Anode for electroplating, and method and system for electroplating article with metal

MYPI2025003136A0Undetermined Publication Date: 2024-05-25DISPOL CHEMICALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025003136
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-11-25
Filing Date
2023-11-17
Publication Date
2024-05-25

AI Technical Summary

Technical Problem

The decomposition of organic compound additives in alkaline zinc-nickel alloy plating baths leads to poor plating performance, increased bath voltage, and frequent bath replacement due to oxidative decomposition catalyzed by metal ions, resulting in reduced plating film thickness and corrosion resistance.

Method used

An electroplating anode design featuring a support part with a larger cross-sectional area than the current-carrying part, where the current-carrying part is covered with an insulating material to suppress heat generation and oxidative decomposition, allowing for stable current distribution and efficient plating without the need for ancillary equipment or special metals.

Benefits of technology

This design effectively suppresses bath voltage and temperature increases, maintaining plating performance and extending bath life by reducing the decomposition of organic additives, thus enhancing the quality and durability of the plating film without increasing costs or requiring complex equipment management.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025003136_DRAWING_001
    Figure PI2025003136_DRAWING_001
  • Figure PI2025003136_DRAWING_002
    Figure PI2025003136_DRAWING_002
  • Figure PI2025003136_DRAWING_003
    Figure PI2025003136_DRAWING_003
Patent Text Reader

Abstract

The present invention aims to provide an anode for electroplating that can be relatively easily manufactured without the need for ancillary facilities or anolyte management, and without requiring expensive or special metals. The present invention relates to an anode for electroplating, comprising: an input part where power is input from a power source; a pair of support parts that extend in a first direction, are arranged at intervals in a second direction intersecting the first direction, receive power supply from the input part, and whose portions in contact with a plating solution are covered with an insulating material; and an electrification part that extends in the second direction, one end of which is connected to one of the pair of support parts, the other end of which is connected to the other of the pair of support parts, and receives power supply from the pair of support parts, wherein the electrification part includes several current paths arranged at intervals in the first direction, and a cross-sectional area of the electrification part is smaller than that of each of the support parts. [Fig. 1]
Need to check novelty before this filing date? Find Prior Art

Description

Electroplating anode and method and system for electroplating an article with a metal

[0001] The present invention relates to an electroplating anode and a method and system for electroplating an article with a metal using the same, and more particularly to an electroplating anode that inhibits decomposition of an organic compound additive added to a plating bath containing metal ions, and a method and system for electroplating an article with a metal using the same.

[0002] Zinc plating is used as a relatively inexpensive anti-rust plating, and its alkaline plating bath contains organic compounds such as quaternary amine polymers as additives. When these organic compounds are decomposed during anodization, they cause dendritic deposition with poor adhesion, making it impossible to form a good zinc anti-rust plating.

[0003] Zinc alloy plating has superior corrosion resistance compared to zinc plating and is therefore widely used in automotive parts and other applications. Alkaline zinc-nickel alloy plating baths, in particular, are used for fuel-cell components and engine parts exposed to high temperatures, which require high corrosion resistance. Alkaline zinc-nickel alloy plating baths use an amine-based chelating agent appropriate for the desired nickel codeposition rate to dissolve nickel and codeposit zinc and nickel into the plating film. However, a problem arises when current is applied: the amine-based chelating agent oxidizes and decomposes on the anode surface, producing oxalic acid and sodium carbonate. When iron-based metal ions, such as nickel and iron ions, coexist, these act as oxidation catalysts, further accelerating the oxidative decomposition of the amine-based chelating agent. Consequently, contact of the alkaline zinc-nickel alloy plating bath with the anode rapidly decomposes the amine-based chelating agent, resulting in a rapid degradation of plating performance. The accumulation of decomposed products can cause a variety of problems, including reduced current efficiency, increased bath voltage, reduced plating film thickness, reduced nickel codeposition rate in the plating film, a narrower range of possible current densities, reduced gloss, and increased chemical oxygen demand (COD). For this reason, the plating bath could not be used for a long period of time and had to be replaced frequently.

[0004] Patent Documents 1 and 2 describe a so-called anode cell system in which anolyte is placed in a cell covered with a diaphragm, separating the plating bath from the anode plate to prevent contact, thereby suppressing decomposition of organic compound additives. In this anode cell system, oxalic acid and sodium carbonate generated in the plating bath migrate from the plating solution into the anode cell, which is expected to also remove decomposed substances from the plating bath. However, the anode cell system requires many auxiliary facilities, such as the anode cell itself, piping, and pumps. Furthermore, the concentration of the anolyte must be managed, and the anolyte must be renewed at regular intervals.

[0005] Patent Document 3 describes suppressing decomposition of organic compound additives by applying a coating to the surface of the conductive substrate of the anode. In this case, no additional equipment or electrode liquid management is required, but the cost of manufacturing the anode becomes an issue. Patent Document 4 also describes applying a coating to the surface of the conductive substrate of the anode, but further improvement is required.

[0006] On the other hand, Patent Document 5 discloses a method for determining the amount of Fe in a plating bath by using an electrode having an iridium oxide coating layer on a conductive substrate at a specific anode current density for iron-based electroplating. 2+ It is described that the oxidation of ions due to the application of current is suppressed, and that the coating layer may be in the form of a mesh. Furthermore, Patent Document 6 describes a porous metal anode in the form of an expanded metal or the like, which has a coating layer of an electrode active material such as iridium oxide, and describes that the electrode is not only lighter and easier to handle than conventional flat anodes, but also facilitates the dissipation of generated gas, making it effective in reducing voltage.

[0007] International Publication No. 2016 / 075963 International Publication No. 2016 / 075964 Patent No. 6582353 Special Publication No. 2019-530800 Publication JP 5-331696 Publication JP 1-208499 Publication

[0008] An object of the present invention is to provide an electroplating anode that can be produced relatively easily without requiring any additional facilities or anolyte management, and without requiring any expensive or special metals.

[0009] As a result of extensive research aimed at solving the above-mentioned problems, the inventors discovered that by providing a specific support part between an input part to which current is input from a power source and a current-carrying part that passes current through the plating solution in an electroplating anode, it is possible to suppress an increase in bath voltage and an increase in bath temperature due to heat generation in the current-carrying part, and thus completed the present invention. That is, the present invention provides the following electroplating anode, method for electroplating an article with a metal, and system for electroplating an article with a metal. [1] An electroplating anode comprising: an input section for receiving power from a power source; a pair of support sections extending in a first direction and spaced apart from each other in a second direction intersecting the first direction, receiving a supply of power from the input section and having a portion that comes into contact with the plating solution covered with an insulating material; and a current conductor extending in the second direction, having one end connected to one of the pair of support sections and the other end connected to the other of the pair of support sections, and receiving a supply of power from the pair of support sections, wherein the current conductor has a plurality of current paths spaced apart from each other in the first direction, and a cross-sectional area of ​​the current conductor is smaller than that of the support sections. [2] The electroplating anode according to [1], wherein a ratio (Sc / So) of an area (Sc) of a portion that comes into contact with the plating solution of the current conductor to an outer area (So) of a region in which the current conductor is disposed is 0.05 to 0.5. [3] The electroplating anode according to [1] or [2], wherein the ratio (S2 / S1) of the cross-sectional area of ​​the current-carrying portion (S2) to the cross-sectional area of ​​the support portion (S1) is 0.5 or less. [4] The electroplating anode according to any one of [1] to [3], wherein the current-carrying portion includes a wire, an expanded metal, and / or a punched metal. [5] The electroplating anode according to any one of [1] to [3], wherein the current-carrying portion has a cross-sectional area of ​​3 to 75 mm 2and / or - contains at least one selected from the group consisting of iron, nickel, stainless steel, and carbon, and / or - is uniformly dispersed and disposed in the anode, and / or - is disposed at intervals of 10 cm or less from each other. [6] The electroplating anode according to any one of [1] to [4], wherein the supporting portion constitutes at least a part of the outer periphery of the anode, and / or the cross-sectional area (S1) of the supporting portion is 15 to 1200 mm 2 [7] A method for electroplating an article with a metal, comprising a step of passing a current through a plating bath containing ions of the metal and an organic compound additive, wherein the plating bath comprises the article as a cathode and the electroplating anode according to any one of [1] to [6]. [8] A method for electroplating an article with a metal, comprising a step of passing a current through a plating bath containing ions of the metal and an organic compound additive, the plating bath comprising the article as a cathode and the electroplating anode according to any one of [1] to [6]. [9] A method for electroplating an article with a metal, comprising a step of passing a current through a plating bath containing ions of the metal and an organic compound additive, the plating bath comprising the article as a cathode and the electroplating anode according to any one of [1] to [6].

[10] A method for electroplating an article with a metal, comprising a step of passing a current through a plating bath containing ions of the metal and an organic compound additive, the plating bath comprising the article as a cathode and the electroplating anode according to any one of [1] to [6].

[11] A method for electroplating an article with a metal, comprising a step of passing a current through a plating bath containing ions of the metal and an organic compound additive, the plating bath comprising the article as a cathode and the electroplating anode according to any one of [1] to [6].

[12] A method for electroplating an article with a metal, comprising a step of passing a current through a plating bath containing ions of the metal and an organic compound additive, the electroplating bath comprising the article as a cathode and the electroplating anode according to any one of [1] to [6]. 2 and / or the magnitude of the current relative to the cross-sectional area (S2) of the current-carrying portion is 2 to 75 A / mm 2 [9] A system for electroplating an article with a metal, comprising a plating bath containing ions of the metal and an organic compound additive, wherein the plating bath comprises the article as a cathode and the electroplating anode according to any one of [1] to [6].

[0010] According to the present invention, an increase in bath voltage can be suppressed by providing a pair of support members between the input portion and the current-carrying portion of the electroplating anode, the support members having a cross-sectional area larger than that of the current-carrying portion and having portions that come into contact with the plating solution covered with an insulating material. The electroplating anode of the present invention does not require any additional equipment or anode solution management, and does not require expensive or special metals, thereby enabling low-cost electroplating.

[0011] 1 shows an embodiment of an electroplating anode of the present invention (ladder type). The hatched area is coated with an insulating material. 2 shows an embodiment of an electroplating anode of the present invention (grid type). The hatched area is coated with an insulating material. 3 shows an embodiment of an electroplating anode of the present invention (mesh type). The hatched area is coated with an insulating material. 4 shows an enlarged view of part IV in FIG. 3. 5 shows a comparative electroplating anode. 6 shows the plating appearance of a cathode plate.

[0012] The present invention will be described in more detail below. The electroplating anode of the present invention comprises: an input section for receiving power from a power source; a pair of support sections extending in a first direction and spaced apart from each other in a second direction intersecting the first direction, receiving power from the input section and having a portion of the support section that comes into contact with the plating solution coated with an insulating material; and a current-carrying section extending in the second direction, one end connected to one of the pair of support sections and the other end connected to the other of the pair of support sections, receiving power from the pair of support sections. The cross-sectional area of ​​the current-carrying section is smaller than that of the support sections. To increase the anode current density using a conventional simple flat electrode, it is necessary to either reduce the outer surface area of ​​the current-carrying section or apply a current greater than the current required for plating. In the former case, a smaller outer surface area causes bias in the current-carrying area in the plating bath, resulting in uneven current distribution and an increase in bath voltage. Furthermore, heat generation at the interface between the outside air and the plating solution can also cause an increase in bath voltage. On the other hand, the support member of the electroplating electrode of the present invention supplies power to the current-carrying member, but the portion in contact with the plating solution is covered with an insulating material, preventing current from flowing through the plating solution. This reduces the risk of heat generation and bath voltage increases at the interface between the outside air and the plating solution. The support member can efficiently supply power to current-carrying members located far from the input member, i.e., current-carrying members that penetrate deep into the plating solution. Furthermore, the current-carrying members can receive a stable supply of power even deep within the plating solution. Because the entire current-carrying member is immersed in the plating solution, heat generation is not an issue even when the current-carrying member is made of a conductive member with a small cross-sectional area. Furthermore, because the current-carrying members are uniformly distributed, there is no bias in the current distribution in the bath. As a result, current can be uniformly and efficiently passed through the plating solution (plating bath), enabling the formation of a good plating film on the object being electroplated. Note that the "cross-sectional area" here refers to the cross-sectional area in a plane perpendicular to the direction of current flow.

[0013] The first direction in which the pair of support portions extend is not particularly limited, and may be a direction extending from the input portion. The second direction is not particularly limited as long as it intersects with the first direction, and may be a direction perpendicular to the first direction. The pair of support portions may be spaced apart on a continuous member, or may be spaced apart on separate members. The specific form is not particularly limited as long as the current-carrying portion can be connected between them. In one embodiment, the pair of support portions may form at least a portion of the outer periphery of the anode, or may surround the entire periphery. That is, the electroplating anode of the present invention may further include additional support portions, and the pair of support portions and the additional support portions may be directly or indirectly connected to form a frame that constitutes a portion or the entire periphery of the anode.

[0014] The cross-sectional area (S1) of the support portion is not particularly limited, but is, for example, about 15 mm 2 ~Approx. 1200mm 2 may be about 100 mm 2 ~Approx. 1100mm 2 or about 125 mm 2 ~ Approximately 1000 mm 2 The conductive member constituting the support is not particularly limited as long as it is capable of conducting electricity, and may include, for example, at least one selected from the group consisting of iron, nickel, stainless steel, carbon, titanium, copper, and members coated with any of these.

[0015] The insulating material is not particularly limited as long as it can withstand use in a plating solution, and may include, for example, at least one selected from the group consisting of polymer resin, rubber, insulating inorganic oxide, insulating inorganic nitride, insulating inorganic carbide, and insulating inorganic boride. More specifically, the polymer resin may include epoxy resin, vinyl chloride resin, melamine resin, phenolic resin, fluororesin, acrylic resin, polystyrene, ABS (acrylonitrile butadiene styrene) resin, polyethylene, polypropylene, nylon polyurethane, methylpentene resin, polycarbonate, etc. The rubber may include silicone rubber, fluororubber, urethane rubber, acrylic rubber, nitrile rubber, ethylene propylene rubber, styrene rubber, butyl rubber, butadiene rubber, natural rubber, etc. The insulating inorganic oxide may include silicon dioxide, magnesium oxide, zinc oxide, beryllium oxide, titanium oxide, tantalum oxide, etc.

[0016] The current-carrying portion of the electroplating anode of the present invention has a plurality of current paths spaced apart from one another in the first direction. The "current path" here refers to a path through which current flows. The plurality of current paths may be formed by installing a plurality of conductive members constituting the current-carrying portion, or by the conductive members constituting the current-carrying portion having a branched structure. In one embodiment, the plurality of current paths are uniformly dispersed and arranged within the anode.

[0017] The fact that the individual current paths are spaced apart means that gaps are formed in the region where the current-carrying portions are present, and therefore the total area of ​​the liquid-contacting portions of all the current-carrying portions is smaller than the area of ​​the liquid-contacting portions if all the current-carrying portions were a series of flat plates, i.e., the outer area of ​​the region where the current-carrying portions are arranged. The ratio (Sc / So) of the area of ​​the liquid-contacting portions of the current-carrying portions (Sc) to the outer area (So) of the region where the current-carrying portions are arranged is not particularly limited, and may be, for example, about 0.5 or less, about 0.3 or less, or about 0.25 or less, or may be about 0.05 or more, 0.1 or more, or 0.125 or more.

[0018] Without being bound by any particular theory, it is believed that an oxidation reaction occurs near the anode, simultaneously generating an oxygen and decomposing an organic compound additive (described later). Limiting the area of ​​the current-carrying part of the electrode in the plating solution increases the anode current density (current per unit area of ​​the current-carrying part of the anode). In this state, the oxygen generation reaction occurs preferentially over the decomposition of the organic compound additive, compared to when the anode current density is low, thereby suppressing the decomposition of the organic compound additive. Furthermore, by spacing the current paths at the anode, it is believed that an increase in plating bath voltage can be suppressed and the current distribution relative to the cathode can be stabilized. If a conventional flat plate were used as the anode and the anode current density were to be increased without changing the area of ​​the current-carrying part, a significant increase in the applied current would be required, which would increase the bath voltage, which would be uneconomical and could affect the durability of the anode. Furthermore, a significant increase in the applied current would also significantly increase the cathode current density, which could adversely affect plating quality. By using the electroplating anode according to this embodiment, the anode current density can be increased without these disadvantages, and decomposition of the organic compound additive can be suppressed.

[0019] The cross-sectional area (S2) of the current-carrying part of the electroplating anode of the present invention is not particularly limited as long as it is smaller than the cross-sectional area of ​​the support part. For example, 2 ~Approx. 75mm 2 may be about 4.5 mm 2 ~ approx. 50 mm 2 The ratio (S2 / S1) of the cross-sectional area (S2) of the current-carrying portion to the cross-sectional area (S1) of the support portion is not particularly limited, but may be, for example, about 0.5 or less, about 0.004 to about 0.25, or about 0.007 to about 0.16.

[0020] The conductive member constituting the current-carrying portion is not particularly limited as long as it is capable of conducting electricity, but may include, for example, at least one selected from the group consisting of iron, nickel, stainless steel, carbon, platinum, platinum-plated titanium, palladium-tin alloy, and members coated therewith, and preferably includes at least one selected from the group consisting of iron, nickel, stainless steel, and carbon. The shape of the current-carrying portion is not particularly limited, but may be, for example, a wire, expanded metal, punched metal, and / or a flat plate, and is preferably a wire. Expanded metal and punched metal have a branched structure, so that multiple current paths can be formed even when used alone.

[0021] In one aspect, the electroplating anode of the present invention may include a plurality of the current-carrying portions, and the plurality of current-carrying portions are preferably uniformly dispersed throughout the anode. The spacing between the current-carrying portions is not particularly limited, but for example, the current-carrying portions may be spaced apart from one another by a distance of about 10 cm or less, or about 3 cm to about 7 cm, center-to-center. In another aspect, the electroplating anode of the present invention may further include a current-carrying portion extending in the first direction. The current-carrying portion extending in the first direction may have a plurality of current paths spaced apart from one another in the second direction, but is not particularly limited thereto.

[0022] In the electroplating anode of the present invention, the manner in which the current-carrying portion is connected to the support portion is not particularly limited as long as they are capable of conducting current to each other. For example, the current-carrying portion 31 may be configured in a ladder shape between both sides of a support portion 41 (frame) configured to include an input portion 21 at its upper portion and surround the periphery of the electrode except for the lower portion (ladder-type electroplating anode 1). In this case, multiple current paths 311 are provided in a direction perpendicular to the support portion 41. Alternatively, the current-carrying portion 32 may be configured in a grid shape inside a support portion 42 (frame) configured to include an input portion 22 at its upper portion and surround the entire periphery of the electrode (grid-type electroplating anode 1A). In this case, not only are multiple current paths 321 provided in a direction perpendicular to the support portion 42, but multiple current paths 322 are also provided in the direction in which the support portion 42 extends. An example of a ladder-type electroplating anode in which the current-carrying portion has a wire shape is shown in FIG. 1, and an example of a grid-type electroplating anode in which the current-carrying portion and the additional current-carrying portion have a wire shape is shown in FIG. 2.

[0023] The electroplating anode of the present invention may be subjected to any modification commonly used in the art, or to a treatment useful for suppressing an increase in bath voltage, suppressing an increase in bath temperature due to heat generation from the current-carrying part, or suppressing decomposition of the organic compound additive, as long as the purpose of the anode is not impaired. For example, if a part of the surface of the conductive member constituting the current-carrying part is covered with an insulating material and the other part is left exposed, the area of ​​the current-carrying part of the electrode in the plating solution is limited, and the anode current density (current per unit area of ​​the current-carrying part of the anode) is increased, which is useful for suppressing decomposition of the organic compound additive.

[0024] In another aspect, the present invention relates to a method for electroplating an article with a metal, the method comprising the step of passing a current through a plating bath containing ions of the metal and an organic compound additive, the plating bath comprising the article as a cathode and the electroplating anode of the present invention described above. According to the method of the present invention, it is possible to uniformly and efficiently pass a current through the plating bath while suppressing an increase in bath voltage and an increase in bath temperature due to heat generation in a current-carrying part, and to form a good plating film on the article.

[0025] The metal is not particularly limited as long as it is used in electroplating, and may include, for example, zinc, nickel, iron, copper, cobalt, tin, manganese, etc. If the metal is zinc only, a zinc coating is formed on the article, and if the metal contains zinc and another metal, a zinc alloy coating is formed on the article. The other metal is not particularly limited as long as it can form the zinc alloy coating, and may be, for example, at least one selected from the group consisting of nickel, iron, cobalt, tin, manganese, etc. The zinc alloy coating is not particularly limited, and may be, for example, a zinc-nickel alloy plating, a zinc-iron alloy plating, a zinc-cobalt alloy plating, a zinc-manganese alloy plating, or a tin-zinc alloy plating.

[0026] The article is a substrate to be plated, and any commonly used article in the art can be used without any particular limitation. The article may be made of various metals, such as iron, nickel, copper, zinc, and aluminum, and alloys thereof. The shape of the article is also not particularly limited, and examples include plate-like articles such as steel sheets and plated steel sheets, and shaped articles such as rectangular parallelepipeds, cylinders, cylinders, and spheres. Specific examples of such shaped articles include fasteners such as bolts, nuts, and washers, pipe parts such as fuel pipes, cast iron parts such as brake calipers and common rails, as well as connectors, plugs, housings, ferrules, and seat belt anchors.

[0027] The conditions for the current application step are not particularly limited as long as a plating film of the metal can be applied to the article. For example, the current may be applied at a temperature of about 15°C to about 40°C, preferably about 25 to about 35°C, or at a current of about 0.1 to 20 A / dm 2 , preferably 0.2 to 10 A / dm 2 The magnitude of the current (anode current density) relative to the area (Sc) of the liquid-contacting portion of the current-carrying portion is not particularly limited, but may be, for example, about 25 to about 150 A / dm 2 , preferably about 25 to about 75 A / dm 2 , more preferably about 30 to about 65 A / dm 2The magnitude of the current relative to the cross-sectional area (S2) of the current-carrying portion is not particularly limited, but may be, for example, about 2 to about 75 A / mm 2 , preferably about 5 to about 20 A / mm 2 may be.

[0028] The term "organic compound additive" as used herein refers to an organic compound added to a plating bath for electroplating. The type of organic compound additive is not particularly limited. For example, when zinc plating is performed, the organic compound additive may be at least one selected from the group consisting of a brightener, a water conditioner, and an antifoaming agent. When zinc alloy plating is performed, the organic compound additive may be at least one selected from the group consisting of a brightener, a metal complexing agent, a water conditioner, and an antifoaming agent. In either case, in a preferred embodiment, the organic compound additive includes a brightener.

[0029] The brightener may be any brightener commonly used in the art without any particular limitation, and examples thereof include base component brighteners that mainly contribute to the covering power and uniform electrodeposition of the plating film, brightener component brighteners that mainly contribute directly to imparting brightness to the plating film, and auxiliary component brighteners that mainly assist in imparting brightness to the plating film in low current density areas.

[0030] The base component brightener is not particularly limited, and examples thereof include: (1) nonionic surfactants such as polyoxyethylene polyoxypropylene block polymers and acetylene glycol EO adducts, and anionic surfactants such as polyoxyethylene lauryl ether sulfates and alkyl diphenyl ether disulfonates; (2) polyallylamine such as a copolymer of diallyldimethylammonium chloride and sulfur dioxide; polyepoxypolyamines such as condensation polymers of ethylenediamine and epichlorohydrin, condensation polymers of dimethylaminopropylamine and epichlorohydrin, condensation polymers of imidazole and epichlorohydrin, condensation polymers of imidazole derivatives such as 1-methylimidazole and 2-methylimidazole and epichlorohydrin, and condensation polymers of heterocyclic amines including triazine derivatives such as acetoguanamine and benzoguanamine and epichlorohydrin; condensation polymers of 3-dimethylaminopropylurea and epichlorohydrin, bis(N,N-dimethylaminopropyl)urea and ethylenediamine; Polyamide polyamines such as polyamine polyurea resins such as condensation polymers of N,N-dimethylaminopropylamine, alkylene dicarboxylic acid and epichlorohydrin, and water-soluble nylon resins such as condensation polymers of N,N-dimethylaminopropylamine, alkylene dicarboxylic acid and epichlorohydrin; condensation polymers of diethylenetriamine, dimethylaminopropylamine, etc. and 2,2'-dichlorodiethyl ether, condensation polymers of dimethylaminopropylamine and 1,3-dichloropropane, condensation polymers of N,N,N',N'-tetramethyl-1,3-diaminopropane and 1,4- (2) polyamine compounds such as polyalkylene polyamines, such as a condensation polymer of dichlorobutane and N,N,N',N'-tetramethyl-1,3-diaminopropane and 1,3-dichloropropan-2-ol; (3) condensation polymers of dimethylamine or the like with dichloroethyl ether; (4) aromatic carboxylic acids, such as benzoic acid or a salt thereof; (5) quaternary ammonium salts not having a nitrogen-containing heterocycle, such as cetyltrimethylammonium chloride; or nitrogen-containing heterocyclic quaternary ammonium salts.

[0031] The nitrogen-containing heterocyclic quaternary ammonium salts are, for example, nitrogen-containing heterocyclic quaternary ammonium salts having a carboxy group and / or a hydroxy group. The nitrogen-containing heterocyclic ring of the nitrogen-containing heterocyclic quaternary ammonium salts is not particularly limited and may be, for example, a pyridine ring, a piperidine ring, an imidazole ring, an imidazoline ring, a pyrrolidine ring, a pyrazole ring, a quinoline ring, or a morpholine ring, and is preferably a pyridine ring. More preferably, the nitrogen-containing heterocyclic quaternary ammonium salt is a quaternary ammonium salt of nicotinic acid or a derivative thereof. In the nitrogen-containing heterocyclic quaternary ammonium salt compound, the carboxy group and / or hydroxy group may be directly bonded to the nitrogen-containing heterocyclic ring or may be bonded via another substituent, such as a carboxymethyl group. The nitrogen-containing heterocyclic quaternary ammonium salts may have an additional substituent, such as an alkyl group, in addition to the carboxy group and the hydroxy group. In the nitrogen-containing heterocyclic quaternary ammonium salts, the N-substituent forming the heterocyclic quaternary ammonium cation is not particularly limited as long as it does not impair the effect as a glossing agent, and may be, for example, a substituted or unsubstituted alkyl group, aryl group, or alkoxy group. The counter anion forming the salt is not particularly limited, and may be, for example, a compound containing a halogen anion, an oxyanion, a borate anion, a sulfonate anion, a phosphate anion, or an imide anion, and is preferably a halogen anion. Such quaternary ammonium salts are preferred because they contain both a quaternary ammonium cation and an oxyanion in the molecule and therefore also exhibit anionic behavior.

[0032] Specifically, the nitrogen-containing heterocyclic quaternary ammonium salts include, for example, pyridinium, N-benzyl-3-carboxypyridinium chloride, N-phenethyl-4-carboxypyridinium chloride, N-butyl-3-carboxypyridinium bromide, N-chloromethyl-3-carboxypyridinium bromide, N-hexyl-6-hydroxy-3-carboxypyridinium chloride, N-hexyl-6-3-hydroxypropyl-3-carboxypyridinium chloride, N-2-hydroxyethyl-6-methoxy-3-carboxypyridinium chloride, N-methoxy-6-methyl-3-carboxypyridinium chloride, N- Examples of the nitrogen-containing heterocyclic quaternary ammonium salt include propyl-2-methyl-6-phenyl-3-carboxypyridinium chloride, N-propyl-2-methyl-6-phenyl-3-carboxypyridinium chloride, N-benzyl-3-carboxymethylpyridinium chloride, 1-butyl-3-methyl-4-carboxyimidazolium bromide, 1-butyl-3-methyl-4-carboxymethylimidazolium bromide, 1-butyl-2-hydroxymethyl-3-methylimidazolium chloride, 1-butyl-1-methyl-3-methylcarboxypyrrolidinium chloride, and 1-butyl-1-methyl-4-methylcarboxypiperidinium chloride. The nitrogen-containing heterocyclic quaternary ammonium salts may be used alone or in combination of two or more.

[0033] The concentration of the base component brightener in the plating bath is not particularly limited, but may be, for example, about 1 to about 500 mg / L, and preferably about 5 to about 100 mg / L, in the case of aromatic carboxylic acids, and about 0.01 to about 10 g / L, and preferably 0.02 to 5 g / L, in other cases.

[0034] The brightening component brightener is not particularly limited, but may include, for example, aromatic aldehydes such as veratraldehyde, vanillin, and anisaldehyde. The concentration of the brightening component brightener in the plating bath is not particularly limited, but may be, for example, about 1 to about 500 mg / L, and preferably about 5 to about 100 mg / L.

[0035] The auxiliary component brightener is not particularly limited, but may include a thiouracil compound, a mercapto compound such as 2-mercaptobenzimidazole, an organic acid, etc. The concentration of the auxiliary component brightener in the plating bath is not particularly limited, but may be, for example, about 0.01 to about 50 g / L.

[0036] The water conditioner may be any water conditioner commonly used in the art without any particular limitation, and may be, for example, a silicic acid. The concentration of the water conditioner in the plating bath is not particularly limited, and may be, for example, about 0.01 to about 50 g / L. The antifoaming agent may be any water conditioner commonly used in the art without any particular limitation, and may be, for example, a surfactant. The concentration of the antifoaming agent in the plating bath is not particularly limited, and may be, for example, about 0.01 to about 5 g / L.

[0037] The metal complexing agent may be any agent commonly used in the art without any particular limitation, and may be, for example, an amine-based chelating agent. Examples of the amine-based chelating agent include alkyleneamine compounds such as ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, and pentaethylenehexamine; alkylene oxide adducts of the alkyleneamines, such as ethylene oxide adducts and propylene oxide adducts; aminoalcohols such as ethanolamine, diethanolamine, triethanolamine, diisopropanolamine, triisopropanolamine, ethylenediaminetetra-2-propanol, N-(2-aminoethyl)ethanolamine, and 2-hydroxyethylaminopropylamine. The metal complexing agent may include coal; alkanolamine compounds such as N-(2-hydroxyethyl)-N,N',N'-triethylethylenediamine, N,N'-di(2-hydroxyethyl)-N,N'-diethylethylenediamine, N,N,N',N'-tetrakis(2-hydroxyethyl)propylenediamine, and N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine; poly(alkyleneimines) obtained from ethyleneimine, 1,2-propyleneimine, and the like; poly(alkyleneamines) obtained from ethylenediamine, triethylenetetramine, and the like; and poly(aminoalcohols). Preferably, the metal complexing agent includes at least one selected from the group consisting of alkyleneamine compounds, alkylene oxide adducts thereof, and alkanolamine compounds. The metal complexing agents may be used alone or in combination of two or more. The concentration of the metal complexing agent in the plating bath is not particularly limited, but may be, for example, about 5 to about 200 g / L, and preferably about 30 to about 100 g / L.

[0038] The method of the present invention may further include any step commonly used in the art, as long as it does not impair the object of the method of the present invention. For example, the method of the present invention may further include a step of washing the article before the energizing step, or a step of washing the article after the energizing step.

[0039] In another aspect, the present invention relates to a system for electroplating an article with a metal, the system comprising a plating bath containing ions of the metal and an organic compound additive, the plating bath comprising the article as a cathode, and the electroplating anode of the present invention described above. According to the system of the present invention, it is possible to uniformly and efficiently energize the plating bath while suppressing an increase in bath voltage and an increase in bath temperature due to heat generation in a current-carrying part, and to form a good plating film on the article.

[0040] Specific aspects of the system of the present invention are as described in detail with respect to the electroplating method of the present invention. The system of the present invention may further include any equipment commonly used in the art, as long as it does not impair the purpose of the system.

[0041] The present invention will be specifically explained below with reference to examples, but the scope of the present invention is not limited to these examples.

[0042] [Preparation Example 1] A U-shaped iron frame (length 620 mm x width 110 mm (inner width 80 mm), cross-sectional area 225 mm) with an open bottom was prepared. 2 ) was used as a support, to which 19 iron wires (diameter 2.5 mm) were attached horizontally (in a ladder-like pattern) at intervals of 30 to 31 mm (the distance from the first to the 19th wire was 550 mm). A member (input part) that contacts the power supply connection was attached to the top of the iron frame. Then, only the iron frame portion was covered with masking paint MR-54 (manufactured by Tokan Corporation) containing styrene-butadiene rubber (insulating material), to prepare the electroplating anode of Example 1. This anode was electrified through the iron wire portion (current-carrying portion; width 80 mm). When the anode was placed along the wall of the electrolytic cell so that the entire anode was immersed in the electrolyte, the area of ​​the liquid-contacting portion (surface area of ​​the iron wire not including the wall side: Sc) was 0.6 dm 2 (=0.025 dm × 3.14 × 0.8 dm × 1 / 2 × 19). On the other hand, the outer area of ​​the liquid-contacting portion of this anode (the outer area of ​​the region where the iron wire is arranged: So) is 4.4 dm 2(= 5.5 dm × 0.8 dm), so Sc / So is calculated to be 0.14. In addition, the ratio (S2 / S1) of the cross-sectional area of ​​the iron wire in the direction of the current (S2) to the cross-sectional area of ​​the iron frame in the direction of the current (S1) is calculated to be 0.022.

[0043] Test Example 1 The electroplating anode of Example 1 was placed in an electrolytic cell containing an electrolytic solution having the composition shown in Table 1, along the wall surface of the electrolytic cell, so that the iron wire, which was the current-carrying part, was entirely immersed in the electrolytic solution. *1 Dipsol amine chelating agent (ethylene oxide adduct of alkyleneamine)

[0044] An iron plate (550 mm long x 80 mm wide; both the outer surface area and the area of ​​the liquid-contacting portion were 4.4 dm²) was prepared in the same manner as the electroplating anode of Example 1. 2 ) or an iron plate with the same wetted area (length 550 mm x width 11 mm; both the outer area and the wetted area are 0.6 dm 2 ) was placed in the electrolytic cell as the anode for Comparative Example 1 or 2. A pickled steel sheet (SPHC-P steel sheet) was placed in each electrolytic cell as the cathode, and electricity was passed through the cells under the conditions shown in Table 2. During the passage of electricity, the electrolytic cells were placed in a larger water tank, and the area around the electrolytic cells was cooled with cooling water and a cooler to maintain the bath temperature.

[0045] Before and after energization, 30 mL of the electrolyte was collected. The IZ-250YB concentration was measured by ion chromatography. The bath voltage immediately after energization and the bath temperature during energization were also measured. The results are shown in Table 3. *2 One hour after the start of energization, the bath temperature rose to 31° C., so energization was stopped and the bath was cooled for 10 minutes until it reached 25° C. Thereafter, energization was continued while repeating this operation.

[0046] When the anode of Comparative Example 1, which consisted of a single iron plate, was used, the chelating agent IZ-250YB was decomposed. However, when the anode of Example 1, which used multiple iron wires as current-carrying parts to reduce the area of ​​the liquid-contacting part (the part that conducts electricity to the electrolyte) and had an insulating coating frame with a larger cross-sectional area than the iron wires as a support part, was used, the decomposition of IZ-250YB was suppressed. On the other hand, when the anode of Comparative Example 2, which consisted of a small single iron plate, was used, the decomposition of IZ-250YB was suppressed, but the bath voltage increased compared to Comparative Example 1, and the cooling method used in this test was unable to maintain the bath temperature. Therefore, for anodes with the same outer surface area, by using a support part and separately arranging multiple conductive members as current-carrying parts, it is possible to suppress the decomposition of organic compound additives without increasing the bath voltage and bath temperature.

[0047] [Preparation Example 2] A copper metal fitting (input part 23) for connecting to a power supply connector was attached to the top of an expanded metal (specifications SW22, LW50.8, T3.2, W3.5; length 600 mm × width 100 mm; aperture ratio 65%) used as the current-carrying part 33, and a copper rod (diameter 5 mm, cross-sectional area 19.6 mm) coated with styrene-butadiene rubber was attached to the side of the metal fitting as the support part 43. 2 ) was attached to the anode, to prepare a mesh-type electroplating anode (with a frame) of Example 2 shown in Figure 3. An enlarged view of the expanded metal portion (part IV in Figure 3) is shown in Figure 4. Each of these branched paths functions as a current path.

[0048] Test Example 2 The electroplating anode of Example 2 was placed in an electrolytic cell containing an electrolytic solution having the composition shown in Table 4, along the wall of the electrolytic cell, so that the lower 500 mm of the expanded metal, which was the current-carrying part, was immersed in the electrolytic solution (the outer surface area of ​​the immersed part of the anode was 5 dm 2 ). *3 Dipsol amine chelating agent (ethylene oxide adduct of alkyleneamine) *4 Dipsol gloss agent (polyamine) *5 Dipsol polishing agent (quaternary ammonium salt of nicotinic acid)

[0049] An electroplating anode (without frame) of Comparative Example 3 shown in FIG. 5 was prepared in the same manner as the electroplating anode of Example 2, except that the copper rod was not attached, and was placed in an electrolytic cell in the same manner as the electroplating anode of Example 2. A 100 mm wide pickled SPHC-P steel plate was placed in each electrolytic cell as the cathode, with the bottom 500 mm of the cathode immersed (electrode distance: 30 cm), as in the anode. Under the conditions shown in Table 5, the current was increased stepwise from 25 A to 150 A, and electricity was applied for 5 minutes at each current value. During the application of electricity, the electrolytic cell was placed in a larger water tank, and the area around the electrolytic cell was cooled with cooling water and a cooler to maintain the bath temperature.

[0050] The anode current density at each current value was calculated, and the bath voltage was measured. The results are shown in Table 6.

[0051] When the anode of Comparative Example 3 without a frame was used, the bath voltage increased with each increase in the current value, and the upper limit of the voltage in the test equipment was reached before the current value reached 150 A, making it impossible to pass current under the condition of 150 A. On the other hand, when the anode of Example 2 with a frame was used, the increase in bath voltage was suppressed. Therefore, if a support part that connects the current-carrying part and the electrode connection part is provided on the electroplating anode, the increase in bath voltage can be suppressed.

[0052] [Preparation Example 3] A U-shaped iron frame (length 200 mm x width 80 mm (inner width 70 mm), cross-sectional area 19.6 mm) with an open bottom was used. 2 ) was used as a support, to which six iron wires (2.5 mm in diameter) were attached horizontally (in a ladder-like pattern) at intervals of 35 to 36 mm (the distance from the first to sixth wires was 179 mm). A member (input part) that contacts the power supply connector was attached to the top of the iron frame. Then, only the iron frame portion was covered with masking paint MR-54 (manufactured by Tokan Corporation) containing styrene-butadiene rubber (an insulating material), to prepare an electroplating anode for Example 3. This anode was electrified through the iron wire portion (current-carrying portion; width 70 mm). When the anode was placed along the wall of an electrolytic cell so that the entire anode was immersed in the electrolyte, the area of ​​the liquid-contacting portion (surface area of ​​the iron wire not including the wall side: Sc) was 0.16 dm 2(=0.025 dm × 3.14 × 0.7 dm × 1 / 2 × 6). On the other hand, the outer area of ​​the liquid-contacting portion of this anode (the outer area of ​​the region where the iron wire is arranged: So) is 1.253 dm 2 (=1.79 dm × 0.7 dm), so Sc / So is calculated to be 0.13. In addition, the ratio (S2 / S1) of the cross-sectional area of ​​the iron wire in the direction of the current (S2) to the cross-sectional area of ​​the iron frame in the direction of the current (S1) is calculated to be 0.25.

[0053] Test Example 3 The electroplating anode of Example 3 was placed in an electrolytic cell containing an electrolytic solution (plating solution) having the composition shown in Table 7, along the wall surface of the electrolytic cell, so that the iron wire, which was the current-carrying part, was entirely immersed in the electrolytic solution. *6 Made by Dipsol *7 Made by Dipsol

[0054] An iron plate (length 179 mm × width 70 mm; outer area and area of ​​the liquid-contacting part are 1.253 dm²) having the same outer area as the electroplating anode of Example 3 was used. 2 ) was installed in the electrolytic cell as the anode for Comparative Example 4. An SPCC steel sheet was installed as the cathode in each electrolytic cell, and electricity was applied under the conditions listed in Table 8. The cathode was replaced every hour until the current applied to the plating solution reached 100 Ah / L. NiSO4·6H2O was replenished at a rate of 200 g / kAh. The plating solution was analyzed by high-performance liquid chromatography or capillary electrophoresis for the amine-based chelating agent and nitrogen-containing heterocyclic compound-based brightener at 50 Ah / L and 100 Ah / L current, respectively, and these organic compound additives were replenished so as to maintain their concentrations at the start of current application. Zinc ions were titrated every hour, and zinc ions were replenished by appropriately immersing metallic zinc in the plating solution to maintain the concentration at the start of current application. During current application, the electrolytic cell was placed in a larger water tank, and the surrounding area was cooled with cooling water and a cooler to maintain the bath temperature.

[0055] When a current of 50 Ah / L and a current of 100 Ah / L were applied, the appearance of the plating solution was visually observed, the concentration of oxalic acid in the plating solution was measured by ion chromatography, and the concentration of sodium carbonate (NaCO) in the plating solution was measured by titration.

[0056] In addition, a Hull cell test (long Hull cell type) was conducted using the plating solution before energization or the plating solution after energization of 100 Ah / L. Briefly, 500 mL of the plating solution before energization or after energization was placed in a long cell for the Hull cell test (anode iron plate: 65 × 65 × 0.5 mm, cathode iron plate: 65 × 200 × 0.5 mm), and a plating test was conducted under conditions of 2 A, 20 minutes, and 25°C. The cathode after plating was removed, and its appearance was visually observed. Then, the plating film thickness was measured every 1 cm from the left end of the cathode plate (the end on the high current density side) using an X-ray fluorescence analyzer, and the Ni co-deposition rate was also measured using the X-ray fluorescence analyzer.

[0057] The concentrations of oxalic acid and sodium carbonate are shown in Table 9, a photograph of the appearance of the cathode after the Hull Cell test is shown in FIG. 6, and the plating film thickness and nickel co-deposition rate are shown in Tables 10 and 11, respectively.

[0058]

[0059]

[0060]

[0061] When the anode of Comparative Example 4, which consisted of a single iron plate, was used, the amount of oxalic acid, a decomposition product of the chelating agent, and the amount of sodium carbonate produced by the reaction of carbon dioxide generated by the decomposition of the chelating agent with caustic soda in the plating solution were large, and the color of the plating solution changed from blue-purple to brown as current was applied. On the other hand, when the anode of Example 3 was used, the amount of oxalic acid and sodium carbonate produced was smaller than in Comparative Example 4, and the color of the plating solution maintained its initial blue-purple color even after current was applied. These results confirmed that the use of the anode of Example 3, which uses multiple iron wires as current-carrying parts to reduce the area of ​​the liquid-contacting part (the part that conducts current to the plating solution) and has an insulating coating frame as a support part with a larger cross-sectional area than the iron wires, suppresses the decomposition of organic compound additives. It was also confirmed that no increase in bath voltage occurred.

[0062] In Test Example 3, the organic compound additive was replenished to maintain the concentration at the start of current application, but when the plating solution after current application using the anode of Comparative Example 4 was used, the cathode gloss range (the black area of ​​the cathode in Figure 6) was narrower, and the plating film thickness and nickel codeposition rate were lower (Tables 10 and 11) than when the plating solution after current application using the anode of Example 3 was used. These results indicate that the generation of decomposition and aging products such as oxalic acid and sodium carbonate reduces plating performance even if organic compound additives are replenished, but it is believed that the use of the anode of Example 3 can suppress such a reduction in plating performance and improve the use efficiency of the plating solution.

[0063] From the above, it has been found that the increase in bath voltage can be suppressed by providing a pair of support parts between the input part and the current-carrying part of the electroplating anode, the support parts having a cross-sectional area larger than that of the current-carrying part and the parts that come into contact with the plating solution covered with an insulating material. An electroplating anode having such a configuration does not require any additional equipment or anode solution management, and does not require expensive or special metals, making it possible to reduce the cost of electroplating.

[0064] REFERENCE SIGNS LIST 1 Ladder-type electroplating anode 21 Input portion 31 Current-carrying portion 311 Current path 41 Support portion 1A Lattice-type electroplating anode 22 Input portion 32 Current-carrying portion 321 Horizontal current path 322 Vertical current path 42 Support portion 1B Mesh-type electroplating anode 23 Input portion 33 Current-carrying portion 331 Current path 43 Support portion 100 Control electroplating anode 200 Input portion 300 Control current-carrying portion

Claims

1. An electroplating anode comprising: an input section to which power is input from a power source; a pair of support sections extending in a first direction and spaced apart from each other in a second direction intersecting the first direction, which receive power from the input section and have portions that come into contact with the plating solution covered with an insulating material; and a current-carrying section extending in the second direction, one end connected to one of the pair of support sections and the other end connected to the other of the pair of support sections, which receives power from the pair of support sections, wherein the current-carrying section has a plurality of current paths spaced apart from each other in the first direction, and the cross-sectional area of ​​the current-carrying section is smaller than the cross-sectional area of ​​the support sections.

2. An electroplating anode as described in claim 1, wherein the ratio (Sc / So) of the area (Sc) of the liquid-contacting portion of the current-carrying portion to the outer area (So) of the region in which the current-carrying portion is disposed is 0.05 to 0.

5.

3. The electroplating anode according to claim 1, wherein the ratio (S2 / S1) of the cross-sectional area (S2) of the current-carrying portion to the cross-sectional area (S1) of the support portion is 0.5 or less.

4. The electroplating anode according to claim 1, wherein the current-carrying portion comprises a wire, an expanded metal, and / or a punched metal.

5. The current-carrying part is: - 3 to 75 mm 2 and / or - comprises at least one selected from the group consisting of iron, nickel, stainless steel, and carbon; and / or - is uniformly dispersed and disposed in the anode; and / or - is disposed at intervals of 10 cm or less from one another.

6. The support portion constitutes at least a part of the outer periphery of the anode, and / or the cross-sectional area (S1) of the support portion is 15 to 1200 mm 2 2. The anode of claim 1, wherein:

7. A method for electroplating an article with a metal, comprising the step of passing an electric current through a plating bath containing ions of the metal and an organic compound additive, the plating bath comprising the article as a cathode and the electroplating anode according to any one of claims 1 to 6.

8. The magnitude of the current (anode current density) relative to the area (Sc) of the liquid-contacting portion of the current-carrying portion is 25 to 150 A / dm 2 and / or the magnitude of the current relative to the cross-sectional area (S2) of the current-carrying portion is 2 to 75 A / mm 2 The method of claim 7, wherein 9. A system for electroplating an article with a metal, comprising a plating bath containing ions of the metal and an organic compound additive, the plating bath comprising the article as a cathode and the electroplating anode according to any one of claims 1 to 6.