Sheet-shaped bonding material and method of producing same, and bonded body and method of producing same

MYPI2025002980A0Undetermined Publication Date: 2024-05-16NIPPON SANSO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025002980
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-11-16
Filing Date
2023-10-24
Publication Date
2024-05-16

AI Technical Summary

Technical Problem

Conventional solder materials exhibit poor heat resistance, making them unsuitable for high-temperature applications, and existing sheet-like bonding materials using copper nanoparticles face issues with uneven sintering and insufficient bonding strength at low temperatures, particularly in inert atmospheres.

Method used

A sheet-like bonding material comprising copper particles with an average diameter of 300 nm or less and optional coarse particles, combined with triethanolamine as a reducing agent, which provides sufficient bonding strength at temperatures of 250°C or less without requiring a reducing gas, ensuring uniform sintering across the joint surface.

Benefits of technology

The bonding material achieves strong and uniform bonding even at low temperatures, preventing uneven sintering between the center and edge parts of the joint surface, enhancing the reliability and durability of bonded bodies in high-temperature environments.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Provided is a bonding material that even in low-temperature bonding at 250C or lower, enables bonding with sufficient bonding strength and with low tendency for unevenness between a sinter state of a central section and a sinter state of a pressed edge section at a pressure bonding surface. A sheet-shaped bonding material contains copper particles and a reductant that reduces the copper particles. The copper particles include fine copper particles having a mean particle diameter of 300 nm or less and optionally include coarse copper particles having a mean particle diameter of 3-11 m. Content of the fine copper particles relative to the total content of the fine copper particles and the coarse copper particles is 50-100 mass%. The reductant is composed of triethanolamine, and content of the triethanolamine is 1.5-10.0 mass% relative to the total content of the fine copper particles and the coarse copper particles.
Need to check novelty before this filing date? Find Prior Art

Description

Sheet-like bonding material and its manufacturing method, and bonded body and its manufacturing method

[0001] The present invention relates to a sheet-like bonding material and a manufacturing method thereof, and a bonded body and a manufacturing method thereof.

[0002] Conventionally, solder materials have been widely used as bonding materials for electronic components. However, solder materials have a problem of poor heat resistance. Therefore, for example, it has been difficult to use solder materials as bonding materials in power devices using SiC elements that are expected to be used at high temperatures of 150°C or higher.

[0003] Therefore, a bonding material using silver particles has been proposed as a sintered bonding material, and copper nanoparticles are expected to be an alternative in terms of cost and ion migration.

[0004] Patent Document 1 describes a plate- or sheet-shaped bonding material that includes a sintered body of fine particles whose main component is copper and whose average particle diameter is 300 nm or less, and has a specific resistance value of 1×10 -5 The document describes a "bonding material having a resistivity of Ω·m or less," which allows a high bonding strength to be exerted even when two or more members to be bonded are bonded in an inert atmosphere.

[0005] However, although Patent Document 1 can achieve bonding in an inert atmosphere, when producing the sheet-shaped bonding material, copper nanoparticles are sintered under pressure in a reducing atmosphere, which requires a reducing gas, and there are limitations in terms of gas equipment such as exhaust gas treatment. In addition, because the copper nanoparticles are sintered by the reducing gas, the surface activity specific to nanoparticles is lost, and there is also the problem that performance is unstable depending on the sintering state.

[0006] Therefore, Patent Documents 2 and 3 propose sheet-shaped bonding materials that can be stably bonded in an inert atmosphere without requiring a reducing gas during bonding by adding a reducing agent during production of the sheet-shaped bonding material. Specifically, Patent Document 2 describes a "plate- or sheet-shaped bonding material containing copper as a main component and copper fine particles having an average particle diameter of 300 nm or less, further containing a reducing agent that reduces the copper fine particles." Patent Document 3 describes a "plate- or sheet-shaped bonding material containing copper fine particles having an average particle diameter of 300 nm or less, coarse copper particles having an average particle diameter of 3 μm to 11 μm, and a reducing agent that reduces the copper fine particles and the coarse copper particles." Examples of reducing agents include polyol solvents such as ethylene glycol and organic acids.

[0007] JP 2018-12871 A JP 2019-203172 A JP 2021-116450 A

[0008] However, in the sheet-shaped bonding materials described in Patent Documents 2 and 3, the reducing effect of the reducing agent is not fully exerted at low-temperature bonding below 250°C, resulting in insufficient bonding strength and uneven sintering between the center and edge portions of the pressurized bonding surface.

[0009] In view of the above problems, the present invention aims to provide a joining material that can obtain sufficient joining strength even when joining at low temperatures of 250°C or less, and that can achieve joining with little unevenness between the sintered state of the center part and the sintered state of the pressurized joining surface at the pressurized edge part, and a suitable manufacturing method thereof.

[0010] Another object of the present invention is to provide a bonded body in which the above-mentioned excellent bonding is achieved using such a bonding material, and a suitable method for producing the same.

[0011] The gist of the present invention for solving the above problems is as follows: [1] A sheet-like bonding material comprising copper particles and a reducing agent that reduces the copper particles, wherein the copper particles comprise copper fine particles having an average particle diameter of 300 nm or less and optionally contained coarse copper particles having an average particle diameter of 3 μm or more and 11 μm or less, wherein the content of the copper fine particles relative to the total content of the copper fine particles and the coarse copper particles is 50 mass % or more and 100 mass % or less, and the reducing agent is triethanolamine, and the content of the triethanolamine is 1.5 mass % or more and 10.0 mass % or less relative to the total content of the copper fine particles and the coarse copper particles.

[0012] [2] The ratio of the mass oxygen concentration to the specific surface area of ​​the copper fine particles is 0.1 mass% g / m 2 1.2% by mass / g / m 2 The sheet-like bonding material according to the above [1], which is as follows.

[0013] [3] The ratio of the mass carbon concentration to the specific surface area of ​​the copper fine particles is 0.008 mass% g / m 2 More than 0.3 mass%・g / m 2 The sheet-like bonding material according to the above [1] or [2], which is as follows:

[0014] [4] A method for producing a sheet-like bonding material, comprising: a mixing step of mixing copper particles with a reducing agent that reduces the copper particles to obtain a mixture; and a pressure molding step of pressure molding the mixture to obtain a sheet-like bonding material, wherein the copper particles include copper fine particles having an average particle diameter of 300 nm or less and optionally contained coarse copper particles having an average particle diameter of 3 μm or more and 11 μm or less, and the content of the copper fine particles in the mixture relative to the total content of the copper fine particles and the coarse copper particles is 50 mass% or more and 100 mass% or less, and the reducing agent is triethanolamine, and the content of the triethanolamine in the mixture is 1.5 mass% or more and 10.0 mass% or less relative to the total content of the copper fine particles and the coarse copper particles.

[0015] [5] The method for producing a sheet-like bonding material according to the above [4], wherein the mixing step includes a step of mixing the copper particles, the reducing agent, and an organic solvent to obtain a slurry, and a step of drying the slurry to obtain the mixture.

[0016] [6] A bonded body comprising a first member, a second member, and the bonding material according to any one of [1] to [3] above, wherein the bonding material is located between the first member and the second member.

[0017] [7] A method for manufacturing a bonded body, comprising a step of placing the bonding material according to any one of [1] to [3] above between a first member and a second member, and applying pressure while the bonding material is placed between the first member and the second member, to obtain a bonded body in which the first member and the second member are bonded together by the bonding material.

[0018] [8] The method for producing a bonded body according to the above [7], wherein the bonding temperature is 250°C or less.

[0019] The bonding material of the present invention can obtain sufficient bonding strength even at low temperatures of 250° C. or less, and can achieve bonding with little unevenness between the sintered state of the center and the sintered state of the pressure-bonded surface. Such a bonding material can be manufactured by the manufacturing method of the present invention.

[0020] The bonded body of the present invention achieves the above-described excellent bonding by using such a bonding material. According to the method for manufacturing a bonded body of the present invention, a bonded body achieving the above-described excellent bonding by using such a bonding material can be manufactured.

[0021] [Sheet-like bonding material] A sheet-like bonding material according to one embodiment of the present invention includes copper particles and a reducing agent that reduces the copper particles. The copper particles include fine copper particles (also referred to as "copper nanoparticles") and coarse copper particles, and preferably consist of fine copper particles and coarse copper particles. Here, "fine copper particles" refers to copper particles having a particle diameter of less than 800 nm, and "coarse copper particles" refers to copper particles having a particle diameter of 800 nm or more.

[0022] (Copper microparticles) The copper microparticles are mainly composed of copper. The copper microparticles preferably contain 95% by mass or more and 100% by mass or less of copper element relative to 100% by mass of copper microparticles, and more preferably 97% by mass or more. When the copper element is contained in an amount of 95% by mass or more, the bonding material has excellent heat resistance and further excellent bonding strength.

[0023] The average particle diameter of the copper microparticles is 300 nm or less. However, the average particle diameter of the copper microparticles is more preferably 150 nm or less. When the average particle diameter of the copper particles is 300 nm or less, the bonding material has excellent bonding strength. The average particle diameter of the copper microparticles is preferably 5 nm or more. When the average particle diameter of the copper microparticles is 5 nm or more, copper microparticles are easily available.

[0024] The particle size distribution of the copper fine particles does not overlap with the particle size distribution of the coarse copper particles. For example, the particle size distribution of the copper fine particles may be D10: 40 nm, D50: 110 nm, and D90: 300 nm.

[0025] The shape (form) of the copper fine particles is not particularly limited. Examples of the shape of the copper fine particles include spherical (sphere), ellipsoid (ellipsoid), and plate-like shapes. Among these, spherical and ellipsoid shapes are preferred, and spherical shapes are more preferred.

[0026] The average particle size of copper microparticles can be determined by observing 10 fields of view at 10,000x magnification using a scanning electron microscope (SEM), measuring the particle size of all copper microparticles (copper particles with a particle size of less than 800 nm) selected according to the following selection criteria (1) to (5), and calculating the arithmetic mean. For particles that are not perfectly round, such as ellipses, the major axis is used as the particle size. The particle size distribution of copper microparticles is also determined by the particle sizes of all copper microparticles measured. When determining the average particle size and particle size distribution of copper microparticles in a sheet-like bonding material, the outermost surface of the sheet is observed. In the powder state before sheet production, the powder is placed on carbon tape with a spatula, excess powder is removed with an air duster, and the tape surface is observed. (1) Particles with parts outside the field of view of the image are not measured. (2) Particles with clear outlines and isolated presence are measured. (3) Even if the particle shape is different from the average, it is measured if it is independent and can be measured as a single particle. (4) If there are overlapping particles but the boundary between them is clear and the overall shape of the particle can be determined, each particle is measured as a single particle. (5) If the boundary between overlapping particles is unclear and the overall shape of the particle cannot be determined, the particle shape cannot be determined and the particle is not measured.

[0027] It is preferable to use copper fine particles that do not require a protective agent, a dispersant, etc. An example of such copper fine particles is the ultrafine metal powder obtained by the manufacturing method described in Japanese Patent No. 4304221. However, the copper fine particles are not limited to this example.

[0028] The copper fine particles preferably have a coating containing copper carbonate on the surface. By having a coating containing copper carbonate on the surface of the copper fine particles, the sintering temperature of the copper fine particles can be kept lower than before while increasing the bonding strength. Furthermore, when the copper fine particles containing copper carbonate are sintered, they also neck against the coarse copper particles, making the entire sintered copper layer stronger. The coating containing copper carbonate may further contain cuprous oxide.

[0029] The ratio of the mass oxygen concentration to the specific surface area of ​​the copper fine particles is set to 0.1 mass% g / m from the viewpoint of reducing the reactivity with oxygen in the air and reducing the influence of reoxidation. 2 It is preferable that the content is 0.2 mass% g / m or more. 2 On the other hand, the ratio of the mass oxygen concentration to the specific surface area of ​​the copper fine particles is preferably 1.2 mass% g / m or more from the viewpoint of facilitating removal of the oxide film during bonding and further increasing the bonding strength. 2 It is preferable that the content is 0.5 mass% g / m or less. 2 More preferably, it is:

[0030] The ratio of the mass carbon concentration to the specific surface area of ​​the copper fine particles is set to 0.3 mass% g / m from the viewpoint of suppressing the occurrence of voids and cracks and further increasing the bonding strength. 2 It is preferable that the content is 0.1 mass% g / m or less. 2 More preferably, it is 0.05 mass% g / m or less. 2 The ratio of the mass carbon concentration to the specific surface area of ​​the copper fine particles is more preferably 0.008 mass% g / m or less. 2 It is preferable that this is equal to or greater than this.

[0031] The ratio of the mass oxygen concentration to the specific surface area of ​​the copper microparticles can be calculated from the measured specific surface area and mass oxygen concentration. The specific surface area can be measured using a nitrogen gas BET adsorption device (e.g., "MACSORB HM-1201" manufactured by Mountech Co., Ltd.). The mass oxygen concentration can be measured using an oxygen / nitrogen analyzer (e.g., "TC600" manufactured by LECO Corporation).

[0032] The ratio of the mass carbon concentration to the specific surface area of ​​the copper microparticles can be calculated from the measured specific surface area and mass carbon concentration. The specific surface area can be measured using a nitrogen gas BET adsorption device (e.g., "MACSORB HM-1201" manufactured by Mountech Co., Ltd.). The mass carbon concentration can be measured using a carbon-sulfur analyzer (e.g., "EMIA-920V" manufactured by Horiba, Ltd.).

[0033] (Coarse Copper Particles) The bonding material of this embodiment optionally contains coarse copper particles. The coarse copper particles are mainly composed of copper. The coarse copper particles preferably contain 95% by mass or more and 100% by mass or less of copper element relative to 100% by mass of the copper coarse particles, and more preferably contain 97% by mass or more. When the coarse copper particles contain 95% by mass or more of copper element, the sinterability of the bonding material is excellent and the bonding strength is further excellent.

[0034] The average particle diameter of the coarse copper particles is 3 μm or more and 11 μm or less. When the average particle diameter of the coarse copper particles is 3 μm or more, shrinkage of the copper fine particles is reduced when the bonding material is sintered, and cracking of the bonded members is suppressed. From this viewpoint, the average particle diameter of the coarse copper particles is preferably 5 μm or more. When the average particle diameter of the coarse copper particles is 11 μm or less, the bonding material can be sufficiently sintered while maintaining the effect of reducing the shrinkage of the copper fine particles, and the bonding strength of the bonded body is not impaired. From this viewpoint, the average particle diameter of the coarse copper particles is preferably 9 μm or less.

[0035] The particle size distribution of the coarse copper particles does not overlap with that of the fine copper particles. For example, the particle size distribution of the coarse copper particles may be D10: 1.9 μm, D50: 3.8 μm, and D90: 8.2 μm.

[0036] The shape (form) of the coarse copper particles is not particularly limited, and examples of the shape of the coarse copper particles include spherical (sphere), ellipsoid (ellipsoid), and plate (flake) shapes, with spherical and ellipsoid shapes being preferred, and ellipsoid shapes being more preferred.

[0037] Examples of the coarse copper particles that can be used include commercially available flake copper such as "MA-C03KP" manufactured by Mitsui Mining & Smelting Co., Ltd. and "MA-C025KFD" manufactured by Mitsui Mining & Smelting Co., Ltd., and commercially available micro copper such as "1300Y" manufactured by Mitsui Mining & Smelting Co., Ltd.

[0038] The average particle size of coarse copper particles can be determined by observing 10 fields of view at 2000x magnification using a scanning electron microscope (SEM). The particle size of all coarse copper particles (copper particles with a particle size of 800 nm or more) selected according to the following selection criteria (1) to (5) is measured in the 10 fields of view, and the arithmetic mean is calculated. For particles that are not perfectly round, such as ellipses, the major axis is used as the particle size. The particle size distribution of coarse copper particles is also determined by the particle sizes of all the coarse copper particles measured. When determining the average particle size and particle size distribution of coarse copper particles in a sheet-like bonding material, the outermost surface of the sheet is observed. In the powder state before sheet production, the powder is placed on carbon tape with a spatula, excess powder is removed with an air duster, and the tape surface is observed. (1) Particles with parts extending outside the field of view of the photograph are not measured. (2) Particles with clear outlines and isolated presence are measured. (3) Even if the particle shape is different from the average, it is measured if it is independent and can be measured as a single particle. (4) If there are overlapping particles but the boundary between them is clear and the overall shape of the particle can be determined, each particle is measured as a single particle. (5) If the boundary between overlapping particles is unclear and the overall shape of the particle cannot be determined, the particle shape cannot be determined and the particle is not measured.

[0039] (Mass ratio of copper fine particles to coarse copper particles) The content of copper fine particles relative to the total content of copper fine particles and coarse copper particles is 50% by mass or more and 100% by mass or less, preferably 75% by mass or more, and more preferably 100% by mass. In other words, the content of coarse copper particles relative to the total content of copper fine particles and coarse copper particles is 0% by mass or more and 50% by mass or less, preferably 25% by mass or less, and more preferably 0% by mass. This allows for a bonding material with sufficient bonding strength.

[0040] The "content of copper fine particles relative to the total content of copper fine particles and coarse copper particles" in the sheet-like bonding material can be calculated, for example, by placing the sheet in an organic solvent such as isopropyl alcohol, ultrasonically dispersing the resulting dispersion, centrifuging the dispersion to separate the copper fine particles and the coarse copper particles, and measuring the weight of each.

[0041] (Reducing Agent) The reducing agent is a compound that reduces copper fine particles and coarse copper particles. The reducing agent is preferably a compound that can function as a dispersion medium in which copper fine particles and coarse copper particles are dispersed. The compound that can function as a dispersion medium is preferably a compound that is liquid at room temperature, and more preferably a liquid compound that vaporizes at high temperatures of 150°C or higher. This causes the reducing agent to vaporize during bonding, making it less likely to remain in the bonded body described below. As a result, voids and cracks are less likely to occur, and the bonding strength is even better.

[0042] As a reducing agent capable of functioning as a dispersion medium, an amine solvent is preferred, and specific examples include ethanolamine, diethanolamine, and triethanolamine. However, in this embodiment, among these, the reducing agent is triethanolamine. This allows for sufficient bonding strength even at low temperatures of 250°C or less, and enables bonding with little unevenness between the sintered state of the center and the sintered state of the pressure-bonded surface. While the reason why triethanolamine is used as a reducing agent is unclear, the inventors believe that the reducing agent present in the pressure-bonded center is unlikely to escape to the outside, while the reducing agent present around the pressure-bonded edge is likely to escape to the outside. In the case of triethanolamine, a reducing agent with a high boiling point and low volatility, the reducing agent is unlikely to escape to the outside even at the pressure-bonded edge. Therefore, it remains at the pressure-bonded edge up to a temperature of approximately 200°C, at which the reduction of copper fine particles begins, and therefore is thought to be less likely to cause uneven sintering.

[0043] The content of the reducing agent, i.e., triethanolamine, is preferably 1.5% by mass or more, more preferably 3.8% by mass or more, and even more preferably 5.5% by mass or more, relative to 100% by mass of the total of the fine copper particles and the coarse copper particles, thereby achieving a superior bonding strength when bonded in a nitrogen atmosphere, a higher bonding strength than when bonded in a reducing atmosphere, and reducing sintering unevenness in the center and edge portions of the pressed material.

[0044] The content of the reducing agent, i.e., triethanolamine, is preferably 10.0 mass% or less, more preferably 7.5 mass% or less, relative to 100 mass% of the total of the fine copper particles and the coarse copper particles, which makes it difficult for voids and cracks to occur, further improves bonding strength, and makes it easier to form the bonding material into a plate or sheet.

[0045] The content of the reducing agent in the sheet-shaped bonding material is equal to the content of the reducing agent in the mixture. However, the "content of the reducing agent" in the sheet-shaped bonding material can be calculated, for example, by measuring the amount of the reducing agent from the weight loss from 175°C to 600°C in thermogravimetry of the sheet-shaped bonding material.

[0046] (Other Components) The bonding material of the present embodiment may further contain optional components such as a dispersant in addition to the copper particles and the reducing agent, as long as the effects of the present invention are not impaired. However, the content of the optional components is preferably 2 mass% or less relative to the copper fine particles.

[0047] (Sheet form) The bonding material of this embodiment is in sheet form, making it easier to handle than conventional paste-like products. Furthermore, even when the bonding material is stored for a long period of time, the dispersibility of the copper microparticles can be easily maintained. Furthermore, there is no need to store the bonding material in a frozen state, and there is no need to mix an excessive amount of dispersant. As a result, the quality of the bonding material and the bonded body described below is excellent.

[0048] The bonding material of this embodiment is formed by mixing copper particles with a required reducing agent and then pressure-molding the mixture into a sheet, as will be described later. The thickness of the bonding material (thickness in the pressure direction) is not particularly limited, and can be, for example, 100 μm or more and less than 1 mm.

[0049] The shape of the bonding material (when viewed from above in the thickness direction) is not particularly limited and can be appropriately selected depending on the shape of the bonding surfaces of the members to be bonded. The shape may be the shape of the pressing surface when the mixture is press-molded under a required pressure to form a sheet. Specific examples include a rectangle and a circle.

[0050] [Method for manufacturing sheet-like bonding material] A method for manufacturing a sheet-like bonding material according to one embodiment of the present invention is a method for suitably manufacturing the sheet-like bonding material according to one embodiment of the present invention described above.

[0051] Therefore, the details and preferred embodiments of the copper fine particles, the copper coarse particles, and the reducing agent are the same as those described above in the section [Sheet-shaped bonding material]. The respective contents of the copper fine particles, the copper coarse particles, and the reducing agent are also the same as those described above in the section [Sheet-shaped bonding material].

[0052] In the method for producing the sheet-shaped bonding material of this embodiment, first, a mixing step is performed in which copper particles (fine copper particles and any coarse copper particles) are mixed with a reducing agent that reduces the copper particles to obtain a mixture. The method for mixing the copper particles and the reducing agent is not particularly limited. Examples of the mixing method include a method using a planetary mixer, a mortar, a mill stirring method, a stirrer stirring method, etc.

[0053] Because triethanolamine as a reducing agent has a very high viscosity, it is difficult to uniformly mix it with copper particles. Therefore, it is preferable to add an organic solvent to the copper particles and triethanolamine, mix them to obtain a slurry, and then dry the slurry to remove the organic solvent to obtain a mixture. The organic solvent is preferably an alcohol or ketone solvent with a low boiling point (less than 100°C) and high volatility. Using an organic solvent with a low boiling point and high volatility makes it easy to remove the diluting organic solvent, which is unnecessary for the bonding material, in the temperature range where triethanolamine does not easily evaporate (less than 100°C), which has the advantage of maintaining almost the same concentration of triethanolamine required for the reduction and sintering of copper particles.

[0054] In the method for producing a sheet-like bonding material of this embodiment, a pressure molding step is then performed in which the mixture obtained in the mixing step is pressure-molded to obtain a sheet-like bonding material. The pressure molding method is not particularly limited. Examples of the pressure molding method include methods using a metal jig, a compression molding machine, etc.

[0055] The atmosphere in which pressure is applied is not particularly limited, and may be an inert atmosphere or an air atmosphere, although it is preferable to apply pressure in the air from the viewpoint of convenience.

[0056] The pressure applied during pressing is preferably 10 MPa or more, more preferably 40 MPa or more. When the pressure applied during pressing is 10 MPa or more, the durability of the bonding material formed into a sheet shape is increased. In addition, the higher the pressure applied, the higher the density of the copper fine particles contained in the bonding material, and the higher the shear strength of the bonding surface of the bonded body. On the other hand, if the pressure applied during pressing is excessive, cracks may occur in the molded body, so the pressure applied during pressing is preferably 500 MPa or less.

[0057] The molding temperature during pressure application is not limited, but in consideration of operability, molding at room temperature (10 to 30° C.) is desirable. The molding time during pressure application is not particularly limited, but can be, for example, from 1 minute to 10 minutes.

[0058] [Jointed Body] A joined body according to one embodiment of the present invention includes a first member (first joined member), a second member (second joined member), and the above-described joining material according to one embodiment of the present invention. The joined body is a joined body in which a pressurized body of the joining material is positioned between the first member and the second member, and the first member and the second member are joined by the joining material.

[0059] The materials of the first member and the second member are not particularly limited as long as they can be bonded when pressure-bonded using the above-mentioned bonding material. Examples of such materials include metals such as copper, silicon, aluminum, copper oxide, silicon oxide, alumina, silicon nitride, aluminum nitride, boron nitride, and silicon carbide; alloys thereof; and mixtures thereof. The first member and the second member may be made of one type of material alone, or may be made of a combination of two or more types of materials. The first member and the second member may be made of the same material or different materials.

[0060] The shear strength of the bonding surface between the first member and the second member is preferably 35 MPa or more, more preferably 45 MPa or more, and even more preferably 55 MPa or more. When the shear strength of the bonding surface between the first member and the second member is 35 MPa or more, the bonding material is less likely to peel off from the bonded members even when the bonded body is repeatedly subjected to thermal shock, and the bonding reliability is excellent.

[0061] The shear strength can be adjusted by the content of the reducing agent in the bonding material, the pressure when the bonding material is press-molded, the pressure when bonding, and the atmospheric conditions when bonding (reducing atmosphere or inert atmosphere).

[0062] [Method for manufacturing a bonded body] A method for manufacturing a bonded body according to one embodiment of the present invention includes a step of placing the bonding material according to one embodiment of the present invention between a first member and a second member, and applying pressure while the bonding material is placed between the first member and the second member, to obtain a bonded body in which the first member and the second member are bonded by the bonding material.

[0063] The bonding conditions are not particularly limited and can be appropriately selected depending on the materials and combination of the first and second members. The atmosphere during bonding is preferably an inert atmosphere. The bonding pressure in the inert atmosphere can be, for example, 1 MPa or more and 40 MPa or less. The bonding temperature in the inert atmosphere can be, for example, 150°C or more and 400°C or less. In particular, in one embodiment of the present invention, good bonding can be achieved even if the bonding temperature (ambient temperature during bonding) is 250°C or less. The bonding time in the inert atmosphere can be, for example, 1 minute or more and 60 minutes or less.

[0064] [Manufacturing of bonding material] Copper microparticles obtained by the manufacturing method described in Japanese Patent No. 4304221 were prepared as raw materials. The copper element content in the obtained copper microparticles was 98.8 mass%. The average particle diameter of the obtained copper microparticles was determined by the method described above and was 110 nm. The particle size distribution of the obtained copper microparticles was D10: 40 nm, D50: 110 nm, D90: 300 nm. In addition, the ratio of the mass oxygen concentration to the specific surface area of ​​the obtained copper microparticles was 0.25 mass% g / m 2 The mass carbon concentration is 0.03 mass% g / m2 It was.

[0065] Furthermore, as the coarse copper particles, "MA-C03KP" (average particle size: 3.8 μm, tap density: 5.26 g / cm) manufactured by Mitsui Mining & Smelting Co., Ltd. 3 ) was prepared. The copper element content in the coarse copper particles was 97.5 mass%. The particle size distribution of the coarse copper particles was D10: 1.9 μm, D50: 3.8 μm, and D90: 8.2 μm. The particle size distribution of the fine copper particles and the particle size distribution of the coarse copper particles did not overlap.

[0066] Fine copper particles and coarse copper particles were mixed so that the content of the copper fine particles relative to the total content of the fine copper particles and the coarse copper particles was the value shown in Table 1, and a reducing agent of the type shown in Table 1 was added so that the content of the reducing agent (when mixed) relative to the total content of the mixed fine copper particles and coarse copper particles was the value shown in Table 1. 2-Propanol was then added as a dilution solvent, and the mixture was stirred with a planetary mixer to obtain a mixed slurry. Next, the 2-propanol was dried from the obtained mixed slurry at 70°C for 2 hours to obtain a mixture of fine copper particles, coarse copper particles (some examples), and a reducing agent.

[0067] Next, the mixture was added to the center hole of a 50 mm long cylindrical jig made of tungsten carbide with a 7 mm square hole in the center. Next, 7 mm square tungsten carbide pillars were inserted perpendicularly to both ends of the center hole of the jig and pressed into a sheet. The pressure molding was performed for 5 minutes under conditions of room temperature and a pressure of 74 MPa. As a result, in each example shown in Table 1, a sheet-like bonding material having a size of 7 mm square and a thickness of 250 μm was obtained. The content of the reducing agent relative to the total content of the copper fine particles and the copper coarse particles in the sheet-like bonding material is equivalent to the content of the reducing agent at the time of mixing shown in Table 1.

[0068] [Production of Bonded Body] Au-plated SiC (5 mm square, 350 μm thick) was prepared as the first member, and oxygen-free copper plate C1020 (20 mm square, 2 mm thick) was prepared as the second member. Using the sheet-like bonding material obtained in each example shown in Table 1, the first member and the second member were pressure-bonded in a 100% by volume nitrogen atmosphere (inert atmosphere) at the bonding temperature (ambient temperature) shown in Table 1, with a bonding pressure of 10 MPa and a bonding time of 5 minutes to produce a bonded body in each example shown in Table 1.

[0069] [Evaluation of Shear Strength] The shear strength of the bonded structure was measured using a bond tester (manufactured by Dage, 4000Plus). The tool height was 100 μm and the tool speed was 200 μm / s. The results are shown in Table 1.

[0070] [Evaluation of sinterability of pressurized bonded surface] The fracture surface of the bonded sample that was destroyed after shear strength measurement was subjected to SEM to observe the sinterability of the copper particles at the center and edge of the pressurized surface. If necking between the copper particles was observed, it was rated as "good", if necking between the copper particles was partially observed, it was rated as "fair", and if necking between the copper particles was not observed, it was rated as "poor". The results are shown in Table 1.

[0071] [Evaluation of the Shape of the Bonding Material] The appearance of the bonded body was checked. If the shape of the bonding material was not distorted, it was rated as "good." If the shape of the bonding material was not distorted but seepage of the reducing agent was observed, it was rated as "passable." If the shape of the bonding material was distorted and leakage of the bonding material from the bonding surface was observed, it was rated as "fail." The results are shown in Table 1.

[0072]

[0073] [Effect of reducing agent type] Inventive Example No. 1, which used triethanolamine as the reducing agent, exhibited good sinterability. On the other hand, Comparative Example No. 12, which used ethylene glycol as the reducing agent, and Comparative Example No. 14, which used diethanolamine, did not exhibit necking at the edge.

[0074] [Effect of Triethanolamine Content] Inventive Examples 1 to 9, which contained a triethanolamine content of 1.5% by mass or more and 10% by mass or less, exhibited good sinterability. On the other hand, Comparative Example 10, which contained 1.0% by mass of triethanolamine, was unable to be bonded. Furthermore, Comparative Example 11, which contained 10.7% by mass of triethanolamine, was unable to be molded into a sheet.

[0075] The results of Inventive Examples 4 and 5 and Inventive Examples 6 to 9 confirmed that the higher the triethanolamine content, the higher the bonding strength. However, in Inventive Examples 5 and 9, which had a triethanolamine content of 9.1% by mass, leakage of the bonding material was observed. This indicated that a triethanolamine content of 7.5% by mass or less is preferable. Although leakage of the bonding material was observed in Inventive Examples 5 and 9, the bonding strength was sufficient and there was no unevenness in the sintering state between the center and edge portions, so they could be used as a bonding material.

[0076] [Effect of Copper Fine Particle Content] Inventive Examples Nos. 1 to 9, in which the content of copper fine particles relative to the total content of copper fine particles and coarse copper particles was 50 mass% or more, exhibited good sinterability. On the other hand, Comparative Example No. 16, in which the content of copper fine particles was small, did not exhibit necking at the edge portion.

[0077] [Effect of Bonding Temperature] Although Example No. 6 exhibited inferior sintering properties at the pressurized edge compared to Example No. 3, which had the same bonding material composition, relatively good results were obtained. These results confirmed that bonding was possible even at a bonding temperature of 200°C when triethanolamine was used as a reducing agent.

[0078] The sheet-like bonding material and its manufacturing method, as well as the bonded body and its manufacturing method of the present invention, can be industrially used for bonding electronic components. Specifically, examples of applications include bonding components such as substrates and elements in high-temperature environments where it is difficult to use bonding materials such as solder, such as in electronic devices called power devices.

Claims

1. A sheet-like bonding material comprising copper particles and a reducing agent that reduces the copper particles, wherein the copper particles comprise copper fine particles having an average particle diameter of 300 nm or less and optionally coarse copper particles having an average particle diameter of 3 μm or more and 11 μm or less, wherein the content of the copper fine particles relative to the total content of the copper fine particles and the coarse copper particles is 50 mass% or more and 100 mass% or less, and the reducing agent is triethanolamine, and the content of the triethanolamine is 1.5 mass% or more and 10.0 mass% or less relative to the total content of the copper fine particles and the coarse copper particles.

2. The ratio of the mass oxygen concentration to the specific surface area of ​​the copper fine particles is 0.1 mass% g / m 2 1.2% by mass / g / m 2 The sheet-like bonding material according to claim 1, wherein:

3. The ratio of the mass carbon concentration to the specific surface area of ​​the copper fine particles is 0.008 mass% g / m 2 More than 0.3 mass%・g / m 2 The sheet-like bonding material according to claim 1, wherein:

4. A method for producing a sheet-like bonding material, comprising: a mixing step of mixing copper particles with a reducing agent that reduces the copper particles to obtain a mixture; and a pressure molding step of pressure molding the mixture to obtain a sheet-like bonding material, wherein the copper particles include copper fine particles having an average particle diameter of 300 nm or less and optionally contained coarse copper particles having an average particle diameter of 3 μm or more and 11 μm or less, and the content of the copper fine particles in the mixture relative to the total content of the copper fine particles and the coarse copper particles is 50 mass% or more and 100 mass% or less, and the reducing agent is triethanolamine, and the content of the triethanolamine in the mixture is 1.5 mass% or more and 10.0 mass% or less relative to the total content of the copper fine particles and the coarse copper particles.

5. A method for manufacturing a sheet-like bonding material as described in claim 4, wherein the mixing process includes a process of mixing the copper particles, the reducing agent, and an organic solvent to obtain a slurry, and a process of drying the slurry to obtain the mixture.

6. A bonded body comprising a first member, a second member, and the bonding material according to any one of claims 1 to 3, wherein the bonding material is positioned between the first member and the second member.

7. A method for manufacturing a bonded body, comprising a step of placing a bonding material according to any one of claims 1 to 3 between a first member and a second member, and applying pressure to the first member and the second member to obtain a bonded body in which the first member and the second member are bonded together by the bonding material.

8. The method for producing a bonded body according to claim 7, wherein the bonding temperature is 250°C or less.