Cold rolled steel sheet and method for manufacturing same

MYPI2025003508A0Undetermined Publication Date: 2024-06-20POHANG IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025003508
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-12-20
Filing Date
2023-12-15
Publication Date
2024-06-20

AI Technical Summary

Technical Problem

Current methods for manufacturing ultra-high strength cold-rolled steel sheets for automotive reinforcement and battery protection face challenges with shape defects due to water cooling and rapid cooling after annealing, leading to inadequate strength, bendability, and weldability.

Method used

A cold-rolled steel sheet with a specific alloy composition (C: 0.19-0.26%, Si: 0.03-0.50%, Mn: 1.4-2.0%, Cr: 0.03-0.30%, Mo: 0.03-0.30%, B: 0.0005-0.005%, P: 0.03% or less, S: 0.003% or less, N: 0.01% or less, Al: 0.01-0.10%, Nb: 0.01-0.05%, Ti: 0.005-0.05%) and controlled manufacturing conditions, including continuous annealing and over-aging treatment, to achieve a microstructure with a high tensile strength of 1470 MPa or more, excellent hole expandability, and improved weldability.

Benefits of technology

The solution results in cold-rolled steel sheets with enhanced mechanical properties, including yield strength of 1150-1400 MPa, tensile strength of 1470-1650 MPa, yield ratio of 0.75-0.96, elongation of 4-11%, and superior bending and hole expandability, while minimizing surface roughness and crack formation during resistance spot welding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025003508_DRAWING_001
    Figure PI2025003508_DRAWING_001
  • Figure PI2025003508_DRAWING_002
    Figure PI2025003508_DRAWING_002
Patent Text Reader

Abstract

The present invention relates to a cold rolled steel sheet and a method for manufacturing same and, more specifically, to a cold rolled steel sheet and a method for manufacturing same, the cold rolled steel sheet being suitable for use as a steel material for automobile reinforcements such as bumper beams, sill side beams, etc. or a steel material for the protection of electric vehicle battery cases, such as side frames, cross members, etc. [FIGURE 2]
Need to check novelty before this filing date? Find Prior Art

Description

Cold rolled steel sheet and its manufacturing method

[0001] The present invention relates to a cold-rolled steel sheet and a method for manufacturing the same, and more particularly, to a cold-rolled steel sheet suitable for use as a steel material for reinforcing automobile parts such as bumper beams and sill side beams, or a steel material for protecting an electric vehicle battery case such as a side frame or cross member, and a method for manufacturing the same.

[0002]

[0003] Steels primarily used in reinforcing parts related to the crashworthiness of automobile occupants require the development of ultra-high-strength steels with excellent processing properties, particularly bending properties, when manufactured using cold forming techniques. To this end, active research is being conducted on ultra-high-strength steels with a tensile strength of 1470 MPa or higher, utilizing a single martensitic phase, and their manufacturing methods. Recently, Hot Press Forming (HPF) has been developed, which forms materials at high temperatures for easy forming, followed by water cooling between the die and the material to achieve the required strength. While HPF is widely used in parts manufacturing due to its ability to achieve high strength per thickness, its application is hindered by excessive facility investment and increased process costs, necessitating the development of materials suitable for cold stamping. Therefore, the development of ultra-high-strength cold-rolled steel sheets suitable for cold stamping, with high strength and yield ratios for ensuring crashworthiness, and excellent bending properties is needed.

[0004]

[0005] A representative prior art of this method is Patent Document 1. Patent Document 1 includes C: 0.25 to 0.4%, Si: 1.0% or less, Mn: 1.5 to 2.5%, P: 0.02% or less, S: 0.003% or less, Al: 0.01 to 0.1%, N: 0.005% or less, B: 0.0005 to 0.005%, and also Ti: 0.005 to 0.1%, Nb: 0.005 to 0.1%, a total of 0.005 to 0.1%, and relates to manufacturing by heating and maintaining in a temperature range of 900°C or less but not less than the Ae3 transformation point using a martensite single-phase structure, then rapidly cooling to 200°C or less at an average cooling rate of 300°C / s or more, and then tempering at 250°C or less. However, in the case of patent document 1, there is a problem that the shape (flatness) is inferior due to water cooling, resulting in defects during molding.

[0006]

[0007] Patent Document 2 relates to a sheet steel sheet having a high strength composition including C: 0.05% or more and 0.35% or less, Si: 0.01% or more and 2.0% or less, Mn: 0.8% or more and 3.0% or less, P: 0.05% or less, S: 0.005% or less, Al: 0.005% or more and 0.10% or less, and N: 0.0060% or less, and having a ferrite area ratio of 0% or more and 90% or less, a bainite area ratio of 5% or less (including 0%), a martensite and tempered martensite area ratio of 10% or more (including 100%), and a retained austenite area ratio of 2.0% or less (including 0%), and having a yield strength standard deviation in the width direction of 30 MPa or less, and a maximum bending amount of the sheet steel sheet when sheared at a length of 1 m of 10 mm or less. However, even in the case of patent document 2, there is a problem that shape defects occur due to rapid cooling after annealing.

[0008]

[0009] Therefore, in order to solve the above-mentioned problems, it is necessary to develop ultra-high strength cold-rolled steel sheets and plated steel sheets having a tensile strength of 1470 MPa or more and excellent hole expandability, bending properties, and weldability.

[0010]

[0011] [Prior Art Literature]

[0012] (Patent Document 1) Japanese Patent Application Laid-Open No. 2010-248565

[0013] (Patent Document 2) Japanese Patent Application Laid-Open No. 2020-019992

[0014]

[0015] One aspect of the present invention is to provide a cold rolled steel sheet and a method for manufacturing the same.

[0016] A preferred aspect of the present invention is to provide an ultra-high strength cold-rolled steel sheet having a tensile strength of 1470 MPa or more and excellent hole expandability, bending properties and weldability, and a method for manufacturing the same.

[0017]

[0018] One embodiment of the present invention comprises, in wt%, carbon (C): 0.19 to 0.26%, silicon (Si): 0.03 to 0.50%, manganese (Mn): 1.4 to 2.0%, chromium (Cr): 0.03 to 0.30%, molybdenum (Mo): 0.03 to 0.30%, boron (B): 0.0005 to 0.005%, phosphorus (P): 0.03% or less (excluding 0%), sulfur (S): 0.003% or less (excluding 0%), nitrogen (N): 0.01% or less (excluding 0%), aluminum (Al): 0.01 to 0.10%, niobium (Nb): 0.01 to 0.05%, titanium (Ti): 0.005 to 0.05%, the remainder being Fe and other unavoidable impurities, and satisfying the following relational expressions 1 to 3: A cold-rolled steel sheet is provided, comprising: a central portion; and a surface portion formed on the outer side of the central portion in the thickness direction; wherein the microstructure of the central portion includes, in area %, a sum of at least one of ferrite and bainite: 5% or less (including 0%), at least one of residual martensite and tempered martensite; and the microstructure of the surface portion includes, in area %, a sum of at least one of ferrite and bainite: 11% or less (excluding 0%), at least one of residual martensite and tempered martensite, and the average size of carbides is 260 nm or less.

[0019] [Relationship 1] 0.31 ≤ X = C + Mn / 20 + Si / 30 + 2P + 4S ≤ 0.40

[0020] [Relationship 2] 125 ≤ Y = 48.8 + 49logC + 35.1Mn + 25.9Si + 14.5Ni + 9.6Cu + 76.5Cr + 105.9Mo + 1325Nb + 10000B ≤ 190

[0021] [Relationship 3] 410 ≤ Y / X ≤ 620

[0022] (However, in the above equations 1 to 3, the content of each alloy element is in weight%.)

[0023]

[0024] The above cold rolled steel sheet may have a surface roughness (Rsk) of -0.7 to -0.1.

[0025]

[0026] The above cold rolled steel sheet may have a yield strength of 1150 to 1400 MPa.

[0027]

[0028] The above cold rolled steel sheet may have a tensile strength of 1470 to 1650 MPa.

[0029]

[0030] The above cold rolled steel sheet may have a yield ratio of 0.75 to 0.96.

[0031]

[0032] The above cold rolled steel sheet may have an elongation of 4 to 11%.

[0033]

[0034] The above cold rolled steel sheet may have a bending workability (R / t) of 2 to 4.

[0035]

[0036] The above cold rolled steel sheet can have a hole expandability of 35 to 70%.

[0037]

[0038] The above cold rolled steel sheet may have a (tensile strength × hole expandability) / (bending workability (R / t)) of 15,000 to 35,000 MPa%.

[0039]

[0040] The above cold rolled steel sheet may have a hardness of 440 to 570 Hv at the spot weld after resistance spot welding.

[0041]

[0042] The above cold-rolled steel sheet may have a crack length of 10 ㎛ or less (including 0 ㎛) at the minimum nugget diameter (3√t, t: thickness of steel) of the spot weld after resistance spot welding.

[0043]

[0044] The above cold rolled steel sheet can have an electrogalvanized layer formed on at least one surface.

[0045]

[0046] The above surface layer may be a region of up to 20㎛ in the thickness direction from the surface of the steel material.

[0047]

[0048] Another embodiment of the present invention comprises, in wt%, carbon (C): 0.19 to 0.26%, silicon (Si): 0.03 to 0.50%, manganese (Mn): 1.4 to 2.0%, chromium (Cr): 0.03 to 0.30%, molybdenum (Mo): 0.03 to 0.30%, boron (B): 0.0005 to 0.005%, phosphorus (P): 0.03% or less (excluding 0%), sulfur (S): 0.003% or less (excluding 0%), nitrogen (N): 0.01% or less (excluding 0%), aluminum (Al): 0.01 to 0.10%, niobium (Nb): 0.01 to 0.05%, titanium (Ti): 0.005 to 0.05%, the remainder being Fe and other unavoidable impurities, and satisfying the following relationships 1 to 3: A step of heating a slab at 1100 to 1300°C; A step of finishing hot rolling the heated slab at Ar3 to Ar3+120°C to obtain a hot-rolled steel sheet; A step of coiling the hot-rolled steel sheet at Ms to 600°C; A step of cold rolling the coiled hot-rolled steel sheet at a cold reduction ratio of 35 to 70% to obtain a cold-rolled steel sheet; A step of continuously annealing the cold-rolled steel sheet at Ac3+20°C to Ac3+80°C; A step of first cooling the continuously annealed cold-rolled steel sheet to a first cooling end temperature (T1) of 670 to 750°C at an average cooling rate of 1 to 6°C / s; A step of second cooling the first-cooled cold-rolled steel sheet to a second cooling end temperature (T2) of 50 to 200°C at an average cooling rate of 40 to 110°C / s; The present invention provides a method for manufacturing a cold rolled steel sheet, comprising: a step of reheating the second-cooled cold rolled steel sheet to an overaging treatment temperature (H) of 100 to 250°C and then performing an overaging treatment for 5 to 12 minutes; a step of subjecting the overaging cold rolled steel sheet to temper rolling with a rolling force of 500 to 1,000 tons; and a step of tension leveling the temper rolled cold rolled steel sheet to an elongation of 0.05 to 0.65%; and, during the second cooling, the following relationships 4 and 5 are satisfied, and the first cooling end temperature (T1) - the second cooling end temperature (T2) is controlled to be 650°C or less, and the overaging treatment temperature (H) - the second cooling end temperature (T2) is controlled to be 30°C or more.

[0049] [Relationship 1] 0.31 ≤ X = C + Mn / 20 + Si / 30 + 2P + 4S ≤ 0.40

[0050] [Relationship 2] 125 ≤ Y = 48.8 + 49logC + 35.1Mn + 25.9Si + 14.5Ni + 9.6Cu + 76.5Cr + 105.9Mo + 1325Nb + 10000B ≤ 190

[0051] [Relationship 3] 410 ≤ Y / X ≤ 620

[0052] [Relationship 4] F = 1 - exp{-(1.10×10 -2 ×△T)} ≥ 0.9

[0053] [Relationship 5] 940 ≤ F×Z ≤ 1200

[0054] (However, in the above equations 1 to 3, the content of each alloy element is weight%, △T is Ms - secondary cooling end temperature (T2), and Z is 3500C + 150Mn + 50(Si+Cr+Mo) + 1000Nb.)

[0055]

[0056] The above continuous annealing can be performed for 30 to 230 seconds.

[0057]

[0058] After the above tension leveling, a step of forming an electrogalvanized layer on at least one surface of the cold-rolled steel sheet may be additionally included.

[0059]

[0060] According to one aspect of the present invention, a cold rolled steel sheet and a method for manufacturing the same can be provided.

[0061] According to a preferred aspect of the present invention, an ultra-high strength cold-rolled steel sheet having a tensile strength of 1470 MPa or more and excellent hole expandability, bending properties and weldability, and a method for manufacturing the same can be provided.

[0062]

[0063] Figure 1 is a schematic diagram for evaluating whether cracks occur at the minimum nugget diameter (3√t) of a resistance spot weld.

[0064] Figure 2 is a microstructure photograph of the surface of Invention Example 1 according to one embodiment of the present invention observed using a scanning electron microscope (SEM).

[0065] Figure 3 is a microstructure photograph of the surface of Comparative Example 5 according to one embodiment of the present invention observed using a scanning electron microscope (SEM).

[0066] Fig. 4 is a microstructure photograph of a cross-section of a welded portion of Invention Example 4 according to one embodiment of the present invention observed using an optical microscope.

[0067] Figure 5 is a microstructure photograph of a weld section of Comparative Example 1 according to one embodiment of the present invention observed with an optical microscope.

[0068]

[0069] The terminology used herein is for the purpose of describing specific embodiments only and is not intended to limit the present invention. As used herein, the singular forms "a," "an," and "the" include plural forms as well, unless the context clearly dictates otherwise. The word "comprising," as used herein, specifies a particular feature, region, integer, step, operation, element, and / or component, but does not exclude the presence or addition of other features, regions, integers, steps, operations, elements, components, and / or groups.

[0070] Although not defined otherwise, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by those of ordinary skill in the technical field to which the present invention pertains. Terms defined in commonly used dictionaries are further interpreted to have meanings consistent with the relevant technical literature and the present disclosure, and are not to be construed as ideal or overly formal unless otherwise defined.

[0071]

[0072] The inventors of the present invention have recognized that by controlling the alloy composition and manufacturing conditions, microstructure and carbides can be appropriately controlled, and in particular, by controlling the surface roughness, an ultra-high strength cold-rolled steel sheet having a tensile strength of 1470 MPa or more and excellent hole expandability, bending properties, and weldability can be manufactured, and have completed the present invention.

[0073]

[0074] Hereinafter, a cold-rolled steel sheet according to one embodiment of the present invention will be described. First, the alloy composition of the present invention will be described. The alloy composition described below refers to weight percent unless otherwise specified.

[0075]

[0076] Carbon (C): 0.19~0.26%

[0077] C is an interstitial solid solution element and is the most effective and important element for improving the strength of steel. In addition, it is an element that must be added to secure the strength of martensitic steel. If the C content is less than 0.19%, it may be difficult to obtain the yield ratio and tensile strength targeted in the present invention. If the C content exceeds 0.26%, martensite may be excessively formed during cooling due to a rapid increase in hardenability, which may rapidly increase the strength and deteriorate the elongation. In addition, weldability may be deteriorated. Therefore, the C content is preferably in the range of 0.19 to 0.26%. In order to further enhance the above-mentioned effect and prevent the occurrence of problems, the lower limit of the C content is more preferably 0.20%, and the upper limit of the C content is more preferably 0.25%.

[0078]

[0079] Silicon (Si): 0.03~0.50%

[0080] Si suppresses the formation of carbides and controls the size of carbides during the reheating and overaging treatment steps performed after continuous annealing and cooling. If the Si content is less than 0.03%, it may be difficult to sufficiently obtain the above-described effect. If the Si content exceeds 0.50%, there is a concern that ferrite may be formed after continuous annealing and cooling, weakening the strength of the steel. In addition, Si is an element that increases resistivity, which may result in poor resistance spot weldability. Therefore, the Si content is preferably in the range of 0.03 to 0.50%. In order to further enhance the above-described effect and prevent the occurrence of problems, the lower limit of the Si content is more preferably 0.05%, the upper limit of the Si content is more preferably 0.40%, and even more preferably 0.30%.

[0081]

[0082] Manganese (Mn): 1.4~2.0%

[0083] Mn is an element added to secure strength. If the Mn content is less than 1.4%, the hardenability is low, so if the cooling rate is not sufficiently fast during cooling after continuous annealing, martensite is not formed, making it difficult to secure the strength targeted by the present invention. If the Mn content exceeds 2.0%, the Ms temperature decreases during cooling after continuous annealing, which lowers the final cooling temperature and thus deteriorates the shape of the steel plate. In addition, it is difficult to secure the initial martensite structure. In addition, during steelmaking / continuous casting, a Mn-based segregation zone occurs in the longitudinal direction of the slab, which deteriorates the bendability. In other words, manganese segregates in the thickness direction, forming a manganese band within the slab, which causes cracks to occur during continuous casting and increases the occurrence of defects during the rolling process. Therefore, the Mn content is preferably in the range of 1.4 to 2.0%. In order to further enhance the aforementioned effects and prevent problems from occurring, it is more preferable that the lower limit of the Mn content be 1.5%, and it is more preferable that the upper limit of the Mn content be 1.9%.

[0084]

[0085] Chromium (Cr): 0.03~0.30%

[0086] Cr is an element that facilitates securing a low-temperature transformed structure by suppressing ferrite transformation. In addition, when utilizing a continuous annealing process with slow cooling as in the present invention, there is an advantage of suppressing ferrite formation. When the Cr content is less than 0.03%, hardenability is low, so if the cooling rate is not sufficiently fast during cooling after continuous annealing, martensite is not formed, making it difficult to secure the strength targeted by the present invention. When the Cr content exceeds 0.30%, delayed fracture resistance may deteriorate, carbides such as CrC may be formed, which may impair hole expandability and bending workability, and cost may increase due to excessive alloy input. Therefore, the Cr content is preferably in the range of 0.03 to 0.30%. In order to further enhance the above-mentioned effect and prevent problems from occurring, the lower limit of the Cr content is more preferably 0.03%, and the upper limit of the Cr content is more preferably 0.25%.

[0087]

[0088] Molybdenum (Mo): 0.03~0.30%

[0089] Mo is an element that has the effect of improving the hardenability of steel, the effect of generating Mo-based fine carbides that become hydrogen trap sites, and the effect of improving delayed fracture resistance by refining martensite. When the content of Mo is less than 0.03%, it may be difficult to sufficiently obtain the above-mentioned effect. When the content of Mo exceeds 0.30%, the above-mentioned effect does not increase significantly compared to the increase in cost due to the addition of expensive alloying elements. Therefore, the content of Mo is preferably in the range of 0.03 to 0.30%. In order to further enhance the above-mentioned effect and prevent the occurrence of problems, the lower limit of the Mo content is more preferably 0.05%, and the upper limit of the Mo content is more preferably 0.25%.

[0090]

[0091] Boron (B): 0.0005~0.005%

[0092] B is an element that suppresses ferrite formation, and therefore, the present invention has the advantage of suppressing the formation of ferrite during cooling after continuous annealing. If the content of B is less than 0.0005%, the hardenability effect is completely absent, so not only cannot the strength targeted by the present invention be secured, but also excessive ferrite is formed on the surface, resulting in poor bending workability. If the content of B exceeds 0.005%, ductility may be significantly reduced. Therefore, the content of B is preferably in the range of 0.0005 to 0.005%. In order to further enhance the above-mentioned effect and prevent problems from occurring, the lower limit of the B content is more preferably 0.0007%, and the upper limit of the B content is more preferably 0.004%.

[0093]

[0094] Phosphorus (P): 0.03% or less (excluding 0%)

[0095] P is an impurity element contained in steel, and when the content of P exceeds 0.03%, weldability deteriorates and there is a risk of steel becoming brittle. Meanwhile, although the amount of P added to steel is advantageous when it is small, 0% is excluded in consideration of cases where it is unavoidably included during the manufacturing process. Therefore, the content of P is preferably 0.03% or less (excluding 0%). In order to further enhance the aforementioned effect and prevent problems from occurring, the content of P is more preferably 0.025% or less.

[0096]

[0097] Sulfur (S): 0.003% or less (excluding 0%)

[0098] S, like P, is an impurity element contained in steel. If the content of S exceeds 0.003%, ductility and weldability may be impaired, and a large amount of MnS precipitates may be formed, resulting in poor bending workability. Meanwhile, although the amount of S added to steel is advantageous when it is small, 0% is excluded in consideration of cases where it is inevitably included in the manufacturing process. Therefore, the content of P is preferably 0.003% (excluding 0%) or less. In order to further enhance the aforementioned effect and prevent problems, the content of S is more preferably 0.0025% or less, and even more preferably 0.0020% or less.

[0099]

[0100]

[0101] Nitrogen (N): 0.01% or less (excluding 0%)

[0102] N is an impurity element, and when its content exceeds 0.01%, it significantly increases the risk of cracks occurring during continuous casting due to AlN formation, etc. The above N content excludes 0% in consideration of cases where it is inevitably included in the manufacturing process. Therefore, it is preferable that the N content be in the range of 0.01% or less (excluding 0%). In order to further enhance the above-mentioned effect and prevent the occurrence of problems, the N content is more preferably 0.008% or less, and even more preferably 0.006% or less.

[0103]

[0104] Aluminum (Al): 0.01~0.10%

[0105] Al can be added to remove oxygen from molten steel. If the Al content is less than 0.01%, deoxidation will not be sufficient, thereby damaging the cleanliness of the steel. If the Al content exceeds 0.10%, not only will the castability of the slab deteriorate, but the temperature required for single-phase heating during continuous annealing will also increase, which may cause production and equipment problems. Therefore, the Al content is preferably in the range of 0.01 to 0.10%. In order to further enhance the aforementioned effects and prevent problems from occurring, the upper limit of the Al content is more preferably 0.075%.

[0106]

[0107] Niobium (Nb): 0.01~0.05%

[0108] Niobium is an element that segregates at austenite grain boundaries, suppresses the coarsening of austenite grains during the continuous annealing process, and contributes to the improvement of strength by forming fine precipitates. When the content of Nb is less than 0.01%, the austenite grain refinement and precipitation strengthening effects cannot be sufficiently obtained. When the content of Nb exceeds 0.05%, the precipitation of coarse carbonitrides increases, and there is a concern that the strength and elongation may decrease due to the reduction in the carbon content in the steel. In addition, there is a problem that the workability of the base material deteriorates and the manufacturing cost increases. Therefore, the content of Nb is preferably in the range of 0.01 to 0.05%. In order to further enhance the above-mentioned effect and prevent the occurrence of problems, the lower limit of the Nb content is more preferably 0.015%, and the upper limit of the Nb content is more preferably 0.045%.

[0109]

[0110] Titanium (Ti): 0.005~0.05%

[0111] Ti is a nitride-forming element that scavenges dissolved nitrogen by precipitating it as TiN. When the Ti content is less than 0.005%, it is difficult to obtain the effect of increasing strength, and the effect of scavenging dissolved nitrogen is reduced, so that cracks may occur during continuous casting due to the formation of a large amount of AlN. When the Ti content exceeds 0.05%, the strength of martensite may decrease due to the precipitation of additional carbides in addition to the removal of dissolved nitrogen, and hole expandability and bending workability may be impaired due to the formation of excessive carbon and nitrides such as TiC and TiN. Therefore, the Ti content is preferably in the range of 0.005 to 0.05%. In order to further enhance the above-mentioned effect and prevent the occurrence of problems, the lower limit of the Ti content is more preferably 0.01%, and the upper limit of the Ti content is more preferably 0.04%.

[0112]

[0113] The remaining component is iron (Fe). However, during the normal manufacturing process, unintended impurities from raw materials or the surrounding environment may inevitably be mixed in, and thus cannot be excluded. Since these impurities are readily apparent to anyone skilled in the normal manufacturing process, their full details are not specifically mentioned in this specification.

[0114]

[0115] It is preferable that the cold-rolled steel sheet of the present invention satisfies the above-described alloy composition and the following relationship equations 1 to 3.

[0116]

[0117] [Relationship 1] 0.31 ≤ X = C + Mn / 20 + Si / 30 + 2P + 4S ≤ 0.40

[0118]

[0119] The above equation 1 is a component equation closely related to the hardness of the weld. When the value of X is less than 0.31, it is difficult to sufficiently secure the hardness and strength of the weld. When the value of X exceeds 0.40, the hardness of the weld becomes excessively high, which increases the risk of brittle fracture, and thus the crash stability may be deteriorated. Therefore, the value of X is preferably in the range of 0.31 to 0.40. In order to further enhance the above-mentioned effect and prevent the occurrence of problems, the lower limit of the X value is more preferably 0.32, and the upper limit of the X value is more preferably 0.39.

[0120]

[0121] [Relationship 2] 125 ≤ Y = 48.8 + 49logC + 35.1Mn + 25.9Si + 14.5Ni + 9.6Cu + 76.5Cr + 105.9Mo + 1325Nb + 10000B ≤ 190

[0122]

[0123] The above equation 2 is a component relationship related to hardenability for securing the microstructure and strength targeted by the present invention. When the value of Y is less than 125, the hardenability is insufficient, making it difficult to obtain the microstructure targeted by the present invention and securing sufficient strength. When the value of Y exceeds 190, not only does the manufacturing cost increase, but the strength becomes excessively high, which causes a problem of reduced elongation. Therefore, the value of Y is preferably in the range of 125 to 190. In order to further enhance the above-mentioned effect and prevent the occurrence of problems, the lower limit of the Y value is more preferably 130, and the upper limit of the Y value is more preferably 185.

[0124]

[0125] [Relationship 3] 410 ≤ Y / X ≤ 620

[0126]

[0127] The above equation 3 is a component relationship for securing an appropriate level of weld hardness and hardenability. When the value of Y / X is less than 410, Ceq is satisfied, but it may be difficult to secure strength because the target microstructure cannot be obtained due to insufficient hardenability. When the value of Y / X exceeds 620, hardenability is sufficiently secured, but it may be difficult to secure weld strength due to low Ceq. Therefore, the value of Y / X is preferably in the range of 410 to 620. In order to further enhance the above-mentioned effect and prevent the occurrence of problems, the lower limit of the Y / X value is more preferably 420, and the upper limit of the Y / X value is more preferably 600.

[0128]

[0129] The cold rolled steel sheet according to the present invention can be divided into a central portion in terms of microstructure; and a surface portion formed on the outer side of the central portion in the thickness direction.

[0130]

[0131] The above-mentioned central microstructure preferably includes, in area %, the sum of at least one type of ferrite and bainite: 5% or less (including 0%), and at least one type of residual martensite and tempered martensite, and the surface microstructure preferably includes, in area %, the sum of at least one type of ferrite and bainite: 11% or less (excluding 0%), and at least one type of residual martensite and tempered martensite.

[0132]

[0133] It is preferable that the main phase of the above-mentioned central microstructure includes at least one of martensite and tempered martensite. The martensite and tempered martensite are very advantageous structures for securing the strength, hole expandability, bending properties, and weldability targeted by the present invention. However, at least one of ferrite and bainite may inevitably be formed during the manufacturing process, and if the total fraction of at least one of the ferrite and bainite exceeds 5%, it may be difficult to secure the properties sought by the present invention. It is more preferable that the total fraction of at least one of the ferrite and bainite is 3% or less.

[0134]

[0135] It is preferable that the main phase of the surface microstructure includes at least one of martensite and tempered martensite. In addition, it is preferable that the total fraction of at least one of ferrite and bainite is 11% or less (excluding 0%). Since the ferrite and bainite are softer than martensite and tempered martensite, the bending properties can be further improved by forming an appropriate level of ferrite and bainite in the surface. If the total fraction of at least one of ferrite and bainite exceeds 11%, it is difficult to secure sufficient strength, and the bending properties may be deteriorated. It is more preferable that the total fraction of at least one of ferrite and bainite is 10% or less. In the present invention, there is no particular limitation on the lower limit of the total fraction of at least one of ferrite and bainite, but as an example, it may be 1%.

[0136]

[0137] Meanwhile, the surface layer may have a depth that varies depending on the thickness of the steel material, and in one embodiment, may be a region of up to 20 μm in the thickness direction from the surface of the steel material.

[0138]

[0139] The cold rolled steel sheet of the present invention preferably has an average size of carbides of 260 nm or less. If the average size of the carbides exceeds 260 nm, the bending properties may be deteriorated. The average size of the carbides is more preferably 250 nm or less. In the present invention, since a smaller average size of the carbides is advantageous, there is no particular limitation on the lower limit thereof. However, the lower limit of the average size of the carbides may be, for example, 10 nm. Meanwhile, the carbides may be, for example, at least one of a carbide containing Fe and Mn, a carbide containing Mn and Cr, and a carbide containing Fe, Mn, Cr, and Mo.

[0140]

[0141] The cold-rolled steel sheet of the present invention may have a surface roughness (Rsk) of -0.7 to -0.1. The surface roughness (Rsk (Skewness)) is one of several factors of surface roughness related to the asymmetry of sharp protrusions. The closer the value of the surface roughness (Rsk) is to 0 or to a positive value, the more advantageous it is for securing bending characteristics. As the negative value of the surface roughness (Rsk) increases, the deeper the valley on the flat surface, which causes stress concentration in this area, increasing the susceptibility to crack generation, resulting in inferior bending characteristics. When the value of the surface roughness (Rsk) is less than -0.7, the bending characteristics may be inferior. When the value of the surface roughness (Rsk) exceeds -0.1, it is advantageous for securing bending characteristics, but manufacturing costs increase significantly because the surface of the roll must be processed. It is more preferable that the lower limit of the value of the surface roughness (Rsk) is -0.65. It is more preferable that the upper limit of the value of the above surface roughness (Rsk) is -0.15.

[0142]

[0143] As described above, the cold rolled steel sheet of the present invention provided may have a yield strength of 1150 to 1400 MPa, a tensile strength of 1470 to 1650 MPa, a yield ratio of 0.75 to 0.96, an elongation of 4 to 11%, a bending workability (R / t): 2 to 4, a hole expandability of 35 to 70%, (tensile strength × hole expandability) / (bending workability (R / t)) of 15000 to 35000 MPa%, a spot weld hardness of 440 to 570 Hv, and a crack length at a minimum nugget diameter (3√t, t: thickness of steel) of a resistance spot weld: 10 μm or less (including 0 μm). The crack length of 0 μm means that no crack occurs. Meanwhile, the present invention does not specifically limit the type of the welded portion, but as an example, as shown in Fig. 1, it may be formed by resistance spot welding by applying a welding current in the range of 5.0 to 6.0 kA under the conditions of Force: 3.8 KN, Welding time: 20 cycles, Holding time: 10 cycles, with a 1.5t gap between two materials of 30 mm x 100 mm size.

[0144]

[0145] The thickness of the cold-rolled steel sheet of the present invention may be 0.6 to 2.2 mm. The lower limit of the thickness of the cold-rolled steel sheet is more preferably 0.7 mm, and even more preferably 0.8 mm. The upper limit of the thickness of the cold-rolled steel sheet is more preferably 2.1 mm, and even more preferably 2.0 mm.

[0146]

[0147] The cold-rolled steel sheet of the present invention may have a plating layer formed on at least one surface. The present invention does not specifically limit the type of plating layer, and any type of plating layer commonly used in the relevant technical field may be formed. However, as an example, the plating layer may be an electrogalvanized layer. Alternatively, as another example, the plating layer may be a hot-dip galvanized layer or an alloyed hot-dip galvanized layer.

[0148]

[0149] Hereinafter, a method for manufacturing a cold-rolled steel sheet according to one embodiment of the present invention will be described.

[0150]

[0151] First, a slab satisfying the aforementioned alloy composition and equations 1 to 3 is heated at 1100 to 1300°C. The slab heating process is performed to smoothly perform the subsequent hot rolling process and to sufficiently obtain the target physical properties of the steel sheet. If the slab heating temperature is lower than 1100°C, a problem occurs in which the hot rolling load increases rapidly. If the slab heating temperature exceeds 1300°C, the amount of surface scale increases, resulting in a decrease in the material yield. The lower limit of the slab heating temperature is more preferably 1110°C, more preferably 1120°C, and most preferably 1130°C. The upper limit of the slab heating temperature is more preferably 1290°C, more preferably 1280°C, and most preferably 1270°C.

[0152]

[0153] Thereafter, the heated slab is subjected to a finish hot rolling at Ar3 to Ar3+120℃ to obtain a hot-rolled steel sheet. When the finish hot rolling temperature is lower than Ar3, a dual-phase region of ferrite + austenite or a ferrite region is rolled, resulting in a mixed grain structure, and sheet breakage may occur due to variations in hot rolling load. When the finish hot rolling temperature exceeds Ar3+120℃, a large amount of surface scale may occur, resulting in poor surface quality. The lower limit of the finish hot rolling temperature is more preferably Ar3+10℃, more preferably Ar3+20℃, and most preferably Ar3+30℃. The upper limit of the finish hot rolling temperature is more preferably Ar3+110℃, more preferably Ar3+100℃, and most preferably Ar3+90℃. Meanwhile, the above Ar3 refers to the temperature at which austenite begins to transform into ferrite during cooling, and can be obtained through the following equation 1.

[0154]

[0155] [Formula 1] Ar3(℃) = 910 - 203√C + 44.7Si + 31.5Mo

[0156]

[0157] Thereafter, the hot-rolled steel sheet is coiled at Ms~600℃. If the coiling temperature exceeds 600℃, internal oxidation may occur on the surface of the steel sheet, causing the microstructure formed in the surface layer to become non-uniform, which may result in poor bending properties. Meanwhile, it is preferable to control the coiling temperature low in order to form the microstructure of the hot-rolled steel sheet as a single-phase structure rather than a composite structure as much as possible, thereby ensuring material uniformity across the entire length and width. However, if the coiling temperature is lower than Ms, the strength of the hot-rolled steel sheet may become excessively high, which may increase the rolling load during the cold rolling process, which is a subsequent process, making actual production impossible. It is more preferable that the lower limit of the coiling temperature be Ms+50℃. It is more preferable that the upper limit of the coiling temperature be 550℃. The Ms refers to the temperature at which austenite begins to transform into martensite upon cooling, and can be obtained through Equation 2 below.

[0158]

[0159] [Equation 2] Ms(℃) = 539 - 423C - 30.4Mn - 7.5Si + 30Al - 17.7Ni - 12.1Cr - 7.5Mo

[0160]

[0161] Meanwhile, after the above-described coiling, cooling can be performed through water cooling. In addition, after the above-described cooling, a pickling process can be performed to remove the oxide layer formed on the surface of the hot-rolled steel sheet.

[0162]

[0163] Thereafter, the coiled hot-rolled steel sheet is cold-rolled at a cold reduction ratio of 35 to 70% to obtain a cold-rolled steel sheet. If the cold reduction ratio is less than 35%, it is not only difficult to secure the thickness desired in the present invention, but also there is a concern that austenite may be generated during annealing heat treatment due to the residual crystal grains formed during hot rolling, which may affect the final physical properties. In addition, the -value of the surface roughness (Rsk) may become excessively large, resulting in poor bending properties. If the cold reduction ratio exceeds 70%, the reduction in the length and width directions may become uneven due to the work hardening that occurs during cold rolling, which may cause material deviations in the steel sheet. In addition, it may be difficult to secure the thickness desired in the present invention due to the rolling load. The lower limit of the cold reduction ratio is more preferably 36%, more preferably 37%, and most preferably 38%. The upper limit of the above cold rolling reduction ratio is more preferably 68%, more preferably 66%, and most preferably 64%.

[0164]

[0165] Thereafter, the cold rolled steel sheet is continuously annealed at Ac3+20℃ to Ac3+80℃. If the continuous annealing temperature is lower than Ac3+20℃, a two-phase annealing instead of a single-phase annealing may occur over the entire length of the steel sheet, thereby forming a mixed grain structure, which may make it difficult to secure the properties targeted by the present invention. If the continuous annealing temperature exceeds Ac3+80℃, equipment trouble may occur due to overload of the annealing furnace. The lower limit of the continuous annealing temperature is more preferably Ac3+21℃, more preferably Ac3+24℃, and most preferably Ac3+25℃. The upper limit of the continuous annealing temperature is more preferably Ac3+70℃, more preferably Ac3+60℃, and most preferably Ac3+50℃. Meanwhile, the above Ac3 refers to the temperature at which austenite begins to appear upon heating, and can be obtained through the following equation 3.

[0166]

[0167] [Equation 3] Ac3(℃) = 910 - 203√C - 15.2Ni + 44.7Si + 104V + 31.5Mo + 13.1W

[0168]

[0169] The continuous annealing can be performed for 30 to 230 seconds. If the continuous annealing time is less than 30 seconds, there is a disadvantage in that it is difficult to secure a single-phase austenite structure. If the continuous annealing time exceeds 230 seconds, there is a disadvantage in that the austenite size becomes coarser, making it difficult to secure strength and bending properties. The lower limit of the continuous annealing time is more preferably 40 seconds, more preferably 50 seconds, and most preferably 60 seconds. The upper limit of the continuous annealing time is more preferably 220 seconds, more preferably 210 seconds, and most preferably 200 seconds.

[0170]

[0171] Thereafter, the continuously annealed cold-rolled steel sheet is first cooled to a first cooling end temperature (T1) of 670 to 750°C at an average cooling rate of 1 to 6°C / s. If the first cooling end temperature (T1) is less than 670°C, a large amount of soft ferrite and bainite other than martensite is formed during the cooling process, which may cause the surface structure to become uneven and deteriorate the bending properties. If the first cooling end temperature (T1) exceeds 750°C, the temperature difference between the first cooling end temperature (T1) and the second cooling end temperature (T2) becomes severe, causing a rapid phase transformation, which may deteriorate the shape of the product. It is more preferable that the lower limit of the first cooling end temperature is 680°C. It is more preferable that the upper limit of the first cooling end temperature is 740°C. If the above first average cooling rate is less than 1°C / s, ferrite is formed during cooling, making it impossible to secure the strength targeted by the present invention. If the above first average cooling rate exceeds 6°C / s, the average cooling rate during the subsequent second cooling decreases, increasing the fraction of low-temperature transformation phases other than martensite, making it impossible to secure the strength targeted by the present invention. The lower limit of the above first average cooling rate is more preferably 2°C / s. The upper limit of the above first average cooling rate is more preferably 5°C / s.

[0172]

[0173] Thereafter, the first-cooled cold-rolled steel sheet is secondarily cooled at an average cooling rate of 40 to 110°C / s to a second cooling end temperature (T2) of 50 to 200°C. The second cooling is to secure at least one of martensite and tempered martensite, which are the main phases of the present invention. When the second cooling end temperature (T2) is less than 50°C, there is a disadvantage in that shape defects are caused by rapid phase transformation and continuous production is difficult due to meandering of the strip. When the second cooling end temperature (T2) exceeds 200°C, it may be difficult to secure the strength targeted by the present invention. The lower limit of the second cooling end temperature is more preferably 55°C, even more preferably 60°C, and most preferably 65°C. The upper limit of the secondary cooling end temperature is more preferably 195°C, more preferably 190°C, and most preferably 185°C. If the secondary average cooling rate is less than 40°C / s, soft ferrite transformation occurs during cooling, making it difficult to secure the target strength. If the secondary average cooling rate exceeds 110°C / s, the product shape may become poor due to rapid phase transformation. The lower limit of the secondary average cooling rate is more preferably 45°C / s, more preferably 50°C / s, and most preferably 55°C / s. The upper limit of the secondary average cooling rate is more preferably 105°C, more preferably 100°C, and most preferably 95°C.

[0174]

[0175] In the above secondary cooling, it is desirable to satisfy the following relationships 4 and 5.

[0176]

[0177] [Relationship 4] F = 1 - exp{-(1.10×10 -2 ×△T)} ≥ 0.9

[0178] (However, in the above relational expression 4, △T is Ms - secondary cooling end temperature (T2).)

[0179]

[0180] The above relational expression 4 is a relational expression for obtaining the strength targeted by the present invention by securing the total fraction of at least one type of martensite and tempered martensite to be obtained by the present invention. If the value of F is less than 0.9, it may be difficult to secure the strength targeted by the present invention. The value of F is more preferably 0.91 or higher. In the present invention, since a higher value of F is advantageous, there is no particular limitation on the upper limit. However, the upper limit of the F value may be, for example, 0.99.

[0181]

[0182] [Relationship 5] 940 ≤ F×Z ≤ 1200

[0183] (Where, △T is Ms - secondary cooling end temperature (T2), and Z is 3500C + 150Mn + 50(Si+Cr+Mo) + 1000Nb.)

[0184]

[0185] The above equation 5 is a equation that examines the relationship between the above equation 4 and the strength-related factors. When the value of F×Z is less than 940, not only is the microstructure that the present invention seeks to obtain not secured, but the solid solution strengthening effect is insufficient, making it difficult to secure the strength that the present invention aims for. When the value of F×Z exceeds 1200, the strength may be excessively high, resulting in a low elongation. It is more preferable that the lower limit of the value of F×Z be 960. It is more preferable that the upper limit of the value of F×Z be 1180.

[0186]

[0187] It is preferable to control the first cooling end temperature (T1) - second cooling end temperature (T2) to be 650°C or lower. If the first cooling end temperature (T1) - second cooling end temperature (T2) exceeds 650°C, shape defects may occur. It is more preferable that the first cooling end temperature (T1) - second cooling end temperature (T2) be 600°C or lower.

[0188]

[0189] Afterwards, the second-cooled cold-rolled steel sheet is reheated to an overaging temperature (H) of 100 to 250°C, and then overaging is performed for 5 to 12 minutes. Through the reheating and overaging, the martensite obtained by the aforementioned rapid cooling process is transformed into tempered martensite, thereby increasing the yield strength. If the reheating temperature and overaging temperature are less than 100°C, tempering is not sufficiently performed, which results in a low yield strength and insufficient toughness. If the reheating temperature and overaging temperature exceed 250°C, which results in a deterioration in bending workability due to the precipitation and coarsening of a large amount of carbides. The lower limit of the reheating temperature and overaging temperature is more preferably 110°C, even more preferably 120°C, and most preferably 130°C. The upper limit of the reheating temperature and overaging temperature is more preferably 245°C, more preferably 240°C, and most preferably 235°C. If the overaging time is less than 5 minutes, tempering may not be sufficient, resulting in a decrease in yield strength. If the overaging time exceeds 12 minutes, excessive tempering may cause coarsening of carbides, resulting in poor bending properties. The lower limit of the overaging time is more preferably 5.5 minutes, more preferably 6.0 minutes, and most preferably 6.5 minutes. The upper limit of the overaging time is more preferably 11.5 minutes, more preferably 11 minutes, and most preferably 10.5 minutes.

[0190]

[0191] It is preferable to control the above overaging temperature (H) - secondary cooling end temperature (T2) to be 30°C or higher. If the above overaging temperature (H) - secondary cooling end temperature (T2) is less than 30°C, tempering is not sufficiently achieved, making it difficult to secure the target yield strength. It is more preferable that the above overaging temperature (H) - secondary cooling end temperature (T2) be 50°C or higher.

[0192]

[0193] Thereafter, the over-aged cold-rolled steel sheet is subjected to skin pass mill (SPM) rolling with a rolling force of 500 to 1,000 tons. The skin pass mill rolling enables control of the surface roughness (Rsk). If the rolling force is less than 500 tons during the skin pass rolling, the load is low, making it difficult to control the surface roughness (Rsk), and if it exceeds 1,000 tons, the work hardening of the surface may be severe, resulting in poor bending properties. The lower limit of the rolling force during the skin pass rolling is more preferably 550 tons, and more preferably 600 tons. The upper limit of the rolling force during the skin pass rolling is more preferably 950 tons, and more preferably 900 tons.

[0194]

[0195] Thereafter, the cold rolled steel sheet subjected to temper rolling is tension leveled (T / L) at an elongation of 0.05 to 0.65%. The tension leveling is for correcting the shape of the steel sheet. If the elongation is less than 0.05% during the tension leveling, shape correction may be difficult. If the elongation exceeds 0.65% during the tension leveling, work hardening may become severe and bending characteristics may deteriorate. The lower limit of the elongation during the tension leveling is more preferably 0.10%, and more preferably 0.15%. The upper limit of the elongation during the tension leveling is more preferably 0.60%, and more preferably 0.55%.

[0196]

[0197] Meanwhile, after the tension leveling, an additional step of forming an electrogalvanized layer on at least one surface of the cold-rolled steel sheet may be included. The present invention does not specifically limit the method for forming the electrogalvanized layer, and any method commonly used in the relevant technical field may be used.

[0198]

[0199] Hereinafter, the present invention will be described in more detail through examples. However, the description of these examples is merely intended to illustrate the implementation of the present invention and is not intended to limit the present invention. This is because the scope of the present invention is determined by the matters set forth in the claims and matters reasonably inferred therefrom.

[0200]

[0201] (Example)

[0202] A slab having the alloy composition described in Tables 1 and 2 below was heated at 1200°C, and then the heated slab was final hot-rolled at 900°C to obtain a hot-rolled steel sheet, which was then coiled at 500°C. Thereafter, cold-rolled at the cold reduction ratio described in Table 3 below to obtain a cold-rolled steel sheet. Thereafter, a cold-rolled steel sheet was manufactured by continuous annealing, primary cooling, secondary cooling, reheating, overaging treatment, temper rolling, and tension leveling under the conditions described in Tables 3 and 4 below. Meanwhile, the conditions described in Tables 3 and 4 below were based on the surface temperature of the steel sheet.

[0203]

[0204] The microstructure, average carbide size, surface roughness (Rsk), and mechanical properties of the cold-rolled steel sheet manufactured in this manner were measured, and the results are shown in Tables 5 and 6 below.

[0205]

[0206] The microstructure was observed using a scanning electron microscope (SEM) and an optical microscope (OM) at the surface of the steel plate (based on this example, at a position of 20 ㎛ in the thickness direction from the surface) and at a position of 1 / 4t (t: thickness of the steel) from the surface of the steel plate. Then, the fraction of each phase was analyzed three times through image analysis and the average value was calculated.

[0207]

[0208] The average size of carbides was measured using a transmission electron microscope (TEM) at a position 1 / 4t (t: thickness of steel) from the surface of the steel plate, and the average value was calculated.

[0209]

[0210] Surface roughness (Rsk) was measured five times using a contact-type 2D roughness meter, and the average value was calculated excluding the maximum (Max) and minimum (Min) values.

[0211]

[0212] Yield strength, tensile strength, yield ratio, and total elongation were measured by processing cold-rolled steel sheets into JIS standard (gauge length width × length: 25 × 50 mm, total specimen length: 200–260 mm) specimens and conducting a tensile test at a test speed of 28 mm / min.

[0213]

[0214] Bending workability (R / t) was measured by processing a cold-rolled steel plate into a specimen with a width of 100 mm × a length of 30 mm, and then performing a 90° bending test at a test speed of 100 mm / min. The presence or absence of cracks in the bent portion was checked using a stereoscopic microscope, and the R / t value was obtained by dividing the minimum bending radius at which no cracks occurred (the R value of the mold) by the thickness of the specimen (mm).

[0215]

[0216] Hole expandability (HER) was measured according to the ISO 16330 standard, and holes were sheared with a 10 mm diameter punch to a clearance of 12%.

[0217]

[0218] The crack length at the minimum nugget diameter (3√t, t: steel thickness (mm)) of the weld was measured by applying a welding current in the range of 5.0 to 6.0 kA under the conditions of Force: 3.8 KN, Welding time: 20 cycles, Holding time: 10 cycles, and a Gap of 1.5 t between two materials of 30 mm × 100 mm size, as shown in Fig. 1, and performing resistance spot welding. Then, the cross-section of the weld was observed with an optical microscope to measure the crack length in the area satisfying the minimum nugget diameter (3√t). Fig. 1 is a schematic diagram for evaluating the presence or absence of crack occurrence at the minimum nugget diameter (3√t) of the resistance spot weld.

[0219]

[0220] The hardness of the spot weld was measured 10 times using Vickers hardness (load: 500 gf) for the spot weld and the average value was calculated.

[0221]

[0222] Steel alloy composition (weight %) CSiMnPSNAl Inventive steel 10.2 20.11.8 50.01 0.00 10.00 40.03 Inventive steel 20.2 30.05 1.78 0.01 10.00 120.00 30.035 Inventive steel 30.2 10.15 1.9 10.01 20.00 0.00 90.00 40.03 Inventive steel 40.2 40.15 1.70.01 20.00 150.00 30.031 Inventive steel 50.2 30.21.6 50.00 90.00 110.00 40.035 Comparative steel 10.2 70.151.850.0110.00140.0050.039Comparative steel 20.250.22.50.0120.00120.0040.035Comparative steel 30.250.61.950.0150.0010.0040.03Comparative steel 40.180.11.750.0140.00150.0030.031Comparative steel 50.220.151.10.010.00110.0050.041Comparative steel 60.210.091.420.0080.0010.0030.035

[0223]

[0224] Steel alloy composition (weight %)CrMoNbTiBXYY / XInventive steel 10.10.050.0350.020.00250.34168496Inventive steel 20.090.070.030.0250.0020.347155447Inventive steel 30.150.090.0340.0230.00210.338174513Inventive steel 40.110.10.0250.0340.00240.36158439Inventive steel 50.150.110.020.0290.0020.342150440Comparative steel 10.16 0.070.0310.0210.00250.395175444Comparative Steel 20.150.090.0250.0250.00210.41187456Comparative Steel 30.10.090.0250.020.0020.402174432Comparative Steel 40.150.080.0290.0270.00240.305159521Comparative Steel 50.070.040.030.0250.00250.304133438Comparative Steel 60.010.020.0210.020.0020.304118390X = C + Mn / 20 + Si / 30 + 2P + 4SY = 48.8 + 49logC + 35.1Mn + 25.9Si + 14.5Ni + 9.6Cu + 76.5Cr + 105.9Mo + 1325Nb +10000B ≤ 190410 ≤ Y / X ≤ 620

[0225]

[0226] Classification Steel grade Cold rolling reduction ratio (%) Cold rolled steel sheet thickness (mm) Ac3 (℃) Annealing temperature (℃) First cooling end temperature (T1) (℃) First average cooling speed (T2) (℃ / s) Second cooling end temperature (℃) Second average cooling speed (℃ / s) T1-T2 (℃) Invention example 1 Invention steel 1501.6821859715312060595 Invention example 2 Invention steel 2501.6817869720311758603 Invention example 3 Invention steel 3501.6827867721313260589 Invention example 4 Invention steel 4501.6820859718313557583 Invention example 5 Invention steel 5501.68 25860725311555610Comparative Example 1Comparative Steel 1501.6813857700312160579Comparative Example 2Comparative Steel 2501.6820855720313254588Comparative Example 3Comparative Steel 3501.6838875715312055595Comparative Example 4Comparative Steel 4501.6831865719315260567Comparative Example 5Comparative Steel 5501.6823860711313561576Comparative Example 6Comparative Steel 6501.6822865705312163584Invention Example 6Invention Steel 4501.6820855695311765578Invention Example 7 Invention example 4501.6820865701312161580Invention example 8Invention example 4501.6820861725312560600Comparative example 7Invention example 4501.6820825720411657604Comparative example 8Invention example 4501.6820861660312560535Comparative example 9Invention example 4501.6820856725325065475Comparative example 10Invention example 4501.6820867715311660599Comparative example 11Invention example 4501.6820864705313560570Comparative example 12Invention example 4501.6820867721 312561596Invention Example 9Invention Steel 2561.4817869720312565595Invention Example 10Invention Steel 2571.2817869720312162599Invention Example 11Invention Steel 2581.6817869720311563605Comparative Example 13Invention Steel 2301.4817869720311957601Comparative Example 14Invention Steel 2301.2817869720312962591Comparative Example 15Invention Steel 2301.6817869720314563575Comparative Example 16Invention Steel 2501.6817869720313565585Ac3(℃) = 910 - 203√C - 15.2Ni + 44.7Si + 104V + 31.5Mo + 13.1W.

[0227]

[0228] Classification Steel grade Ms (℃) FZF × Z Reheating / overaging treatment temperature (H) (℃) Overaging treatment time (min) H-T2 (℃) Temper rolling Rolling force (ton) Tension leveling Elongation (%) Invention example 1 Invention steel 1 3880.95 1095 1040 180 960 6000.35 Invention example 2 Invention steel 2 3870.95 111 310 57 1909.57 36000.3 Invention example 3 Invention steel 3 3890.94 1075 101 1959.56 36000.25 Invention example 4 Invention steel 4 3840.94 1138 1070 1859.55 06000.15 Invention example 5 Invention steel 5 3880.95 1096 104 120 1108 66000.2 Comparative Example 1 Comparative Steel 1 3660.93 12 73 11 84 1859.56 46 000.35 Comparative Example 2 Comparative Steel 2 3540.91 12 9 7 1 1 80 17 49.54 26 000.35 Comparative Example 3 Comparative Steel 3 3680.93 12 3 2 1 1 4 6 18 69.56 6 6 000.35 Comparative Example 4 Comparative example 44070.9493888219510436000.35 Comparative example 5 Comparative example 54110.9597892920010656000.35 Comparative example 6 Comparative example 64070.969759362019.5806000.35 Invention example 6 Invention 43840.9511381078 1859.5686000.35 Invention Example 7 Invention Steel 43840.941138107518010596000.25 Invention Example 8 Invention Steel 43840.941138107219110666000.35 Comparative Example 7 Invention Steel 43840.95113810781859.5696000 .35 Comparative Example 8 Inventive Steel 43840.941138107219010656000.35 Comparative Example 9 Inventive Steel 43840.77113887726010106000.35 Comparative Example 10 Inventive Steel 43840.9511381078280101646000.35 Comparative Example 11 Inventive Steel 43 840.941138106418710522000.03 Comparative Example 12 Invention Steel 43840.941138107219410692000.80 Invention Example 9 Invention Steel 23870.94111310511789.5537000.25 Invention Example 10 Invention Steel 23870.9511131 0531819.5607000.25Invention Example 11Invention Steel 23870.95111310571859.5707000.25Comparative Example 13Invention Steel 23870.95111310551809.5617000.25Comparative Example 14Invention Steel 23870.94111310481879.5587000.25Comparative Example 15Inventive Steel 23870.93111310351819.5366000.25Comparative Example 16Inventive Steel 23870.94111310431899.5542500.25Ms(℃) = 539 - 423C - 30.4Mn - 7.5Si + 30Al - 17.7Ni - 12.1Cr - 7.5Mo△T = Ms - Second Cooling End Temperature(T2)Z = 3500C + 150Mn + 50(Si+Cr+Mo) + 1000Nb.

[0229]

[0230] Classification Microstructure (area%) Average size of carbide (nm) Surface roughness (Rsk) Surface center At least one of F and B At least one of M and TM At least one of F and B At least one of M and TM Invention example 15.294.8 19956-0.35 Invention example 24795.3 19950-0.31 Invention example 3595 19990-0.3 Invention example 43.996.1 19968-0.31 Invention example 54.795.3 19945-0.32 Comparative example 13.596.5 19950-0.4 Comparative example 23.996.1 19956-0.39 Comparative example 39.690.439795-0.31 Comparative Example 412.387.7257545-0.32 Comparative Example 514.585.5307098-0.3 Comparative Example 616.783.33565105-0.34 Invention Example 64.595.519975-0.38 Invention Example 73.996.119966-0.35 Invention Example 85.394.719987 -0.41Comparative Example 713.586.5208078-0.32Comparative Example 816.883.219956-0.38Comparative Example 94.595.5199269-0.35Comparative Example 10496199360-0.85Comparative Example 114.295.819985-0.79Comparative Example 123.996.119955-0.41Invention Example 95.294. 819955-0.21 Invention Example 104.795.319961-0.25 Invention Example 114.795.319948-0.15 Comparative Example 133.596.519962-0.75 Comparative Example 144.695.419954-0.79 Comparative Example 153.996.119955-0.81 Comparative Example 164.595.519952-0.72 F: Ferrite, B: Bainite, M: Martensite, TM: Tempered Martensite

[0231]

[0232] Yield strength (YS) (MPa) Tensile strength (TS) (MPa) YR Total elongation (%) Bending workability (R / t) Hole expandability (%) (TS×HER) / (R / t) (MPa%) Weld strength (Hv) at 3√t Crack length (㎛) Invention example 1 1 2 7 6 1 5 5 6 0.8 2 7 3 4 5 0 2 6 1 6 4 9 10 Invention example 2 1 3 0 3 1 5 7 5 0.8 2 7 3 4 5 2 3 8 0 8 5 0 10 Invention example 3 1 2 6 7 1 5 4 8 0.8 2 7 3 4 5 9 2 0 5 0 4 9 50 Invention example 4 1 2 5 4 1 5 4 9 0.8 1 7 3 4 5 9 2 6 5 6 7 5 150 Invention example 5 1 2 8 2 1 5 5 3 0.8 3 7 3 4 5 5 2 4 8 3 0 4 9 10 Comparative example 1 1 3 5 0 1 6 6 0 0.8 1 3 4 3 4 5 13 2 6 5 5 9 2 2 8 7 Comparative example 2 1 4 2 0 1 6 9 0.8 4 3 4 3 84517363589251Comparative Example 3124015200.8263.755020267581198Comparative Example 4101113700.74114.0628122564320Comparative Example 5116814300.82104.0629120554210Comparative Example 691012300.74124.062589394200Invention Example 6132115740.8473.4450228784900Invention Example 7129715640.8373.4452236424920Invention Example 813011579 0.8273.444922492950Comparison Example 7105414520.73104.3832106084910Comparison Example 8123115360.8074.692891704980Comparison Example 9102014650.7094.693196834920Comparison Example 10129814790.8884.6942132454900Comparison Example 11113015420.7374.0645201725010Comparison Example 12148515340.9734.6943140644950Invention Example 91285 15560.8373.2152252064920Invention Example 10130115750.8373.3349231764900Invention Example 11128215530.8373.2253255624950Comparative Example 13129515650.8374.2941149574920Comparative Example 14131115660.8474.2239144734890Comparative Example 15126515340.8284.0639147354920Comparative Example 16129715640.8374.0645173354950

[0233]

[0234] As can be seen from Tables 1 to 6 above, in the case of Invention Examples 1 to 11 that satisfy the alloy composition and manufacturing conditions proposed by the present invention, it can be seen that the mechanical properties are excellent by securing the microstructure, average carbide size, and surface roughness (Rsk) that the present invention seeks to obtain.

[0235]

[0236] It can be seen that in the case of Comparative Examples 1 to 6, which do not satisfy the alloy composition proposed by the present invention, the mechanical properties are inferior.

[0237]

[0238] In the case of Comparative Examples 7 to 16, which do not satisfy the manufacturing conditions proposed by the present invention, it can be seen that the mechanical properties are inferior because the microstructure, average carbide size, or surface roughness (Rsk) are not satisfied.

[0239]

[0240] Fig. 2 is a microstructure photograph of the surface layer of Invention Example 1 observed with a scanning electron microscope (SEM), and Fig. 3 is a microstructure photograph of the surface layer of Comparative Example 5 observed with a scanning electron microscope (SEM). As can be seen from Figs. 2 and 3, in the case of Invention Example 1, it can be seen that it has mostly martensite and tempered martensite structures, but in the case of Comparative Example 5, it can be seen that it contains a considerable amount of ferrite and bainite structures.

[0241]

[0242] Fig. 4 is a microstructure photograph of a welded section of Invention Example 4 observed with an optical microscope, and Fig. 5 is a microstructure photograph of a welded section of Comparative Example 1 observed with an optical microscope. As can be seen from Figs. 4 and 5, no cracks occurred in the case of Invention Example 4, but cracks occurred in the case of Comparative Example 1.

Claims

1. Contains, by weight%, carbon (C): 0.19 to 0.26%, silicon (Si): 0.03 to 0.50%, manganese (Mn): 1.4 to 2.0%, chromium (Cr): 0.03 to 0.30%, molybdenum (Mo): 0.03 to 0.30%, boron (B): 0.0005 to 0.005%, phosphorus (P): 0.03% or less (excluding 0%), sulfur (S): 0.003% or less (excluding 0%), nitrogen (N): 0.01% or less (excluding 0%), aluminum (Al): 0.01 to 0.10%, niobium (Nb): 0.01 to 0.05%, titanium (Ti): 0.005 to 0.05%, the remainder being iron and other unavoidable impurities. Satisfies the following relationships 1 to 3, central; and Includes a surface layer formed on the outer side based on the thickness direction of the center; The microstructure of the above center is, in area %, the sum of at least one type of ferrite and bainite: 5% or less (including 0%), and the remainder includes at least one type of martensite and tempered martensite. The microstructure of the above surface layer is, in area %, the sum of at least one type of ferrite and bainite: 11% or less (excluding 0%), and at least one type of residual martensite and tempered martensite. Cold rolled steel sheet with an average carbide size of 260 nm or less. [Relationship 1] 0.31 ≤ X = C + Mn / 20 + Si / 30 + 2P + 4S ≤ 0.40 [Relationship 2] 125 ≤ Y = 48.8 + 49logC + 35.1Mn + 25.9Si + 14.5Ni + 9.6Cu + 76.5Cr + 105.9Mo + 1325Nb + 10000B ≤ 190 [Relationship 3] 410 ≤ Y / X ≤ 620 (However, in the above equations 1 to 3, the content of each alloy element is in weight%.) 2. In claim 1, The above cold rolled steel sheet is a cold rolled steel sheet with a surface roughness (Rsk) of -0.7 to -0.

1.

3. In claim 1, The above cold rolled steel sheet is a cold rolled steel sheet with a yield strength of 1150 to 1400 MPa.

4. In claim 1, The above cold rolled steel sheet is a cold rolled steel sheet with a tensile strength of 1470 to 1650 MPa.

5. In claim 1, The above cold rolled steel sheet is a cold rolled steel sheet with a yield ratio of 0.75 to 0.

96.

6. In claim 1, The above cold rolled steel sheet is a cold rolled steel sheet with an elongation of 4 to 11%.

7. In claim 1, The above cold rolled steel sheet is a cold rolled steel sheet with a bending workability (R / t) of 2 to 4.

8. In claim 1, The above cold rolled steel sheet is a cold rolled steel sheet with a hole expandability of 35 to 70%.

9. In claim 1, The above cold-rolled steel sheet is a cold-rolled steel sheet having (tensile strength × hole expandability) / (bending workability (R / t)) of 15000 to 35000 MPa%.

10. In claim 1, The above cold-rolled steel sheet is a cold-rolled steel sheet with a hardness of 440 to 570 Hv at the spot weld after resistance spot welding.

11. In claim 1, The above cold-rolled steel sheet is a cold-rolled steel sheet in which, after resistance spot welding, the crack length at the minimum nugget diameter (3√t, t: thickness of steel) of the spot weld is 10㎛ or less (including 0㎛).

12. In claim 1, The above cold rolled steel sheet is a cold rolled steel sheet having an electrogalvanized layer formed on at least one surface.

13. In claim 1, The above surface layer is a cold rolled steel sheet in the area from the surface of the steel to 20㎛ in the thickness direction.

14. Contains, by weight%, carbon (C): 0.19 to 0.26%, silicon (Si): 0.03 to 0.50%, manganese (Mn): 1.4 to 2.0%, chromium (Cr): 0.03 to 0.30%, molybdenum (Mo): 0.03 to 0.30%, boron (B): 0.0005 to 0.005%, phosphorus (P): 0.03% or less (excluding 0%), sulfur (S): 0.003% or less (excluding 0%), nitrogen (N): 0.01% or less (excluding 0%), aluminum (Al): 0.01 to 0.10%, niobium (Nb): 0.01 to 0.05%, titanium (Ti): 0.005 to 0.05%, the remainder being Fe and other unavoidable impurities, and satisfying the following relationships 1 to 3. Step of heating the slab at 1100~1300℃; A step of obtaining a hot-rolled steel sheet by finishing hot rolling the above-mentioned heated slab at Ar3~Ar3+120℃; A step of coiling the above hot-rolled steel sheet at Ms~600℃; A step of obtaining a cold rolled steel sheet by cold rolling the above-mentioned coiled hot rolled steel sheet at a cold rolling reduction ratio of 35 to 70%; A step of continuously annealing the above cold rolled steel sheet at Ac3+20℃ to Ac3+80℃; A step of first cooling the continuously annealed cold rolled steel sheet to a first cooling end temperature (T1) of 670 to 750°C at an average cooling rate of 1 to 6°C / s; A step of secondary cooling the first-cooled cold-rolled steel sheet at an average cooling rate of 40 to 110°C / s to a secondary cooling end temperature (T2) of 50 to 200°C; A step of reheating the above-mentioned second-cooled cold-rolled steel sheet to an overaging temperature (H) of 100 to 250°C and then performing an overaging treatment for 5 to 12 minutes; and A step of subjecting the above-mentioned cold-rolled steel sheet to temper rolling with a pressing force of 500 to 1000 tons; and A step of tension leveling the above cold rolled steel sheet with an elongation of 0.05 to 0.65%; In the above secondary cooling, the following relationships 4 and 5 are satisfied, Control the above first cooling end temperature (T1) - second cooling end temperature (T2) to be 650℃ or less, A method for manufacturing a cold-rolled steel sheet, wherein the above-mentioned over-aging temperature (H) - secondary cooling end temperature (T2) is controlled to be 30°C or higher. [Relationship 1] 0.31 ≤ X = C + Mn / 20 + Si / 30 + 2P + 4S ≤ 0.40 [Relationship 2] 125 ≤ Y = 48.8 + 49logC + 35.1Mn + 25.9Si + 14.5Ni + 9.6Cu + 76.5Cr + 105.9Mo + 1325Nb + 10000B ≤ 190 [Relationship 3] 410 ≤ Y / X ≤ 620 [Relationship 4] F = 1 - exp{-(1.10×10 -2 ×△T)} ≥ 0.9 [Relationship 5] 940 ≤ F×Z ≤ 1200 (However, in the above equations 1 to 3, the content of each alloy element is weight%, △T is Ms - secondary cooling end temperature (T2), and Z is 3500C + 150Mn + 50(Si+Cr+Mo) + 1000Nb.) 15. In claim 14, A method for manufacturing cold rolled steel sheets in which the above continuous annealing is performed for 30 to 230 seconds.

16. In claim 14, A method for manufacturing a cold-rolled steel sheet, further comprising, after the above tension leveling, a step of forming an electrogalvanized layer on at least one surface of the cold-rolled steel sheet.