm in Si-NMR spectrum measurement is 88% or more and the area of ​​Q3 is 11% or less. International Publication No. 2015 / 046603 (Patent Document 2) proposes a method for manufacturing a magnetic disk substrate, which includes a polishing process in which a polishing liquid containing silica abrasive grains as free abrasive grains is supplied between the main surface of a glass substrate and a polishing pad to polish the main surface of the glass substrate, wherein the silica abrasive grains have a ratio (Si-OH) / Si of silanol groups (Si-OH) inside the abrasive grains to elemental silicon (Si) in the entire abrasive grains of 0.4 or more. Japanese Patent Laid-Open Publication No. 2017-19978 (Patent Document 3) proposes a polishing composition containing silica abrasive grains, wherein the silica abrasive grains have an average primary particle size of 40 nm or more and an average silanol group density of 1.25 / nm 2 The following polishing composition has been proposed.

[0004] In one aspect, the present disclosure relates to a polishing liquid composition for magnetic disk substrates, which contains silica particles (component A), an acid (component B), and water, wherein component A has a silicon atom concentration (atom %) of 28 atom % or more and 38 atom % or less, as measured by X-ray photoelectron spectroscopy (XPS) at a detection angle of 15°.

[0005] In one aspect, the present disclosure relates to a method for polishing a substrate, comprising a step of polishing a substrate to be polished with the polishing liquid composition of the present disclosure, wherein the substrate to be polished is a substrate used in the manufacture of magnetic disk substrates.

[0006] In one aspect, the present disclosure relates to a method for producing a magnetic disk substrate, comprising the steps of selecting silica particles (component A) having a silicon atom concentration (atom %) of 28 atom % or more and 38 atom % or less, as measured by X-ray photoelectron spectroscopy (XPS) at a detection angle of 15°, a slurry of the silica particles (component A), or a polishing liquid composition containing the silica particles (component A) as abrasive grains, and obtaining a polishing liquid composition containing the silica particles (component A), an acid (component B), and water; and polishing a substrate to be polished using the polishing liquid composition containing the silica particles (component A), an acid (component B), and water.

[0007] With the increase in the capacity of magnetic disk drives, the required characteristics for the surface quality of substrates are becoming more stringent, and there is a demand for the development of a polishing composition that can further reduce scratches on the substrate surface. In addition, there is generally a trade-off between removal rate and scratches, and there is a problem that improving one will worsen the other. Furthermore, from the viewpoint of improving productivity, the polishing composition is also required to have excellent dispersion stability.

[0008] Therefore, in one aspect, the present disclosure provides a polishing composition that can improve the removal rate and reduce scratches on the substrate surface after polishing, and that has excellent dispersion stability.

[0009] In one aspect, the present disclosure can provide a polishing composition that can improve the removal rate and reduce scratches on the substrate surface after polishing, and that has excellent dispersion stability.

[0010] This disclosure is based on the finding that when a polishing composition containing silica particles, acid, and water, whose silicon atom concentration (atom%) measured by X-ray photoelectron spectroscopy (XPS) at a detection angle of 15° is within a specific range, is used to polish a magnetic disk substrate, the polishing rate can be improved, scratches on the substrate surface after polishing can be reduced, and dispersion stability can be improved. In this disclosure, the silicon atom concentration (atom%) measured by X-ray photoelectron spectroscopy (XPS) at a detection angle of 15° refers to the percentage of the silicon atom concentration relative to the total silicon atom (Si) concentration and oxygen atom (O) concentration [Si / (Si+O)] × 100, which is calculated by elemental analysis of the spectrum obtained by measuring component A using XPS at a detection angle of 15°. Here, X-ray photoelectron spectroscopy (XPS) is a surface analysis method that measures the kinetic energy of photoelectrons emitted when a sample surface is irradiated with soft X-rays. Because elements have their own specific kinetic energy, it is possible to identify elements at a depth of a few nanometers from the surface and analyze their element concentration. In XPS, the measurement depth can be adjusted by changing the detection angle. The smaller the angle between the sample and the detector (detection angle), the smaller the measurement depth, making it possible to measure near the surface of the sample. The larger the detection angle, the greater the measurement depth, making it possible to measure deeper into the sample.

[0011] That is, in one aspect, the present disclosure relates to a polishing liquid composition for magnetic disk substrates (hereinafter also referred to as "the polishing liquid composition of the present disclosure") that contains silica particles (component A), an acid (component B), and water, in which component A has a silicon atom concentration (atom %) of 28 atom % or more and 38 atom % or less relative to the total of the silicon atom concentration and the oxygen atom concentration, as measured by X-ray photoelectron spectroscopy (XPS) at a detection angle of 15°.

[0012] Although the details of the mechanism by which the effects of the present disclosure are realized are unclear, it is speculated as follows. Measurements using X-ray photoelectron spectroscopy (XPS) at a detection angle of 15° are elemental analysis of the extreme surface layer of the target silica particles, and it is presumed that a high silicon atom concentration (atom%) indicates a relatively low oxygen element ratio. It is presumed that a high oxygen element concentration also attracts more water molecules in the system, hindering direct interaction between the silica particles and the substrate during polishing. Therefore, it is presumed that the high silicon atom concentration present in the extreme surface layer of the silica particles allows direct interaction between the silica particles and the substrate, thereby achieving a good polishing rate. Furthermore, when the oxygen element concentration in the extreme surface layer of the target silica particles decreases, the water molecules in the system also decrease relatively, but this does not affect the silica particles to the extent that they come into contact with each other, so the silica particles are stably dispersed in water. In addition, the decrease in water molecules between the silica particles narrows the distance between the silica particles, thereby increasing the frequency of contact between the silica particles and the substrate being polished. It is presumed that the increased contact frequency between the silica particles and the substrate being polished causes the stress of the silica particles to be dispersed from the depth direction to the entire substrate surface, thereby suppressing the generation of localized stress on the substrate surface and reducing scratches. However, the present disclosure need not be interpreted as being limited to these mechanisms.

[0013] In the present disclosure, scratches on the substrate surface can be detected, for example, by an optical defect inspection device and quantitatively evaluated as the number of scratches. The number of scratches can be specifically evaluated by the method described in the Examples.

[0014] [Silica Particles (Component A)] The polishing composition of the present disclosure contains silica particles (hereinafter also referred to as "Component A") as abrasive grains. Component A is silica particles having a silicon atom concentration (atom %) of 28 atom % or more and 38 atom % or less, as measured by X-ray photoelectron spectroscopy (XPS) at a detection angle of 15°. Component A is preferably used in the form of a slurry polishing liquid component. Component A may be one type or a combination of two or more types.

[0015] <Silicon atom (Si) concentration (atom %) measured by XPS under the condition of a detection angle of 15°> From the viewpoint of improving the polishing rate, the silicon atom concentration (atom %) is 28 atom % or more, preferably 29 atom % or more, and more preferably 30 atom % or more, and from the viewpoint of reducing scratches, it is 38 atom % or less, preferably 36 atom % or less, and more preferably 34 atom % or less. More specifically, the silicon atom concentration (atom %) measured by XPS under the condition of a detection angle of 15° is 28 atom % or more and 38 atom % or less, preferably 29 atom % or more and 36 atom % or less, and more preferably 30 atom % or more and 34 atom % or less. In the present disclosure, the silicon atomic concentration (atom %) measured by XPS at a detection angle of 15° refers to the percentage of the silicon atomic concentration relative to the total of the silicon atomic (Si) concentration and the oxygen atomic (O) concentration calculated by elemental analysis of the spectrum obtained by measuring component A using XPS at a detection angle of 15° [Si / (Si+O)] × 100. From the viewpoint of improving the polishing rate, the silicon atomic concentration (atom %) measured by XPS at a detection angle of 45° is preferably 28 atom % or more, more preferably 28.5 atom % or more, and even more preferably 29 atom % or more, and from the viewpoint of reducing scratches, is preferably 36 atom % or less, more preferably 34 atom % or less, and even more preferably 32 atom % or less. More specifically, the silicon atomic concentration (atom %) measured by XPS at a detection angle of 45° is preferably 28 atom % or more and 36 atom % or less, more preferably 28.5 atom % or more and 34 atom % or less, and even more preferably 29 atom % or more and 32 atom % or less. In the present disclosure, the silicon atomic concentration (atom %) measured by XPS at a detection angle of 45° refers to the percentage of the silicon atomic concentration to the sum of the silicon atomic (Si) concentration and the oxygen atomic (O) concentration [Si / (Si+O)] × 100, which is calculated by elemental analysis of the spectrum obtained by measuring component A using XPS at a detection angle of 45°.The silicon atomic concentration (atom %) measured by XPS at a detection angle of 75° is preferably 28 atom % or more, more preferably 28.2 atom % or more, and even more preferably 28.4 atom % or more from the viewpoint of improving the polishing rate, and is preferably 36 atom % or less, more preferably 35.5 atom % or less, and even more preferably 35.0 atom % or less from the viewpoint of improving dispersion stability. More specifically, the silicon atomic concentration (atom %) measured by XPS at a detection angle of 75° is preferably 28 atom % or more and 36 atom % or less, more preferably 28.2 atom % or more and 35.5 atom % or less, and even more preferably 28.4 atom % or more and 35.0 atom % or less. In the present disclosure, the silicon atom concentration (atom %) measured by XPS at a detection angle of 75° refers to the percentage of the silicon atom concentration to the total of the silicon atom (Si) concentration and the oxygen atom (O) concentration [Si / (Si+O)]×100, which is calculated by elemental analysis of the spectrum obtained by measuring component A using XPS at a detection angle of 75°.

[0016] The concentration ratio (15° / 45°) of the silicon atomic concentration (atom%) measured by XPS at a detection angle of 15° to the silicon atomic concentration (atom%) measured by XPS at a detection angle of 45° is preferably 1.02 or more, more preferably 1.025 or more, and even more preferably 1.03 or more, from the viewpoint of improving the polishing rate, and is preferably 1.4 or less, more preferably 1.3 or less, and even more preferably 1.2 or less, from the viewpoint of reducing scratches. More specifically, the concentration ratio (15° / 45°) is preferably 1.02 or more and 1.4 or less, more preferably 1.025 or more and 1.3 or less, and even more preferably 1.03 or more and 1.2 or less. The concentration ratio (15° / 75°) of the silicon atomic concentration (atom%) measured by XPS at a detection angle of 15° to the silicon atomic concentration (atom%) measured by XPS at a detection angle of 75° is preferably 1.05 or more, more preferably greater than 1.05, even more preferably 1.06 or more, and even more preferably 1.07 or more, from the viewpoint of improving the polishing rate, and is preferably 1.4 or less, more preferably 1.3 or less, even more preferably 1.2 or less, even more preferably 1.15 or less, and even more preferably 1.10 or less, from the viewpoint of reducing scratches. More specifically, the concentration ratio (15° / 75°) is preferably 1.05 or more and 1.4 or less, more preferably 1.06 or more and 1.3 or less, even more preferably 1.07 or more and 1.2 or less, even more preferably 1.07 or more and 1.15 or less, and even more preferably 1.07 or more and 1.10 or less.

[0017] In the present disclosure, the concentrations of each atom (Si, O) measured by XPS can be measured using an XPS measurement device manufactured by ULVAC-PHI, Inc., which uses ALKα radiation as characteristic X-rays. The silicon atom (Si) concentration can be calculated, for example, by performing elemental analysis of a spectrum obtained by XPS at a predetermined detection angle (15°, 45°, 75°) in a binding energy range of 96 to 106 eV. The oxygen atom (O) concentration can be calculated, for example, by performing elemental analysis of a spectrum obtained by XPS at a predetermined detection angle (15°, 45°, 75°) in a binding energy range of 526 to 536 eV. Specifically, the concentration can be calculated using the measurement method described in the Examples.

[0018] Component A can be produced, for example, by mixing an alkali silicate and a strong acid to prepare a solution containing silica hydrogel, aging the silica at a predetermined temperature range (e.g., 10 to 40°C), removing the salt from the solution, adding an alkali solution to the silica hydrogel to colloidize the silica hydrogel to obtain a silica sol, and then hydrothermally treating the silica sol to grow silica particles. There are several methods for adjusting the silicon atom concentration of component A, but one example is controlling the hydrothermal treatment conditions during the silica particle growth process. Examples of hydrothermal treatment conditions include adjusting the pH using an alkaline agent such as sodium hydroxide, and controlling the heating temperature and pressure using an apparatus. Alternatively, the silicon atom concentration on the silica particle surface can be controlled by varying the pH using an alkaline agent such as sodium hydroxide as described above and storing the resulting aqueous solution over time.

[0019] From the viewpoints of improving the polishing rate and reducing scratches, examples of Component A include colloidal silica, fumed silica, pulverized silica, and surface-modified silica thereof, of which colloidal silica is preferred. In one or more embodiments, from the viewpoints of improving the polishing rate and reducing scratches, the abrasive grains contained in the polishing composition of the present disclosure are preferably only Component A, and more preferably only colloidal silica.

[0020] The shape of component A may be spherical or non-spherical.

[0021] In one or more embodiments, when used for finish polishing, the average primary particle diameter of Component A is preferably 5 nm or more from the viewpoint of improving the polishing rate and reducing scratches, and from the same viewpoint, it is preferably 100 nm or less, more preferably 40 nm or less. More specifically, the average primary particle diameter of Component A is preferably 5 nm or more and 100 nm or less, more preferably 5 nm or more and 40 nm or less. In one or more embodiments, when used for rough polishing, the average primary particle diameter of Component A is preferably 30 nm or more, more preferably 40 nm or more, even more preferably 50 nm or more from the viewpoint of improving the polishing rate, and from the same viewpoint, it is preferably 200 nm or less, more preferably 180 nm or less, even more preferably 160 nm or less. More specifically, in one or more embodiments, the average primary particle diameter of Component A is preferably 30 nm or more and 200 nm or less, more preferably 40 nm or more and 180 nm or less, even more preferably 50 nm or more and 160 nm or less. In the present disclosure, the average primary particle diameter of component A is determined by the specific surface area S (m 2 The average primary particle size is calculated using the formula (1 / g). The average primary particle size is a value measured by the method described in the examples.

[0022] The content of component A in the polishing liquid composition of the present disclosure is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, from the viewpoint of improving the polishing rate, and is preferably 15% by mass or less, more preferably 12% by mass or less, and even more preferably 9% by mass or less, from the viewpoint of reducing scratches. More specifically, the content of component A in the polishing liquid composition of the present disclosure is preferably 1% by mass or more and 15% by mass or less, more preferably 2% by mass or more and 12% by mass or less, and even more preferably 3% by mass or more and 9% by mass or less. When component A consists of two or more types of silica particles, the content of component A refers to the total content thereof.

[0023] [Acid (Component B)] The polishing liquid composition of the present disclosure contains an acid (Component B). In the present disclosure, the use of an acid includes the use of an acid or a salt thereof. Component B may be one type or a combination of two or more types.

[0024] Examples of component B include inorganic acids such as nitric acid, sulfuric acid, sulfurous acid, persulfuric acid, hydrochloric acid, perchloric acid, phosphoric acid, phosphonic acid, phosphinic acid, pyrophosphoric acid, tripolyphosphoric acid, and amidosulfuric acid; and organic acids such as organic phosphoric acid, organic phosphonic acid, and carboxylic acid. Among these, from the viewpoint of improving the polishing rate and reducing scratches, it is preferable to contain an inorganic acid and an organic phosphonic acid, and it is preferable to contain an inorganic acid. From the same viewpoint, the content of the inorganic acid in component B is preferably 0.5 mass% or more, more preferably 0.75 mass% or more, and even more preferably 1.0 mass% or more. From the same viewpoint, the inorganic acid is preferably at least one selected from nitric acid, sulfuric acid, hydrochloric acid, perchloric acid, and phosphoric acid, more preferably at least one selected from sulfuric acid and phosphoric acid, and even more preferably phosphoric acid. From the same viewpoint, the organic phosphonic acid is preferably at least one selected from 1-hydroxyethylidene-1,1-diphosphonic acid (HEDP), aminotri(methylenephosphonic acid), ethylenediaminetetra(methylenephosphonic acid), and diethylenetriaminepenta(methylenephosphonic acid), with HEDP being more preferred. Examples of salts of these acids include salts of the above acids with at least one selected from metals, ammonia, and alkylamines. Examples of the above metals include metals belonging to Groups 1 to 11 of the periodic table. Among these, from the viewpoints of improving the polishing rate and reducing scratches, salts of the above acids with metals belonging to Group 1A or ammonia are preferred.

[0025] The content of component B in the polishing composition of the present disclosure is preferably 0.5 mass% or more, more preferably 0.75 mass% or more, and even more preferably 1.0 mass% or more, from the viewpoint of the removal rate, and is preferably 5.0 mass% or less, more preferably 4.0 mass% or less, and even more preferably 3.0 mass% or less, from the viewpoint of scratches. More specifically, the content of component B in the polishing composition of the present disclosure is preferably 0.5 mass% or more and 5.0 mass% or less, more preferably 0.75 mass% or more and 4.0 mass% or less, and even more preferably 1.0 mass% or more and 3.0 mass% or less. When component B is a combination of two or more types, the content of component B refers to the total content thereof.

[0026] [Water] The polishing composition of the present disclosure contains water as a medium. Examples of water include distilled water, ion-exchanged water, pure water, and ultrapure water. The content of water in the polishing composition of the present disclosure can be the remainder excluding Component A, Component B, and the optional components described below.

[0027] [Oxidizing Agent (Component C)] The polishing composition of the present disclosure may further contain an oxidizing agent (hereinafter also referred to as "Component C") from the viewpoints of improving the removal rate and reducing scratches. In one or more embodiments, Component C is an oxidizing agent that does not contain a halogen atom. Component C may be one type or a combination of two or more types.

[0028] Examples of component C, from the viewpoints of improving the polishing rate and reducing scratches, include peroxides, permanganic acid or its salts, chromic acid or its salts, peroxoacids or their salts, oxyacids or their salts, metal salts, nitric acids, sulfuric acids, etc. Among these, at least one selected from hydrogen peroxide, iron(III) nitrate, peracetic acid, ammonium peroxodisulfate, iron(III) sulfate, and ammonium iron(III) sulfate is preferred, and hydrogen peroxide is more preferred from the viewpoints of improving the polishing rate, preventing metal ions from adhering to the surface of the substrate to be polished, and ease of availability.

[0029] When the polishing liquid composition of the present disclosure contains component C, the content of component C in the polishing liquid composition of the present disclosure is preferably 0.01 mass% or more, more preferably 0.05 mass% or more, and even more preferably 0.1 mass% or more from the viewpoint of improving the polishing rate, and is preferably 4 mass% or less, more preferably 3 mass% or less, and even more preferably 2 mass% or less from the viewpoint of reducing scratches. More specifically, the content of component C in the polishing liquid composition of the present disclosure is preferably 0.01 mass% or more and 4 mass% or less, more preferably 0.05 mass% or more and 3 mass% or less, and even more preferably 0.1 mass% or more and 2 mass% or less. When component C is a combination of two or more types, the content of component C refers to the total content thereof.

[0030] [Other Components] In one or more embodiments, the polishing liquid composition of the present disclosure may contain other components as needed, to the extent that the effects of the present disclosure are not impaired. Examples of other components include heterocyclic aromatic compounds, aliphatic amine compounds, alicyclic amine compounds, thickeners, dispersants, rust inhibitors, basic substances, polishing rate enhancers, surfactants, water-soluble polymers, etc.

[0031] [pH of Polishing Liquid Composition] From the viewpoint of scratch prevention, the pH of the polishing liquid composition of the present disclosure is preferably 0.1 or more, more preferably 0.3 or more, and even more preferably 0.5 or more, and from the viewpoint of the polishing rate, it is preferably 6 or less, more preferably 5 or less, and even more preferably 4 or less. More specifically, the pH of the polishing liquid composition of the present disclosure is preferably 0.1 or more and 6 or less, more preferably 0.3 or more and 5 or less, and even more preferably 0.5 or more and 4 or less. The pH can be adjusted using the above-mentioned acid (component B) or a known pH adjuster. In the present disclosure, the pH is the pH of the polishing liquid composition at 25°C, and can be measured using a pH meter. For example, the value can be determined 2 minutes after immersing the electrode of the pH meter in the polishing liquid composition.

[0032] [Method for Producing Polishing Liquid Composition] The polishing liquid composition of the present disclosure can be produced, for example, by blending component A, component B, and water, and, if desired, optional components (component C and other components) using a known method. For example, in one or more embodiments, the polishing liquid composition of the present disclosure can be produced by blending at least component A, component B, and water. Therefore, in one aspect, the present disclosure relates to a method for producing a polishing liquid composition, including a step of blending at least component A, component B, and water. In this disclosure, "blending" includes mixing component A, component B, and water, and, if necessary, optional components (component C and other components), simultaneously or in any order. Silica particles (component A) may be mixed in the form of a concentrated slurry, or may be diluted with water or the like before mixing. When component A consists of multiple types of silica particles, the multiple types of silica particles can be blended simultaneously or separately. When component B consists of multiple types of acids, the multiple types of acids can be blended simultaneously or separately. The blending can be performed using a mixer such as a homomixer, homogenizer, ultrasonic disperser, or wet ball mill. The preferred amount of each component in the method for producing the polishing composition can be the same as the preferred content of each component in the polishing composition of the present disclosure described above.

[0033] An embodiment of the polishing liquid composition of the present disclosure may be a so-called one-component type in which all components are premixed and supplied to the market, or may be a so-called two-component type in which components are mixed at the time of use.

[0034] In the present disclosure, the "content of each component in the polishing liquid composition" refers to the content of each component at the time of use, i.e., at the time when the polishing liquid composition is first used for polishing. In one or more embodiments, the content of each component in the polishing liquid composition of the present disclosure can be considered as the blending amount of each component.

[0035] [Concentrate of Polishing Liquid Composition] The polishing liquid composition of the present disclosure may be stored and supplied in a concentrated state to the extent that its storage stability is not impaired. This is preferable in that it can further reduce production and transportation costs. The concentrate of the polishing liquid composition of the present disclosure may be diluted appropriately with the above-mentioned water as needed before use. The dilution ratio is not particularly limited as long as the contents (at the time of use) of each of the above-mentioned components can be ensured after dilution, and can be, for example, 10 to 100 times.

[0036] [Polishing Liquid Kit] In one aspect, the present disclosure relates to a kit for preparing the polishing liquid composition of the present disclosure, the kit including a first liquid containing component A and a second liquid containing component B in a mutually unmixed state (hereinafter also referred to as the "polishing liquid kit of the present disclosure"). The first liquid and the second liquid are mixed at the time of use and may be diluted with water as needed. The water contained in the first liquid may be the entire amount of water used to prepare the polishing liquid composition, or a portion thereof. The second liquid may contain a portion of the water used to prepare the polishing liquid composition. The first liquid and the second liquid may each contain the above-mentioned optional components (component C, other components) as needed. The above-mentioned optional components (component C, other components) may be further mixed when the first liquid and the second liquid are mixed. According to the present disclosure, a polishing liquid composition having excellent dispersion stability can be obtained, which can achieve both an improved polishing rate and reduced scratches on the substrate surface after polishing.

[0037] [Substrate to be polished] In one or more embodiments, the substrate to be polished is a substrate used in the manufacture of a magnetic disk substrate. In one or more embodiments, the magnetic disk substrate can be manufactured by polishing the surface of the substrate to be polished with the polishing composition of the present disclosure, followed by forming a magnetic layer on the substrate surface by sputtering or the like.

[0038] Suitable materials for the substrate to be polished in the present disclosure include, for example, metals or semimetals such as silicon, aluminum, nickel, tungsten, copper, tantalum, and titanium, or alloys thereof; glassy materials such as glass, glassy carbon, and amorphous carbon; ceramic materials such as alumina, silicon dioxide, silicon nitride, tantalum nitride, and titanium carbide; and resins such as polyimide resins. Among these, substrates containing metals such as aluminum, nickel, tungsten, and copper, and alloys primarily composed of these metals, are particularly suitable. Examples of suitable substrates include Ni-P-plated aluminum alloy substrates and glass substrates such as crystallized glass, tempered glass, aluminosilicate glass, and aluminoborosilicate glass, with Ni-P-plated aluminum alloy substrates being even more suitable. In the present disclosure, the term "Ni-P-plated aluminum alloy substrate" refers to an aluminum alloy substrate whose surface has been ground and then electrolessly plated with Ni-P.

[0039] The shape of the substrate to be polished may be, for example, a shape having a flat surface such as a disk, plate, slab, or prism, or a shape having a curved surface such as a lens. Of these, a disk-shaped substrate to be polished is suitable. In the case of a disk-shaped substrate to be polished, its outer diameter is, for example, about 2 to 100 mm, and its thickness is, for example, about 0.4 to 2 mm.

[0040] Generally, magnetic disks are manufactured by polishing a substrate that has undergone a grinding step through a rough polishing step and a finish polishing step, and then forming the substrate into a magnetic disk in a recording portion forming step. The polishing composition of the present disclosure is a polishing composition for magnetic disk substrates, and is preferably used for polishing in the finish polishing step. The polishing composition of the present disclosure may also be used for polishing in the rough polishing step.

[0041] [Method for polishing a substrate] In one aspect, the present disclosure relates to a method for polishing a substrate (hereinafter also referred to as the "polishing method of the present disclosure"), which includes a step of polishing a substrate to be polished using the polishing composition of the present disclosure (hereinafter also referred to as the "polishing step"), and the substrate to be polished is a substrate used in the production of magnetic disk substrates. According to the polishing method of the present disclosure, it is possible to achieve both an improvement in the polishing rate and a reduction in scratches on the substrate surface after polishing, and by using the polishing composition of the present disclosure, which has excellent dispersion stability, high-quality magnetic disk substrates can be produced with high yield and good productivity. As described above, the substrate to be polished in the polishing method of the present disclosure can be one used in the production of magnetic disk substrates, and among them, substrates used in the production of magnetic disk substrates for perpendicular magnetic recording systems are preferred.

[0042] In one or more embodiments, the polishing step in the polishing method of the present disclosure is a step of supplying the polishing liquid composition of the present disclosure to the surface to be polished of a substrate to be polished, bringing a polishing pad into contact with the surface to be polished, and moving at least one of the polishing pad and the substrate to be polished to perform polishing; alternatively, it is a step of sandwiching the substrate to be polished between plates to which a polishing pad such as a nonwoven organic polymer-based polishing cloth is attached, and polishing the substrate to be polished by moving the platen and the substrate to be polished while supplying the polishing liquid composition of the present disclosure to a polishing machine.

[0043] The polishing pad used in the polishing step is not particularly limited, and for example, a suede type, a nonwoven fabric type, a polyurethane closed-cell type, or a two-layer type in which these are laminated can be used, and from the viewpoint of improving the polishing rate, a suede type polishing pad is preferred.

[0044] The polishing load in the polishing step is preferably 5.9 kPa or more, more preferably 6.9 kPa or more, and even more preferably 7.5 kPa or more from the viewpoint of improving the polishing rate, and is preferably 20 kPa or less, more preferably 18 kPa or less, and even more preferably 16 kPa or less from the viewpoint of reducing scratches. In the manufacturing method of the present disclosure, the polishing load refers to the pressure of the platen applied to the polishing surface of the substrate to be polished during polishing. The polishing load can be adjusted by applying air pressure or a weight to at least one of the platen and the substrate to be polished.

[0045] In the polishing step, the polishing composition of the present disclosure is supplied at a rate of 1 cm per 1 cm of the substrate to be polished from the viewpoint of reducing scratches. 2 The flow rate is preferably 0.05 mL / min or more and 15 mL / min or less, more preferably 0.06 mL / min or more and 10 mL / min or less, even more preferably 0.07 mL / min or more and 1 mL / min or less, and even more preferably 0.07 mL / min or more and 0.5 mL / min or less.

[0046] The polishing composition of the present disclosure can be supplied to a polishing machine by, for example, continuous supply using a pump or the like. When supplying the polishing composition to a polishing machine, in addition to a method of supplying it as a single liquid containing all components, it can also be divided into a plurality of blending component liquids and supplied as two or more liquids, taking into consideration the stability of the polishing composition, etc. In the latter case, the plurality of blending component liquids are mixed, for example, in the supply pipe or on the substrate to be polished, to produce the polishing composition of the present disclosure.

[0047] [Method for manufacturing magnetic disk substrate] In one aspect, the present disclosure relates to a method for manufacturing a magnetic disk substrate (hereinafter also referred to as the "substrate manufacturing method of the present disclosure"), which includes a step of polishing a substrate to be polished using the polishing composition of the present disclosure (hereinafter also referred to as the "polishing step"). In one or more embodiments, the polishing step in the substrate manufacturing method of the present disclosure is a rough polishing step and / or a finish polishing step. The substrate manufacturing method of the present disclosure is particularly suitable for manufacturing magnetic disk substrates for perpendicular magnetic recording systems. The polishing method and conditions in the polishing step in the substrate manufacturing method of the present disclosure may be the same as the method and conditions in the polishing step in the polishing method of the present disclosure described above.

[0048] In one or more embodiments, the substrate manufacturing method of the present disclosure may further include a step of selecting component A contained in the polishing liquid composition of the present disclosure, a slurry of component A, or a polishing liquid composition containing component A as abrasive grains, to obtain the polishing liquid composition of the present disclosure. Thus, in one or more embodiments, the substrate manufacturing method of the present disclosure is a method for manufacturing a magnetic disk substrate, comprising a step of selecting component A, a slurry of component A, or a polishing liquid composition containing component A as abrasive grains to obtain a polishing liquid composition containing component A, component B, and water (the polishing liquid composition of the present disclosure), and a step of polishing a substrate to be polished using the polishing liquid composition of the present disclosure. The step of obtaining the polishing liquid composition of the present disclosure includes preparing the polishing liquid composition of the present disclosure using component A, a slurry of component A, or a polishing liquid composition containing component A as abrasive grains.

[0049] In one or more embodiments, the polishing step in the substrate manufacturing method of the present disclosure is a step of supplying the polishing liquid composition of the present disclosure to a surface to be polished of a substrate to be polished, bringing a polishing pad into contact with the surface to be polished, and moving at least one of the polishing pad and the substrate to be polished. In another one or more embodiments, the polishing step in the substrate manufacturing method of the present disclosure is a step of sandwiching the substrate to be polished between plates to which a polishing pad such as a nonwoven organic polymer-based polishing cloth is attached, and polishing the substrate to be polished by moving the platen and the substrate to be polished while supplying the polishing liquid composition of the present disclosure to a polishing machine.

[0050] When the polishing process of the substrate to be polished is performed in multiple stages, the polishing process is preferably performed in the second stage or later, and more preferably in the final polishing process or finish polishing process. In this case, separate polishing machines may be used for each stage to avoid contamination with abrasive grains or polishing compositions from the previous process, and when separate polishing machines are used, it is preferable to clean the substrate to be polished after each polishing process. Furthermore, the polishing composition of the present disclosure can also be used in circulating polishing in which the used polishing liquid is reused. The polishing machine is not particularly limited, and known polishing machines for substrate polishing can be used.

[0051] According to the substrate manufacturing method of the present disclosure, it is possible to achieve both an improved removal rate and a reduced number of scratches on the substrate surface after polishing, and by using the polishing liquid composition of the present disclosure, which has excellent dispersion stability, it is possible to manufacture high-quality magnetic disk substrates with high yield and good productivity.

[0052] [Silica Particles] In one aspect, the present disclosure relates to silica particles having a silicon atom concentration (atom%) of 28 atom% or more and 38 atom% or less, as measured by X-ray photoelectron spectroscopy (XPS) at a detection angle of 15° (hereinafter, silica particles having this silicon atom concentration are also referred to as "silica particles of the present disclosure"). The silica particles of the present disclosure can be suitably used as abrasive grains for polishing magnetic disk substrates. In one or more embodiments, the silica particles of the present disclosure are the above-mentioned component A. The silicon atom concentration of the silica particles of the present disclosure, as measured by X-ray photoelectron spectroscopy (XPS) at a detection angle of 15°, is preferably 28 atom% or more, more preferably 29 atom% or more, and even more preferably 30 atom% or more, from the viewpoint of improving the polishing rate when the silica particles of the present disclosure are used as abrasive grains for polishing magnetic disk substrates, and is preferably 38 atom% or less, more preferably 36 atom% or less, and even more preferably 34 atom% or less, from the viewpoint of reducing scratches. More specifically, the silicon atom concentration of the silica particles of the present disclosure measured by X-ray photoelectron spectroscopy (XPS) under the condition of a detection angle of 15 ° is preferably 28 atom% or more and 38 atom% or less, more preferably 29 atom% or more and 36 atom% or less, and even more preferably 30 atom% or more and 34 atom% or less.The silicon atom concentration of the silica particles of the present disclosure measured by X-ray photoelectron spectroscopy (XPS) under the condition of a detection angle of 75 ° is preferably 28 atom% or more, more preferably 28.2 atom% or more, and even more preferably 28.4 atom% or more, from the viewpoint of improving the polishing rate when the silica particles of the present disclosure are used as abrasive grains for polishing magnetic disk substrates, and from the viewpoint of reducing scratches, is preferably 36 atom% or less, more preferably 35.5 atom% or less, and even more preferably 35.0 atom% or less. More specifically, the silicon atom concentration of the silica particles of the present disclosure, as measured by X-ray photoelectron spectroscopy (XPS) at a detection angle of 75°, is preferably 28 atom% or more and 36 atom% or less, more preferably 28.2 atom% or more and 35.5 atom% or less, and even more preferably 28.4 atom% or more and 35.0 atom% or less.

[0053] Hereinafter, the present disclosure will be described in more detail with reference to examples, but these are merely illustrative examples and the present disclosure is not limited to these examples.

[0054] 1. Silica Particles A1 to A12 (Component A or Non-Component A) The following were used for the silica particles A1 to A12 shown in Table 1. (Component A) A1: Colloidal silica, BET specific surface area 136.4 m 2 / g The alkali silicate, the raw material for silica microparticles, is dissolved in water to a concentration of 2 to 8 mass %. A strong acid such as hydrochloric acid, sulfuric acid, or nitric acid is added to the aqueous solution to neutralize the silicic acid, resulting in a silica hydrogel. The pH at this stage is preferably approximately 4 to 6. The alkali silicate hydrogel neutralized with the strong acid is allowed to stand at a temperature range of 10 to 40°C for 1 to 5 hours to mature the silica. The solution is then washed with pure water or alkaline water to remove the salt. An alkaline solution such as sodium hydroxide, potassium hydroxide, or ammonium hydroxide is added to the washed dispersion, and the pH of the resulting dispersion is adjusted to a range of 6 to 12. The temperature at this stage is preferably 40 to 120°C. The dispersion thus prepared is stirred for approximately 30 minutes to 3 hours to form a colloidal silica hydrogel. The resulting silica sol is then subjected to hydrothermal treatment at a temperature of 100 to 300°C and a pressure of 0.1 to 0.3 MPa for approximately 30 minutes to 6 hours to grow and stabilize the silica particles, and the silicon atom concentration at a detection angle of 15° is adjusted to 28 atom% or more and 38 atom% or less to obtain silica particles A1. A2: Colloidal silica, BET specific surface area 136.4 m 2 Silica particles A2 are obtained by adjusting the hydrothermal treatment conditions, such as temperature (100°C to 300°C), pressure (0.1 to 0.3 MPa), and time (30 minutes to 6 hours), so that the silicon atom concentration at a detection angle of 15° is 28 atom% or more and 38 atom% or less. A3: Colloidal silica, BET specific surface area 124.0 m 2Silica particles A3 are obtained by adjusting the hydrothermal treatment conditions, such as temperature (100°C to 300°C), pressure (0.1 to 0.3 MPa), and time (1 to 6 hours), so that the silicon atom concentration at a detection angle of 15° is 28 atom% or more and 38 atom% or less. A4: Colloidal silica, BET specific surface area 97.4 m 2 Silica particles A4 are obtained by adjusting the hydrothermal treatment conditions, such as temperature (100°C to 300°C), pressure (0.1 to 0.3 MPa), and time (2 to 6 hours), so that the silicon atom concentration at a detection angle of 15° is 28 atom% or more and 38 atom% or less. A5: Colloidal silica, BET specific surface area 124.0 m 2 Silica particles A5 are obtained by preparing the same preparation procedure as silica particles A1, controlling the hydrothermal treatment conditions of temperature (100°C to 300°C), pressure (0.1 to 0.3 MPa), and time (30 minutes to 6 hours), mixing the two prepared silica particles in a specific ratio, and adjusting the silicon atom concentration at a detection angle of 15° to 28 atom% or more and 38 atom% or less. A6: Colloidal silica, BET specific surface area 143.5 m 2 Silica particles A6 are obtained by preparing the same preparation procedure as silica particles A1, controlling the hydrothermal treatment conditions of temperature (100°C to 300°C), pressure (0.1 to 0.3 MPa), and time (30 minutes to 6 hours), mixing the two prepared silica particles in a specific ratio, and adjusting the silicon atom concentration at a detection angle of 15° to 28 atom% or more and 38 atom% or less. A7: Colloidal silica, BET specific surface area 30.0 m 2 Silica particles A7 are obtained by adjusting the hydrothermal treatment conditions, such as temperature (100°C to 300°C), pressure (0.1 to 0.3 MPa), and time (3 to 6 hours), so that the silicon atom concentration at a detection angle of 15° is 28 atom% or more and 38 atom% or less. A8: Colloidal silica, BET specific surface area 31.0 m 2Silica particles A8 are obtained by adjusting the hydrothermal treatment conditions, such as temperature (100°C to 300°C), pressure (0.1 to 0.3 MPa), and time (3 to 6 hours), so that the silicon atom concentration at a detection angle of 15° is 28 atom% or more and 38 atom% or less. (Non-Component A) A9: Ultra-high purity colloidal silica, BET specific surface area 113.6 m 2 / g A10: Ground silica, BET specific surface area 27.8 m 2 / g A11: Colloidal silica, BET specific surface area 136.4 m 2 Silica particles A11 are obtained by preparing the silica particles A12 using the same preparation procedure as silica particles A1, controlling the hydrothermal treatment conditions of temperature (100°C to 300°C), pressure (0.1 to 0.3 MPa), and time (30 minutes to 6 hours) so that the silicon atom concentration at a detection angle of 15° is 28 atom% or more and 38 atom% or less, and then storing the particles in an aqueous solution having a pH of 11 to 13 for 12 hours. 2 / g

[0055] 2. Preparation of Polishing Compositions (Examples 1 to 8 and Comparative Examples 1 to 5) Polishing compositions (pH 1.6) of Examples 1 to 8 and Comparative Examples 1 to 5 shown in Tables 1 and 2 were prepared by blending and stirring silica particles A1 to A12 (component A or non-component A), acid (component B), oxidizing agent (component C) shown in Table 1. The content (mass %, effective amount) of each component in each polishing composition was 6 mass % for silica particles (component A or non-component A), 1.6 mass % for acid (component B), and 1.0 mass % for oxidizing agent (component C). The content of ion-exchanged water in each polishing composition is the remainder excluding component A or non-component A, component B, and component C.

[0056] The following components B and C were used to prepare each polishing composition: (Component B) Phosphoric acid [75% phosphoric acid manufactured by Nippon Chemical Industry Co., Ltd.] (Component C) Hydrogen peroxide solution [concentration 35% by mass, manufactured by ADEKA Corporation]

[0057] 3. Measurement of Each Parameter [Measurement of Silicon Atom Concentration (atom %) by XPS] The concentrations of each atom (Si, O) measured by XPS are measured using an XPS measurement device manufactured by ULVAC-PHI, Inc., which uses ALKα rays as characteristic X-rays. The silicon atom (Si) concentration is calculated by performing elemental analysis of a spectrum obtained by XPS at predetermined detection angles (15°, 45°, 75°) in a binding energy range of 96 to 106 eV. The oxygen atom (O) concentration is calculated by performing elemental analysis of a spectrum obtained by XPS at predetermined detection angles (15°, 45°, 75°) in a binding energy range of 526 to 536 eV.

[0058] [Measurement of Average Primary Particle Diameter of Silica Particles] The average primary particle diameter (nm) of silica particles (component A) is determined by the specific surface area S (m 2 / g), the average primary particle diameter (nm) was calculated using the following formula: Average primary particle diameter (nm) = 2727 / S The specific surface area S of component A was measured by carrying out the following [pretreatment], then accurately weighing approximately 0.1 g of the measurement sample into a measurement cell to four decimal places, drying it in an atmosphere at 110°C for 30 minutes immediately before measuring the specific surface area, and then measuring it by the nitrogen adsorption method (BET method) using a specific surface area measurement device (Micromeritic automatic specific surface area measurement device "Flowsorb III2305", manufactured by Shimadzu Corporation). <Pretreatment> (a) The pH of the slurry of component A was adjusted to 2.5±0.1 with an aqueous nitric acid solution. (b) The slurry of component A adjusted to pH 2.5±0.1 was placed in a petri dish and dried in a hot air dryer at 150°C for 1 hour. (c) After drying, the obtained sample was finely crushed in an agate mortar. (d) The pulverized sample is suspended in ion-exchanged water at 40°C and filtered through a membrane filter with a pore size of 1 μm. (e) The residue on the filter is washed five times with 20 g of ion-exchanged water (40°C). (f) The filter with the residue attached is placed in a petri dish and dried in an atmosphere at 110°C for four hours. (g) The dried residue (component A) is taken, being careful not to mix with filter debris, and finely pulverized in a mortar to obtain a measurement sample.

[0059] [Measurement of pH] The pH of the polishing composition was measured at 25° C. using a pH meter (manufactured by DKK-Toa Corporation), and the value measured 2 minutes after immersing the electrode in the polishing composition was adopted.

[0060] 4. Polishing Method The polishing compositions prepared in Examples 1 to 8 and Comparative Examples 1 to 5 were used to polish the following substrates under the polishing conditions shown below (Examples 1 to 6 and Comparative Examples 1 and 2: finish polishing, Examples 7 and 8 and Comparative Examples 3 to 5: rough polishing). Then, the polishing rate, number of scratches, and dispersion stability were measured by the measurement methods described below, and the results are shown in Tables 1 and 2.

[0061] [Polished Substrate] (Examples 1 to 6, Comparative Examples 1 and 2) The substrate to be polished was a Ni-P plated aluminum alloy substrate that had been roughly polished in advance with a polishing composition containing alumina abrasive grains. This substrate to be polished had a thickness of 0.6 mm, an outer diameter of 97 mm, and an inner diameter of 25 mm, and the center line average roughness Ra measured with an AFM (Digital Instrument NanoScope IIIa Multi Mode AFM) was 1 nm. (Examples 7 to 8, Comparative Examples 3 to 5) The substrate to be polished was a Ni-P plated aluminum alloy substrate with a thickness of 0.8 mm, a diameter of 95 mm, and an inner diameter of 25 mm.

[0062] [Finish polishing conditions (Examples 1 to 6, Comparative Examples 1 and 2)] Polishing tester: "Double-sided 9B polisher" manufactured by SpeedFam Co., Ltd. Polishing pad: Suede type manufactured by Fujibo Co., Ltd. (foam layer: polyurethane elastomer, thickness 0.9 mm, average pore size 10 μm) Supply rate of polishing composition: 100 mL / min (1 cm of substrate to be polished) 2 Supply rate per cm of substrate to be polished: 0.076 mL / min) Lower surface plate rotation speed: 32.5 rpm Polishing load: 10.5 kPa Polishing time: 5 minutes Number of substrates: 10 [Rough polishing conditions (Examples 7 to 8, Comparative Examples 3 to 5)] Polishing tester: "Double-sided 9B polisher" manufactured by SpeedFam Co., Ltd. Polishing pad: Suede type manufactured by Fujibo Co., Ltd. (foam layer: polyurethane elastomer, thickness 1.0 mm, average pore size 30 μm) Supply rate of polishing liquid composition: 100 mL / min (per cm of substrate to be polished) 2Supply rate per unit: 0.8 mL / min) Lower platen rotation speed: 40 rpm Polishing load: 9.8 kPa Polishing time: 5 minutes Number of substrates: 10

[0063] 5. Evaluation [Evaluation of Polishing Rate] The mass of each substrate was measured before and after polishing using a polishing machine (manufactured by Sartorius, "BP-210S"), and the mass loss was calculated from the change in mass of each substrate. The polishing rate was calculated by dividing the average mass loss of all 10 substrates by the polishing time using the following formula. The measurement results of the polishing rates (finish polishing) for Examples 1 to 6 and Comparative Examples 1 and 2 are shown in Table 1 as relative values, with Comparative Example 1 set to 100. The measurement results of the polishing rates (coarse polishing) for Examples 7 to 8 and Comparative Examples 3 to 5 are shown in Table 2 as relative values, with Comparative Example 3 set to 100. Mass loss (mg) = {mass before polishing (mg) - mass after polishing (mg)} Polishing rate (mg / min) = mass loss (mg) / polishing time (min)

[0064] [Scratch Evaluation] Measuring equipment: "Candela OSA6110" manufactured by KLA-Tencor Corporation Evaluation: Four substrates were randomly selected from the substrates placed in the polishing tester, and each substrate was irradiated with a laser at 10,000 rpm to measure the number of scratches. The total number of scratches on both sides of each of the four substrates was divided by 8 to calculate the number of scratches per substrate surface. The evaluation results of the number of scratches in Examples 1 to 6 and Comparative Examples 1 and 2 are shown in Table 1 as relative values, with Comparative Example 1 set to 100.

[0065] [Evaluation of Dispersion Stability] To evaluate dispersion stability, a silica aqueous solution or silica powder was added to water to adjust the target silica particle concentration to 10%. The adjusted 10% silica aqueous solution was placed in a test tube and allowed to stand for 30 minutes. After that, if silica sedimentation could be visually confirmed in the test tube, the dispersion stability was marked as B, and if silica sedimentation could not be confirmed and a uniform slurry state was maintained, the dispersion stability was marked as A. The results are shown in Tables 1 and 2.

[0066]

[0067] As shown in Table 1 above, the polishing compositions of Examples 1 to 6 improved the removal rate and reduced scratches on the substrate surface after polishing, compared to Comparative Examples 1 and 2, in which the silicon atom concentration (atom %) at a detection angle of 15° was not 28 to 38 atom %. Furthermore, the polishing compositions of Examples 1 to 6 had excellent dispersion stability.

[0068]

[0069] As shown in Table 2 above, the polishing compositions of Examples 7 and 8 had improved removal rates compared to Comparative Examples 3 to 5, in which the silicon atom concentration (atom %) at a detection angle of 15° was less than 28 atom %. Furthermore, the polishing compositions of Examples 7 and 8 had excellent dispersion stability.

[0070] According to the present disclosure, for example, a magnetic disk substrate suitable for high recording density can be provided.

Claims

1. A polishing composition for magnetic disk substrates, comprising silica particles (component A), an acid (component B), and water, wherein component A has a silicon atom concentration (atom %) of 28 atom % or more and 38 atom % or less, as measured by X-ray photoelectron spectroscopy (XPS) at a detection angle of 15°.

2. The polishing composition according to claim 1, wherein component A has a silicon atom concentration (atom %) of 28 atom % or more and 36 atom % or less as measured by XPS at a detection angle of 75°.

3. A polishing composition according to claim 1 or 2, wherein component A has a concentration ratio (15° / 75°) of the silicon atom concentration (atom %) measured by XPS at a detection angle of 15° to the silicon atom concentration (atom %) measured by XPS at a detection angle of 75° of 1.05 or more.

4. The polishing composition according to any one of claims 1 to 3, having a pH of 0.1 or more and 6 or less.

5. The polishing composition according to any one of claims 1 to 4, wherein the average primary particle size of component A is 5 nm or more and 100 nm or less.

6. A polishing composition according to any one of claims 1 to 5, wherein component A is colloidal silica.

7. A method for polishing a substrate, comprising a step of polishing a substrate to be polished with the polishing composition according to any one of claims 1 to 6, wherein the substrate to be polished is a substrate used in the manufacture of magnetic disk substrates.

8. A method for manufacturing a magnetic disk substrate, comprising the steps of: selecting silica particles (component A) having a silicon atom concentration (atom %) of 28 atom % or more and 38 atom % or less as measured by X-ray photoelectron spectroscopy (XPS) at a detection angle of 15°; a slurry of the silica particles (component A); or a polishing liquid composition containing the silica particles (component A) as abrasive grains; and obtaining a polishing liquid composition containing the silica particles (component A), an acid (component B), and water; and polishing a substrate to be polished using the polishing liquid composition containing the silica particles (component A), an acid (component B), and water.