Integrated hollow-core optical fiber preform, optical fiber and fabrication method thereof
Patent Information
- Application Number
- MYPI2025002815
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-11-10
- Filing Date
- 2023-10-13
- Publication Date
- 2024-05-10
AI Technical Summary
The transmission loss of existing hollow-core microstructured optical fibers is high, and the complexity and small deviations of the anti-resonant structure make accurate and repeatable production more difficult. In particular, there are challenges in preparing anti-resonant layers with thinner wall thickness.
An integrated hollow-core optical fiber preform is used, and the initial preform is prepared by drilling. During the drawing process, air pressure is used to control the formation of an anti-resonant ring with negative curvature to ensure the precise positioning and uniformity of the anti-resonant unit, reduce impurity contamination, and reduce The wall thickness of the anti-resonance unit is used to reduce the attenuation of the fiber.
Achieving lower transmission loss, reducing the attenuation rate to a minimum of 30dB/km or lower, improving the attenuation and strength performance of the optical fiber, ensuring the precise positioning and uniformity of the anti-resonance unit, and reducing the attenuation of the optical fiber.
Smart Images

Figure PI2025002815_DRAWING_001 
Figure PI2025002815_DRAWING_002 
Figure PI2025002815_DRAWING_003
Abstract
Description
An integrated hollow-core optical fiber preform, optical fiber, and preparation method thereof Technical Field
[0001] The present invention belongs to the field of optical fiber communication technology, and more specifically, relates to an integrated hollow-core optical fiber preform and an optical fiber preparation method, which can be used to prepare hollow-core microstructure optical fibers. Background Art
[0002] Hollow-core microstructured optical fiber has the characteristics of simple structure, hollow-core single-mode light guidance, and wide transmission spectrum. It has important applications in the fields of interaction between light and filling materials, nonlinear optics, gas detection, gas laser generation, optofluidic technology, etc.; large air hole core light guidance has ultra-low Rayleigh scattering, low nonlinear coefficient, and adjustable dispersion characteristics, which can provide a higher laser damage threshold, making it potentially applicable in high-power laser transmission, ultraviolet / mid-infrared light transmission, pulse compression and optical soliton transmission. The ultra-low loss, low dispersion, low nonlinearity, and propagation speed close to the speed of light of the air core can realize the development of hollow-core optical fiber communication transmission and communication devices, laying the foundation for the construction and development of the next generation of ultra-large capacity, low latency, and high-speed optical communication systems.
[0003] Despite the significant advantages of hollow-core fiber in design and application, its transmission loss has consistently been higher than that of traditional quartz fiber. Recent discoveries have shown that hollow-core fiber, based on the principle of antiresonance, can effectively reduce transmission loss with appropriate structural design, demonstrating its potential as an ultra-long-haul communication fiber. Further reducing attenuation is a key issue in the fabrication of hollow-core microstructured fibers.
[0004] Although known antiresonant hollow-core fibers, especially those with nested structural elements, can significantly reduce fiber attenuation, their complex internal geometry and the fact that even slight geometric deviations can cause variations in antiresonance conditions make their precise and repeatable production difficult. At the same time, thinner-walled antiresonant layers help achieve lower loss and wider bandwidth, so the production of thinner-walled antiresonant layers is also an urgent issue to be addressed.
[0005] Summary of the Invention
[0006] In response to the above-mentioned defects or improvement needs of the prior art, the present invention provides a hollow-core microstructured optical fiber preform, an optical fiber and a preparation method thereof, the purpose of which is to provide a method for manufacturing antiresonant hollow-core optical fibers with higher precision positioning, which avoids the limitations of traditional manufacturing methods.
[0007] To achieve the above object, the present invention adopts the following technical solutions:
[0008] A one-piece hollow-core optical fiber preform comprises a sleeve, wherein a plurality of circumferentially distributed axial holes are opened in the sleeve wall, the minimum distance t1 between the inner wall of the axial hole and the inner wall of the sleeve is located on the side close to the center of the sleeve, and the ratio of t1 to the diameter of the axial hole is ≤0.35.
[0009] Furthermore, the axial holes are evenly distributed along the same ring line, and the number thereof is ≥4.
[0010] Furthermore, the ratio of the inner diameter to the outer diameter of the sleeve is 0.2 to 0.8.
[0011] Furthermore, a capillary is inserted into the axial hole to form an optical fiber preform rod with a nested structure.
[0012] Furthermore, a quartz plate is inserted into the axial hole to form an optical fiber preform with a connecting plate structure, and the quartz plate is arranged perpendicular to the radial line of the sleeve.
[0013] A method for preparing a hollow-core microstructured optical fiber comprises the following steps:
[0014] Step 1: Select a casing and start drilling from the end of the casing to prepare the above-mentioned integrated hollow-core optical fiber preform;
[0015] Step 2: The integrated hollow-core optical fiber preform obtained in step 1 is subjected to high-temperature drawing. During the drawing process, gas is introduced into the axial hole so that the air pressure in the axial hole is higher than the air pressure in the central hole of the sleeve. Due to the pressure difference between the axial hole and the central hole of the sleeve and the effect of surface tension, the axial hole protrudes toward the central hole of the sleeve after drawing, forming an anti-resonance ring with negative curvature. All anti-resonance rings together constitute an annular anti-resonance layer, and the area surrounded by the anti-resonance layer constitutes a hollow fiber core, thereby forming a hollow-core microstructure optical fiber with a negative curvature anti-resonance ring.
[0016] Furthermore, in step 1, after drilling, acid solution is introduced to corrode the axial hole so that the ratio of the minimum distance t1 between the inner wall of the axial hole and the inner wall of the casing to the diameter of the axial hole is ≤0.1.
[0017] Preferably, the acid solution is hydrofluoric acid.
[0018] Furthermore, in step 1, when a capillary is embedded in the axial hole, gas is also introduced into the capillary, and the gas pressure in the capillary, the axial hole and the central hole of the sleeve is controlled to decrease gradually in sequence.
[0019] Furthermore, in step 1, the gas introduced into the axial hole or the capillary is any one or more of compressed air, nitrogen, helium, and argon.
[0020] Furthermore, in step 2, the anti-resonance layer and the drawn sleeve form a cladding, the outer diameter of the cladding is 100 to 300 μm, and the diameter of the fiber core is 10 to 50 μm.
[0021] Furthermore, in step 2, the minimum wall thickness of the antiresonant ring is ≤2 μm, more preferably ≤1 μm.
[0022] The hollow-core microstructure optical fiber prepared by the method of the present invention has low transmission loss, with the lowest transmission loss being ≤30dB / km, and the best being ≤1dB / km.
[0023] Compared with the prior art, the present invention can achieve the following beneficial effects through the above technical solutions.
[0024] 1. The hollow-core microstructured optical fiber preform provided by the present invention differs from the traditional "rod stacking-drawing" method in that it uses a drilling method to obtain the initial preform. The antiresonant ring structure of the optical fiber is then achieved by controlling the pressure in the hole during the drawing process. One of the benefits of this method is that it can achieve precise positioning of the antiresonant unit through mechanical drilling, ensuring axial uniformity and avoiding azimuthal deviation of the antiresonant unit during the drawing process.
[0025] 2. The present invention does not introduce other materials to position the anti-resonance unit, thereby reducing impurity contamination and improving the attenuation and strength performance of the optical fiber;
[0026] 3. The present invention expands the anti-resonance unit by controlling the air pressure during the drawing process, thereby further reducing the wall thickness of the anti-resonance unit and reducing the attenuation of the optical fiber. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] FIG1 is a schematic structural diagram of an optical fiber preform having a hollow core microstructure provided by Example 1 of the present invention;
[0028] FIG2 is a schematic diagram of the structure of a hollow-core microstructured optical fiber provided in Example 1 of the present invention;
[0029] FIG3 is a schematic structural diagram of an optical fiber preform having a hollow core microstructure provided by Example 2 of the present invention;
[0030] FIG4 is a schematic diagram of the structure of a hollow-core microstructured optical fiber provided in Example 2 of the present invention;
[0031] FIG5 is a schematic structural diagram of an optical fiber preform with a nested structure provided by Example 3 of the present invention;
[0032] FIG6 is a schematic diagram of the structure of a hollow-core microstructured optical fiber provided in Example 3 of the present invention;
[0033] 7 is a schematic structural diagram of an optical fiber preform with a connecting piece structure provided in Example 4 of the present invention;
[0034] Figure 8 is a schematic diagram of the hollow-core microstructured optical fiber structure provided in Example 4 of the present invention. 1 - optical fiber preform, 2 - sleeve, 3 - axial hole, 4 - hollow-core microstructured optical fiber, 5 - optical fiber cladding, 6 - antiresonant ring, 7 - optical fiber hollow core, 10 - capillary, 11 - first layer of antiresonant rings, 12 - second layer of antiresonant rings, 13 - quartz plate, 14 - antiresonant ring, 15 - antiresonant plate, 16 - axial hole, 17 - sleeve inner wall, 18 - large circular hole. DETAILED DESCRIPTION
[0035] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below with reference to the following embodiments. It should be understood that the specific embodiments described herein are merely for the purpose of explaining the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below may be combined with each other as long as they do not conflict with each other.
[0036] The present invention provides a method for preparing a hollow-core microstructure optical fiber, comprising the following steps:
[0037] Step 1: Select a casing and start drilling from the end of the casing to prepare an integrated hollow-core optical fiber preform;
[0038] An integrated hollow-core optical fiber preform comprises a sleeve having a plurality of circumferentially distributed axial holes formed in its wall. The minimum distance t1 between the inner wall of the axial hole and the inner wall of the sleeve is located on the side close to the center of the sleeve, and the ratio of t1 to the diameter of the axial hole is ≤0.35.
[0039] Step 2: The integrated hollow-core optical fiber preform obtained in step 1 is subjected to high-temperature drawing. During the drawing process, gas is introduced into the axial hole so that the air pressure in the axial hole is higher than the air pressure in the central hole of the sleeve. Due to the pressure difference between the axial hole and the central hole of the sleeve and the effect of surface tension, the axial hole protrudes toward the central hole of the sleeve after drawing, forming an anti-resonance ring with negative curvature. All anti-resonance rings together constitute an annular anti-resonance layer, and the area surrounded by the anti-resonance layer constitutes a hollow fiber core, thereby forming a hollow-core microstructure optical fiber with a negative curvature anti-resonance ring.
[0040] Example 1
[0041] Preparation of optical fiber preform:
[0042] As shown in Figure 1, a cannula 2 is first selected. The cannula is made of pure silica, has an inner diameter d0 of 30 mm, an outer diameter D0 of 50 mm, and a length of 1000 mm. Five axial holes 3 are drilled in the cannula using a drilling method. The axial holes are arranged at an equal azimuth angle (an azimuth angle of 72°), and the diameter d1 of the axial holes 3 is 6.5 mm. The ratio of the minimum distance t1 between the inner wall of the axial hole 3 and the inner wall 17 of the cannula to the diameter d1 of the axial hole is 0.08. This completes the preparation of an optical fiber preform 1 with a hollow-core microstructure.
[0043] Preparation of hollow core microstructured optical fiber:
[0044] An optical fiber preform 1 with a hollow-core microstructure is placed in a high-temperature drawing furnace at 1710°C for drawing. The hollow core in the center of the preform is maintained at atmospheric pressure, and an isobaric gas pressure of 2.9 kPa is introduced into the five axial holes. Due to the pressure difference between the inside and outside of the axial holes, the holes expand after drawing, forming antiresonant rings 6, ultimately resulting in the hollow-core microstructured optical fiber 4 shown in Figure 3. The outer diameter of the optical fiber cladding 5 is 124.7 μm, the diameter of the hollow core 7 is 27.4 μm, and the thinnest wall thickness of the antiresonant ring is 637 nm. The attenuation of this optical fiber at 1550 nm is 12.7 dB / km.
[0045] Example 2
[0046] Preparation of optical fiber preform:
[0047] As shown in Figure 3, a cannula is first selected. The cannula is made of pure silica, has an inner diameter of 40 mm, an outer diameter of 80 mm, and a length of 900 mm. Six axial holes 3 are drilled into the cannula using a drilling method. The axial holes 3 are arranged at equal azimuth angles (at an azimuth angle of 60°), have a diameter of 8.2 mm, and the ratio of the minimum distance 8 between the inner wall of the axial hole 3 and the inner wall 17 of the cannula to the diameter of the axial hole 3 is 0.21. The cannula is then etched in an acid solution. After etching, the ratio of the minimum distance 9 between the inner wall of the axial hole 16 and the inner wall 17 of the cannula to the diameter of the axial hole 16 is 0.06, thus completing the preparation of an optical fiber preform 1 having a hollow-core microstructure.
[0048] Preparation of hollow core microstructured optical fiber:
[0049] An optical fiber preform 1 with a hollow-core microstructure is placed in a high-temperature drawing furnace at 1760°C for drawing. Gas is introduced into the hollow core of the preform to maintain a pressure of approximately 0.56 kPa. Isobaric gas, at a pressure of 1.9 kPa, is introduced into the six axial holes 16. Due to the pressure difference between the inside and outside of the axial holes 16, the holes expand after drawing, forming antiresonant rings 6. Finally, the hollow-core microstructured optical fiber 4 shown in Figure 4 is formed. The outer diameter of the optical fiber cladding 5 is 243 μm, the diameter of the optical fiber hollow core 7 is 42.7 μm, and the thinnest wall thickness of the antiresonant rings 6 is 336 nm. The attenuation of this optical fiber at 1550 nm is 1.45 dB / km.
[0050] Example 3
[0051] Preparation of optical fiber preform:
[0052] As shown in Figure 5, a sleeve 2 is first selected. The sleeve material is pure silica, the inner diameter of the sleeve 2 is 13mm, the outer diameter is 28mm, and the length is 700mm. Using the drilling method, six axial holes 3 are drilled on the sleeve. The axial holes 3 are arranged at equal azimuth angles (the azimuth angle is 60°), the diameter of the axial holes is 2.4mm, and the ratio of the minimum distance between the inner wall of the axial hole and the inner wall 17 of the sleeve to the diameter of the axial hole is 0.13. The drilled sleeve is placed in an acid solution for etching. The ratio of the minimum distance between the inner wall of the axial hole 3 and the inner wall 17 of the sleeve after etching to the diameter of the axial hole is 0.06. Then, a capillary 10 with an outer diameter of 1.1mm and a wall thickness of 0.12mm is inserted into the axial hole, and the preparation of the nested optical fiber preform rod 1 is completed.
[0053] Preparation of hollow core microstructured optical fiber:
[0054] A nested optical fiber preform 1 was placed in a high-temperature drawing furnace at 1770°C for drawing. The hollow core of the preform was maintained at atmospheric pressure. Isobaric gas at 3.7 kPa was introduced into the six axial holes 3, and isobaric gas at 4.6 kPa was introduced into the six nested capillaries. Due to the pressure differences between the inside and outside of the axial holes and the nested capillaries, nested antiresonant rings were formed, ultimately resulting in the nested hollow-core microstructured optical fiber 4 shown in Figure 6. The outer diameter of the optical fiber cladding 5 was 153 μm, the diameter of the optical fiber hollow core was 33.2 μm, the thinnest wall thickness of the first antiresonant ring 11 was 217 nm, and the thinnest wall thickness of the second antiresonant ring 12 was 265 nm. The attenuation of this optical fiber at 1550 nm was 0.78 dB / km.
[0055] Example 4
[0056] Preparation of optical fiber preform:
[0057] As shown in Figure 7, a solid core rod made of pure silica with an outer diameter of 63 mm and a length of 1000 mm is first selected. Six small circular holes are drilled into the solid core rod to serve as axial holes 3. These holes are arranged at equal azimuth angles (60°) and have a diameter of 7.4 mm. A large circular hole 18 is then drilled in the center of the solid core rod to serve as the sleeve center hole. The ratio of the minimum distance between the inner wall of the axial hole 3 and the inner wall of the sleeve center hole (large circular hole 18) to the axial hole diameter is 0.16. The sleeve is then etched in an acid solution. The ratio of the minimum distance between the inner wall of the axial hole and the inner wall of the sleeve center hole to the axial hole diameter is 0.07. A quartz plate 13 with a wall thickness of 0.19 mm is then inserted into the axial hole, with the perpendicular bisector of the plate 13 passing through the center of the solid core rod. This completes the preparation of the optical fiber preform 1 with a connecting plate structure.
[0058] Preparation of hollow core microstructured optical fiber:
[0059] An optical fiber preform 1 with a connector structure is placed in a high-temperature drawing furnace for drawing at 1735°C. The hollow core of the preform is maintained at atmospheric pressure, and isobaric gas is introduced into the six axial holes at a pressure of 2.6 kPa. Due to the pressure difference between the inside and outside of the axial holes, the holes expand after drawing, forming antiresonant rings 14. The quartz plates 13 inserted into the axial holes 3 form antiresonant plates 15. Together, these antiresonant plates 15 form a second antiresonant layer, ultimately forming the hollow-core microstructured optical fiber 4 shown in Figure 8. The outer diameter of the optical fiber cladding 5 is 201 μm, the diameter of the optical fiber hollow core 7 is 53.2 μm, the thinnest wall thickness of the antiresonant ring 14 is 616 nm, and the thinnest wall thickness of the antiresonant plates 15 is 543 nm. The attenuation of this optical fiber at 1550 nm is 1.54 dB / km.
[0060] It will be easily understood by those skilled in the art that the above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. An integrated hollow core optical fiber preform, characterized in that: The invention comprises a sleeve, wherein a plurality of circumferentially distributed axial holes are opened in the sleeve wall, the minimum distance t1 between the inner wall of the axial hole and the inner wall of the sleeve is located on the side close to the center of the sleeve, and the ratio of t1 to the diameter of the axial hole is ≤0.
35.
2. The integrated hollow-core optical fiber preform according to claim 1, characterized in that: The axial holes are evenly distributed along the same ring line, and the number thereof is ≥4.
3. The integrated hollow-core optical fiber preform according to claim 1, wherein: The ratio of the inner diameter to the outer diameter of the sleeve is 0.2 to 0.
8.
4. The integrated hollow-core optical fiber preform according to claim 1, wherein: A capillary tube is inserted into the axial hole to form an optical fiber preform rod with a nested structure.
5. The integrated hollow-core optical fiber preform according to claim 1, wherein: A quartz plate is inserted into the axial hole to form an optical fiber preform rod with a connecting plate structure.
6. A method for preparing a hollow core microstructured optical fiber, characterized in that: The following steps are involved: Step 1: Select a sleeve and drill a hole from the end of the sleeve to prepare the integrated hollow-core optical fiber preform according to any one of claims 1 to 5; Step 2: The integrated hollow-core optical fiber preform obtained in step 1 is subjected to high-temperature drawing. During the drawing process, gas is introduced into the axial hole so that the air pressure in the axial hole is higher than the air pressure in the central hole of the sleeve. Due to the pressure difference between the axial hole and the central hole of the sleeve and the effect of surface tension, the axial hole protrudes toward the central hole of the sleeve after drawing, forming an anti-resonance ring with negative curvature. All anti-resonance rings together constitute an annular anti-resonance layer, and the area surrounded by the anti-resonance layer constitutes a hollow fiber core, thereby forming a hollow-core microstructure optical fiber with a negative curvature anti-resonance ring.
7. The method for preparing a hollow-core microstructured optical fiber according to claim 6, wherein: In step 1, after drilling, acid solution is introduced to etch the axial hole so that the ratio of the minimum distance t1 between the inner wall of the axial hole and the inner wall of the casing to the diameter of the axial hole is ≤0.
1.
8. The method for preparing a hollow-core microstructured optical fiber according to claim 7, wherein: In step 1, the acid solution is hydrofluoric acid.
9. The method for preparing a hollow-core microstructured optical fiber according to claim 6, wherein: In step 1, when a capillary is embedded in the axial hole, gas is also introduced into the capillary, and the pressure gradient in the capillary, the axial hole and the central hole of the sleeve is controlled to decrease.
10. The method for preparing a hollow-core microstructured optical fiber according to claim 9, wherein: In step 1, the gas introduced into the axial hole or the capillary is any one or more of compressed air, nitrogen, helium, and argon.
11. The method for preparing a hollow-core microstructured optical fiber according to claim 6, wherein: In step 2, the anti-resonance layer and the drawn sleeve form a cladding, the outer diameter of the cladding is 100-300 μm, and the diameter of the fiber core is 10-50 μm.
12. The method for preparing a hollow-core microstructured optical fiber according to claim 6, wherein: In step 2, the minimum wall thickness of the antiresonance ring is ≤ 2 μm.
13. A hollow core microstructure optical fiber, characterized in that: Prepared by the preparation method according to any one of claims 6 to 12.