Surface treatment composition for zinc alloy plated steel sheet, zinc alloy plated steel sheet surface-treated using same and method for manufacturing same
Patent Information
- Application Number
- MYPI2025002862
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-11-18
- Filing Date
- 2023-11-17
- Publication Date
- 2024-05-18
AI Technical Summary
Zinc alloy-plated steel sheets face issues with corrosion resistance, white rust, and fingerprint discoloration, especially in high-temperature and humid environments, and existing surface treatment agents often contain heavy metals like chromium, leading to environmental pollution and safety concerns.
A surface treatment composition comprising a resin mixture of high molecular weight polysilicon modified polyurethane, low molecular weight polysilicon modified polyurethane, and epoxy auxiliary resins, along with melamine-based hardener, oxidation and discoloration inhibitors, silane compounds, and anti-fingerprint improvers, which forms a surface treatment film that provides excellent corrosion resistance and anti-fingerprint properties without using heavy metals.
The composition effectively prevents corrosion, white rust, and fingerprint discoloration on zinc alloy-plated steel sheets, ensuring excellent surface appearance and environmental safety by eliminating the use of hazardous heavy metals.
Abstract
Description
Surface treatment composition for zinc alloy-plated steel sheet, zinc alloy-plated steel sheet surface-treated using the same, and method for manufacturing the same
[0001] The present invention relates to a surface treatment composition for a zinc alloy-plated steel sheet, a zinc alloy-plated steel sheet surface-treated using the composition, and a method for manufacturing the same.
[0002]
[0003] In general, steel sheets with a zinc alloy plating layer (a representative example is hot-dip zinc alloy plating steel sheets containing magnesium (Mg) and aluminum (Al)) have superior corrosion resistance to red rust compared to pure zinc-plated steel sheets, and most of the exposed surface is composed of zinc (Zn) or zinc alloy (Zn alloy), so when exposed to general living environments or, especially, a humid atmosphere, white rust occurs on the surface. In addition, since magnesium and aluminum contained in the plating layer have a higher affinity for oxygen than zinc, blackening is likely to occur when there is a shortage of oxygen that binds to zinc.
[0004] Moreover, compared to pure galvanized steel sheets, if fingerprint resistance is not secured when the surface is contaminated with fingerprints and contaminants, the contaminants will penetrate the plating layer and incompletely oxidize, causing black stains and discoloration, which will deteriorate the surface appearance. Such surface stains and discoloration defects tend to occur more frequently, especially when used in high-temperature and humid environments.
[0005]
[0006] Traditionally, as part of rust prevention treatment, the metal surface was treated with 5 to 100 mg / m 2After pretreatment with chromate, an organic film was formed. However, due to the heavy metals such as chromium (Cr) contained in the pretreatment agent, not only additional pretreatment facilities and processes were required, but also the safety of workers was a problem due to heavy metal wastewater. In addition, since the solution containing hexavalent chromium generated from wash water and wastewater had to be treated according to a special treatment process, there was a problem of increasing manufacturing costs, and the chromate-treated plated steel sheet also had a problem of chromium ions being dissolved during use or disposal, resulting in serious environmental pollution.
[0007]
[0008] To address these issues and ensure corrosion resistance, prior art has developed surface treatment agents, such as corrosion-resistant metal coatings that do not contain chromium. For example, Patent Documents 1 and 2 disclose techniques for forming a film by containing aluminum biphosphate, or combining tannic acid with aromatic carboxylic acids such as sodium acetate, sodium borate, and imidazole, and surfactants, but these have the problem of poor corrosion resistance. Patent Document 3 discloses a surface treatment agent composed of zirconium carbonate, vanadyl ions, and zirconium compounds, but while this has good corrosion resistance, it has the problem of being susceptible to blackening.
[0009] Meanwhile, Patent Document 4 discloses a surface treatment agent composed of titanium-based, zirconium-based, phosphoric acid-based, and molybdenum-based compounds, but has the problem that it cannot suppress blackening in zinc alloy-plated steel sheets using magnesium (Mg), aluminum (Al), etc. Patent Document 5 discloses a surface treatment agent composed of ammonium molybdate, water-dispersed urethane resin, isopropylamine, ammonium zirconium carbonate, an epoxy-based silane coupling agent, and silica sol, but has the problem that it cannot provide sufficient corrosion resistance.
[0010]
[0011] Recently, in order to use zinc alloy-plated steel sheets as building materials, they must have beautiful surface characteristics and exhibit excellent corrosion resistance in corrosive environments. In addition, it is important to ensure that they do not discolor when exposed to fingerprints or contaminants during handling by customers and that they are fingerprint-resistant or discoloration-resistant.
[0012]
[0013] (Patent Document 1) Japanese Patent Publication No. 53-28857
[0014] (Patent Document 2) Japanese Patent Publication No. 51-71233
[0015] (Patent Document 3) Japanese Patent Publication No. 2002-332574
[0016] (Patent Document 4) Japanese Patent Publication No. Hei 7-096699
[0017] (Patent Document 5) Japanese Patent Publication No. 2005-146340
[0018]
[0019] One aspect of the present invention is to provide a surface treatment composition capable of imparting excellent corrosion resistance, fingerprint resistance, and contamination discoloration resistance to zinc alloy-plated steel sheets used as building materials, etc.
[0020] In particular, it is intended to provide a surface treatment composition capable of imparting excellent corrosion resistance and anti-fingerprint discoloration properties to a zinc alloy-plated steel sheet under a high temperature and high humidity environment.
[0021] In addition, we aim to provide a surface treatment composition that does not contain any heavy metal components such as chromium, which are environmental pollutants, and is therefore harmless to the human body and does not cause problems due to environmental pollution.
[0022] In addition, the present invention aims to provide a zinc alloy plated steel sheet having excellent corrosion resistance, fingerprint resistance, and contamination discoloration resistance, and a method for manufacturing the same.
[0023]
[0024] The objectives of the present invention are not limited to the above-described matters. Additional objectives of the present invention are described throughout the specification, and those skilled in the art will have no difficulty understanding the additional objectives of the present invention from the contents described in the specification.
[0025]
[0026] One aspect of the present invention is a surface treatment composition comprising a solid and a solvent,
[0027] The above surface treatment composition, based on 100 wt% of solid content,
[0028] 70 to 90 wt% of a resin mixture comprising a high molecular weight polysilicon-modified polyurethane main resin, a low molecular weight polysilicon-modified polyurethane auxiliary resin, and an epoxy auxiliary resin;
[0029] 5 to 25 wt% of melamine-based curing agent;
[0030] 0.5 to 10 wt% of anti-oxidation and discoloration agent;
[0031] 0.5 to 10 wt% of silane compound;
[0032] 0.5 to 10 wt% of anti-corrosion agent; and
[0033] It relates to a surface treatment composition comprising 0.5 to 5 wt% of an anti-fingerprint improving agent.
[0034] The above high molecular weight polysilicon-modified polyurethane main resin (A), low molecular weight polysilicon-modified polyurethane auxiliary resin (B), and epoxy auxiliary resin (C) may be mixed in a weight ratio of 1:4.5:4.5 to 9:0.5:0.5.
[0035] The above high molecular weight polysilicon modified polyurethane main resin (A) may have a glass transition temperature (Tg) of -20°C to -10°C and a weight average molecular weight (Mw) of 100,000 to 200,000.
[0036] The above low molecular weight polysilicon modified polyurethane auxiliary resin (B) may have a glass transition temperature (Tg) of -30°C to -20°C and a weight average molecular weight (Mw) of 30,000 to 70,000.
[0037] The above epoxy auxiliary resin (C) may have an epoxide equivalent ratio of 450 to 550 g / eq and a weight average molecular weight (Mw) of 450 to 4,000.
[0038] The above melamine-based curing agent includes at least one functional group selected from the group consisting of methoxy methyl, methylol, and imino functional groups, and the functional group may be a crosslinking skeletal polymer resin containing a carboxyl group.
[0039] The above-mentioned anti-oxidation and anti-discoloration agent may be at least one selected from the group consisting of ammonium molybdate and sodium molybdate.
[0040] The above silane compounds are vinylmethoxy silane, vinyltrimethoxy silane, vinylepoxy silane, vinyltriepoxy silane, methyltrimethoxysilane, tetraethylorthosilicate, tetramethylorthosilicate, 3-aminopropyltriepoxy silane, 3-glycidoxypropyltrimethoxy silane, 3-glycidoxypropyltriethoxy silane, 3-mercaptopropyltrimethoxy silane, N-(1,3 dimethylbutylidene)-3-(triepoxy silane)-1-propanamine, N,N-bis[3-(trimethoxysilyl)propyl]ethylenediamine, N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxy silane, It may be at least one selected from the group consisting of γ-mercaptopropyltriethoxysilane, and N-[2-(vinylbenzylamino) ethyl]-3-aminopropyltrimethoxysilane.
[0041] The above silane compound may be hydrolyzed by one or more acids selected from the group consisting of formic acid, acetic acid, phosphoric acid, hydrochloric acid, and nitric acid.
[0042] The above-mentioned rust inhibitor may be at least one selected from the group consisting of a phosphoric acid rust inhibitor, a fluorine rust inhibitor, a vanadium rust inhibitor, a cerium salt rust inhibitor, and a selenium salt rust inhibitor.
[0043] The above-mentioned anti-fingerprint improving agent may be at least one selected from the group consisting of paraffin wax, olefin wax, carnauba wax, polyester wax, polypropylene wax, polyethylene-Teflon wax, and polyTeflon wax.
[0044] The solid content may be 20 to 40 wt% based on the total weight of the surface treatment composition, and the remainder may be a solvent.
[0045] The solvent may contain 20 to 40 wt% of N-ethyl-2-pyrrolidone (NEP) and the remainder of water based on the total weight of the solvent.
[0046]
[0047] Another aspect of the present invention is a steel plate;
[0048] A zinc alloy plating layer formed on at least one surface of the steel plate; and
[0049] It includes a surface treatment film layer formed on the above zinc alloy plating layer,
[0050] The above surface treatment film layer relates to a surface-treated zinc alloy plated steel sheet formed from the above surface treatment composition.
[0051] The above ternary zinc alloy plating layer may include an Al-concentrated layer formed at an interface, and the occupancy area ratio of the Al-concentrated layer may be 70% to 100%.
[0052] The above ternary zinc alloy plating layer may contain Al: 0.2 to 15 wt%, Mg: 0.5 to 3.5 wt%, the remainder Zn, and unavoidable impurities.
[0053] The above surface treatment film layer may have a thickness of 1 µm to 10 µm.
[0054]
[0055] Another aspect of the present invention comprises the steps of coating the surface treatment composition on a zinc alloy-plated steel sheet having a zinc alloy plating layer formed thereon; and
[0056] A step of drying the above surface treatment composition to form a surface treatment film layer.
[0057] It relates to a method for manufacturing a surface-treated zinc alloy plated steel sheet including .
[0058] The above surface treatment composition can be coated to a thickness of 2.5 ㎛ to 50 ㎛.
[0059] In the step of forming the surface treatment film layer, the surface treatment composition can be dried by raising the temperature to 70 to 250°C.
[0060]
[0061] By coating a surface treatment composition according to the present invention on a zinc alloy plated steel sheet to form a surface treatment film layer, a zinc alloy plated steel sheet having excellent corrosion resistance, fingerprint resistance, and contamination discoloration resistance can be provided.
[0062] In addition, the surface treatment composition according to the present invention does not contain any heavy metal components such as chromium, which are environmental pollutants, and therefore is harmless to the human body and does not cause problems due to environmental pollution.
[0063]
[0064] The various advantageous and beneficial advantages and effects of the present invention are not limited to the above-described contents, and will be more easily understood in the course of explaining specific embodiments of the present invention.
[0065]
[0066] The terminology used herein is for the purpose of describing the present invention and is not intended to limit the present invention. Furthermore, the singular forms used herein also include the plural forms, unless the context clearly dictates otherwise.
[0067] The meaning of "comprising" as used in the specification is to specify a configuration and not to exclude the presence or addition of other configurations.
[0068] Unless otherwise defined, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by a person of ordinary skill in the art to which this invention pertains. Terms defined in the dictionary are to be interpreted to have meanings consistent with the relevant technical literature and the present disclosure.
[0069]
[0070] The present invention relates to a surface treatment composition for a zinc alloy-plated steel sheet having excellent solution stability, excellent flat plate corrosion resistance, machined part corrosion resistance, and anti-fingerprint properties when applied to a ternary hot-dip zinc alloy-plated steel sheet, as a preferred example of a zinc alloy-plated steel sheet, and excellent contamination and discoloration resistance. In addition, the present invention relates to a zinc alloy-plated steel sheet surface-treated using the surface treatment composition and a method for manufacturing the same.
[0071]
[0072] First, a surface treatment composition, which is one embodiment of the present invention, will be described in detail.
[0073] The surface treatment composition is a surface treatment composition containing a solid content and a solvent, and the surface treatment composition may contain, based on 100 wt% of the solid content, 70 to 90 wt% of a resin mixture containing a high molecular weight polysilicon-modified polyurethane main resin, a low molecular weight polysilicon-modified polyurethane auxiliary resin, and an epoxy auxiliary resin; 5 to 25 wt% of a melamine-based curing agent; 0.5 to 10 wt% of an oxidation-discoloration inhibitor; 0.5 to 10 wt% of a silane compound; 0.5 to 10 wt% of a rust-preventive and corrosion-resistant agent; and 0.5 to 5 wt% of an anti-fingerprint improver.
[0074]
[0075] Below, the composition of each composition is described in detail.
[0076]
[0077] resin mixture
[0078] High molecular weight polysilicon-modified polyurethane resin is a component that can provide excellent corrosion resistance, water resistance, and solvent resistance to zinc alloy-plated steel sheets. The high molecular weight polysilicon-modified polyurethane resin is not limited thereto, but can be synthesized from silicone polymers and polycarbonate polyols, and has self-crosslinking characteristics due to the use of a three-dimensional (Trimer) isocyanate polymer during synthesis.
[0079] The weight average molecular weight (Mw) of the high molecular weight polysilicon-modified polyurethane main resin may be 100,000 to 200,000. If the weight average molecular weight is less than 100,000, it is difficult to secure sufficient corrosion resistance, whereas if the weight average molecular weight exceeds 200,000, the solution stability may be reduced and the hardness of the film may increase, which may cause problems such as reduced processability.
[0080] The glass transition temperature (Tg) of the high molecular weight polysilicon-modified polyurethane resin may be between -20°C and -10°C. If the glass transition temperature is lower than -20°C, it is difficult to secure sufficient corrosion resistance, whereas if the glass transition temperature exceeds -10°C, the solution stability may decrease and the hardness of the film may increase, resulting in problems such as reduced processability.
[0081] Low-molecular-weight polysilicon-modified polyurethane auxiliary resin is a component that can impart soft properties to zinc alloy-plated steel sheets and improve processability and adhesion. The low-molecular-weight polysilicon-modified polyurethane auxiliary resin is not limited thereto, but can be synthesized from silicone polymers and polycarbonate polyols. Unlike the high-molecular-weight polysilicon-modified polyurethane main resin, the low-molecular-weight polysilicon-modified polyurethane auxiliary resin does not have self-crosslinking properties.
[0082] The weight average molecular weight of the low molecular weight polysilicon modified polyurethane auxiliary resin may be 30,000 to 70,000. If the weight average molecular weight is less than 30,000, it is difficult to secure sufficient corrosion resistance due to a decrease in the density of the film, whereas if the weight average molecular weight exceeds 70,000, the effect of imparting soft properties to the film is insufficient, which may cause problems such as reduced processability and adhesion.
[0083] The glass transition temperature (Tg) of the low-molecular-weight polysilicon-modified polyurethane auxiliary resin may be between -30°C and -20°C. If the glass transition temperature is lower than -30°C, it is difficult to secure sufficient corrosion resistance due to a decrease in the density of the film, whereas if the glass transition temperature exceeds -20°C, the effect of imparting soft properties to the film may be insufficient, resulting in problems such as reduced processability and adhesion.
[0084] Epoxy auxiliary resin is a component that forms a dense film on zinc alloy-plated steel plates and improves flat plate corrosion resistance.
[0085] The epoxide equivalent ratio of the epoxy auxiliary resin may be 450 to 550 g / eq. If the epoxide equivalent ratio is less than 450 g / eq, the effect of improving the density and plate corrosion resistance of the film is not sufficient, whereas if the epoxide equivalent ratio exceeds 550 g / eq, the film may be excessively hard, resulting in a problem of reduced processability.
[0086] The weight average molecular weight (Mw) of the epoxy auxiliary resin may be 450 to 4,000. If the weight average molecular weight (Mw) is less than 450, the effect of improving the density and plate corrosion resistance of the film is not sufficient, whereas if the weight average molecular weight (Mw) exceeds 4,000, the hardness of the film may be excessive, which may cause a problem of reduced processability.
[0087] The resin mixture may be a mixture of a high molecular weight polysilicon-modified polyurethane main resin (A), a low molecular weight polysilicon-modified polyurethane auxiliary resin (B), and an epoxy auxiliary resin (C) in a weight ratio of 1:4.5:4.5 to 9:0.5:0.5, preferably 1:0.5:0.5 to 9:0.5:0.5, and more preferably 2:0.5:0.5 to 9:0.5:0.5. For example, A:B:C may be mixed and used in a weight ratio of 2:0.5:0.5, and more preferably 1:0.5:0.5.
[0088] If the content of the high molecular weight polysilicon-modified polyurethane resin in the resin mixture is too low, the flat plate corrosion resistance, machined area corrosion resistance, and alkali resistance of the steel plate may deteriorate. Conversely, if the content of the high molecular weight polysilicon-modified polyurethane resin in the resin mixture is too high, the machined area corrosion resistance and blackening resistance of the steel plate may deteriorate.
[0089] The content of the resin mixture may be 70 to 90 wt% based on 100 wt% of the solid content of the surface treatment composition. 70.0 to 90.0 wt% may be preferable. If the content of the resin mixture is less than 70 wt%, it is difficult to secure sufficient corrosion resistance and alkali resistance, and if the content of the resin mixture exceeds 90 wt%, the content of additives for improving physical properties in the surface treatment composition becomes relatively small, so corrosion resistance may actually decrease and solution stability may decrease.
[0090]
[0091] Melamine-based hardener
[0092] The above melamine-based curing agent is included to form a dense cross-linking bond by reacting with the main resin and the auxiliary resin of the surface treatment solution composition for zinc alloy-plated steel sheets to form a strong coating film. The melamine-based curing agent includes at least one functional group selected from among methoxymethyl, methylol, and imino functional groups, and the functional group is characterized in that it cross-links a backbone polymer resin containing a carboxyl group, and may be composed of at least one selected from the group consisting of, for example, methoxymethylmelamine, butoxymethylmelamine, ethoxymethylmelamine, and combinations thereof.
[0093] The melamine-based curing agent is preferably contained in an amount of 5 to 25 wt% based on 100 wt% of the solid content of the surface treatment composition. If the amount is less than 5 wt%, sufficient crosslinking cannot be formed, and thus improvement in physical properties cannot be expected. If the amount exceeds 25 wt%, excessive crosslinking may result in a decrease in the stability of the solution, causing solidification over time. The melamine-based curing agent is more preferably contained in an amount of 5.0 to 25.0 wt% based on 100 wt% of the solid content of the surface treatment composition.
[0094]
[0095] Antioxidant
[0096] The above-mentioned anti-oxidation and discoloration inhibitor is a component included to prevent discoloration of zinc alloy-plated steel sheets when they come into contact with contaminants in a high-temperature and humid environment. The anti-oxidation and discoloration inhibitor may be one or more compounds selected from the group consisting of ammonium molybdate and sodium molybdate.
[0097] The content of the oxidation-discoloration inhibitor may be 0.5 to 10 wt% based on 100 wt% of the solid content of the surface treatment composition. If the content of the oxidation-discoloration inhibitor is less than 0.5 wt%, sufficient oxidation-discoloration resistance cannot be expected to be secured, and if the content of the oxidation-discoloration inhibitor exceeds 10 wt%, the effect of improving oxidation-discoloration resistance is minimal, but the problem of reduced corrosion resistance may occur. The content of the oxidation-discoloration inhibitor is preferably 0.50 to 10.0 wt% based on 100 wt% of the solid content of the surface treatment composition.
[0098]
[0099] silane compounds
[0100] The above silane compound is included to perform a coupling reaction by modifying the water-soluble organic resin to form a strong bond between the water-soluble organic resin and the inorganic additive of the surface treatment composition.
[0101] The silane compound is preferably included in an amount of 0.5 to 10 wt% based on 100 wt% of the solid content of the surface treatment composition. If the amount of the silane compound is less than 0.5 wt%, the amount required for coupling the organic resin and the inorganic additive is insufficient, making it difficult to secure corrosion resistance. If the amount of the silane compound exceeds 10 wt%, unreacted silane compounds may remain after reaction with the organic resin, resulting in a problem of reduced corrosion resistance after processing. It is more preferable that the amount of the silane compound is 0.50 to 10.0 wt% based on 100 wt% of the solid content of the surface treatment composition.
[0102] The above silane hydrolysis compounds are vinylmethoxy silane, vinyltrimethoxy silane, vinylepoxy silane, vinyltriepoxy silane, methyltrimethoxysilane, tetraethylorthosilicate, tetramethylorthosilicate, 3-aminopropyltriepoxy silane, 3-glycidoxypropyltrimethoxy silane, 3-glycidoxypropyltriethoxy silane, 3-mercaptopropyltrimethoxy silane, N-(1,3 dimethylbutylidene)-3-(triepoxy silane)-1-propanamine, N,N-bis[3-(trimethoxysilyl)propyl]ethylenediamine, N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxy silane, It may include at least one selected from the group consisting of γ-mercaptopropyltriethoxysilane, and N-[2-(vinylbenzylamino) ethyl]-3-aminopropyltrimethoxysilane, and may be hydrolyzed by at least one solvent selected from the group consisting of formic acid, acetic acid, phosphoric acid, hydrochloric acid, and nitric acid.
[0103]
[0104] Anti-corrosion agent
[0105] The above-mentioned rust inhibitor is a component included to improve the corrosion resistance of zinc alloy-plated steel sheets, and may be at least one selected from the group consisting of a phosphoric acid-based rust inhibitor, a fluorine-based rust inhibitor, a vanadium-based rust inhibitor, a cerium salt-based rust inhibitor, and a selenium salt-based rust inhibitor.
[0106] The content of the rust prevention / corrosion agent may be 0.5 to 10 wt% based on 100 wt% of the solid content of the surface treatment composition. If the content of the rust prevention / corrosion agent is less than 0.5 wt%, it may be difficult to secure blackening resistance and alkali resistance, and if the content of the rust prevention / corrosion agent exceeds 10 wt%, it may be difficult to secure corrosion resistance. The content of the rust prevention / corrosion agent is preferably 0.50 to 10.0 wt% based on 100 wt% of the solid content of the surface treatment composition.
[0107]
[0108] Fingerprint-resistant enhancer
[0109] The above-mentioned anti-fingerprint improving agent may preferably be one or two or more selected from the group consisting of paraffin wax, olefin wax, carnauba wax, polyester wax, polypropylene wax, polyethylene-Teflon wax, and polyTeflon wax.
[0110] The content of the anti-fingerprint improver may be 0.5 to 5 wt% based on 100 wt% of the solid content of the surface treatment composition. If the content of the anti-fingerprint improver is less than 0.5 wt%, it may be difficult to secure sufficient anti-fingerprint properties, and if the content of the anti-fingerprint improver exceeds 5 wt%, it may be difficult to secure corrosion resistance. It is preferable that the content of the anti-fingerprint improver is 0.50 to 5.0 wt% based on 100 wt% of the solid content of the surface treatment composition.
[0111]
[0112] menstruum
[0113] The surface treatment composition above contains water as a solvent to dilute each component, and the water may be deionized water or distilled water. The solvent is included as a remainder in addition to each component of the present invention, and its content may be 60 to 80 wt%. Furthermore, the surface treatment composition according to one embodiment may further contain N-ethyl-2-pyrrolidone (NEP, N-Ethyl-2-pyrrolidone) as an auxiliary solvent to ensure solution stability, and the N-ethyl-2-pyrrolidone may be included in an amount of 20 to 40 wt% of the total solvent.
[0114] A zinc alloy-plated steel sheet surface-treated with a surface treatment composition containing a water-soluble organic resin, an anti-oxidation and discoloration agent, and a corrosion-resistant inorganic compound according to one embodiment of the present invention not only exhibits excellent corrosion resistance and staining and discoloration resistance, but also has excellent surface color and gloss. In addition, the surface treatment composition according to one embodiment of the present invention does not contain hexavalent chromium, a hazardous environmental substance, and contains a water-soluble organic resin and an inorganic compound that are harmless to the human body as main components, thereby having the effect of preventing damage to the human body and environmental pollution.
[0115]
[0116] According to one embodiment of the present invention, a zinc alloy plated steel sheet surface-treated with the above-described surface treatment composition is provided.
[0117] Specifically, the surface-treated zinc alloy-plated steel sheet may include a steel sheet, a zinc alloy plating layer formed on at least one surface of the steel sheet, and a surface-treated film layer formed on the zinc alloy plating layer.
[0118]
[0119] An example of the zinc alloy plating layer may be a ternary molten zinc alloy plating layer, and a specific example may be a plating layer containing Al: 0.2 to 15 wt%, Mg: 0.5 to 3.5 wt%, the remainder Zn, and unavoidable impurities.
[0120] In the above ternary zinc alloy-coated steel sheet, Mg plays a very important role in improving the corrosion resistance of the ternary zinc alloy-coated steel sheet, and effectively prevents corrosion of the ternary zinc alloy-coated steel sheet by forming a dense zinc hydroxide-based corrosion product on the surface of the plating layer under a corrosive environment. In order to secure the corrosion resistance effect targeted in the present invention, the plating layer should contain Mg in an amount of 0.5 wt% or more, and more preferably, 0.9 wt% or more. However, if the content is excessive, Mg oxidizing dross rapidly forms on the surface of the plating bath, thereby offsetting the anti-oxidation effect of the trace element addition. In order to prevent this, Mg should be contained in the plating layer in an amount of 3.5 wt% or less, and more preferably, 3.2 wt% or less.
[0121] Meanwhile, in ternary zinc alloy-coated steel sheets, Al suppresses the formation of Mg oxide dross in the plating bath and reacts with Zn and Mg in the plating bath to form Zn-Al-Mg intermetallic compounds, thereby improving the corrosion resistance of the plating steel sheet. To achieve the above effect, the plating layer should contain at least 0.2 wt% of Al, and more preferably, at least 0.9 wt%. However, if the content is excessive, the weldability and phosphate treatability of the plating steel may deteriorate. To prevent this, Al should be contained in the plating layer at no more than 15 wt%, and more preferably, at no more than 12 wt%.
[0122]
[0123] The above ternary zinc alloy-coated steel sheet includes an Al-enriched layer formed at the interface between the steel sheet and the ternary zinc alloy plating layer, and the occupancy area ratio of the Al-enriched layer may be 70% to 100%, more preferably, 73% to 100%. Here, the occupancy area ratio means the ratio of the area of the Al-enriched layer to the area of the base steel when projected in the thickness direction of the base steel from the surface of the plated steel sheet and assumed to be a plane without considering three-dimensional curvature, etc. When the occupancy area ratio of the Al-enriched layer is secured to be 70% or more, the Al-enriched layer has a form in which fine particles are continuously formed, so that the plating property and plating adhesion can be significantly improved.
[0124]
[0125] The surface treatment film formed on the zinc alloy plating layer can be formed from a surface treatment composition comprising, based on 100 wt% of the solid content of the composition, 70 to 90 wt% of a resin mixture including a high molecular weight polysilicon-modified polyurethane main resin, a low molecular weight polysilicon-modified polyurethane auxiliary resin, and an epoxy auxiliary resin; 5 to 25 wt% of a melamine-based curing agent; 0.5 to 10 wt% of an oxidation-discoloration inhibitor; 0.5 to 10 wt% of a silane compound; 0.5 to 10 wt% of a rust-preventive and corrosion-resistant agent; and 0.5 to 5 wt% of an anti-fingerprint improver. Since the surface treatment composition has the same technical characteristics as those described above, they will not be described again.
[0126] The above surface treatment film layer is a coating layer formed by drying the above-described surface treatment composition, and corresponds to the remaining components after all volatile substances contained in the surface treatment film layer containing the organic resin and the inorganic compound have volatilized. Therefore, the surface treatment film layer containing the organic resin and the inorganic compound does not contain water or N-ethyl-2-pyrrolidone as a solvent, and also does not contain the solvent contained in the surface treatment component containing the organic resin and the inorganic compound. Therefore, the components contained in the surface treatment film layer containing the organic resin and the inorganic compound correspond to the content based on 100 wt% of the total solid content.
[0127]
[0128] According to one embodiment of the present invention, a method for manufacturing a zinc alloy plated steel sheet surface-treated with the above-described surface treatment composition is provided.
[0129] The above manufacturing method includes a step of coating the above-described surface treatment composition on a zinc alloy-plated steel sheet having a molten zinc alloy plating layer formed thereon; and a step of drying the surface treatment composition to form a surface treatment film layer.
[0130]
[0131] The surface treatment composition may be coated with a thickness of 2.5 to 50 μm. In addition, the coated surface treatment composition forms a dry film layer through a drying process, and the thickness of the dry film layer may be 1 to 10 μm. If the coating thickness of the surface treatment composition is less than 2.5 μm, the surface treatment composition may be applied too thinly on the acid portion of the steel plate roughness, which may cause a problem of reduced corrosion resistance. If the thickness exceeds 50 μm, the film layer may be formed too thickly, which may cause deterioration in processability and may cause a problem of economic feasibility due to an increase in solution treatment costs.
[0132] The method for coating the surface treatment composition is not particularly limited as long as it is a commonly performed coating method, but it is preferable to perform the coating using any one coating method selected from, for example, roll coating, spraying, dipping, spray squeezing, and dipping squeezing.
[0133]
[0134] The process of drying the surface treatment composition coated on the zinc alloy-plated steel sheet is preferably performed at a temperature of 70 to 250°C based on the final temperature reached (PMT) of the steel sheet. If the drying temperature is lower than 70°C based on the final temperature reached (PMT) of the steel sheet, the curing reaction of the organic resin may not be completely accomplished, resulting in a failure to form a solid film structure and poor corrosion resistance and alkali resistance. On the other hand, if the drying temperature exceeds 250°C based on the final temperature reached (PMT) of the steel sheet, work productivity may deteriorate due to the generation of water vapor and fumes during the water cooling process, and the surface quality of the product may deteriorate due to condensation, in which the evaporated water vapor condenses on the upper part of the drying equipment.
[0135] Meanwhile, the drying process is preferably performed in a hot air drying furnace or an induction heating furnace. When drying the surface treatment composition using a hot air drying furnace, the internal temperature of the hot air drying furnace is preferably 100 to 300°C. When drying the surface treatment composition using an induction heating furnace, the current applied to the induction heating furnace is preferably 1000 to 5000A, and more preferably 1500 to 3500A. If the internal temperature of the hot air drying furnace is less than 100°C or the current applied to the induction heating furnace is less than 1000A, the curing reaction of the surface treatment composition may not be completely performed, resulting in poor corrosion resistance and alkali resistance. In addition, if the internal temperature of the hot air drying furnace exceeds 300°C or the current applied to the induction heating furnace exceeds 5000A, work productivity may deteriorate due to the generation of water vapor and fume during the water cooling process, and the surface quality of the product may deteriorate due to the condensation phenomenon in which the evaporated water vapor condenses on the upper part of the drying equipment.
[0136]
[0137] In addition, after drying the surface treatment composition to form a surface treatment film layer, the surface treatment film layer can be cooled with water to finally provide a surface-treated zinc alloy plated steel sheet.
[0138]
[0139] A method for manufacturing a zinc alloy-plated steel sheet according to one embodiment of the present invention may be performed as a continuous process, and the speed of the continuous process is preferably 80 to 120 mpm. If the speed of the continuous process is less than 80 mpm, a problem of reduced productivity may occur, and if it exceeds 120 mpm, the solution may fly during the drying process of the surface treatment composition, causing surface defects.
[0140]
[0141] Hereinafter, embodiments of the present invention will be described. It should be understood that those skilled in the art will appreciate that various modifications to the following embodiments can be made without departing from the scope of the present invention. The following embodiments are intended to facilitate understanding of the present invention, and the scope of the present invention should not be limited to the following embodiments, but should be determined not only by the claims set forth below but also by their equivalents.
[0142]
[0143] (Example)
[0144]
[0145] Fabrication of test specimens
[0146] As a zinc alloy-coated steel sheet, the ternary zinc alloy plating layer is composed of Mg: 1.5%, Al: 1.5%, and the balance Zn in weight %. The ternary zinc alloy-coated steel sheet (coating amount 0.5 to 2.0 g / m on one side) 2 ) was cut into a size of 7 cm x 15 cm (width x length) and the oil was removed, and each manufactured composition was applied to a hot-dip zinc alloy plated steel plate using a bar coater. Then, the composition was cured under the condition of PMT (Peak Metal Temperature) 180±20℃ to produce a test specimen.
[0147]
[0148] Testing and Evaluation Methods
[0149] In this example, the method and criteria for evaluating the properties of the surface-treated steel plate are as follows.
[0150] <Reputational Corrosion Resistance>
[0151] The rate of white rust development on steel plates over time was measured after specimen treatment according to the method specified in ASTM B117. The evaluation criteria were as follows.
[0152] ◎: The time until white rust occurs is 144 hours or more
[0153] ○: The time until white rust occurs is 96 hours or more but less than 144 hours.
[0154] △: The time until white rust occurs is 55 hours or more but less than 96 hours.
[0155] ×: Time taken for white rust to occur is less than 55 hours
[0156] <Corrosion resistance of processing part>
[0157] The specimen was pushed up to a height of 6 mm using an Erichsen tester, and the degree of white rust formation was measured after 24 hours. The evaluation criteria were as follows.
[0158] ◎: Less than 5% of the area affected by white rust after 48 hours
[0159] ○: After 48 hours, the area of white rust occurrence is 5% or more but less than 7%
[0160] ×: After 48 hours, white rust occurs in 7% or more of the area
[0161] <Oxidation discoloration resistance>
[0162] 0.05 ml of artificial sweat was dropped on the surface of the specimen at 5 points at intervals of approximately 10 mm, and left in a constant temperature and humidity chamber at 65°C and 90-95% humidity for 48 hours. After waiting at room temperature for 2 hours, the surface was washed with tap water and evaluated by observing the surface with an eye. The artificial sweat solution was made by dissolving 8 g of sodium phosphate, 8 g of sodium chloride, and 5 g of acetic acid in distilled water to a pH of approximately 4.5 (finely adjusted with sodium hydroxide) and making 1 liter.
[0163] At this time, the evaluation criteria are as follows.
[0164] ◎: Excellent, no surface discoloration
[0165] ○: Good, minor surface marks
[0166] △: Normal, light gray surface discoloration
[0167] ×: Defective, surface blackening and discoloration
[0168] <Alkaline resistance>
[0169] The specimens were immersed in an alkaline degreasing solution at 60°C for 2 minutes, rinsed with water, and air-blown. The color difference (ΔE) before and after the degreasing was measured. The alkaline degreasing solution used was Finecleaner L 4460 A: 20g / 2.4L + L 4460 B 12g / 2.4L (pH=12) from Daehan Parkerizing Co., Ltd. The evaluation criteria were as follows.
[0170] ◎: ΔE ≤ 2
[0171] ○: 2 < ΔE ≤ 3
[0172] △: 3 < ΔE ≤ 4
[0173] Х: ΔE > 4
[0174] <Fingerprint>
[0175] After applying a thin layer of Vaseline evenly to the surface of the specimen, the area was blotted with gauze. The color difference (ΔE) before and after the application of Vaseline was measured. The evaluation criteria were as follows.
[0176] ◎: ΔE ≤ 2
[0177] ○: 2 < ΔE ≤ 3
[0178] △: 3 < ΔE ≤ 4
[0179] Х: ΔE > 4
[0180] <Solution stability>
[0181] The surface treatment composition was placed in a container and stored in a constant temperature oven at 50°C for 7 days. After that, the formation of sediment was visually observed and changes in viscosity were measured. The evaluation criteria were as follows.
[0182] ○: No sedimentation, viscosity change less than 1 cP
[0183] △: No sedimentation, viscosity change of 1 cP or more and less than 5 cP
[0184] ×: Sedimentation occurs, or viscosity change is 5 cP or more
[0185] <Gloss>
[0186] The gloss of the specimen was measured at an angle of incidence of 60° using a gloss meter. The evaluation criteria were as follows.
[0187] ○: Good, gloss value 80 or higher
[0188] ×: Defective, gloss value less than 80
[0189]
[0190] Components of surface treatment composition
[0191] The components of the surface treatment composition used in this example are as follows.
[0192] The components of the surface treatment composition used in the examples are as follows.
[0193] resin mixture
[0194] - High molecular weight polysilicon-modified polyurethane resin (A): Polyurethane resin with a weight average molecular weight of 150,000
[0195] - Low molecular weight polysilicon modified polyurethane auxiliary resin (auxiliary resin 1, B): polyurethane resin with a weight average molecular weight of 50,000.
[0196] - Epoxy auxiliary resin (auxiliary resin 2, C): Epoxy resin with an equivalence ratio of 500 g / eq and a weight average molecular weight of 2,000.
[0197] Melamine-based hardener: ethoxymethylmelamine
[0198] Antioxidant: Ammonium molybdate
[0199] Silane compound: 3-aminopropyltriepoxy silane
[0200] Rust and corrosion inhibitor: Fluorine-based rust inhibitor
[0201] Anti-fingerprint enhancer: polyethylene-Teflon wax
[0202] Solvent: Mixed solvent of water and N-ethyl-2-pyrrolidone (NEP)
[0203]
[0204] Example 1: Changes in physical properties according to the content of the resin mixture
[0205] A surface treatment composition was prepared by mixing a resin mixture in which the above-described main resin, auxiliary resin 1, and auxiliary resin 2 were mixed in a weight ratio of 1:0.5:0.5, a curing agent, an anti-oxidation discoloration agent, a silane compound, an anti-corrosion agent, and an anti-fingerprint improver in the contents shown in Table 1. The surface treatment composition includes a mixed solvent of 49 wt% of water and 21 wt% of N-ethyl-2-pyrrolidone (70 wt% based on the total weight of the composition).
[0206] The solution stability of the surface treatment composition prepared above was evaluated. Furthermore, the surface treatment composition was applied to the test specimens described above, and the specimens' plate corrosion resistance, machined area corrosion resistance, oxidation blackening resistance, and alkali resistance were evaluated. The evaluation results are shown in Table 1 below.
[0207]
[0208] Classification Composition Composition (weight %) Plate corrosion resistance Processing part corrosion resistance Oxidation discoloration resistance Alkaline solution stability Resin mixture Melanin type hardener Oxidation discoloration inhibitor Silane compound Anti-corrosion agent Anti-fingerprint property enhancer Comparative example 167 10 10 10 2 1 XX ○ X ○ Invention example 17 0 9 9.5 1 0 10.5 ○ ○ ○ ○ ○ ○ Invention example 28 0 5 5.5 8 10.5 ◎ ○ ○ ○ ○ ○ Invention example 39 0 5 2 1.5 10.5 ◎ ○ ...
[0209] * The composition content is based on 30 wt% solid content, see Table 1 above.
[0210] Referring to Table 1 above, Inventive Examples 1 to 3, in which the content of the resin mixture satisfies the content proposed by the present invention, showed results rated as good (○) or higher in all physical properties. However, Comparative Example 1, which contained too little resin mixture, showed poor results in plate corrosion resistance, machined part corrosion resistance, and alkali resistance, and Comparative Example 2, which contained too much resin mixture, showed poor results in plate corrosion resistance, machined part corrosion resistance, blackening resistance, and solution stability.
[0211]
[0212] Example 2: Changes in physical properties according to the content ratio of the main resin and auxiliary resin.
[0213] A surface treatment composition was prepared, comprising 80 wt% of a resin mixture including the above-described main resin (A), auxiliary resin 1 (B), and auxiliary resin 2 (C), 5 wt% of a curing agent, 5.5 wt% of an oxidation-discoloration inhibitor, 8 wt% of a silane compound, 1 wt% of a rust-preventive and corrosion-resistant agent, and 0.5 wt% of an anti-fingerprint improver. The surface treatment composition comprises a mixed solvent of 49 wt% of water and 21 wt% of N-ethyl-2-pyrrolidone (70 wt% based on the total weight of the composition).
[0214] In the above resin mixture, the main resin, auxiliary resin 1, and auxiliary resin 2 were mixed in the weight ratios described in Table 2 below.
[0215] After applying the above surface treatment composition to the test specimen described above, the flat plate corrosion resistance, machined part corrosion resistance, oxidation blackening resistance, and alkali resistance of the specimen were evaluated, and the evaluation results are shown in Table 2 below.
[0216]
[0217] Classification Weight ratio (A:B:C) Plate corrosion resistance Processing corrosion resistance Oxidation discoloration resistance Alkali resistance Main resin (A) Auxiliary resin 1 (B) Auxiliary resin 2 (C) Invention example 4547.547.5○○○○ Invention example 5104545○◎○○ Invention example 6502525◎◎◎◎ Invention example 76716.516.5◎◎◎◎ Invention example 89055◎◎◎◎ Invention example 9952.52.5○○○○
[0218] * The composition content is based on 30% by weight of solids
[0219] Referring to Table 2, Invention Examples 4 to 9 showed results of good (○) or higher in all physical properties. However, in the case of Invention Examples 5 to 9, where the weight ratio of the main resin and the auxiliary resin satisfied the content ratio preferably proposed by the present invention, better effects were confirmed in terms of plate corrosion resistance, processed part corrosion resistance, oxidation resistance, and alkali resistance.
[0220]
[0221] Example 3: Changes in physical properties according to curing agent content
[0222] A surface treatment composition was prepared by mixing a resin mixture in which the above-described main resin, auxiliary resin 1, and auxiliary resin 2 were mixed in a weight ratio of 1:0.5:0.5, a curing agent, an anti-oxidation discoloration agent, a silane compound, an anti-corrosion agent, and an anti-fingerprint improver in the contents shown in Table 3. The surface treatment composition includes a mixed solvent of 49 wt% of water and 21 wt% of N-ethyl-2-pyrrolidone (70 wt% based on the total weight of the composition).
[0223] The solution stability of the surface treatment composition prepared above was evaluated. Furthermore, the surface treatment composition was applied to the test specimens described above, and the specimens' plate corrosion resistance, machined area corrosion resistance, oxidation discoloration resistance, and alkali resistance were evaluated. The evaluation results are shown in Table 3 below.
[0224]
[0225] Classification Composition Composition (weight %) Plate corrosion resistance Processing area corrosion resistance Oxidation discoloration resistance Alkaline solution stability Hardener Resin mixture Oxidation discoloration inhibitor Silane compound Anti-rust Anti-corrosion agent Anti-fingerprint property Improver Comparative example 34845511XXXX○ Invention example 105845411○○○○○ Invention example 1115745411◎◎◎◎○ Invention example 1225702111◎◎○◎○ Comparative example 426701111○○○XX
[0226] * The composition content is based on 30% by weight of solids
[0227] Referring to Table 3 above, Inventive Examples 10 to 12, in which the content of the melamine-based curing agent satisfies the content proposed by the present invention, showed results of good (○) or higher in all physical properties. On the other hand, when too little melamine-based curing agent was added (Comparative Example 3), poor results were shown in all physical properties except solution stability, and when too much melamine-based curing agent was added (Comparative Example 4), poor results were shown in alkali resistance and solution stability.
[0228]
[0229] Example 4: Changes in physical properties according to the content of antioxidant
[0230] A surface treatment composition was prepared by mixing a resin mixture in which the above-described main resin, auxiliary resin 1, and auxiliary resin 2 were mixed in a weight ratio of 1:0.5:0.5, a curing agent, an anti-oxidation discoloration agent, a silane compound, an anti-corrosion agent, and an anti-fingerprint improver in the contents shown in Table 4. The surface treatment composition includes a mixed solvent of 49 wt% of water and 21 wt% of N-ethyl-2-pyrrolidone (70 wt% based on the total weight of the composition).
[0231] The solution stability of the surface treatment composition prepared above was evaluated. Furthermore, the surface treatment composition was applied to the test specimens described above, and the specimens' plate corrosion resistance, machined area corrosion resistance, oxidation discoloration resistance, and alkali resistance were evaluated. The evaluation results are shown in Table 4 below.
[0232]
[0233] Classification Composition Composition (weight %) Plate corrosion resistance Processing part corrosion resistance Oxidation Discoloration resistance Alkaline stability Solution stability Oxidation Discoloration inhibitor Resin mixture Hardener Silane compound Anti-rust Anti-corrosion agent Anti-fingerprint Improver Comparative example 50.382.28810.5○○XX○ Invention example 130.5828810.5○○○○○ Invention example 14577.58810.5◎◎◎◎○ Invention example 151072.58810.5◎◎◎◎○ Comparative example 61272.57710.5XX◎◎X
[0234] * The composition content is based on 30% by weight of solids
[0235] Referring to Table 4 above, Inventive Examples 13 to 15, in which the content of the antioxidant satisfying the content proposed by the present invention, showed results of good (○) or higher in all physical properties. On the other hand, Comparative Example 5, which contained too little antioxidant, showed poor results in oxidation discoloration resistance and alkali resistance, and Comparative Example 6, which contained too much antioxidant, showed poor results in plate corrosion resistance, machined part corrosion resistance, and solution stability.
[0236]
[0237] Example 5: Changes in physical properties according to silane compound content
[0238] A surface treatment composition was prepared by mixing a resin mixture in which the above-described main resin, auxiliary resin 1, and auxiliary resin 2 were mixed in a weight ratio of 1:0.5:0.5, a curing agent, an anti-oxidation discoloration agent, a silane compound, an anti-corrosion agent, and an anti-fingerprint improver in the contents shown in Table 5. The surface treatment composition includes a mixed solvent of 49 wt% of water and 21 wt% of N-ethyl-2-pyrrolidone (70 wt% based on the total weight of the composition).
[0239] The solution stability of the surface treatment composition prepared above was evaluated. Furthermore, the surface treatment composition was applied to the test specimens described above, and the specimens' plate corrosion resistance, machined area corrosion resistance, oxidation discoloration resistance, and alkali resistance were evaluated. The evaluation results are shown in Table 4 below.
[0240]
[0241] Classification Composition Composition (weight %) Plate corrosion resistance Processing part corrosion resistance Oxidation discoloration resistance Alkaline solution stability Silane compound Resin mixture Hardener Oxidation discoloration inhibitor Rust prevention Anti-corrosion agent Fingerprint improvement agent Comparative example 70.382.285.52.51.5 XXX○○ Invention example 160.58285.52.51.5 ○◎○○○ Invention example 17577.585.52.51.5◎◎◎◎○ Invention example 181072.585.52.51.5◎◎◎◎○ Comparative example 81272.5752.51○XX○○
[0242] * The composition content is based on 30% by weight of solids
[0243] Referring to Table 5 above, when the content of the silane compound satisfies the content proposed by the present invention (Invention Examples 16 to 18), all physical properties showed results better than good.
[0244] On the other hand, when too little silane compound is added (Comparative Example 7), the plate corrosion resistance, post-processing corrosion resistance, and oxidation discoloration resistance are poor, and when too much is added (Comparative Example 8), the dryness of the film increases, forming a hard film, resulting in poor corrosion resistance of the processed area and poor oxidation discoloration resistance.
[0245]
[0246] The surface treatment solution composition according to the above invention example 17 was used, but the type of silane hydrolysis compound was a silane coupling agent as described in Table 6 below. As described above, a specimen was manufactured using the composition using the silane coupling agent as described in Table 6 below, and the plate corrosion resistance was evaluated, and the results are described in Table 6.
[0247]
[0248] Classification abcdefghijk plate corrosion resistance content content content content content content content content content invention example 19500000000000 ○ invention example 2005000000000◎ invention example 2100500000000○ invention example 2200050000000◎ invention example 2300005000000○ invention example 2400000500000◎ invention example 2500000050000○ invention example 26000000 05000○Invention Example 2700000000500○Invention Example 2800000000050◎Invention Example 2900000000005○Invention Example 302.52.500000000○Invention Example 312.5002.50000000○Invention Example 3202.50002.50000◎Invention Example 330002.502.500000○Invention Example 3400002.502.50000○Invention Example 3500 0002.50002.50◎Invention Example 36002.5002.500000○Invention Example 370000002.5002.50○Invention Example 382.5000000002.50○Invention Example 390000000002.52.5○Invention Example 400002.500002.500○Invention Example 4100002.5002.5000○Invention Example 4200000002.5002.5○Invention Example 4302. 52.500000000◎Invention Example 4402200000001○Invention Example 4500010020200○Invention Example 4600002100200○Invention Example 470203.50010002○Invention Example 4802000000012◎Invention Example 492020000001○Invention Example 5001000000220○Invention Example 5102001000020○Invention Example 5200000022001○a: 2-(3,4-epoxycyclohexyl)-ethyltrimethoxysilane g: N-2-(aminoethyl)-3-aminopropyl triethoxysilane b: 3-glycidoxypropyl trimethoxysilane h: 3-aminopropyl trimethoxy silane c: 3-glycidoxypropyl methyldiethoxysilane i: 3-aminopropyl triethoxy silane d: 3-glycidoxypropyl triethoxysilane j: vinyltriepoxy silane e: N-2-(aminoethyl)-3-aminopropyl methyldimethoxysilane k: methyltrimethoxy silane f: N-2-(aminoethyl)-3-aminopropyl trimethoxysilane
[0249] As shown in Table 6 above, Invention Examples 19 to 52 showed good or excellent flat plate corrosion resistance results. In particular, the test specimen treated with the surface treatment solution composition prepared according to the composition of Invention Example 48 showed the best result, with a white rust area of 0% after 144 hours or more.
[0250]
[0251] Example 6: Changes in physical properties according to the content of anti-corrosion agent
[0252] A surface treatment composition was prepared by mixing a resin mixture in which the above-described main resin, auxiliary resin 1, and auxiliary resin 2 were mixed in a weight ratio of 1:0.5:0.5, a curing agent, an anti-oxidation discoloration agent, a silane compound, an anti-corrosion agent, and an anti-fingerprint improver in the contents shown in Table 7. The surface treatment composition includes a mixed solvent of 49 wt% of water and 21 wt% of N-ethyl-2-pyrrolidone (70 wt% based on the total weight of the composition).
[0253] The solution stability of the surface treatment composition prepared above was evaluated. Furthermore, the surface treatment composition was applied to the test specimens described above, and the specimens' plate corrosion resistance, machined area corrosion resistance, oxidation discoloration resistance, and alkali resistance were evaluated. The evaluation results are shown in Table 7 below.
[0254]
[0255] Classification Composition Composition (weight %) Plate corrosion resistance Processing part corrosion resistance Oxidation discoloration resistance Alkaline stability Solution stability Anti-rust Anti-corrosion agent Resin mixture Hardener Oxidation discoloration inhibitor Silane compound Anti-fingerprint enhancer Comparative example 90.382.28180.5XX○○○ Invention example 530.5828180.5○◎○○○ Invention example 54577.58180.5◎◎◎◎○ Invention example 551072.58180.5◎◎◎◎○ Comparative example 101272.57170.5○○XX○
[0256] * The composition content is based on 30% by weight of solids
[0257] Referring to Table 7 above, Inventive Examples 53 to 55, in which the content of the rust-preventive agent satisfies the content proposed by the present invention, showed results of good (○) or higher in all physical properties. However, Comparative Example 9, which contained too little rust-preventive agent, showed poor results in plate corrosion resistance and machined part corrosion resistance, and Comparative Example 10, which contained too much rust-preventive agent, showed poor results in oxidation discoloration resistance and alkali resistance.
[0258]
[0259] Example 7: Changes in physical properties according to the content of anti-fingerprint enhancer
[0260] A surface treatment composition was prepared by mixing a resin mixture in which the above-described main resin, auxiliary resin 1, and auxiliary resin 2 were mixed in a weight ratio of 1:0.5:0.5, a curing agent, an anti-oxidation discoloration agent, a silane compound, an anti-corrosion agent, and an anti-fingerprint improver in the contents shown in Table 8. The surface treatment composition includes a mixed solvent of 49 wt% of water and 21 wt% of N-ethyl-2-pyrrolidone (70 wt% based on the total weight of the composition).
[0261] The solution stability of the surface treatment composition prepared above was evaluated. In addition, after applying the surface treatment composition to the test specimens described above, the specimens were evaluated for flat plate corrosion resistance, machined area corrosion resistance, oxidation discoloration resistance, alkali resistance, and fingerprint resistance. The evaluation results are shown in Table 8 below.
[0262]
[0263] Classification Composition Composition (weight %) Plate corrosion resistance Processing area corrosion resistance Oxidation discoloration resistance Alkali resistance Fingerprint resistance Solution stability Fingerprint resistance Improver Resin mixture Hardener Oxidation discoloration inhibitor Silane compound Anti-rust Anti-corrosion agent Comparative example 110.382.264.552○◎○○X○ Invention example 560.58264.552○◎○○○○ Invention example 57280.564.552◎◎◎◎◎○ Invention example 58580.55.5351◎◎◎◎◎○ Comparative example 126805351XX◎○◎X
[0264] * The composition content is based on 30% by weight of solids
[0265] Referring to Table 8 above, inventive examples 56 to 58, in which the content of the anti-fingerprint improving agent satisfies the content proposed by the present invention, results were good (○) or higher in all physical properties. However, comparative example 11, which contained too little anti-fingerprint improving agent, showed poor anti-fingerprint results, and comparative example 12, which contained too much anti-fingerprint improving agent, showed poor flat plate corrosion resistance, machined area corrosion resistance, and solution stability.
[0266]
[0267] Example 8: Changes in physical properties according to film thickness and drying temperature
[0268] The surface treatment composition according to Invention Example 2 was bar-coated on a test specimen and dried in a hot air dryer. The plate corrosion resistance, machined area corrosion resistance, blackening resistance, and alkali resistance of the specimen were evaluated while controlling the thickness of the film layer and the PMT temperature as described in Table 9 below.
[0269]
[0270] Thickness of the film layer (㎛) Drying temperature (℃) Plate corrosion resistance Processing corrosion resistance Blackening resistance Alkali resistance Comparative example 130.5180△X△△Invention example 591180◎◎◎◎Invention example 604180◎◎◎◎Invention example 617180◎◎○◎Invention example 6210180◎◎○◎Comparative example 1411180◎X○◎Comparative example 15550XXXXInvention example 63570○○○△Invention example 645100◎◎◎◎Invention example 655250◎◎○◎Comparative example 165270◎◎X◎
[0271]
[0272] As shown in Table 9 above, inventive examples 59 to 65, in which a film layer having a thickness of 1 to 10 μm was formed, all physical properties showed results of good (○) or higher. On the other hand, comparative example 13, in which the film formed was excessively thin, showed average (β) results in plate corrosion resistance, blackening resistance, and alkali resistance, and poor results in corrosion resistance at the machined part. On the other hand, comparative example 14, in which an excessively thick film was formed, showed poor results in corrosion resistance at the machined part, and since no physical properties were improved compared to inventive example 62, a film thickness exceeding 10 μm is not required from an economical perspective.
[0273] Meanwhile, as shown in Table 9 above, inventive examples 62 to 65, in which a film layer was formed by drying the film at 70 to 250°C, showed results of good (○) or higher in all physical properties. On the other hand, comparative example 15, in which the drying temperature was excessively low, showed poor results in all physical properties because the film was not sufficiently dried. Meanwhile, comparative example 16, in which the drying temperature was excessively high, showed poor blackening resistance due to fume drops on the steel plate caused by condensation of water vapor generated on the steel plate during the air cooling process (water cooling).
Claims
1. A surface treatment composition comprising a solid component and a solvent, The above surface treatment composition, based on 100 wt% of solid content, 70 to 90 wt% of a resin mixture comprising a high molecular weight polysilicon-modified polyurethane main resin, a low molecular weight polysilicon-modified polyurethane auxiliary resin, and an epoxy auxiliary resin; 5 to 25 wt% of melamine-based curing agent; 0.5 to 10 wt% of anti-oxidation and discoloration agent; 0.5 to 10 wt% of silane compound; 0.5 to 10 wt% of anti-corrosion agent; and 0.5 to 5 wt% of anti-fingerprint improving agent; A surface treatment composition comprising:
2. In claim 1, A surface treatment composition in which the high molecular weight polysilicon-modified polyurethane main resin (A), the low molecular weight polysilicon-modified polyurethane auxiliary resin (B), and the epoxy auxiliary resin (C) are mixed in a weight ratio of 1:4.5:4.5 to 9:0.5:0.
5.
3. In claim 1, The above high molecular weight polysilicon modified polyurethane main resin (A) is a surface treatment composition having a glass transition temperature (Tg) of -20°C to -10°C and a weight average molecular weight (Mw) of 100,000 to 200,000.
4. In claim 1, The above low molecular weight polysilicon modified polyurethane auxiliary resin (B) is a surface treatment composition having a glass transition temperature (Tg) of -30°C to -20°C and a weight average molecular weight (Mw) of 30,000 to 70,000.
5. In claim 1, The above epoxy auxiliary resin (C) is a surface treatment composition having an epoxide equivalent ratio of 450 to 550 g / eq and a weight average molecular weight (Mw) of 450 to 4,000.
6. In claim 1, A surface treatment composition wherein the melamine-based curing agent comprises at least one functional group selected from the group consisting of methoxy methyl, methylol, and imino functional groups, and the functional group crosslinks a skeletal polymer resin containing a carboxyl group.
7. In claim 1, A surface treatment composition comprising at least one selected from the group consisting of the above-mentioned oxidation and discoloration inhibitors ammonium molybdate and sodium molybdate.
8. In claim 1, The above silane compounds are vinylmethoxy silane, vinyltrimethoxy silane, vinylepoxy silane, vinyltriepoxy silane, methyltrimethoxysilane, tetraethylorthosilicate, tetramethylorthosilicate, 3-aminopropyltriepoxy silane, 3-glycidoxypropyltrimethoxy silane, 3-glycidoxypropyltriethoxy silane, 3-mercaptopropyltrimethoxy silane, N-(1,3 dimethylbutylidene)-3-(triepoxy silane)-1-propanamine, N,N-bis[3-(trimethoxysilyl)propyl]ethylenediamine, N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxy silane, A surface treatment composition comprising at least one selected from the group consisting of γ-mercaptopropyltriethoxysilane and N-[2-(vinylbenzylamino) ethyl]-3-aminopropyltrimethoxysilane.
9. In claim 1, A surface treatment composition wherein the above silane compound is hydrolyzed by at least one acid selected from the group consisting of formic acid, acetic acid, phosphoric acid, hydrochloric acid, and nitric acid.
10. In claim 1, A surface treatment composition in which the above-mentioned rust inhibitor is at least one selected from the group consisting of a phosphoric acid rust inhibitor, a fluorine rust inhibitor, a vanadium rust inhibitor, a cerium salt rust inhibitor, and a selenium salt rust inhibitor.
11. In claim 1, A surface treatment composition in which the above-mentioned anti-fingerprint improving agent is at least one selected from the group consisting of paraffin wax, olefin wax, carnauba wax, polyester wax, polypropylene wax, polyethylene-Teflon wax, and polyTeflon wax.
12. In claim 1, A surface treatment composition characterized in that the solid content is 20 to 40 wt% based on the total weight of the surface treatment composition, and the remainder is a solvent.
13. In claim 12, The above solvent is a surface treatment composition containing 20 to 40 wt% of N-ethyl-2-pyrrolidone (NEP) and the remainder water based on the total weight of the solvent.
14. Steel plate; A ternary molten zinc alloy plating layer formed on at least one surface of the steel plate; and It includes a surface treatment film layer formed on the above ternary molten zinc alloy plating layer, A surface-treated ternary zinc alloy-plated steel sheet, wherein the surface-treated film layer is formed from a surface-treated composition according to any one of claims 1 to 13.
15. In claim 14, The above ternary molten zinc alloy plating layer includes an Al concentrated layer formed at the interface, A ternary zinc alloy-coated steel sheet having an area ratio of 70% to 100% of the above Al-concentrated layer.
16. In claim 14, A ternary zinc alloy plating steel sheet comprising the ternary zinc alloy plating layer comprising Al: 0.2 to 15 wt%, Mg: 0.5 to 3.5 wt%, the remainder Zn, and unavoidable impurities.
17. In claim 14, The above surface treatment film layer is a ternary zinc alloy plated steel sheet having a thickness of 1 ㎛ to 10 ㎛.
18. A step of coating a surface treatment composition of any one of claims 1 to 13 on a ternary zinc alloy-plated steel sheet having a ternary zinc alloy plating layer formed thereon; and A step of drying the above surface treatment composition to form a surface treatment film layer. A method for manufacturing a surface-treated ternary zinc alloy-plated steel sheet including:
19. In claim 18, A method for manufacturing a ternary zinc alloy plated steel sheet by coating the surface treatment composition in a thickness of 2.5 ㎛ to 50 ㎛.
20. In claim 18, A method for manufacturing a ternary zinc alloy plated steel sheet, wherein the surface treatment composition is dried by raising the temperature to 70 to 250°C in the step of forming the surface treatment film layer.