Method for the treatment of porous substrates, and treated substrate and its use

MYPI2025003047A0Undetermined Publication Date: 2024-05-21FRAUNHOFER GESELLSCHAFT ZUR FORDERUNG DER ANGEWANDTEN FORSCHUNG EV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025003047
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-11-21
Filing Date
2023-11-16
Publication Date
2024-05-21

AI Technical Summary

Technical Problem

Current methods for treating porous carbon or graphite materials are costly and complex, especially when aiming for high thermal and mechanical stability, as they often result in incomplete infiltration, surface residue formation, and increased permeability, making them unsuitable for long-term use in high-temperature applications.

Method used

A method involving the application of an aqueous suspension containing silicon particles and a binder to the surface of porous carbon-containing substrates, followed by a drying process and heat treatment, where the silicon coating melts and infiltrates into the substrate, converting into silicon carbide to seal the pores and enhance mechanical stability.

Benefits of technology

This method achieves a high degree of sealing with reduced permeability and open porosity, preventing corrosion and increasing the substrate's resistance and surface quality, while avoiding surface residues and reducing the need for post-processing, thus providing a cost-effective and simple treatment process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025003047_DRAWING_001
    Figure PI2025003047_DRAWING_001
  • Figure PI2025003047_DRAWING_002
    Figure PI2025003047_DRAWING_002
  • Figure PI2025003047_DRAWING_003
    Figure PI2025003047_DRAWING_003
Patent Text Reader

Abstract

This invention relates to a method for treating porous substrates. In the method, at least one surface of a porous carbon-containing substrate is first provided with at least one silicon coating by applying at least one aqueous suspension comprising silicon particles, at least one binding agent, and water to the at least one surface and then subjecting it to a drying process. The at least one silicon coating is then subjected to at least one heat treatment in which the silicon coating melts to form a melt that infiltrates into the pores of the porous carbon-containing substrate, wherein silicon contained in the melt is at least partially converted to silicon carbide. Furthermore, the pre-sent invention also relates to a treated substrate and its use.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Process for the treatment of porous substrates as well as treated substrate and its use

[0002] The present invention relates to a method for treating porous substrates. In the method, at least one surface of a porous carbon-containing substrate is first provided with at least one silicon coating by applying at least one aqueous suspension comprising silicon particles, at least one binder and water to the at least one surface and then subjecting it to a drying process. The at least one silicon coating is then subjected to at least one heat treatment in which the silicon coating melts to form a melt which infiltrates into the pores of the porous carbon-containing substrate, wherein silicon contained in the melt is at least partially converted into silicon carbide. Furthermore, the present invention also relates to a treated substrate and its use. Carbon or.Graphite materials, especially isostatically pressed graphite (iso-graphite) and carbon fiber reinforced carbon (CFG), are widely used in systems subject to high thermal stress due to their good thermomechanical stability and ease of processing. These include components for high-temperature furnaces, such as heaters, insulation components, support brackets, and crucibles. However, long-term contact with corrosive atmospheres or media under the influence of high temperatures and mechanical stress can lead to increased degradation of the carbon or graphite materials. This reduces the service life of these components and leads to increased maintenance and repair costs.

[0003] To increase service life, carbon or graphite-silicon carbide composites (C / SiC composites) can be used. C / SiC composites are typically produced by infiltrating porous carbon or graphite bodies, e.g., carbon fiber reinforced carbon (CFG), with molten silicon (see, for example, Manish Patel et al., Bulletin of Materials Science, 2012, pp. 63-73). The component to be infiltrated is brought into contact with liquid silicon, which is absorbed by the component via capillary action. This results in a reaction between the carbon portion of the graphite and the liquid silicon, resulting in the formation of silicon carbide (SiC). The kinetics of the SiC formation reaction is determined by the contact angle and the spreading of the silicon melt on or in the carbon or graphite material (see O. Dezellus et al., Journal of Materials Science, 2005, 2307- 2311).This can be influenced by external factors, such as the gas atmosphere and the system pressure, during the process. In general, it must be noted that the increase in volume or differences in thermal expansion during SiC formation can cause stresses in the component, which can lead to pronounced cracking in graphite materials with low mechanical stability (see R. Israel et al., J. Mater. Sci., 2010, 45, 2210-2217). The amount of silicon must also be precisely dosed to ensure the most complete infiltration possible and, at the same time, to prevent silicon residues on the surface after cooling. This is of fundamental importance in order to avoid costly post-processing and scrap. However, avoiding silicon residues is generally very difficult to achieve. This is particularly true for dense graphite materials, such asIn the case of iso-graphite, infiltration by Si melt is unsuitable for sealing the surface due to the low porosity and absorption capacity of liquid silicon.

[0004] Alternatively, a dense coating with a chemically inert and mechanically stable, usually ceramic component (e.g., SiC) can be applied to the carbon or graphite materials. For this purpose, pyrolytic carbon or SiC is typically applied using chemical vapor deposition (CVD) or chemical vapor infiltration (CVI) (see, for example, W. Zhou et al., Ceramics International 21730-21733). This generally produces crack-free and highly dense layers that almost completely prevent the carbon or graphite components from being permeable to fluids or gases. If a material system is selected (e.g., SiC) that also offers a significant increase in mechanical or chemical resistance, the carbon or graphite material can be used for significantly broader applications.

[0005] However, these processes are associated with high costs and considerable technical effort. In particular, both processes are very difficult to apply homogeneous coatings to complex, large-area, and three-dimensional components.

[0006] Based on this, the object of the present invention was to provide a simple and cost-effective method for treating porous substrates, with which substrates with high resistance and high surface quality can be obtained.

[0007] This object is achieved with respect to a method for treating porous substrates having the features of patent claim 1 and with respect to a treated substrate having the features of patent claim 12. Claim 18 specifies possible uses of the treated substrate according to the invention. The dependent claims represent advantageous developments.According to the invention, a method for the (surface) treatment of porous substrates is thus specified, in which a) at least one surface of a porous carbon-containing substrate is provided with at least one silicon coating by applying at least one aqueous suspension comprising silicon particles, at least one binder and water to the at least one surface and then subjecting it to a drying process, and b) the at least one silicon coating is subjected to at least one heat treatment in which the silicon coating melts to form a melt which infiltrates into the pores of the porous carbon-containing substrate, wherein silicon contained in the melt is at least partially converted into silicon carbide.

[0008] In step a) of the process according to the invention, at least one surface of a porous carbon-containing substrate is provided with at least one silicon coating. For this purpose, at least one aqueous suspension is applied to the at least one surface, and the applied at least one aqueous suspension is then subjected to a drying process. The at least one aqueous suspension comprises silicon particles, at least one binder, and water. Preferably, the at least one aqueous suspension can also consist of silicon particles, at least one binder, and water. The silicon particles contained in the at least one aqueous suspension are preferably silicon granules or silicon powder, particularly preferably silicon granules. The at least one aqueous suspension is preferably applied in layer form to the at least one surface.

[0009] A binder can generally be understood as a substance that creates or promotes chemical bonds at phase boundaries of other substances or that triggers or increases effects such as cohesion, adsorption, adhesion or friction.

[0010] The at least one binder leads to an increase in the viscosity and the yield point of the aqueous suspension so that it adheres to the at least one surface after it has been applied thereto.

[0011] The drying process can remove the water contained in the applied at least one aqueous suspension, resulting in a silicon coating arranged on the at least one surface, which comprises the silicon particles and the at least one binder, wherein the silicon particles are further fixed to the at least one surface by the at least one binder. The at least one binder can thus prevent the silicon particles from slipping on the at least one surface or falling from the at least one surface during or after the drying process (e.g. during transport of the substrate or due to an at least partially vertical, oblique or non-planar profile of the at least one surface). In other words, the at least one binder can ensure that the silicon coating present after the drying process is abrasion-resistant and adheres well.The distribution of the silicon particles on the at least one surface achieved during application of the at least one suspension is thus retained due to the at least one binder even during or after the drying process (up to melting in step b) of the process according to the invention).

[0012] In step b) of the process according to the invention, the at least one silicon coating obtained in step a) of the process according to the invention is then subjected to at least one heat treatment. During this heat treatment, the silicon coating melts into a melt that infiltrates into the pores of the porous carbon-containing substrate. The region(s) of the substrate into which the melt infiltrates can be referred to as the infiltration zone. Furthermore, during the heat treatment, silicon contained in the melt is at least partially converted into silicon carbide. Preferably, during the heat treatment, silicon contained in the melt is essentially completely, preferably completely, converted into silicon carbide.

[0013] Due to the (at least partial) conversion of the silicon into silicon carbide, the pores of the ultimately obtained substrate in the infiltration zone are at least partially filled with silicon carbide. As a result (with a sufficiently high infiltration depth), an almost complete closure, preferably a substantially complete closure, of the pores near the treated surface by chemically stable silicon carbide and thus an almost complete sealing, preferably a substantially complete sealing, of the treated surface of the substrate can be achieved, which can be demonstrated by the only low permeability of the substrates obtained by the process according to the invention and only low open porosity in the infiltration zone of the substrates obtained by the process according to the invention. The degree of sealing of the treated surface depends on the infiltration depth, i.e. the thickness of the infiltration zone.It should be noted that the degree of sealing achieved at a certain infiltration depth depends on the material and the properties of the substrate. Thus, depending on the material, a different infiltration depth may be necessary to achieve a certain degree of sealing of the surface. The thickness of the infiltration zone (or the infiltration depth) and thus the degree of sealing can be adjusted using various parameters (such as the amount per unit area of ​​the at least one aqueous suspension applied to the at least one surface, the proportion of silicon particles in the at least one aqueous suspension, the gas atmosphere during the at least one heat treatment, the temperature during the at least one heat treatment, the duration of the at least one heat treatment, and / or the process pressure during the at least one heat treatment). The thickness of the infiltration zone (orThe infiltration depth (the infiltration depth) can be, for example, at least 50 pm, preferably at least 100 pm, particularly preferably at least 200 pm. The degree of sealing can be determined by the permeability of the substrate and the open porosity in the infiltration zone. The lower the permeability of the substrate and the lower the open porosity in the infiltration zone, the higher the degree of sealing.

[0014] The method according to the invention is particularly characterized by the fact that the use of an aqueous suspension comprising silicon particles, at least one binder, and water enables a very defined silicon application, which both achieves the most complete sealing of the treated surface and at least largely prevents the formation of silicon residues on the surface of the substrate. A particular advantage of the method according to the invention is that, even with very dense and therefore poorly infiltrable materials or substrates, the most complete sealing of the treated surface is achieved, and the formation of silicon residues on the surface of the substrate can be at least largely avoided.

[0015] The highly defined silicon deposition is achieved in the process according to the invention by applying the silicon particles to at least one surface of the substrate using an aqueous suspension that additionally contains at least one binder. Applying the silicon particles using an aqueous suspension allows a very homogeneous distribution of the silicon particles on the at least one surface of the substrate, with the at least one binder ensuring that the aqueous suspension adheres to the at least one surface.In addition, the at least one binder ensures that the silicon particles continue to be fixed to the at least one surface after the water has been removed (through the drying process), so that the very homogeneous distribution of the silicon particles is maintained even after the water has been removed, even if the substrate is transported during the process or if the at least one surface is at least partially vertical, oblique, or non-planar. This ensures that the very homogeneous distribution of the silicon particles is maintained until the particles melt. The homogeneous distribution of the silicon particles ultimately achieves a very defined application of the silicon.This highly precise application allows a sufficiently high amount of silicon (using the aqueous suspension) to be applied to each individual area of ​​the surface to be treated, ultimately achieving sufficient sealing of the surface or adequate closure of the near-surface pores. On the other hand, the pore capacity for the silicon melt is not exceeded, thus largely preventing silicon residues on the treated surface. This highly precise silicon application is particularly advantageous for very dense and therefore difficult-to-infiltrate materials or substrates.

[0016] The substrates obtained by the process according to the invention exhibit both increased hardness and increased wear resistance due to the presence of silicon carbide in the pores in the infiltration zone of the substrate. For this reason alone, the durability of the substrates obtained by the process according to the invention is significantly increased.

[0017] Furthermore, since an almost or essentially complete sealing of the treated surface or an almost or essentially complete closure of the near-surface pores can be achieved, the penetration of gases or fluids into the material and, accordingly, interaction with corrosive media (e.g., oxygen), which would lead to degradation of the carbon material of the substrate, can be prevented. This also contributes to the high resistance of the substrates obtained with the process according to the invention.

[0018] It should be emphasized that the process according to the invention can achieve a better and more complete sealing of the treated surface than with prior art processes, such as processes in which coating is carried out using CVI. Consequently, the process according to the invention can be used to obtain substrates that have lower permeability and lower open porosity in the infiltration zone than substrates treated according to the prior art.

[0019] In addition, the process according to the invention also achieves a better or more complete sealing of the treated surface than with processes in which a coating is applied by applying silicon particles without using a suspension, or a coating is applied using a suspension with silicon particles but without water and / or binder. Consequently, the process according to the invention can be used to obtain substrates that have lower permeability and lower open porosity in the infiltration zone than substrates treated according to processes in which a coating is applied by applying silicon particles without using a suspension, or a coating is applied using a suspension with silicon particles but without water and / or binder.

[0020] At the same time, the substrates obtained with the process according to the invention are characterized by a high surface quality without the need for complex post-processing. Thus, the use of an aqueous suspension comprising silicon particles, at least one binder, and water in the process according to the invention enables a very defined silicon application, which at least largely prevents the deposition of silicon residues on the surface of the substrate, which would otherwise lead to a reduction in surface quality. Furthermore, complex post-processing to remove such silicon residues (e.g., an additional grinding or abrasive step to remove the silicon residues) can be dispensed with.

[0021] Since the method according to the invention does not require complex coating processes and technologies, such as CVD processes, and furthermore, post-processing of the substrates to remove silicon residues is not necessary, the method according to the invention can be carried out in a simple manner and is also cost-effective.

[0022] Thus, the method according to the invention provides a simple and cost-effective method for treating porous substrates, with which substrates with high resistance and high surface quality can be obtained.

[0023] A preferred variant of the process according to the invention is characterized in that the silicon particles have an average particle size (d50 value) in the range from 10 μm to 3500 μm, preferably from 310 μm to 1700 μm, particularly preferably from 500 to 1000 μm. Such an average particle size of the silicon particles makes it even easier to avoid silicon residues on the treated surface, so that the resulting substrate has an even higher surface quality. In particular, with a particle size of at least 310 μm, preferably of at least 500 μm, the silicon particles can be melted even more effectively during the infiltration process, and the resulting melt can be distributed even more efficiently over the surface to be treated. Thus, with appropriate dosing, the silicon melt can be absorbed completely, residue-free, and across the entire surface by the graphite substrate.In this way, silicon residues on the treated surface can be completely avoided, so that an even higher surface quality is achieved without the need for post-processing to remove silicon residues.

[0024] The mean particle size (d50 value) of the silicon particles can be determined, for example, by laser diffraction (e.g. according to ISO 13320:2020-01).

[0025] A further preferred variant of the process according to the invention is characterized in that the silicon particles have an average particle size (d50 or d50 value) of more than 500 pm and up to 3500 pm, preferably in the range from 550 pm to 3500 pm, particularly preferably in the range from 650 pm to 1700 pm, and most particularly preferably in the range from 750 pm to 1000 pm. The average particle size (d50 or d50 value) of the silicon particles can be determined, for example, by means of laser diffraction (e.g., according to ISO 13320:2020-01). A particle size of the silicon particles of more than 500 pm enables even more efficient melting of the silicon particles during the infiltration process than a smaller average particle size of up to 500 pm. Surprisingly, it was found that a larger particle size of the silicon particles leads to more efficient melting of the silicon particles.In particular, with an average particle size of the silicon particles of more than 500 pm and up to 3500 pm, e.g. in the range of 550 pm to 3500 pm, complete melting of the silicon particles can be ensured, so that the silicon (with appropriate dosage) can be absorbed by the substrate completely without leaving any residue. In this way, a highly crystalline and crack- and pore-free surface can be achieved. Ultimately, an excellent surface quality is achieved without the need for post-processing to remove silicon residues. Fundamentally, it was surprisingly found that finer Si material tends to have a lower capacity for complete melting. A crucial aspect here is the high specific surface area, which typically increases with decreasing particle size.Firstly, in the case of Si, there is increased oxidation of the surface in air but also in contact with water during suspension production and processing. The resulting silicon oxide layer on the particle surface subsequently impairs the formation of a molten phase and thus inhibits the infiltration process. To avoid this, the powder can be freed of the oxide layer using chemical (e.g. treatment with hydrofluoric acid HF) or thermal processes. However, this is technically complex and not feasible for a Si-based coating. Furthermore, a high specific surface area can react with free carbon from the furnace atmosphere or residues of the carbon-based organic suspension additives (e.g. binders) close to the surface before the actual melting to form SiC.The melting of the particles only takes place partially and not completely, leaving cracked and porous structures.

[0026] A further preferred variant of the process according to the invention is characterized in that the silicon particles have an average particle size (d50 or d50 value) of 800 pm, or an average particle size (d50 or d50 value) of more than 500 pm and up to 3500 pm, preferably in the range from 550 pm to 3500 pm, particularly preferably in the range from 650 pm to 1700 pm, very particularly preferably in the range from 750 pm to 1000 pm, wherein the average particle size (d50 or d50 value) of the silicon particles is not 800 pm.

[0027] A further preferred variant of the process according to the invention is characterized in that the silicon particles have an average particle size (d50 or d50 value) of more than 500 pm and less than 800 pm, preferably at least 550 pm and less than 800 µm, particularly preferably of at least 650 µm and less than 800 µm, very particularly preferably of at least 700 µm and less than 800 µm, or have an average particle size (d50 or d50 value) of 800 µm, or have an average particle size (d50 or d50 value) of more than 800 µm and up to 3500 µm, preferably of more than 800 µm and up to 1700 µm, particularly preferably of more than 800 µm and up to 1000 µm.

[0028] The mean particle size (d50 or d50 value) of the silicon particles can be determined, for example, by laser diffraction (e.g. according to ISO 13320:2020-01).

[0029] A further preferred variant of the process according to the invention is characterized in that the silicon particles have a tendency to oxidize, which is characterized in that upon contact of the silicon particles with water over a period of 24 hours, an amount of hydrogen (Hz) is released which is less than 5 • 10 -5 Vol.-%. The measurement can be carried out, for example, using a hydrogen measuring probe at a distance of 1 cm from the suspension surface. The silicon particles therefore have a very low tendency to oxidize (upon contact with water). The oxidation tendency of the silicon particles upon contact with water can be determined via the release of hydrogen H2. According to the reaction Si + 2 SiO2 + 2 Fh, the water molecule is split during the oxidation of Si. This reaction is further promoted with increasing specific surface area or decreasing particle size.

[0030] A further preferred variant of the method according to the invention is characterized in that the at least one binder ensures an adhesive strength of the silicon coating of at least 0.15 MPa, and / or is selected from the group consisting of polyvinyl alcohol, polyethylene glycol, polyvinyl butyral, polyacrylic acid, polyurethane, chloroprene rubber, phenolic resin, acrylic resin, cellulose, cellulose derivatives, alginic acid, dextrin, and mixtures thereof.

[0031] The adhesion strength of the silicon coating can be determined, for example, by means of a tear-off test according to DIN EN ISO 4624:2016-08.

[0032] Preferably, the at least one binder is at least one organic binder. Particularly preferably, the at least one binder is selected from the group consisting of polyvinyl alcohol, polyethylene glycol, polyvinyl butyral, polyacrylic acid, polyurethane, chloroprene rubber, phenolic resin, acrylic resin, cellulose, cellulose derivatives, alginic acid, dextrin, and mixtures thereof. Such a binder can achieve particularly high adhesive strength of the silicon coating.

[0033] The cellulose derivatives are preferably selected from the group consisting of cellulose ether, methylcellulose, carboxymethylcellulose, ethylcellulose, hydroxyethylcellulose, hydroxypropylcellulose and mixtures thereof.

[0034] For example, the product “Peptapon 520” from Zschimmer & Schwarz Chemie GmbH can be used as a binding agent.

[0035] A further preferred variant of the process according to the invention is characterized in that the at least one aqueous suspension

[0036] 1 to 50 wt.%, preferably 5 to 35 wt.%, of the silicon particles, based on the total weight of the at least one aqueous suspension, and / or

[0037] 0.01 to 10 wt.%, preferably 0.03 to 3 wt.%, particularly preferably 0.05 to 0.3 wt.%, of the at least one binder, based on the total weight of the at least one aqueous suspension.

[0038] The amount of silicon applied can be varied by varying the proportion of silicon particles in the at least one aqueous suspension. A particularly advantageous adhesion effect can be achieved by using 0.01 to 3 wt.%, preferably 0.05 to 0.3 wt.%, of the at least one binder, based on the total weight of the at least one aqueous suspension.

[0039] According to a further preferred variant of the process according to the invention, the at least one aqueous suspension is applied in step a) by dipping, brushing, doctor blade coating, and / or spray application. More preferably, the at least one aqueous suspension is applied in step a) by spray application. Using these methods, flat, three-dimensional, and complex components can be homogeneously coated with the at least one aqueous suspension in a particularly simple manner. A particularly homogeneous application is possible using spray application. Furthermore, using the methods mentioned, in particular spray application, the amount of suspension applied and thus the amount of silicon per unit area can be adjusted very precisely, thereby enabling an even more defined application of the at least one aqueous suspension and thus the amount of silicon.The amount of suspension applied can also be influenced by the number of coating cycles.

[0040] Preferably, by applying the at least one aqueous suspension in step a), a silicon quantity (or a quantity of silicon particles) of 0.003 to 0.5 g / cm 2 , preferably from 0.01 to 0.2 g / cm 2 , particularly preferably from 0.02 to 0.1 g / cm 2 , most preferably from 0.03 to 0.08 g / cm 2 , especially from 0.04 to 0.07 g / cm 2 , applied to at least one surface.

[0041] Preferably, in step a) an amount of the aqueous suspension of 0.001 g / cm 2 up to 1.5 g / cm 2 , preferably 0.005 g / cm 2 up to 0.5 g / cm 2 , particularly preferably 0.06 g / cm 2 up to 0.4 g / cm 2 , applied to at least one surface.

[0042] A further preferred variant of the process according to the invention is characterized in that the drying process takes place at a temperature in the range from 10 °C to 200 °C, preferably from 80 °C to 100 °C, and / or over a period of 5 h to 48 h, preferably from 10 h to 12 h. A further preferred variant of the process according to the invention is characterized in that the at least one heat treatment takes place at a temperature in the range from 1400 °C to 1800 °C, preferably from 1450 °C to 1550 °C, and / or over a period of 1 h to 10 h, preferably from 4 h to 6 h, and / or under o vacuum or o inert gas atmosphere, preferably argon atmosphere, at a (process) pressure of 10 mbar to 2000 mbar, preferably from 100 mbar to 1800 mbar, particularly preferably from 500 mbar to 1500 mbar, very particularly preferably from 800 mbar to 1200 mbar.

[0043] A further preferred variant of the method according to the invention is characterized in that the at least one heat treatment takes place at a temperature in the range from 1400 °C to 1800 °C, preferably from 1450 °C to 1550 °C, and / or over a period of 1 h to 10 h, preferably from 4 h to 6 h, and / or under an inert gas atmosphere, preferably an argon atmosphere, and / or at a (process) pressure of 10 mbar to 2000 mbar, preferably from 100 mbar to 1800 mbar, particularly preferably from 500 mbar to 1500 mbar, very particularly preferably from 800 mbar to 1200 mbar.

[0044] By varying the gas atmosphere, the temperature, the duration and / or the process pressure, the thickness of the infiltration zone (or the infiltration depth) and thus the degree of sealing can be influenced and adjusted. A further preferred variant of the method according to the invention is characterized in that the porous carbonaceous substrate contains or consists of a material selected from the group consisting of graphite, preferably iso-graphite; carbon fiber reinforced carbon; silicon carbide fiber reinforced carbon; silicon carbide fiber reinforced silicon carbide; glassy carbon; sintered silicon carbide; silicon infiltrated silicon carbide; and combinations thereof, and / or the porous carbonaceous substrate contains or consists of a material which has a thermal expansion coefficient (or a heat expansion coefficient) of at least 2.0 • 10 -6 K 1, preferably at least 2.8 • IO -6 K 1 , particularly preferably at least 3.0 • IO -6 K 1 , most preferably at least 3.2 • IO -6 K 1 , and / or the porous carbonaceous substrate has an open porosity, measured by means of mercury porosimetry, of at least 12%, preferably from 12% to 30%, particularly preferably from 14% to 25%, very particularly preferably from 15% to 20%, and / or the pores of the porous carbonaceous substrate have an average pore diameter in the range from 0.1 pm to 100 pm, preferably from 0.1 pm to 10 pm, particularly preferably from 1 pm to 5 pm, very particularly preferably from 1.5 pm to 5 pm.

[0045] The porous carbonaceous substrate preferably contains graphite, particularly preferably iso-graphite.

[0046] The porous carbonaceous substrate is preferably a porous graphite substrate, particularly preferably a porous iso-graphite substrate. The process according to the invention is particularly advantageous for graphite substrates, especially iso-graphite substrates, since these have a high density and are therefore difficult to infiltrate. Due to the very precise application of the aqueous suspension and the resulting advantages, these substrates can also be treated without problems using the process according to the invention. Iso-graphite refers to graphite produced by the isostatic pressing process.

[0047] For example, the porous substrate may be a crucible, preferably a graphite crucible, most preferably an iso-graphite crucible.

[0048] Preferably, the porous carbonaceous substrate contains or consists of a material which has a thermal expansion coefficient (or a thermal expansion coefficient) of at least 2.8 • IO -6 K 1 , preferably at least 3.0 • IO -6 K 1 , particularly preferably at least 3.2 • IO -6 K 1 ,. In this way, the risk of cracking and deformation of the substrate during the process can be reduced.

[0049] The thermal expansion coefficient (or heat expansion coefficient) can be determined, for example, according to DIN 51909:2009-05.

[0050] During the infiltration of liquid silicon into a carbonaceous substrate, a chemical reaction between silicon and carbon occurs to form silicon carbide (SiC), resulting in the formation of SiC in the pores. The associated increase in volume during SiC formation induces mechanical stresses in the carbonaceous material, which increase with increasing infiltration depth. In addition, with the increasing difference between the thermal expansion coefficients of the carbonaceous material and SiC, thermal stresses can also occur during heat treatment. If the mechanical stability of the carbonaceous material is exceeded, cracking can occur in the substrate and thus the destruction of the component. By using a carbonaceous material with high mechanical stability, e.g.Characterized by high flexural strength and / or high compressive strength, the risk of cracking and deformation of the substrate can be reduced. Likewise, the risk of cracking and deformation of the substrate can be reduced if the carbonaceous material has a suitable thermal expansion coefficient, i.e., a thermal expansion coefficient with as little difference as possible from the thermal expansion coefficient of silicon carbide.Preferably, the porous carbonaceous substrate contains or consists of a material which has a flexural strength of at least 30 MPa, preferably of at least 45 MPa, particularly preferably of at least 50 MPa, very particularly preferably of at least 60 MPa, in particular of at least 70 MPa and / or a compressive strength of at least 50 MPa, preferably of at least 90 MPa, particularly preferably of at least 110 MPa, very particularly preferably of at least 130 MPa, in particular of at least 140 MPa.

[0051] It is preferred that the porous carbonaceous substrate has an open porosity, measured by mercury porosimetry, of at least 12%, preferably from 12% to 30%, particularly preferably from 14% to 25%, most preferably from 15% to 20%, and / or that the pores of the porous carbonaceous substrate have an average pore diameter in the range from 0.1 pm to 10 pm, preferably from 1 pm to 5 pm, particularly preferably from 1.5 pm to 5 pm. In this way, a particularly good closure of the near-surface pores or a particularly good sealing of the treated surface can be achieved, which is demonstrated by a very low permeability of the substrate and only a very low open porosity in the infiltration zone.It is particularly advantageous if the porous carbonaceous substrate has an open porosity, measured by means of mercury porosimetry, of at least 12%, preferably from 12% to 30%, particularly preferably from 14% to 25%, very particularly preferably from 15% to 20%, and the pores of the porous carbonaceous substrate have an average pore diameter in the range from 0.1 pm to 10 pm, preferably from 1 pm to 5 pm, particularly preferably from 1.5 pm to 5 pm.

[0052] The open porosity of the porous carbonaceous substrate is determined by mercury porosimetry (e.g. according to DIN 66133:1993-06).

[0053] The average pore diameter of the pores of the porous carbonaceous substrate can be determined, for example, using mercury porosimetry (e.g., according to DIN 15901-1:2019-03). Preferably, the infiltration depth of the melt (or the thickness of the infiltration zone) is adjusted by the amount per unit area of ​​the at least one aqueous suspension applied to the at least one surface, and / or the proportion of silicon particles in the at least one aqueous suspension, and / or the gas atmosphere during the at least one heat treatment, and / or the temperature during the at least one heat treatment, and / or the duration during the at least one heat treatment, and / or the process pressure during the at least one heat treatment. The degree of sealing of the treated surface can be adjusted via the thickness of the infiltration zone or the infiltration depth of the melt.

[0054] According to a further preferred variant of the method according to the invention, the infiltration depth of the melt (or the thickness of the infiltration zone) is adjusted by the amount per unit area of ​​the at least one aqueous suspension applied to the at least one surface and / or by the pressure during the at least one heat treatment. The degree of sealing of the treated surface can be adjusted via the thickness of the infiltration zone or the infiltration depth of the melt.

[0055] According to a particularly preferred process variant, the infiltration depth of the melt (or the thickness of the infiltration zone) is adjusted by the atmospheric pressure, preferably the argon atmosphere, during at least one heat treatment. In this case, the infiltration depth can also be influenced independently of the carbon-containing material by selecting the appropriate process pressure.

[0056] A further preferred variant of the method according to the invention is characterized in that after step b) at least one aqueous suspension containing at least one refractory metal carbide (e.g. tantalum carbide) and water is applied to the at least one surface of the carbon-containing substrate and the substrate is subsequently subjected to a sintering process.

[0057] A further preferred variant of the method according to the invention is characterized in that the porous carbon-containing substrate is doped with at least one dopant selected from the group consisting of nitrogen (N), aluminum (Al), boron (B), phosphorus (P), vanadium (V), scandium (Sc), gallium (Ga), indium (In), germanium (Ge), tin (Sn), lead (Pb), arsenic (As), antimony (Sb), bismuth (Bi), and mixtures thereof, wherein the at least one dopant is preferably selected from the group consisting of nitrogen (N), aluminum (Al), boron (B), phosphorus (P), vanadium (V), scandium (Sc), and mixtures thereof, and / or the silicon particles are doped with at least one dopant selected from the group consisting of nitrogen (N), aluminum (Al), boron (B), phosphorus (P), vanadium (V), scandium (Sc), gallium (Ga), indium (In), germanium (Ge), tin (Sn), lead (Pb), arsenic (As), antimony (Sb), bismuth (Bi), and mixtures thereof,wherein the at least one dopant is preferably selected from the group consisting of nitrogen (N), aluminum (Al), boron (B), phosphorus (P), vanadium (V), scandium (Sc), and mixtures thereof, and / or the at least one aqueous suspension additionally comprises at least one (powdered and / or water-soluble) compound containing at least one dopant selected from the group consisting of nitrogen (N), aluminum (Al), boron (B), phosphorus (P), vanadium (V), scandium (Sc), gallium (Ga), indium (In), germanium (Ge), tin (Sn), lead (Pb), arsenic (As), antimony (Sb), bismuth (Bi), and mixtures thereof, wherein the at least one dopant is preferably selected from the group consisting of nitrogen (N), aluminum (Al), boron (B), phosphorus (P), vanadium (V), scandium (Sc), and mixtures thereof, and / or the at least one heat treatment is carried out in the presence of a process gas that contains or consists of nitrogen.

[0058] In this way, at least one dopant or doping element can be incorporated into the silicon carbide produced in step b), ie the silicon carbide is doped with the at least one dopant.

[0059] The at least one (powdered and / or water-soluble) compound is preferably at least one (powdered and / or water-soluble) salt.

[0060] By incorporating one or more dopants or doping elements into the (e.g., polycrystalline) silicon carbide produced in step b), the electrical and / or thermal properties of the treated substrate can be varied or specifically adjusted. Material parameters that can be adjusted in this way include, for example, the (specific) resistance, electrical conductivity, and thermal conductivity of the silicon carbide. Depending on the selection and concentration of the respective doping element, the electrical conductivity and thermal conductivity can also be adjusted independently of each other.

[0061] The doping of the silicon carbide can be achieved in various ways, namely via the silicon particles, via the carbon-containing substrate, via an additional compound contained in the suspension, and / or via a process gas. For example, silicon (Si) doped with the corresponding dopant(s) can be used as the starting material for the infiltration process, i.e., the silicon particles used are doped with the corresponding dopant(s). In principle, some of the listed silicon carbide dopants, such as B, P, N, Ga, As, Sb, and Al, are also established in Si crystal growth, and such doped material is available in a wide variety of dopant concentrations. With the melting and formation reaction of silicon carbide during infiltration, the dopants introduced by the Si material can also be incorporated into the resulting silicon carbide.In the case of nitrogen (N), the introduction can also occur via the gas phase. If N (or N2) is used as the process gas during the infiltration process in the presence of a molten Si phase, or if it is partially mixed with the process gas, N is dissolved in the melt.

[0062] Another possibility is to introduce the corresponding dopant(s) into the coating suspension in the form of (powdered and / or water-soluble) compounds (e.g., salts). Using the spraying process, these can be homogeneously distributed over the substrate surface, similar to the Si material, and dissolved in the liquid Si during melting or absorbed directly as a dopant during the silicon carbide formation reaction.

[0063] Additionally, the starting material of the carbonaceous substrate (e.g., graphite) can be provided with the appropriate dopant(s) prior to the silicon coating process. These can be mixed with the raw materials during the actual manufacturing process of the substrate material, for example, or the processed substrate material can be impregnated with dopant compounds using a solution, colloid, or suspension. During the reaction of the Si melt with the substrate material, these dopant compounds can then be absorbed into the Si melt and / or the resulting silicon carbide.

[0064] A general advantage of producing doped silicon carbide by means of silicon infiltration is that a more homogeneous p-type doping can potentially be achieved, which cannot be achieved in crystal growth using conventional methods. Preferably, the at least one dopant can therefore be at least one p-type dopant, which is particularly preferably selected from the group consisting of aluminum (Al), boron (B), vanadium (V), scandium (Sc), gallium (Ga), indium (In), and mixtures thereof, wherein the at least one p-type dopant is very particularly preferably selected from the group consisting of aluminum (Al), boron (B), vanadium (V), scandium (Sc), and mixtures thereof.

[0065] Furthermore, it is also possible, for example, through the use of the suspension-based spraying process, to locally coat defined sample areas with dopant-containing silicon coatings. This also makes it possible to generate defined regions with and without doping, or regions with different dopant concentrations or doping elements, within a component.

[0066] The present invention also relates to a substrate or (surface-)treated substrate comprising a carbon-containing substrate material with pores, wherein the substrate has an infiltration zone on at least one surface, in which the pores of the substrate material are at least partially filled with silicon carbide, wherein the substrate or treated substrate has a (gas) permeability of at most 5 • 10 15 m 2and wherein the substrate or treated substrate in the infiltration zone has an open porosity, determined by mercury porosimetry, of a maximum of 10%.

[0067] The (gas) permeability of the treated substrate can be determined, for example, using the differential pressure method (e.g. according to EN 993-4 : 1995).

[0068] The open porosity in the infiltration zone of the treated substrate is determined by mercury porosimetry (e.g. according to DIN 66133:1993-06).

[0069] The infiltration zone is ultimately the area(s) of the treated substrate in which silicon carbide is present in the pores of the substrate material. In the area(s) of the treated substrate outside the infiltration zone, no silicon carbide is present in the pores of the substrate material. The infiltration zone thus extends from the at least one surface of the treated substrate to the point(s) on the treated substrate furthest from the at least one surface, up to which point(s) silicon carbide is present in the pores of the substrate material (continuously from the at least one surface).

[0070] Preferably, the proportion of elemental silicon deposited on the at least one surface, based on the total weight of the treated substrate, is a maximum of 0.01 wt.%, particularly preferably a maximum of 0.001 wt.%. Preferably, the treated substrate has no residues of elemental silicon particles with a particle diameter of at least 500 μm on the at least one surface. The particle size of the silicon particles can be determined, for example, by laser diffraction (e.g., according to ISO 13320:2020-01).

[0071] Particularly preferably, the treated substrate has no residues of elemental silicon (or no elemental silicon) on the at least one surface.

[0072] Most preferably, the treated substrate contains no residues of elemental silicon (or no elemental silicon).

[0073] Preferably, the pores of the substrate material in the infiltration zone are not filled (or partially filled) with any substance other than silicon carbide.

[0074] Preferably, the pores of the substrate material in the infiltration zone are completely filled with silicon carbide

[0075] A preferred embodiment of the treated substrate according to the invention is characterized in that the treated substrate has a permeability of maximum 1 • 10 16 m 2 , preferably from a maximum of 1 • 10 17 m 2 , particularly preferably a maximum of 1 • 10 19 m 2, and / or has a permeability which is lower by a factor of at least 10, preferably of at least 100, than (or the) permeability of the substrate before treatment, and / or has an open porosity in the infiltration zone, determined by means of mercury porosimetry, of a maximum of 8%, preferably a maximum of 5%, and / or has an open porosity in the infiltration zone, determined by means of mercury porosimetry, which is at least 7%, preferably at least 10%, particularly preferably at least 12%, based on the total volume of the treated substrate, lower than (or the) open porosity (determined by means of mercury porosimetry) of the treated substrate outside the infiltration zone, and / or has a specific resistance of a maximum of 1500 mΩcm, preferably of a maximum of 10 mΩcm, and / or has no elemental silicon.

[0076] The (gas) permeability of the treated substrate and / or the (gas) permeability of the substrate before treatment can be determined, for example, using differential pressure methods (e.g. according to EN 993-4 : 1995).

[0077] The presence of the feature that the treated substrate has a permeability which is at least 10-fold, preferably at least 100-fold, lower than the permeability of the substrate before treatment can, for example, be determined solely on the treated substrate by first determining the permeability of the treated substrate, e.g. using a differential pressure method (e.g. in accordance with EN 993-4:1995), then removing the infiltration zone from the treated substrate, e.g. by grinding, then determining the permeability of the substrate thus obtained without the infiltration zone, e.g. using a differential pressure method (e.g. in accordance with EN 993-4:1995), and finally comparing the two determined permeabilities or setting them in an appropriate ratio. The permeability of the treated substrate from which the infiltration zone was removed corresponds to the permeability of the untreated substrate.

[0078] The open porosity in the infiltration zone of the treated substrate and the open porosity of the treated substrate outside the infiltration zone are determined by mercury porosimetry (e.g. according to DIN 66133:1993-06).

[0079] The open porosity of the treated substrate outside the infiltration zone corresponds to the open porosity of the untreated substrate (also in the region of the subsequent infiltration zone). A further preferred embodiment of the treated substrate according to the invention is characterized in that the infiltration zone has an average thickness of at least 100 μm, preferably from 100 μm to 1200 μm, particularly preferably from 200 μm to 800 μm, and / or the silicon carbide with which the pores of the substrate material in the infiltration zone are at least partially filled contains 3C-SiC (3C silicon carbide), preferably has 3C-SiC (3C silicon carbide) as the main phase.

[0080] The (average) thickness of the infiltration zone can also be referred to as the (average) infiltration depth. In other words, the average infiltration depth is preferably in a range of at least 100 pm, preferably from 100 pm to 1200 pm, particularly preferably from 200 pm to 800 pm. The thickness of the infiltration zone, or infiltration depth, extends from the treated surface to the edge of the infiltration zone opposite the treated surface.

[0081] The average thickness of the infiltration zone or the average infiltration depth can be determined, for example, by taking individual measurements of the thickness of the infiltration zone or the infiltration depth at various locations distributed across the entire length and / or width of the infiltration zone using optical microscopy on cross-sections (vertical to the infiltration direction) and then calculating an average of the individual measurements. The thickness of the infiltration zone or the infiltration depth can be averaged over the entire length and / or width of the infiltration zone.

[0082] The mean thickness of the infiltration zone or the mean infiltration depth can be determined, for example, according to DIN EN ISO 1463:2021-08.

[0083] The fact that the silicon carbide with which the pores of the substrate material in the infiltration zone are at least partially filled contains 3C-SiC can be determined, for example, by X-ray diffraction (XRD). Preferably, the silicon carbide with which the pores of the substrate material in the infiltration zone are at least partially filled has 3C-SiC (3C silicon carbide) as its main phase.

[0084] The fact that the silicon carbide with which the pores of the substrate material in the infiltration zone are at least partially filled has 3C-SiC as the main phase means that the silicon carbide with which the pores of the substrate material in the infiltration zone are at least partially filled has a 3C-silicon carbide phase and has no further phases which have a higher weight percentage of the total silicon carbide with which the pores of the substrate material in the infiltration zone are at least partially filled than the 3C-silicon carbide phase.

[0085] The fact that the silicon carbide with which the pores of the substrate material in the infiltration zone are at least partially filled has 3C-SiC as the main phase can be determined, for example, by X-ray diffraction (XRD).

[0086] 3C-SiC (3C-silicon carbide) can also be called ß-SiC (ß-silicon carbide).

[0087] Preferably, the silicon carbide with which the pores of the substrate material in the infiltration zone are at least partially filled has a proportion of at least 50 wt.%, preferably a proportion of at least 70 wt.%, particularly preferably a proportion of at least 90 wt.%, very particularly preferably a proportion of at least 95 wt.%, for example a proportion of at least 99 wt.%, of 3C-SiC (3C-silicon carbide) or ß-SiC (ß-silicon carbide).

[0088] The silicon carbide with which the pores of the substrate material in the infiltration zone are at least partially filled preferably has a proportion of at most 5 wt.%, preferably a proportion of at most 1 wt.%, particularly preferably a proportion of at most 0.1 wt.%, of a-SiC (a-silicon carbide). Most preferably, the silicon carbide with which the pores of the substrate material in the infiltration zone are at least partially filled does not contain a-SiC (a-silicon carbide). The proportion of 3C-SiC or ß-SiC and / or the proportion of a-SiC in the silicon carbide with which the pores of the substrate material in the infiltration zone are at least partially filled can be determined, for example, by means of X-ray diffraction (XRD).

[0089] A particularly preferred embodiment of the substrate according to the invention is characterized in that the infiltration zone has an average thickness of at least 100 pm (e.g. 100 pm to 1200 pm), preferably of at least 200 pm (e.g. 200 pm to 800 pm), and the silicon carbide with which the pores of the substrate material in the infiltration zone are at least partially filled contains ß-SiC (or 3C-SiC), preferably has ß-SiC (or 3C-SiC) as the main phase.

[0090] The fact that the silicon carbide with which the pores of the substrate material in the infiltration zone are at least partially filled has ß-SiC (or 3C-SiC) as the main phase can be determined, for example, by means of X-ray diffraction (XRD).

[0091] A further preferred embodiment of the treated substrate according to the invention is characterized in that the carbonaceous material is selected from the group consisting of graphite, preferably iso-graphite; carbon fiber reinforced carbon; silicon carbide fiber reinforced carbon; silicon carbide fiber reinforced silicon carbide; sintered silicon carbide; glassy carbon; and combinations thereof.

[0092] A further preferred embodiment of the treated substrate according to the invention is characterized in that the silicon carbide is doped with at least one dopant selected from the group consisting of nitrogen (N), aluminum (Al), boron (B), phosphorus (P), vanadium (V), scandium (Sc), gallium (Ga), indium (In), germanium (Ge), tin (Sn), lead (Pb), arsenic (As), antimony (Sb), bismuth (Bi), and mixtures thereof, wherein the at least one dopant is preferably selected from the group consisting of nitrogen (N), aluminum (Al), boron (B), phosphorus (P), vanadium (V), scandium (Sc), and mixtures thereof, and / or in the infiltration zone in a concentration in the range of 1 • IO 10 Atoms per cm 3 up to 1 • 10 23 Atoms per cm 3 , preferably in the range of 1 • 10 12 Atoms per cm 3 up to 1 • 10 21 Atoms per cm 3 , particularly preferably in the range of 1 • 10 15 Atoms per cm3 up to 1 • 10 18 Atoms per cm 3 , is present.

[0093] By incorporating one or more dopants or doping elements into the (e.g., polycrystalline) silicon carbide, the electrical and / or thermal properties of the treated substrate can be varied or specifically adjusted. Material properties that can be adjusted in this way include, for example, the (specific) resistivity, electrical conductivity, and thermal conductivity of the silicon carbide. Depending on the selection and concentration of the respective doping element, electrical and thermal conductivity can also be adjusted independently of each other.

[0094] Preferably, the at least one dopant can be at least one p-type dopant, which is particularly preferably selected from the group consisting of aluminum (Al), boron (B), vanadium (V), scandium (Sc), gallium (Ga), indium (In), and mixtures thereof, wherein the at least one p-type dopant is very particularly preferably selected from the group consisting of aluminum (Al), boron (B), vanadium (V), scandium (Sc), and mixtures thereof.

[0095] A further preferred embodiment of the treated substrate according to the invention is characterized in that the treated substrate has on each surface (or over the entire surface of the substrate) the infiltration zone in which the pores of the substrate material are at least partially filled with silicon carbide, and / or has an oxidation resistance which is characterized in that, after exposure of the treated substrate for at least 100 h, preferably for at least 150 h, particularly preferably for at least 162 h, at 1100 °C to synthetic air (200 ml / min, 1 bar), a mass decrease of the treated substrate (compared to the treated substrate before exposure to synthetic air) is less than 1 • 10 -4 g / cm 2 , preferably less than 2.5 • 10 -5 g / cm 2(based on the total surface of the treated substrate). A further preferred embodiment of the treated substrate according to the invention is characterized in that the treated substrate can be produced or is produced using the method according to the invention.

[0096] A further preferred embodiment of the treated substrate according to the invention is characterized in that at least one protective layer containing at least one refractory metal carbide (e.g., tantalum carbide) is arranged on the at least one surface on which the substrate has an infiltration zone. Preferably, the at least one protective layer is a refractory metal carbide layer (e.g., a tantalum carbide layer).

[0097] The present invention further relates to the use of the treated substrate according to the invention as a component for high-temperature furnaces, preferably a heater, insulation component, holder; as a crucible or crucible element.

[0098] The present invention also relates to the following aspects:

[0099] Aspect 1

[0100] A method for treating porous substrates, in which a) at least one surface of a porous carbon-containing substrate is provided with at least one silicon coating by applying at least one aqueous suspension comprising silicon particles, at least one binder and water to the at least one surface and then subjecting it to a drying process, and b) the at least one silicon coating is subjected to at least one heat treatment in which the silicon coating melts to form a melt which infiltrates into pores of the porous carbon-containing substrate, wherein silicon contained in the melt is at least partially converted into silicon carbide.

[0101] Aspect 2 Process according to the preceding aspect, characterized in that the silicon particles have an average particle size in the range from 10 pm to 3500 pm, preferably from 310 pm to 1700 pm, particularly preferably from 500 to 1000 pm.

[0102] Aspect 3

[0103] Method according to one of the preceding aspects, characterized in that the at least one binder ensures an adhesive strength of the silicon coating of at least 0.15 MPa, and / or is selected from the group consisting of polyvinyl alcohol, polyethylene glycol, polyvinyl butyral, polyacrylic acid, polyurethane, chloroprene rubber, phenolic resin, acrylic resin, cellulose, cellulose derivatives, alginic acid, dextrin, and mixtures thereof.

[0104] Aspect 4

[0105] Method according to one of the preceding aspects, characterized in that the at least one aqueous suspension

[0106] 1 to 50 wt.%, preferably 5 to 35 wt.%, of the silicon particles, based on the total weight of the at least one aqueous suspension, and / or

[0107] 0.01 to 3 wt.%, preferably 0.05 to 0.3 wt.%, of the at least one binder, based on the total weight of the at least one aqueous suspension.

[0108] Aspect 5

[0109] Method according to one of the preceding aspects, characterized in that the application of the at least one aqueous suspension in step a) is carried out by dipping, brushing, doctoring and / or spraying, preferably by spraying.

[0110] Aspect 6

[0111] Method according to one of the preceding aspects, characterized in that the drying process takes place at a temperature in the range from 10 °C to 200 °C, preferably from 80 °C to 100 °C, and / or over a period of from 5 h to 48 h, preferably from 10 h to 12 h.

[0112] Aspect 7

[0113] Method according to one of the preceding aspects, characterized in that the at least one heat treatment takes place at a temperature in the range from 1400 °C to 1800 °C, preferably from 1450 °C to 1550 °C, and / or over a period of 1 h to 10 h, preferably from 4 h to 6 h, and / or under vacuum or under an inert gas atmosphere, preferably an argon atmosphere, at a (process) pressure of 10 mbar to 2000 mbar, preferably from 100 mbar to 1800 mbar, particularly preferably from 500 mbar to 1500 mbar, very particularly preferably from 800 mbar to 1200 mbar.

[0114] Aspect 8

[0115] Method according to one of the preceding aspects, characterized in that the porous carbonaceous substrate contains or consists of a material which is selected from the group consisting of graphite, preferably iso-graphite; carbon fiber reinforced carbon; silicon carbide fiber reinforced carbon; silicon carbide fiber reinforced silicon carbide; glassy carbon; sintered silicon carbide; silicon infiltrated silicon carbide; and combinations thereof, and / or the porous carbonaceous substrate contains or consists of a material which has a thermal expansion coefficient of at least 2.8 • IO -6 K 1 , preferably at least 3.0 • IO -6 K 1 , particularly preferably at least 3.2 • IO -6 K 1, and / or the porous carbonaceous substrate has an open porosity, measured by means of mercury porosimetry, of at least 12%, preferably from 12% to 30%, particularly preferably from 14% to 25%, most preferably from 15% to 20%, and / or the pores of the porous carbonaceous substrate have an average pore diameter in the range from 0.1 pm to 10 pm, preferably from 1 pm to 5 pm, particularly preferably from 1.5 pm to 5 pm.

[0116] Aspect 9

[0117] Method according to one of the preceding aspects, characterized in that the infiltration depth of the melt is adjusted by the amount per unit area of ​​the at least one aqueous suspension applied to the at least one surface and / or by the pressure during the at least one heat treatment.

[0118] Aspect 10

[0119] Treated substrate comprising a carbonaceous substrate material with pores, wherein the substrate has an infiltration zone on at least one surface, in which the pores of the substrate material are at least partially filled with silicon carbide, wherein the treated substrate has a permeability of at most 5 • 10 15 m 2 and wherein the treated substrate in the infiltration zone has an open porosity, determined by mercury porosimetry, of a maximum of 10%.

[0120] Aspect 11

[0121] Treated substrate according to aspect 10, characterized in that the treated substrate has a permeability of at most 1 • 10 16 m 2 , preferably from a maximum of 1 • 10 17 m 2 , particularly preferably a maximum of 1 • 10 19 m 2, and / or has a permeability which is lower by a factor of at least 10, preferably at least 100, than a permeability of the substrate before the treatment, and / or has an open porosity in the infiltration zone, determined by means of mercury porosimetry, of a maximum of 8%, preferably a maximum of 5%, and / or has an open porosity in the infiltration zone, determined by means of mercury porosimetry, which is at least 7%, preferably at least 10%, particularly preferably at least 12%, based on the total volume of the treated substrate, lower than an open porosity of the treated substrate outside the infiltration zone, and / or has a specific resistance of a maximum of 1500 mΩcm, preferably of a maximum of 10 mΩcm, and / or has no elemental silicon.

[0122] Aspect 12

[0123] Treated substrate according to aspect 10 or 11, characterized in that the infiltration zone has an average thickness of at least 100 pm, preferably from 100 pm to 1200 pm, particularly preferably from 200 pm to 800 pm, and / or the silicon carbide with which the pores of the substrate material in the infiltration zone are at least partially filled contains 3C-SiC, preferably has 3C-SiC as the main phase.

[0124] Aspect 13

[0125] Treated substrate according to any one of aspects 10 to 12, characterized in that the carbonaceous material is selected from the group consisting of graphite, preferably iso-graphite; carbon fiber reinforced carbon; silicon carbide fiber reinforced carbon; silicon carbide fiber reinforced silicon carbide; sintered silicon carbide; glassy carbon; and combinations thereof.

[0126] Aspect 14

[0127] Treated substrate according to one of aspects 10 to 13, characterized in that it can be produced or is produced by a method according to one of aspects 1 to 9.

[0128] Aspect 15

[0129] Use of a treated substrate according to any one of aspects 10 to 14 as a component for high-temperature furnaces, preferably a heater, insulation component, holder; as a crucible or crucible element.

[0130] The present invention is explained in more detail with reference to the following figures and examples, without limiting the invention to the specifically illustrated parameters.

[0131] Example 1

[0132] Four different porous graphite substrates are provided, each differing in average pore diameter. The pores of graphite substrate 1A have an average pore diameter of 0.6 pm, the pores of graphite substrate 1B have an average pore diameter of 1.5 pm, the pores of graphite substrate 1C have an average pore diameter of 1.8 pm, and the pores of graphite substrate ID have an average pore diameter of 2.2 pm.

[0133] The porous graphite substrates have a substrate geometry of 5x5x1 cm 3 a) Preparation of the suspension

[0134] A suspension with the following composition is prepared:

[0135] 66.7 wt.% H2O dist.

[0136] 0.3 wt.% binder (e.g. Peptapon 520, powdered solid, Zschimmer & Schwarz Chemie GmbH)

[0137] 33 wt% silicon granules (Si fraction, d50 approx. 800 pm) First, the distilled water (distilled H2O) and the binder are weighed and placed in a container. To homogenize and dissolve the binder, the suspension is aged for 20 hours on a roller stand at 30 rpm (container). The silicon granules are then weighed and added to the suspension. To homogenize the suspension with the solids content, it is aged for 15 minutes on a roller stand at 30 rpm (container).

[0138] The coating is applied by spraying. The suspension is atomized using compressed air (4 bar). The suspension is applied via a nozzle (2.5 mm diameter). The substrates are each coated with an area of ​​5 x 5 cm. 2) perpendicular to the nozzle and thus to the spray jet direction, with the respective substrate being rotated at 10 rpm. The distance from the nozzle to the substrate surface is 20 cm. The coating is carried out for all substrates with a spray time of 8 s. A constant application of 0.06 ± 0.015 g suspension / cm 2 or 0.02 ± 0.005 g Si / cm 2 .

[0139] The coated substrates are stored in an oven for 20 h at 90 °C in air to dry. d) Infiltration process

[0140] The dried substrates are placed in a graphite sample chamber in a furnace. The coated surfaces have no contact with the furnace internals. The furnace volume is evacuated (10 3mbar) and heating at 250 K / h from room temperature to 1500°C. The temperature of 1500°C is maintained for 5 h. This is followed by cooling from 1500°C to room temperature at 200 K / h (the cooling rate decreases to 50 K / min from 700°C, as there is no active cooling). After cooling, the furnace volume is flooded with argon up to atmospheric pressure, and the substrates are removed. The treated substrates obtained in this way all exhibit no elemental silicon residues on the treated surface and are therefore all characterized by a very high surface quality.

[0141] The permeability of the treated substrates was determined using the differential pressure method (e.g., according to EN 993-4: 1995). The diagram in Fig. 1 compares the permeability of the treated substrates with the permeability of the untreated starting substrates. As can be clearly seen, the permeability of the substrates was significantly reduced by treatment with the method according to the invention. Each of the treated substrates has a permeability of less than 5 • 10 15 m 2 In addition, the treated substrates in the infiltration zone exhibit an open porosity of a maximum of 10%, determined by mercury porosimetry.

[0142] Based on the low permeability and low open porosity of the treated substrates, it can be concluded that the near-surface pores of each of the treated substrates are almost or essentially completely closed, thus sealing the respective treated surface almost or essentially completely. All substrates are very well protected against the penetration of corrosive gases or fluids into the material. Since the treated substrate obtained by treating graphite substrate 1B has the lowest permeability, the treated surface of this substrate is best sealed.

[0143] Example 2

[0144] Several porous iso-graphite substrates (substrates made of isostatically pressed graphite) of four different iso-graphite types are provided. The iso-graphite type 2A substrates have a porosity of 15% and pores with an average pore diameter of 2.2 μm. The iso-graphite type 2B substrates have a porosity of 14% and pores with an average pore diameter of 1.5 μm. The iso-graphite type 2C substrates have a porosity of 10% and pores with an average pore diameter of 1.8 μm. The iso-graphite type 2D substrates have a porosity of 10% and pores with an average pore diameter of 0.6 μm.

[0145] The porous graphite substrates have a substrate geometry of 5x5x1 cm 3 a) Preparation of the suspension

[0146] A suspension with the following composition is prepared:

[0147] 66.7 wt.% H2O dist.

[0148] 0.3 wt.% binder (e.g. Peptapon 520, powdered solid, Zschimmer & Schwarz Chemie GmbH)

[0149] 33 wt-% silicon granules (Si fraction, d50 approx. 800 pm)

[0150] First, the distilled water (distilled H2O) and the binder are weighed and placed in a container. To homogenize and dissolve the binder, the suspension is aged for 20 hours on a roller stand at 30 rpm (container). The silicon granules are then weighed and added to the suspension. To homogenize the suspension with the solids content, it is aged for 15 minutes on a roller stand at 30 rpm (container). b) Coating process

[0151] The coating is applied by spraying. The suspension is atomized using compressed air (4 bar). The suspension is applied via a nozzle (2.5 mm diameter). The substrates are each coated with an area of ​​5 x 5 cm. 2) perpendicular to the nozzle and thus to the spray jet direction, with the respective substrate being rotated at 10 rpm. The distance from the nozzle to the substrate surface is 20 cm. The coating is carried out with different spray times of 4 s, 8 s, 12 s, 16 s, 20 s, and 24 s, depending on the amount to be applied. One application per 4 s of approximately 0.01 ± 0.005 g Si / cm 2 After each coating cycle of 4 s, the samples are dried on a hot plate in air at 100 °C for 15 min. Different amounts of silicon per unit area are applied to the substrates of the four different iso-graphite types. Six substrates of iso-graphite type 2A are subjected to a coating process, with the silicon amounts used per unit area being 0.008 g / cm 2 , 0.018 g / cm 2 , 0.033 g / cm 2 , 0.044 g / cm 2 , 0.055 g / cm 2 and 0.076 g / cm 2Six substrates of iso-graphite type 2B are also subjected to a coating process, with the silicon quantities used per unit area being 0.007 g / cm 2 , 0.022 g / cm 2 , 0.028 g / cm 2 , 0.038 g / cm 2 , 0.056 g / cm 2 and 0.072 g / cm 2 Four substrates of iso-graphite type 2C are subjected to a coating process, whereby the silicon quantities used per unit area are 0.011 g / cm 2 , 0.02 g / cm 2 , 0.03 g / cm 2 and 0.045 g / cm 2 Finally, three substrates of the iso-graphite type 2D are subjected to a coating process, whereby the silicon quantities used per unit area are 0.008 g / cm 2 , 0.02 g / cm 2 and 0.025 g / cm 2 be.

[0152] The coated substrates are stored in the oven for 20 h at 90 °C in air to dry. process

[0153] The dried substrates are placed in a graphite sample chamber in a furnace. The coated surfaces have no contact with the furnace internals. The furnace volume is evacuated (10 3 mbar) and heating at 250 K / h from room temperature to 1500°C. The temperature of 1500°C is maintained for 5 h. This is followed by cooling from 1500°C to room temperature at 200 K / h (the cooling rate decreases to 50 K / min from 700°C onwards, as there is no active cooling). After cooling, the furnace volume is flooded with argon up to atmospheric pressure, and the substrates are removed.

[0154] The treated substrates obtained in this way all exhibit no elemental silicon residues on the treated surface and are therefore all characterized by a very high surface quality. The permeability of the treated substrates was determined using the differential pressure method (e.g., according to EN 993-4: 1995). The diagram in Fig. 2 shows the determined permeability values ​​for the respective treated substrates. In addition, the permeability of an untreated starting substrate of the four iso-graphite types is also plotted in the diagram. As can be clearly seen, the permeability of the substrates could be significantly reduced by treatment with the method according to the invention. Each of the treated substrates has a permeability of < 5 • 10 15 m 2 In addition, the treated substrates in the infiltration zone exhibit an open porosity of a maximum of 10%, determined by mercury porosimetry.

[0155] From Fig. 2 it can be seen that the permeability decreases with increasing amount of silicon deposited, whereby for graphite substrate 2D a deposited silicon amount of 0.025 gSi / cm 2 sufficient to achieve a permeability < 1 • 10 19 m 2 and thus below the measurement limit. The higher the initial permeability of the untreated substrate, the more silicon must be infiltrated to achieve a permeability < 1 • 10 19 m 2 and thus below the measuring limit.

[0156] From the low permeability and the low open porosity of the treated substrates, it can be concluded that the near-surface pores of each of the treated substrates are almost or essentially completely closed and thus the respective treated surface is almost or essentially completely sealed, so that all substrates are very well protected against the penetration of corrosive gases or fluids into the material.

[0157] By varying the amount of Si applied, the permeability or open porosity of the substrate can be varied and adjusted accordingly for the application. Example 3

[0158] Several porous iso-graphite substrates (substrates made of isostatically pressed graphite) of four different iso-graphite types are provided. The iso-graphite type 3A substrates have a porosity of 15% and pores with an average pore diameter of 2.2 μm. The iso-graphite type 3B substrates have a porosity of 14% and pores with an average pore diameter of 1.5 μm. The iso-graphite type Be substrates have a porosity of 10% and pores with an average pore diameter of 1.8 μm. The iso-graphite type 3D substrates have a porosity of 10% and pores with an average pore diameter of less than 0.6 μm.

[0159] The porous graphite substrates have a substrate geometry of 5x5x1 cm 3 a) Preparation of the suspension

[0160] A suspension with the following composition is prepared:

[0161] 66.7 wt.% H2O dist.

[0162] 0.3 wt.% binder (e.g. Peptapon 520, powdered solid, Zschimmer & Schwarz Chemie GmbH)

[0163] 33 wt-% silicon granules (Si fraction, d50 approx. 800 pm)

[0164] First, the distilled water (distilled H2O) and the binder are weighed and placed in a container. To homogenize and dissolve the binder, the suspension is aged for 20 hours on a roller stand at 30 rpm (container). The silicon granules are then weighed and added to the suspension. To homogenize the suspension with the solids content, it is aged for 15 minutes on a roller stand at 30 rpm (container).

[0165] The coating is applied by spraying. The suspension is atomized using compressed air (4 bar). The suspension is applied via a nozzle (2.5 mm diameter). The substrates are each coated with an area of ​​5 x 5 cm. 2) perpendicular to the nozzle and thus to the spray jet direction, with the respective substrate being rotated at 10 rpm. The distance from the nozzle to the substrate surface is 20 cm. The coating is carried out with different spray times of 4 s, 8 s, 12 s, 16 s, 20 s, and 24 s, depending on the amount to be applied. One application per 4 s of approximately 0.01 ± 0.005 g Si / cm 2 After each coating cycle of 4 s, the samples are dried on a hot plate in air at 100 °C for 15 min.

[0166] Different amounts of silicon per unit area are applied to the substrates of the four different iso-graphite types. Four substrates of iso-graphite type 3A are subjected to a treatment according to the invention, with the amounts of silicon used per unit area being 0.008 g / cm 2 , 0.018 g / cm 2 , 0.033 g / cm 2 and 0.044 g / cm 2Four substrates of iso-graphite type 3B are also subjected to a treatment according to the invention, the amounts of silicon used per unit area being 0.007 g / cm 2 , 0.022 g / cm 2 , 0.038 g / cm 2 and 0.056 g / cm 2 Four substrates of iso-graphite type 3C are also subjected to a treatment according to the invention, the amounts of silicon used per unit area being 0.011 g / cm 2 , 0.02 g / cm 2 , 0.03 g / cm 2 and 0.045 g / cm 2 Finally, three substrates of the iso-graphite type 3D are subjected to a treatment according to the invention, with the silicon quantities used per unit area being 0.02 g / cm 2 , 0.025 g / cm 2 and 0.035 g / cm 2 c) Drying process

[0167] The coated substrates are stored in an oven for 20 h at 90 °C in air to dry. d) Infiltration process

[0168] The dried substrates are placed in a graphite sample chamber in a furnace. The coated surfaces have no contact with the furnace internals. The furnace volume is evacuated (10 3 mbar) and heating at 250 K / h from room temperature to 1500°C. The temperature of 1500°C is maintained for 5 h. This is followed by cooling from 1500°C to room temperature at 200 K / h (the cooling rate decreases to 50 K / min from 700°C onwards, as there is no active cooling). After cooling, the furnace volume is flooded with argon up to atmospheric pressure, and the substrates are removed.

[0169] The treated substrates obtained in this way all show no residues of elemental silicon on the treated surface and are therefore all characterized by a very high surface quality.

[0170] The permeability of the treated substrates was determined using the differential pressure method (e.g., according to EN 993-4: 1995). The diagram in Fig. 3 shows the determined permeability values ​​for the respective treated substrates. Each of the treated substrates has a permeability of < 5 • 10 15 m 2 In addition, the treated substrates in the infiltration zone exhibit an open porosity of a maximum of 10%, determined by mercury porosimetry.

[0171] The mean infiltration depth (or mean thickness of the infiltration zone) was determined by optical microscopy on cross sections vertical to the infiltration direction and averaged over the entire sample length (5 cm).

[0172] The diagram in Fig. 3 shows that the permeability of the infiltrated substrate generally decreases with the infiltration depth (or the thickness of the infiltration zone). The decrease over the infiltration depth becomes more pronounced with decreasing initial permeability of the untreated graphite material. The permeability can therefore be adjusted by the infiltration depth of the graphite material and thus by the amount of Si applied.

[0173] Example 4

[0174] Six substrates of iso-graphite type 4A are provided. These have a porosity of 10% and pores with an average pore diameter of 1.8 pm.

[0175] The porous graphite substrates have a substrate geometry of 5x5x1 cm 3 on. a the suspension

[0176] A suspension with the following composition is prepared:

[0177] 66.7 wt.% H2O dist.

[0178] 0.3 wt.% binder (e.g. Peptapon 520, powdered solid, Zschimmer & Schwarz Chemie GmbH)

[0179] 33 wt-% silicon granules (Si fraction, d50 approx. 800 pm)

[0180] First, the distilled water (distilled H2O) and the binder are weighed and placed in a container. To homogenize and dissolve the binder, the suspension is aged for 20 hours on a roller stand at 30 rpm (container). The silicon granules are then weighed and added to the suspension. To homogenize the suspension with the solids content, it is aged for 15 minutes on a roller stand at 30 rpm (container).

[0181] The coating is applied by spraying. The suspension is atomized using compressed air (4 bar). The suspension is applied via a nozzle (2.5 mm diameter). The substrates are each coated with an area of ​​5 x 5 cm. 2) perpendicular to the nozzle and thus to the spray jet direction, with the respective substrate being rotated at 10 rpm. The distance from the nozzle to the substrate surface is 20 cm. The coating is applied with different spray times of 8 s and 12 s, depending on the amount to be applied. One application per 4 s of approximately 0.01 ± 0.005 g Si / cm 2 After each coating cycle of 4 s, the samples are dried on a hot plate in air at 100 °C for 15 min.

[0182] Different amounts of silicon per unit area are applied to the six substrates of iso-graphite type 4A, whereby the amount of silicon used per unit area for three of the six substrates is 0.02 ± 0.005 g / cm 2 and for the other three of the six substrates 0.03 ± 0.005 g / cm 2 amounts.

[0183] The coated substrates are stored in the oven for 20 h at 90 °C in air to dry. process

[0184] The dried substrates are subjected to different infiltration processes with different process conditions.

[0185] All dried substrates are placed in a graphite sample chamber in a furnace, with the coated surfaces having no contact with the furnace internals. For all substrates, the furnace volume is evacuated (10 3 mbar).

[0186] For the first of the substrates, which were coated with a silicon amount of 0.02 ± 0.005 g / cm 2 were infiltrated, and the first of the substrates, which were infiltrated with a silicon amount of 0.03 ± 0.005 g / cm 2 The vacuum is maintained throughout the process. For the second of the substrates, which were infiltrated with a silicon quantity of 0.02 ± 0.005 g / cm 2 were infiltrated, and the second of the substrates infiltrated with a silicon amount of 0.03 ± 0.005 g / cm 2were infiltrated, is instead flooded with argon and a pressure of 20 mbar is maintained throughout the process. For the third of the substrates, which were infiltrated with a silicon quantity of 0.02 ± 0.005 g / cm 2 were infiltrated, and the third of the substrates infiltrated with a silicon amount of 0.03 ± 0.005 g / cm 2 infiltrated, is finally flooded with argon and a pressure of 1000 mbar is maintained throughout the process.

[0187] Subsequently, all substrates were heated from room temperature to 1500 °C at 250 K / h, with the temperature being maintained at 1500 °C for 5 h. All substrates were then cooled from 1500 °C to room temperature at 200 K / h (the cooling rate decreases to 50 K / min from 700 °C due to the lack of active cooling). After cooling, the furnace volume was flooded with argon to atmospheric pressure, and the substrates were removed. The mean infiltration depth (or mean thickness of the infiltration zone) was determined using optical microscopy on cross-sections perpendicular to the infiltration direction and averaged over the entire sample length (5 cm).

[0188] The determined mean infiltration depths of the treated substrates are shown in the diagram in Fig. 4 as a function of the applied amount of silicon.

[0189] It is evident that the Si infiltration depth can be adjusted by the process pressure. If the infiltration process is carried out in vacuum, an infiltration depth between 325 and 350 pm can be achieved for a Si amount of 0.02 ± 0.005 g / cm 2 up to 0.03 ± 0.005 g / cm 2 If an argon pressure of 20 mbar is set for the infiltration process, a decrease in the infiltration depth to 275 pm or 290 pm can be observed. If the process pressure is further increased to 1000 mbar, a significant increase in the infiltration depth to 375 pm or 400 pm can be achieved.

[0190] By varying the process pressure, the depth of the infiltration zone can be influenced and adjusted.

[0191] Example 5

[0192] Two substrates of iso-graphite type 5A are provided. This has pores with an average pore diameter of 1.8 pm.

[0193] One of the two substrates is used for the determination of permeability after infiltration and has a substrate geometry of 5x5x1 cm 3 on.

[0194] The other of the two substrates is used for the determination of the open porosity in the infiltration zone after infiltration and has a substrate geometry of 2x0.5x0.5 cm 3 on a) Preparation of the suspension

[0195] A suspension with the following composition is prepared:

[0196] 66.7 wt.% H2O dist. 0.3 wt.% binder (e.g. Peptapon 520, powdered solid, Zschimmer & Schwarz Chemie GmbH)

[0197] 33 wt-% silicon granules (Si fraction, d50 approx. 800 pm)

[0198] First, the distilled water (distilled H2O) and the binder are weighed and placed in a container. To homogenize and dissolve the binder, the suspension is aged for 20 hours on a roller stand at 30 rpm (container). The silicon granules are then weighed and added to the suspension. To homogenize the suspension with the solids content, it is aged for 15 minutes on a roller stand at 30 rpm (container).

[0199] The two substrates are subjected to different coating processes.

[0200] Substrate for the determination of permeability:

[0201] The coating is applied by spraying. The suspension is atomized using compressed air (4 bar). The suspension is applied via a nozzle (2.5 mm diameter). The substrates are each coated with an area of ​​5 x 5 cm. 2) perpendicular to the nozzle and thus to the spray jet direction, with the respective substrate being rotated at 10 rpm. The distance from the nozzle to the substrate surface is 20 cm. The coating is applied with a spray time of 20 s, depending on the amount to be applied. One application per 4 s of approximately 0.01 ± 0.005 g Si / cm 2 After each coating cycle of 4 s, the samples are dried on a hot plate in air at 100 °C for 15 min. The total amount of silicon used per unit area is 0.05 ± 0.005 g / cm 2 .

[0202] Substrate for the determination of open porosity:

[0203] The coating is applied to all surfaces of the substrate. Due to the small sample dimensions, the coating could not be applied by spraying. For each surface of the graphite sample, the required amount of suspension is weighed to 0.05 ± 0.005 gSi / cm 2The weighed amount of suspension is applied to the appropriate surface and evenly distributed manually with a spatula. Intermediate drying takes place on a hot plate in air at 100 °C for 15 minutes. The process is then repeated until all surfaces of the samples are coated with Si.

[0204] The coated substrates are stored in an oven for 20 h at 90 °C in air to dry. d) Infiltration process

[0205] The dried substrates are placed in a graphite sample chamber in a furnace. The coated surfaces have no contact with the furnace internals. The furnace volume is evacuated (10 3mbar) and heating at 250 K / h from room temperature to 1500°C. The temperature of 1500°C is maintained for 5 h. This is followed by cooling from 1500°C to room temperature at 200 K / h (the cooling rate decreases to 50 K / min from 700°C onwards, as there is no active cooling). After cooling, the furnace volume is flooded with argon up to atmospheric pressure, and the substrates are removed.

[0206] For both the untreated and treated substrates, both the permeability was determined using the differential pressure method (e.g., according to EN 993-4:1995) and the open porosity was determined using mercury porosimetry (e.g., according to DIN 66133:1993-06). The determined values ​​for permeability and open porosity are graphically presented in Fig. 5a.

[0207] The mercury porosity measurements on the iso-graphite type 5A substrates show that with the infiltration of Si, a significant reduction in porosity from approximately 17.5% in the initial state to approximately 6% is achieved. The infiltration of the Si melt leads to the extensive filling of the pore structures in the graphite material. The images of the microstructure shown in Fig. 5b without and with Si infiltration clearly show that after infiltration, only very small pore structures remain unclosed. Thus, analogous to the porosity, the gas permeability of the substrate can also be measured up to the permeability measurement limit (1 • 10 19 m 2 ) can be reduced.

[0208] Example 6

[0209] In order to investigate the influence of the particle size of the silicon particles on the quality of the surface and the infiltration zone of the treated substrate, experiments were carried out in which the particle size of the silicon particles used was specifically varied.

[0210] The remaining conditions, such as coating application, substrate material, Si concentration per area, process duration and time, temperature profile, process pressure, and atmosphere, were kept constant. a) Preparation of the suspension

[0211] Two suspensions with the following compositions are prepared:

[0212] 1. Suspension:

[0213] 66.7 wt.% H2O dist.

[0214] 0.3 wt.% binder (e.g. Peptapon 520, powdered solid, Zschimmer & Schwarz Chemie GmbH)

[0215] 33 wt% silicon powder (Si fraction, d50 approx. 5 pm, max. 20 pm)

[0216] 2. Suspension:

[0217] 66.7 wt.% H2O dist.

[0218] 0.3 wt.% binder (e.g. Peptapon 520, powdered solid, Zschimmer & Schwarz Chemie GmbH)

[0219] 33 wt-% silicon granules (Si fraction, d50 approx. 800 pm, max. 1600 pm)

[0220] First, the distilled water (distilled H2O) and the binder are weighed and placed in a container. To homogenize and dissolve the binder, the suspension is aged for 20 hours on a roller stand at 30 rpm (container). The silicon powder or silicon granules are then weighed and added to the suspension. To homogenize the suspension with the solids content, it is aged for 15 minutes on a roller stand at 30 rpm (container).

[0221] With each of the two suspensions, a graphite substrate with a substrate geometry of 5x5x1 cm 3 coated.

[0222] The coating is applied by spraying. The suspension is atomized using compressed air (4 bar). The suspension is applied via a nozzle (2.5 mm diameter). The substrates are each coated with an area of ​​5 x 5 cm. 2 ) perpendicular to the nozzle and thus to the spray jet direction, with the respective substrate being rotated at 10 rpm. The distance from the nozzle to the substrate surface is 20 cm. A constant application of approximately 0.07 ± 0.015 g Si / cm 2 .

[0223] The coated substrates are stored in the oven for 20 h at 90 °C in air to dry. process

[0224] The dried substrates are placed in a graphite sample chamber in a furnace. The coated surfaces have no contact with the furnace internals. The furnace volume is evacuated (10 3mbar) and heating at 250 K / h from room temperature to 1500°C. The temperature of 1500°C is maintained for 5 h. This is followed by cooling from 1500°C to room temperature at 200 K / h (the cooling rate decreases to 50 K / min from 700°C onwards, as there is no active cooling). After cooling, the furnace volume is flooded with argon up to atmospheric pressure, and the substrates are removed.

[0225] Both treated substrates exhibit an open porosity of a maximum of 10% in the infiltration zone, determined by mercury porosimetry. Figure 6 shows an overview of the surfaces of the samples coated with the suspension and the infiltrated samples. For the latter, vertical cross-sections were also taken along the infiltration direction.

[0226] Fig. 6 shows that in the case of the Si powder (d50 approx. 5 pm) there are isolated silicon carbide crystals on the surface, but these are embedded in a cracked, granular matrix of incompletely melted particles. For the coarser Si granulate (d50 approx. 800 pm), on the other hand, a highly polycrystalline, crack-free surface can be achieved. Fundamentally, this shows that finer Si material tends to have a lower capacity for complete melting. A crucial aspect here is the high specific surface area, which typically increases with decreasing particle size. On the one hand, in the case of Si, there is increased oxidation of the surface in air but also in contact with water during suspension production and processing.The resulting silicon oxide layer on the particle surface subsequently impairs the formation of a molten phase and thus inhibits the infiltration process. To avoid this, the powder can be freed of the oxide layer using chemical (e.g., treatment with hydrofluoric acid HF) or thermal processes. However, this is technically complex and not feasible for a Si-based coating. Furthermore, a high specific surface area can react with free carbon from the furnace atmosphere or residues of the carbon-based organic suspension additives (e.g., binders) close to the surface before the actual melting to form silicon carbide. Thus, the melting of the particles only occurs partially and incompletely, leaving cracked and porous structures.

[0227] As a consequence of these observations, it can be stated that a larger average particle size of the silicon particles leads to a more complete melting of the silicon particles, which promotes the formation of a highly crystalline, crack- and pore-free surface, whereas the use of silicon particles with a lower average particle size can lead to cracks in the surface due to incomplete melting of the silicon particles. This can be further confirmed by measuring the (gas) permeability using the differential pressure method (e.g., according to EN 993-4: 1995). The corresponding measurement results are shown in Fig. 7, where the graph initially shows the values ​​for both samples of the exemplary embodiment, for which a deposition of approximately 0.07 g Si / cm 2was carried out, and additional values ​​are given for further samples, where the second suspension was applied with a different application rate. In the present case, for the infiltration of the fine Si powder (d50 approx. 5 pm), a permeability of 5.3 • 10 18 m 2 The initial permeability of the graphite substrate used is 2.5 • 10 15 m 2 . If, however, Si granules with an average particle size of 800 pm are used, the permeability of the infiltrated substrate (at a coating of approx. 0.07 g Si / cm 2 ) below the measuring limit of 1 • 10 19 m 2, which corresponds to a completely gas-tight sample. This demonstrates that while the permeability of graphite materials can be reduced by infiltration with fine Si powder, they cannot be made completely gas-tight and therefore not oxidation-resistant.

[0228] Ultimately, the studies show that the use of larger silicon particles allows for significantly more gas-tight and defect-free surfaces than is possible with finer silicon powder. Furthermore, in the case of fine silicon powder, post-processing may be necessary due to the formation of macrocracks (see Fig. 6) and the associated poor coating adhesion to make the component usable for further processing steps or for use.

[0229] In addition, the oxidation tendency of the silicon powder or silicon granules used upon contact with water was determined via the release of hydrogen H2. According to the reaction Si + 2 SiO2 + 2 FU, the water molecule is split during the oxidation of Si. With increasing specific surface area and decreasing particle size, this reaction is further promoted. Fig. 8 shows the measured EU concentrations over the service life. The measurement was carried out using a hydrogen measuring probe at a distance of 1 cm from the suspension surface. For the Si powder, an initial hydrogen concentration of 1 • IO -4 Vol.-% were measured. This increased over time and finally reached a concentration of 0.04 vol.-% after 24 h. For the Si granulate, the value for the entire measurement interval was below the measurement limit (< 5 • 10 -5 Vol.-%).

[0230] Example 7

[0231] To investigate the oxidation behavior of a treated substrate produced using silicon particles with a high average particle size, a corresponding treated substrate was prepared and then the permeability and oxidation behavior of the thus prepared treated substrate were investigated.

[0232] To produce the treated substrate, a cuboid graphite substrate with dimensions of 5 x 2.5 x 1 cm 3 (Surface 40 cm 2 ) using a suspension comprising silicon particles with a high average particle size (d50 approx. 800 pm), the sample was fully coated with a silicon coating and then subjected to a heat treatment to melt and infiltrate the silicon and convert it into silicon carbide. The sample was prepared in the following steps: a) Preparation of the suspension

[0233] A suspension with the following composition is prepared:

[0234] 66.7 wt.% H2O dist.

[0235] 0.3 wt.% binder (e.g. Peptapon 520, powdered solid, Zschimmer & Schwarz Chemie GmbH)

[0236] 33 wt-% silicon granules (Si fraction, d50 approx. 800 pm, max. 1600 pm)

[0237] First, the distilled water (distilled H2O) and the binder are weighed and placed in a container. To homogenize and dissolve the binder, the suspension is aged for 20 hours on a roller stand at 30 rpm (container). The silicon granules are then weighed and added to the suspension. To homogenize the suspension with the solids content, it is aged for 15 minutes on a roller stand at 30 rpm (container).

[0238] The suspension is used to coat a graphite substrate with a substrate geometry of 5x5x1 cm 3 coated.

[0239] The coating is applied by spray application. The suspension is atomized using compressed air (4 bar). The suspension is delivered through a nozzle (2.5 mm diameter). The substrate is positioned with the surface to be coated perpendicular to the nozzle and thus to the spray jet direction, while the substrate is rotated at 10 rpm. The distance from the nozzle to the substrate surface is 20 cm. A constant application of 0.04 ± 0.015 g Si / cm 2 After drying, the sample is rotated so that the uncoated surface is perpendicular to the spray jet, and this surface is coated in the same way. The process is repeated until all surfaces are coated.

[0240] The coated substrate is placed in the drying cabinet at 90 °C in air for 20 h. process

[0241] The dried substrate is placed in a graphite sample chamber in a furnace. The coated surfaces have no contact with the furnace internals. The furnace volume is evacuated (10 3 mbar) and heating at 250 K / h from room temperature to 1500°C. The temperature of 1500°C is maintained for 5 h. This is followed by cooling from 1500°C to room temperature at 200 K / h (the cooling rate decreases to 50 K / min from 700°C onwards, as there is no active cooling). After cooling, the furnace volume is flooded with argon up to atmospheric pressure, and the substrate is removed.

[0242] The treated substrate has an open porosity in the infiltration zone, determined by mercury porosimetry, of a maximum of 10%. In addition, a permeability of < 1 • 10 can be determined for the treated substrate using the differential pressure method (e.g., according to EN 993-4: 1995). 19 m 2 be determined.

[0243] To investigate the oxidation behavior, the prepared treated substrate was exposed to synthetic air (200 ml / min, 1 bar) at 1100 °C for up to 162 h and the mass was determined at intervals of 6 or 24 h.

[0244] The results of this investigation of the oxidation behavior are summarized in Fig. 9. It is clear that for the prepared sample after up to 162 h within the measurement accuracy (± 0.001 g) no mass loss could be detected or this was below 2.5 • 10 -5 g / cm 2 relative to the sample surface. A slight increase in mass was even observed, as oxygen is absorbed through the formation of an oxide layer on the silicon carbide infiltration layer. This study also provides further evidence of the enormous density of the infiltration zone and thus of the surface of the treated substrate.

[0245] By using silicon particles with a large particle size and thereby creating an extremely dense surface, the oxidation behavior of such coated components can be significantly improved, resulting in exceptionally high oxidation resistance.

Claims

Patent claims Method for treating porous substrates, in which a) at least one surface of a porous carbon-containing substrate is provided with at least one silicon coating by applying at least one aqueous suspension comprising silicon particles, at least one binder, and water to the at least one surface and then subjecting it to a drying process, and b) the at least one silicon coating is subjected to at least one heat treatment in which the silicon coating melts to form a melt that infiltrates into pores of the porous carbon-containing substrate, wherein silicon contained in the melt is at least partially converted into silicon carbide. Method according to the preceding claim, characterized in that the silicon particles have an average particle size in the range from 10 pm to 3500 pm, preferably from 310 pm to 1700 pm, particularly preferably from 500 to 1000 pm.Method according to one of the preceding claims, characterized in that the silicon particles have an average particle size of more than 500 pm and up to 3500 pm, preferably in the range from 550 pm to 3500 pm, particularly preferably in the range from 650 pm to 1700 pm, very particularly preferably in the range from 750 pm to 1000 pm. Method according to one of the preceding claims, characterized in that the at least one binder ensures an adhesive strength of the silicon coating of at least 0.15 MPa, and / or. is selected from the group consisting of polyvinyl alcohol, polyethylene glycol, polyvinyl butyral, polyacrylic acid, polyurethane, chloroprene rubber, phenolic resin, acrylic resin, cellulose, cellulose derivatives, alginic acid, dextrin, and mixtures thereof.

5. Method according to one of the preceding claims, characterized in that the at least one aqueous suspension 1 to 50 wt.%, preferably 5 to 35 wt.%, of the silicon particles, based on the total weight of the at least one aqueous suspension, and / or 0.01 to 3 wt.%, preferably 0.05 to 0.3 wt.%, of the at least one binder, based on the total weight of the at least one aqueous suspension.

6. Method according to one of the preceding claims, characterized in that the application of the at least one aqueous suspension in step a) is carried out by dipping, brushing, doctoring and / or spraying, preferably by spraying.

7. Method according to one of the preceding claims, characterized in that the drying process takes place at a temperature in the range from 10 °C to 200 °C, preferably from 80 °C to 100 °C, and / or over a period of 5 h to 48 h, preferably from 10 h to 12 h.

8. Method according to one of the preceding claims, characterized in that the at least one heat treatment takes place at a temperature in the range from 1400 °C to 1800 °C, preferably from 1450 °C to 1550 °C, and / or over a period of 1 h to 10 h, preferably from 4 h to 6 h, and / or under vacuum or under an inert gas atmosphere, preferably argon atmosphere, at a (process) pressure of 10 mbar to 2000 mbar, preferably from 100 mbar to 1800 mbar, particularly preferably from 500 mbar to 1500 mbar, very particularly preferably from 800 mbar to 1200 mbar.

9. Method according to one of the preceding claims, characterized in that the porous carbonaceous substrate contains or consists of a material which is selected from the group consisting of graphite, preferably iso-graphite; carbon fiber reinforced carbon; silicon carbide fiber reinforced carbon; silicon carbide fiber reinforced silicon carbide; glassy carbon; sintered silicon carbide; silicon infiltrated silicon carbide; and combinations thereof, and / or the porous carbonaceous substrate contains or consists of a material which has a thermal expansion coefficient of at least 2.8 • IO -6 K 1 , preferably at least 3.0 • IO -6 K 1 , particularly preferably at least 3.2 • IO -6 K 1, and / or the porous carbonaceous substrate has an open porosity, measured by means of mercury porosimetry, of at least 12%, preferably from 12% to 30%, particularly preferably from 14% to 25%, most preferably from 15% to 20%, and / or the pores of the porous carbonaceous substrate have an average pore diameter in the range from 0.1 pm to 10 pm, preferably from 1 pm to 5 pm, particularly preferably from 1.5 pm to 5 pm.

10. Method according to one of the preceding claims, characterized in that the infiltration depth of the melt is adjusted by the amount per unit area of ​​the at least one aqueous suspension applied to the at least one surface and / or by the pressure during the at least one heat treatment. Method according to one of the preceding claims, characterized in that the porous carbon-containing substrate is doped with at least one dopant selected from the group consisting of nitrogen (N), aluminum (Al), boron (B), phosphorus (P), vanadium (V), scandium (Sc), gallium (Ga), indium (In), germanium (Ge), tin (Sn), lead (Pb), arsenic (As), antimony (Sb), bismuth (Bi), and mixtures thereof, and / or the silicon particles are doped with at least one dopant selected from the group consisting of nitrogen (N), aluminum (Al), boron (B), phosphorus (P), vanadium (V), scandium (Sc), gallium (Ga), indium (In), germanium (Ge), tin (Sn), lead (Pb), arsenic (As), antimony (Sb), bismuth (Bi), and mixtures thereof, and / or the at least one aqueous suspension additionally comprises at least one compound containing at least one dopant selected from the group consisting of Group consisting of nitrogen (N), aluminum (AI), boron (B), phosphorus (P),Vanadium (V), scandium (Sc), gallium (Ga), indium (In), germanium (Ge), tin (Sn), lead (Pb), arsenic (As), antimony (Sb), bismuth (Bi), and mixtures thereof, and / or the at least one heat treatment is carried out in the presence of a process gas that contains or consists of nitrogen. Treated substrate comprising a carbonaceous substrate material with pores, wherein the substrate has an infiltration zone on at least one surface in which the pores of the substrate material are at least partially filled with silicon carbide, wherein the treated substrate has a permeability of at most 5 • 10, 15 m 2 and wherein the treated substrate in the infiltration zone has an open porosity, determined by mercury porosimetry, of a maximum of 10%. Treated substrate according to claim 12, characterized in that the treated substrate a maximum permeability of 1 • 10 16 m 2, preferably from a maximum of 1 • 10 17 m 2 , particularly preferably a maximum of 1 • 10 19 m 2 , and / or has a permeability which is lower by a factor of at least 10, preferably at least 100, than a permeability of the substrate before treatment, and / or in the infiltration zone an open porosity, determined by means of mercury porosimetry, of a maximum of 8%, preferably a maximum of 5%, and / or has an open porosity in the infiltration zone, determined by means of mercury porosimetry, which is at least 7%, preferably at least 10%, particularly preferably at least 12%, based on the total volume of the treated substrate, lower than an open porosity of the treated substrate outside the infiltration zone, and / or has a specific resistance of at most 1500 mΩcm, preferably of at most 10 mΩcm, and / or has no elemental silicon. Treated substrate according to claim 12 or 13, characterized in that the infiltration zone has an average thickness of at least 100 pm, preferably from 100 pm to 1200 pm, particularly preferably from 200 pm to 800 pm, and / or the silicon carbide with which the pores of the substrate material in the infiltration zone are at least partially filled contains 3C-SiC, preferably has 3C-SiC as the main phase.Treated substrate according to one of claims 12 to 14, characterized in that the carbon-containing material is selected from the group consisting of graphite, preferably iso-graphite; carbon. Fiber reinforced carbon; silicon carbide fiber reinforced carbon; silicon carbide fiber reinforced silicon carbide; sintered silicon carbide; glassy carbon; and combinations thereof. Treated substrate according to one of claims 12 to 15, characterized in that the silicon carbide is doped with at least one dopant selected from the group consisting of nitrogen (N), aluminum (Al), boron (B), phosphorus (P), vanadium (V), scandium (Sc), gallium (Ga), indium (In), germanium (Ge), tin (Sn), lead (Pb), arsenic (As), antimony (Sb), bismuth (Bi), and mixtures thereof, wherein the at least one dopant is preferably selected from the group consisting of nitrogen (N), aluminum (Al), boron (B), phosphorus (P), vanadium (V), scandium (Sc), and mixtures thereof, and / or in the infiltration zone in a concentration in the range of 1 • IO 10 Atoms per cm 3 up to 1 • 10 23 Atoms per cm 3, preferably in the range of 1 • 10 12 Atoms per cm 3 up to 1 • 10 21 Atoms per cm 3 , particularly preferably in the range of 1 • 10 15 Atoms per cm 3 up to 1 • 10 18 Atoms per cm 3 , is present. Treated substrate according to one of claims 12 to 16, characterized in that it can be produced or is produced by a method according to one of claims 1 to 11. Use of a treated substrate according to one of claims 12 to 17 as a component for high-temperature furnaces, preferably a heater, insulation component, or holder; as a crucible or crucible element.