Preparation method of super absorbent polymer

MYPI2025003336A0Undetermined Publication Date: 2024-06-15LG CHEM LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025003336
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-12-15
Filing Date
2023-09-04
Publication Date
2024-06-15

AI Technical Summary

Technical Problem

The production of superabsorbent polymers generates a large amount of fine powder during the drying and grinding process, which deteriorates the physical properties of the final product and increases energy usage and equipment load, particularly in pulpless diapers where a higher proportion of superabsorbent resin is required for efficient liquid absorption.

Method used

A method involving cross-polymerizing water-soluble ethylenically unsaturated monomers with an internal cross-linking agent, followed by drying, primary pulverization, surface hydrolysis, and secondary pulverization to reduce fine powder generation, with specific particle size ranges and conditions to maintain excellent physical properties.

Benefits of technology

Significantly reduces fine powder generation and enhances the physical properties of superabsorbent polymers, improving absorption performance and productivity by controlling particle size and moisture content during the manufacturing process.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present disclosure relates to a preparation method of a super absorbent polymer. More specifically, it relates to a preparation method of a super absorbent polymer, and a super absorbent polymer exhibiting excellent physical properties by performing pulverization and hydration processes under specific conditions to significantly reduce the amount of fine powder generated.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing superabsorbent resin

[0001] Cross-citation with related application(s)

[0002] This application claims the benefit of priority to Korean Patent Application No. 10-2022-0175627, filed December 15, 2022, the entire contents of which are incorporated herein by reference.

[0003] The present invention relates to a method for manufacturing a superabsorbent resin. More specifically, the present invention relates to a method for manufacturing a superabsorbent resin and a superabsorbent resin that exhibits superior physical properties by performing a grinding and hydrolysis process under specific conditions, thereby significantly reducing the amount of fine particles generated.

[0004]

[0005] Super absorbent polymer (SAP) is a synthetic polymer material that can absorb 500 to 1,000 times its own weight in water. Different developers call it by different names, such as SAM (Super Absorbency Material) and AGM (Absorbent Gel Material). The above super absorbent polymer began to be put to practical use as a sanitary product, and is currently widely used as a soil conditioner for horticulture, a water-stopping material for civil engineering and construction, a sheet for nursery cultivation, a freshness-preserving agent in the food distribution industry, and a material for steaming.

[0006] These superabsorbent polymers are widely used in sanitary products, such as diapers and sanitary napkins. Within these sanitary products, the superabsorbent polymers are typically dispersed within pulp. However, recent efforts to provide thinner sanitary products, such as diapers, are ongoing. As part of this effort, the development of so-called pulpless diapers, which contain reduced pulp content or even eliminate pulp altogether, is actively underway.

[0007] Thus, in sanitary materials with reduced pulp content or no pulp, a relatively high proportion of superabsorbent resin is included, and superabsorbent resin particles are inevitably embedded in multiple layers within the sanitary material. In order for the superabsorbent resin particles embedded in multiple layers to efficiently absorb large amounts of liquids such as urine, the superabsorbent resin must fundamentally exhibit not only high absorption performance but also a rapid absorption rate.

[0008] Meanwhile, these superabsorbent resins are generally manufactured through a step of polymerizing monomers to produce a hydrogel polymer containing a large amount of moisture, followed by a step of drying the hydrogel polymer and then grinding it into resin particles having a desired particle size. However, when the hydrogel polymer is dried and then ground, as described above, a large amount of fine particles are generated, which has the problem of deteriorating the physical properties of the final superabsorbent resin.

[0009] Furthermore, to reuse these fine particles, it is common to mix the fine particles with water, coagulate them, and then manufacture a fine particle re-assembly. The resulting fine particle re-assembly is then introduced through processes such as drying, grinding, and classification. However, the water used in this process increases energy consumption during the drying process, increasing the load on the equipment, and other problems, which can reduce the productivity of superabsorbent polymer production.

[0010] Accordingly, there is a continuous demand for the development of technology that can manufacture superabsorbent polymers without generating fine particles to fundamentally solve these problems.

[0011]

[0012] Accordingly, the present invention aims to provide a method for manufacturing a superabsorbent resin and a superabsorbent resin capable of significantly reducing the amount of fine particles generated by performing a grinding and hydrolysis process under specific conditions and thereby exhibiting excellent physical properties.

[0013]

[0014] In order to solve the above problem, according to one embodiment of the present invention,

[0015] A step (step 1) of forming a hydrogel polymer comprising a crosslinked polymer obtained by crosslinking a water-soluble ethylenically unsaturated monomer having an acidic group in the presence of an internal crosslinking agent;

[0016] A step of drying the above functional gel polymer to obtain a base resin (step 2);

[0017] A step of first crushing the above dried base resin and classifying it into particles larger than or equal to a standard particle size and particles smaller than or equal to a standard particle size (step 3);

[0018] A step (step 4) of obtaining a hydrophilic superabsorbent resin using a surface hydrophilic solution containing water for a base resin having a particle size greater than the above-mentioned standard particle size; and

[0019] It includes a step (step 5) of obtaining a superabsorbent resin by secondarily crushing the above-mentioned superabsorbent resin,

[0020] The above standard particle size is determined within the particle size range of 300 ㎛ or more and 850 ㎛ or less.

[0021] A method for producing a superabsorbent resin is provided.

[0022]

[0023] According to the method for producing a superabsorbent resin of the present invention, by performing the grinding and hydrolysis processes under specific conditions, the amount of fine powder generated is significantly reduced, making it possible to produce a superabsorbent resin exhibiting excellent physical properties.

[0024]

[0025] The terminology used herein is for the purpose of describing exemplary embodiments only and is not intended to limit the present invention. The singular expression includes the plural expression unless the context clearly indicates otherwise. In this specification, it should be understood that the terms "comprise," "include," or "have" indicate the presence of a feature, step, component, or combination thereof, but do not preclude the possibility of the presence or addition of one or more other features, steps, components, or combinations thereof.

[0026] The present invention is susceptible to various modifications and takes various forms. Specific embodiments are illustrated and described in detail below. However, this is not intended to limit the present invention to specific disclosed forms, but rather to encompass all modifications, equivalents, and alternatives falling within the spirit and technical scope of the present invention.

[0027] The present invention is susceptible to various modifications and takes various forms. Specific embodiments are illustrated and described in detail below. However, this is not intended to limit the present invention to specific disclosed forms, but rather to encompass all modifications, equivalents, and alternatives falling within the spirit and technical scope of the present invention.

[0028] Hereinafter, a method for manufacturing a superabsorbent resin and a superabsorbent resin will be described in more detail according to specific embodiments of the invention.

[0029] Before proceeding, it should be noted that the technical terminology used herein is solely for the purpose of describing specific embodiments and is not intended to limit the present invention. Furthermore, the singular forms used herein also include the plural forms, unless the context clearly dictates otherwise.

[0030] The term "polymer" or "high molecular weight polymer" as used in the specification of the present invention means a polymerized state of a water-soluble ethylenically unsaturated monomer, and may encompass any moisture content range or particle size range.

[0031] In addition, the term "superabsorbent resin" is used to mean, depending on the context, a base resin in powder form made of a crosslinked polymer or superabsorbent resin particles obtained by pulverizing the crosslinked polymer, or to encompass all of the crosslinked polymer or the base resin that have been subjected to additional processes, such as drying, pulverization, classification, surface crosslinking, etc., to make them suitable for commercialization.

[0032] Additionally, the term "fine particles" refers to particles having a particle size of less than 150 μm among superabsorbent resin particles. The particle size of such resin particles can be measured according to the European Disposables and Nonwovens Association (EDANA) standard EDANA WSP 220.3 method.

[0033] Additionally, the term "chopping" is used to refer to cutting the hydrogel polymer into small pieces on the order of millimeters to increase drying efficiency, as distinguished from grinding to the micrometer or normal particle level.

[0034] Additionally, the term “micronizing” refers to grinding a hydrogel polymer into particle sizes of tens to hundreds of micrometers, and is used to distinguish it from “chopping.”

[0035]

[0036] According to one embodiment of the invention,

[0037] A step (step 1) of forming a hydrogel polymer comprising a crosslinked polymer obtained by crosslinking a water-soluble ethylenically unsaturated monomer having an acidic group in the presence of an internal crosslinking agent;

[0038] A step of drying the above functional gel polymer to obtain a base resin (step 2);

[0039] A step of first crushing the above dried base resin and classifying it into particles larger than or equal to a standard particle size and particles smaller than or equal to a standard particle size (step 3);

[0040] A step (step 4) of obtaining a hydrophilic superabsorbent resin using a surface hydrophilic solution containing water for a base resin having a particle size greater than the above-mentioned standard particle size; and

[0041] It includes a step (step 5) of obtaining a superabsorbent resin by secondarily crushing the above-mentioned superabsorbent resin,

[0042] The above standard particle size is determined within the particle size range of 300 ㎛ or more and 850 ㎛ or less.

[0043] A method for producing a superabsorbent resin is provided.

[0044]

[0045] Typically, superabsorbent polymers are manufactured through a process of polymerizing monomers to produce a hydrogel polymer containing a large amount of moisture, followed by drying and pulverizing the hydrogel polymer into resin particles having a desired particle size. However, the process of pulverizing the hydrogel polymer after drying it as described above has the problem of generating a large amount of fine particles, which deteriorates the properties of the final superabsorbent polymer.

[0046] Accordingly, in order to reuse the generated fine powder, a method was applied in which the fine powder was introduced into a hydrogel grinding step, or the fine powder was mixed with water to coagulate and manufacture a fine powder re-assembly, and then the fine powder re-assembly manufactured through processes such as drying / grinding / classification was introduced. However, due to the water used in the re-assembly manufacturing process, problems such as increased energy consumption during the drying process and increased load on the equipment occurred, resulting in a decrease in the productivity of the production of superabsorbent resins.

[0047] Accordingly, the inventor of the present invention confirmed that the amount of fine powder generated can be significantly reduced by performing the crushing and hydrolysis process under specific conditions, and completed the present invention.

[0048] Specifically, it was confirmed that the degree of fine particle generation can be significantly reduced by first crushing the dried functional gel polymer to have a relatively large particle size, and then performing surface hydrolysis on particles larger than a standard particle size among the crushed particles and then second crushing them.

[0049] Hereinafter, the method for manufacturing a superabsorbent resin will be described in more detail step by step according to specific implementation examples of the invention.

[0050]

[0051] (Polymerization stage)

[0052] First, a method for manufacturing a superabsorbent resin according to one embodiment of the invention includes a step (step 1) of forming a hydrogel polymer by crosslinking and polymerizing a water-soluble ethylenically unsaturated monomer having at least a portion of a neutralized acidic group in the presence of an internal crosslinking agent.

[0053] Specifically, it is a step of forming a hydrogel polymer by thermally polymerizing or photopolymerizing a monomer composition including a monomer mixture and a polymerization initiator in the presence of an internal crosslinking agent. The monomer composition may include, in addition to the aforementioned components, components generally used in the production of superabsorbent resins.

[0054] The water-soluble ethylenically unsaturated monomer may be any monomer commonly used in the production of superabsorbent resins. As a non-limiting example, the water-soluble ethylenically unsaturated monomer may be a compound represented by the following chemical formula 1:

[0055] [Chemical Formula 1]

[0056] R1-COOM 1

[0057] In the above chemical formula 1,

[0058] R1 is an alkyl group having 2 to 5 carbon atoms containing an unsaturated bond,

[0059] M 1 is a hydrogen atom, a monovalent or divalent metal, an ammonium group, or an organic amine salt.

[0060] Preferably, the monomer may be at least one selected from the group consisting of acrylic acid, methacrylic acid, and monovalent metal salts, divalent metal salts, ammonium salts, and organic amine salts of these acids. In this way, when acrylic acid or a salt thereof is used as a water-soluble ethylenically unsaturated monomer, a superabsorbent resin with improved absorbency can be obtained, which is advantageous. In addition, examples of the monomer include anionic monomers of maleic anhydride, fumaric acid, crotonic acid, itaconic acid, 2-acryloylethane sulfonic acid, 2-methacryloylethane sulfonic acid, 2-(meth)acryloylpropanesulfonic acid, or 2-(meth)acrylamide-2-methyl propane sulfonic acid and salts thereof; Nonionic hydrophilic monomers containing (meth)acrylamide, N-substituted (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, methoxypolyethylene glycol (meth)acrylate or polyethylene glycol (meth)acrylate; and amino group-containing unsaturated monomers containing (N,N)-dimethylaminoethyl (meth)acrylate or (N,N)-dimethylaminopropyl (meth)acrylamide and quaternary compounds thereof may be used.

[0061] The term "internal cross-linking agent" used in this specification is a term used to distinguish it from a "surface cross-linking agent" that cross-links the surface of the base resin, and plays a role in polymerizing by cross-linking the unsaturated bonds of the above-described water-soluble ethylenically unsaturated monomers. The cross-linking in the above step proceeds without distinction between the surface and the interior, but through the surface cross-linking process of the base resin described below, the particle surface of the finally manufactured superabsorbent resin is formed into a structure cross-linked by the surface cross-linking agent, and the interior is formed into a structure cross-linked by the internal cross-linking agent.

[0062] Non-limiting examples of the internal cross-linking agent include N,N'-methylenebisacrylamide, trimethylolpropane tri(meth)acrylate, ethylene glycol di(meth)acrylate, polyethylene glycol(meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol(meth)acrylate, butanediol di(meth)acrylate, butylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, hexanediol di(meth)acrylate, triethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, dipentaerythritol pentaacrylate, glycerin tri(meth)acrylate, pentaerythritol tetraacrylate, triarylamine, ethylene glycol diglycidyl ether, propylene glycol, Polyfunctional cross-linking agents such as glycerin or ethylene carbonate may be used alone or in combination of two or more, but are not limited thereto. Preferably, among these, ethylene glycol diglycidyl ether may be used.

[0063] The internal cross-linking agent may be used in an amount of 0.01 to 5 parts by weight based on 100 parts by weight of the water-soluble ethylenically unsaturated monomer. For example, the internal cross-linking agent may be used in an amount of 0.01 parts by weight or more, 0.05 parts by weight or more, 0.1 parts by weight or more, or 0.45 parts by weight or more, and 5 parts by weight or less, 3 parts by weight or less, 2 parts by weight or less, 1 part by weight or less, or 0.7 parts by weight or less, based on 100 parts by weight of the water-soluble ethylenically unsaturated monomer. If the content of the upper internal cross-linking agent is too low, cross-linking may not occur sufficiently, making it difficult to achieve a strength higher than an appropriate level, and if the content of the upper internal cross-linking agent is too high, the internal cross-linking density may increase, making it difficult to achieve a desired water retention capacity.

[0064] In the above crosslinking polymerization step, a polymerization initiator commonly used in the production of superabsorbent resins may be included. Non-limiting examples of the polymerization initiator include thermal polymerization initiators or photopolymerization initiators, depending on the polymerization method. In particular, a thermal polymerization initiator may be used. However, even with a photopolymerization method, a certain amount of heat is generated by ultraviolet irradiation, etc., and a certain amount of heat is also generated as the polymerization reaction, which is an exothermic reaction, progresses. Therefore, a thermal polymerization initiator may be additionally included.

[0065] As the above thermal polymerization initiator, one or more compounds selected from the group consisting of a persulfate-based initiator, an azo-based initiator, hydrogen peroxide, and ascorbic acid may be used. Specifically, examples of the persulfate-based initiator include sodium persulfate (Na2S2O8), potassium persulfate (K2S2O8), and ammonium persulfate ((NH4)2S2O8). In addition, as azo initiators, 2,2-azobis-(2-amidinopropane) dihydrochloride, 2,2-azobis-(N,N-dimethylene)isobutyramidine dihydrochloride, 2-(carbamoylazo)isobutylonitril, 2,2-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, 4,4-azobis-(4-cyanovaleric acid) Examples include 4,4-azobis-(4-cyanovaleric acid)). For a more diverse range of thermal polymerization initiators, see page 203 of Odian's book, "Principle of Polymerization (Wiley, 1981)".

[0066] As the photopolymerization initiator, for example, one or more compounds selected from the group consisting of benzoin ether, dialkyl acetophenone, hydroxyl alkylketone, phenyl glyoxylate, benzyl dimethyl ketal, acyl phosphine, and α-aminoketone may be used. Among them, specific examples of the acyl phosphine include diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, phenylbis (2,4,6-trimethylbenzoyl) phosphine oxide, and ethyl (2,4,6-trimethylbenzoyl) phenylphosphinate. A more detailed description of various photoinitiators is given in Reinhold Schwalm's book "UV Coatings: Basics, Recent Developments and New Applications (Elsevier 2007)" p115, and is not limited to the examples described above.

[0067] Such polymerization initiator may be added at a concentration of about 0.001 to 1 wt% with respect to the monomer composition including the water-soluble ethylenically unsaturated monomer. That is, if the concentration of the polymerization initiator is too low, the polymerization rate may be slowed and a large amount of residual monomer may be extracted from the final product, which is not preferable. Conversely, if the concentration of the polymerization initiator is higher than the above range, the polymer chains forming the network may become shorter, which may increase the content of water-soluble components and lower the pressure absorbency, thereby deteriorating the physical properties of the resin, which is not preferable.

[0068] In addition, the monomer composition may further include additives such as a foaming agent, a surfactant, a thickener, a plasticizer, a preservation stabilizer, and an antioxidant, as needed.

[0069] And, such monomer composition can be prepared in the form of a solution in which raw materials such as the aforementioned monomer, polymerization initiator, and internal crosslinking agent are dissolved in a solvent.

[0070] The concentration of the water-soluble ethylenically unsaturated monomer in the monomer composition including the internal crosslinking agent and the water-soluble ethylenically unsaturated monomer having an acidic group can be appropriately controlled in consideration of the polymerization time and reaction conditions, and can be about 20 to about 60 wt%, or about 20 to about 40 wt%.

[0071] At this time, any solvent that can dissolve the above-mentioned raw materials can be used without limitation in its composition. For example, the solvent may include water, ethanol, ethylene glycol, diethylene glycol, triethylene glycol, 1,4-butanediol, propylene glycol, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, methyl ethyl ketone, acetone, methyl amyl ketone, cyclohexanone, cyclopentanone, diethylene glycol monomethyl ether, diethylene glycol ethyl ether, toluene, xylene, butyrolactone, carbitol, methyl cellosolve acetate, N,N-dimethylacetamide, or mixtures thereof.

[0072] In addition, the formation of a hydrogel polymer through polymerization of the monomer composition can be performed using a conventional polymerization method, and the process is not particularly limited. As a non-limiting example, the polymerization method is largely divided into thermal polymerization and photopolymerization depending on the type of polymerization energy source. In the case of thermal polymerization, it can be performed in a reactor having a stirring shaft such as a kneader, and in the case of photopolymerization, it can be performed in a reactor equipped with a movable conveyor belt.

[0073] For example, the monomer composition may be introduced into a reactor, such as a kneader, equipped with a stirring shaft, and thermal polymerization may be performed by supplying hot air thereto or heating the reactor, thereby obtaining a hydrogel polymer. At this time, depending on the shape of the stirring shaft equipped in the reactor, the hydrogel polymer discharged through the reactor outlet may be obtained as particles of several millimeters to several centimeters. Specifically, the obtained hydrogel polymer may be obtained in various forms depending on the concentration and injection speed of the injected monomer composition, and typically, a hydrogel polymer having a (weight average) particle diameter of 2 to 50 mm may be obtained.

[0074] In addition, as another example, when photopolymerization of the monomer composition is performed in a reactor equipped with a movable conveyor belt, a functional gel polymer in the form of a sheet can be obtained. At this time, the thickness of the sheet can vary depending on the concentration and injection speed of the injected monomer composition, but in order to ensure that the entire sheet can be polymerized evenly while also securing production speed, etc., it is generally preferable to adjust the thickness to 0.5 to 5 cm.

[0075] According to one embodiment of the invention, the crosslinking polymerization step may be performed at a temperature of 10°C to 140°C, and preferably, at a temperature of 70°C to 130°C or 70°C to 120°C. When performed within the above temperature range, it is suitable for realizing an appropriate crosslinking density realized by the chelating agent of the present disclosure.

[0076] The typical moisture content of the hydrogel polymer obtained by the above method may be 30 to 80 wt%. Meanwhile, the "moisture content" refers to the moisture content relative to the total weight of the hydrogel polymer, which is the value obtained by subtracting the weight of the dry polymer from the weight of the hydrogel polymer. Specifically, it is defined as a value calculated by measuring the weight loss due to evaporation of moisture in the polymer during the drying process by increasing the temperature of the polymer through infrared heating. At this time, the drying condition is maintained at about 180°C for about 40 minutes at room temperature to measure the moisture content.

[0077]

[0078] According to one embodiment of the invention, a step of neutralizing at least a portion of the acidic groups of a water-soluble ethylenically unsaturated monomer having acidic groups may be included prior to the polymerization step.

[0079] Specifically, the step of forming the functional gel polymer (step 1) may be performed including a step of neutralizing at least a portion of the acidic groups of a water-soluble ethylenically unsaturated monomer having an acidic group (step 1-1') and a step of crosslinking and polymerizing the water-soluble ethylenically unsaturated monomer having at least a portion of the neutralized acidic groups in the presence of an internal crosslinking agent to form the functional gel polymer (step 1-2').

[0080] The neutralization step of the acid group is carried out by mixing with a neutralizing agent capable of neutralizing the acid group. Examples of the neutralizing agent include, but are not limited to, basic substances such as sodium hydroxide, potassium hydroxide, and ammonium hydroxide.

[0081] At this time, the degree of neutralization of the acid group may be 40 to 95 mol%, or 40 to 90 mol%, or 45 to 80 mol%. The range of the degree of neutralization may vary depending on the final physical properties, but if the degree of neutralization is too high, the surface crosslinking reaction may not sufficiently occur, which may cause a problem of a decrease in absorbency under pressure (AUP), and conversely, if the degree of neutralization is too low, not only will the absorbency of the polymer significantly decrease, but it may also exhibit properties like elastic rubber that are difficult to handle.

[0082] According to one embodiment of the invention, a method may include forming a polymer using a water-soluble ethylenically unsaturated monomer having an unneutralized acidic group, followed by a step of neutralizing the polymer. In this case, the polymerized polymer has an acidic group, and thus, a neutralization step may be included after the polymerization step. The neutralizing agent used in the neutralization step and the degree of neutralization of the acidic group after neutralization may be applied in the same manner as described above.

[0083] Specifically, the step of forming the functional gel polymer (step 1) may be performed including a step of crosslinking and polymerizing a water-soluble ethylenically unsaturated monomer having an acidic group in the presence of an internal crosslinking agent to form a polymer (step 1-1); a step of micronizing the neutralizing agent (step 1-2); and a step of neutralizing at least a portion of the acidic groups of the polymer to form the functional gel polymer (step 1-3). Meanwhile, in the neutralization step (1-3), a coagulation process of the polymer is performed simultaneously.

[0084] Water-soluble ethylenically unsaturated monomers, in which the acid groups are not neutralized, are liquid at room temperature and have high miscibility with the solvent (water), so they exist as a mixed solution in the monomer composition. However, water-soluble ethylenically unsaturated monomers, in which the acid groups are neutralized, are solid at room temperature and have different solubility depending on the temperature of the solvent (water), with the solubility decreasing at lower temperatures.

[0085] In this way, a water-soluble ethylenically unsaturated monomer in which the acidic groups are not neutralized has higher solubility or miscibility in a solvent (water) than a monomer in which the acidic groups are neutralized, and thus does not precipitate even at low temperatures, and is therefore advantageous for long-term polymerization at low temperatures. Accordingly, a water-soluble ethylenically unsaturated monomer in which the acidic groups are not neutralized can be used for long-term polymerization to stably form a polymer having a higher molecular weight and a uniform molecular weight distribution.

[0086] In addition, it is possible to form polymers of longer chains, and thus achieve the effect of reducing the content of water-soluble components that exist in an uncrosslinked state due to incomplete polymerization or crosslinking.

[0087] Meanwhile, when polymerization is first performed to form a polymer in a state where the acidic groups of the monomer are not neutralized, it was confirmed that when the polymer is formed in the presence of a surfactant after neutralization, or when the acidic groups present in the polymer are neutralized after or simultaneously with the formation of the polymer, the surfactant is present in large quantities on the surface of the polymer, thereby lowering the adhesiveness of the polymer and allowing the polymer to exhibit an appropriate degree of coagulation.

[0088] According to one embodiment of the invention, when the step of forming the functional gel polymer (step 1) is performed as a neutralization step (step 1-3) after polymerization (step 1-1), the neutralization step may be performed sequentially, simultaneously, or alternately with the polymer atomization step (1-2). More preferably, the polymerization step (step 1-1), the polymer atomization step (1-2), and the neutralization step (1-3) may be performed sequentially. Here, in the neutralization step, polymer agglomeration is performed simultaneously.

[0089] That is, after a mixture of a polymer and a surfactant (optional) is micronized, a neutralizing agent is added to neutralize the mixture, or a neutralizing agent is sprayed onto the polymer to neutralize the acidic groups of the polymer first, and then a surfactant (optional) is added to the neutralized polymer to micronize the mixture containing the surfactant, or a neutralizing agent and a surfactant (optional) are added to the polymer at the same time to neutralize and micronize the polymer.

[0090] In this way, when the polymer is micronized in the presence of the surfactant, the hydrophobic functional group contained in the surfactant imparts hydrophobicity to the surface of the pulverized superabsorbent resin particles, thereby alleviating the friction between particles, thereby minimizing the deterioration of physical properties due to the friction between particles while micronizing the superabsorbent resin.

[0091] Meanwhile, it may be desirable to leave a certain time gap between the introduction of the neutralizing agent and the atomization process to ensure even neutralization of the entire polymer.

[0092] The surfactant used in the above atomization process may be a compound represented by the following chemical formula 2 or a salt thereof, but the present invention is not limited thereto:

[0093] [Chemical Formula 2]

[0094]

[0095] In the above chemical formula 2,

[0096] A1, A2 and A3 are each independently a single bond, carbonyl, , or and, provided that at least one of these is carbonyl or , wherein, m1, m2 and m3 are each independently an integer from 1 to 8, are each connected to an adjacent oxygen atom, are connected to adjacent R1, R2 and R3 respectively,

[0097] R1, R2 and R3 are each independently hydrogen, straight or branched chain alkyl having 6 to 18 carbon atoms or straight or branched chain alkenyl having 6 to 18 carbon atoms,

[0098] n is an integer from 1 to 9.

[0099] The above surfactant is added to the polymer so that the ultra-fine grinding step can be easily performed without agglomeration.

[0100] The surfactant represented by the above chemical formula 2 is a nonionic surfactant, and has excellent surface adsorption performance by hydrogen bonding even with a polymer that is not neutralized, and is therefore suitable for implementing the desired coagulation control effect. On the other hand, in the case of anionic surfactants, not nonionic surfactants, when mixed with a polymer that has been neutralized with a neutralizing agent such as NaOH or Na2SO4, the Na ionized in the carboxyl group substituent of the polymer + It is adsorbed through ions, and when mixed with an unsaturated polymer, there is a problem that the adsorption efficiency for the polymer is relatively reduced due to competition with the anion of the carboxyl group substituent of the polymer.

[0101] Specifically, in the surfactant represented by the above chemical formula 2, the hydrophobic functional group is the terminal functional group R1, R2, R3 portion (if not hydrogen), and the hydrophilic functional group is the glycerol-derived portion in the chain and the terminal hydroxyl group (A n is a single bond, and at the same time R n When the polymer is hydrogen, n=1~3) is further included, and the glycerol-derived portion and the terminal hydroxyl group serve as hydrophilic functional groups to improve the adsorption performance on the polymer surface. Accordingly, the aggregation of superabsorbent resin particles can be effectively suppressed.

[0102] In the above chemical formula 2, the hydrophobic functional groups R1, R2, and R3 (if not hydrogen) are each independently a straight-chain or branched alkyl having 6 to 18 carbon atoms or a straight-chain or branched alkenyl having 6 to 18 carbon atoms. In this case, if the R1, R2, and R3 portions (if not hydrogen) are alkyl or alkenyl having less than 6 carbon atoms, there is a problem that the agglomeration control of the pulverized particles is not effectively performed due to the short chain length, and if the R1, R2, and R3 portions (if not hydrogen) are alkyl or alkenyl having more than 18 carbon atoms, the mobility of the surfactant may be reduced so that it may not be effectively mixed with the polymer, and there may be a problem that the unit price of the composition increases due to the increase in the cost of the surfactant.

[0103] Preferably, R1, R2, R3 may be hydrogen, or, if it is a straight-chain or branched alkyl having 6 to 18 carbon atoms, 2-methylhexyl, n-heptyl, 2-methylheptyl, n-octyl, n-nonyl, n-decanyl, n-undecanyl, n-dodecanyl, n-tridecanyl, n-tetradecanyl, n-pentadecanyl, n-hexadecanyl, n-heptadecanyl, or n-octadecanyl, or, if it is a straight-chain or branched alkenyl having 6 to 18 carbon atoms, 2-hexenyl, 2-heptenyl, 2-octenyl, 2-nonenyl, n-dekenyl, 2-undekenyl, 2-dodekenyl, 2-tridekenyl, 2-tetradekenyl, 2-pentadekenyl, 2-hexadekenyl, It can be 2-heptadekenyl or 2-octadekenyl.

[0104] The above surfactant may be selected from compounds represented by the following chemical formulas 2-1 to 2-14:

[0105] [Chemical Formula 2-1]

[0106]

[0107] [Chemical Formula 2-2]

[0108]

[0109] [Chemical Formula 2-3]

[0110]

[0111] [Chemical Formula 2-4]

[0112]

[0113] [Chemical Formula 2-5]

[0114]

[0115] [Chemical Formula 2-6]

[0116]

[0117] [Chemical Formula 2-7]

[0118]

[0119] [Chemical Formula 2-8]

[0120]

[0121] [Chemical Formula 2-9]

[0122]

[0123] [Chemical Formula 2-10]

[0124]

[0125] [Chemical Formula 2-11]

[0126]

[0127] [Chemical Formula 2-12]

[0128]

[0129] [Chemical Formula 2-13]

[0130]

[0131] [Chemical Formula 2-14]

[0132] .

[0133] Meanwhile, the surfactant may be used in an amount of 0.1 part by weight or less relative to 100 parts by weight of the polymer, depending on productivity or device load conditions. If the surfactant is used in excessive amounts, the surface tension value may decrease, which may deteriorate the overall physical properties of the finally manufactured superabsorbent resin. For example, the surfactant may be used in an amount of 0.1 part by weight or less relative to 100 parts by weight of the polymer, preferably 0.05 part by weight or less, 0.005 part by weight or less, or 0.001 part by weight or less.

[0134] The method for mixing these surfactants into the polymer is not particularly limited, and any method capable of evenly mixing them into the polymer may be appropriately employed. Specifically, the surfactants may be mixed dry, dissolved in a solvent and then mixed in a solution state, or melted and then mixed.

[0135] For example, the surfactant may be mixed in a solution state dissolved in a solvent. Any type of solvent, whether inorganic or organic, may be used, but water is most suitable considering the ease of drying and the cost of the solvent recovery system. Furthermore, the solution may be prepared by mixing the surfactant and polymer in a reactor, placing the polymer in a mixer and spraying the solution, or continuously supplying the polymer and solution to a continuously operating mixer for mixing.

[0136]

[0137] (Drying stage)

[0138] Next, a method for manufacturing a superabsorbent resin according to one embodiment of the invention includes a step (step 2) of drying a functional gel polymer formed through the polymerization step to obtain a base resin.

[0139] According to one embodiment of the invention, when the step of forming the above-described functional gel polymer (step 1) is performed including the step of neutralizing at least a portion of the acidic groups of a water-soluble ethylenically unsaturated monomer having an acidic group (step 1-1') and the step of crosslinking and polymerizing the water-soluble ethylenically unsaturated monomer having at least a portion of the neutralized acidic groups in the presence of an internal crosslinking agent to form the functional gel polymer (step 1-2') (pre-neutralization polymerization process), the step 2 may be performed as a process of drying the functional gel polymer that has undergone the step.

[0140] If necessary, a step of grinding the functional gel polymer before drying may be further performed to increase the efficiency of the drying step.

[0141] The crusher used is not limited in configuration, but specifically, may include any one selected from a group of crushing devices consisting of a vertical pulverizer, a turbo cutter, a turbo grinder, a rotary cutter mill, a cutter mill, a disc mill, a shred crusher, a crusher, a chopper, and a disc cutter, but is not limited to the examples described above.

[0142] At this time, the grinding step can be performed so that the particle size of the hydrogel polymer is 2 to 10 mm. Grinding to a particle size of less than 2 mm is technically difficult due to the high moisture content of the hydrogel polymer, and agglomeration may also occur between the ground particles. On the other hand, if the particle size is greater than 10 mm, the efficiency increase effect of the subsequent drying step may be minimal.

[0143] Meanwhile, when the step of forming the aforementioned functional gel polymer (step 1) is performed including the step of forming a polymer by crosslinking and polymerizing a water-soluble ethylenically unsaturated monomer having an acidic group in the presence of an internal crosslinking agent (step 1-1); and the step of forming a functional gel polymer by neutralizing at least a portion of the acidic groups of the polymer (step 1-2) (post-neutralization polymerization process), agglomeration of particles can be suppressed without an additional grinding process before drying, thereby realizing excellent drying efficiency.

[0144] Drying is performed on the hydrogel polymer immediately after polymerization, which has been pulverized as described above or has not gone through the pulverization step. At this time, the drying temperature of the drying step may be 150°C to 250°C. If the drying temperature is less than 150°C, the drying time may be excessively long and there is a concern that the properties of the superabsorbent resin ultimately formed may deteriorate. If the drying temperature exceeds 250°C, only the surface of the polymer may be excessively dried, which may cause fine powder to be generated in the subsequent pulverization step and there is a concern that the properties of the superabsorbent resin ultimately formed may deteriorate. Therefore, the drying may preferably be performed at a temperature of 150°C to 200°C, and more preferably at a temperature of 170°C to 195°C. The drying may be performed in multiple stages by varying the temperature within the above temperature range.

[0145] Meanwhile, in terms of drying time, it may be carried out for 20 to 90 minutes, taking into account process efficiency, etc., but is not limited thereto.

[0146] The drying method of the above-mentioned drying step can be selected and used without limitation in its composition, as long as it is a method commonly used in the drying process of functional gel polymers. Specifically, the drying step can be performed using methods such as hot air supply, infrared irradiation, ultrashort wave irradiation, or ultraviolet irradiation. The moisture content of the polymer after such a drying step can be about 0.1 wt% to about 10 wt%.

[0147]

[0148] (1st crushing stage)

[0149] Next, the method for manufacturing a superabsorbent resin according to one embodiment of the invention includes a step (step 3) of first crushing the dried base resin and classifying it into particles having a standard particle size or larger and particles having a standard particle size or smaller. The step of crushing the dried polymer is referred to as "first crushing" in this specification to distinguish it from the crushing of step 4 (referred to as "second crushing") described below.

[0150] In the above first crushing process, the functional gel polymer is crushed to have a relatively large particle size, thereby reducing the occurrence of initial fine particles and facilitating the operation of the second crushing process performed to have the final target particle size, thereby reducing the degree of fine particle occurrence in the final product.

[0151] The above “particles having a particle size larger than the standard particle size” refers to particles having a relatively large particle size compared to particles that have undergone a conventional drying and pulverization process, and specifically, the standard particle size is determined within a particle size range of 300 ㎛ to 850 ㎛. When the standard particle size is determined within the above range, the initial amount of fine powder generated can be significantly controlled. Preferably, the standard particle size may be determined within a particle size range of 600 ㎛ to 850 ㎛, and more preferably, the standard particle size may be 710 ㎛.

[0152] Typically, “fine powder” means a particle having a particle size of less than 150 ㎛. As described above, the first crushing process of the present invention crushes particles to have a relatively large particle size, so that the amount of initial fine powder generated among the base resin to be classified is significantly reduced.

[0153] In the above step 3, the first pulverization may be performed so that the particles having a standard particle size or larger are 40 wt% or more based on the total weight of the pulverized particles. When the particles having a standard particle size or larger are included in the above content range, the amount of fine powder generated in the final product can be effectively controlled through the hydrolysis process described below, which is preferable. Preferably, the first pulverization may be performed so that the particles having a standard particle size or larger are 45 wt% or more, 48 wt% or more, 50 wt% or more, 55 wt% or more, or 60 wt% or more based on the total weight of the pulverized particles.

[0154] In addition, in the above step 3, the first crushing may be performed so that the particles of 10 mm or more are less than 5 wt% based on the total weight of the crushed particles. The particles of 10 mm or more are particles that are not crushed normally and may put a load on the device in the second crushing process. Therefore, by crushing the particles of 10 mm or more in the first crushing so that a small amount is included, the operation of the device can be facilitated during the second crushing and excessive crushing can be reduced, thereby reducing the amount of fine powder generated. Preferably, the first crushing may be performed so that the particles of 10 mm or more are less than 4 wt%, less than 3 wt%, less than 2 wt%, less than 1 wt%, and most preferably about 0 wt% based on the total weight of the crushed particles.

[0155] The method for performing the above first crushing process is not particularly limited and can be appropriately adjusted so as to satisfy the above-mentioned particle content range.

[0156] Specifically, the first pulverization process can be performed using a pulverizer having a hole plate of 5 mm to 20 mm, and more preferably, can be performed using a pulverizer having a hole plate of 8 mm to 12 mm. Here, the hole plate is a porous plate having a plurality of holes formed therein, and the particle diameters of the holes satisfy the above-mentioned range. When the first pulverization is performed under the above conditions, the surface hydration and second pulverization processes for particles having a specific particle diameter range described below can be easily performed, and thus, the generation of fine particles can be significantly reduced during the manufacture of the final superabsorbent resin.

[0157] Preferably, the grinder used in the first grinding may be a rotary cutter mill including the hole plate and the rotating screw. When the cutting mill is used, it can have a high grinding throughput and is more suitable for the first grinding process in that it is easier to grind particles having a high moisture content.

[0158]

[0159] (Singer stage)

[0160] Next, a method for manufacturing a superabsorbent resin according to one embodiment of the invention includes a step (step 4) of obtaining a hydrolyzed superabsorbent resin using a surface hydrolysis solution containing water, for a base resin having a particle size greater than a standard particle size that has undergone the first crushing and classification steps. Through the hydrolysis step, the amount of fine particles generated in the second crushing step described below can be significantly reduced.

[0161] Here, water alone can be used as the surface water solution.

[0162] The above surface water solution may be used in an amount of 0.1 to 10 parts by weight, preferably 0.5 to 7 parts by weight, or 1 to 5 parts by weight, based on 100 parts by weight of the base resin, and uniform surface water may be achieved within the above content range, which is preferable.

[0163] In addition, the surface water solution may further include, in addition to water, one or more additives selected from the group consisting of polyacrylic acid-polyethylene oxide comb polymer (GK), aluminum sulfate, polyethylene glycol, sodium dodecyl sulfate, glycerol monolaurate, and sodium stearoyl lactylate, and preferably, polyacrylic acid-polyethylene oxide comb polymer (GK) and aluminum sulfate may be used. The use of the additive improves the dispersibility of the surface water solution, thereby enabling more uniform surface water to be applied to the surface of the base resin particles.

[0164] The above additive can be used in an amount of 0.01 to 10 parts by weight, preferably 0.01 to 5 parts by weight, 0.05 to 3 parts by weight, or 0.1 to 1 part by weight, based on 100 parts by weight of the surface water solution, and is suitable for performing uniform surface water with appropriate dispersibility when used in the above content range.

[0165] The method for adding the surface cross-linking solution to the above-mentioned base resin is not particularly limited, but for example, a method of putting the base resin and the surface cross-linking solution into a reaction tank and mixing them, and spraying the surface cross-linking solution onto the base resin, or a method of continuously supplying the base resin and the surface cross-linking solution to a continuously operated mixer and mixing them, etc. can be applied.

[0166] Preferably, the above-mentioned water step can be performed by placing the base resin and the surface water solution in a reaction vessel and stirring at a rotation speed of 100 rpm to 1,000 rpm, and preferably stirring at a rotation speed of 300 rpm to 800 rpm. When performed under the above conditions, it is suitable for performing uniform surface water.

[0167]

[0168] (2nd crushing stage)

[0169] Next, a method for manufacturing a superabsorbent resin according to one embodiment of the invention includes a step (step 5) of secondarily crushing the hydrolyzed superabsorbent resin to obtain a superabsorbent resin.

[0170] The aforementioned water-scaling step is performed on base resins with particle sizes larger than the standard, and the resulting superabsorbent resin has particles larger than the standard particle size. Accordingly, a secondary crushing step is performed to ensure that the final superabsorbent resin has the desired particle size.

[0171] In some cases, a reclassification process may be further performed to exclude particles with large particle sizes among the superabsorbent resins subject to the secondary pulverization. For example, particles with a particle size of 20 mm or more, preferably 10 mm or more, may be reclassified and subjected to a process of excluding them. In the case of particles with excessively large particle sizes as described above, they are excluded so as not to increase the load in the pulverization process as an undried body.

[0172] The above secondary crushing is crushed to have a smaller particle size compared to the primary crushing. In the case of a superabsorbent resin that has gone through a water step, even if it is crushed to a smaller particle size, the amount of fine powder generated is significantly reduced due to the appropriate moisture content.

[0173] In the above step 5, the secondary crushing may be performed so that the particles having a particle size of 150 ㎛ to 850 ㎛ account for 90 wt% or more of the total weight of the crushed particles, and preferably 95 wt% or more.

[0174] The method for performing the above secondary crushing process is not particularly limited and can be appropriately adjusted so as to satisfy the above-mentioned particle content range.

[0175] Preferably, the secondary crushing can be performed using a crusher including a roller having a plurality of pleats. The pleats of the roller have 2 to 12 pleats per about 1 cm, and the spacing between the plurality of rollers can be independently about 0.1 mm to about 1 mm. The crusher can rotate the plurality of rollers at different rotational speeds per minute, and the plurality of rollers can be configured in a plurality of stages. More preferably, the crusher can use a two-stage roll mill. In the case of a roll mill using a plurality of stages, the spacing between the corresponding rollers becomes narrower depending on the order of the stages to be crushed, and it is easy to control the desired particle size through crushing.

[0176]

[0177] (Other steps)

[0178] According to one embodiment of the invention, the superabsorbent resin manufactured through the secondary pulverization step may undergo a classification step according to particle size in order to manage the physical properties of the superabsorbent resin to be manufactured as a final product. Preferably, the particle size of the superabsorbent resin may be classified to be 150 μm to 850 μm. As described above, in the case of the superabsorbent resin manufactured through the pulverization and hydrolysis process under specific conditions, the fine powder having a particle size of less than 150 μm may be less than about 3 wt%, preferably less than about 1 wt%.

[0179] A method for manufacturing a superabsorbent resin according to one embodiment of the invention may further include a step (step 6) of mixing the superabsorbent resin (or the superabsorbent resin that has undergone an additional classification process) secondarily pulverized in step 5 with particles having a particle size smaller than a standard particle size classified after the first pulverization in step 3.

[0180] Even in the case of particles smaller than the standard particle size classified after the first pulverization in the above step 3, the particles may be pulverized into a relatively large particle size range, so that the fine particles having a particle size of less than 150 μm may be less than about 3 wt%, preferably less than about 1 wt%, and the superabsorbent resin pulverized for the second time in the above step 5 may also have a fine particles having a particle size of less than 150 μm in a content of less than about 3 wt%, preferably less than about 1 wt%.

[0181] More preferably, the total content of the superabsorbent resin that has undergone the mixing step of step 6 may be less than about 3 wt%, preferably less than about 1 wt%, of the fine powder having a particle size of less than 150 μm.

[0182] Meanwhile, an additional classification process can optionally be performed after the mixing in step 6, and superabsorbent resin particles having a particle size of 150 μm to 850 μm can be recovered using a classifier.

[0183]

[0184] (Surface cross-linking step)

[0185] A method for manufacturing a superabsorbent resin according to one embodiment of the invention may further include a step (step 7) of crosslinking the surface of the superabsorbent resin by heat-treating the superabsorbent resin in the presence of a surface crosslinking agent. Here, the superabsorbent resin to be subjected to surface crosslinking may be a superabsorbent resin that has been secondarily pulverized in step 5, or a superabsorbent resin that has undergone a mixing step in step 6. In addition, a resin that has optionally undergone an additional classification step may be used as the object of the surface crosslinking.

[0186] The above surface cross-linking step induces a cross-linking reaction on the surface of the superabsorbent resin in the presence of a surface cross-linking agent, so that the unsaturated bonds of the water-soluble ethylenically unsaturated monomer remaining on the surface without being cross-linked are cross-linked by the surface cross-linking agent, thereby forming a superabsorbent resin with a high surface cross-linking density.

[0187] Specifically, a surface cross-linking layer can be formed by a heat treatment process in the presence of a surface cross-linking agent, and the heat treatment process increases the surface cross-linking density, i.e., the external cross-linking density, while the internal cross-linking density does not change, so the manufactured superabsorbent resin having a surface cross-linking layer formed has a structure in which the external cross-linking density is higher than the internal cross-linking density.

[0188] In the above surface crosslinking step, a surface crosslinking agent composition containing an alcohol-based solvent and water in addition to a surface crosslinking agent can be used.

[0189] Meanwhile, as the surface cross-linking agent included in the surface cross-linking agent composition, any surface cross-linking agent that has been conventionally used in the production of superabsorbent resins can be used without particular limitation. For example, the surface cross-linking agent may be at least one polyol selected from the group consisting of ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, 1,2-hexanediol, 1,3-hexanediol, 2-methyl-1,3-propanediol, 2,5-hexanediol, 2-methyl-1,3-pentanediol, 2-methyl-2,4-pentanediol, tripropylene glycol, and glycerol; at least one carbonate compound selected from the group consisting of ethylene carbonate and propylene carbonate; an epoxy compound such as ethylene glycol diglycidyl ether; an oxazoline compound such as oxazolidinone; a polyamine compound; It may include an oxazoline compound; a mono-, di- or polyoxazolidinone compound; or a cyclic urea compound; etc. Preferably, the same internal crosslinking agent as described above may be used, and for example, a diglycidyl ether compound of an alkylene glycol such as ethylene glycol diglycidyl ether may be used.

[0190] Such surface cross-linking agents may be used in an amount of 0.001 to 2 parts by weight per 100 parts by weight of the superabsorbent resin. Preferably, the amount is 0.005 parts by weight or more, 0.01 parts by weight or more, or 0.02 parts by weight or more, and 0.5 parts by weight or less, or 0.3 parts by weight or less. By adjusting the content range of the surface cross-linking agent within the above-described range, a superabsorbent resin exhibiting excellent absorption performance, liquid permeability, and other physical properties can be manufactured.

[0191] Meanwhile, the surface cross-linking agent is added to the superabsorbent resin in the form of a surface cross-linking agent composition containing the surface cross-linking agent. There is no particular limitation on the composition of the method for adding the surface cross-linking agent composition. For example, a method of mixing the surface cross-linking agent composition and the base resin powder in a reaction tank, a method of spraying the surface cross-linking agent composition onto the base resin powder, a method of continuously supplying the base resin powder and the surface cross-linking agent composition to a continuously operating mixer, and a method of mixing them may be used.

[0192] In addition, the surface cross-linking agent composition may further include water and / or a hydrophilic organic solvent as a medium. This has the advantage that the surface cross-linking agent, etc. can be evenly dispersed on the base resin powder. At this time, the content of water and hydrophilic organic solvent can be applied by adjusting the addition ratio with respect to 100 parts by weight of the base resin powder for the purpose of inducing even dissolution / dispersion of the surface cross-linking agent, preventing clumping of the base resin powder, and optimizing the surface penetration depth of the surface cross-linking agent.

[0193] The above surface crosslinking step can be performed by heat treatment at a temperature of 110°C to 200°C, or 110°C to 150°C, for 30 minutes or more. More specifically, the surface crosslinking reaction can be performed by heat treatment at the above-described temperature as the highest reaction temperature for 30 to 80 minutes, or 40 to 70 minutes.

[0194] By satisfying these surface cross-linking process conditions (particularly, temperature-elevation conditions and reaction conditions at the highest reaction temperature), a superabsorbent resin that appropriately satisfies physical properties such as superior pressure permeability can be manufactured.

[0195] The means for increasing the temperature for the surface crosslinking reaction is not particularly limited. Heating can be achieved by supplying a heat medium or directly supplying a heat source. Usable heat mediums include, but are not limited to, heated fluids such as steam, hot air, and hot oil. Furthermore, the temperature of the supplied heat medium can be appropriately selected considering the means of the heat medium, the heating rate, and the target temperature. Meanwhile, directly supplied heat sources include, but are not limited to, heating via electricity or gas.

[0196] Meanwhile, the method for manufacturing a superabsorbent resin according to one embodiment of the invention may further use various polyvalent metal salts, such as aluminum sulfate salt, during surface crosslinking to further improve permeability, etc. Such polyvalent metal salts may be included on the surface crosslinking layer of the finally manufactured superabsorbent resin.

[0197] Hereinafter, the functions and effects of the invention will be described in more detail through specific examples. However, these examples are provided merely as examples of the invention and do not define the scope of the invention.

[0198]

[0199] <Example>

[0200] Example 1

[0201] (Step 1 - Polymerization Stage)

[0202] A monomer composition was prepared by mixing 100 g of acrylic acid, 130 g of 31.5 wt% caustic soda (NaOH) solution, 0.15 g of polyethylene glycol diacrylate as an internal crosslinking agent, 0.2 g of sodium persulfate as a thermal polymerization initiator, 0.01 g of diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide as a photopolymerization initiator, and 45.0 g of water in a 3 L glass vessel equipped with a stirrer and a thermometer at room temperature (25±1°C). Thereafter, the monomer composition was placed in a square reaction vessel measuring 30 cm in width and 30 cm in length, and subjected to a 10 mW / cm 2 A functional gel polymer was obtained by irradiating ultraviolet rays having a strength of 100 to cause a polymerization reaction for 60 seconds.

[0203] (Step 2 - Drying Stage)

[0204] The functional gel polymer for which the polymerization reaction was completed was cut into pieces 5 cm wide and 5 cm long, and then chopped using a screw-type chopper (meat chopper) with a hole size of 10 mm.

[0205] The above-mentioned chopped functional gel polymer was placed in an air dryer and dried at 180°C for 30 minutes to obtain a base resin.

[0206] (Step 3 - Primary crushing and classification stage)

[0207] The above-mentioned dried base resin was fed into a cutter mill having a mesh size of 8 mm and subjected to primary pulverization at a rotational blade speed of 2000 rpm. The pulverized base resin particles were classified through a standard mesh sieve of ASTM standards into particles (A) having a standard particle size of 710 μm or more and particles (B) having a standard particle size of less than 710 μm. At this time, the particles (A) having a standard particle size of 710 μm or more accounted for 64 wt% of the total weight of the pulverized particles. In addition, among the particles pulverized at this time, particles having a size of 10 mm or more accounted for 0 wt% of the total weight of the pulverized particles.

[0208] (Step 4 - Singer Stage)

[0209] 100 g of particles (A) having a standard particle size of 710 μm or more that had gone through the first crushing and classification steps above were placed in a high-speed mixer and stirred at a speed of 300 rpm. 5 g of a surface-water solution (0.1% GK aqueous solution) was added and stirred for an additional 30 seconds to obtain a surface-water absorbent resin by surface-watering the base resin.

[0210] (Step 5 - Secondary Crushing Stage)

[0211] The above-mentioned superabsorbent resin was fed into a two-stage roll mill with a roll spacing of 0.3 m and 0.15 mm, and secondary crushing was performed to obtain a superabsorbent resin (C).

[0212] (Step 6 - Mixing Stage)

[0213] A step (step 6) was performed in which particles (B) smaller than the standard particle size classified in step 3 and the superabsorbent resin (C) secondarily crushed in step 5 were mixed.

[0214] (Step 7 - Surface Cross-linking Step)

[0215] In the above step 6, the superabsorbent resin mixed was further classified with a standard mesh sieve compliant with ASTM standards to have a particle size of 150 μm to 850 μm. To 100 g of the resin, a surface cross-linking solution of 5.0 g of water, 0.1 g of propylene glycol, 1.0 g of ethylene carbonate, 1.0 g of propylene carbonate, and 1.0 g of a 23% aqueous aluminum sulfate solution was added, mixed for 2 minutes, and a surface cross-linking reaction was performed at 180°C for 40 minutes. After the surface cross-linking process, the superabsorbent resin was classified again with a standard mesh sieve compliant with ASTM standards to have a particle size of 150 μm to 850 μm.

[0216]

[0217] Example 2

[0218] In step 4 of Example 1, a superabsorbent resin was manufactured in the same manner as in Example 1, except that the amount of surface water solution added was changed to 4 g.

[0219]

[0220] Example 3

[0221] In step 4 of Example 1, a superabsorbent resin was manufactured in the same manner as in Example 1, except that the amount of surface water solution added was changed to 3 g.

[0222]

[0223] Example 4

[0224] In step 4 of Example 1, a superabsorbent resin was manufactured in the same manner as in Example 1, except that 5 g of water was used instead of the GK aqueous solution as the surface water solution.

[0225]

[0226] Example 5

[0227] In step 4 of Example 1, a superabsorbent resin was prepared in the same manner as in Example 1, except that a 0.2% GK aqueous solution was used as the surface water solution.

[0228]

[0229] Example 6

[0230] In step 4 of Example 1, a superabsorbent resin was prepared in the same manner as in Example 1, except that a 0.3% GK aqueous solution was used as the surface water solution.

[0231]

[0232] Example 7

[0233] In step 4 of Example 1, a superabsorbent resin was manufactured in the same manner as in Example 1, except that 5 g of a 2% aluminum sulfate aqueous solution was used as the surface water solution.

[0234]

[0235] Example 8

[0236] In step 4 of Example 1, a superabsorbent resin was manufactured in the same manner as in Example 1, except that 5 g of 0.1% GK + 2% aluminum sulfate aqueous solution was used as the surface water solution.

[0237]

[0238] Example 9

[0239] In step 3 of Example 1, a superabsorbent resin was manufactured in the same manner as in Example 1, except that the pulverization process was performed so that particles (A) having a standard particle size of 710 μm or more accounted for 48 wt% of the total weight of the pulverized particles.

[0240]

[0241] Example 10

[0242] In step 3 of Example 1, a superabsorbent resin was manufactured in the same manner as in Example 1, except that the pulverization process was performed so that particles (A) having a standard particle size of 710 μm or more accounted for 75 wt% of the total weight of the pulverized particles.

[0243]

[0244] Example 11

[0245] Except that the polymerization step of step 1 and the drying step of step 2 of Example 1 were changed as follows, steps 3 to 7 were performed in the same manner to produce a superabsorbent resin.

[0246] (Step 1-1: Polymerization stage)

[0247] In a 10 L glass vessel equipped with a stirrer and a thermometer, 1500 g of acrylic acid, 6.3 g of pentaerythritol triallyl ether as an internal cross-linking agent, and 3387 g of water were stirred and mixed, and the mixture was maintained at 5°C while stirring. The glass vessel containing the mixture was replaced with nitrogen at a nitrogen flow rate of 1000 cc / min for 1 hour. Next, 20.1 g of a 0.3% aqueous hydrogen peroxide solution as a polymerization initiator, 22.5 g of a 1% aqueous ascorbic acid solution, and 45.0 g of a 2% aqueous 2,2'-azobis-(2-amidinopropane)dihydrochloric acid solution were added, and simultaneously, 22.3 g of a 0.01% aqueous ferrous sulfate solution as a reducing agent were added to initiate polymerization. After the temperature of the mixture reached 85°C, polymerization was performed at 90±2°C for about 3 hours to obtain a polymer.

[0248] (Step 1-3: Atomization and Step 1-2: Neutralization (Flocculation) Step)

[0249] 5,000 g of the obtained polymer was introduced into a micronizer (F200, Karl Schnell) equipped with a porous plate having a plurality of holes with a hole size of 10 mm, rotating at 1,500 rpm, and atomized into primary particles having a particle size of several tens to several hundred micrometers. At this time, 90 g of a 1.5 w% aqueous solution of Glycerol Monolaurate (GML) was introduced to prevent excessive agglomeration.

[0250] Afterwards, the meat chopper, which is a screw-type mincer equipped with a perforated plate with a plurality of holes having a hole size of 6 mm, was rotated at 500 rpm, and the finely divided polymer was fed into it, and the process of manufacturing secondary aggregated particles was repeated three times. At this time, 1,904 g of a 50% NaOH aqueous solution was added in the first pass to neutralize some of the acidic groups of the polymer. In the second pass, 18.8 g of a 15% Na2SO3 aqueous solution was added to reduce some of the polymer. In the third pass, the polymer was passed without adding any additives to manufacture a neutralized and finely divided hydrogel polymer.

[0251] (Step 2: Drying Stage)

[0252] The above polymerization reaction was performed by cutting the functional gel polymer into pieces 5 cm wide and 5 cm long, and then using a screw-type chopper (meat chopper) with a hole size of 10 mm.

[0253] The above-mentioned chopped functional gel polymer was placed in an air dryer and dried at 120°C for 40 minutes to obtain a base resin.

[0254] Thereafter, steps 3 to 7 were performed in the same manner as in Example 1 to manufacture a superabsorbent resin.

[0255]

[0256] Comparative Example 1

[0257] A superabsorbent resin was manufactured in the same manner as in Example 1, except that the water step of Step 4 of Example 1 was not performed and the roller gaps of the two-stage roll mill were set to 0.3 mm and 0.2 mm in the second crushing step of Step 5. That is, Steps 1 to 3 of Example 1 were performed in the same manner.

[0258]

[0259] Comparative Example 2

[0260] (Manufacturing of differential reassembly)

[0261] First, in Comparative Example 1, particles less than 150 μm were obtained after classification at each stage to obtain fine particles (obtained from the classification process of steps 3 and 7).

[0262] 100 g of the above-obtained fine particles were placed in a high-speed mixer, stirred at a rotation speed of 500 rpm, 100 g of water was added, and mixed for 10 seconds to prepare a fine powder reassembled body.

[0263] (Circulation of differential reassembly)

[0264] Step 1 of Comparative Example 1 (= A functional gel polymer was manufactured using the same method as in the Example).

[0265] Next, 100 g of the previously obtained finely divided reassembled body was mixed with 1,000 g of the functional gel polymer, which had undergone the polymerization reaction, cut into 5 cm wide and 5 cm long pieces, and the mixture was chopped using a screw-type chopper (meat chopper) with a hole size of 10 mm.

[0266] The above-described chopped functional gel polymer was placed in an air-flow dryer and dried at 180°C for 30 minutes to obtain a base resin. The subsequent process was performed in the same manner as in Comparative Example 1 to obtain a superabsorbent resin.

[0267]

[0268] Comparative Example 3

[0269] A superabsorbent resin was manufactured in the same manner as in Example 11, except that the water step of Step 4 of Example 11 was not performed and the second crushing step of Step 5 was performed with the roller gaps of a two-stage roll mill set to 0.3 mm and 0.2 mm. That is, Steps 1 to 3 of Example 11 were performed in the same manner.

[0270]

[0271] <Experimental Example>

[0272] Experimental Example 1 - Evaluation of Particle Properties

[0273] The superabsorbent resins of the above examples and comparative examples were placed in a classifier with 4000 ㎛, 2000 ㎛, 1400 ㎛, 850 ㎛, 710 ㎛, 600 ㎛, 300 ㎛, and 150 ㎛ pans according to ASTM standards, and were classified by vibrating at an amplitude of 1.5 mm / g for 10 minutes. The weight of the particles on the upper side of each sieve was measured, and the average particle size and the amount of fine powder generated were measured according to the following method.

[0274] (1) Average particle size (㎛)

[0275] The average particle size of the above-classified superabsorbent resin was measured according to the following mathematical formula 1, and the results are shown in Table 1.

[0276] [Mathematical Formula 1]

[0277]

[0278] (2) Amount of fine particles generated (%)

[0279] The amount of fine particles generated from the above-classified superabsorbent resin was measured according to the following mathematical formula 2, and the results are shown in Table 1.

[0280] [Equation 2]

[0281] Fine particle generation amount (%) = (Weight of particles less than 150㎛) / (Weight of particles greater than 150㎛ and less than 850㎛) * 100

[0282]

[0283] Experimental Example 2 - Evaluation of the physical properties of superabsorbent resin

[0284] In the above examples and comparative examples, the properties of the superabsorbent resin were evaluated using the following method and are listed in Table 1 below.

[0285] Unless otherwise specified, all of the following property evaluations were conducted under constant temperature and humidity (23±1℃, relative humidity 50±10%), and physiological saline solution or saline refers to a 0.9 wt% sodium chloride (NaCl) aqueous solution.

[0286] (1) Centrifuge Retention Capacity (CRC, g / g)

[0287] The water retention capacity of the superabsorbent resins of the above examples and comparative examples by the absorption rate under no load was measured according to the European Disposables and Nonwovens Association (EDANA) standard EDANA WSP 241.3.

[0288] Specifically, the superabsorbent resin obtained through each of the examples and comparative examples was uniformly placed in a non-woven bag (W0(g)) (approximately 0.2 g), sealed, and then immersed in a physiological saline solution (0.9 wt%) at room temperature. After 30 minutes, water was removed from the bag for 3 minutes using a centrifuge at 250 G, and the mass W2(g) of the bag was measured. In addition, the same operation was performed without using the resin, and the mass W1(g) at that time was measured.

[0289] Using each mass obtained, CRC (g / g) was calculated according to the following mathematical formula 3.

[0290] [Equation 3]

[0291] CRC (g / g) = {[W2(g) - W1(g)] / W0(g)} - 1

[0292] (2) Absorbency under Pressure (AUP: Absorbency under Pressure, g / g)

[0293] The 0.3 psi pressurized absorbency of the superabsorbent resins of the above examples and comparative examples was measured according to EDANA method WSP 242.3.

[0294] Specifically, a 400-mesh stainless steel wire mesh was installed on the bottom of a plastic cylinder with an inner diameter of 25 mm. Under conditions of room temperature and 50% humidity, superabsorbent resin W0 (g) (0.9 g) was uniformly sprayed on the wire mesh, and a piston capable of uniformly applying a load of 0.3 psi thereon was installed, with an outer diameter slightly smaller than 25 mm, no gap with the inner wall of the cylinder, and unobstructed up-and-down movement. At this time, the weight W3 (g) of the device was measured.

[0295] A glass filter with a particle size of 90 mm and a thickness of 5 mm was placed inside a petroleum dish with a particle size of 150 mm, and a saline solution consisting of 0.9 wt% sodium chloride was placed so that it was level with the upper surface of the glass filter. A sheet of filter paper with a particle size of 90 mm was placed on top of it. The measuring device was placed on the filter paper, and the liquid was absorbed under a load for 1 hour. After 1 hour, the measuring device was lifted, and its weight W4 (g) was measured.

[0296] Using each mass obtained, the pressurized absorbency (g / g) was calculated according to the following mathematical formula 4.

[0297] [Equation 4]

[0298] AUP(g / g) = [W4(g) - W3(g)] / W0(g)

[0299] The above measurement was repeated five times, and the average value and standard deviation were calculated.

[0300] (3) Absorption speed (Vortex time, sec)

[0301] The absorption rate (vortex time) was measured in seconds according to the method described in International Publication No. 1987-003208.

[0302] Specifically, 2 g of superabsorbent resin was added to 50 mL of physiological saline solution at 23°C to 24°C, and the time until the vortex disappeared was measured in seconds while stirring at 600 rpm with a magnetic bar (particle diameter 8 mm, length 30 mm).

[0303] ClassificationAverage particle size(㎛)Particulate matter generation amount(%)CRC(g / g)AUP(g / g)Vortex absorption speed(sec)Example 14668.037.131.933Example 24668.336.832.034Example 347110.336.531.835Example 44769.136.731.536Example 54618.136.231.035Example 64557.836.630.534Example 748010.336.530.634Example 84728.436.231.835Example 94629.436.531.434Example 104707.536.431.836 Example 114607.537.433.130 Comparative Example 147114.436.731.439 Comparative Example 246515.935.830.838 Comparative Example 346213.537.232.937

[0304] As can be seen in Table 1 above, in the examples, the amount of fine particles generated was significantly reduced by performing the grinding and hydrolysis processes under specific conditions, thereby realizing excellent absorption properties. In the comparative examples in which the grinding and hydrolysis processes according to the present invention were not performed, the amount of fine particles generated was significantly increased compared to the examples, and it was confirmed that the physical properties, such as the absorption rate, were somewhat reduced accordingly.

Claims

1. A step of forming a functional gel polymer including a crosslinked polymer obtained by crosslinking a water-soluble ethylenically unsaturated monomer having an acidic group in the presence of an internal crosslinking agent (step 1); A step of drying the above functional gel polymer to obtain a base resin (step 2); A step of first crushing the above dried base resin and classifying it into particles larger than or equal to a standard particle size and particles smaller than or equal to a standard particle size (step 3); A step (step 4) of obtaining a hydrophilic superabsorbent resin using a surface hydrophilic solution containing water for a base resin having a particle size greater than the above-mentioned standard particle size; and It includes a step (step 5) of obtaining a superabsorbent resin by secondarily crushing the above-mentioned superabsorbent resin, The above standard particle size is determined within the particle size range of 300 ㎛ or more and 850 ㎛ or less. Method for producing superabsorbent resin.

2. In paragraph 1, In the above step 3, the first crushing is performed so that particles having a standard particle size or larger account for 40% or more by weight of the total crushed particle weight. Method for producing superabsorbent resin.

3. In paragraph 1, In the above step 3, the first crushing is performed so that the particles of 10 mm or more are less than 5 wt% of the total crushed particle weight. Method for producing superabsorbent resin.

4. In paragraph 1, The above standard particle size is determined within the particle size range of 600 ㎛ or more and 850 ㎛ or less. Method for producing superabsorbent resin.

5. In paragraph 1, In the above step 4, the surface water solution is used in an amount of 0.1 to 10 parts by weight per 100 parts by weight of the base resin. Method for producing superabsorbent resin.

6. In paragraph 1, In the above step 4, the surface water solution further comprises at least one additive selected from the group consisting of polyacrylic acid-polyethylene oxide comb polymer (GK), aluminum sulfate, polyethylene glycol, sodium dodecyl sulfate, glycerol monolaurate and sodium stearoyl lactylate. Method for producing superabsorbent resin.

7. In paragraph 6, The above additive is included in an amount of 0.01 to 10 parts by weight per 100 parts by weight of the surface water solution. Method for producing superabsorbent resin.

8. In paragraph 1, The above step 4 is performed by stirring at a rotation speed of 100 rpm to 1,000 rpm. Method for producing superabsorbent resin.

9. In paragraph 1, In the above step 5, the secondary crushing is performed so that particles having a particle size of 150 ㎛ to 850 ㎛ account for 90% or more by weight of the total crushed particle weight. Method for producing superabsorbent resin.

10. In paragraph 1, A step (step 6) further comprising mixing particles smaller than the standard particle size classified in step 3 and the superabsorbent resin secondarily crushed in step 5. Method for producing superabsorbent resin.

11. In paragraph 1 or paragraph 10, A method further comprising a step (step 7) of crosslinking the surface of the superabsorbent resin by heat treating the superabsorbent resin in the presence of a surface crosslinking agent. Method for producing superabsorbent resin.