Cold rolled steel sheet and method for manufacturing same
Patent Information
- Application Number
- MYPI2025003512
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-12-20
- Filing Date
- 2023-12-14
- Publication Date
- 2024-06-20
AI Technical Summary
Existing cold rolled steel sheets lack excellent bending formability and high strength, which is essential for advanced automotive applications, particularly in ultra-high strength steels required for electric vehicles and enhanced passenger safety in car crashes.
A cold rolled steel sheet composition with specific alloying elements (C, Si, Al, Mn, Cr, Mo, B, Nb, Ti, P, S, N, Cu, Ni, and V) and a manufacturing process involving hot rolling, coiling, cold rolling, continuous annealing, primary and secondary cooling, and reheating to achieve a microstructure with tempered martensite, retained austenite, and controlled phase fractions, satisfying specific relational equations for strength and formability.
The solution achieves a tensile strength of 1470 MPa or more, yield strength of 1000 MPa or more, total elongation of 8.5% or more, and improved bending formability, ensuring the steel sheet can absorb impact energy without cracking, thus enhancing safety and performance in automotive applications.
Abstract
Description
Cold rolled steel sheet and its manufacturing method
[0001] The present invention relates to a cold rolled steel sheet and a method for manufacturing the same.
[0002]
[0003] The development of high-strength steel plates has been continuously pursued to reduce vehicle weight and enhance safety. Recently, the importance of ultra-high-strength steels with a tensile strength of 1,500 MPa or higher has increased to extend the driving range of electric vehicles and protect batteries. However, existing MART steels lack formability, so the development of ultra-high-strength steel plates for cold forming that combine formability with formability is expected to have significant economic value. One widely used method to improve formability in steels is to utilize TRansformation Induced Plasticity (TRIP) by introducing retained austenite to increase elongation. However, TRIP steel plates require the addition of Si and Al to introduce retained austenite, and even greater amounts of retained austenite can be obtained when accompanied by bainite transformation. However, because bainite transforms at relatively high temperatures, the tensile strength (TS) is low, and the yield strength (YS) is too low for use as ultra-high-strength steel.
[0004]
[0005] Therefore, the recent trend is to adopt a quenching and partitioning process to enhance the strength of steel plates while also leveraging the TRIP phenomenon. In the case of so-called Q&P steels, the primary matrix structure is tempered martensite, resulting in excellent yield strength and hole expansion ratio (HER). Actively forming retained austenite can also yield an appropriate level of elongation.
[0006]
[0007] Meanwhile, the importance of automotive safety from the perspective of passenger protection is growing day by day. While improvements in autonomous driving technology are expected to fundamentally eliminate the risk of car crashes, there is a risk that passengers' unawareness of the accident situation during the transition period until the technology matures, which could increase the severity of accidents. Consequently, regulations on automobile crash testing have recently been strengthened. The bending properties of steel are known to be crucial for reducing the risk of cracking in automotive structural components during a crash. When steel has excellent bending properties, the material folds instead of cracking, absorbing more of the impact energy. This allows the remaining components to withstand the impact, leading to stable structural collapse.
[0008]
[0009] However, obtaining excellent bending formability is not enough by simply applying the Q&P process, and additional ideas are needed to secure excellent bending formability along with high strength of over 1500 MPa.
[0010]
[0011] One aspect of the present invention is to provide a cold rolled steel sheet and a method for manufacturing the same.
[0012] A preferred aspect of the present invention is to provide a cold-rolled steel sheet having excellent strength and bending formability and a method for manufacturing the same.
[0013]
[0014] One embodiment of the present invention comprises, in wt%, C: 0.15% or more and less than 0.30%, Si: 0.8 to 2.5%, Al: 0.005 to 0.3%, Mn: 2.0 to 3.0%, Cr: 0.001 to 0.5%, Mo: 0.001 to 0.2%, B: 0.0005 to 0.0050%, Nb: 0.001 to 0.05%, Ti: 0.001 to 0.05%, P: 0.04% or less (excluding 0%), S: 0.01% or less (excluding 0%), N: 0.01% or less (excluding 0%), the remainder Fe and other unavoidable impurities, and the microstructure comprises, in area%, ferrite: 15% or less (excluding 0%), fresh martensite 5% or less (excluding 0%), and tempered martensite. A cold rolled steel sheet is provided, which is composed of 75% or more and 95% or less of residual austenite, 12% or less (excluding 0%), and residual bainite, and satisfies the following relational expression 1.
[0015] [Relationship 1] (RA unstable +RA stable ) / RA stable ≤ 2.0
[0016] (However, in the above relational expression 1, RA unstable means the fraction of unstable retained austenite, and RA stable refers to the fraction of stable retained austenite.)
[0017]
[0018] The above cold rolled steel sheet may additionally include at least one of Cu: 0.1% or less (excluding 0%) and Ni: 0.1% or less (excluding 0%).
[0019]
[0020] The above cold rolled steel sheet may additionally include V: 0.05% or less (excluding 0%).
[0021]
[0022] The above-mentioned retained austenite may have an average grain size of 0.5㎛ or less.
[0023]
[0024] The above cold rolled steel sheet can satisfy the following relationship 2.
[0025] [Relationship 2] 4×P.El - U.El ≥ 13.0
[0026] (However, in the above relational expression 2, P.El means local elongation, and U.El means uniform elongation.)
[0027]
[0028] The above cold rolled steel sheet has a tensile strength of 1470 MPa or more, a yield strength of 1000 MPa or more, a total elongation (T.El) of 8.5% or more, and a bending formability (R) of 2.5 or less. min / t) can be used.
[0029]
[0030] One embodiment of the present invention comprises the steps of: heating a slab containing, in wt%, C: 0.15% or more and less than 0.30%, Si: 0.8 to 2.5%, Al: 0.005 to 0.3%, Mn: 2.0 to 3.0%, Cr: 0.001 to 0.5%, Mo: 0.001 to 0.2%, B: 0.0005 to 0.0050%, Nb: 0.001 to 0.05%, Ti: 0.001 to 0.05%, P: 0.04% or less (excluding 0%), S: 0.01% or less (excluding 0%), N: 0.01% or less (excluding 0%), the remainder Fe and other unavoidable impurities; and subjecting the heated slab to a finish hot rolling at 830 to 950°C to obtain a hot-rolled steel sheet. A method for manufacturing a cold rolled steel sheet is provided, comprising: a step of coiling the hot rolled steel sheet at 400 to 650°C; a step of cold rolling the coiled hot rolled steel sheet to obtain a cold rolled steel sheet; a step of continuously annealing the cold rolled steel sheet at 800 to 950°C; a step of first cooling the continuously annealed cold rolled steel sheet to a first cooling end temperature of 500 to 700°C at an average cooling rate of 1°C / s or more and less than 10°C / s; a step of second cooling the first-cooled cold rolled steel sheet to a second cooling end temperature of 25 to 300°C at an average cooling rate of 10°C / s or more; and a step of reheating the second-cooled cold rolled steel sheet at 150 to 450°C and then maintaining the temperature for more than 500 seconds and less than 1,500 seconds.
[0031]
[0032] The above slab may additionally contain at least one of Cu: 0.1% or less (excluding 0%) and Ni: 0.1% or less (excluding 0%).
[0033]
[0034] The above slab may additionally contain V: 0.05% or less (excluding 0%).
[0035]
[0036] The heating temperature of the above slab can be 1150 to 1250°C.
[0037]
[0038] The cold rolling reduction ratio during the above cold rolling can be 30 to 60%.
[0039]
[0040] According to one aspect of the present invention, a cold rolled steel sheet and a method for manufacturing the same can be provided.
[0041] According to a preferred aspect of the present invention, a cold-rolled steel sheet having excellent strength and bending formability and a method for manufacturing the same can be provided.
[0042]
[0043] Hereinafter, a cold-rolled steel sheet according to one embodiment of the present invention will be described. First, the alloy composition will be described. Unless otherwise specified, the content of the alloy composition described below refers to weight percent.
[0044]
[0045] C: 0.15% or more and less than 0.30%
[0046] Carbon (C) is an element that secures the strength of steel through solid solution strengthening and precipitation strengthening. If the C content is less than 0.15%, it is difficult to secure a tensile strength (TS) of 1.5 GPa. On the other hand, if the C content is 0.30% or more, arc weldability and laser weldability deteriorate, and the risk of cracking due to the formation of coarse carbides increases. Therefore, the C content is preferably in the range of 0.15% or more and less than 0.30%. In terms of securing strength, the lower limit of the C content is more preferably 0.17%. In addition, in terms of weldability and the possibility of brittleness due to coarse carbides, the upper limit of the C content is more preferably 0.28%.
[0047]
[0048] Si: 0.8~2.5%
[0049] Silicon (Si) is a key element of TRIP (Transformation Induced Plasticity) steels, which inhibit the precipitation of cementite and thereby increase the fraction of retained austenite and elongation. If the Si content is less than 0.8%, almost no retained austenite remains, resulting in excessively low elongation. On the other hand, if the Si content exceeds 2.5%, the deterioration of the weld properties due to the formation of LME cracks cannot be prevented, and the surface properties and plating properties of the steel deteriorate. Therefore, the Si content is preferably in the range of 0.8 to 2.5%. Taking the elongation into account, the lower limit of the Si content is more preferably 0.9%, even more preferably 1.0%, and may be controlled to 1.1% depending on the elongation required for the application product. The upper limit of the above Si content is more preferably 2.2%, more preferably 2.0%, and may be controlled to 1.7% in consideration of the intended use of the product or the plating method.
[0050]
[0051] Al: 0.005~0.3%
[0052] Aluminum (Al) is not only an element included for deoxidation of steel, but is also an element that is effective in stabilizing residual austenite by suppressing precipitation of cementite. If the Al content is less than 0.005%, deoxidation of the steel is not sufficient, and the cleanliness of the steel is impaired. On the other hand, if the Al content exceeds 0.3%, the castability of the steel is impaired. Therefore, the Al content is preferably in the range of 0.005 to 0.3%. In terms of the cleanliness of the steel, the lower limit of the Al content is more preferably 0.01%, more preferably 0.02%, and may be controlled to 0.03% in consideration of the product to be used or the request of the user. In consideration of the castability of the steel mentioned above, the upper limit of the Al content is more preferably 0.27%, more preferably 0.22%, and may be controlled to 0.17% in consideration of the processing environment of the product to be used or the user.
[0053]
[0054] Mn: 2.0~3.0%
[0055] Manganese (Mn) is an element added to secure strength. If the Mn content is less than 2.0%, it becomes difficult to secure strength. On the other hand, if the content exceeds 3.0%, the phase transformation rate becomes slow, forming too much fresh martensite, making it difficult to obtain excellent formability. In addition, segregation of Mn forms a band structure, which impairs the material uniformity and formability of the material. Therefore, the Mn content is preferably in the range of 2.0 to 3.0%. Considering the target strength of the steel, the lower limit of the Mn content is more preferably 2.2%. Considering formability, the upper limit of the Mn content is more preferably 2.8%.
[0056]
[0057] Cr: 0.001~0.5%
[0058] Chromium (Cr) is an element added to secure strength and hardenability. When Mn is added alone, a very large amount of Mn must be added, exceeding the Mn content range of the present invention. This problem can be solved by adding Cr in an amount of 0.001% or more. When the Cr content exceeds 0.5%, local corrosion resistance deteriorates and oxides are formed on the surface, thereby impairing phosphate treatment properties. Therefore, the Cr content is preferably in the range of 0.001 to 0.5%. Depending on the characteristics of the product to be used, the upper limit of the Cr content may be controlled to 0.3% in consideration of corrosiveness and phosphate treatment properties.
[0059]
[0060] Mo: 0.001~0.2%
[0061] Molybdenum (Mo) is added to secure strength and hardenability. To achieve these strength and hardenability enhancement effects, the Mo content must be added at least 0.001%. However, as it is an expensive element, it may reduce the economic feasibility of the steel sheet and excessively delay phase transformation, thereby inducing the formation of fresh martensite. Therefore, it is preferable that the Mo content does not exceed 0.2%. In terms of the aforementioned cost, the upper limit of the Mo content is more preferably 0.15%, and can be controlled to 0.12%.
[0062]
[0063] B: 0.0005~0.0050%
[0064] Boron (B) is an element added to secure hardenability. When Mn is added alone, a very large amount of Mn must be added exceeding the Mn content range of the present invention. This problem can be solved by adding B in an amount of 0.0005% or more. However, when the B content exceeds 0.0050%, boron-based carbides are formed at grain boundaries, which actually impairs hardenability. Therefore, the B content is preferably in the range of 0.0005 to 0.0050%. In terms of hardenability, the upper limit of the B content is more preferably 0.0040%, more preferably 0.0030%, and can be controlled to 0.0025%.
[0065]
[0066] Nb: 0.001~0.05%
[0067] Niobium (Nb) is an element added to secure the strength of steel plates and refine the structure. If the Nb content is less than 0.001%, it is difficult to obtain the effects of improving strength and refining the structure. In addition, if the Nb content exceeds 0.05%, recrystallization is delayed due to local grain fixation, which harms the uniformity of the structure. Therefore, the Nb content is preferably in the range of 0.001 to 0.05%. In terms of uniformity, the upper limit of the Nb content is more preferably 0.03%.
[0068]
[0069] Ti: 0.001~0.05%
[0070] Titanium (Ti) is an element added to steel plates to secure strength and refine the structure. If the Ti content is less than 0.001%, it is difficult to obtain the effects of strength improvement and structure refinement. If the Ti content exceeds 0.05%, castability is impaired due to excessive TiN formation, and the impact properties of the steel are impaired due to excessive carbide formation. Therefore, the Ti content is preferably in the range of 0.001 to 0.05%. In terms of improving impact properties, the upper limit of the Ti content is more preferably 0.03%.
[0071]
[0072] P: 0.04% or less (excluding 0%)
[0073] Phosphorus (P) exists as an impurity in steel, and it is advantageous to control its content as low as possible, but it is also intentionally added to increase the strength of the steel. However, if the above-mentioned P is added excessively, the toughness of the steel deteriorates, so in the present invention, it is preferable to limit the upper limit to 0.04% to prevent this. In terms of improving toughness, the above-mentioned P content is more preferably 0.015% or less, and even more preferably 0.010% or less. If the toughness of the steel is required to exceed the standard, it may be controlled to 0.007% or less.
[0074]
[0075] S: 0.01% or less (excluding 0%)
[0076] Sulfur (S), like the above-mentioned P, exists as an impurity in steel, and it is advantageous to control its content as low as possible. In addition, since the above-mentioned S deteriorates the ductility and impact properties of steel, it is desirable to limit its upper limit to 0.01%. The above-mentioned S content is more preferably 0.005% or less, even more preferably 0.003% or less, and most preferably 0.0015% or less.
[0077]
[0078] N: 0.01% or less (excluding 0%)
[0079] In the present invention, nitrogen (N) is inevitably included in the steel as an impurity during the process, and its upper limit is preferably limited to 0.01%. The N content is more preferably 0.007% or less, more preferably 0.005% or less, and most preferably 0.003% or less.
[0080]
[0081] In addition to the steel composition described above, the remainder may contain iron and unavoidable impurities. Unavoidable impurities are those that can be unintentionally incorporated during the typical steelmaking process, and cannot be completely excluded. Those skilled in the art of conventional steelmaking can readily understand their significance. Furthermore, the present invention does not completely exclude the addition of components other than the aforementioned steel composition.
[0082]
[0083] Meanwhile, the cold rolled steel sheet according to the present invention may additionally include at least one of Cu: 0.1% or less (excluding 0%) and Ni: 0.1% or less (excluding 0%) depending on the embodiment. Copper (Cu) and nickel (Ni) are elements that increase the strength of steel. However, although the above elements are elements that increase the strength and hardenability of steel, if they are added in excessive amounts, the target strength grade may be exceeded, and since they are expensive elements, it is preferable to limit the upper limit to 0.1% each from an economical perspective. Meanwhile, since Cu and Ni act as solid solution strengthening elements, if they are added in amounts less than 0.03%, the solid solution strengthening effect may be minimal, and therefore, they may be added in amounts of 0.03% or more each.
[0084]
[0085] In addition, the cold-rolled steel sheet according to the present invention may additionally include V: 0.05% or less (excluding 0%) depending on the embodiment. Vanadium (V) can increase the strength of steel even with a small amount of addition, but its effect on improving elongation is not significant, so it is preferable to control its content to 0.05% or less. The content of V is more preferably 0.04% or less, and even more preferably 0.03% or less.
[0086]
[0087] The cold-rolled steel sheet according to the present invention may be composed of a microstructure in terms of area % of ferrite: 15% or less (excluding 0%), fresh martensite: 5% or less (excluding 0%), tempered martensite: 75% or more and less than 95%, retained austenite: 12% or less (excluding 0%), and the remainder bainite.
[0088]
[0089] The cold-rolled steel sheet according to the present invention is intended to secure excellent bending formability at a tensile strength of 1470 MPa or higher. In particular, in order to obtain high local formability, the hardness difference between the microstructural phases constituting the steel sheet must be reduced. If the fraction of the softest ferrite exceeds 15%, the yield strength decreases and the hole expandability and bending formability deteriorate. In addition, if the fraction of fresh martensite, which is brittle and has high strength because it is not tempered, exceeds 5%, the formability also deteriorates. Tempered martensite is a structure obtained by tempering martensite formed when the steel sheet is cooled below the Ms temperature through a reheating or temperature maintenance process, and has high strength. When the fraction is 75% or more, a high strength of 1470 MPa or higher and excellent bending formability can be obtained. However, if the fraction of the above tempered martensite exceeds 95%, the entire microstructure becomes a full martensite structure with high strength but insufficient ductility, making it impossible to obtain the necessary formability. Retained austenite refers to the austenite that remains at room temperature after the steel plate manufacturing process is complete. If it has sufficient stability, when additional deformation is applied to the steel, it will not immediately transform into martensite, but will gradually transform into martensite depending on the deformation level, thereby contributing to the elongation and bending properties. If the retained austenite is sufficiently stable, the higher the fraction, the better. However, if the fraction exceeds 12%, the stability will decrease, which may significantly deteriorate the bending properties.
[0090]
[0091] The above-mentioned retained austenite may have an average grain size of 0.5 μm or less. If the average grain size of the above-mentioned retained austenite exceeds 0.5 μm, it may be difficult to secure excellent bending properties. Meanwhile, the above-mentioned retained austenite can be measured through EBSD, and a phase classified as FCC when analyzed through EBSD can be regarded as retained austenite.
[0092]
[0093] It is preferable that the cold rolled steel sheet according to the present invention satisfies the following relational expression 1.
[0094] [Relationship 1] (RA unstable +RA stable ) / RA stable ≤ 2.0
[0095] (However, in the above relational expression 1, RA unstable means the fraction of unstable retained austenite, and RA stable refers to the fraction of stable retained austenite.)
[0096]
[0097] The above unstable residual austenite can be defined as the difference between the fraction of residual austenite before the tensile test and the fraction of residual austenite after the tensile test, after measuring the fraction of residual austenite in the grip portion of the tensile specimen before and after the tensile test, and the above stable residual austenite can be defined as the fraction of residual austenite after the tensile test. The pressure applied to the grip portion during the tensile test may be 250 N. The fraction of residual austenite can be measured through XRD peak analysis. In order to have good bending properties, the proportion of stable residual austenite that is maintained as austenite even when a small deformation is applied must be high compared to the unstable residual austenite that is easily transformed into martensite when a small deformation is applied.
[0098]
[0099] As described above, the cold rolled steel sheet according to the present invention can satisfy the following relationship 2.
[0100] [Relationship 2] 4×P.El - U.El ≥ 13.0
[0101] (However, in the above relational expression 2, P.El means local elongation, and U.El means uniform elongation.)
[0102]
[0103] In a tensile test of a steel plate, the material deforms relatively uniformly from the start of the tensile test until the flow stress reaches the tensile strength (TS). However, after the tensile strength (TS), which corresponds to the maximum flow stress that the steel plate can support, the deformation non-uniformity between the microstructures within the material increases, and it is known that it goes through the process of void creation, coalescence, and macroscopic fracture at the phase boundary. The final fracture process of the material during a tensile test can be represented by the local elongation value, and the extreme surface area where fracture occurs during a bending test is also a process in which the material fractures due to high strain, and it was found to be closely related to the local elongation. Therefore, the local elongation and bending characteristics in a tensile test are closely related. Accordingly, the inventors of the present invention were able to find that the local elongation (post-elongation) increases when the hardness difference between phases is reduced by controlling the phase fraction of the microstructure and the alloy composition range is controlled by suppressing excessive alloy addition. Meanwhile, when the fraction of retained austenite is high, the uniform elongation of the material increases, but when the deformation reaches the tensile strength, some of the retained austenite is transformed into high-carbon martensite, which deteriorates the bending properties. From these results, it was found that the bending properties of the steel sheet can be improved by limiting the local elongation to be high and the uniform elongation to be relatively low, as in the above relational expression 2. If the value of the above relational expression 2 is less than 13.0, the bending properties may be inferior, and the bending formability (R) may be 2.5 or less. min / t) may be difficult to obtain. Meanwhile, total elongation (T.El) can be measured through a tensile test, and the total nominal strain until the specimen breaks is called total elongation (T.El). The total elongation (T.El) can be divided into uniform elongation (U.El) until the tensile strength is reached and local elongation (P.El) until the final break thereafter.
[0104]
[0105] The above cold rolled steel sheet has a tensile strength of 1470 MPa or more, a yield strength of 1000 MPa or more, a total elongation (T.El) of 8.5% or more, and a bending formability (R) of 2.5 or less. min / t). In the present invention, the higher the tensile strength, yield strength and total elongation, the more preferable it is, so there is no limitation on the upper limit, but the tensile strength is unlikely to exceed 1650 MPa, the yield strength is unlikely to exceed 1300 MPa, and the total elongation is unlikely to exceed 16%. In addition, in the present invention, the bending formability (R min / t) is desirable, the lower the value, the more preferable it is, so there is no limitation on the lower limit, but as an example, the bending formability (R min The lower limit of / t) may be 0.8. Meanwhile, the bending formability (R min / t) in R min refers to the minimum punch radius of curvature at which no cracks occur when a 90-degree V-bending bending test is performed using punches with various radius of curvature (R), and t refers to the thickness of the steel plate (mm). When bending is performed using a 90-degree V-bending die, if the bending is possible with an acute-angle punch with a small R value, the bending properties of the material can be considered better, and therefore, the minimum R value (R) at which no cracks occur min ) is smaller, the better the bending properties of the material. On the other hand, R min The value is affected by the thickness of the material being tested, and the thicker the material, the smaller the R minIt is usually R because it is difficult to have a value min The bending characteristics are represented by the ratio of the value and the thickness t.
[0106]
[0107] Hereinafter, a method for manufacturing a cold-rolled steel sheet according to one embodiment of the present invention will be described.
[0108]
[0109] First, the slab having the above-mentioned alloy composition is heated. The slab heating temperature may be 1150 to 1250°C. If the slab heating temperature is lower than 1150°C, hot rolling, which is the next step, may not be possible. On the other hand, if it exceeds 1250°C, a lot of energy is unnecessarily consumed to raise the slab temperature. Therefore, the slab heating temperature is preferably in the range of 1150 to 1250°C. Considering the condition temperature of the hot rolling process, the lower limit of the slab heating temperature is more preferably 1170°C, and even more preferably 1180°C. In terms of reducing cost and energy consumption, the upper limit of the slab heating temperature is more preferably 1230°C, and even more preferably 1220°C.
[0110]
[0111] Thereafter, the heated slab is subjected to finish hot rolling at 830 to 950°C to obtain a hot-rolled steel sheet. If the finish hot rolling temperature (hereinafter also referred to as 'FDT') is less than 830°C, the rolling load becomes large and shape defects increase, resulting in poor productivity. On the other hand, if the finish hot rolling temperature exceeds 950°C, the surface quality deteriorates due to an increase in oxides caused by excessive high-temperature work. Therefore, the finish hot rolling temperature is preferably in the range of 830 to 950°C. In terms of the aforementioned productivity, the lower limit of the finish hot rolling temperature is more preferably 850°C, and more preferably 880°C. In terms of securing surface quality, the upper limit of the finish hot rolling temperature is more preferably 930°C, and more preferably 910°C.
[0112]
[0113] Thereafter, the hot-rolled steel sheet is coiled at 400 to 650°C. If the coiling temperature (hereinafter also referred to as 'CT') exceeds 650°C, there is a disadvantage that coarse internal hot-rolled oxidation occurs and surface properties deteriorate, and if the coiling temperature is lower than 400°C, it corresponds to the transition boiling range, so the controllability of the coiling temperature deteriorates and the shape of the steel sheet deteriorates, which has a disadvantage that the shape of the steel sheet deteriorates. In order to prevent the above-mentioned problems, the lower limit of the coiling temperature is more preferably 440°C, and the upper limit of the coiling temperature is more preferably 610°C, and the upper limit of the coiling temperature is more preferably 570°C.
[0114]
[0115] Thereafter, the coiled hot-rolled steel sheet is cold-rolled to obtain a cold-rolled steel sheet. During the cold rolling, the cold reduction ratio may be 30 to 60%. If the cold reduction ratio is less than 30%, it may be difficult to secure the target thickness precision and shape correction of the steel sheet may also become difficult. On the other hand, if the cold reduction ratio exceeds 60%, the possibility of cracks occurring at the edge of the steel sheet increases and the cold-rolling load may become excessively large. Therefore, the cold reduction ratio may have a range of 30 to 60%.
[0116]
[0117] Thereafter, the cold-rolled steel sheet is continuously annealed at 800 to 950°C. If the continuous annealing temperature (hereinafter also referred to as 'SS') is less than 800°C, sufficient austenite reverse transformation may not occur, and there is a concern that a ferrite phase may be formed at a level exceeding 15% after annealing. On the other hand, if the continuous annealing temperature exceeds 950°C, the surface quality and productivity may deteriorate, and coarse austenite may be formed, resulting in material deterioration. The lower limit of the continuous annealing temperature is more preferably 820°C, and even more preferably 840°C. The upper limit of the continuous annealing temperature is more preferably 930°C, and even more preferably 900°C.
[0118]
[0119] Thereafter, the continuously annealed cold rolled steel sheet is first cooled to a first cooling end temperature (hereinafter referred to as 'SCS') of 500 to 700°C at an average cooling rate of 1°C / s or more and less than 10°C / s. The first cooling end temperature can be defined as the point in time at which a rapid cooling facility that was not applied in the first cooling is additionally applied and the second cooling (rapid cooling) is initiated. If the cooling process is divided into first and second cooling and performed in stages, the temperature distribution of the steel sheet can be made uniform in the slow cooling stage, thereby reducing the final temperature and material deviation. If the first cooling end temperature is less than 500°C, there is a concern that soft bainite transformation may be induced, and it is also difficult to cool to less than 500°C at a cooling rate of less than 10°C / s due to the actual equipment length. If the first cooling end temperature exceeds 700°C, the cooling amount to the second cooling end temperature becomes large, resulting in a poor shape of the steel sheet. Meanwhile, when the primary cooling rate is less than 1°C / s, a ferrite phase is formed during cooling, making it difficult to obtain high-strength steel, and when it is 10°C / s or more, the cooling amount in the secondary cooling increases, resulting in an increase in the final temperature deviation and material deviation. Therefore, it is preferable that the primary cooling rate be in the range of 1°C / s or more and less than 10°C / s. The lower limit of the primary cooling rate is more preferably 2°C / s, and more preferably 3°C / s. The upper limit of the primary cooling rate is more preferably 7°C / s, and more preferably 5°C / s.
[0120]
[0121] Thereafter, the first-cooled cold-rolled steel sheet is secondarily cooled at an average cooling rate of 10°C / s or more to a second cooling end temperature (hereinafter referred to as 'RCS') of 25 to 300°C. The second cooling end temperature is set to ensure that the temperature of the steel sheet is lower than Ms so that martensite transformation occurs during cooling, and this martensite ultimately becomes tempered martensite through a subsequent reheating step. It is difficult to cool the second cooling end temperature to below 25°C, which is lower than room temperature. On the other hand, when the second cooling end temperature exceeds 300°C, martensite is not sufficiently generated during cooling, making it difficult to obtain sufficient yield strength, tensile strength, and bending formability. If the secondary cooling rate is less than 10°C / s, even if the target secondary cooling end temperature is reached, a high-temperature phase such as upper bainite is mixed in during cooling, making it impossible to obtain the target tempered martensite fraction and high strength. Meanwhile, in the present invention, a faster secondary cooling rate is advantageous, and therefore, there is no particular limitation on the upper limit thereof; however, it is difficult to exceed 100°C / s due to limitations in equipment.
[0122]
[0123] Thereafter, the secondarily cooled cold-rolled steel sheet is heated at 150 to 450°C and maintained for more than 500 seconds and less than 1,500 seconds. Through the above process, the interphase carbon distribution and additional phase transformation necessary for stabilizing the retained austenite are obtained. In the present invention, the end point temperature of the heating section is conveniently referred to as the reheating temperature (hereinafter, also referred to as 'RHS'), and the end point temperature of the holding section is conveniently referred to as the overaging temperature (hereinafter, also referred to as 'OAS'). If the RHS or OAS temperature is less than 150°C, the strength becomes excessively high and the formability deteriorates, whereas, if the RHS or OAS temperature exceeds 450°C, it is difficult to obtain the high strength desired by the present invention. If the holding time in the holding section is less than 500 seconds, the total phase transformation amount is insufficient at the end of the holding step, so that the retained austenite fraction increases and a lot of fresh martensite is generated, which may deteriorate the bending characteristics. In addition, the value of the above relational expression 1 may exceed 2.0. The lower limit of the above holding time is more preferably 600 seconds, and even more preferably 700 seconds. The upper limit of the above holding time is more preferably 1300 seconds, and even more preferably 1000 seconds. Meanwhile, the holding time in the above holding section refers to the time required from the end point of the heating section to the end point of the holding section.
[0124]
[0125] Hereinafter, the present invention will be described in more detail through examples. However, it should be noted that the following examples are intended only to illustrate and concretize the present invention and are not intended to limit the scope of the invention. This is because the scope of the invention is determined by the matters set forth in the patent claims and matters reasonably inferred therefrom.
[0126]
[0127] (Example)
[0128] Cold rolled steel sheets were manufactured by performing slab heating, hot rolling, coiling, cold rolling, annealing, primary cooling, secondary cooling, reheating, and maintenance processes on slabs having the alloy compositions described in Tables 1 and 2 below under the conditions described in Tables 3 and 4 below. Meanwhile, the conditions described in Tables 3 and 4 below were based on the surface temperature of the steel sheets.
[0129]
[0130] The microstructure and mechanical properties of the cold-rolled steel sheet manufactured in this manner were measured, and the results are shown in Tables 5 and 6 below.
[0131]
[0132] The microstructure was measured using the point counting method from photographs observed using a scanning electron microscope (SEM), and in particular, the fraction of retained austenite was measured using XRD. The average grain size of retained austenite was measured using EBSD analysis.
[0133]
[0134] Tensile strength (TS), yield strength (YS), and total elongation (T.El) were measured by taking specimens perpendicular to the rolling direction for cold-rolled steel sheets and then performing a tensile test on the specimens. In addition, total elongation (T.El) was divided into uniform elongation (U.El) until the tensile strength was reached and local elongation (P.El) until the final fracture thereafter. In the tensile test, No. 5 tensile test specimens of the KS B0801 standard were used, with a gauge length of 50 mm and a width of the tensile test section of 25 mm. The elongation in the tensile test was measured as the so-called nominal strain, which is calculated by dividing the amount by which the specimen was elongated by the initial gauge length (50 mm), and the total nominal strain until the fracture of the specimen occurred is called total elongation (T.El). Strength is measured by the so-called nominal stress, which is calculated by dividing the load measured during the tensile test by the initial cross-section of the specimen, and the stress value when this nominal stress reaches its maximum value is called the tensile strength (TS). Here, the uniform elongation (U.El) refers to the nominal strain value when the nominal stress reaches the tensile strength (TS), and the local elongation (P.El) refers to the nominal strain amount from when the tensile strength is reached until the final fracture occurs. In other words, the total elongation is the sum of the uniform elongation and the local elongation.
[0135]
[0136] The bending properties are the minimum R values that do not cause cracks when the surface of the cold-rolled steel plate is observed with a magnifying glass at 1000x magnification after a 90-degree V-bending test. min / t value was obtained. At this time, a 90-degree V-bending bending test method was used in which a steel plate of a certain thickness (t) was placed between 90-degree V-shaped dies and the punch and die were brought into close contact after preparing 90-degree punches with different radii (R).
[0137]
[0138] Steel alloy composition (weight %) CSiMnAlMoTiBCrA0.2371.932.540.03820.0570.0230.00240.03B0.2791.942.630.04730.1030.0220.00230.02C0.1701.482.620.01920.0070.0200 .00130.28D0.2461.962.500.20400.1130.0250.00240.01E0.2702.322.550.046 00.1030.0240.00160.02F0.1970.952.610.02060.1080.0190.00220.01G0.2400 .942.220.03080.1010.0220.00220.02H0.2401.912.470.02300.1060.0210.002 00.01I0.3351.972.520.04400.1080.0220.00200.01J0.4102.002.470.03900.0 020.0190.00190.02K0.1761.512.580.04400.0500.0210.00220.47L0.1911.902 .580.04300.1030.0210.00230.02M0.3911.982.460.04680.1100.0240.00220.01
[0139]
[0140] Steel alloy composition (weight %)NbPSNCuNiVA0.0010.01200.00170.00350.0320.0110.003B0.0190.01030.00220.00370.0070.0050.001C0.0050.00820.00180.00430.0250.00 70.005D0.0190.01070.00240.00440.0410.0140.004E0.0180.00950.00200.0 0320.0230.0210.003F0.0190.00850.00190.00490.0170.0050.002G0.0180.0 0950.00190.00290.0330.0150.001H0.0180.00850.00280.00300.0270.0040. 003I0.0030.00970.00260.00340.0210.0030.004J0.0060.00900.00290.0044 0.0340.0080.005K0.0030.00800.00090.00330.0160.0130.006L0.0200.0089 0.00210.00490.0120.0110.011M0.0190.01030.00220.00470.0370.0220.007
[0141]
[0142] ClassificationSteel gradeSlab heating temperature(℃)Finishing hot rolling temperature(FDT)(℃)Hot rolled steel sheet thickness(mm)Coiling temperature(CT)(℃)Cold reduction ratio(%)Cold rolled steel sheet thickness(mm)Continuous annealing temperature(SS)(℃)Invention example 1A11789123.2624561.4867Invention example 2B12119272.8605501.4823Invention example 3C12239132.5557361.6850Invention example 4D11938822.3540391.0878Invention example 5E11978702.2492361.4 865 Invention Example 6F12188462.0447401.2873 Invention Example 7G11828512.1633331.4882 Invention Example 7H12019042.3582391.4871 Comparative Example 1I12118992.5577441.4892 Comparative Example 2J11939122.4630501.2867 Comparative Example 3K12318812.1442521.0838 Comparative Example 4L12428422.1438331.4821 Comparative Example 5M11878952.6644461.4888
[0143]
[0144] Classification Steel grade 1st cooling end temperature (SCS) (℃) 1st average cooling rate (℃ / s) 2nd cooling end temperature (RCS) (℃) 2nd average cooling rate (℃ / s) Heating section end point temperature (RHS) (℃) Maintenance section end point temperature (OAS) (℃) Maintenance time (sec) Invention example 1A6023.815535403402695 Invention example 2B5884.41473841140735 Invention example 3C5924.43548212202596 Invention example 4D5784.619633318262625 Invention example 5E6475.1140473053111092 Invention example 6F6284.121 239247252811 Invention Example 7G6063.224541298261754 Invention Example 8H6202.824832296292621 Comparative Example 1I5973.722138412372622 Comparative Example 2J5923.419842411366592 Comparative Example 3K6054.732127462452545 Comparative Example 4L6025.224628398403425 Comparative Example 5M5773.519735388372550
[0145]
[0146] Classification Microstructure Fraction (Area %) RA Characteristics FTM FMBRA Average Grain Size (㎛) Formula 1 Invention Example 11.29 2.30.3 1.05.20.3 21.2 Invention Example 28.47 8.02.20.2 11.20.3 11.4 Invention Example 311.187.60.20.20.90.27 0.8 Invention Example 45.68 8.90.50.24.80.45 1.5 Invention Example 53.188.50.31.86.30.3 1.1 Invention Example 60.39 3.61.52.52.10.4 10.9 Invention Example 71.19 1.13.50.5 3.80.441.6Invention Example 82.980.13.81.711.50.481.4Comparative Example 11.572.92.55.617.50.662.1Comparative Example 20.469.14.36.719.50.723.1Comparative Example 310.849.79.523.56.50.542.4Comparative Example 422.362.48.75.41.20.652.3Comparative Example 50.367.23.810.218.50.772.9F: Ferrite, RM: Tempered Martensite, FM: Fresh Martensite, B: Bainite, RA: Retained Austenite [Formula 1] (RA unstable +RA stable ) / RA stable (However, in the above formula 1, RA unstable refers to the fraction of retained austenite after tensile test, and RA stable refers to the fraction of retained austenite before tensile test.)
[0147]
[0148] Classification YS(MPa) TS(MPa) T.El(%) U.El(%) P.El(%) R min / t type 2 invention example 1 1 3 6 1 1 5 0 6 8.9 2.46.5 1.8 2.3.6 invention example 2 1 4 3 5 1 5 4 6 12.45.6 6.82.5 2.1.6 invention example 3 1 1 7 8 1 4 9 6 10.24.75.52.5 1.7.3 invention example 4 1 1 0 2 1 5 7 2 12.77.05.72.5 1.5.8 invention example 5 1 3 7 0 1 7 0 7 10.35.35.02.5 1.4.7 invention example 6 1 0 5 7 1 5 0 2 10.25.44.82.0 1.3.8 invention example 7 1 1 0 2 1 4 7 9 1 0.05.44.62.413.0Invention Example 81042149311.76.65.12.113.8Comparative Example 11158152416.712.64.12.93.8Comparative Example 21121154018.914.74.23.22.1Comparative Example 377415096.24.71.52.81.3Comparative Example 472214958.46.81.64.3-0.4Comparative Example 51006154317.914.53.45.7-0.9[Formula 2] 4×P.El - U.El
[0149]
[0150] As can be seen from Tables 1 to 6 above, in the case of Invention Examples 1 to 8 that satisfy the alloy composition and manufacturing conditions proposed by the present invention, it can be seen that excellent mechanical properties are secured by securing the microstructure that the present invention seeks to obtain.
[0151]
[0152] In the case of Comparative Examples 1, 2 and 5, the manufacturing conditions proposed by the present invention are satisfied, but since the alloy composition is not satisfied, the microstructure sought by the present invention is not secured, and as a result, it can be seen that the mechanical properties are inferior.
[0153]
[0154] In the case of Comparative Examples 3 and 4, the alloy composition proposed by the present invention is satisfied, but since the manufacturing conditions are not satisfied, the microstructure sought by the present invention is not secured, and as a result, it can be seen that the mechanical properties are inferior.
Claims
1. In weight%, C: 0.15% or more and less than 0.30%, Si: 0.8~2.5%, Al: 0.005~0.3%, Mn: 2.0~3.0%, Cr: 0.001~0.5%, Mo: 0.001~0.2%, B: 0.0005~0.0050%, Nb: 0.001~0.05%, Ti: 0.001~0.05%, P: 0.04% or less (excluding 0%), S: 0.01% or less (excluding 0%), N: 0.01% or less (excluding 0%), the remainder including Fe and other unavoidable impurities. The microstructure is composed of area%, ferrite: 15% or less (excluding 0%), fresh martensite: 5% or less (excluding 0%), tempered martensite: 75% or more but less than 95%, retained austenite: 12% or less (excluding 0%), and the remainder bainite. Cold rolled steel sheet satisfying the following relationship 1. [Formula 1] (RA unstable +RA stable ) / RA stable ≤ 2.0 (However, in the above relational expression 1, RA unstable means the fraction of unstable retained austenite, and RA stable refers to the fraction of stable retained austenite.) 2. In claim 1, The above cold-rolled steel sheet is a cold-rolled steel sheet additionally containing at least one of Cu: 0.1% or less (excluding 0%) and Ni: 0.1% or less (excluding 0%).
3. In claim 1, The above cold rolled steel sheet is a cold rolled steel sheet additionally containing V: 0.05% or less (excluding 0%).
4. In claim 1, The above-mentioned residual austenite is a cold-rolled steel sheet having an average grain size of 0.5㎛ or less.
5. In claim 1, The above cold rolled steel sheet is a cold rolled steel sheet that satisfies the following relationship 2. [Relationship 2] 4×P.El - U.El ≥ 13.0 (However, in the above relational expression 2, P.El means local elongation, and U.El means uniform elongation.) 6. In claim 1, The above cold rolled steel sheet has a tensile strength of 1470 MPa or more, a yield strength of 1000 MPa or more, a total elongation (T.El) of 8.5% or more, and a bending formability (R) of 2.5 or less. min Cold rolled steel sheet having / t).
7. A step of heating a slab containing, by weight%, C: 0.15% or more and less than 0.30%, Si: 0.8 to 2.5%, Al: 0.005 to 0.3%, Mn: 2.0 to 3.0%, Cr: 0.001 to 0.5%, Mo: 0.001 to 0.2%, B: 0.0005 to 0.0050%, Nb: 0.001 to 0.05%, Ti: 0.001 to 0.05%, P: 0.04% or less (excluding 0%), S: 0.01% or less (excluding 0%), N: 0.01% or less (excluding 0%), the remainder Fe and other unavoidable impurities; A step of obtaining a hot-rolled steel sheet by finishing hot rolling the above-mentioned heated slab at 830 to 950°C; A step of coiling the above hot-rolled steel sheet at 400 to 650°C; A step of cold rolling the above-mentioned hot-rolled steel sheet to obtain a cold-rolled steel sheet; A step of continuously annealing the above cold rolled steel sheet at 800 to 950°C; A step of first cooling the continuously annealed cold rolled steel sheet to a first cooling end temperature of 500 to 700°C at an average cooling rate of 1°C / s or more and less than 10°C / s; A step of secondary cooling the first-cooled cold-rolled steel sheet at an average cooling rate of 10°C / s or more to a secondary cooling end temperature of 25 to 300°C; and A method for manufacturing a cold-rolled steel sheet, comprising: a step of reheating the secondarily cooled cold-rolled steel sheet at 150 to 450°C and then maintaining the temperature for more than 500 seconds and less than 1,500 seconds.
8. In claim 7, A method for manufacturing a cold-rolled steel sheet, wherein the above slab additionally contains at least one of Cu: 0.1% or less (excluding 0%) and Ni: 0.1% or less (excluding 0%).
9. In claim 7, The above slab is a method for manufacturing a cold rolled steel sheet additionally containing V: 0.05% or less (excluding 0%).
10. In claim 7, A method for manufacturing cold rolled steel sheets in which the heating temperature of the above slab is 1150 to 1250°C.
11. In claim 7, A method for manufacturing a cold rolled steel sheet having a cold rolling reduction ratio of 30 to 60% during the above cold rolling.