Transfer-type sheet-shaped bonding material

MYPI2025003535A0Undetermined Publication Date: 2024-07-12NIPPON SANSO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025003535
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-01-12
Filing Date
2023-10-24
Publication Date
2024-07-12

AI Technical Summary

Technical Problem

Conventional sheet-like bonding materials face issues with cracking, poor transferability under mild conditions, and insufficient bonding strength at low temperatures, especially when using copper particles, which are prone to sintering and surface activity impairment at high transfer temperatures.

Method used

A transfer-type sheet-like bonding material is developed with a glass transition point of -35°C to 25°C, containing copper particles, a reducing agent, an acrylic resin, and a plasticizer, optimized to suppress cracking and ensure excellent transferability and bonding strength at temperatures of 250°C or lower by controlling the copper particle size and surface characteristics.

Benefits of technology

The material effectively suppresses cracking, achieves excellent transferability under mild conditions, and ensures sufficient bonding strength at low temperatures, enhancing the reliability and performance of copper-based bonding in electronic components.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Provided is a transfer-type sheet-shaped bonding material with which (I) cracking is sufficiently suppressed, (II) excellent transferability is achieved even with mild transfer conditions under which sintering of copper particles does not proceed, and (III) sufficient bonding strength can be ensured even in low-temperature bonding at 250C or lower. The transfer-type sheet-shaped bonding material is obtained through application and drying, on a resin substrate, of a paste that contains copper particles, a reductant, an organic material including a resin and optionally including a plasticizer, and a solvent. The transfer-type sheet-shaped bonding material has a glass-transition point of not lower than 35C and not higher than 25C.
Need to check novelty before this filing date? Find Prior Art

Description

Transfer-type sheet adhesive material

[0001] The present invention relates to a transfer type sheet-like bonding material.

[0002] Conventionally, solder materials have been widely used as bonding materials for electronic components. However, solder materials have a problem of poor heat resistance. Therefore, for example, it has been difficult to use solder materials as bonding materials in power devices using SiC elements that are expected to be used at high temperatures of 150°C or higher.

[0003] Therefore, a bonding material using silver particles has been proposed as a sintered bonding material. In addition, copper particles are expected to be a promising option from the viewpoints of cost and ion migration, and the development of a transfer-type sheet-type bonding material using copper particles is underway.

[0004] The transfer-type sheet-like bonding material is formed by applying a paste containing at least copper particles, a reducing agent, a resin, and a solvent onto a resin substrate such as a release PET film and drying it. Bonding of two members (a first member and a second member) using the transfer-type sheet-like bonding material is performed as follows: First, the sheet-like bonding material is transferred to the first member under predetermined transfer conditions, and then the resin substrate is peeled off. Next, the sheet-like bonding material transferred to the first member is brought into contact with the second member, and the first member and the second member are bonded via the sheet-like bonding material under predetermined bonding conditions.

[0005] Patent Document 1 describes a sheet-like bonding material obtained by applying a paste containing copper particles (D10: 100 nm or more, D90: 2000 nm or less) surface-coated with triethanolamine as a capping agent, dicarboxylic acid as an activator, a dispersant, epoxy methacrylate urethane as a binder, and terpineol as an organic solvent to a PET film and drying the paste. Patent Document 1 also describes that this sheet-like bonding material can be transferred to an Au-plated silicon die under transfer conditions of a transfer temperature of 200 to 225°C, a pressure of 5 MPa, and a transfer time of 1 to 10 seconds.

[0006] Special Publication No. 2021-529258

[0007] However, according to the inventors' investigations, although the epoxy methacrylate urethane resin described in Patent Document 1 does not exist, it has been found that in any case, with existing sheet-like bonding materials, cracks occur in the dried film due to the resin components contained in the sheet-like bonding material (paste dried film).

[0008] In addition, in Patent Document 1, since the transfer temperature is 200°C or higher, copper sinters during transfer, impairing the surface activity of the copper particles, which may impair the sintering of copper and the atomic diffusion into the joined material during subsequent joining, resulting in a problem that sinterability and atomic diffusion (joinability) tend to become unstable. If transfer is performed under gentle transfer conditions that do not cause sintering of copper particles, there are problems such as the sheet-shaped bonding material not being able to be transferred to the entire surface of the transferred material, or residues of the dried paste film (transfer-type sheet-shaped bonding material) remaining on the resin substrate.

[0009] Furthermore, although the sheet-shaped bonding material of Patent Document 1 allows low-temperature bonding at a bonding temperature of 250° C. or less, there is also the problem that it is difficult to ensure sufficient bonding strength.

[0010] In view of the above problems, the present invention aims to provide a transfer-type sheet-like bonding material that (I) sufficiently suppresses cracking, (II) provides excellent transferability even under gentle transfer conditions in which sintering of copper particles does not progress, and (III) ensures sufficient bonding strength even at low-temperature bonding of 250°C or less.

[0011] In order to solve the above problems, the present inventors have conducted extensive research and have found that the above problems (I) to (III) can be solved by optimizing the glass transition point of a transfer type sheet-like bonding material obtained by applying a paste containing copper particles, a reducing agent, an organic material containing a resin and optionally a plasticizer, and a solvent onto a resin substrate and drying the paste.

[0012] The gist of the present invention, which was completed based on the above findings, is as follows: [1] A transfer-type sheet-like bonding material, which is obtained by applying a paste containing copper particles, a reducing agent, an organic material containing a resin and optionally a plasticizer, and a solvent onto a resin substrate and then drying the paste, and which is characterized by having a glass transition temperature of -35°C or higher and 25°C or lower.

[0013] [2] The transfer type sheet-like bonding material according to the above [1], wherein the resin is an acrylic resin.

[0014] [3] The transfer sheet-like bonding material according to the above [1] or [2], wherein the content of the resin is 1.0 parts by mass or more and 5.0 parts by mass or less per 100 parts by mass of copper particles.

[0015] [4] The plasticizer is one or more selected from the group consisting of butylphthalyl butyl glycolate, dimethyl phthalate, dioctyl phthalate, and diisodecyl phthalate. [1] The transfer type sheet-like bonding material according to any one of the above [3] to [4].

[0016] [5] The content of the plasticizer is 10 parts by mass or more and 50 parts by mass or less with respect to 100 parts by mass of the resin. [1] to [4] The transfer type sheet-like bonding material according to any one of the above.

[0017] [6] The transfer sheet-like bonding material according to any one of the above [1] to [5], wherein the reducing agent is triethanolamine.

[0018] [7] The content of the reducing agent is 3 parts by mass or more and 9 parts by mass or less per 100 parts by mass of copper particles. [1] The transfer sheet-like bonding material according to any one of the above [1] to [6].

[0019] [8] The transfer sheet-like bonding material according to any one of [1] to [7] above, wherein the average particle diameter of the copper particles is 70 nm or more and 300 nm or less.

[0020] The transfer-type sheet-like bonding material of the present invention (I) sufficiently suppresses cracking, (II) provides excellent transferability even under gentle transfer conditions where sintering of copper particles does not progress, and (III) ensures sufficient bonding strength even at low-temperature bonding of 250°C or less.

[0021] [Transfer-type sheet-like bonding material] A transfer-type sheet-like bonding material according to one embodiment of the present invention is obtained by applying a paste containing copper particles, a reducing agent, an organic material containing a resin and optionally a plasticizer, and a solvent onto a resin substrate and drying the paste, and is characterized by having a glass transition point of -35°C or higher and 25°C or lower.

[0022] (Copper particles) The copper particles are mainly composed of copper. The copper particles preferably contain 95% by mass or more and 100% by mass or less of copper element relative to 100% by mass of the copper particles, and more preferably 97% by mass or more. When the copper element is contained in an amount of 95% by mass or more, the bonding material has excellent heat resistance and further excellent bonding strength.

[0023] The average particle diameter of the copper particles is preferably 300 nm or less. When the average particle diameter of the copper particles is 300 nm or less, a sufficiently high bonding strength can be ensured even at low-temperature bonding at 250°C or less. The average particle diameter of the copper particles is more preferably 150 nm or less. Furthermore, the average particle diameter of the copper particles is preferably 5 nm or more. When the average particle diameter of the copper particles is 5 nm or more, copper microparticles are easily available. The average particle diameter of the copper particles is more preferably 70 nm or more. When the average particle diameter of the copper particles is 70 nm or more, a sufficiently high bonding strength can be ensured even at low-temperature bonding at 250°C or less.

[0024] The shape (form) of the copper particles is not particularly limited. Examples of the shape of the copper particles include spherical (sphere), ellipsoid (ellipsoid), and plate-like shapes. Among these, spherical and ellipsoid shapes are preferred, and spherical shapes are more preferred.

[0025] The average particle size of copper particles can be determined by observing 10 fields of view at 10,000x magnification using a scanning electron microscope (SEM). The particle size of each copper particle in the 10 fields of view was measured for all copper particles selected according to the following selection criteria (1) to (5), and the resulting D50 was calculated. For particles that are not perfectly round, such as ellipses, the major axis was used as the particle size. The particle size distribution of copper particles was also determined based on the particle sizes of all copper particles measured. When determining the average particle size and particle size distribution of copper particles in a sheet-like bonding material, the outermost surface of the sheet was observed. In the powder state before sheet production, the powder was placed on carbon tape with a spatula, excess powder was removed with an air duster, and the tape surface was observed. (1) Particles with parts outside the field of view of the image were not measured. (2) Particles with clear outlines and isolated locations were measured. (3) Even if particles deviate from the average particle shape, particles that are independent and can be measured as individual particles were measured. (4) If particles overlap but the boundaries between them are clear and the overall shape of the particle can be determined, measure each particle as a single particle. (5) If particles overlap but the boundaries are unclear and the overall shape of the particle cannot be determined, do not measure them as their shape cannot be determined.

[0026] It is preferable to use copper particles that do not require a protective agent, a dispersant, etc. An example of such copper particles is ultrafine metal powder obtained by the manufacturing method described in Japanese Patent No. 4304221. However, the copper particles are not limited to this example.

[0027] The copper particles preferably have a coating containing copper carbonate on the surface. By having a coating containing copper carbonate on the surface of the copper particles, the sintering temperature of the copper particles can be kept lower than conventionally while increasing the bonding strength. The coating containing copper carbonate may further contain cuprous oxide.

[0028] It is preferable to use copper particles that are not coated with an organic protective film. When the copper particles are coated with an organic protective film, sintering of the copper particles does not proceed unless the organic protective film is decomposed. Therefore, a bonding temperature higher than the decomposition temperature of the organic protective film is required, and low-temperature bonding at 250°C or lower may not be possible. In addition, decomposition gases from the organic protective film may form voids in the bonding layer or cracks may occur in the bonding layer, resulting in a risk of reduced reliability.

[0029] The ratio of the mass oxygen concentration to the specific surface area of ​​the copper particles is set to 0.1 mass% g / m from the viewpoint of reducing the reactivity with oxygen in the air and reducing the influence of reoxidation. 2 It is preferable that the content is 0.2 mass% g / m or more. 2 On the other hand, the ratio of the mass oxygen concentration to the specific surface area of ​​the copper particles is preferably 1.2 mass% g / m or more from the viewpoint of facilitating removal of the oxide film during bonding and further increasing the bonding strength. 2 It is preferable that the content is 0.5 mass% g / m or less. 2 More preferably, it is:

[0030] The ratio of the mass carbon concentration to the specific surface area of ​​the copper particles is set to 0.3 mass% g / m from the viewpoint of suppressing the occurrence of voids and cracks and further increasing the bonding strength. 2 It is preferable that the content is 0.1 mass% g / m or less. 2 More preferably, it is 0.05 mass% g / m or less. 2 The ratio of the mass carbon concentration to the specific surface area of ​​the copper particles is more preferably 0.008 mass% g / m or less. 2 It is preferable that this is equal to or greater than this.

[0031] The ratio of the mass oxygen concentration to the specific surface area of ​​the copper particles can be calculated from the measured specific surface area and mass oxygen concentration. The specific surface area can be measured using a nitrogen gas BET adsorption device (e.g., "MACSORB HM-1201" manufactured by Mountech Co., Ltd.). The mass oxygen concentration can be measured using an oxygen / nitrogen analyzer (e.g., "TC600" manufactured by LECO Corporation).

[0032] The ratio of the mass carbon concentration to the specific surface area of ​​the copper particles can be calculated from the measured specific surface area and mass carbon concentration. The specific surface area can be measured using a nitrogen gas BET adsorption device (e.g., "MACSORB HM-1201" manufactured by Mountech Co., Ltd.). The mass carbon concentration can be measured using a carbon-sulfur analyzer (e.g., "EMIA-920V" manufactured by Horiba, Ltd.).

[0033] The "copper particle content" in the sheet-shaped bonding material is equivalent to the copper particle content in the paste, and can be determined, for example, by heating the sheet to about 1000°C in a nitrogen atmosphere and determining the weight after heating.

[0034] (Reducing Agent) The reducing agent is a compound that reduces the oxide film that inevitably exists on the surface of the copper particles during bonding. During bonding, the oxide film is removed by the reducing agent, causing the copper particles (pure copper) to come into contact with each other, promoting sintering and diffusion bonding.

[0035] In this embodiment, the reducing agent is preferably triethanolamine, which is highly effective in removing oxide films, has a high boiling point, and is low volatile, so it is not easily removed during transfer, and has high stability over time, so it has excellent storage stability before bonding.

[0036] In this embodiment, the content of the reducing agent is preferably 3 parts by mass or more and 9 parts by mass or less per 100 parts by mass of copper particles. If the content of the reducing agent is 3 parts by mass or more, the amount of reducing agent is sufficient, and even at low-temperature bonding at 250°C or less, the amount of reducing agent is sufficient, and sufficiently high bonding strength can be ensured. Furthermore, if the content of the reducing agent is 9 parts by mass or less, the reducing agent is less likely to seep out during transfer and bonding, and transfer and bonding in the same shape as the bonded material can be achieved. Furthermore, there is no increase in decomposition gas components, and voids and cracks are less likely to occur in the bonding layer.

[0037] The content of the reducing agent in the sheet-like bonding material is the same as the content of the reducing agent in the paste.

[0038] (Organic Material) In this embodiment, the organic material includes a resin and optionally a plasticizer.

[0039] <Resin> The resin functions as an adhesive when the transfer-type bonding sheet is transferred to the first member, and preferably also functions as a dispersant for dispersing the copper particles.

[0040] The resin is preferably a resin such as an acrylic resin or an aliphatic polycarbonate, which is a highly degradable binder. In particular, the resin is preferably an acrylic resin. This is because acrylic resin has an adhesive function and therefore has excellent transferability. Specifically, one or more selected from poly(alkyl methacrylate), poly(alkyl methacrylate), and methacrylic acid ester copolymers can be used.

[0041] In this embodiment, the resin content is preferably 1.0 part by mass or more and 5.0 parts by mass or less per 100 parts by mass of copper particles. If the resin content is less than 1.0 part by mass, cracks are likely to occur in the dried paste film, and excellent transferability is difficult to obtain under gentle transfer conditions in which sintering of the copper particles does not progress. Furthermore, if the resin content exceeds 5.0 parts by mass, decomposable components and undecomposed substances in the binder form voids in the bonding layer, impairing adhesion to the bonded materials, making it impossible to ensure sufficient bonding strength at low temperatures of 250 ° C or less.

[0042] The resin content in the sheet-like bonding material is the same as the resin content in the paste.

[0043] <Plasticizer> The plasticizer lowers the glass transition point of the sheet-shaped bonding material, imparts flexibility to the sheet, and also plays a role in suppressing drying shrinkage of the coating film containing copper particles.

[0044] The plasticizer may be one or more selected from the group consisting of dimethyl phthalate, diethyl phthalate, diallyl phthalate, dibutyl phthalate, diisobutyl phthalate, di-n-hexyl phthalate, bis(2-ethylhexyl) phthalate, dioctyl phthalate, di-n-octyl phthalate, diisononyl phthalate, diisodecyl phthalate, dinonyl phthalate, bisbutylbenzyl phthalate, and butylphthalyl butyl glycolate. In particular, the plasticizer is preferably one or more selected from the group consisting of butylphthalyl butyl glycolate, dimethyl phthalate, dioctyl phthalate, and diisodecyl phthalate.

[0045] In this embodiment, the content of the plasticizer is preferably 10 parts by mass or more and 50 parts by mass or less per 100 parts by mass of the resin. If the content of the plasticizer is less than 10 parts by mass, the plasticizing effect is not fully exerted, so cracks are likely to occur in the dried paste film, and excellent transferability is difficult to obtain under gentle transfer conditions where sintering of the copper particles does not proceed. Furthermore, since the copper particles may sinter during transfer, sufficient bonding strength cannot be ensured at low temperatures of 250 °C or less. Furthermore, if the content of the plasticizer exceeds 50 parts by mass, poor dispersion of the copper particles, binder, and reducing agent in the paste is likely to occur, making it difficult to obtain excellent transferability under gentle transfer conditions where sintering of the copper particles does not proceed, and sufficient bonding strength cannot be ensured at low temperatures of 250 °C or less.

[0046] The content of the plasticizer in the sheet-like bonding material is the same as the content of the plasticizer in the paste.

[0047] <Glass transition point of transfer sheet-like bonding material> It is important that the transfer sheet-like bonding material of this embodiment has a glass transition point of -35 ° C or higher and 25 ° C or lower. By setting the glass transition point of the transfer sheet-like bonding material to 25 ° C or lower, a flexible transfer sheet-like bonding material can be obtained, (I) cracking is sufficiently suppressed, (II) excellent transferability can be obtained even under gentle transfer conditions where sintering of copper particles does not progress, and (III) sufficient bonding strength can be ensured even at low temperatures of 250 ° C or lower. From this perspective, the glass transition point of the transfer sheet-like bonding material is preferably 10 ° C or lower. On the other hand, if the glass transition point of the transfer sheet-like bonding material is too low, it may be impossible to transfer the sheet-like bonding material from the resin substrate. Therefore, the glass transition point of the transfer sheet-like bonding material is -35 ° C or higher, preferably -20 ° C or higher.

[0048] The glass transition point of the transfer type sheet-like bonding material can be controlled mainly by the type of resin and the type and content of the plasticizer.

[0049] The glass transition point of the transfer-type sheet-like bonding material can be determined by peeling the dried paste film (transfer-type sheet-like bonding material) from the resin substrate and subjecting the resulting powder to differential scanning calorimetry. For example, using a differential scanning calorimeter (DSC60) manufactured by Shimadzu Corporation, 20 mg of dried paste powder (70 ° C., 60-minute dried product) is placed in the device, and the measurement range is -50 ° C. to 150 ° C. (heating rate: 10 ° C. / min) under a nitrogen atmosphere (flow rate 50 mL / min). In the DSC thermograph obtained, when the baseline shifts downward due to the glass transition, the midpoint of the displacement from the original baseline can be calculated as the glass transition point.

[0050] (Solvent) The solvent should preferably have a boiling point of about 200°C and low volatility. This is because if the solvent evaporates during paste application and the metal concentration changes, uneven thickness of the coating film will occur. In addition, the solvent must be able to dissolve the resin used. From these perspectives, for example, a terpene-based solvent such as terpineol can be used.

[0051] (Sheet Shape) The bonding material of this embodiment is in the shape of a sheet. The thickness of the bonding material is not particularly limited, and can be, for example, 10 μm or more and less than 1 mm.

[0052] Furthermore, the shape of the joining material (the shape when viewed in a plane from the thickness direction) is not particularly limited and can be selected appropriately depending on the shape of the joining surfaces of the joined members, etc., and examples include rectangular and circular shapes.

[0053] [Method for manufacturing transfer-type sheet-like bonding material] The transfer-type sheet-like bonding material of this embodiment can be produced by applying a paste containing copper particles, a reducing agent, an organic material containing a resin and optionally a plasticizer, and a solvent onto a resin substrate and drying it.

[0054] The method for preparing the paste is not particularly limited, and it can be prepared by mixing the components using a planetary mixer, a mortar, mill stirring, stirrer stirring, or the like. The method for applying and drying the paste onto a resin substrate is also not particularly limited, and for example, a dried paste film can be obtained by applying the paste onto a resin substrate using an applicator and drying the applied film in a hot air oven. Drying conditions can be 50 to 110°C (ambient temperature) and a drying time of 10 to 90 minutes.

[0055] The resin substrate is not particularly limited, and examples thereof include a release PET film, a silicone film, a fluororesin film, etc. The thickness of the resin substrate can be set to about 50 to 200 μm in consideration of release properties.

[0056] The joining of two members (a first member and a second member) using the transfer-type sheet-like joining material is carried out through the following two steps of transfer and joining.

[0057] (Transfer) First, the sheet-like bonding material is bonded to the first member, and then the resin substrate is peeled off. That is, the sheet-like bonding material is transferred to the first member. The conditions for transferring the transfer-type sheet-like bonding material formed on the resin substrate to the first member are not particularly limited, but in this embodiment, excellent transferability can be obtained even under gentle transfer conditions that do not cause sintering of the copper particles, such as a transfer temperature of 150°C or less, a pressure of 10 MPa or less, and a transfer time of 1 minute or less. The transfer conditions can be a transfer temperature of 50 to 150°C, a pressure of 1 to 10 MPa, and a transfer time in the range of 10 seconds to 1 minute. The atmosphere during transfer is nitrogen (N 2 It is preferable to use an inert atmosphere such as a fluorine-containing atmosphere.

[0058] (Bonding) Next, the sheet-like bonding material transferred onto the first member is brought into contact with the second member, and the first member and the second member are bonded via the sheet-like bonding material under predetermined bonding conditions. The bonding conditions are not particularly limited, but in this embodiment, sufficient bonding strength can be ensured even at low temperatures of 250°C or less. The bonding conditions can be in the range of a bonding temperature of 200 to 250°C, a pressure of 1 to 40 MPa, and a transfer time of 1 to 60 minutes. The atmosphere during bonding is nitrogen (N 2 It is preferable to use an inert atmosphere such as a fluorine-containing atmosphere.

[0059] [Production of Transfer-Type Sheet-Like Bonding Material] (Test Example No. 1) 40 g of Taiyo Nippon Sanso copper particles (particle diameter 110 nm product; D10: 39 nm, D50: 112 nm, D90: 310 nm), 3.2 g of triethanolamine as a reducing agent, 1.78 g of acrylic binder (Orikox KC-500, manufactured by Kyoeisha Chemical Co., Ltd.), and 12.2 g of terpineol as a solvent were mixed in a planetary mixer to obtain a paste. The surface layer of the copper particles was coated with cuprous oxide, and the ratio of the mass oxygen concentration to the specific surface area of ​​the copper particles was 0.25 mass% g / m 2 The mass carbon concentration is 0.03 mass% g / m 2 is.

[0060] Next, the prepared paste was applied to a 100 μm-thick release PET film using an applicator to form a coating film of 200 μm thick, and the coating film was dried in a hot air oven at 70 ° C for 60 minutes to remove terpineol, thereby obtaining a paste dried film (transfer-type sheet-like bonding material). The composition of the obtained transfer-type sheet-like bonding material and the glass transition temperature of the transfer-type sheet-like bonding material measured by the above-mentioned method are shown in Table 1.

[0061] (Test Examples Nos. 2 to 26) The copper particle content was fixed at 40 g, and the type of copper particles, the type and content of reducing agent, the type and content of acrylic binder, and the type and content of plasticizer were changed as shown in Table 1, and pastes were obtained in the same manner as Test Example No. 1. The terpineol content was set so that the concentration of copper particles in the paste was 70 mass%. Next, a paste dried film (transfer-type sheet-like bonding material) was obtained in the same manner as Test Example No. 1. The composition of the obtained transfer-type sheet-like bonding material and the glass transition temperature of the organic material measured by the above-mentioned method are shown in Table 1.

[0062] [Evaluation of cracking of paste dried film] In each test example, the paste dried film (transfer-type sheet-like bonding material) was observed under a microscope at a magnification of 20x in 10 visual fields. A case in which there were no cracks in all 10 visual fields was rated as "excellent," and a case in which there were cracks in even one visual field was rated as "poor," as shown in the "Cracking resistance of paste dried film" column in Table 1. In the case of "poor" where the dried film had cracks, the crack pattern and degree could not be controlled, which resulted in variations in the shear strength of the bonded sample after bonding, and therefore subsequent transfer and bonding tests were not performed.

[0063] [Evaluation of Transferability] In each test example, an Au-plated SiC (4 mm square, 350 μm thick) was mounted on a transfer-type sheet-shaped bonding material, and the transfer temperature (atmospheric temperature) was 150° C., the pressure was 10 MPa, the transfer time was 30 seconds, and N 2The transfer sheet bonding material was transferred to the Au-plated surface of SiC under transfer conditions in an ambient atmosphere. The case where the sheet bonding material could be transferred to the entire surface of the SiC and there was no residue of the dried paste film (transfer sheet bonding material) on the release PET film was rated as "excellent," while the case where the sheet bonding material could not be transferred to the entire surface of the SiC or there was residue of the dried paste film (transfer sheet bonding material) on the release PET film was rated as "poor." These results are shown in the "Transferability" column in Table 1. Note that when the transferability was "poor," the shear strength of the bonded samples after bonding varied, so subsequent bonding tests were not performed.

[0064] [Evaluation of shear strength of bonded product] In each test example, the transfer type sheet-shaped bonding material transferred onto SiC was brought into contact with an oxygen-free copper plate C1020 (20 mm square, 2 mm thick), and the bonding was performed in a pressure bonding device at a bonding temperature (atmospheric temperature) of 250°C, a pressure of 10 MPa, a bonding time of 5 minutes, and N 2 A bonded product was produced by bonding a SiC plate and an oxygen-free copper plate via a sheet-shaped bonding material under bonding conditions in an atmosphere. The shear strength of the bonded product was measured using a bond tester (manufactured by Daige, 4000Plus) at a tool height of 100 μm and a tool speed of 200 μm / s, and the results are shown in Table 1. A shear strength of 50 MPa or more is considered good.

[0065] [Evaluation of Exudation of Bonding Layer After Bonding] In each test example, the outer periphery of the SiC in the bonded product was observed at 20x magnification using a microscope (L-KIT504, manufactured by Hozan Corporation) to check for the presence or absence of liquid exudation around the outer periphery of the SiC. The results are shown in Table 1.

[0066]

[0067] *1 110 nm product (D10: 39 nm, D50: 112 nm, D90: 310 nm) 300 nm product (D10: 52 nm, D50: 298 nm, D90: 652 nm) 70 nm product (D10: 24 nm, D50: 72 nm, D90: 284 nm) 100 nm product (D10: 34 nm, D50: 101 nm, D90: 308 nm) 400 nm product (D10: 66 nm, D50: 403 nm, D90: 811 nm) 50 nm product (D10: 15 nm, D50: 51 nm, D90: 194 nm) *2: Reducing agent content (parts by mass) per 100 parts by mass of copper particles *3: Acrylic resin content (parts by mass) in acrylic binder per 100 parts by mass of copper particles *4: Plasticizer content (parts by mass) per 100 parts by mass of acrylic resin

[0068] As is clear from Table 1, in the comparative examples in which the glass transition point of the transfer type sheet-like bonding material was outside the range of -35°C or higher and 25°C or lower, cracks were observed in the dried film, whereas in the inventive examples in which the glass transition point of the transfer type sheet-like bonding material was within the range of -35°C or higher and 25°C or lower, no cracks occurred in the dried film, excellent transferability was obtained even under gentle transfer conditions in which sintering of the copper particles did not progress, and sufficient bonding strength was ensured even at a low temperature of 250°C. In particular, in some of the inventive examples in which the acrylic binder content, the reducing agent content, and the average particle size of the copper particles were optimized, a high shear strength of 50 MPa or higher was obtained.

[0069] The transfer type sheet-like bonding material of the present invention can be industrially used for bonding electronic components. Specifically, it can be used to bond components such as substrates and elements in high-temperature environments where it is difficult to use bonding materials such as solder, such as in electronic devices called power devices.

Claims

1. A transferable sheet-like bonding material characterized by having a glass transition temperature of -35°C or higher and 25°C or lower, which is obtained by applying a paste containing copper particles, a reducing agent, an organic material containing resin and optionally a plasticizer, and a solvent onto a resin substrate and then drying it.

2. The transfer type sheet-like bonding material according to claim 1, wherein the resin is an acrylic resin.

3. A transfer sheet-like bonding material according to claim 1 or 2, wherein the content of the resin is 1.0 part by mass or more and 5.0 parts by mass or less per 100 parts by mass of copper particles.

4. A transferable sheet-like bonding material according to claim 1 or 2, wherein the plasticizer is one or more selected from the group consisting of butylphthalyl butyl glycolate, dimethyl phthalate, dioctyl phthalate, and diisodecyl phthalate.

5. A transfer sheet-like bonding material according to claim 1 or 2, wherein the content of the plasticizer is 10 parts by mass or more and 50 parts by mass or less per 100 parts by mass of the resin.

6. A transferable sheet-like bonding material according to claim 1 or 2, wherein the reducing agent comprises triethanolamine.

7. A transfer-type sheet-like bonding material according to claim 1 or 2, wherein the content of the reducing agent is 3 parts by mass or more and 9 parts by mass or less per 100 parts by mass of copper particles.