Chip packaging method and device
Patent Information
- Application Number
- MYPI2025002859
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-11-08
- Filing Date
- 2023-04-23
- Publication Date
- 2024-05-08
AI Technical Summary
During the chip packaging process, indium chip spatter and voids cause damage to the thermal interface, affecting the reliability and heat dissipation performance of the chip. The existing technology relies on a vacuum environment and has complex processes and low efficiency.
The method of curing the sealing material first and then reflowing is used to form a protective layer on the surface of the indium chip to form a layered indium structure, which avoids the use of flux and vacuum environment, simplifies the process flow, and improves packaging efficiency.
It effectively improves the coverage of the connection surface, avoids the formation of voids, improves the stability and efficiency of the package, simplifies the process conditions, and reduces the risk of displacement between components.
Smart Images

Figure PI2025002859_DRAWING_001 
Figure PI2025002859_DRAWING_002 
Figure PI2025002859_DRAWING_003
Abstract
Description
Chip packaging method and device Technical Field
[0001] The present invention relates to the field of semiconductor packaging, and in particular to a chip packaging method and equipment. Background Art
[0002] During the packaging process, indium sheets are used as thermal interface materials, and flux assists in soldering the chip to the thermally conductive cover. During reflow soldering, indium material spatters, causing short circuits in surrounding capacitors and chips. It also creates voids in the thermal interface of the indium sheet, disrupting the thermal interface. During subsequent reflow soldering, spatter and voiding are further exacerbated, ultimately leading to a sharp decline in chip reliability and heat dissipation performance, potentially causing semiconductor device failure. Figure 1 illustrates the exacerbation of voiding during multiple reflow soldering processes. Existing techniques use flux at both soldering interfaces during the reflow soldering process to remove the indium oxide layer, achieving an oxidation-free indium surface. This allows the surface to wet the chip metal coating and the heat dissipation cover substrate, establishing a metallized bond and improving the joint coverage. However, while flux provides an oxide-free indium surface, its residues can become trapped between the indium and chip, and between the indium and the heat dissipation cover substrate, making voids more likely to form during subsequent reflow soldering.
[0003] Summary of the Invention
[0004] In order to solve the technical problems of the prior art, such as high void rate of thermal interface and dependence of packaging process on vacuum, the present invention provides a chip packaging method, comprising:
[0005] Arranging a sealing material on the substrate on which the chip is placed;
[0006] placing a layered indium structure on the upper surface of the chip, the layered indium structure comprising at least: a protective layer on a surface in contact with the chip, and a protective layer on a surface opposite to the surface in contact with the chip;
[0007] Placing a heat dissipation structure on the upper surface of the substrate, wherein the heat dissipation structure is combined with the sealing material to form a first preform;
[0008] curing the sealing material in the first preform at the first temperature as the peak temperature to form a second preform;
[0009] connecting the chip, the layered indium structure, and the heat dissipation structure of the second preform at a second temperature as a peak temperature;
[0010] Wherein, the first temperature is lower than the melting point of indium, and the second temperature is higher than the melting point of indium;
[0011] The protective layer volatilizes before the layered indium structure melts.
[0012] Preferably, the connecting the second preform with the second temperature as the peak temperature is not limited to a vacuum environment.
[0013] Preferably, the layered indium structure is formed by contacting a solution containing dissolved paraffin or resin with an indium sheet so that the solution adheres to the surface of the indium sheet, the organic solvent in the solution evaporates, and the paraffin or resin adheres to the surface of the indium sheet to form the layered indium structure.
[0014] Preferably, the chip packaging method includes: providing a connection structure on the lower surface of the substrate;
[0015] The connection of the connection structure to the lower surface of the substrate occurs simultaneously with the connection of the second preform with the second temperature being the peak temperature;
[0016] or,
[0017] The connection between the connection structure and the lower surface of the substrate occurs after the second preform is connected with the second temperature as the peak temperature, and the connection between the connection structure and the lower surface of the substrate is connected with the third temperature as the peak temperature.
[0018] Preferably, the connection structure is a solder ball.
[0019] Preferably, the first temperature ranges from 30°C to 150°C.
[0020] Preferably, the second temperature ranges from 157°C to 300°C.
[0021] Preferably, if the connection of the connection structure to the lower surface of the substrate occurs simultaneously with the connection of the second preform with the second temperature as the peak temperature, the second temperature ranges from 220° C. to 300° C.;
[0022] If the connection between the connection structure and the lower surface of the substrate occurs after the second preform is connected with the second temperature as the peak temperature, the connection structure and the lower surface of the substrate are connected with the third temperature as the peak temperature, the second temperature range is 157℃-200℃, and the third temperature range is 220℃-300℃.
[0023] Preferably, an active agent is provided on the outside of the protective layer, and the active agent is used to clean the surface of the protective layer in contact with the chip, and the surface opposite to the surface of the protective layer in contact with the chip.
[0024] A chip packaging device comprises a first workstation, a second workstation, a third workstation, a fourth workstation, and a fifth workstation;
[0025] The first workstation is used to arrange a sealing material on the substrate on which the chip is placed;
[0026] The second station is used to place a layered indium structure on the upper surface of the chip, the layered indium structure comprising at least: a protective layer on a surface in contact with the chip, and a protective layer on a surface opposite to the surface in contact with the chip;
[0027] The third workstation is used to place the heat dissipation structure on the upper surface of the substrate to form a first preform;
[0028] The fourth station is used to cure the sealing material to form a second preform; the method of curing the sealing material includes: curing the sealing material with a first temperature as a peak temperature;
[0029] wherein the first temperature is lower than the melting point of indium;
[0030] The fifth station is used to connect the second preform, and the method of connecting the second preform includes: connecting the chip, the layered indium structure, and the heat dissipation structure of the second preform at a second temperature as a peak temperature;
[0031] The second temperature is higher than the melting point of indium; and the protective layer volatilizes before the layered indium structure melts.
[0032] Preferably, the connecting the second preform with the second temperature as the peak temperature is not limited to a vacuum environment.
[0033] Preferably, the packaging equipment further comprises a sixth station, the sixth station being used to connect the connection structure with the lower surface of the substrate;
[0034] The connection of the connection structure to the lower surface of the substrate occurs simultaneously with the connection of the second preform with the second temperature being the peak temperature;
[0035] or,
[0036] The connection between the connection structure and the lower surface of the substrate occurs after the second preform is connected with the second temperature as the peak temperature, and the connection between the connection structure and the lower surface of the substrate is connected with the third temperature as the peak temperature.
[0037] Preferably, the connection structure is a solder ball.
[0038] Preferably, the first temperature ranges from 30°C to 150°C.
[0039] Preferably, the second temperature ranges from 157°C to 300°C.
[0040] Preferably, if the connection of the connection structure to the lower surface of the substrate occurs simultaneously with the connection of the second preform with the second temperature as the peak temperature, the second temperature ranges from 220° C. to 300° C.;
[0041] The connection between the connection structure and the lower surface of the substrate occurs after the second preform is connected with the second temperature as the peak temperature, and the connection structure and the lower surface of the substrate are connected with the third temperature as the peak temperature. The second temperature range is 157°C-200°C, and the third temperature range is 220°C-300°C.
[0042] Preferably, the second workstation and the third workstation are the same workstation, which sequentially perform placing the layered indium structure on the upper surface of the chip and placing the heat dissipation structure on the upper surface of the substrate.
[0043] Preferably, the first workstation, the second workstation and the third workstation are the same workstation, which sequentially perform the steps of arranging the sealing material on the substrate with the chip, placing the layered indium structure on the upper surface of the chip and placing the heat dissipation structure on the upper surface of the substrate.
[0044] Preferably, the fourth workstation and the fifth workstation are the same workstation, which sequentially perform the steps of curing the sealing material and connecting the second prefabricated component.
[0045] Preferably, the fifth station and the sixth station are the same station, and connect the second preform and the connection structure to the lower surface of the substrate sequentially or simultaneously.
[0046] Preferably, the fourth workstation, the fifth workstation and the sixth workstation are the same workstation, and sequentially perform curing of the sealing material, connecting the second preform, and connecting the connecting structure to the lower surface of the substrate;
[0047] Alternatively, after curing the sealing material, the second preform and the connection structure are connected to the lower surface of the substrate simultaneously.
[0048] The chip packaging method provided by the present invention adopts a method of first curing the seal and then reflowing to combine with a protective layer, thereby avoiding the necessary vacuum environment required in the reflow process, avoiding the vacuum pumping time, improving the packaging efficiency, and simplifying the process conditions; the layered indium structure obtained by attaching the indium sheet to the protective layer does not require flux, effectively improves the void condition of the connection surface, and improves the coverage rate of the connection surface. The layered indium structure provided with the protective layer has a similar bonding effect to the indium sheet provided with flux without affecting the packaging; with the support of achieving better coverage under the condition of the layered indium structure without flux, the present invention is able to adjust the process, integrate the process, avoid displacement between components, especially displacement of the layered indium structure relative to the chip, and improve the efficiency and stability of the packaging. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] In order to more clearly illustrate the embodiments of the invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0050] Figure 1 is a cross-sectional view of a soldering surface using flux;
[0051] FIG2 is a structural diagram of a chip packaged by the chip packaging method provided in Example 1;
[0052] FIG3 is a structural diagram of a chip packaging method provided in Example 1, which is applied to a chip packaged in a BGA manner;
[0053] FIG4 is a structural diagram of a chip packaging method provided in Example 1, which is applied to a chip packaged in a PGA manner;
[0054] FIG5 is a structural diagram of a chip packaging method provided in Example 1, which is applied to a chip packaged in an LGA manner;
[0055] FIG6 is a structural diagram of a layered indium structure in a chip packaging method provided in Example 1;
[0056] Figure 7 shows the soldered surface after the first reflow using the conventional process with flux solder sheets in the first set of tests.
[0057] FIG8 shows the soldering surface after the first reflow soldering using the packaging method provided in Example 1 in the first set of tests.
[0058] Figure 9 shows the soldering surface after the second reflow using the conventional process with flux solder sheets in the first set of tests.
[0059] FIG10 shows the soldering surface after the second reflow soldering using the packaging method provided in Example 1 in the first set of tests.
[0060] FIG11 is a comparison of the coverage distribution of the chip packaging method provided in Example 1 and the conventional process using flux solder sheets after the first and second reflow soldering in the first set of tests.
[0061] Figure 12 shows the soldering surface after the first reflow using the conventional process with flux solder sheets in the second set of tests.
[0062] FIG13 shows the soldering surface after the first reflow soldering using the packaging method provided in Example 1 in the second set of tests.
[0063] FIG14 shows the soldering surface after the second reflow process using the conventional process of flux solder sheets in the second set of tests.
[0064] FIG15 shows the soldering surface after the second reflow soldering using the packaging method provided in Example 1 in the second set of tests.
[0065] FIG16 is a comparison of the coverage distribution of the chip packaging method provided in Example 1 and the conventional process using flux solder sheets after the first and second reflow soldering in the second set of tests.
[0066] FIG17 shows the welding surface of the packaging method provided in the first embodiment in the third set of tests.
[0067] FIG18 shows the coverage distribution of the packaging method provided in Example 1 in the third group of tests.
[0068] FIG19 shows the welding surface of the packaging method provided in the first embodiment in the fourth set of tests.
[0069] FIG20 shows the coverage distribution of the packaging method provided in Example 1 in the fourth group of tests. DETAILED DESCRIPTION
[0070] In order to more clearly understand the above-mentioned objects, features and advantages of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be noted that, in the absence of conflict, the embodiments of the present application and the features therein can be combined with each other.
[0071] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways different from those described herein. Therefore, the scope of protection of the present invention is not limited to the specific embodiments disclosed below.
[0072] Example 1
[0073] This embodiment provides a chip 3 packaging method, forming a packaged device as shown in Figures 2-5. As shown in Figure 2, the packaged device includes: a substrate 1, a sealant 2 applied to the substrate 1, a heat dissipation cover 5 bonded to the sealant 2, a chip 3 disposed on the substrate 1, an interconnect structure 6 within the chip 3, and a layered indium structure 4 disposed on the chip 3.
[0074] The packaging method comprises:
[0075] The substrate 1 with the chip 3 on its upper surface is placed on the first workstation, and the sealant 2 is coated on the substrate 1 around the chip 3 .
[0076] The substrate 1 coated with the sealant 2 is transferred to the next workstation, where the layered indium structure 4 is placed on the upper surface of the chip 3. Without the need for station turnover, the heat dissipation cover plate 5 is placed on the upper surface of the substrate 1 where the layered indium structure 4 is placed at the same workstation.
[0077] In contrast, the typical process for chip packaging methods that require flux is as follows: apply flux to the chip's upper surface; transfer it to the next workstation, place an indium sheet on the flux-coated chip's surface; transfer it to the next workstation, apply flux to the indium sheet's upper surface; transfer it to the next workstation, apply sealant to the substrate surrounding the chip; transfer it to the next workstation, place a heat dissipation cover plate on the substrate in the area where the sealant is located; transfer it to the next workstation, and heat-press cure the sealant. This embodiment eliminates the need for flux, providing conditions for improving the processes of sealant, layered indium structure, and heat dissipation cover plate, avoiding unnecessary station transfers. Furthermore, because the heat dissipation cover plate is pressed against the layered indium structure, even if the packaging structure moves during subsequent processing, the layered indium structure will not shift from its fixed position on the chip's upper surface, thereby improving the stability of the package.
[0078] The layered indium structure 4 provided in this embodiment is free of flux on its surface, and no initial flux application process is required before the layered indium structure 4 is placed on the upper surface of the chip 3. After the layered indium structure 4 is placed on the upper surface of the chip 3, no secondary flux application process is required before the heat dissipation cover plate 5 or other heat dissipation structure is superimposed. This saves the time required for two flux application processes and optimizes the process flow. Furthermore, the flux-free layered indium structure 4 avoids the possibility of flux residue being trapped between the indium and the chip 3, or between the indium and the heat dissipation cover plate 1, which could cause voids in the indium sheet during the subsequent reflow process.
[0079] The area of the layered indium structure 4 is 0.5-30% larger than the area of the chip 3, preferably 5-15% larger than the area of the chip 3, and more preferably 7-12%. A protective layer is attached to the surface of the layered indium structure 4, and the protective layer prevents the layered indium structure 4 from being oxidized and completely volatilizes in the subsequent high-temperature process. The temperature of the protective layer is lower than the melting point of indium, so an oxide-free indium surface can be presented after the protective layer volatilizes. When the temperature of the reflow process reaches a peak and the temperature reaches the melting point of indium, the indium melts and acts as a solder to wet the chip 3 and the heat dissipation cover plate 5 and form a bond at the interface to complete the welding. In the traditional indium welding process, flux is required, and the flux acts as a temporary glue to achieve adhesion between the indium sheet and the surface of the chip 3. The packaging method provided in this embodiment does not use flux, and obtains temporary adhesion by applying pressure, so that in the absence of flux, the layered indium structure 4 as a thermal interface material (TIM) is pressed on the chip 3 to achieve temporary adhesion. Every 1mm 2 The flux-free layered indium structure 4 requires a pressure of more than 0.01kg (0.1N / mm 2 ). After the pressure is applied, the layered indium structure 4 is repeatedly 2The above-mentioned process of achieving adhesion without flux can therefore be handled normally without extra care. The layered indium structure 4 does not need to be placed at every 1 mm. 2 A force exceeding 0.01 kg is applied. Regardless of the size of the flux-free layered indium structure 4, a force of 100 N can be applied to a localized area of 10 x 10 mm to achieve spot adhesion. Furthermore, the use of liquid droplets can also provide temporary adhesion. For example, deionized water, isopropyl alcohol, ethane alcohol, or any volatile liquid below 110°C can be used.
[0080] The surface of the layered indium structure 4 is provided with a protective layer, and the formation method of the layered indium structure 4 is: a solution dissolving paraffin or resin is brought into contact with an indium sheet so that the solution is attached to the surface of the indium sheet, the organic solvent in the solution volatilizes, and the paraffin or resin is attached to the surface of the indium sheet to form the layered indium structure. The method of bringing the solution dissolving paraffin or resin into contact with the indium sheet includes placing the indium sheet in the solution, or spraying the solution on the indium sheet, etc. This embodiment does not limit the contact route, and the implementation of different contact routes does not affect the realization of the technical effect of this embodiment. The solution is a solution with a non-corrosive organic substrate, which complies with the provisions of RoHS and REACH, and specifically includes: an active agent, paraffin or resin, an organic solvent that can dissolve paraffin or resin, and the active agent is preferably an organic acid or a composition of an organic acid and an inorganic acid. The indium sheet is placed in the solution, and the surface treatment and protective layer setting are completed at the same time. The surface treatment removes the oxide layer on the surface of the indium sheet through organic acid treatment to obtain a pure indium sheet. Then, a solution is attached to the surface of the pure indium sheet. The pure indium sheet is removed from the solution. As the organic solvent that dissolves paraffin or resin evaporates, the paraffin or resin adheres to the surface of the pure indium sheet, forming a protective layer for the layered indium structure 4. The ultra-thin protective layer provided in this embodiment protects the surface of the layered indium structure 4, effectively preventing oxidation of the layered indium structure 4 during subsequent processing, storage, transportation, and before reflow soldering. In a high-temperature environment and during the indium reflow soldering process, the ultra-thin protective layer completely evaporates, exposing the oxide-free indium solder surface to achieve optimal wetting and prevent void formation.
[0081] In some embodiments, an active agent is further provided outside the protective layer on the surface of the layered indium structure 4. FIG6 is a structural diagram of a layered indium structure provided with a granular active agent, wherein 10 is an indium sheet, 11 is a protective layer, and 12 is an active agent. The form of the active agent is not limited, and it can be granular or layered, and it does not affect the realization of the technical effect of this embodiment. The active agent is used to clean the oxide on the surface of the protective layer of the layered indium structure in contact with the chip, and the oxide on the surface opposite to the surface of the protective layer of the layered indium structure in contact with the chip. The method of attaching the active agent to the protective layer on the surface of the layered indium structure 4 is not limited, and it can be carried out simultaneously with the setting of the protective layer, or it can be formed by coating or spraying after the protective layer is formed.
[0082] The substrate 1, on which the layered indium structure 4 and the heat dissipation cover plate 5 have been placed, is transferred to the next workstation and heat-cured with the sealant 2 by hot pressing. The temperature range for hot pressing curing is 30°C-150°C, more preferably 70°C-130°C, and even more preferably 120°C. During the hot pressing process of curing the sealant 2, the heat dissipation cover plate 5 and the substrate 1 form a sealed cavity, providing conditions for subsequent welding in a non-vacuum environment. At the same time, the protective layer on the surface of the layered indium structure 4 evaporates with heating, exposing the surface of the layered indium structure 4 without oxidation and protective layer, ready to form an intermetallic compound with the metal layer on the chip 3 or the heat dissipation cover plate 5 as pure indium, completing welding in the absence of flux.
[0083] The chip 3 and the heat dissipation cover plate 5 are connected through a reflow soldering process. The peak temperature of the reflow soldering process ranges from 157°C to 300°C, preferably 170°C. Since the surface of the layered indium structure 4 is not oxidized, and the heat dissipation cover plate 5 and the substrate 1 have been cured by the sealant 2, the layered indium structure 4 is in a sealed environment. The above-mentioned reflow soldering process does not need to be carried out in a vacuum environment to avoid oxidation of the layered indium structure 4. When the reflow soldering process temperature reaches the melting point of indium, the layered indium structure 4 wets the chip 3 and forms a bond at the interface. The reflow soldering process provided in this embodiment no longer requires a vacuum environment, simplifying the packaging process. In some embodiments, the sealant 2 curing process can be combined with the indium reflow soldering process, which is particularly beneficial for LGA packaging.
[0084] A connection structure is provided on the lower surface of the substrate 1, and the substrate 1 and the connection structure are connected by a reflow process. The peak temperature of the reflow process ranges from 220°C to 300°C, preferably 260°C. Similarly, the reflow process does not require a vacuum environment.
[0085] In some embodiments, the reflow process for the layered indium structure and the reflow process for the connection structure on the bottom surface of the substrate can be combined into a single reflow process. With a peak temperature of 220°C-300°C, a single high-temperature reflow process replaces the two-step low-temperature reflow process for the layered indium structure and the high-temperature reflow process for the connection structure, achieving simultaneous indium attachment and connection structure attachment. Conventional packaging methods that utilize flux or that require avoiding surface oxides on the indium sheet cannot support the simultaneous reflow of the layered indium structure and the connection structure on the bottom surface in some embodiments due to their reliance on vacuum.
[0086] The chip packaging method provided in this embodiment is not limited to a specific packaging method. For example, a BGA packaging method, as shown in FIG3 , includes a substrate 1, a sealant 2 applied on the substrate 1, a heat dissipation cover plate 5 combined with the sealant 2, a chip 3 disposed on the substrate 1, a layered indium structure 4 disposed on the chip 3, and solder balls 7. For example, a PGA packaging method, as shown in FIG4 , includes a substrate 1, a sealant 2 applied on the substrate 1, a heat dissipation cover plate 5 combined with the sealant 2, a chip 3 disposed on the substrate 1, a layered indium structure 4 disposed on the chip 3, and solder pins 8. For example, an LGA packaging method, as shown in FIG5 , includes a substrate 1, a sealant 2 applied on the substrate 1, a heat dissipation cover plate 5 combined with the sealant 2, a chip 3 disposed on the substrate 1, a layered indium structure 4 disposed on the chip 3, and array electrode contacts 9.
[0087] As shown in Figures 7 to 11, the coverage of the chip 3 packaging method provided by this embodiment is compared with the traditional process using flux solder sheets. The test conditions are:
[0088] Analog chip 3 size: 20mm*35mm;
[0089] First reflow conditions: peak temperature of 170°C, vacuum conditions;
[0090] Second reflow conditions: peak temperature of 260°C, no vacuum conditions.
[0091] As shown in Figure 7, after the first reflow, the coverage of the conventional process using flux pads was 89.1%. As shown in Figure 8, after the first reflow, the coverage of the chip 3 packaging method provided by this embodiment was 98.2%. As shown in Figure 9, after the second reflow, the coverage of the conventional process using flux pads was 78.3%. As shown in Figure 10, after the second reflow, the coverage of the chip 3 packaging method provided by this embodiment was 97.5%. Figure 11 compares the coverage of the chip 3 packaging method provided by this embodiment with the coverage distribution of the conventional process using flux pads after the first and second reflows. As shown in Figure 11, the coverage of the chip 3 packaging method provided by the present invention is significantly better than that of the conventional process using flux pads under the above test conditions, and the confidence interval is narrower.
[0092] Figures 12-16 show a comparison of the coverage of the chip 3 packaging method provided in this embodiment with the conventional process using flux solder sheets. The test conditions are:
[0093] Analog chip 3 size: 20mm*35mm;
[0094] The first reflow soldering conditions: peak temperature of 170°C, no vacuum conditions;
[0095] Second reflow conditions: peak temperature of 260°C, no vacuum conditions.
[0096] As shown in Figure 12, after the first reflow, the coverage of the conventional process using flux pads was 83.1%. As shown in Figure 13, after the first reflow, the coverage of the chip 3 packaging method provided by this embodiment was 97.9%. As shown in Figure 14, after the second reflow, the coverage of the conventional process using flux pads was 62.3%. As shown in Figure 15, after the second reflow, the coverage of the chip 3 packaging method provided by this embodiment was 94.5%. Figure 16 compares the coverage of the chip 3 packaging method provided by this embodiment with the coverage distribution of the conventional process using flux pads after the first and second reflows. As shown in Figure 16, the coverage of the chip 3 packaging method provided by the present invention is significantly better than that of the conventional process using flux pads under the above test conditions, and the confidence interval is narrower. As the vacuum conditions change to no-vacuum conditions, the coverage of the traditional process using flux solder sheets is significantly reduced due to the removal of the vacuum conditions, which greatly affects the welding effect. However, the coverage reduction of the chip 3 packaging method provided in this embodiment is relatively small and does not have a significant impact on the welding situation.
[0097] FIG17 shows the coverage of the chip 3 packaging method provided in this embodiment, in which the indium attachment reflow process is combined with the ball attachment reflow process, using a single high-temperature reflow process to replace the two-step low-temperature layered indium structure 4 reflow process and the high-temperature ball attachment reflow process. This single high-temperature reflow process cannot be achieved using the traditional process using flux solder sheets. The test conditions are:
[0098] Analog chip 3 size: 20mm*35mm;
[0099] Reflow conditions: peak temperature of 260°C, no vacuum conditions.
[0100] Without the pre-indium attachment reflow step, as shown in Figure 17, after a single high-temperature reflow, the coverage of the chip 3 packaging method provided by this embodiment is 97.6%. Figure 18 shows the distribution of the coverage of the chip 3 packaging method provided by this embodiment, which still has a small confidence interval and a high coverage.
[0101] FIG18 shows the coverage of the sealant 2 curing process combined with the indium reflow soldering process.
[0102] The test conditions are:
[0103] Analog chip 3 size: 20mm*35mm;
[0104] Sealant 2 curing: 190°C for 3 minutes, applying a pressure of 100N.
[0105] As shown in Figure 19, the distribution of the coverage of the sealant 2 curing process that can be combined with the indium reflow soldering process has a confidence interval smaller than the confidence interval of the coverage of the traditional process using flux solder sheets, and the overall coverage is higher than the coverage of the traditional process using flux solder sheets.
[0106] The chip packaging method provided in this embodiment adopts the method of first curing the seal and then reflowing to combine with the protective layer, avoiding the necessary vacuum environment required in the reflow process, avoiding the vacuum pumping time, improving the packaging efficiency, and simplifying the process conditions; the layered indium structure obtained by attaching the indium sheet to the protective layer in this embodiment does not require flux, effectively improves the void condition of the connection surface, and improves the coverage rate of the connection surface. The layered indium structure with the protective layer has a similar bonding effect to the indium sheet with flux without affecting the packaging; with the support of achieving better coverage under the condition of flux-free layered indium structure, this embodiment is able to adjust the process, integrate the process, avoid displacement between components, especially displacement of the layered indium structure relative to the chip, and improve the efficiency and stability of packaging.
[0107] Example 2
[0108] This embodiment provides a chip packaging device, including a first workstation, a second workstation, a third workstation, and a fourth workstation.
[0109] The first workstation is used to apply sealant on the substrate around the chip.
[0110] The second station is used to place a layered indium structure on the upper surface of the chip.
[0111] The layered indium structure includes at least a surface in contact with the chip and a protective layer on a surface opposite to the surface in contact with the chip.
[0112] The layered indium structure provided in this embodiment is flux-free. Furthermore, there is no need for a first flux application process before the layered indium structure is placed on the chip surface. After the layered indium structure is placed on the chip surface, there is no need for a second flux application process before the heat dissipation cover or other heat dissipation structure is stacked. This saves time during the two flux application processes and optimizes the process flow. Furthermore, the flux-free layered indium structure prevents the possibility of flux residue being trapped between the indium and the chip, or between the indium and the heat dissipation cover substrate, which could lead to voids in the indium sheet during the subsequent reflow process.
[0113] The area of the layered indium structure 4 is 0.5-30% larger than the area of the chip 3, preferably 5-15% larger than the area of the chip 3, more preferably 7-12%. A protective layer is attached to the surface of the layered indium structure 4, and the protective layer prevents the layered indium structure 4 from being oxidized and completely volatilizes in the subsequent high-temperature process. The temperature of the protective layer is lower than the melting point of indium, so an oxide-free indium surface can be presented after the protective layer volatilizes. When the temperature of the reflow process reaches a peak and the temperature reaches the melting point of indium, the indium melts and acts as a solder to wet the chip 3 and the heat dissipation cover plate 5 and form a bond at the interface to complete the welding. In the traditional indium welding process, flux is required, and the flux acts as a temporary glue to achieve adhesion between the indium sheet and the surface of the chip 3. The packaging method provided in this embodiment does not use flux, and obtains temporary adhesion by applying pressure, so that in the absence of flux, the layered indium structure 4 as a thermal interface material (TIM) is pressed on the chip 3 to achieve temporary adhesion. Every 1mm 2 The flux-free layered indium structure 4 requires a pressure of more than 0.01kg (0.1N / mm 2 ). After the pressure is applied, the layered indium structure 4 is repeatedly 2 The above-mentioned process of achieving adhesion without flux can therefore be handled normally without extra care. The layered indium structure 4 does not need to be placed at every 1 mm. 2A force exceeding 0.01 kg is applied. Regardless of the size of the flux-free layered indium structure 4, a force of 100 N can be applied to a localized area of 10 x 10 mm to achieve spot adhesion. Furthermore, the use of liquid droplets can also provide temporary adhesion. For example, deionized water, isopropyl alcohol, ethane alcohol, or any volatile liquid below 110°C can be used.
[0114] The surface of the layered indium structure 4 is provided with a protective layer, and the formation method of the layered indium structure 4 is: a solution dissolving paraffin or resin is brought into contact with an indium sheet so that the solution is attached to the surface of the indium sheet, the organic solvent in the solution volatilizes, and the paraffin or resin is attached to the surface of the indium sheet to form the layered indium structure. The method of bringing the solution dissolving paraffin or resin into contact with the indium sheet includes placing the indium sheet in the solution, or spraying the solution on the indium sheet, etc. This embodiment does not limit the contact route, and the implementation of different contact routes does not affect the realization of the technical effect of this embodiment. The solution is a solution with a non-corrosive organic substrate, which complies with the provisions of RoHS and REACH, and specifically includes: an active agent, paraffin or resin, an organic solvent that can dissolve paraffin or resin, and the active agent is preferably an organic acid or a composition of an organic acid and an inorganic acid. The indium sheet is placed in the solution, and the surface treatment and protective layer setting are completed at the same time. The surface treatment removes the oxide layer on the surface of the indium sheet through organic acid treatment to obtain a pure indium sheet. Then, a solution is attached to the surface of the pure indium sheet. The pure indium sheet is removed from the solution. As the organic solvent that dissolves paraffin or resin evaporates, the paraffin or resin adheres to the surface of the pure indium sheet, forming a protective layer for the layered indium structure 4. The ultra-thin protective layer provided in this embodiment protects the surface of the layered indium structure 4, effectively preventing oxidation of the layered indium structure 4 during subsequent processing, storage, transportation, and before reflow soldering. In a high-temperature environment and during the indium reflow soldering process, the ultra-thin protective layer completely evaporates, exposing the oxide-free indium solder surface to achieve optimal wetting and prevent void formation.
[0115] In some embodiments, an active agent is provided outside the protective layer on the surface of the layered indium structure 4. The active agent is used to clean oxides on the surface of the protective layer in contact with the chip, as well as on the surface opposite the surface of the protective layer in contact with the chip. The method for attaching the active agent to the protective layer on the surface of the layered indium structure 4 is not limited and can be applied simultaneously with the provision of the protective layer, or after the protective layer is formed by coating or spraying.
[0116] The third workstation is used to place a heat dissipation cover plate on the upper surface of the substrate.
[0117] The fourth station is used to cure the sealing material, and the method for curing the sealing material includes: curing the first preform sealing material with a first temperature as the peak temperature to form a second preform; the first temperature is higher than the volatilization temperature of the protective layer, and the first temperature is lower than the melting point of indium. Specifically, the sealant is cured by hot pressing, and the temperature range of hot pressing curing is 30°C-150°C, more preferably 70°C-130°C, and more preferably 120°C. In the process of hot pressing curing the sealant, the heat dissipation cover layer and the substrate form a sealed cavity, providing conditions for subsequent welding in a non-vacuum environment. At the same time, the protective layer on the surface of the layered indium structure evaporates as it is heated, exposing the surface of the layered indium structure without oxidation and protective layer, so that it can be used as pure indium to form an intermetallic compound with the metal-plated layer on the chip or the heat dissipation cover, and complete welding without flux.
[0118] The fifth workstation is used to weld the second preform, and the method of welding the second preform includes: welding the second preform with a second temperature as the peak temperature, and the second temperature is higher than the melting point of indium. Specifically, the chip and the heat dissipation cover are connected by a reflow soldering process. The peak temperature of the reflow soldering process ranges from 157°C to 300°C, preferably 170°C. Since the surface of the layered indium structure is not oxidized, and the heat dissipation cover and the substrate have been cured by the sealant, the periphery of the layered indium structure is in a sealed environment, and the above-mentioned reflow soldering process does not need to be carried out in a vacuum environment to avoid oxidation of the layered indium structure. When the temperature of the reflow soldering process reaches the melting point of indium, the layered indium structure wets the chip and forms a bond at the interface. The reflow soldering process provided in this embodiment no longer requires a vacuum environment, simplifies the packaging process, avoids vacuum pumping time, and thus effectively improves production efficiency. In some embodiments, the sealant curing process can be combined with the indium reflow soldering process, which is particularly beneficial for LGA packaging.
[0119] The packaging equipment may further include a sixth station configured to connect a connection structure to the lower surface of the substrate; the connection structure to the lower surface of the substrate is connected simultaneously with the connection of the second preform at the second peak temperature; or the connection structure to the lower surface of the substrate is connected after the second preform is connected at the second peak temperature, and then the connection structure to the lower surface of the substrate is connected at a third peak temperature. The type of the connection structure is not limited and may include solder balls, solder pins, arrayed electrode contacts, etc.
[0120] The chip packaging method provided in this embodiment is not limited to a specific packaging method. For example, a BGA packaging method includes a substrate, a sealant applied on the substrate, a heat dissipation cover plate combined with the sealant, a chip disposed on the substrate, a layered indium structure disposed on the chip, and solder balls. For example, a PGA packaging method includes a substrate, a sealant applied on the substrate, a heat dissipation cover plate combined with the sealant, a chip disposed on the substrate, a layered indium structure disposed on the chip, and solder pins. For example, an LGA packaging method includes a substrate, a sealant applied on the substrate, a heat dissipation cover plate combined with the sealant, a chip 3 disposed on the substrate, a layered indium structure disposed on the chip, and array electrode contacts.
[0121] For example, a BGA package is placed on the bottom surface of the substrate, and solder balls are connected to the substrate via a reflow process. The peak temperature of the reflow process ranges from 220°C to 300°C, preferably 260°C. Similarly, the reflow process does not require a vacuum environment.
[0122] In some embodiments, the layered indium structure reflow process and the solder ball reflow process can be combined into one reflow process, with a peak temperature of 220°C-300°C. A single high-temperature reflow process is used to replace the two-step low-temperature layered indium structure reflow process and the high-temperature connection structure reflow process, thereby simultaneously achieving the welding of indium attachment and connection structure attachment.
[0123] In some embodiments, the second workstation and the third workstation are the same workstation, which sequentially perform the steps of placing the layered indium structure on the upper surface of the chip and placing the heat dissipation structure on the upper surface of the substrate. The layered indium structure is placed on the upper surface of the chip at this workstation. There is no need for workstation turnover, and the heat dissipation cover is placed on the upper surface of the substrate where the layered indium structure is placed at the same workstation. Since the heat dissipation cover is pressed on the layered indium structure, even if the packaging structure moves in the subsequent process, the layered indium structure will not shift from the fixed position on the upper surface of the chip, thereby improving the stability of the package. In some embodiments, the first workstation, the second workstation, and the third workstation are the same workstation, which sequentially perform the steps of arranging the sealing material on the substrate with the chip, placing the layered indium structure on the upper surface of the chip, and placing the heat dissipation structure on the upper surface of the substrate. The above-mentioned completion of multiple arrangement tasks at the same workstation avoids the flow of semi-finished products between workstations, reduces the possibility of relative position shifting between components, and improves the stability of the package.
[0124] In some embodiments, the fourth station and the fifth station are the same station, and sequentially perform the curing of the sealing material and the connection of the second preform. In some embodiments, the fifth station and the sixth station are the same station, and sequentially perform the connection of the second preform and the connection structure to the lower surface of the substrate, or simultaneously perform the connection of the second preform and the connection structure to the lower surface of the substrate. In some embodiments, the fourth station, the fifth station and the sixth station are the same station, and sequentially perform the curing of the sealing material, the connection of the second preform and the connection structure to the lower surface of the substrate; or, after curing the sealing material, simultaneously perform the connection of the second preform and the connection structure to the lower surface of the substrate. The above-mentioned completion of multiple layout tasks by the same station improves the utilization rate of the equipment, reduces the overall volume of the packaging equipment, reduces the flow of semi-finished products, and the simultaneous realization of multiple heating temperatures at the same station can greatly improve the production efficiency.
[0125] The chip packaging equipment provided by this embodiment supports the use of a method of first curing the seal and then reflow soldering to combine with a protective layer, avoiding the necessary vacuum environment required in the reflow soldering process, avoiding the vacuum pumping time, improving the packaging efficiency, and simplifying the process conditions; the layered indium structure obtained by attaching the indium sheet to the protective layer in this embodiment does not require flux, effectively improves the void condition of the connection surface, and improves the coverage rate of the connection surface. The layered indium structure with a protective layer has a similar bonding effect to the indium sheet with flux, which does not affect the packaging; with the support of achieving better coverage under the condition of flux-free layered indium structure, this embodiment is able to adjust the process, integrate the process and workstations, avoid displacement between components, especially the displacement of the layered indium structure relative to the chip, and improve the efficiency and stability of packaging.
[0126] For the purpose of illustration, the foregoing description uses specific nomenclature to provide a thorough understanding of the embodiments. However, it will be apparent to those skilled in the art that specific details are not required to practice the embodiments. Therefore, for the purpose of illustration and description, the foregoing description of the specific embodiments described herein is presented. These descriptions are not intended to be exhaustive or to limit the embodiments to the precise form disclosed. It will be apparent to those skilled in the art that, in view of the above teachings, many modifications and variations are feasible. In addition, when used herein to refer to the position of a component, the terms above and below or their synonyms do not necessarily refer to an absolute position relative to an external reference, but rather to the relative position of the component with reference to the accompanying drawings.
[0127] Furthermore, the foregoing figures and descriptions include many concepts and features that can be combined in various ways to achieve a variety of benefits and advantages. Thus, features, components, elements, and / or concepts from various different figures can be combined to produce embodiments or implementations that are not necessarily shown or described in this specification. Furthermore, in any particular embodiment and / or implementation, not all features, components, elements, and / or concepts shown in the specific figures or descriptions are necessarily required. It should be understood that such embodiments and / or implementations fall within the scope of this specification.
Claims
1. A chip packaging method, characterized in that: include: Arranging a sealing material on the substrate on which the chip is placed; placing a layered indium structure on the upper surface of the chip, the layered indium structure comprising at least: a protective layer on a surface in contact with the chip, and a protective layer on a surface opposite to the surface in contact with the chip; Placing a heat dissipation structure on the upper surface of the substrate, wherein the heat dissipation structure is combined with the sealing material to form a first preform; curing the sealing material in the first preform at the first temperature as the peak temperature to form a second preform; connecting the chip, the layered indium structure, and the heat dissipation structure of the second preform at a second temperature as a peak temperature; Wherein, the first temperature is lower than the melting point of indium, and the second temperature is higher than the melting point of indium; The protective layer volatilizes before the layered indium structure melts.
2. The chip packaging method according to claim 1, wherein: The connecting of the second preform with the second temperature as the peak temperature is not limited to a vacuum environment.
3. The chip packaging method according to claim 1, wherein: The layered indium structure is formed by contacting a solution containing dissolved paraffin or resin with an indium sheet so that the solution adheres to the surface of the indium sheet, and the organic solvent in the solution evaporates, and the paraffin or resin adheres to the surface of the indium sheet to form the layered indium structure.
4. The chip packaging method according to claim 1, wherein: The chip packaging method includes: providing a connection structure on the lower surface of the substrate; The connection of the connection structure to the lower surface of the substrate occurs simultaneously with the connection of the second preform with the second temperature being the peak temperature; or, The connection between the connection structure and the lower surface of the substrate occurs after the second preform is connected with the second temperature as the peak temperature, and the connection between the connection structure and the lower surface of the substrate is connected with the third temperature as the peak temperature.
5. The chip packaging method according to claim 4, characterized in that: The connection structure is a solder ball.
6. The chip packaging method according to claim 1, wherein: The first temperature ranges from 30°C to 150°C.
7. The chip packaging method according to claim 1, wherein: The second temperature ranges from 157°C to 300°C.
8. The chip packaging method according to claim 4, wherein: If the connection of the connection structure to the lower surface of the substrate occurs simultaneously with the connection of the second preform with the second temperature as the peak temperature, the second temperature is in the range of 220° C. to 300° C.; If the connection between the connection structure and the lower surface of the substrate occurs after the second preform is connected with the second temperature as the peak temperature, the connection structure and the lower surface of the substrate are connected with the third temperature as the peak temperature, the second temperature range is 157℃-200℃, and the third temperature range is 220℃-300℃.
9. The chip packaging method according to claim 1, wherein: An active agent is disposed on the outside of the protective layer, and the active agent is used to clean the surface of the protective layer in contact with the chip, and the surface opposite to the surface of the protective layer in contact with the chip.
10. A chip packaging device, characterized in that: Including the first workstation, the second workstation, the third workstation, the fourth workstation, and the fifth workstation; The first workstation is used to arrange a sealing material on the substrate on which the chip is placed; The second station is used to place a layered indium structure on the upper surface of the chip. At least comprising: a protective layer on a surface in contact with the chip, and a protective layer on a surface opposite to the surface in contact with the chip; The third workstation is used to place the heat dissipation structure on the upper surface of the substrate to form a first preform; The fourth station is used to cure the sealing material to form a second preform; the method of curing the sealing material includes: curing the sealing material with a first temperature as a peak temperature; wherein the first temperature is lower than the melting point of indium; The fifth station is used to connect the second preform, and the method of connecting the second preform includes: connecting the chip, the layered indium structure, and the heat dissipation structure of the second preform at a second temperature as a peak temperature; The second temperature is higher than the melting point of indium; and the protective layer volatilizes before the layered indium structure melts.
11. The chip packaging device according to claim 10, wherein: The connecting of the second preform with the second temperature as the peak temperature is not limited to a vacuum environment.
12. The chip packaging device according to claim 10, wherein: The packaging equipment further includes a sixth station, the sixth station being configured to connect the connection structure to the lower surface of the substrate; The connection of the connection structure to the lower surface of the substrate occurs simultaneously with the connection of the second preform with the second temperature being the peak temperature; or, The connection between the connection structure and the lower surface of the substrate occurs after the second preform is connected with the second temperature as the peak temperature, and the connection between the connection structure and the lower surface of the substrate is connected with the third temperature as the peak temperature.
13. The chip packaging device according to claim 12, wherein: The connection structure is a solder ball.
14. The chip packaging device according to claim 10, wherein: The first temperature ranges from 30°C to 150°C.
15. The chip packaging device according to claim 10, wherein: The second temperature ranges from 157°C to 300°C.
16. The chip packaging device according to claim 12, wherein: If the connection of the connection structure to the lower surface of the substrate occurs simultaneously with the connection of the second preform with the second temperature as the peak temperature, the second temperature is in the range of 220° C. to 300° C.; The connection between the connection structure and the lower surface of the substrate occurs after the second preform is connected with the second temperature as the peak temperature, and the connection structure and the lower surface of the substrate are connected with the third temperature as the peak temperature. The second temperature range is 157°C-200°C, and the third temperature range is 220°C-300°C.
17. The chip packaging device according to any one of claims 10 to 16, characterized in that: The second workstation and the third workstation are the same workstation, which sequentially place the layered indium structure on the upper surface of the chip and place the heat dissipation structure on the upper surface of the substrate.
18. The chip packaging device according to any one of claims 10 to 16, characterized in that: The first station, the second station and the third station are the same station, which sequentially arrange the sealing material on the substrate with the chip, place the layered indium structure on the upper surface of the chip and place the heat dissipation structure on the upper surface of the substrate.
19. The chip packaging device according to any one of claims 10-16, characterized in that: The fourth work station and the fifth work station are the same work station, and sequentially perform curing of the sealing material and connection of the second prefabricated component.
20. The chip packaging device according to any one of claims 12, 13 or 16, characterized in that: The fifth station and the sixth station are the same station, and sequentially connect the second preform and the connection structure to the lower surface of the substrate, or simultaneously connect the second preform and the connection structure to the lower surface of the substrate.
21. The chip packaging device according to any one of claims 12, 13 or 16, characterized in that: The fourth work station, the fifth work station and the sixth work station are the same work station, and sequentially perform curing of the sealing material, connecting the second preform, and connecting the connecting structure to the lower surface of the substrate; Alternatively, after curing the sealing material, the second preform and the connection structure are connected to the lower surface of the substrate simultaneously.