Resin-coated metal sheet and production method therefor

MYPI2025002926A0Undetermined Publication Date: 2024-06-20JFE STEEL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025002926
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-12-20
Filing Date
2023-12-14
Publication Date
2024-06-20

AI Technical Summary

Technical Problem

Resin-coated metal plates used in container manufacturing face issues with moldability and ink adhesion due to the addition of lubricating components, which can lead to resin layer breakage, peeling, and reduced corrosion and weather resistance, as well as impaired design and beauty from ink peeling.

Method used

A resin-coated metal plate with a polyester resin layer having a specific melting point range, a polyolefin lubricating component with controlled exposure and acid value, and an intermediate layer with inorganic particles, combined with a manufacturing method involving masterbatch pellets and biaxial stretching, to enhance adhesion and ink adhesion while maintaining moldability.

Benefits of technology

The solution provides improved moldability and ink adhesion, reducing resin layer breakage and peeling, while maintaining excellent adhesion to the metal plate and ink, thus enhancing the durability and appearance of the coated metal plates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025002926_DRAWING_001
    Figure PI2025002926_DRAWING_001
  • Figure PI2025002926_DRAWING_002
    Figure PI2025002926_DRAWING_002
  • Figure PI2025002926_DRAWING_003
    Figure PI2025002926_DRAWING_003
Patent Text Reader

Abstract

Provided is a resin-coated metal sheet and a production method therefor. The resin-coated metal sheet includes: a metal sheet layer 2; and a resin layer 3 containing a polyester resin and coating a sheet surface of the metal sheet layer 2, in which the resin layer 3 has a melting point of 225 °C to 255 °C and includes: a surface layer 31 located on a surface opposite to a side facing the metal sheet layer 2; a lower layer 33 facing the metal sheet layer 2; and an intermediate layer 32 between the surface layer 31 and the lower layer 33, the surface layer 31 contains a lubricating component composed of a polyolefin having a melting point of 75 °C to 140 °C, and a coverage ratio of the lubricating component exposed on a surface of the layer 31 is 0.040 % to 0.80 %.
Need to check novelty before this filing date? Find Prior Art

Description

Resin-coated metal sheet and its manufacturing method

[0001] The present invention relates to a resin-coated metal sheet and a method for producing the same.

[0002] As described in Patent Document 1, metal plates such as tin-free steel (TFS) and aluminum used as materials for metal containers are coated with paint to improve corrosion resistance and weather resistance. This coating method has the problem of requiring a significant amount of processing time for the coating and baking processes. Furthermore, it is problematic in terms of environmental impact due to the large amount of solvent discharged. To solve these problems, laminated steel sheets, in which a thermoplastic resin film is coated on the surface of a metal plate to form a resin layer, are increasingly used. Laminated steel sheets are widely used, for example, in the fields of beverage cans and food cans, which require high levels of forming processing. The resin layer located on the outer surface of the container may be printed to improve design.

[0003] In recent years, from the viewpoint of resource conservation and material cost reduction, materials used for metal containers, particularly metal plates and resin layers, have been made thinner. As a result, the degree of processing during can manufacturing has increased, and there is a possibility that the resin layer on the outer surface of the container may break or be chipped, especially after molding. Therefore, in order to suppress breakage or chipping of the resin layer during can manufacturing, a lubricating component may be added to the resin layer (see, for example, Patent Document 1).

[0004] Patent Document 1 discloses a resin-coated metal sheet for containers. This resin-coated metal sheet for containers has resin coating layers on both sides of a metal sheet. In this resin-coated metal sheet for containers, the resin coating layer located on the outer surface of the container after molding is mainly composed of a polyester resin having a melting point in the range of 230°C to 254°C and also contains a lubricating component, the melting point of which is 80°C to 230°C, and the average particle size of the lubricating component present on the surface of the resin coating layer is 17.0 nm or less.

[0005] Patent Document 1 also discloses that a drawing method or a DI (draw and iron) method may be used to process resin-coated metal sheets for containers. It also discloses that a white pigment may be added to the resin coating layer located on the outer surface of the container after molding, in order to improve the design and aesthetics of the can body after printing.

[0006] International Publication No. 2019 / 116706

[0007] Adding a lubricating component to a resin layer coating a metal sheet can suppress breakage and abrasion of the resin layer, ensuring good formability. However, the lubricating component can reduce adhesion between the resin layer and the metal sheet, which can cause the resin layer to peel off from the metal sheet during can manufacturing. Such peeling is problematic because it can lead to molding defects during can manufacturing and subsequent deterioration of corrosion resistance and weather resistance. Furthermore, the lubricating component can reduce the adhesion of printing ink to the resin layer, causing ink peeling during can manufacturing. Ink peeling is problematic because it impairs the design and aesthetic appeal of the can body appearance. Therefore, it is desirable to provide a resin-coated metal sheet with excellent formability and adhesion of the resin layer and excellent ink adhesion.

[0008] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a resin-coated metal sheet having excellent formability and adhesion of the resin layer and excellent ink adhesion, and a method for producing the same.

[0009] In order to achieve the above object, the resin-coated metal sheet according to the present invention is as follows.

[0010] [1] A resin-coated metal sheet comprises: a metal sheet layer; and a resin layer containing a polyester resin that coats the sheet surface of the metal sheet layer, wherein the resin layer has a melting point of 225°C or higher and 255°C or lower, and comprises a surface layer disposed on the surface opposite to the side facing the metal sheet layer, a lower layer facing the metal sheet layer, and an intermediate layer between the surface layer and the lower layer, wherein the surface layer contains a lubricating component made of polyolefin having a melting point of 75°C or higher and 140°C or lower, and the coverage of the lubricating component exposed on the surface of the surface layer is 0.040% or higher and 0.80% or lower, as determined by peak intensity ratio analysis of Raman spectrum data obtained when Raman measurement is performed on the surface layer using a confocal Raman device.

[0011] The resin-coated metal sheet according to the present invention may further be as follows.

[0012] [2] The resin-coated metal sheet according to the above [1], wherein the resin layer is formed from a resin material containing 90 mol% or more of ethylene terephthalate units.

[0013] [3] The resin-coated metal sheet according to the above [1] or [2], wherein the surface layer contains the lubricating component in an amount of 0.10 mass % or more and 1.0 mass % or less.

[0014] [4] The resin-coated metal sheet according to any one of [1] to [3] above, wherein the lubricating component includes an acid-modified polyolefin or an oxidized polyolefin.

[0015] [5] The resin-coated metal sheet according to [4] above, wherein the lubricating component has an acid value of 1.0 mgKOH / g or more and 80 mgKOH / g or less.

[0016] [6] The resin-coated metal sheet according to any one of the above [1] to [5], wherein the intermediate layer contains 10% by mass or more and 30% by mass or less of inorganic particles.

[0017] [7] The resin-coated metal sheet according to any one of [1] to [6], wherein the surface layer has a thickness of 1.0 μm or more and 5.0 μm or less, the intermediate layer has a thickness of 6.0 μm or more and 30 μm or less, and the lower layer has a thickness of 1.0 μm or more and 5.0 μm or less.

[0018] The resin-coated metal sheet according to any one of the above [1] to [7] can be produced by the following production method.

[0019] [8] A method for producing a resin-coated metal sheet, comprising: preparing masterbatch pellets in which the lubricating component is dispersed using a polyester resin having a melting point of 230°C or higher and 254°C or lower and an intrinsic viscosity of 0.45 or higher and 0.88 or lower as a base; kneading the masterbatch pellets and the polyester resin pellets, extruding the mixture at a predetermined extrusion temperature, and stretching the mixture by a biaxial stretching method to form a film; and thermocompression bonding the film to a metal sheet using a laminating roll.

[0020] [9] The method for producing a resin-coated metal sheet according to the above [8], wherein the predetermined extrusion temperature is 255°C or higher and 285°C or lower.

[0021]

[10] The method for producing a resin-coated metal sheet according to the above [8] or [9], wherein the stretching ratio of the film is 2.0 times or more and 5.0 times or less.

[0022] According to the present invention, it is possible to provide a resin-coated metal sheet having excellent formability and adhesion of the resin layer and excellent ink adhesion, and a method for producing the same.

[0023] 1 is a cross-sectional view illustrating the structure of a resin-coated metal sheet according to one embodiment of the present invention; FIG. 2 is a cross-sectional view illustrating the structure of a resin-coated metal sheet according to another embodiment of the present invention; and FIG. 3 is a cross-sectional view illustrating the structure of a resin-coated metal sheet according to another embodiment of the present invention.

[0024] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS A resin-coated metal sheet according to an embodiment of the present invention and a method for manufacturing the same will be described with reference to the drawings.

[0025] FIG. 1 shows a cross-sectional view of a resin-coated metal sheet 100 (hereinafter referred to as sheet material 100) according to this embodiment.

[0026] An overview of the plate material 100 will be described. The plate material 100 includes a metal plate layer 2 and a resin layer 3 containing a polyester resin that coats the plate surface of the metal plate layer 2. The resin layer 3 includes a surface layer 31 disposed on the surface opposite the side facing the metal plate layer 2, a lower layer 33 facing the metal plate layer 2, and an intermediate layer 32 positioned between the surface layer 31 and the lower layer 33. The melting point of the resin layer 3 is 225°C or higher and 255°C or lower. The surface layer 31 contains a lubricating component made of polyolefin having a melting point of 75°C or higher and 140°C or lower. The coverage of the lubricating component exposed on the surface of the surface layer 31 is 0.040% or higher and 0.80% or lower. This coverage is determined by peak intensity ratio analysis of Raman spectrum data obtained when Raman measurement is performed on the surface layer 31 using a confocal Raman spectrometer.

[0027] 1 shows a case where the plate material 100 further includes a resin layer 4. The plate material 100 will be described in detail below.

[0028] The metal plate layer 2 is a layer of a metal plate. The metal plate layer 2 is, for example, a steel plate such as tinplate or TFS. For tinplate, the plating amount is 0.5 g / m. 2 15g / m or more 2 It is preferable to use TFS with a metal chromium deposition amount of 50 mg / m 2 More than 200g / m 2 The metallic chromium layer has a chromium oxide coating amount of 3 mg / m2 as metallic chromium. 2 30g / m or more 2 It is preferable that the steel sheet has a chromium oxide layer on its surface as described below. The steel sheet may have a plating or chromium oxide layer on both sides, only one side, or only a portion thereof. When the steel sheet has a plating or chromium oxide layer on only a portion, such as one side, it is preferable to provide a resin layer 3 on at least the surface portion of the steel sheet where no plating or chromium oxide layer is present.

[0029] When a steel plate is used as the metal plate layer 2, the type of steel plate is not particularly limited as long as it can be formed into the desired shape, but steel plates having the following components and manufactured by the following manufacturing method are preferred.

[0030] It is preferable that the steel sheet is made of low carbon steel having a C content (carbon content) in the range of about 0.010 mass % to 0.10 mass %, and is recrystallized by continuous annealing.

[0031] Furthermore, it is preferable that the steel sheet is made of low carbon steel having a C content in the range of about 0.010 mass % to 0.10 mass %, and is subjected to recrystallization annealing and overaging treatment by continuous annealing.

[0032] It is also preferable that the steel be made of low carbon steel having a C content in the range of about 0.010 mass % to 0.10 mass %, and that the steel be recrystallized by box annealing.

[0033] It is also preferable that the steel sheet is made of low carbon steel having a C content in the range of about 0.010 mass % to 0.10 mass %, and is subjected to recrystallization annealing by continuous annealing or box annealing, followed by secondary cold rolling.

[0034] It is also preferable to use IF (Interstitial Free) steel, which is ultra-low carbon steel having a C content of about 0.003 mass % or less and to which elements such as Nb and Ti that fix the dissolved C are added, and which is recrystallized by continuous annealing.

[0035] The mechanical properties of the steel sheet are not particularly limited as long as they can be formed into the desired shape. Regarding the mechanical properties of the steel sheet, in order to maintain sufficient can body strength without impairing formability, it is preferable to use a steel sheet having a yield point (YP) in the range of approximately 220 MPa to 580 MPa. Furthermore, the Lankford value (r value), which is an index of plastic anisotropy, is preferably 0.8 or more. Furthermore, it is preferable that the absolute value of the in-plane anisotropy Δr of the r value is 0.7 or less.

[0036] Regarding the steel sheet, the steel components required to satisfy the above mechanical properties are not particularly limited, but may contain, for example, components such as Si, Mn, P, S, Al, and N. The Si content is preferably 0.001% by mass to 0.1% by mass, the Mn content is 0.01% by mass to 0.6% by mass, the P content is 0.002% by mass to 0.05% by mass, the S content is 0.002% by mass to 0.05% by mass, the Al content is 0.005% by mass to 0.100% by mass, and the N content is 0.0005% by mass to 0.020% by mass. Other components such as Ti, Nb, B, Cu, Ni, Cr, Mo, and V may also be contained, but from the viewpoint of ensuring corrosion resistance, the total content of these components is preferably 0.02% by mass or less.

[0037] As described above, the resin layer 3 has the surface layer 31, the intermediate layer 32, and the lower layer 33. In this embodiment, when the surface layer 31 is the outermost layer, the lower layer 33 is the lowermost layer in the resin layer 3.

[0038] The resin layer 3 has a melting point of 225°C or higher and 255°C or lower, and contains a polyester resin as a main component. Preferably, the melting point of the resin layer 3 is 232°C or higher and 252°C or lower. More preferably, the melting point of the resin layer 3 is 238°C or higher and 250°C or lower. If the melting point of the resin layer 3 is lower than 225°C, the resin softens due to heat applied to the resin during molding, causing breakage or scraping of the resin layer 3 and reducing moldability. On the other hand, if the melting point of the resin layer 3 exceeds 255°C, the crystallinity of the polyester resin increases, making the resin layer 3 more likely to break or scrape during molding, reducing moldability.

[0039] Various dicarboxylic acid components and glycol components may be used as raw materials for the polyester resin. Furthermore, multiple dicarboxylic acid components and glycol components may be copolymerized as long as heat resistance and processability are not impaired. Examples of dicarboxylic acid components include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, diphenyldicarboxylic acid, diphenylsulfonedicarboxylic acid, diphenoxyethanedicarboxylic acid, 5-sodium sulfoisophthalic acid, and phthalic acid; aliphatic dicarboxylic acids such as oxalic acid, succinic acid, adipic acid, sebacic acid, dimer acid, maleic acid, and fumaric acid; alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid; and oxycarboxylic acids such as p-oxybenzoic acid. Examples of glycol components include aliphatic glycols such as ethylene glycol, propanediol, butanediol, pentanediol, hexanediol, and neopentyl glycol; alicyclic glycols such as cyclohexanedimethanol; aromatic glycols such as bisphenol A and bisphenol S; and diethylene glycol.

[0040] In order to ensure excellent sliding properties and abrasion resistance during can body molding during can manufacturing, it is sufficient that a lubricating component be added to at least the surface layer 31, which is the outermost layer, of the three layers constituting the resin layer 3. When forming the resin layer 3, the surface layer 31 and the lower layer 33 may be formed from resins extruded using a single extruder. In this case, the surface layer 31 and the lower layer 33 have the same composition, and not only the surface layer 31, which is the outermost layer, but also the lower layer 33, which is the lowermost layer, contains a lubricating component. Of course, the surface layer 31 and the lower layer 33 may be formed from resins of the same or different compositions extruded using two separate extruders.

[0041] The lubricating component is a polyolefin with a melting point of 75°C or higher and 140°C or lower, due to its excellent film-forming and dispersibility properties. To ensure sufficient affinity with the polyester resin, the main component of the resin layer 3, the polyolefin preferably has a polar group. Examples of polyolefins having polar groups include acid-modified polyolefins such as ethylene-maleic anhydride copolymers, oxidized polyolefins such as polyethylene oxide, and ethylene-acrylic acid copolymers. These can be used alone or in combination. The affinity between the lubricating component and the resin layer 3 varies depending on the acid value of the polyolefin constituting the lubricating component. For example, the higher the acid value of the polyolefin constituting the lubricating component, the higher the affinity between the lubricating component and the resin layer 3. As the affinity increases, the dispersed particle size of the lubricating component on the surface of the resin layer 3 decreases, and the coverage of the lubricating component, as determined by peak intensity ratio analysis of Raman spectrum data, tends to decrease.

[0042] The melting point of the lubricating component is preferably 90°C or higher and 130°C or lower, more preferably 100°C or higher and 120°C or lower. If the melting point of the lubricating component is lower than 75°C, the lubricating component is likely to concentrate on the surface of the resin layer 3 due to the heat treatment performed during the process of coating the resin layer 3 on the metal plate layer 2 and during the molding of the resin-coated metal plate. Furthermore, much of the lubricating component is likely to melt due to the heat during processing. Therefore, the resin layer 3 may be scraped during processing in a mold, potentially reducing moldability. Furthermore, the low affinity between the lubricating component and the printing ink may impair the adhesion of the printing ink, potentially resulting in peeling of the printing ink during molding. Furthermore, if the melting point of the lubricating component exceeds 140°C, sufficient slip properties and abrasion resistance may not be ensured, and the resin layer 3 may break or be scraped during molding, potentially reducing moldability.

[0043] The coverage of the lubricating component exposed on the outermost surface of the resin layer 3, i.e., the surface of the surface layer 31 (hereinafter also simply referred to as "coverage") is 0.040% or more and 0.80% or less, preferably 0.060% or more and 0.70% or less, more preferably 0.070% or more and 0.65% or less, and even more preferably 0.080% or more and 0.50% or less.

[0044] The coverage is determined by peak intensity ratio analysis (hereinafter also simply referred to as "this measurement method") of Raman spectrum data obtained when Raman measurement is performed on the surface layer 31 using a confocal Raman device. This measurement method makes it possible to calculate the dispersion state of the lubricating component nondestructively and with high resolution, and to capture even minute lubricating components on the surface of the surface layer 31 that cannot be captured by other analytical methods.

[0045] Although there is a method for evaluating the hydrophilic and hydrophobic states of the surface of the surface layer 31 by measuring the contact angle using water or the like, contact angle measurement is also significantly affected by surface roughness, making it difficult to capture the influence of the lubricating component alone. On the other hand, Raman measurement is not affected by surface roughness and can capture the dispersion state of the lubricating component, making it possible to evaluate the influence of the lubricating component on the surface of the surface layer 31 with higher accuracy.

[0046] If the coverage of the lubricating component exposed on the outermost surface of the resin layer 3 is very small, such as less than 0.040%, it will be impossible to ensure sufficient slip properties and abrasion resistance to withstand processing during can manufacturing, which could result in breakage or abrasion during molding, and reduced formability. Also, if the coverage of the lubricating component exposed on the outermost surface of the resin layer 3 is excessive, exceeding 0.80%, the lubricating component could inhibit the adhesion of printing ink, potentially causing peeling of the printing ink during molding.

[0047] The coverage is affected by the content and dispersion state or dispersibility of the lubricating component in the surface layer 31. Therefore, in order to improve the dispersion state of the lubricating component in the surface layer 31, it is preferable to use a masterbatch when forming the film that constitutes the surface layer 31 or the resin layer 3.

[0048] The masterbatch is a polyester resin having a high concentration of a lubricating component dispersed therein. The melting point of the polyester resin serving as the base of the masterbatch is preferably 230°C or higher and 254°C or lower, more preferably 234°C or higher and 252°C or lower, and even more preferably 238°C or higher and 250°C or lower.

[0049] The intrinsic viscosity of the polyester resin that is the base of the masterbatch is preferably 0.45 or more and 0.88 or less, more preferably 0.50 or more and 0.85 or less, and even more preferably 0.55 or more and 0.80 or less.

[0050] As described above, the melting point of the lubricating component used in the masterbatch is 75°C or higher and 140°C or lower, preferably 90°C or higher and 130°C or lower, and more preferably 100°C or higher and 120°C or lower.

[0051] The acid value of the lubricating component used in the masterbatch is preferably 1.0 mgKOH / g or more and 80 mgKOH / g or less. It is more preferably 1.0 mgKOH / g or more and 60 mgKOH / g or less, and even more preferably 2.0 mgKOH / g or more and 45 mgKOH / g or less. By controlling the melting point and intrinsic viscosity of the polyester resin and the melting point and acid value of the lubricating component within the above ranges, it is possible to control the coverage of the lubricating component exposed on the outermost surface of the resin layer 3 (i.e., the surface of the outer layer 31) to 0.040% or more and 0.80% or less. Furthermore, by controlling the coverage rather than the content of the lubricating component, it is possible to provide a resin-coated metal sheet having excellent moldability and ink adhesion of the resin layer 3.

[0052] The resin layer 3 is preferably formed from a resin material containing 90 mol% or more of ethylene terephthalate units. The content of ethylene terephthalate units in the resin material is more preferably 92 mol% or more, and even more preferably 95 mol% or more. When the ethylene terephthalate unit content is 90 mol% or more, the melting point of the resin layer 3 is sufficiently high. This suppresses thermal degradation of the resin material during the process of coating the metal plate layer 2 with the resin layer 3 and the heat treatment performed during molding of the resin-coated metal plate, improving the formability of the resin layer 3. As long as the resin layer 3 as a whole satisfies the above-mentioned ethylene terephthalate unit content, the surface layer 31, the intermediate layer 32, and the lower layer 33 may be formed from polyester resin materials of the same composition or polyester resin materials of different compositions.

[0053] The lubricating component content of the surface layer 31 of the resin layer 3 is preferably 0.10% by mass or more and 1.0% by mass or less. More preferably, it is 0.20% by mass or more and 0.90% by mass or less, and even more preferably, it is 0.40% by mass or more and 0.80% by mass or less. When the lubricating component content is within the above range, the coverage of the lubricating component exposed on the surface of the surface layer 31 falls within an appropriate range, ensuring sufficient slip properties and abrasion resistance during molding, and preventing breakage or abrasion of the resin layer 3. Furthermore, sufficient ink adhesion is ensured, preventing ink peeling during molding. The lower layer 33 may optionally contain a lubricating component content within the above range, similar to the surface layer 31. When the lubricating component content is within the above range, sufficient adhesion between the lower layer 33 and the metal plate layer 2 can be ensured, making peeling of the resin layer 3 less likely to occur during molding. The intermediate layer 32 may contain a lubricating component content within the above range, but preferably does not contain a lubricating component from a cost perspective.

[0054] The acid value of the lubricating component is preferably 1.0 mgKOH / g or more and 80 mgKOH / g or less, more preferably 1.0 mgKOH / g or more and 60 mgKOH / g or less, and even more preferably 2.0 mgKOH / g or more and 45 mgKOH / g or less. When the acid value of the lubricating component is within the above range, affinity with the resin layer 3 and the printing ink can be sufficiently ensured, and adhesion of the printing ink can be improved. Furthermore, since the lubricating component is not compatible with the polyester resin that forms the resin layer 3 and softening and deterioration of the resin layer 3 can be suppressed, sufficient slip properties and abrasion resistance can be ensured during molding, and the resin layer 3 does not break or chip, resulting in good moldability.

[0055] The resin layer 3 may be required to be white to enhance the design and aesthetic appeal of the can body appearance after printing. To achieve a white resin layer 3, the intermediate layer 32 preferably contains 10% to 30% by mass of inorganic particles. The content of inorganic particles in the intermediate layer 32 is more preferably 10% to 25% by mass, and even more preferably 15% to 20% by mass. When the content of inorganic particles in the intermediate layer 32 is within the above range, the resin layer 3 can ensure sufficient whiteness and hiding power. Furthermore, the resin layer 3 is less likely to break or chip during can forming, resulting in good moldability. The content of inorganic particles is the amount relative to 100% by mass of the resin composition (including the polyester resin material and inorganic particles) used to form the intermediate layer 32.

[0056] The inorganic particles contained in the intermediate layer 32 are not particularly limited, but may be rutile-type titanium oxide (TiO 2 When the inorganic particles are titanium oxide as specified above, the titanium oxide exhibits good dispersibility when mixed with the resin material, resulting in a uniform whiteness and improved design and aesthetic appeal of the appearance.

[0057] The resin layer 3 is not limited to a three-layer structure, and may have a laminated structure of four or more layers, as long as it has a surface layer 31, a lower layer 33, and an intermediate layer 32. By configuring at least one of the three layers (for example, the intermediate layer 32) with two or more layers, the resin layer 3 can have a laminated structure of four or more layers. As an example of a case where the resin layer 3 has a three-layer structure of the surface layer 31, the intermediate layer 32, and the lower layer 33, the layer thicknesses (film thicknesses) of the surface layer 31, the intermediate layer 32, and the lower layer 33 are as follows:

[0058] The thickness of the surface layer 31 is preferably 1.0 μm to 5.0 μm, more preferably 1.5 μm to 4.0 μm, and even more preferably 2.0 μm to 3.0 μm. When the thickness of the surface layer 31 is within the above range, sufficient slip properties and abrasion resistance can be ensured during molding, and the resin layer 3 is less likely to break or be abraded, resulting in good moldability. In addition, sufficient whiteness can be ensured, improving the design and beauty of the appearance.

[0059] The thickness of the lower layer 33 is preferably 1.0 μm or more and 5.0 μm or less, more preferably 1.5 μm or more and 4.0 μm or less, and even more preferably 2.0 μm or more and 3.0 μm or less. When the thickness of the lower layer 33 is within the above range, the overall thickness of the resin layer 3 falls within an appropriate range, thereby ensuring sufficient abrasion resistance during molding. Furthermore, when the lower layer 33 contains a lubricating component, the absolute amount of the lubricating component dispersed to the surface of the metal plate layer 2 falls within an appropriate range, thereby improving the adhesion between the resin layer 3 and the metal plate layer 2.

[0060] The thickness of the intermediate layer 32 is preferably 6.0 μm or more and 30 μm or less, more preferably 8.0 μm or more and 25 μm or less, and even more preferably 10 μm or more and 20 μm or less. When the thickness of the intermediate layer 32 is within the above range, there is no need to vary the thicknesses of the surface layer 31 and the lower layer 33, and fluctuations in the absolute amount of the lubricating component are suppressed. Therefore, the coverage rate of the lubricating component tends to fall within an appropriate range, peeling, breaking, or scraping of the resin layer 3 does not occur during molding, and the adhesion of printing ink to the resin layer 3 can be improved.

[0061] The film for forming the resin layer 3 can be manufactured using general laminate film manufacturing techniques, such as coextrusion or film lamination. From the viewpoint of simplifying the manufacturing process, it is preferable to manufacture the film by coextrusion. Manufacturing the film by coextrusion can be performed, for example, as follows: Using a multilayer die, resin compositions for each layer are coextruded from extruders for each layer to produce an unstretched laminate film, which is then stretched to form a film. Film formation is preferably performed by biaxially stretching the unstretched laminate film once in the film-forming direction and then once in a direction perpendicular to the film-forming direction. When the surface layer 31 and the lower layer 33 have the same composition, the unstretched laminate film may be manufactured by coextruding the respective resin compositions from an extruder for the intermediate layer 32 and an extruder for the surface layer 31 and the lower layer 33.

[0062] The method for incorporating the lubricating component into the surface layer 31 is not particularly limited, but as an example, it may be added as follows. As described above, a masterbatch (masterbatch pellets) is first prepared using a kneading extruder, in which the lubricating component is dispersed at a high concentration in a polyester resin. Then, when forming the above-mentioned film, the polyester resin pellets, which are the main component of the resin layer 3, are kneaded with the masterbatch, and the resulting resin composition is introduced into an extruder for the surface layer 31 and extruded at a predetermined extrusion temperature to form the surface layer 31. The same applies when incorporating the lubricating component into the lower layer 33. Note that the predetermined extrusion temperature is preferably adjusted to 255°C or higher and 285°C or lower, which is 30°C higher than the melting point of the resin pellets.

[0063] In order to improve the dispersion state of the lubricating component in the layer containing the lubricating component in the resin layer 3, at least in the surface layer 31, it is preferable to adjust the extrusion temperature to a higher temperature within the above temperature range.

[0064] In addition, in order to improve the dispersion state of the lubricating component in the layer, the stretching ratio after producing the unstretched laminated film is preferably 2.0 times or more and 5.0 times or less in both the longitudinal direction and the width direction, and more preferably 3.0 times or more and 4.5 times or less.

[0065] In addition, in order to improve the dispersion state of the lubricating component in the layer, the temperature of the kneading extrusion and the screw rotation speed of the extruder during the preparation of the masterbatch may be adjusted.

[0066] The metal plate layer 2 may be covered with a film to be the resin layer 3 (laminating the film onto the metal plate layer 2) by thermocompression bonding the film to the metal plate layer 2 using a laminating roll.

[0067] The resin layer 4 is a layer formed on the surface of the plate material 100 opposite to the resin layer 3. The resin layer 4 is, for example, a layer containing a polyester resin. The resin layer 4 is not essential for the plate material 100, and as shown in FIG. 2, the plate material 100 may not include the resin layer 4. The resin layer 4 may be a single layer as shown in FIG. 1, or may be formed as a multilayer of two or more layers. In the plate material 100, the resin layer 4 does not need to be a layer having a structure different from that of the resin layer 3, and as shown in FIG. 3, the resin layer 3 may be formed on both sides of the plate material 100. That is, the plate material 100 may include the resin layer 3 (see FIG. 3) as the resin layer 4 (see FIG. 1).

[0068] Resin-coated metal sheets according to Examples 1 to 28 and Comparative Examples 1 to 8 were produced as follows.

[0069] The metal plate layer has a thickness of 0.22 mm and a metal chromium layer of 120 mg / m 2 , the chromium oxide layer is 10 mg / m in terms of metallic chromium 2 A TFS with a temper of T3CA was prepared.

[0070] Next, a three-layer resin layer having a surface layer, an intermediate layer, and a lower layer was formed as follows using the formulations and conditions shown in Tables 1 to 3. First, a film for the resin layer was produced using the formulations shown in Tables 1 to 3, with the extrusion temperature during kneading of the resin pellets and masterbatch at 275°C. The film was stretched by biaxial stretching, stretching 4.0 times in both the longitudinal and transverse directions. The metal plate was then heated, and the film was thermocompressed to the metal plate using a laminating roll. After 1.5 seconds had elapsed since thermocompression bonding, the film was water-cooled in a water-cooled tank to produce a resin-coated metal plate in which both sides of the metal plate were coated with a resin layer. Table 1 shows the formulations and production conditions for the resin-coated metal plates of Examples 1 to 13, and Table 2 shows the formulations and production conditions for the resin-coated metal plates of Examples 14 to 24. Table 3 shows the formulations and production conditions for the resin-coated metal plates of Examples 25 to 28 and Comparative Examples 1 to 8. In Tables 1 to 3, descriptions such as "Ethylene terephthalate 90, ethylene isophthalate 10" (quoting the case of Example 1) in the column "Resin composition [mol %]" mean that the content of ethylene terephthalate units in the resin material forming the resin layer is 90 mol %, and the content of ethylene isophthalate units is 10 mol %.

[0071]

[0072]

[0073]

[0074] For the resin-coated metal sheets of the examples and comparative examples, the melting point of the resin layer, the melting point of the lubricating component, the coverage of the lubricating component exposed on the outermost surface (surface) of the resin layer, the resin composition of the resin layer, the acid value of the lubricating component, and the film thickness of the resin layer were measured using the methods described below.

[0075] (1) Melting Point of Resin Layer The melting point of the resin layer was determined as follows. First, a resin-coated metal plate was immersed in a mixed solution of concentrated hydrochloric acid (30 wt%) and distilled water (1:1) at room temperature (20°C), dissolving the metal plate and peeling off the resin layer. Then, a differential scanning calorimeter (DSCQ100) manufactured by TA Instruments was used to measure the melting point of the resin layer in a N atmosphere. 2The peeled resin layer was measured under the conditions of a flow rate of 50 ml / min, a temperature range of room temperature to 290°C, and a heating rate of 10°C / min. From the obtained heat flow, the peak top temperature of the endothermic peak in the range of 200°C to 280°C was taken as the melting point.

[0076] (2) Melting Point of Lubricating Component The melting point of the lubricating component was determined as follows. The resin layer was peeled off from the resin-coated metal plate as described in (1) above, and the resin layer was dissolved using hexafluoro-2-propanol as a solvent. The solution was centrifuged and then pressure-filtered through filters with pore sizes of 1 μm and 0.1 μm in order to extract the lubricating components contained in the surface layer and the lower layer. Furthermore, the filter was subjected to Soxhlet extraction using xylene as a solvent, and additional lubricating components were extracted by concentration, reprecipitation, and centrifugation. The lubricating components extracted as described above were measured using a differential scanning calorimeter: DSCQ100 manufactured by TA Instruments under conditions of N ambient gas. 2 The measurement was carried out under the conditions of a flow rate of 50 ml / min, a temperature range of room temperature to 290°C, and a heating rate of 10°C / min. The peak top temperature of the endothermic peak in the range of 50°C to 170°C of the obtained heat flow was taken as the melting point.

[0077] (3) Coverage of lubricating component The coverage of the lubricating component exposed on the outermost surface (surface) of the resin layer was determined as follows. Raman measurement was performed on the outermost surface of the resin-coated metal sheet using a micro-Raman analyzer: LabRAM HR VIS-NIR manufactured by Horiba, Ltd. The measurement conditions were a confocal laser with a laser wavelength of 532 nm, laser power of 10%, aperture of 25 μm, exposure time of 0.08 sec, number of exposures of 1, grating of 300 lines / mm, objective lens of 100x magnification, and wavenumber range of 310 cm -1 From 3400 cm -1 The measurement range was 50 μm (lamination direction of the resin-coated metal sheet) × 50 μm (direction perpendicular to the lamination direction within the sheet surface of the resin-coated metal sheet). The measurement pitch was 0.5 μm in both the lamination direction and the direction perpendicular to the lamination direction within the sheet surface.

[0078] From the Raman spectrum data obtained by the above measurement, a CH stretching vibration peak (2850 cm ) derived from polyethylene, which is the main component of the lubricating component, was observed. -1 ) and a CH stretching vibration peak (2960 cm ) derived from polyester, the main component of the resin layer. -1 The intensity ratio of the resin-coated metal sheet to the surface of the resin-coated metal sheet was calculated, and mapping analysis was performed to calculate the coverage of the lubricating components. Measurements were performed on three randomly selected visual fields for each resin-coated metal sheet, and all lubricating components within the measured visual fields were included in the calculation.

[0079] (4) Resin composition of the resin layer The resin composition of the resin layer was calculated as follows. After peeling the resin layer from the resin-coated metal plate in the same manner as in (1) above, the resin layer was dissolved in a solvent prepared by adding an appropriate amount of trifluoroacetic acid-d to chloroform-d. At this time, in order to remove the insoluble matter generated during the dissolution process, centrifugation was carried out and the soluble matter was used for measurement. The measurement was carried out using a nuclear magnetic resonance apparatus: AVANCE NEO cryo-500 model manufactured by Bruker Biospin Corporation, and the measurement nucleus was 1 The measurement was carried out under the conditions of H (500 MHz) and the number of accumulations was 16. The resin composition ratio was calculated from the integrated intensity of each signal in the obtained spectrum.

[0080] (5) Acid Value of Lubricating Component The acid value of the lubricating component was calculated as follows. A predetermined amount of the lubricating component extracted in the same manner as in (2) above, corresponding to the estimated acid value in accordance with JIS K5902, was weighed into a flask and dissolved in 100 mL of a neutral solvent. The neutral solvent used was a 1:1 or 2:1 volumetric mixture of diethyl ether specified in JIS K8103 and ethanol (purity 99.5 or higher) specified in JIS K8101. This solution was titrated with 0.1 mol / L potassium hydroxide standard solution using phenolphthalein as an indicator. The acid value was calculated using the following formula, with the neutralization endpoint being the time when the indicator color change continued for 30 seconds. In the following formula (I), α represents the amount (mL) of 0.1 mol / L potassium hydroxide standard solution used, β represents the amount (g) of sample collected, and F represents the factor of the 0.1 mol / L potassium hydroxide standard solution.

[0081] Acid value (mgKOH / g) = 5.611×α×F / β (I)

[0082] (6) Thickness of each resin layer The thickness of each resin layer was determined as follows. After peeling the resin layer from the resin-coated metal plate in the same manner as in (1) above, a Pt coating was applied to the outermost surface of the resin layer, and a cross section was prepared using an ion milling device (EM TIC 3X) manufactured by Leica Microsystems. Then, using a scanning electron microscope (SEM) (Regulus 8220) manufactured by Hitachi High-Technologies Corporation, backscattered electron images were observed at two magnifications of 2500x and 8000x, and the thicknesses of the surface layer, middle layer, and lower layer of the resin layer were calculated from the observed images.

[0083] The resin-coated metal sheets of Examples 1 to 28 and Comparative Examples 1 to 8 were further evaluated for film adhesion, formability, and ink adhesion of the resin layer by the methods described below. The evaluation results are shown in Table 4.

[0084]

[0085] (7) Film Adhesion The film adhesion was evaluated as follows. The resin-coated metal sheets of Examples 1 to 28 and Comparative Examples 1 to 8 were molded into can bodies (cylindrical shapes with a diameter of 50 mm and a height of 160 mm), and then T-shaped test pieces were cut out from the top of the can body. Next, a score-cutting blade was used to make cuts in the resin layer and metal sheet, which are the non-symmetrical surfaces, to separate them. Using a Tensilon universal testing machine manufactured by Orientec Co., Ltd., the resin layer, which is the symmetrical surface, was pulled 15 mm in the opposite direction (180°) from the separated metal sheet, and the peel strength of the resin layer was measured. Two sheets were cut out per can and measurements were performed to evaluate whether the resin layer was sufficiently adhered to the metal sheet even after being subjected to strong processing.

[0086] The film adhesion was evaluated on a four-point scale from "A" (best) to "D" (worst), and the evaluation criteria were set as follows:

[0087] Rating "A": The average maximum load at two points per can is 2.5N / 15mm or more.

[0088] Rating "B": The average maximum load at two points per can was 2.0 N / 15 mm or more and less than 2.5 N / 15 mm.

[0089] Rating "C": The average maximum load at two points per can was 1.5 N / 15 mm or more and less than 2.0 N / 15 mm.

[0090] Rating "D": The average maximum load at two points per can is less than 1.5 N / 15 mm.

[0091] (8) Moldability Moldability was evaluated as follows. After wax was applied to the resin-coated metal sheets of Examples 1 to 28 and Comparative Examples 1 to 8, they were punched into disks with a diameter of 123 mm and drawn into cups at a drawing ratio of 1.7 using a cupping press. The resulting cups were inserted into a DI forming device and subjected to redrawing and DI processing at a drawing ratio of 1.3 to form cans with an inner diameter of 52 mm and a can height of 90 mm. The surface of the resin layer of the formed cans was visually observed to evaluate processability.

[0092] The moldability was evaluated on a four-point scale from "A" (best) to "D" (worst), and the evaluation criteria were set as follows:

[0093] Evaluation "A": No scraping was observed visually.

[0094] Rating "B": Chipping is visually observed at a height within 10 mm from the flange of the can.

[0095] Rating "C": Chipping is visually observed at a height of more than 10 mm and up to 30 mm from the flange of the can.

[0096] Rating "D": Chipping or broken bodies reaching a height of more than 30 mm from the flange of the can are visually observed.

[0097] (9) Ink Adhesion Ink adhesion was evaluated as follows. The resin-coated metal plates of Examples 1 to 28 and Comparative Examples 1 to 8 were subjected to a heat treatment in a hot air drying oven, reaching 240°C in 2 minutes, and then cooled to room temperature. Thereafter, for each of the heat-treated resin-coated metal plates, a polyester-based printing ink (red) was printed on the resin layer located on the outer surface of the container after molding using a universal printing tester manufactured by Kumagai Riki Kogyo Co., Ltd. The resin-coated metal plates were subjected to a heat treatment in a hot air drying oven, reaching 185°C in 1 minute, and then cooled to room temperature. A scratch test was performed on the ink-printed surface of the cooled resin-coated metal plate in the lamination direction of the resin layer. A load-varying friction and wear tester: HHS2000 manufactured by Shinto Scientific Co., Ltd. was used, and the test conditions were a continuous load of 10 gf to 1000 gf from the printing edge, a movement speed of 0.5 mm / sec, a movement distance of 30 mm, and a sapphire indenter (diameter 0.6 mm). Ten tests (two sheets x five tests) were carried out for each resin-coated metal plate, and the ink peel load was calculated from the resulting ink peel length to evaluate the ink adhesion.

[0098] The ink adhesion was evaluated on a four-level scale from "A" (best) to "D" (worst), and the evaluation criteria were set as follows:

[0099] Evaluation "A": Of the 10 tests, the peel load for 10 points (all) was equal to or greater than the lower limit for material without lubricating components added.

[0100] Evaluation "B": Of the 10 tests, the peel load for 7 to 9 points was equal to or greater than the lower limit for material without lubricating components added.

[0101] Rating "C": Of the 10 tests, the peel load was equal to or greater than the lower limit for the material without lubricating components added at 5 to 6 points.

[0102] Rating "D": Of the 10 tests, the peel load for 6 or more points was below the lower limit for the material without lubricating components added.

[0103] As shown in Table 4, the resin-coated metal sheets according to the examples received good ratings of B or higher (rating A or B) for film adhesion, formability, and ink adhesion. In contrast, the resin-coated metal sheets according to the comparative examples received poor ratings of C or lower (rating C or D) for film adhesion, formability, and ink adhesion, and were inferior to the resin-coated metal sheets according to the examples.

[0104] When each resin-coated metal sheet according to the examples is examined individually, the following trends can be seen. Even when the lubricating component of the surface layer is less than 0.10% by mass (Example 15), good film adhesion, formability, and ink adhesion can be achieved. However, when the lubricating component of the surface layer is 0.40% by mass or more, the results are even better, with formability being particularly improved. Furthermore, even when the lubricating component of the surface layer is 1.0% by mass (Example 13), good film adhesion, formability, and ink adhesion can be achieved. However, when the lubricating component of the surface layer is 0.90% by mass or less, the results are even better, with ink adhesion being particularly improved.

[0105] Focusing on the coverage of the lubricating component in Examples 11, 13, 15-17, and 24, a coverage of 0.040% or more and 0.80% or less ensures sufficient slip properties and abrasion resistance to withstand can-making processing, making breakage or abrasion less likely to occur during molding, and improving formability. Considering the balance with ink adhesion (Examples 13, 17, 18, and 24), a coverage of 0.50% or less provides an even better balance between formability and ink adhesion.

[0106] Titanium dioxide (TiO 2 It is important to add a predetermined amount of titanium dioxide (TiO) to the intermediate layer in order to ensure sufficient whiteness and hiding power in the resin layer. 2 Although there is no problem if the amount exceeds 30% by mass (Example 20), an amount of 10% by mass or more and 30% by mass or less is appropriate, and this provides better moldability.

[0107] When the melting point of the resin layer is 238° C. or higher, the moldability is better.

[0108] In this way, a resin-coated metal sheet and a method for producing the same can be provided.

[0109] It should be noted that the embodiments disclosed in this specification are merely examples, and the present invention is not limited to these embodiments, and can be modified as appropriate within the scope of the purpose of the present invention.

[0110] The present invention can be applied to a resin-coated metal sheet and a method for manufacturing the same.

[0111] 100: Plate material (resin-coated metal plate) 2: Metal plate layer 3: Resin layer 31: Surface layer 32: Intermediate layer 33: Lower layer 4: Resin layer

Claims

1. A resin-coated metal plate comprising: a metal plate layer; and a resin layer containing a polyester resin coating the surface of the metal plate layer, wherein the resin layer has a melting point of 225°C or higher and 255°C or lower, and comprises a surface layer disposed on the surface opposite to the side facing the metal plate layer, a lower layer facing the metal plate layer, and an intermediate layer between the surface layer and the lower layer, wherein the surface layer contains a lubricating component made of polyolefin having a melting point of 75°C or higher and 140°C or lower, and wherein the coverage of the lubricating component exposed on the surface of the surface layer is 0.040% or higher and 0.80% or lower, as determined by peak intensity ratio analysis of Raman spectrum data obtained when Raman measurement is performed on the surface layer using a confocal Raman device.

2. The resin-coated metal sheet according to claim 1, wherein the resin layer is formed from a resin material containing 90 mol % or more of ethylene terephthalate units.

3. A resin-coated metal sheet according to claim 1 or 2, wherein the surface layer contains 0.10 mass % or more and 1.0 mass % or less of the lubricating component.

4. A resin-coated metal sheet according to any one of claims 1 to 3, wherein the lubricating component comprises an acid-modified polyolefin or an oxidized polyolefin.

5. The resin-coated metal sheet according to claim 4, wherein the lubricating component has an acid value of 1.0 mgKOH / g or more and 80 mgKOH / g or less.

6. A resin-coated metal sheet according to any one of claims 1 to 5, wherein the intermediate layer contains 10% by mass or more and 30% by mass or less of inorganic particles.

7. A resin-coated metal sheet according to any one of claims 1 to 6, wherein the surface layer has a thickness of 1.0 μm or more and 5.0 μm or less, the intermediate layer has a thickness of 6.0 μm or more and 30 μm or less, and the lower layer has a thickness of 1.0 μm or more and 5.0 μm or less.

8. A method for producing a resin-coated metal sheet according to any one of claims 1 to 7, comprising: preparing masterbatch pellets in which the lubricating component is dispersed using a polyester resin as a base, the polyester resin having a melting point of 230°C or higher and 254°C or lower and an intrinsic viscosity of 0.45 or higher and 0.88 or lower; kneading the masterbatch pellets with the polyester resin pellets, extruding the extrusion at a predetermined extrusion temperature, and stretching the extrusion by a biaxial stretching method to form a film; and thermocompression bonding the film to a metal sheet using a laminating roll.

9. The method for producing a resin-coated metal sheet according to claim 8, wherein the predetermined extrusion temperature is 255°C or higher and 285°C or lower.

10. The method for producing a resin-coated metal sheet according to claim 8 or 9, wherein the stretching ratio of the film is 2.0 times or more and 5.0 times or less.