Method for degrading polyurethane acrylic resin material and degradable polyurethane acrylic resin material
Patent Information
- Application Number
- MYPI2025003200
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-12-30
- Filing Date
- 2023-01-06
- Publication Date
- 2024-06-30
AI Technical Summary
Polyurethane acrylic resin composite materials are difficult to melt or dissolve in the three-dimensional network cross-linked state, making recycling difficult. Existing recycling methods such as burial and incineration have high costs and environmental pollution problems, and lack effective degradation technology.
The degradation liquid containing reactive NH or NH2 groups and OH groups is used to heat and decompose the polyurethane acrylic resin material. Through ammonolysis and alcoholysis, efficient degradation is achieved, and the degradation liquid is separated through vacuum distillation to realize the reuse of the material.
It achieves efficient degradation of polyurethane acrylic resin, separates fibers without plastic attachment, realizes material recycling and reuse, reduces waste and reduces environmental pollution.
Smart Images

Figure PI2025003200_DRAWING_001 
Figure PI2025003200_DRAWING_002 
Figure PI2025003200_DRAWING_003
Abstract
Description
[0001] FIELD OF THE INVENTION The present invention relates to a method for degrading polyurethane materials, and more particularly to a method for degrading polyurethane materials containing network-crosslinked polyurethane acrylic resins, polyurethane acrylic resins, compositions thereof, preparation methods, and composite materials. Background Art Polyurethane acrylic resins offer a wide range of design options, allowing for adjustments in rigidity or flexibility to meet specific requirements. Their molecular structure offers advantages such as excellent corrosion resistance, wear resistance, adhesion, heat resistance, mechanical properties, and good wetting properties for various fibers, making them suitable for composite material design. However, these excellent properties make the decomposition and recycling of these composite materials difficult, ultimately leading to landfill shortages and environmental pollution. Therefore, the decomposition and recycling of waste composite materials has become a significant issue. Because polyurethane acrylic resin composites are present in a three-dimensional network of crosslinked resins, they are difficult to recycle by melting or dissolving. According to existing technologies, polyurethane acrylic resin composites can only be recycled through methods that consume significant energy and time, and are costly, such as landfill and incineration. Degradation-based recycling technologies are lacking. However, landfill and incineration are becoming increasingly unfeasible in the future. Only by developing biodegradable resins can composite material recycling be achieved, thereby achieving waste reduction. Therefore, finding suitable degradation solutions to degrade polyurethane acrylic resins and thereby achieve recycling has become a goal of relevant industry players. SUMMARY OF THE INVENTION One object of the present invention is to provide a method for degrading polyurethane acrylic resin materials, which utilizes a degradation solution containing reactive NH or NH2 groups and OH groups to thermally decompose the polyurethane acrylic resin material for recycling and reuse. Another object of the present invention is to provide a polyurethane acrylic resin, its composition, preparation method, and composite material, which are synthesized by esterifying an isophthalic acid ester with a polyol and then adding a diluent monomer to produce a degradable polyurethane acrylic resin. One embodiment of the present invention provides a method for degrading a polyurethane acrylic resin material, comprising providing a polyurethane acrylic resin material, providing a degradation solution, performing a mixing step, and performing a heating step. The polyurethane acrylic resin material is obtained by curing a polyurethane acrylic resin.The degradation solution contains at least a degradation compound, and the degradation compound contains at least a reactive NH or NH? group and a reactive OH group. The mixing step involves mixing the polyurethane acrylic resin material with the degradation solution to form a degradation mixture. The heating step involves heating the degradation mixture to a degradation temperature and maintaining the temperature for a degradation time to degrade the polyurethane acrylic resin material. According to the method for degrading a polyurethane acrylic resin material described in the preceding paragraph, the polyurethane acrylic resin material may be a cured polyurethane acrylic resin or a composite material containing a cured polyurethane acrylic resin. According to the method for degrading a polyurethane acrylic resin material described in the preceding paragraph, the composite material containing a cured polyurethane acrylic resin may comprise a polyurethane acrylic resin and fiber. According to the method for degrading a polyurethane acrylic resin material described in the preceding paragraph, the fiber may be glass fiber, carbon fiber, polyamide fiber, or a mixture thereof. According to the method for degrading a polyurethane acrylic resin material described in the preceding paragraph, the degradation compound may have a structure as shown in formula (i):
[0002] NHmfX-OH) n Formula (1), wherein X is an alkyl or oxyalkyl group, m is 1 or 2, and m + n = 3. According to the method for degrading a polyurethane acrylic resin material described in the preceding paragraph, the degradation temperature may be from 135°C to the boiling point of the degradation solution. According to the method for degrading a polyurethane acrylic resin material described in the preceding paragraph, the degradation time may be from 2 hours to 24 hours. According to the method for degrading a polyurethane acrylic resin material described in the preceding paragraph, more than 40% of the total weight of the polyurethane acrylic resin may be oligomers. According to the method for degrading a polyurethane acrylic resin material described in the preceding paragraph, the oligomers may have Formula (I), wherein A is a polyethoxy group, a polypropoxy group, or a polytetrahydrofuranyl group. According to the method for degrading a polyurethane acrylic resin material described in the preceding paragraph, the preparation of the polyurethane acrylic resin may include a polyurethane polymerization step and a polyurethane acrylate esterification step. The polyurethane polymerization step comprises mixing an isocyanate compound, an inhibitor, and a catalyst in a diluent monomer, heating the mixture to a first temperature to obtain a first mixture, then adding a polyol compound to the first mixture and maintaining the reaction at the first temperature to obtain a second mixture. The polyurethane acrylate esterification step comprises adding a hydroxyl-containing (meth)acrylate compound to the second mixture and maintaining the reaction at the first temperature to obtain a polyurethane acrylic resin. According to the method for degrading a polyurethane acrylic resin material described in the preceding paragraph, the preparation of the polyurethane acrylic resin may further include a dilution step, wherein the second mixture containing the hydroxyl-containing (meth)acrylate compound is reacted at the first temperature, then cooled and the diluent monomer is added to obtain the polyurethane acrylic resin. According to the method for degrading a polyurethane acrylic resin material described in the preceding paragraph, the isocyanate compound may be a difunctional or polyfunctional isocyanate compound. Furthermore, the bifunctional or multifunctional isocyanate compound may be an aromatic ring isocyanate. According to the method for degrading a polyurethane acrylic resin material described in the preceding paragraph, the aromatic ring isocyanate may be tolyl diisocyanate, polymethylene phenyl isocyanate, diphenylmethane diisocyanate, or a mixture thereof. According to the method for degrading a polyurethane acrylic resin material described in the preceding paragraph, the polyol compound may be a bifunctional or multifunctional polyol compound, and the number average molecular weight of the polyol compound may be less than 2000. Furthermore, the polyol compound may be polyoxyethylene amide, polyoxypropylene amide, polytetrahydrofuran, or a mixture thereof. According to the method for degrading a polyurethane acrylic resin material described in the preceding paragraph, the polyurethane acrylic resin compound may be a bifunctional or multifunctional polyol compound, and the number average molecular weight of the polyol compound may be less than 2000. Formula (I), wherein A is a polyethoxy group, a polypropoxy group, or a polytetrahydrofuranyl group. According to the method for degrading a polyurethane acrylic resin material described in the preceding paragraph, the equivalent ratio of the NCO group of the isocyanate compound to the OH group of the polyol compound can be 1.5:1 to 10:1. According to the method for degrading a polyurethane acrylic resin material described in the preceding paragraph, the hydroxyl-containing (meth)acrylate compound can be hydroxyethyl methacrylate, hydroxyethyl acrylate, hydroxypropyl methacrylate, hydroxypropyl acrylate, or a mixture thereof. According to the method for degrading a polyurethane acrylic resin material described in the preceding paragraph, the diluent monomer can be a free radical-curable diluent monomer and can be methyl (meth)acrylate, ethyl (meth)acrylate, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, isobornyl (meth)acrylate, cyclohexane (meth)acrylate, tetrahydrofuranyl (meth)acrylate, styrene, methylstyrene, vinyltoluene, or a mixture thereof. According to the method for degrading a polyurethane acrylic resin material described in the preceding paragraph, the first temperature may be between 40°C and 80°C. According to the method for degrading a polyurethane acrylic resin material described in the preceding paragraph, the catalyst may be organotin, organotin, or organozinc, and the amount of the catalyst added may be between 50 ppm and 200 ppm based on the total content of the polyurethane acrylic resin. According to the method for degrading a polyurethane acrylic resin material described in the preceding paragraph, the equivalent ratio of the OH groups of the hydroxyl-containing (meth)acrylate compound to the NCO groups of the isocyanate compound remaining after the reaction may be between 1:1 and 1.05:1. Another embodiment of the present invention provides a composition for preparing a polyurethane acrylic resin, comprising an isocyanate compound, a polyol compound, a hydroxyl-containing (meth)acrylate compound, and a diluent monomer. Yet another embodiment of the present invention provides a method for preparing a polyurethane acrylic resin, comprising a polyurethane polymerization step, a polyurethane acrylate esterification step, and a dilution step. The polyurethane polymerization step involves mixing an isophthalate ester compound, an inhibitor, and a catalyst in a diluent monomer and heating the mixture to a first temperature to produce a first mixture. The polyol compound is then added to the first mixture and the mixture is maintained at the first temperature to react and produce a second mixture. The polyurethane acrylate step involves adding a hydroxyl-containing (meth)acrylate compound to the second mixture and maintaining the reaction temperature at the first temperature to produce a third mixture. The dilution step involves cooling the third mixture and adding the diluent monomer to produce a polyurethane acrylic resin.Another embodiment of the present invention provides a polyurethane acrylic resin, which comprises the following formula (1): Formula (I), wherein A is polyethoxy, polypropoxy or polytetrahydrofuranyl. A further embodiment of the present invention provides a composite material containing a cured polyurethane acrylic resin, comprising a polyurethane acrylic resin and a fiber, wherein the polyurethane acrylic resin comprises a polyurethane acrylic resin as shown in Formula (I): Formula (I), wherein A is a polyethoxy group, a polypropoxy group, or a polytetrahydrofuranyl group. According to the composite material containing a cured polyurethane acrylic resin described in the preceding paragraph, the fibers may be glass fibers, carbon fibers, polyamide fibers, or a mixture thereof. Thus, the method for degrading a polyurethane acrylic resin material of the present invention primarily utilizes a degradation solution containing reactive NH or NH2 groups and OH groups to degrade the polyurethane acrylic resin material by heating, and the degradation solution can be separated by vacuum steaming for reuse. Brief Description of the Drawings To facilitate understanding of the above and other objects, features, advantages, and embodiments of the present invention, the drawings are described as follows: FIG1 is a flow chart illustrating the steps of a polyurethane acrylic resin degradation method according to one embodiment of the present invention. FIG2 is a flow chart illustrating the steps of a polyurethane acrylic resin preparation method according to another embodiment of the present invention. FIG3 is a flow chart illustrating the steps of a polyurethane acrylic resin preparation method according to yet another embodiment of the present invention.
[0003] [Main component symbol description] 100: Degradation method of polyurethane acrylic resin material
[0004] 200,300: Preparation method of polyurethane acrylic resin
[0005] 110, 120, 130, 140, 210, 220, 310, 320, 330: Steps for Best Modes of Implementing the Invention The following describes various embodiments of the present invention in greater detail. However, these embodiments may encompass various applications of the inventive concepts and may be embodied within a variety of specific scopes. The specific embodiments are provided for illustrative purposes only and are not intended to limit the scope of this disclosure.
[0006] <Polyurethane Acrylic Resin Material Degradation Method> Please refer to Figure 1, which is a flow chart illustrating a polyurethane acrylic resin material degradation method 100 according to one embodiment of the present invention. In Figure 1, polyurethane acrylic resin material degradation method 100 includes steps 110, 120, 130, and 140. Step 110 involves providing a polyurethane acrylic resin material, which is obtained by curing a polyurethane acrylic resin. Specifically, the polyurethane acrylic resin material of the present invention can be a polyurethane acrylic resin cured product or a composite material containing a polyurethane acrylic resin cured product. The polyurethane acrylic resin cured product can be cured at room temperature or elevated temperature by adding a conventional accelerator and a free radical initiator to form a network-like crosslinked cured product. The composite material containing a polyurethane acrylic resin cured product is obtained by impregnating a polyurethane acrylic resin with fibers at room temperature or elevated temperature. The fibers can be glass fibers, carbon fibers, polyamide fibers, or a mixture thereof, but are not limited thereto. Step 120 involves providing a degradation solution, which at least contains a degradation compound, and the degradation compound contains at least reactive NH or NH2 groups and reactive OH groups. Specifically, the reactive NH or NH? groups and reactive OH groups serve as functional groups that react with the polyurethane acrylic resin, allowing aminolysis and alcoholysis without damaging the fibers in the composite material. Specifically, the degradation compound may have a structure as shown in formula (i): NHm(x-OH) nFormula (i> wherein X is an alkyl or oxyalkyl group, m is 1 or 2, and m + n = 3, can have sufficient reactivity to the polyurethane acrylic resin without adding a catalyst, achieving the purpose of high-efficiency degradation. Step 130 is a mixing step, which is to mix the polyurethane acrylic resin material with the degradation liquid to form a degradation mixture. Step 140 is a heating step, which is to heat the degradation mixture to a degradation temperature and maintain the degradation time to degrade the polyurethane acrylic resin material. The degradation temperature can be from 135°C to the boiling point of the degradation liquid, and the degradation time can be from 2 hours to 24 hours. In this way, the present invention reacts the polyurethane acrylic resin material containing network crosslinks with the degradation liquid containing at least reactive NH or NH2 groups and reactive OH groups through aminolysis and alcoholysis, and achieves a high-efficiency degradation effect by increasing the temperature. The highest degradation temperature can be achieved at the boiling point of the degradation liquid. The excess degradation liquid can act as a solvent during the degradation process to dilute and suspend the fibers. After degradation is complete, the volatile substances can be separated by decompression steaming. This volatile substance is the degradation liquid containing reactive NH or Nth groups and OH groups, and can be reused. In addition, after degradation, the composite material containing the polyurethane acrylic resin solid can be decomposed and removed to form recycled fibers without plastic attachment, thus realizing a recycling mechanism for separating fibers and organic matter. According to the polyurethane acrylic resin material degradation method 100 of the present invention, the polyurethane acrylic resin Formula (I), wherein A is a polyethoxy group, a polypropoxy group, or a polytetrahydrofuranyl group. The preparation of the polyurethane acrylic resin according to the present invention is described below with reference to FIG2 , which illustrates a flow chart of a method 200 for preparing a polyurethane acrylic resin according to another embodiment of the present invention. In FIG2 , the method 200 for preparing a polyurethane acrylic resin comprises steps 210 and 220. Step 210 is a polyurethane polymerization step, in which an isocyanate compound, an inhibitor, and a catalyst are mixed in a diluted monomer and heated to a first temperature to obtain a first mixture. A polyol compound is then added to the first mixture and the mixture is maintained at the first temperature to react to obtain a second mixture. Step 220 is a polyurethane acrylate esterification step, in which a hydroxyl-containing (meth)acrylate compound is added to the second mixture and the mixture is maintained at the first temperature to react to obtain a polyurethane acrylic resin. The aforementioned isoester compound may be a difunctional or multifunctional isocyanate compound. The difunctional or multifunctional isocyanate compound may be an aromatic ring isocyanate, and the aromatic ring isocyanate may be tolyl diisocyanate, polymethylene phenyl isocyanate, diphenylmethane diisocyanate, or a mixture thereof. Specifically, the aforementioned isocyanate compound may be, but is not limited to, one or more of MR200 (available from Tosoh), PM200 (available from Wanhua), M20S (available from BASF), 44V20 (available from Costron), 5005 (available from Huntsman), NM (available from Tosoh), and MDI-50 (available from Wanhua). The aforementioned inhibitor is a conventional inhibitor added to conventional free radical curing resins to ensure the storage stability (stability) of the resin. A suitable inhibitor may be selected from conventional inhibitors as needed and will not be further described here. The catalyst may be organotin, organotin, or organozinc, and the added amount of the catalyst may be 50 ppm to 200 ppm based on the total content of the polyurethane acrylic resin. The diluent monomer is a free radical curable diluent monomer and may be methyl (meth)acrylate, ethyl (meth)acrylate, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, isobornyl (meth)acrylate, cyclohexane (meth)acrylate, tetrahydrofuranyl (meth)acrylate, styrene, methylstyrene, vinyltoluene, or a mixture thereof. The first temperature may be 40°C to 80°C, preferably 50°C to 70°C.The aforementioned polyol compound can be a difunctional or multifunctional polyol compound, such as polyoxyethylene amide, polyoxypropylene amide, polytetrahydrofuran, or a mixture thereof. The number average molecular weight of the polyol compound should be less than 2000. If the number average molecular weight of the polyol compound exceeds 2000, it will be difficult to achieve the desired high-rigidity composite material. The aforementioned hydroxyl-containing (meth)acrylate compound can be hydroxyethyl methacrylate (2-HEMA), hydroxyethyl acrylate (2-HEA), hydroxypropyl methacrylate (2-HPMA), hydroxypropyl acrylate (2-HPA), or a mixture thereof. The equivalent ratio of NCO groups in the aforementioned isocyanate compound to OH groups in the polyol compound can be between 1.5:1 and 10:1. When the NCO group / OH group ratio is less than 1.5, the polymer molecular weight will be too high and the rigidity will be insufficient. When the NCO group / OH group ratio is greater than 10, the rigidity after curing will be too high and the degradation efficiency will be poor. Furthermore, step 210 leaves residual NCO groups of the isocyanate compound, allowing the hydroxyl-containing (meth)acrylate compound in step 220 to react with them. The equivalent ratio of the OH groups of the hydroxyl-containing (meth)acrylate compound to the NCO groups of the isocyanate compound remaining after the reaction can be 1:1 to 1.05:1. The aforementioned polyurethane acrylic resin comprises an oligomer as represented by Formula (1). For details about the oligomer, please refer to the above description and will not be further described here. Specifically, the composition of the aforementioned polyurethane acrylic resin comprises an isocyanate compound, a polyol compound, a hydroxyl-containing (meth)acrylate compound, and a diluent monomer. The oligomer is synthesized from the isocyanate compound, the polyol compound, and the hydroxyl-containing (meth)acrylate compound. The preparation of the polyurethane acrylic resin according to the polyurethane acrylic resin degradation method 100 of the present invention can also be described below with reference to FIG. FIG. 3 illustrates a flow chart of a method 300 for preparing a polyurethane acrylic resin according to another embodiment of the present invention. In Figure 3, method 300 for preparing a polyurethane acrylic resin includes steps 310, 320, and 330. Details of steps 310 and 320 are described in detail in steps 210 and 220 above and are omitted here. Specifically, step 330 is a dilution step, wherein the second mixture containing the hydroxyl (meth)acrylate compound is reacted at a first temperature (i.e., the third mixture), the temperature is then lowered, and a diluting monomer is added to obtain the polyurethane acrylic resin.Specifically, step 330 involves adjusting the operating viscosity. The optimal viscosity of vacuum infusion resin is 100 to 250 cps, while the optimal viscosity of hand lay-up resin is 300 to 450 cps. By adding an appropriate amount of diluent monomer in step 330 to control the viscosity of the polyurethane acrylic resin, a polyurethane acrylic resin suitable for operation is obtained, thereby facilitating subsequent applications of the polyurethane acrylic resin material. These applications refer to the manufacture of corresponding products using processes such as hand lay-up, compression molding, prepreg molding, pultrusion, filament winding, resin transfer molding, and vacuum infusion molding. Regarding the diluent monomer, please refer to the previous description and will not be elaborated here. Furthermore, the dilution step in the polyurethane acrylic resin preparation method 300 of the present invention is determined by the viscosity requirements of the operating process. In the polyurethane acrylic resin preparation method 200 of the present invention, the polyurethane acrylic resin of the present invention is obtained after the polyurethane acrylate esterification step. The polyurethane acrylic resin of the present invention utilizes a polyurethane chain extension reaction between a difunctional or higher-functional isocyanate and a polyol, followed by end-capping with a hydroxyl-containing acrylate compound. The resulting product is then diluted with a free-radical curable diluent monomer according to the operating viscosity to obtain a degradable polyurethane acrylic resin. Specifically, the reaction equation for the preparation method of the polyurethane acrylic resin of the present invention is shown in Table 1 below, where M represents the diluent monomer, which forms a network copolymer structure with the polyurethane acrylic resin after free-radical curing. The urethane acrylic resin structure undergoes alcoholysis and aminolysis to form small-molecule aminocarboxylic acid esters, small-molecule urea esters, polyols, and polyacrylic acid molecules. Under continued action, the final degradation products are speculated to be aromatic amine compounds, oxadione, urethane alcoholamine, and aminodiol.
[0007] At least 40% of the total weight of the polyurethane acrylic resin is comprised of oligomers prepared from the composition for preparing the polyurethane acrylic resin of the present invention. The oligomers have a structure as shown in Formula (I) of the present invention, but are not limited thereto. The polyurethane acrylic resin material of the present invention can be used in surface coatings, adhesives, 3D printing, or as a main structural layer. Fillers such as titanium dioxide, silica, calcium carbonate, aluminum oxide, aluminum hydroxide, silicon carbide, or combinations thereof can be added depending on the function, thereby enabling applications in the manufacture of automotive parts, marine parts, railcar parts, sports product parts, aviation parts, wind turbine parts, furniture parts, and architectural components. The following specific examples further illustrate the present invention and are intended to facilitate those skilled in the art to utilize and practice the present invention without undue interpretation. These examples should not be construed as limiting the scope of the present invention, but rather serve to illustrate how to implement the materials and methods of the present invention.
[0008] 〈Synthesis example〉
[0009] Synthesis of Polyurethane Acrylic Resin Synthesis Example 1: 280 g of polymethylene phenyl isophthalate, 0.318 g of 2,5-dihydroxytoluene, and 0.159 g of a catalyst (DBTDL) were dispersed in 228 g of methyl methacrylate, mixed thoroughly in a reaction kettle, and heated to 45°C to 60°C. Next, 138.9 g of polypropylene glycol (PPG400) was slowly added dropwise to the reaction kettle over a period of 40 to 60 minutes, maintaining the temperature below 60°C. After addition, the temperature was maintained at 45°C to 60°C for 2 to 4 hours. Next, 180.8 g of hydroxyethyl methacrylate (2-HEMA) was slowly added dropwise over a period of 40 to 60 minutes, maintaining the temperature below 60°C. After addition, the temperature was maintained at 45°C to 60°C for 2 to 4 hours. When the NCO value was lower than 0.5%, 228 g of methyl methacrylate was added for dilution to obtain the polyurethane acrylic resin of Synthesis Example 1, having a viscosity of 130 cps / s. Synthesis Example 2: 250 g of polymethylene phenyl isophthalate, 0.317 g of 2,5-dihydroxytoluene, and 0.159 g of a catalyst (DBTDL) were dispersed in 227 g of methyl methacrylate, mixed uniformly in a reaction kettle, and heated to 45°C to 60°C for later use. Next, 186 g of polyethylene glycol (PEG600) was slowly added dropwise to the reaction kettle over a period of 40 to 60 minutes, maintaining the temperature below 60°C during the addition. After the addition was complete, the temperature was maintained at 45°C to 60°C for 2 to 4 hours. Then, 161.4 g of hydroxyethyl methacrylate (2-HEMA) was slowly added dropwise over 40 to 60 minutes, maintaining the temperature below 60°C. After the addition was complete, the mixture was maintained at 45°C to 60°C for 2 to 4 hours. When the NCO value was below 0.5%, 227 g of methyl methacrylate was added for dilution to obtain the polyurethane acrylic resin of Synthesis Example 2, which had a viscosity of 320 cps / s. Synthesis Example 3: 330 g of polymethylene phenyl isophthalate, 0.308 g of 2,5-dihydroxytoluene, and 0.179 g of catalyst (DBTDL) were dispersed in 169 g of methyl methacrylate, mixed uniformly in a reactor, and heated to 45°C to 60°C for later use. Next, 61.4 g of polypropylene glycol (PPG400) was slowly added dropwise to the reactor over a period of 4 minutes.The reaction mixture was added dropwise for 40 to 60 minutes, maintaining the temperature below 60°C during the addition. After the addition was complete, the temperature was raised to 45°C to 60°C and maintained at this temperature for 2 to 4 hours. Subsequently, 293.6 g of hydroxyethyl methacrylate (2-HEMA) was slowly added dropwise over a period of 40 to 60 minutes, maintaining the temperature below 60°C during the addition. After the addition was complete, the temperature was raised to 45°C to 60°C and maintained at this temperature for 2 to 4 hours. When the NCO value was lower than 0.5%, 169 g of styrene was added for dilution to obtain the polyurethane acrylic resin of Synthesis Example 3, with a viscosity of 300 cps / s. Synthesis Example 4: 270 g of a mixture of 2,4-diphenylmethane diisocyanate and 4,4'-diphenylmethane diisocyanate, 0.287 g of 2,5-dihydroxytoluene, and 0.143 g of a catalyst (DBTDL) were dispersed in 167 g of methyl methacrylate, mixed uniformly in a reactor, and heated to 45°C to 60°C for later use. Next, 143.6 g of polypropylene glycol (PPG400) was slowly added dropwise to the reactor over 40 to 60 minutes, maintaining the temperature below 60°C during the addition. After the addition was complete, the temperature was maintained at 45°C to 60°C for 2 to 4 hours. Next, 206.7 g of hydroxypropyl methacrylate (2-HPMA) was slowly added dropwise over 40 to 60 minutes, maintaining the temperature below 60°C. After the addition was complete, the mixture was maintained at 45°C to 60°C for 2 to 4 hours. When the NCO value dropped below 0.5%, 207 g of methyl methacrylate was added for dilution to obtain the polyurethane acrylic resin of Synthesis Example 4, which had a viscosity of 150 cps / s. Synthesis Example 5: 150 g of polymethylene phenyl isophthalate, 0.309 g of 2,5-dihydroxytoluene, and 0.181 g of a catalyst (DBTDL) were dispersed in 412 g of methyl methacrylate, mixed thoroughly in a reaction kettle, and heated to 45°C to 60°C for later use. Next, 372.0 g of polypropylene glycol (PPG2000) was slowly added dropwise to the reactor over a period of 40 to 60 minutes, maintaining the temperature below 60°C. After the addition was complete, the mixture was heated to 45°C to 60°C and maintained at this temperature for 2 to 4 hours. Next, 96.8 g of hydroxyethyl methacrylate (2-HEMA) was slowly added dropwise over a period of 40 to 60 minutes, maintaining the temperature below 60°C. After the addition was complete, the mixture was heated to 45°C to 60°C and maintained at this temperature for 2 to 4 hours.When the NCO value is lower than 0.5%, it is the polyurethane acrylic resin of Synthesis Example 5, and its viscosity is 400 cpso.
[0010] <Preparation of Polyurethane Acrylic Resin Materials> Polyurethane acrylic resin materials can include cured polyurethane acrylic resins and composite materials containing cured polyurethane acrylic resins. Specifically, the polyurethane acrylic resins of Synthesis Examples 1 to 5 were cured at room temperature for 24 hours by adding cobalt 2-ethylhexanoate (0.1% to 0.2%) and methyl ethyl ketone peroxide (1% to 2%). The cured polyurethane acrylic resins of Synthesis Examples 6 to 10 were then baked at 105°C for 2 hours. Alternatively, depending on the specific process requirements, the curing system of the polyurethane acrylic resin can be adjusted to an appropriate gelation time, followed by room temperature fiber impregnation molding, followed by baking at 105°C for 2 hours to produce a cured composite material containing fibers.
[0011] <Examples / Comparative Examples> Example 1: 5 grams of the cured polyurethane acrylic resin of Synthesis Example 6 and 2-aminoethanol at a weight ratio of 1:5 were placed in a round-bottom flask equipped with a serpentine condenser. The mixture was held at 135°C for 10 hours. A clear solution was obtained, indicating smooth degradation. Example 2: 5 grams of the cured polyurethane acrylic resin of Synthesis Example 6 and 2-aminoethoxyethanol at a weight ratio of 1:5 were placed in a round-bottom flask equipped with a serpentine condenser. The mixture was held at 135°C for 24 hours. A clear solution was obtained, indicating smooth degradation. Comparative Example 1: 5 grams of the cured polyurethane acrylic resin of Synthesis Example 6 and ethylene glycol at a weight ratio of 1:5 were placed in a round-bottom flask equipped with a serpentine condenser. The mixture was held at 135°C for 24 hours. The result was a complete, undissolved solid, indicating poor degradation efficiency. Comparative Example 2: 5 grams of the polyurethane acrylic resin cured product from Synthesis Example 6 and triethylenetetramine were placed in a round-bottom flask equipped with a serpentine condenser at a weight ratio of 1:5. The mixture was then held at 135°C for 24 hours. Undissolved solids remained intact, indicating poor degradation efficiency. The resin types, cured product types, degradation solution types, degradation times (hours), and degradation status for Examples 1, 2, Comparative Examples 1, and 2 are shown in Table 3 below. The results in Table 3 above show that the degradation solutions containing reactive NH2 and OH groups used in Examples 1 and 2 can indeed degrade polyurethane acrylic resin to obtain a clear solution. Example 3: 5 grams of the cured polyurethane acrylic resin of Synthesis Example 7 and 2-aminoethanol were placed in a round-bottom flask equipped with a serpentine condenser at a weight ratio of 1:5. The mixture was then maintained at 135°C for 10 hours. A clear solution was obtained, demonstrating successful degradation. Example 4: 5 grams of the cured polyurethane acrylic resin of Synthesis Example 8 and 2-aminoethanol were placed in a round-bottom flask equipped with a serpentine condenser at a weight ratio of 1:5. The mixture was then maintained at 135°C for 10 hours. A clear solution was obtained, demonstrating successful degradation. Example 5: 5 grams of the cured polyurethane acrylic resin of Synthesis Example 9 and 2-aminoethanol were placed in a round-bottom flask equipped with a serpentine condenser at a weight ratio of 1:5. The mixture was then maintained at 135°C for 10 hours. A clear solution was obtained, demonstrating successful degradation. Example 6: 5 grams of the cured polyurethane acrylic resin from Synthesis Example 10 and 2-aminoethanol were placed in a round-bottom flask equipped with a serpentine condenser at a weight ratio of 1:5. The mixture was then maintained at 135°C for 10 hours. A powdery precipitate solution was obtained, demonstrating smooth degradation. The resin types, cured product types, degradation times (hours), and degradation profiles for Examples 3 to 6 are shown in Table 4 below. Example 7: The glass fibers of Synthesis Example 1 were vacuum infused, with a fiber content of 68% to 75% by weight. After complete curing, the fibers were cut into appropriate sizes and loaded into a round-bottom flask equipped with a serpentine condenser tube at a weight ratio of 1:5 with 2-aminoethanol. The solution was then maintained at 150°C for 2 hours to obtain a solution for separating the fibers from the polyurethane acrylic resin. The fibers were then rinsed with ethanol / water, allowing for smooth fiber recovery. Example 8: The carbon fibers of Synthesis Example 1 were vacuum infused, with a fiber content of 5% to 55% by weight. After complete curing, the fibers were cut into appropriate sizes and loaded into a round-bottom flask equipped with a serpentine condenser tube at a weight ratio of 1:5 with 2-aminoethanol. The solution was then maintained at 150°C for 2 hours to obtain a solution for separating the fibers from the polyurethane acrylic resin. The fibers were then rinsed with ethanol / water, allowing for smooth fiber recovery. Example 9: The aromatic polyamide fibers from Synthesis Example 1 were vacuum-infused to a fiber content of 50% to 55% by weight. After complete curing, the fibers were cut into appropriate sizes and loaded into a round-bottom flask equipped with a serpentine condenser tube at a weight ratio of 1:5 with 2-aminoethanol. The solution was then maintained at 150°C for 2 hours to obtain a solution separating the fibers from the polyurethane acrylic resin. The fibers were then rinsed with ethanol / water, allowing smooth fiber recovery. Example 1: The glass fibers from Synthesis Example 3 were hand-laid to a fiber content of 3% to 50% by weight. After complete curing, the fibers were cut into appropriate sizes and loaded into a round-bottom flask equipped with a serpentine condenser tube at a weight ratio of 1:5 with 2-aminoethanol. The solution was then maintained at 150°C for 2.5 hours to obtain a solution separating the fibers from the polyurethane acrylic resin. The fibers were then rinsed with ethanol / water, allowing smooth fiber recovery. The resin type, fiber type, degradation time (hours) and degradation status of Examples 7 to 10 are shown in Table 5 below. The results in Table 5 above demonstrate that after degradation of a composite material containing polyurethane acrylic resin and fibers using a degradation solution containing reactive NH2 and OH groups, the polyurethane acrylic resin can be decomposed and removed, separating the resin from the fibers, leaving behind plastic-free fibers, which can be recycled and reused. In summary, the present invention utilizes a degradation solution containing reactive NH2 or NH2 groups and OH groups, and heat to degrade polyurethane acrylic resin materials, achieving highly efficient depolymerization. Furthermore, the degraded solution can be recycled and reused, achieving the goal of reducing waste. While the present invention has been disclosed above with reference to specific embodiments, this is not intended to be limiting. Persons skilled in the art will readily be able to make various modifications and alterations without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be determined by the claims.
Claims
Claims 1. A method for degrading polyurethane acrylic resin material. It is characterized in that The method comprises: providing a polyurethane acrylic resin material obtained by curing a polyurethane acrylic resin; providing a degradation liquid, which at least comprises a degradation compound, and the degradation compound at least comprises a reactive NH or NH2 group and a reactive OH group; performing a mixing step, which is to mix the polyurethane acrylic resin material with the degradation liquid to form a degradation mixture; and performing a heating step, which is to heat the degradation mixture to a degradation temperature and maintain the degradation time to degrade the polyurethane acrylic resin material.
2. The method for degrading the polyurethane acrylic resin material according to claim 1, It is characterized in that The polyurethane acrylic resin material is a polyurethane acrylic resin cured product or a composite material containing the polyurethane acrylic resin cured product.
3. The method for degrading the polyurethane acrylic resin material according to claim 2, It is characterized in that The composite material containing polyurethane acrylic resin cured product comprises the polyurethane acrylic resin and fibers.
4. The method for degrading the polyurethane acrylic resin material according to claim 3, It is characterized in that The fiber is glass fiber, carbon fiber, polyamide fiber or a mixture thereof.
5. The method for degrading the polyurethane acrylic resin material according to claim 1, It is characterized in that The degradation compound has a structure as shown in formula (1): NHmfX-OH) n Formula (1) Wherein, X is an alkyl or oxyalkyl group, m is 1 or 2 and m + n = 3.
6. The method for degrading the polyurethane acrylic resin material according to claim 1, It is characterized in that The degradation temperature is from 135°C to the boiling point of the degradation liquid.
7. The method for degrading the polyurethane acrylic resin material according to claim 1, It is characterized in that The degradation time is from 2 hours to 24 hours.
8. The method for degrading the polyurethane acrylic resin material according to claim 1, It is characterized in that More than 40% of the total weight of the polyurethane acrylic resin is oligomers.
9. The method for degrading polyurethane acrylic resin material according to claim 8, characterized in that Formula (I); wherein A is polyethoxy, polypropoxy or polytetrahydrofuranyl.
10. The method for degrading the polyurethane acrylic resin material according to claim 1, It is characterized in that The preparation of the polyurethane acrylic resin comprises the following steps: a polyurethane polymerization step, wherein an isocyanate compound, an inhibitor and a catalyst are mixed in a diluent monomer, and the mixture is heated to a first temperature to obtain a first mixture, and then a polyol compound is added to the mixture. Adding the hydroxyl (meth)acrylate compound to the first mixture and maintaining the reaction at the first temperature to obtain the second mixture; and performing a polyurethane acrylate esterification step, which is adding the hydroxyl (meth)acrylate compound to the second mixture and maintaining the reaction at the first temperature to obtain the polyurethane acrylic resin.
11. The method for degrading the polyurethane acrylic resin material according to claim 10, It is characterized in that The preparation of the polyurethane acrylic resin further comprises: performing a dilution step, wherein the second mixture to which the hydroxyl (meth)acrylate compound is added reacts at the first temperature, then the temperature is lowered and the dilution monomer is added to obtain the polyurethane acrylic resin.
12. The method for degrading the polyurethane acrylic resin material according to claim 10 or 11, It is characterized in that The isocyanate compound is a bifunctional or polyfunctional isocyanate compound.
13. The method for degrading the polyurethane acrylic resin material according to claim 12, It is characterized in that The bifunctional or multifunctional isocyanate compound is an aromatic ring isocyanate.
14. The method for degrading the polyurethane acrylic resin material according to claim 13, It is characterized in that The aromatic ring isocyanate is tolyl diisocyanate, polymethylene phenyl isocyanate, diphenylmethane diisocyanate or a mixture thereof.
15. The method for degrading the polyurethane acrylic resin material according to claim 10 or 11, It is characterized in that The polyol compound is a difunctional or multifunctional polyol compound, and the number average molecular weight of the polyol compound is less than 2000.
16. The method for degrading the polyurethane acrylic resin material according to claim 15, It is characterized in that The polyol compound is polyoxyethylene amide, polyoxypropylene amide, polytetrahydrofuran or a mixture thereof.
17. The method for degrading the polyurethane acrylic resin material according to claim 10 or 11, Formula (I); wherein A is polyethoxy, polypropoxy or polytetrahydrofuranyl.
18. The method for degrading the polyurethane acrylic resin material according to claim 10 or 11, It is characterized in that The equivalent ratio of the NCO group of the isocyanate compound to the OH group of the polyol compound is 1.5:1 to 10:
1.
19. The method for degrading the polyurethane acrylic resin material according to claim 10 or 11, It is characterized in that The hydroxyl (meth)acrylate compound is hydroxyethyl methacrylate, hydroxyethyl acrylate, hydroxypropyl methacrylate, hydroxypropyl acrylate or a mixture thereof.
2. The method for degrading a polyurethane acrylic resin material according to claim 10 or 11, It is characterized in that The diluent monomer is a free radical curable diluent monomer, and is methyl (meth)acrylate, ethyl (meth)acrylate, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, isobornyl (meth)acrylate, cyclohexane (meth)acrylate, tetrahydrofuran (meth)acrylate, styrene, methylstyrene, vinyltoluene or a mixture thereof.
21. The method for degrading the polyurethane acrylic resin material according to claim 10 or 11, It is characterized in that The first temperature is 40°C to 80°C 22. The method for degrading the polyurethane acrylic resin material according to claim 10 or 11, It is characterized in that The catalyst is organic tin, organic zirconium or organic zinc, and the added amount of the catalyst is 50 ppm to 200 ppm of the total content of the polyurethane acrylic resin.
23. The method for degrading the polyurethane acrylic resin material according to claim 10 or 11, It is characterized in that The equivalent ratio of the OH group of the hydroxyl-containing (meth)acrylate compound to the NCO group of the isocyanate compound remaining after the reaction is 1:1 to 1.05:
1.
24. A composition for preparing polyurethane acrylic resin, It is characterized in that The invention comprises an isocyanate compound, a polyol compound, a hydroxyl-containing (meth)acrylate compound and a diluent monomer.
25. A method for preparing polyurethane acrylic resin. It is characterized in that The method comprises: performing a polyurethane polymerization step, which is to mix an isocyanate compound, an inhibitor and a catalyst in a diluent monomer, and heating the mixture to a first temperature to obtain a first mixture, and then adding a polyol compound to the first mixture, and maintaining the mixture at the first temperature to react to obtain a second mixture; performing a polyurethane acrylate step, which is to add a hydroxyl (methyl) acrylate compound to the second mixture, and maintaining the mixture at the first temperature to react to obtain a third mixture; and performing a dilution step, which is to cool the third mixture and add the diluent monomer to obtain a polyurethane acrylic resin.
26. A polyurethane acrylic resin, It is characterized in that Contains an oligomer as shown in formula (I) Formula (I); wherein A is polyethoxy, polypropoxy or polytetrahydrofuranyl.
27. A composite material containing a cured polyurethane acrylic resin, It is characterized in that It comprises a polyurethane acrylic resin and fibers, wherein the polyurethane acrylic resin comprises a Formula (I); wherein A is polyethoxy, polypropoxy or polytetrahydrofuranyl.
28. The composite material containing polyurethane acrylic resin cured product according to claim 27, characterized in that the fiber is glass fiber, carbon fiber, polyamide fiber or a mixture thereof.