High-corrosion resistance oil well pipe steel and its preparation method

MYPI2025003386A0Undetermined Publication Date: 2024-06-13
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025003386
Authority / Receiving Office
MY · MY
Patent Type
Applications
Priority Date
2022-12-13
Filing Date
2023-12-08
Publication Date
2024-06-13

AI Technical Summary

Technical Problem

Existing oil well pipe steel has high alloying element content, high cost and complex process, which cannot meet the needs of mass production and practical applications, especially in environments containing H2S and CO2. The corrosion resistance is insufficient.

Method used

Provided is a highly corrosion-resistant oil well pipe steel, the composition of which includes C: ≤0.03%, Cr: 17.3% ~ 18.4%, Mo: 0.5% ~ 2.0%, Ni: 1.0% ~ 2.8%, Mn: 1.0% ~ 3.5% , Si: 0.1% ~ 0.5%, N: 0.1% ~ 0.25%, P: ≤0.03%, S: ≤0.01%. Through the mixed structure of ferrite + austenite + martensite, combined with the hot deformation process of controlled rolling and cooling, the Cr and Ni are controlled , Mn, Mo, N element ratio to improve corrosion resistance and strength.

Benefits of technology

It achieves high strength, excellent corrosion resistance and H2S stress corrosion resistance at low Cr content, reduces raw material costs, and is suitable for high-pressure and high-temperature oil and gas mining environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025003386_DRAWING_001
    Figure PI2025003386_DRAWING_001
  • Figure PI2025003386_DRAWING_002
    Figure PI2025003386_DRAWING_002
  • Figure PI2025003386_DRAWING_003
    Figure PI2025003386_DRAWING_003
Patent Text Reader

Abstract

The present application discloses a high-corrosion resistance oil well pipe steel and its preparation method, belongs to the technical field of corrosion-resistant steel, and solves the problems of higher alloy element content and higher cost of existing oil well pipe steels. By mass percentage, the components of the high-corrosion resistance steel comprise: C: ≤0.03%, Cr: 17.3%~18.4%, Mo: 0.5%~2.0%, Ni: 1.0%~2.8%, Mn: 1.0%~3.5%, Si: 0.1%~0.5%, N: 0.1%~0.25%, P: ≤0.03%, S: ≤0.01%, and the rest is Fe and unavoidable impurities. The oil well pipe steel of the present application has high strength, good plasticity and toughness and excellent corrosion resistance. Fig.1 is the figure accompanying the abstract.
Need to check novelty before this filing date? Find Prior Art

Description

High corrosion-resistant oil well pipe steel and preparation method thereof Technical Field

[0001] The present application relates to the technical field of corrosion-resistant steel, and in particular to a highly corrosion-resistant oil well pipe steel and a preparation method thereof. Background Art

[0002] Oil well pipes are important consumables in the process of oil and natural gas exploration and development, accounting for about 40% of the total steel used in the oil and gas industry, and are an important component of oil and natural gas extraction equipment. As an important petroleum equipment material, oil well pipes account for an average of 20% to 30% of the entire well construction cost. Therefore, whether the entire petroleum project can proceed smoothly is inseparable from the quality of oil well pipes. Oil well pipes are placed in casings and are used to collect oil and gas. Due to the flow of corrosive liquids in oil well pipes, various corrosion-resistant products must be selected according to the corrosion conditions. In China, Sichuan gas fields contain H2S, and some oil and gas wells in Sichuan, North China and western oil and gas fields contain CO2 and H2S, CO2, C1 - Coexistence. Under such oil production conditions, higher requirements are also placed on the corrosion resistance of oil well pipes. At present, the material for oil well pipes that resist CO2 corrosion is mainly 13Cr martensitic stainless steel, but martensitic steel cannot be used in environments containing H2S. Although the use of 22Cr (or 25Cr, 27Cr, the higher the Cr content, the better the corrosion resistance) duplex stainless steel with a higher alloy content can meet the requirements for oil well pipe use, the material cost is high and it is not suitable for large-scale industrial applications in oil and gas production scenarios. In view of the actual situation of China's oil and gas production and the limitations of mineral resources, it is imperative to develop highly corrosion-resistant oil well pipe materials.

[0003] At present, there are many patents at home and abroad on the varieties of oil well pipe steel with good comprehensive performance and the corresponding process flow, but most of them have problems such as high cost or complex process and cannot meet the needs of mass production and practical application.

[0004] Summary of the Invention

[0005] In view of the above situation, the present application aims to provide a highly corrosion-resistant oil well pipe steel and a preparation method thereof, so as to solve the problems of high alloy element content and high cost of existing oil well pipe steel.

[0006] The purpose of this application is mainly achieved through the following technical solutions:

[0007] On the one hand, the present application provides a high-corrosion-resistant oil well pipe steel, wherein the components of the high-corrosion-resistant oil well pipe steel include, by mass percentage, C: ≤0.03%, Cr: 17.3% to 18.4%, Mo: 0.5% to 2.0%, Ni: 1.0% to 2.8%, Mn: 1.0% to 3.5%, Si: 0.1% to 0.5%, N: 0.1% to 0.25%, P: ≤0.03%, S: ≤0.01%, and the balance is Fe and unavoidable impurities.

[0008] In a possible design, the composition of the high corrosion resistant oil well pipe steel is Cr+3.3Mo+16N≥26.

[0009] In a possible design, the composition of the high corrosion resistant oil well pipe steel is 60Ni+17Mn-12Mo-800N≤0.

[0010] In one possible design, the composition of the high-corrosion-resistant oil well tubular steel, in percentage by mass, may be: C: 0.01% to 0.03%, Cr: 17.4% to 18.4%, Mo: 1.0% to 2.0%, Ni: 1.0% to 2.7%, Mn: 1.4% to 3.2%, Si: 0.1% to 0.5%, N: 0.13% to 0.25%, P: ≤0.03%, S: ≤0.01%, with the balance being Fe and unavoidable impurities.

[0011] In a possible design, the microstructure of the high corrosion resistant oil well tubular steel is a mixed structure of ferrite + austenite + martensite.

[0012] In a possible design, in the microstructure of the high corrosion resistant oil well pipe steel, the volume percentage of austenite is 20% to 40%, and the volume percentage of martensite is 10% to 40%.

[0013] In a possible design, the austenite grain size in the microstructure of the high corrosion resistant oil well tubular steel is less than 3 μm.

[0014] On the other hand, the present application also provides a method for preparing high-corrosion-resistant oil-well tubular steel, which is used to prepare the above-mentioned high-corrosion-resistant oil-well tubular steel, comprising:

[0015] Step 1: Melt the metal raw materials into molten steel;

[0016] Step 2: smelting the molten steel into continuous casting billets or ingots by continuous casting or mold casting;

[0017] Step 3: Forging the continuous casting billet or ingot into a forging billet;

[0018] Step 4: Roll the forged billet into a tube billet, and obtain high corrosion-resistant oil well pipe steel by controlling the hot rolling and cooling process parameters.

[0019] In a possible design, in step 3, the forging temperature is 1150-1250°C.

[0020] In one possible design, in step 4, controlling the hot rolling and cooling process parameters includes: controlling the starting rolling temperature to be above 1050°C, the final rolling temperature to be above 950°C, the deformation of the first rolling pass to be no more than 30%, and the deformation of the final rolling pass to be no more than 50%.

[0021] Compared with the prior art, this application has the following beneficial effects:

[0022] a) The highly corrosion-resistant oil well pipe steel of this application precisely controls the mass percentages of Cr, Ni, Mn, Mo, and N in the steel. Combined with a controlled rolling and controlled cooling hot deformation process, a mixed structure of ferrite + austenite + martensite can be obtained, significantly improving the corrosion resistance and strength of the oil well pipe steel. Because the 17Cr material of this application contains ultrafine martensite, the tensile strength of the material is superior to that of duplex stainless steel with a higher Cr content, achieving high strength with a lower Cr content. Compared with the martensitic stainless steel of the prior art, the stainless steel of this application introduces ferrite and austenite to achieve superior intergranular corrosion resistance and H2S stress corrosion resistance. The austenite content in the stainless steel of this application is much higher than that of martensitic stainless steel. It is difficult to obtain an austenite content greater than 20% in martensitic stainless steel. Therefore, the material of this application has better resistance to hydrogen embrittlement.

[0023] b) The steel of this application not only ensures high strength, good ductility and excellent corrosion resistance, but also ensures a yield strength greater than 600 MPa (e.g., 601-648 MPa), a tensile strength greater than 910 MPa (e.g., 911-1010 MPa), and an elongation greater than 22% (e.g., 23%-24%). (180°C) CO2 corrosion rate 0.028 g / m 2 h or less (e.g. 0.0203 to 0.0275 g / m 2 h); (200℃) CO2 corrosion rate 0.1g / m 2 h or less (e.g. 0.078 to 0.099 g / m 2 h); pitting corrosion rate 2.5g / m 2 h or less (e.g. 1.693 to 2.433 g / m 2 h); crevice corrosion rate 5.9g / m 2 h or less (e.g. 3.303 to 5.852 g / m 2 h); H2S stress corrosion test passed.

[0024] c) The steel of this application exhibits excellent strength, toughness, and corrosion resistance, combining the high strength of super martensitic stainless steel oil well pipe with the stress corrosion, intergranular corrosion, and low-level H2S stress corrosion resistance of duplex stainless steel. Due to its low Cr and Ni content, the raw material cost of this steel is comparable to or slightly lower than that of existing super 13Cr martensitic stainless steel. Furthermore, its excellent hot workability makes this steel low-cost, economical, and practical.

[0025] Other features and advantages of the present application will be described in the following description, and some will become apparent from the description or be understood by practicing the present application. The objectives and other advantages of the present application can be realized and obtained by the structures particularly pointed out in the written description, claims, and drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The accompanying drawings are only for the purpose of illustrating particular embodiments and are not to be considered as limiting the present application. Like reference symbols denote like components throughout the drawings.

[0027] FIG1 is a microstructure diagram of the steel after hot rolling of Example 1 of the present application;

[0028] FIG2 is a transmission electron microscope image of point M in FIG1 of the present application;

[0029] FIG3 is a microstructure diagram of the steel of Example 2 of the present application;

[0030] FIG4 is a microstructure diagram of the steel of Example 3 of the present application;

[0031] FIG5 is a microstructure diagram of the steel of Example 4 of the present application;

[0032] FIG6 is a photograph of the hot-rolled plate of Example 1 of the present application. DETAILED DESCRIPTION

[0033] The preferred embodiments of the present application are described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of the present application and are used together with the embodiments of the present application to illustrate the principles of the present application.

[0034] The present application provides a high-corrosion-resistant oil well pipe steel. The high-corrosion-resistant oil well pipe steel comprises, by mass percentage, C: ≤0.03%, Cr: 17.3% to 18.4%, Mo: 0.5% to 2.0%, Ni: 1.0% to 2.8%, Mn: 1.0% to 3.5%, Si: 0.1% to 0.5%, N: 0.1% to 0.25%, P: ≤0.03%, S: ≤0.01%, and the balance being Fe and unavoidable impurities.

[0035] Specifically, Cr+3.3Mo+16N (i.e., PREN) ≥ 26, and 60Ni+17Mn-12Mo-800N ≤ 0; Cr, Mo, N, Ni, and Mn refer to the mass percentage of these elements multiplied by 100. For example, if the mass percentage of Cr is 18.4%, then Cr here is 18.4.

[0036] The following is a detailed description of the functions and dosage of the components contained in this application:

[0037] C: Although the addition of carbon can significantly improve the hardness and strength of steel, due to the high diffusion capacity of carbon, it is easy to combine with Cr to form M 23 C6 carbide: This type of carbide precipitates rapidly (≤0.5 hours) in the temperature range of 700-900°C, or precipitates when kept at 550-700°C for a longer period of time. The precipitation of carbides causes local Cr depletion, increases the material's susceptibility to intergranular corrosion, and deteriorates its corrosion resistance. Therefore, in this application, considering the combined effects of strength and corrosion resistance, its content is controlled to ≤0.03%.

[0038] Cr: The main element that ensures the corrosion resistance of stainless steel. It is also a ferrite-forming element. Improper control of Cr content will increase the ferrite content in the organization and reduce the strength. Considering comprehensive considerations, its content is controlled at 17.3% to 18.4%.

[0039] Ni: It is an element that strongly forms and stabilizes austenite and expands the austenite phase region. Ni is an element that improves the toughness and corrosion resistance of stainless steel in reducing media. Ni is also an important element for improving the austenite phase's resistance to transgranular stress corrosion in various media. At the same time, compared with Mn, Ni can reduce the cold work hardening tendency of the austenite phase. Considering cost control, this application controls its content within a range of 1.0% to 2.8%.

[0040] Mn: It can increase the solubility of N in steel and inhibit the precipitation of harmful phase chromium nitride, but Mn reduces the toughness of stainless steel. Compared with Ni, Mn is an austenite-forming element. Mn has different hardening effects on the austenite phase of stainless steel and the overall material. Therefore, this application controls its content within 1.0% to 3.5%.

[0041] Mo: In addition to improving the corrosion resistance of stainless steel in oxidizing media, it also has a good effect on improving the corrosion resistance of stainless steel in reducing media. At the same time, in order to ensure pitting resistance, alloying elements such as Cr and Mo that increase the PREN value should not be too low. At the same time, alloy cost control and phase balance must also be taken into account. Comprehensive considerations should be taken to control its content to 0.5% to 2.0%.

[0042] Si: Added as a deoxidizer during the smelting process, it can achieve a deoxidizing effect. Excessive addition will deteriorate the material's intergranular corrosion resistance. This application controls its content to 0.1% to 0.5%.

[0043] Nitrogen: Like nickel, it is an element that strongly forms and stabilizes austenite and expands the austenite phase. Nitrogen also significantly improves the pitting corrosion resistance of the austenite phase in stainless steel, thereby improving the overall pitting corrosion resistance of the stainless steel. In some media, nitrogen has a positive effect on the stress resistance of stainless steel, and there is an optimal value. Further increasing the nitrogen content decreases its stress corrosion resistance. Nitrogen is also a relatively economical alloying element, but it reduces the hot workability of stainless steel. Therefore, this application controls its content to 0.1% to 0.25%.

[0044] S: It significantly reduces the hot working properties of steel and easily reacts with Mn to form MnS inclusions, which reduces the material's resistance to pitting and crevice corrosion. Therefore, its content is controlled to ≤ 0.01%.

[0045] P: It is a harmful impurity element that will not only deteriorate the plasticity of the material, but also reduce the corrosion resistance of the material. Therefore, its content is controlled to be ≤0.03%.

[0046] Specifically, this application comprehensively considers three aspects: ensuring corrosion resistance, raw material costs caused by alloy element matching, harmful phase precipitation caused by alloy element matching, and cost changes caused by hot working yield. In addition to controlling the content of individual elements of the main alloying elements Cr, Ni, Mn, and N in steel, in order to ensure corrosion resistance, Cr+3.3Mo+16N≥26 is controlled. In order to make the maximum precipitation temperature of harmful phases lower than 750°C and ensure that the material has good hot working properties, and considering that the three-phase ratio can be controlled during the hot working process between 900 and 1180°C, it is necessary to control the content of Ni, Mn, Mo, and N elements to meet the following requirements: 60Ni+17Mn-12Mo-800N≤0.

[0047] To further improve the comprehensive performance of the highly corrosion-resistant oil-well tubular steel, the composition of the highly corrosion-resistant oil-well tubular steel, by mass percentage, may be: C: 0.01%-0.03%, Cr: 17.4%-18.4%, Mo: 1.0%-2.0%, Ni: 1.0%-2.7%, Mn: 1.4%-3.2%, Si: 0.1%-0.5%, N: 0.13%-0.25%, P: ≤0.03%, S: ≤0.01%, with the balance being Fe and unavoidable impurities. The ratio of Cr + 3.3Mo + 16N (i.e., PREN) is 26.1-27.8, and the ratio of 60Ni + 17Mn - 12Mo - 800N is ≤-0.42.

[0048] Specifically, the microstructure of the high-corrosion-resistant oil well tubular steel is a mixed structure of ferrite, austenite, and martensite, wherein the volume percentage of austenite is 20% to 40% (e.g., 20% to 35%), and the volume percentage of martensite is 10% to 40% (e.g., 30% to 40%). The martensite is dispersed in the austenite in the form of ultrafine flakes, alternately stacked and divided with the austenite, resulting in a smaller austenite grain size (e.g., austenite grain size <3 μm), and the thickness of the martensite flakes is less than 100 nm.

[0049] Compared with the existing technology, the high corrosion-resistant oil well pipe steel of the present application is a three-phase structure. The steel of the present application has the characteristics of low Cr and low alloy element content to obtain higher strength. It can simultaneously have the characteristics of high strength, resistance to intergranular corrosion, stress corrosion, high toughness and good welding performance, and has excellent comprehensive performance. At the same time, the composite structure of martensite and austenite can increase the interface density in the organization, thereby obtaining high-strength mechanical properties that are superior to traditional duplex stainless steel. Its balanced phase ratio in the conventional hot working temperature range (900-1180℃) brings excellent hot working performance. The multi-phase composite organizational form after hot working has better corrosion resistance than single-phase martensitic stainless steel while ensuring certain cold working performance.

[0050] The present application also provides a method for preparing the above-mentioned high corrosion-resistant oil well pipe steel, comprising:

[0051] Step 1: Melt the metal raw materials into molten steel;

[0052] Step 2: smelting the molten steel into continuous casting billets or ingots by continuous casting or mold casting;

[0053] Step 3: heating the continuous casting billet or ingot at 1150-1250° C. and forging the billet to form a forging billet;

[0054] Step 4: The forged billet is heated at 1050-1250°C and rolled into a tube billet. High-corrosion-resistant oil-well tubular steel is obtained by controlling the hot rolling and cooling process parameters. The three-phase structure of the high-corrosion-resistant oil-well tubular steel is: 10%-40% martensite, 20%-40% austenite, and the remainder ferrite.

[0055] Specifically, in the above steps 1 and 2, a converter or electric furnace is used for smelting, LF refining, and casting into ingots.

[0056] Specifically, in step 3 above, the forging temperature is 1150-1250°C. This is because the material of the present application is a two-phase ferrite + austenite at temperatures above 800°C. The ratio of the two phases changes with the heating temperature. The higher the heating temperature, the more ferrite content there is, and the corresponding austenite content decreases. Selecting this temperature range for heating simultaneously ensures the full dissolution of harmful precipitated phases and also increases the ferrite phase content in the material to greater than 70%, allowing the steel to be forged in a region close to the single-phase region with better thermoplasticity. This avoids forging cracking caused by the uncoordinated deformation of the two phases during the forging process due to the different thermal deformation capabilities of the ferrite and austenite phases.

[0057] Specifically, in the above step 4, the tube is hot rolled and then water-cooled to room temperature to avoid precipitation of harmful phases.

[0058] Specifically, in step 4 above, since the oil well tubular steel of the present application has an excellent hot working window, controlling the hot rolling and cooling process parameters includes: controlling the starting rolling temperature to be above 1050°C (e.g., 1050-1200°C), the finishing rolling temperature to be above 950°C (e.g., 950-1050°C), the deformation in the first rolling pass to be no more than 30%, and the deformation in the final rolling pass to be no more than 50%.

[0059] Compared with the prior art, the high corrosion-resistant oil well pipe steel of the present application precisely controls the mass percentages of Cr, Ni, Mn, Mo, and N elements in the steel, and combined with the controlled rolling and controlled cooling hot deformation process, can obtain a mixed structure of ferrite + austenite + martensite, which greatly improves the corrosion resistance and toughness of the oil well pipe steel. In stainless steel, increasing the Cr content can increase the strength of the material, but because the 17Cr material of the present application contains ultrafine martensite, the tensile strength of the material is better than that of duplex stainless steel with a higher Cr content. Compared with the duplex stainless steel of the prior art, the 17Cr three-phase structure stainless steel of the present application controls the content combination of Cr, Ni, Mn, Mo, and N to obtain a three-phase structure with adjustable martensite content after hot rolling, thereby achieving high strength with a lower Cr content. Compared with the martensitic stainless steel of the prior art, the introduction of ferrite and austenite in the stainless steel of the present application obtains better intergranular corrosion resistance and H2S stress corrosion resistance. The austenite content in the stainless steel of the present application is much higher than that in martensitic stainless steel. It is difficult to obtain an austenite content greater than 20% in martensitic stainless steel. Therefore, the material of the present application has better resistance to hydrogen embrittlement.

[0060] The steel of this application not only ensures high strength, good ductility and excellent corrosion resistance, but also ensures a yield strength greater than 600 MPa (e.g., 601-648 MPa), a tensile strength greater than 910 MPa (e.g., 911-1010 MPa), and an elongation greater than 22% (e.g., 23%-24%). (180°C) CO2 corrosion rate 0.028 g / m 2h or less (e.g. 0.0203 to 0.0275 g / m 2 h); (200℃) CO2 corrosion rate 0.1g / m 2 h or less (e.g. 0.078 to 0.099 g / m 2 h); pitting corrosion rate 2.5g / m 2 h or less (e.g. 1.693 to 2.433 g / m 2 h); crevice corrosion rate 5.9g / m 2 h or less (e.g. 3.303 to 5.852 g / m 2 h); H2S stress corrosion test passed.

[0061] The steel presented in this application has excellent strength, toughness, and corrosion resistance, combining the high strength of super martensitic stainless steel oil well pipe with the stress corrosion, intergranular corrosion, and low-level H2S stress corrosion resistance of duplex stainless steel. Due to its low Cr and Ni content, the raw material cost of this steel is comparable to or slightly lower than that of existing super 13Cr martensitic stainless steel. Furthermore, its excellent hot workability makes this steel low-cost, economical, and practical.

[0062] Examples 1-4

[0063] The advantages of precise control of the composition and process parameters of the steel of the present application are demonstrated below with specific examples and comparative examples. 13Cr is selected as a comparison object for corrosion performance.

[0064] Examples 1-4 of the present application provide a highly corrosion-resistant oil well pipe steel and a preparation method thereof. The chemical compositions of the steels of Examples 1-4 are shown in Table 1.

[0065] The preparation method of Example 1 comprises:

[0066] Step 1: Melt the metal raw materials into molten steel; use the die casting method to smelt the molten steel into steel ingots to obtain castings;

[0067] Step 2: After heating the ingot to 1150°C and keeping it for 2 hours, forging and opening the ingot to make a forging ingot;

[0068] Step 3: The forging billet is kept at 1050℃ for 2h and rolled into a tube billet. By controlling the hot rolling and cooling process parameters (the deformation amount of the first pass is 25%, the deformation amount of the final rolling pass is 48%, the final rolling plate thickness is controlled at about 3.5mm, and water cooling), the final rolling temperature is controlled at 960℃ to adjust the three-phase structure content, ferrite content is 40%, martensite content is 40%, and austenite content is 20%.

[0069] The preparation method of Example 2 comprises:

[0070] Step 1: Melt the metal raw materials into molten steel; use the die casting method to smelt the molten steel into steel ingots to obtain castings;

[0071] Step 2: After heating the ingot to 1180℃ and keeping it at that temperature for 1.5h, forging and opening the ingot to make a forging ingot;

[0072] Step 3: The forging billet is kept at 1150℃ for 2h and rolled into a tube billet. By controlling the hot rolling and cooling process parameters (the deformation amount of the first pass is 28%, the deformation amount of the final rolling pass is 45%, the final rolling plate thickness is controlled at about 3.5mm, and water cooling), and by controlling the final rolling temperature at 1000℃, the three-phase structure content is adjusted to 45% ferrite content, 30% martensite content, and 25% austenite content.

[0073] The preparation method of Example 3 comprises:

[0074] Step 1: Melt the metal raw materials into molten steel; use the die casting method to smelt the molten steel into steel ingots to obtain castings;

[0075] Step 2: After heating the ingot to 1200℃ and keeping it at that temperature for 1 hour, forging and opening the ingot to make a forging ingot;

[0076] Step 3: The forging billet is kept at 1200℃ for 2h and rolled into a tube billet. By controlling the hot rolling and cooling process parameters (the deformation of the first pass is 23%, the deformation of the final rolling pass is 46%, the final rolling thickness is controlled at about 3.5mm, and water cooling), and by controlling the final rolling temperature at 1050℃ (adjusting the three-phase structure content, the ferrite content is 40%, the martensite content is 30%, and the austenite content is 30%).

[0077] The preparation method of Example 4 comprises:

[0078] Step 1: Melt the metal raw materials into molten steel; use the die casting method to smelt the molten steel into ingots to obtain billets;

[0079] Step 2: After heating the ingot to 1250℃ and keeping it for 1 hour, forging and blanking are carried out to make forging blanks;

[0080] Step 3: The forging billet is kept at 1200℃ for 2h and rolled into a tube billet. By controlling the hot rolling and cooling process parameters (the deformation amount of the first pass is 26%, the deformation amount of the final rolling pass is 45%, the final rolling plate thickness is controlled at about 3.5mm, and water cooling), and by controlling the final rolling temperature at 1050℃, the three-phase structure content is adjusted to 35% ferrite content, 30% martensite content, and 35% austenite content.

[0081] The specific process parameters of Examples 1-4 are shown in Table 2, and the mechanical properties of Examples 1-4 are shown in Table 3. Figure 1 is a microstructure diagram of the steel of Example 1 of the present application, and Figure 2 is a transmission electron microscope image of point M in Figure 1 of the present application, in which the upper left corner is the diffraction spot of the martensite and austenite matrix at point A, which can prove the crystal structure of the black martensite sheet and the thickness of the martensite sheet is less than 100nm.

[0082] Figures 3-5 are microstructure diagrams of the steels of Examples 2-4 of the present application, respectively; the microstructures of Examples 1-4 are shown in Table 4 below. The microstructure of the high-corrosion-resistant oil well tubular steel of the present application is a mixed structure of ferrite, austenite, and martensite, wherein the volume percentage of austenite is 20% to 40% (e.g., 20% to 35%), and the volume percentage of martensite is 10% to 40% (e.g., 30% to 40%). The martensite is dispersed in the austenite in the form of ultrafine flakes, alternating with and intersecting the austenite, resulting in a smaller austenite grain size (e.g., austenite grain size <3 μm), and the thickness of the martensite flakes is less than 100 nm.

[0083] Table 1 Chemical composition of Examples 1-4 (wt%)

[0084] Table 2 Specific process parameters of Examples 1-4

[0085] Table 3 Mechanical properties of Examples 1-4

[0086] Table 4 Microstructure of the steel of Examples 1-4

[0087] To demonstrate the corrosion resistance of the steel of this application, the corrosion resistance of the steels of Examples 1-4 was measured under five different conditions and compared with 13Cr under the same test conditions. This experiment evaluated the corrosion resistance of the steel of this application in different corrosive environments. The results of the corrosion resistance test are shown in Table 5, and the corresponding test conditions are as follows:

[0088] (180℃ or 200℃) The corrosion conditions of CO2 corrosion rate are as follows:

[0089] 1. Medium (formation water) mg / L: CO3 2- / 0,HCO3 - / 189,OH - / 0,Cl - / 128000,SO4 2- / 430,Ca 2+ / 8310,Mg 2+ / 561,K + / 6620,Na+ / 76500);

[0090] 2. CO2 partial pressure: 4.48MPa, total test pressure: 10MPa;

[0091] 3. Test temperature: 180℃ or 200℃;

[0092] 4. Test time: 720 hours.

[0093] The corrosion conditions for pitting corrosion rate are as follows:

[0094] 1. Test temperature: 22±2℃;

[0095] 2. Medium: 100g reagent grade ferric chloride FeCl3·6H2O dissolved in 900mL IV reagent grade water (mass ratio about 6%);

[0096] 3. Test time: 72 hours;

[0097] 4. Sample size: 50×25×3mm, polished to 2000# sandpaper.

[0098] The corrosion conditions for crevice corrosion rate are as follows:

[0099] 1. The test temperature is 22±2℃;

[0100] 2. Dissolve 100g of reagent-grade ferric chloride (FeCl3·6H2O) in 900mL of Type IV reagent-grade water (approximately 6% by mass).

[0101] 3. Test time: 72 hours;

[0102] 4. Sample size: 50×25×3mm, polished to 2000# sandpaper.

[0103] The corrosion conditions of the H2S stress corrosion test are as follows:

[0104] 1. The test temperature is 22±2℃;

[0105] 2. Dissolve 50 g NaCl, 25 g [23.8 mL] CH3COOH, and 4.1 g CH3COONa in 921 mL IV reagent grade water (approximately 5 wt% sodium chloride, 2.5 wt% glacial acetic acid, and 0.41 wt% sodium acetate by weight);

[0106] 3. Test time: 720 hours;

[0107] 4. Sample size: 50×5×2mm, polished to 2000# sandpaper;

[0108] 5. Four-point bending test, loading force is 80% yield stress.

[0109] From Table 5, it can be seen that the (180°C) CO2 corrosion rate of the high corrosion resistant oil well pipe steel of Examples 1-4 is 0.028 g / m 2 h or less (e.g. 0.0203 to 0.0275 g / m 2 h); (200℃) CO2 corrosion rate 0.1g / m 2 h or less (e.g. 0.078 to 0.099 g / m 2 h); pitting corrosion rate 2.5g / m 2 h or less (e.g. 1.693 to 2.433 g / m 2 h); crevice corrosion rate 5.9g / m 2 h or less (e.g. 3.303 to 5.852 g / m 2 h); all passed the H2S stress corrosion test. Examples 1-4 of this application all exhibited superior corrosion resistance to 13Cr, particularly CO2 corrosion resistance at 200°C. This material far surpasses Super 13Cr, enabling use in more demanding environments, including those at greater well depths. Figure 5 shows the H2S stress corrosion test results for Example 1.

[0110] Table 5 Corrosion test data

[0111] To illustrate the hot working properties of the steel of this application, the edge quality of the hot-rolled steel plates of Examples 1-4 was statistically analyzed, using Example 1 as an example. Figure 6 shows a photograph of the hot-rolled plate of Example 1, showing no cracking at the edge. The steel of this application's examples achieved a yield rate exceeding 90% during actual production.

[0112] The inventors have conducted a lot of in-depth research, and now some of the solutions with poor effects are listed as comparative examples as follows:

[0113] Comparative Example 1

[0114] This comparative example provides a corrosion-resistant oil-well tubular steel and a preparation method thereof. The corrosion-resistant oil-well tubular steel in this comparative example is 13Cr and is prepared using a currently mature 13Cr process. The corrosion-resistant oil-well tubular steel in this comparative example has a composition of 0.03% C, 13% Cr, 5% Ni, 2% Mo, 0.5% Mn, and 0.5% Si. The preparation method involves heating and forging at 1150°C, water cooling, reheating to 860°C, holding for 2 hours, quenching, and tempering at 620°C for 1 hour.

[0115] The microstructure of the steel of this comparative example is martensite (93%) + austenite (7%). The mechanical properties are shown in Table 3 above, and the corrosion resistance results are shown in Table 5 above.

[0116] Comparative Example 2

[0117] This comparative example provides a corrosion-resistant oil well pipe steel and a preparation method thereof. The corrosion-resistant oil well pipe steel of this comparative example has the following composition: C: 0.03%, Cr: 16%, Mo: 1.21%, N: 0.22%, Mn: 2.11%, and Si: 0.5%. The preparation method is the same as that of Example 1.

[0118] The microstructure of the steel of this comparative example is ferrite (15%) + martensite (65%) + austenite (20%). The mechanical properties are shown in Table 3, and the corrosion resistance results are shown in Table 5.

[0119] Comparative Example 3

[0120] This comparative example provides a corrosion-resistant oil well pipe steel and a preparation method thereof. The corrosion-resistant oil well pipe steel in this comparative example has the following composition: C: 0.04%, Cr: 16.5%, Ni: 1.12%, Mo: 1.32%, N: 0.16%, Mn: 2.82%, and Si: 0.5%. The preparation method is the same as that in Example 1.

[0121] The microstructure of the steel of this comparative example is ferrite (20%) + martensite (60%) + austenite (20%). The mechanical properties are shown in Table 3, and the corrosion resistance results are shown in Table 5.

[0122] Comparing the Examples and Comparative Examples, it can be seen that the high-corrosion-resistant oil well pipe steel of the present application precisely controls the mass percentages of Cr, Ni, Mn, Mo, and N in the steel, and, combined with a controlled rolling and controlled cooling hot deformation process, can obtain a mixed structure of ferrite + austenite + martensite, significantly improving the corrosion resistance and toughness of the oil well pipe steel. The raw material cost is comparable to or slightly lower than that of the super 13Cr martensitic stainless steel of the prior art, and the hot working performance is excellent. The corrosion resistance of the high-corrosion-resistant oil well pipe steel of the present application is superior to that of the super 13Cr martensitic stainless steel. Therefore, the steel of the present application has a low overall cost, is economical, and is practical.

[0123] The above is only a preferred specific implementation method of the present application, but the scope of protection of the present application is not limited thereto. Any changes or replacements that can be easily thought of by any technician familiar with this technical field within the technical scope disclosed in this application should be covered by the scope of protection of the present application.

Claims

1. A highly corrosion-resistant oil well pipe steel, characterized in that: The components of the high-corrosion-resistant oil well pipe steel include, by mass percentage, C: ≤0.03%, Cr: 17.3% to 18.4%, Mo: 0.5% to 2.0%, Ni: 1.0% to 2.8%, Mn: 1.0% to 3.5%, Si: 0.1% to 0.5%, N: 0.1% to 0.25%, P: ≤0.03%, S: ≤0.01%, and the balance is Fe and unavoidable impurities.

2. The high corrosion resistant oil well pipe steel according to claim 1, characterized in that: Among the components of the high corrosion-resistant oil well pipe steel, Cr+3.3Mo+16N≥26.

3. The high corrosion resistant oil well pipe steel according to claim 1, characterized in that: Among the components of the high corrosion-resistant oil well pipe steel, 60Ni+17Mn-12Mo-800N≤0.

4. The high corrosion resistant oil well pipe steel according to claim 1, characterized in that: The composition of the high-corrosion-resistant oil well pipe steel may be, by mass percentage, C: 0.01% to 0.03%, Cr: 17.4% to 18.4%, Mo: 1.0% to 2.0%, Ni: 1.0% to 2.7%, Mn: 1.4% to 3.2%, Si: 0.1% to 0.5%, N: 0.13% to 0.25%, P: ≤0.03%, S: ≤0.01%, with the balance being Fe and unavoidable impurities.

5. The high corrosion resistant oil well pipe steel according to claim 1, characterized in that: The microstructure of the high corrosion-resistant oil well pipe steel is a mixed structure of ferrite+austenite+martensite.

6. The high corrosion resistant oil well pipe steel according to claim 5, characterized in that: In the microstructure of the high corrosion-resistant oil well pipe steel, the volume percentage of austenite is 20% to 40%, and the volume percentage of martensite is 10% to 40%.

7. The high corrosion resistant oil well pipe steel according to claim 5, characterized in that: In the microstructure of the high corrosion-resistant oil well pipe steel, the austenite grain size is less than 3 μm.

8. A method for preparing highly corrosion-resistant oil well pipe steel, characterized in that: For preparing the high corrosion-resistant oil well pipe steel according to any one of claims 1 to 7, comprising: Step 1: Melt the metal raw materials into molten steel; Step 2: smelting the molten steel into continuous casting billets or ingots by continuous casting or mold casting; Step 3: Forging the continuous casting billet or ingot into a forging billet; Step 4: Roll the forged billet into a tube billet, and obtain high corrosion-resistant oil well pipe steel by controlling the hot rolling and cooling process parameters.

9. The preparation method according to claim 8, characterized in that In step 3, the forging temperature is 1150-1250°C.

10. The preparation method according to any one of claims 7 to 9, characterized in that: In step 4, controlling the hot rolling and cooling process parameters includes: controlling the starting rolling temperature to be above 1050° C., the final rolling temperature to be above 950° C., the deformation of the first rolling pass to be no more than 30%, and the deformation of the final rolling pass to be no more than 50%.