Sputtering target

MYPI2025003333A0Undetermined Publication Date: 2024-06-05SANYO SPECIAL STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025003333
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-12-05
Filing Date
2023-10-13
Publication Date
2024-06-05

AI Technical Summary

Technical Problem

Existing sputtering targets fail to produce thin films with sufficiently fine crystal structures, and they are prone to cracking during the sputtering process.

Method used

A sputtering target made of a Cr-based alloy with a composition of 10.0 at% to 30.0 at% boron (B), containing both a CrB phase and a Cr single phase, with specific X-ray diffraction peak ratios and low oxygen content, is used to form a homogeneous thin film that is resistant to cracking.

Benefits of technology

The target produces a homogeneous thin film with small grain size and high smoothness, suitable for applications like adhesion layers in perpendicular magnetic recording media, while being resistant to cracking during sputtering due to its enhanced toughness and boron dispersion.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

There is provided a sputtering target that has Cr as a main component and that can be used to obtain a uniform thin film. The sputtering target is composed of a Cr-based alloy. The Cr-based alloy contains 10.0 at% or more and 30.0 at% or less of B. A metal structure of the target includes a CrB phase and a Cr single phase. A ratio of an X-ray diffraction peak associated with a (111) plane of the CrB phase to an X-ray diffraction peak associated with a (110) plane of the Cr single phase is 10% or more and 80% or less. In a three-point bending test, the target has a flexural strength of preferably 300 MPa or more. The oxygen content of the Cr-based alloy is preferably 2000 ppm or less.
Need to check novelty before this filing date? Find Prior Art

Description

Sputtering Target

[0001] The present disclosure relates to a target used in sputtering to form a metal thin film.

[0002] Sputtering is a well-known method for forming thin films. In sputtering, a target is used. In sputtering, positive ions in the plasma collide with the target. These collisions cause atoms to fly out of the target. These atoms then adhere to the substrate, forming a thin film.

[0003] An example of a sputtering target is disclosed in Patent Document 1 (JP 2014-164780 A). The target disclosed in this publication is obtained by sintering powder. This powder is composed of a Cr-based alloy. From this target, a thin film (adhesion layer) suitable for perpendicular magnetic recording media can be obtained.

[0004] JP 2014-164780 A

[0005] There is a demand for a finer crystalline structure in thin films. The target disclosed in Patent Document 1 (JP 2014-164780 A) does not allow a thin film with a sufficiently fine crystalline structure to be obtained.

[0006] An object of the present disclosure is to provide a sputtering target that is mainly composed of Cr and that can yield a uniform thin film.

[0007] A sputtering target according to the present disclosure is made of a Cr-based alloy containing 10.0 at% to 30.0 at% B. The metal structure of this target includes a CrB phase and a single Cr phase. The ratio of the X-ray diffraction peak associated with the (111) plane of the CrB phase to the X-ray diffraction peak associated with the (110) plane of the single Cr phase is 10% to 80%.

[0008] Preferably, in this target, the X-ray diffraction peak of Cr relative to the (110) plane of the Cr single phase is 5 B 3 The ratio of the X-ray diffraction peak relating to the (213) plane of the phase is 20% or less.

[0009] Preferably, the target has a bending strength of 300 MPa or more in a three-point bending test.

[0010] Preferably, the oxygen content of the Cr-based alloy is 2000 ppm or less.

[0011] A method for manufacturing a sputtering target according to the present disclosure includes: (1) preparing a first powder composed of CrB; (2) preparing a second powder composed of Cr; (3) mixing the first powder and the second powder to obtain a mixed powder; and (4) pressurizing and heating the mixed powder.

[0012] Preferably, in step (2), the second powder has an average particle diameter D50 of 20 μm or more.

[0013] The sputtering target of the present invention can provide a uniform thin film, and the target is less likely to crack during sputtering.

[0014] Preferred embodiments will be described in detail below with reference to the drawings as appropriate.

[0015] The sputtering target according to this embodiment is made of a Cr-based alloy containing B. Preferably, in this alloy, the remainder other than Cr and B is unavoidable impurities. A thin film can be formed by sputtering using this target. This thin film is suitable for various applications. A typical application of the thin film is as an adhesion layer for a perpendicular magnetic recording medium. This adhesion layer can suppress orientation in the perpendicular magnetic recording medium.

[0016] Cr can contribute to the non-magnetic properties, adhesion, and corrosion resistance of the adhesion layer. Cr has a BCC structure and has a lattice constant with a small mismatch with the (001) layer (such as an MgO layer) on which the adhesion layer is laminated. Cr can suppress the orientation of the layer on which the adhesion layer is laminated. From these viewpoints, the Cr content in the Cr-based alloy is preferably 60 at% or more.

[0017] B combines with Cr. In the target, B exists as chromium boride. This boride is presumed to pin the growth of crystal grains. A thin film with a small crystal grain size can be formed from this target. Furthermore, B can realize a structure without crystal grain boundaries (amorphous). This structure is homogeneous and isotropic. This structure can contribute to the smoothness of the thin film. From these viewpoints, the B content in the Cr-based alloy is preferably 10 at% or more, more preferably 15 at% or more, and particularly preferably 20 at% or more. From the viewpoint of suppressing cracking of the target during sputtering, this content is preferably 30 at% or less.

[0018] The oxygen content (by mass) of the Cr-based alloy is preferably 2000 ppm or less. A target made of this Cr-based alloy is less likely to crack during sputtering. Furthermore, a thin film with fewer particles can be obtained from this target. From these viewpoints, the oxygen content is more preferably 1500 ppm or less, and particularly preferably 1000 ppm or less. Ideally, the oxygen content is less than the detection limit.

[0019] The metal structure of the target includes a CrB phase and a single Cr phase. The single Cr phase (hereinafter sometimes referred to as the Cr phase) has extremely excellent toughness. The toughness of the CrB phase is inferior to that of the single Cr phase. However, the CrB phase has superior toughness to other chromium borides. The metal structure including the CrB phase and the single Cr phase can suppress cracking of the target during sputtering.

[0020] Among the multiple peaks of the Cr phase obtained by X-ray diffraction, peak P1 corresponding to the (110) plane is the largest. Among the multiple peaks of the CrB phase obtained by X-ray diffraction, peak P2 corresponding to the (111) plane is the largest. The ratio of the X-ray diffraction peak P2 corresponding to the (111) plane of the CrB phase to the X-ray diffraction peak P1 corresponding to the (110) plane of the Cr phase is preferably 10% or more and 80% or less. In a target having this ratio of 10% or more, B is sufficiently dispersed and the amount of compounds with poor toughness is small. From these viewpoints, this ratio is more preferably 20% or more, and particularly preferably 25% or more. In a target having this ratio of 80% or less, the amount of the CrB phase is not excessive. This target is less likely to crack during sputtering. From this viewpoint, this ratio is more preferably 60% or less, and particularly preferably 40% or less.

[0021] Cr obtained by X-ray diffraction 5 B 3 Among the multiple peaks of the Cr phase, the peak P3 relating to the (213) plane is the largest. 5 B 3 The ratio of the X-ray diffraction peak P3 relating to the (213) plane of the Cr phase is preferably 20% or less. In a target in which this ratio is 20% or less, 5 B 3 The amount of the phase is not excessive. This target is less likely to crack during sputtering. From this viewpoint, this ratio is more preferably 10% or less, and particularly preferably 5% or less. Ideally, this ratio is 0%.

[0022] Peaks P1, P2, and P3 are measured using an X-ray diffraction device. A test piece for X-ray diffraction is cut out from the target by wire cutting. The surface of this test piece is smoothed by polishing. The measurement conditions are as follows: test piece size: 10 mm x 20 mm x 5 mm X-ray source: CuKα ray Scan speed: 4° / min 2θ: 20-80°. The peaks (peak intensity) are read from the chart obtained by this X-ray diffraction.

[0023] The flexural strength of the target is preferably 300 MPa or more. This target is less likely to crack during sputtering. From this viewpoint, the flexural strength is more preferably 400 MPa or more, and particularly preferably 500 MPa or more.

[0024] The flexural strength is measured by a three-point bending test in accordance with the provisions of "JIS Z 2511." Test pieces for the three-point bending test are cut out from the target by a wire cutting method. The measurement conditions are as follows: Test piece size: 2 mm x 2 mm x 20 mm Distance between supports: 10 mm. The flexural strength BS (MPa) is calculated using the following formula: BS = 3 / 2 x P x L / (t 2 × W) (where P is the load at break (kN), L is the distance between supports (mm), t is the thickness of the test piece (mm), and W is the width of the sample (mm)).

[0025] This sputtering target can be obtained by a powder metallurgy method. This method includes the steps of: (1) preparing a first powder composed of CrB; (2) preparing a second powder composed of Cr; (3) mixing the first powder and the second powder to obtain a mixed powder; and (4) pressurizing and heating the mixed powder. By pressing and heating, a sputtering target that is a sintered body is obtained. This target is then processed to a predetermined size and used for sputtering.

[0026] As described above, the Cr-based alloy of the target contains B. This B originates from the first powder. The first powder is composed of CrB. In other words, the first powder contains 50 at % Cr and 50 at % B. This target does not contain any component derived from a powder composed of only B. In this target, B can be uniformly dispersed. A homogeneous thin film can be formed from this target.

[0027] Since B originates from the first powder, uniform dispersion of B can be achieved even in the second powder having a relatively large particle size. Since the second powder having a large particle size is mixed with the first powder, a target with a low oxygen content can be obtained. Specifically, a target with an oxygen content of 2000 ppm or less can be obtained by this manufacturing method. This target is less likely to crack during sputtering.

[0028] From the viewpoint of a low oxygen content, the average particle diameter D50 of the second powder is preferably 20 μm or more, more preferably 40 μm or more, and particularly preferably 50 μm or more. The average particle diameter D50 is preferably 250 μm or less. The average particle diameter D50 is the particle diameter at which the cumulative volume is 50% in the cumulative volume curve of the powder. The average particle diameter D50 is measured using a laser diffraction / scattering particle size distribution analyzer.

[0029] The CrB of the first powder is a thermally stable compound. CrB is unlikely to become the source of new compounds during sintering. This manufacturing method can produce a target that is substantially free of layers other than the CrB phase and the Cr single phase. 5 B 3 A target having a small amount of compounds such as these can be obtained. By this manufacturing method, a target having a ratio of peak P2 to peak P1 of 10% or more and 80% or less can be obtained. By this manufacturing method, a target having a ratio of peak P3 to peak P1 of 20% or less can be obtained. By this manufacturing method, a target having a flexural strength of 300 MPa or more can be obtained. This target is less likely to crack during sputtering. A homogeneous thin film can be formed from this target.

[0030] From this target, an adhesion layer for a perpendicular magnetic recording medium can be obtained by sputtering, and from this target, other thin films can be obtained by sputtering.

[0031] This specification also relates to a method for manufacturing a thin film. This manufacturing method includes the steps of: (1) preparing a target made of a Cr-based alloy containing 10.0 at% to 30.0 at% B, the target having a metallographic structure including a CrB phase and a single Cr phase, and the ratio of the X-ray diffraction peak associated with the (111) plane of the CrB phase to the X-ray diffraction peak associated with the (110) plane of the Cr phase being 10% to 80%; and (2) sputtering the target. This manufacturing method can produce a high-quality thin film. An example of this thin film is the adhesion layer of a perpendicular magnetic recording medium.

[0032] The effects of the sputtering targets according to the examples will be clarified below, but the scope of the present disclosure should not be construed as being limited based on the descriptions of these examples.

[0033] Example 1 A first powder was prepared. This first powder was composed of CrB. This CrB contained 50 at% B. The average particle diameter D50 of this first powder was 10 μm. Furthermore, a second powder was prepared. This second powder was composed of pure Cr. The average particle diameter D50 of this second powder was 60 μm. The first powder and the second powder were charged into a V-type mixer to obtain a mixed powder. The mixed powder was filled into a carbon steel can having a diameter of 200 mm and a length of 10 mm. After vacuum degassing of this powder, a billet was made by HIP. The HIP conditions were as follows: sintering temperature: 1000°C, pressure: 120 MPa, and holding time: 2 hours. This billet was sliced ​​to obtain the sputtering target of Example 1.

[0034] [Examples 2 to 6 and Comparative Examples 1 and 7] Sputtering targets of Examples 2 to 6 and Comparative Examples 1 and 7 were obtained in the same manner as in Example 1, except that the mixing ratio of the first powder and the second powder was adjusted and the sintering temperature was set as shown in Table 2 below.

[0035] [Comparative Examples 2 to 6] Sputtering targets of Comparative Examples 2 to 6 were obtained in the same manner as in Example 1, except that a predetermined amount of pure B powder was used instead of the first powder, a predetermined amount of powder made of pure Cr and having an average particle diameter D50 of 60 μm was used instead of the second powder, and the sintering temperature was set as shown in Table 2 below.

[0036] Comparative Example 8 A sputtering target of Comparative Example 8 was obtained in the same manner as in Example 1, except that the starting material was pure Cr powder alone.

[0037] [Comparative Examples 9 to 11] Sputtering targets of Comparative Examples 9 to 11 were obtained in the same manner as in Example 1, except that a predetermined amount of pure B powder was used instead of the first powder, and a predetermined amount of fine powder made of pure Cr and having an average particle diameter D50 of 10 μm was used instead of the second powder.

[0038] [Oxygen Content] A test piece was cut out from the target by a wire cutting method. The mass of this test piece was approximately 1 g. The surface of this test piece was polished, and the oxygen content was measured using an oxygen / nitrogen analyzer (manufactured by Horiba, Ltd., trade name "EMGA-920"). The results are shown in Table 2 below.

[0039] [X-ray Diffraction] The target was subjected to X-ray diffraction by the method described above. The ratio (P2 / P1) of the X-ray diffraction peak P2 corresponding to the (111) plane of the CrB phase to the X-ray diffraction peak P1 corresponding to the (110) plane of the Cr phase was calculated. Furthermore, the ratio of the Cr 5 B 3 The ratio (P3 / P1) of the X-ray diffraction peak P3 related to the (213) plane of the phase was calculated. The results are shown in Table 3 below. When peak P2 could not be distinguished from noise and the ratio (P2 / P1) was 1% or less, it was indicated as "<1%." When peak P3 could not be distinguished from noise and the ratio (P3 / P1) was 1% or less, it was indicated as "<1%." In the targets of Examples 1 to 6 and Comparative Examples 1 to 3, 7, and 9 to 11, no peaks other than peak P2 whose ratio to diffraction peak P1 was 1% or more were observed. In the targets of Comparative Examples 4 to 6, no peaks other than peaks P2 and P3 whose ratio to diffraction peak P1 was 1% or more were observed.

[0040] [Measurement of Area Ratio] A test piece was cut from the target by a wire cutting method. The size of this test piece was 10 mm x 20 mm x 5 mm. The distribution of Cr and B in this test piece was observed using an EPMA (electron probe microanalyzer), and the area ratio Ps of the portion where B was not present was calculated. The results are shown in Table 3 below. In the EPMA, counts of 70 or more were counted. The area ratio was calculated by dividing each count by the total count (62,500). The EPMA measurement conditions were as follows: Range: 2 mm x 2 mm Beam size: 8 μm Number of data points: 250 x 250 The results are shown in Table 2 below.

[0041] [Transverse Strength Test] The transverse strength of the target was measured by the method described above, and the results are shown in Table 3 below.

[0042] [Number of particles in thin film] A thin film was formed by sputtering a target (diameter: 95 mm, thickness: 2 mm). The sputtering conditions were as follows: Substrate material: cleaned glass Chamber atmosphere: atmospheric pressure of 1×10 -4 The chamber was evacuated to a pressure of 0.6 Pa or less, and 99.99% pure Ar gas was introduced at 0.6 Pa. The film thickness was 20 nm. The film was observed with an optical surface analyzer, and the number of particles with a size of 0.1 μm or more was counted. The results are shown in Table 2 below.

[0043] [Crystalline Grain Size] The thin film was observed with a TEM to measure the average crystal grain size. The ratio of this average crystal grain size to the crystal grain size of Cr in Comparative Example 1 was calculated. The results are shown in Table 2 below.

[0044]

[0045] In addition to the components listed in Table 1, each sputtering target contains unavoidable impurities.

[0046]

[0047] As is clear from Table 2, the sputtering targets of each example have excellent bending strength. Furthermore, the thin films obtained from these targets have few particles and small crystal grain sizes. These evaluation results clearly demonstrate the superiority of these sputtering targets.

[0048] Thin films for various applications can be produced from the sputtering targets described above.

Claims

1. A sputtering target made of a Cr-based alloy containing 10.0 at% or more and 30.0 at% or less of B, wherein the metal structure of the sputtering target includes a CrB phase and a single Cr phase, and the ratio of the X-ray diffraction peak relating to the (111) plane of the CrB phase to the X-ray diffraction peak relating to the (110) plane of the single Cr phase is 10% or more and 80% or less.

2. Cr with respect to the X-ray diffraction peak for the (110) plane of the Cr single phase 5 B 3 2. The sputtering target according to claim 1, wherein the ratio of the X-ray diffraction peak relating to the (213) plane of the phase is 20% or less.

3. The sputtering target according to claim 1 or 2, which has a bending strength of 300 MPa or more in a three-point bending test.

4. The sputtering target according to claim 1 or 2, wherein the Cr-based alloy has an oxygen content of 2000 ppm or less.

5. A method for manufacturing a sputtering target, comprising: (1) a step of preparing a first powder composed of CrB; (2) a step of preparing a second powder composed of Cr; (3) a step of mixing the first powder and the second powder to obtain a mixed powder; and (4) a step of pressurizing and heating the mixed powder.

6. The manufacturing method according to claim 5, wherein in step (2), the second powder has an average particle diameter D50 of 20 μm or more.