Austenitic steel material and manufacturing method therefor

MYPI2025003674A0Undetermined Publication Date: 2024-06-20POHANG IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025003674
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-12-20
Filing Date
2023-12-04
Publication Date
2024-06-20

AI Technical Summary

Technical Problem

Current materials used for ultra-low temperature applications, such as liquefied gas storage and transportation, face challenges with high costs and poor weldability, particularly with aluminum alloys, and economic inefficiencies due to high nickel content in Cr-Ni stainless steel alternatives.

Method used

Development of an austenitic steel with specific composition ranges for manganese, carbon, chromium, and other elements to stabilize austenite microstructure, ensuring excellent cryogenic toughness and weld heat-affected zone properties, including a manufacturing method involving hot rolling and welding processes.

Benefits of technology

The austenitic steel exhibits enhanced cryogenic toughness and structural integrity, meeting safety requirements for ultra-low temperature environments with improved economic viability by controlling microstructure and grain size, thereby ensuring reliable performance and safety in cryogenic structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025003674_DRAWING_001
    Figure PI2025003674_DRAWING_001
Patent Text Reader

Abstract

The present invention relates to an austenitic steel material, and a manufacturing method therefor, and, more specifically, to an austenitic steel material and a manufacturing method therefor, the material being preferably applicable as a structural material used in a cryogenic environment such as that of a liquefied gas storage tank and liquefied gas transportation equipment. FIGURE 1
Need to check novelty before this filing date? Find Prior Art

Description

Austenitic steel and its manufacturing method

[0001] The present invention relates to an austenitic steel and a method for manufacturing the same, and more specifically, to an austenitic steel that can be preferably applied as a structural material used in ultra-low temperature environments such as liquefied gas storage tanks and liquefied gas transport facilities, and a method for manufacturing the same.

[0002]

[0003] Liquefied gases such as liquefied hydrogen (boiling point: -253°C), liquefied natural gas (LNG, boiling point: -164°C), liquefied oxygen (boiling point: -183°C), and liquefied nitrogen (boiling point: -196°C) require ultra-low temperature storage. Therefore, to store these gases, structures such as pressure vessels made of materials with sufficient toughness and strength at ultra-low temperatures are required.

[0004]

[0005] Materials that can be used at low temperatures in liquefied gas atmospheres include Cr-Ni stainless steel alloys such as AISI 304, 9% Ni steel, and 5000 series aluminum alloys. However, aluminum alloys have limited use due to their high alloy cost, low strength, increased design thickness of structures, and poor weldability. Cr-Ni stainless steel and 9% nickel (Ni) steel have improved many of the physical properties of aluminum, but they contain large amounts of expensive nickel (Ni), making them undesirable from an economic perspective.

[0006]

[0007] One aspect of the present invention is to provide an austenitic steel and a method for manufacturing the same.

[0008] A preferred aspect of the present invention is to provide an austenitic steel having excellent ultra-low temperature toughness and a method for manufacturing the same.

[0009]

[0010] One embodiment of the present invention provides an austenitic steel, which comprises manganese (Mn): 10 to 45% by weight, carbon (C): a range satisfying 24×[C]+[Mn]≥25 and 33.5×[C]-[Mn]≤18, chromium (Cr): 10% or less (excluding 0%), and at least one of Cu: 5% or less (excluding 0%), Si: 5% or less (excluding 0%), Al: 5% or less (excluding 0%), Mo: 5% or less (excluding 0%), and B: 0.5% or less (excluding 0%), the remainder being iron (Fe) and unavoidable impurities, and a microstructure in a weld heat-affected zone includes austenite of 95% or more (including 100%) and carbides of 5% or less (including 0%) by area%, and the content of C dissolved in the austenite is 60% or more of the average C content of the steel.

[0011]

[0012] The above austenite may have an average grain size of 10 to 200 μm.

[0013]

[0014] The above weld heat affected zone may have a transverse expansion of 0.32 mm or more after a Charpy impact test at -253°C.

[0015]

[0016] The above welding heat affected zone may have a Charpy impact energy of 27 J or more at -253°C.

[0017]

[0018] Another embodiment of the present invention provides a method for manufacturing an austenitic steel, comprising the steps of: heating a slab containing, in wt%, manganese (Mn): 10 to 45%, carbon (C): a range satisfying 24×[C]+[Mn]≥25 and 33.5×[C]-[Mn]≤18, chromium (Cr): 10% or less (excluding 0%), and at least one of Cu: 5% or less (excluding 0%), Si: 5% or less (excluding 0%), Al: 5% or less (excluding 0%), Mo: 5% or less (excluding 0%), and B: 0.5% or less (excluding 0%), the remainder being iron (Fe) and unavoidable impurities, at 1000 to 1300°C; subjecting the heated slab to a finish hot rolling at 800 to 1050°C to obtain a hot-rolled steel sheet; and welding the hot-rolled steel sheet.

[0019]

[0020] According to one aspect of the present invention, an austenitic steel and a method for manufacturing the same can be provided.

[0021] According to a preferred aspect of the present invention, an austenitic steel having excellent ultra-low temperature toughness and a method for manufacturing the same can be provided.

[0022]

[0023] FIG. 1 is a diagram illustrating the correlation between the carbon content and the manganese content of an austenitic steel according to one aspect of the present invention.

[0024] FIG. 2 is a drawing schematically illustrating a method for measuring the transverse expansion value of an austenitic steel according to one aspect of the present invention.

[0025]

[0026] Hereinafter, an austenitic steel according to one embodiment of the present invention will be described. First, the alloy composition will be described. Unless otherwise specified, the contents of the alloy composition described below are in weight percent.

[0027]

[0028] Manganese (Mn): 10-45%

[0029] Manganese is an element that plays a crucial role in stabilizing austenite. To stabilize austenite at ultra-low temperatures, a manganese (Mn) content of at least 10% is desirable. If the Mn content is below this level, epsilon martensite, a metastable phase, is formed, which easily transforms into alpha martensite through work-induced transformation at ultra-low temperatures, making it difficult to secure toughness. One strategy to suppress epsilon martensite formation is to increase the carbon (C) content to stabilize austenite. However, this can lead to the precipitation of large amounts of carbides, rapidly deteriorating physical properties. Therefore, a manganese (Mn) content of at least 10% is desirable. A more desirable Mn content of at least 15% is preferable, and a more desirable Mn content of at least 18% is preferable. Excessive Mn content can slow the corrosion rate of steel and is not economically feasible. Therefore, the manganese (Mn) content is preferably 45% or less. A more preferable manganese (Mn) content may be 40% or less, and a more preferable manganese (Mn) content may be 35% or less.

[0030]

[0031] Carbon (C): A range satisfying 24×[C]+[Mn]≥25 and 33.5×[C]-[Mn]≤18

[0032] Carbon (C) is an element that stabilizes austenite and increases its strength. In particular, carbon (C) lowers the transformation point Ms or Md from austenite to epsilon or alpha martensite during cooling or processing. Therefore, carbon (C) is an element that effectively contributes to the stabilization of austenite. If the carbon (C) content is insufficient, the stability of austenite is insufficient, making it difficult to obtain stable austenite at ultra-low temperatures. In addition, external stress can easily cause a working-induced transformation into epsilon or alpha martensite, which can reduce the toughness of the steel or lower its strength. On the other hand, if the carbon (C) content is excessive, the toughness of the steel can deteriorate rapidly due to carbide precipitation, and the strength of the steel can increase excessively, lowering its workability.

[0033]

[0034] The inventor of the present invention has conducted an in-depth study on the relative behavior between carbon (C) and manganese (Mn) contents in relation to carbide formation, and as a result, has reached the conclusion that determining the relative content relationship between carbon (C) and manganese (Mn) as shown in Fig. 1 can effectively promote austenite stabilization while effectively controlling the amount of carbide precipitation. Although carbides are formed by carbon (C), carbon (C) does not independently affect the formation of carbides, but rather affects the formation of carbides by acting in combination with manganese (Mn).

[0035]

[0036] In order to stabilize austenite, it is preferable to control the value of 24×[C]+[Mn] (wherein, [C] and [Mn] mean the contents of each component expressed in wt%) to 25 or more, provided that other components satisfy the ranges specified in the present invention. The boundary means the inclined left boundary of the parallelogram region illustrated in Fig. 1. When 24×[C]+[Mn] is less than 25, the stability of austenite decreases, causing work-induced transformation by impact at ultra-low temperatures, which may lower the impact toughness of the steel. On the other hand, in order to suppress the formation of carbides, it is preferable to control the value of 33.5×[C]-[Mn] (wherein, [C] and [Mn] mean the contents of each component expressed in wt%) to 18 or less, provided that other components satisfy the ranges specified in the present invention. When 33.5×[C]-[Mn] exceeds 18, carbides may precipitate due to the excessive addition of carbon (C), which may reduce the low-temperature impact toughness of the steel. Therefore, in the present invention, it is preferable that carbon (C) be added so as to satisfy 24×[C]+[Mn] ≥ 25 and 33.5×[C]-[Mn] ≤ 18. As can be seen in Fig. 1, the lowest limit of the carbon (C) content within the range satisfying the above-mentioned formula is 0%.

[0037]

[0038] Chromium (Cr): 10% or less (excluding 0%)

[0039] Chromium (Cr) is also an austenite stabilizing element. It stabilizes austenite up to an appropriate amount of addition, thereby improving the low-temperature impact toughness of steel, and acts to increase the strength of steel by being dissolved in austenite. In addition, chromium (Cr) is also an element that effectively contributes to improving the corrosion resistance of steel. Therefore, the present invention adds chromium (Cr) as an essential element. The lower limit of the preferable chromium (Cr) content may be 1%, and the more preferable lower limit of the chromium (Cr) content may be 2%. However, chromium (Cr) is a carbide-forming element, and in particular, it may form carbides at austenite grain boundaries, thereby reducing the low-temperature impact toughness of steel. In addition, when the amount of chromium (Cr) added exceeds a certain level, excessive carbides may be precipitated in the heat-affected zone (HAZ) of the weld, which may deteriorate the ultra-low-temperature toughness. Therefore, the upper limit of chromium (Cr) in the present invention may be limited to 10%. The upper limit of the desirable chromium (Cr) content may be 8%, and the upper limit of the more desirable chromium (Cr) content may be 7%.

[0040]

[0041] At least one of Cu: 5% or less (excluding 0%), Si: 5% or less (excluding 0%), Al: 5% or less (excluding 0%), Mo: 5% or less (excluding 0%), and B: 0.5% or less (excluding 0%)

[0042]

[0043] Cu: 5% or less (excluding 0%)

[0044] Copper (Cu) has a very low solubility in carbides and slow diffusion into austenite, so it concentrates at the interface between austenite and nucleated carbides. Therefore, by hindering the diffusion of carbon, it effectively slows down the growth of carbides, ultimately suppressing carbide formation. In addition, copper has the effect of stabilizing austenite and improving ultra-low temperature toughness. However, when the Cu content exceeds 5%, there is a problem of lowering the hot workability of steel, so the upper limit is preferably limited to 5 wt%. The upper limit of the preferable copper (Cu) content may be 3%, and the more preferable upper limit of the copper (Cu) content may be 2%. The lower limit of the preferable copper (Cu) content may be 0.1%, and the more preferable lower limit of the copper (Cu) content may be 0.3%.

[0045]

[0046] Si: 5% or less (excluding 0%)

[0047] Silicon (Si) improves the castability of molten steel and, especially, when added to austenitic steel, it is an element that effectively increases strength by being dissolved in the steel. It is also an element that affects the activity of carbon in steel, effectively suppressing the formation of carbides and increasing toughness. However, when added in excess of 5%, there is a problem that the stacking fault energy is reduced, promoting twinning, and a decrease in toughness may occur due to high strength, so it is desirable to limit the upper limit to 5%. The desirable upper limit of the silicon (Si) content may be 3%, and a more desirable upper limit of the silicon (Si) content may be 2.5%. The desirable lower limit of the silicon (Si) content may be 0.1%, and a more desirable lower limit of the silicon (Si) content may be 0.3%.

[0048]

[0049] Al: 5% or less (excluding 0%)

[0050] Aluminum (Al) is an element that improves the toughness of steel by stabilizing austenite within an appropriate addition range and lowering the transformation points Ms and Md from austenite to epsilon or alpha martensite during the cooling process or working. It is also an element that increases strength by being dissolved in steel, and in particular, it is an element that effectively suppresses carbide formation by affecting the activity of carbon in steel, thereby increasing toughness. In particular, it is well known as an element that effectively increases stacking fault energy and promotes slip. However, when added in excess of 5%, there is a problem of deteriorating the castability and surface quality of steel through the formation of oxides and nitrides, so the upper limit is preferably limited to 5 wt%. The upper limit of the preferable aluminum (Al) content may be 3%, and the upper limit of the more preferable aluminum (Al) content may be 2.5%. The lower limit of the preferable aluminum (Al) content may be 0.2%, and the lower limit of the more preferable aluminum (Al) content may be 0.3%.

[0051]

[0052] Mo: 5% or less (excluding 0%)

[0053] Molybdenum (Mo) is an element that improves the toughness of steel by stabilizing austenite within an appropriate addition range and lowering the transformation points Ms and Md from austenite to epsilon or alpha martensite during the cooling process or working. In addition, it is an element that increases strength when dissolved in steel, and in particular, it is an element that segregates at austenite grain boundaries to increase the stability of the grain boundaries, thereby reducing energy and suppressing grain boundary precipitation of carbonitrides. In addition, molybdenum (Mo) is well known as an element that effectively increases stacking fault energy and promotes slip. However, when added in excess of 5 wt%, it is an expensive element, which reduces economic feasibility and there is a problem that toughness may decrease due to high strength. Therefore, it is recommended that the upper limit be limited to 5 wt%. The upper limit of the desirable molybdenum (Mo) content may be 4.5%, and the upper limit of the more desirable molybdenum (Mo) content may be 4%. The lower limit of the desirable molybdenum (Mo) content may be 0.1%, and the lower limit of the more desirable molybdenum (Mo) content may be 0.3%.

[0054]

[0055] B: 0.5% or less (excluding 0%)

[0056] Boron (B) is a representative element that improves the hardenability of steel. It preferentially segregates at austenite grain boundaries at high temperatures, lowering the energy of the austenite grain boundaries and stabilizing them. Therefore, it improves the hardenability by preventing the formation of undesirable structures such as ferrite and pearlite at the austenite grain boundaries during quenching of carbon steel. Boron (B) also segregates at the austenite grain boundaries of high-manganese steel, lowering the energy of the austenite grain boundaries and preventing carbon diffusion, making it an effective element in suppressing the formation of carbides. However, if added in excess of 0.5 wt%, coarse boron nitrides are formed, which reduces the physical properties. Therefore, the upper limit is preferably limited to 0.5 wt%. The upper limit of the preferred boron (B) content may be 0.4%, and a more preferred upper limit may be 0.3%. The lower limit of the desirable boron (B) content may be 0.0005%, and the lower limit of the more desirable boron (B) content may be 0.001%.

[0057]

[0058] Since structures are typically manufactured by processing and welding steel, even if the ultra-low-temperature impact toughness of the base material itself is secured, if the ultra-low-temperature impact toughness of the weld is not secured, the safety of the structure itself may be significantly reduced. Therefore, the austenitic steel according to one aspect of the present invention seeks to secure ultra-low-temperature impact toughness of the weld heat-affected zone (HAZ) as well as the ultra-low-temperature impact toughness of the base material itself. Accordingly, the present invention controls the microstructure of the weld heat-affected zone as well as the microstructure of the base material within a specific range.

[0059]

[0060] In one aspect of the present invention, an austenitic steel may include a microstructure of 95 area% or more of austenite not only in the base material but also in the heat-affected zone (HAZ) of the weld in order to secure the desired properties. The preferred austenite fraction may be 97 area% or more, and may include a case where the austenite fraction is 100 area%. Meanwhile, in one aspect of the present invention, an austenitic steel may actively suppress the carbide fraction to 5 area% or less in order to prevent a decrease in ultra-low temperature impact toughness. The preferred carbide fraction may be 3 area% or less, and may include a case where the carbide fraction is 0 area%. In the present invention, the method for measuring the austenite fraction and the carbide fraction is not particularly limited, and can be easily confirmed through a measuring method commonly used by a person skilled in the art to which the present invention pertains for measuring microstructure and carbide.

[0061]

[0062] It is preferable that the content of C dissolved in the austenite is 60% or more of the average C content of the steel. When all of the C contained in the steel is dissolved in austenite, the content of C dissolved in the austenite is 100%, and when the C contained in the steel is precipitated as carbide, the content of C dissolved in the austenite is less than 100%. By dissolving a large amount of C in the austenite in this way, the precipitation of carbide can be suppressed, and at the same time, the deterioration of impact toughness can be prevented. The content of C dissolved in the austenite relative to the average C content of the steel is more preferably 70% or more, more preferably 85%, and most preferably 100%. The method for measuring the content of C incorporated into austenite relative to the average C content of the above steel is not particularly limited, and can be easily confirmed through a measuring method commonly used by a person skilled in the art to which the present invention pertains for measuring microstructure and carbide.

[0063]

[0064] The above austenite preferably has an average grain size of 10 to 200 μm. If the average austenite grain size in the weld heat-affected zone (HAZ) is excessively small, the strength of the weld is improved, but localized ultra-low temperature impact toughness degradation may occur in the weld heat-affected zone (HAZ). In addition, since the main precipitation location of carbides is the austenite grain boundary, if the grain size is excessively fine, excessive precipitation of carbides may occur, resulting in a decrease in impact toughness. Therefore, the average austenite grain size in the weld heat-affected zone may be limited to 10 μm or more. Meanwhile, a larger average austenite grain size in the weld heat-affected zone is advantageous for securing ultra-low temperature impact toughness of the weld, but localized strength degradation may occur in the weld heat-affected zone. Therefore, the average austenite grain size may be limited to 200 μm or less. The lower limit of the average grain size of the austenite is more preferably 15 µm, and more preferably 20 µm. The upper limit of the average grain size of the austenite is more preferably 180 µm, and more preferably 150 µm.

[0065]

[0066] When welding is performed under typical welding conditions for ultra-low temperature structures using an austenitic steel as a base material according to one aspect of the present invention, the weld heat-affected zone may have a transverse expansion value of 0.32 mm or more after a Charpy impact test at -253°C. Meanwhile, in the present invention, a higher transverse expansion value is advantageous, and therefore, there is no particular limitation on the upper limit thereof. However, the upper limit of the transverse expansion value may be, for example, 2.30 mm.

[0067]

[0068] The inventor of the present invention has determined that plastic deformation characteristics are a key factor in ensuring safety for steels applied to ultra-low temperature environments. That is, after in-depth research, the inventor of the present invention has confirmed that, for steels satisfying the composition system suggested by the present invention, the transverse expansion value (mm) in the weld heat-affected zone is a more important factor in ensuring the safety of the weld than the Charpy impact energy value (J) of the weld heat-affected zone.

[0069]

[0070] The transverse expansion value in the weld heat-affected zone refers to the average value of the transverse plastic deformation of the specimens subjected to the Charpy impact test at -253℃. Fig. 2 shows a photograph of the specimen subjected to the Charpy impact test at -253℃, and as shown in Fig. 2, the transverse length increase (△X1+△X2) near the fracture surface can be calculated to derive the transverse window value. If the transverse expansion value in the weld heat-affected zone is 0.32 mm or more, it can be determined that the minimum low-temperature safety required for ultra-low-temperature structures is met.

[0071]

[0072] According to the research results of the present inventors, it was confirmed that the Charpy impact energy (J) at -253℃ and the transverse expansion value (mm) of the corresponding specimen generally showed a tendency similar to the following relationship 1, and it was confirmed that the transverse expansion value (mm) is preferably 0.32 mm or more. It can be seen that the larger the transverse expansion value (mm), the better the low-temperature impact toughness is, and 0.72 to 1.4 mm is more effective.

[0073]

[0074] [Relationship 1]

[0075] Transverse expansion value (mm) = 0.0088 × Charpy impact energy value (J) + 0.0893

[0076]

[0077] When welding is performed under normal welding conditions for welding ultra-low temperature structures using an austenitic steel according to one aspect of the present invention as a base material, the transverse expansion value in the heat-affected zone of the weld of a specimen subjected to a Charpy impact test at -253°C is at a level of 0.32 mm or more, so that when an ultra-low temperature structure is manufactured using the steel, excellent structural safety can be secured.

[0078]

[0079] When welding is performed using the austenitic steel of the present invention as a base material under normal welding conditions for welding ultra-low temperature structures, the heat-affected zone of the weld can have a Charpy impact energy of 27 J or more at -253°C. By securing such a high level of ultra-low temperature Charpy impact energy, a ductile fracture occurs when the structure is destroyed, and thus the fracture stability of the ultra-low temperature structure can be secured. Meanwhile, in the present invention, since a higher ultra-low temperature Charpy impact energy is advantageous, there is no particular limitation on the upper limit thereof. However, the upper limit of the ultra-low temperature Charpy impact energy may be, for example, 250 J.

[0080]

[0081] Hereinafter, a method for manufacturing an austenitic steel according to one embodiment of the present invention will be described.

[0082]

[0083] First, the slab having the above-mentioned alloy composition is heated at 1000 to 1300°C. If the slab heating temperature is lower than 1100°C, there are disadvantages in that re-dissolution and homogenization of the alloy components do not occur or it takes a long time to reach the target temperature to the center of the slab. If the slab heating temperature exceeds 1300°C, there are disadvantages in that partial melting occurs in the segregation of the slab alloy components or severe surface oxidation occurs. The lower limit of the slab heating temperature is more preferably 1030°C, more preferably 1070°C, and most preferably 1100°C. The upper limit of the slab heating temperature is more preferably 1250°C, more preferably 1230°C, and most preferably 1200°C.

[0084]

[0085] Thereafter, the heated slab is subjected to finish hot rolling at 800 to 1050°C to obtain a hot-rolled steel sheet. If the finish hot rolling temperature is less than 800°C, rolling is not easy due to the high high-temperature strength of the material, and there is a disadvantage that the strength of the material increases excessively due to non-recrystallization rolling, thereby reducing the impact toughness. If the finish hot rolling temperature exceeds 1050°C, there is a disadvantage that the austenite coarsens and the strength decreases. The lower limit of the finish hot rolling temperature is more preferably 820°C, more preferably 850°C, and most preferably 870°C. The upper limit of the slab finish hot rolling temperature is more preferably 1030°C, more preferably 1000°C, and most preferably 980°C. Meanwhile, the reduction ratio during the hot rolling can be applied within an appropriate range depending on the desired plate thickness, and as a non-limiting example, the final thickness of the hot-rolled hot-rolled steel plate can be 5 to 80 mm.

[0086]

[0087] Afterwards, the hot-rolled steel sheet can be cooled to room temperature.

[0088]

[0089] Thereafter, the hot-rolled steel plates are welded. In the present invention, in order to form a weld heat-affected zone, welding can be performed under normal welding conditions for welding ultra-low temperature structures using a covered arc welding rod, a flux-cored arc welding wire, a TIG welding rod and wire, a submerged arc welding wire and flux, etc.

[0090]

[0091] Hereinafter, austenitic steel and its manufacturing method according to one aspect of the present invention will be described in more detail through specific examples. It should be noted that the following examples are intended solely to facilitate understanding of the present invention and are not intended to define the scope of the invention. The scope of the invention can be determined by the matters set forth in the patent claims and matters reasonably inferred therefrom.

[0092]

[0093] (Example)

[0094] After preparing a 250 mm thick slab having the alloy composition described in Table 1 below, the slab was heated and hot rolled under the conditions described in Table 2 below, and submerged arc welding was performed under normal conditions to manufacture a steel material having a welded heat affected zone.

[0095]

[0096] The microstructure and physical properties of the weld heat-affected zone of the steel manufactured in this manner were measured, and the results are shown in Table 2 below.

[0097]

[0098] The microstructure was measured using an optical microscope at room temperature.

[0099]

[0100] The average austenite grain size was measured by taking microstructural photographs using an optical microscope and then using image analysis.

[0101]

[0102] The content of C incorporated into austenite relative to the average C content of the steel was measured using point analysis of the matrix and carbides using an energy dispersive X-ray spectrometer of a scanning electron microscope.

[0103]

[0104] Charpy impact energy was measured using a Charpy impact tester after keeping the specimen at -253℃ for more than 15 minutes.

[0105]

[0106] The above transverse expansion was calculated as the average value of the transverse plastic deformation of the specimens subjected to the Charpy impact test at -253℃.

[0107]

[0108] Steel alloy composition (weight %)Mn24×[C]+[Mn]33.5×[C]-[Mn]CrCuSiAlMoBA23.8529.13-16.482.92--2.31--B26.9433.90-17.233.140.83----C21.0930.45-8.032.64-0.801.05--D20.8129.69-8.423.440.41-- --E27.2637.34-13.192.25----0.003F19.4025.40-11.036.35---1.32-G22.5030.90-10.782.85 -----H33.6047.04-14.8411.70-----I18.0625.02-8.351.17-----J15.3044.3425.241.12-----

[0109]

[0110] ClassificationSteel gradeSlab heating temperature(℃)Finishing hot rolling temperature(℃)Steel thickness(mm)Microstructure(area%)Austenite average grain size(㎛)Charpy impact energy of C content dissolved in austenite compared to average C content of steel(J, @-253℃)Transverse expansion(mm)Example 1A118491420100%γ431001341.27Example 2B118191025100%γ401001121.11Example 3C120591630100%γ37100860.85Example 4D11908963298%γ, 2% carbide 5285840.80 Example 5E121292418100%γ75100920.89 Example 6F12049272299%γ, 1% carbide 6491840.81 Comparative Example 1G11808362094%γ, 6% carbide 9.657260.18 Comparative Example 2H11939253592%γ, 8% carbide 3352250.12 Comparative Example 3I12009151880%γ, 20%ε5010050.00 Comparative Example 4J12058623089%γ, 11% carbide 4248310.05 γ: austenite, ε: epsilon martensite

[0111]

[0112] As can be seen from Tables 1 and 2 above, in the case of Examples 1 to 6 that satisfy the alloy composition and manufacturing conditions of the present invention, it can be seen that excellent physical properties are secured by securing the content of C dissolved in austenite compared to the average C content of the microstructure and steel material to be obtained by the present invention.

[0113]

[0114] In the case of Comparative Examples 1 to 4 that do not satisfy the alloy composition of the present invention, it can be seen that the physical properties are at a low level because the content of C dissolved in austenite is not secured compared to the average C content of the microstructure or steel material that the present invention seeks to obtain.

Claims

1. In weight%, manganese (Mn): 10 to 45%, carbon (C): a range satisfying 24×[C]+[Mn]≥25 and 33.5×[C]-[Mn]≤18, chromium (Cr): 10% or less (excluding 0%), and at least one of Cu: 5% or less (excluding 0%), Si: 5% or less (excluding 0%), Al: 5% or less (excluding 0%), Mo: 5% or less (excluding 0%), and B: 0.5% or less (excluding 0%), the remainder including iron (Fe) and unavoidable impurities. The microstructure in the weld heat affected zone contains, in area %, 95% or more (including 100%) of austenite and 5% or less (including 0%) of carbides. An austenitic steel having a content of C employed in the austenite of at least 60% of the average C content of the steel.

2. In claim 1, The above austenite is an austenitic steel with an average grain size of 10 to 200 ㎛.

3. In claim 1, The above weld heat affected zone is an austenitic steel having a transverse expansion of 0.32 mm or more after a Charpy impact test at -253℃.

4. In claim 1, The above weld heat affected zone is an austenitic steel having a Charpy impact energy of 27 J or more at -253°C.

5. A step of heating a slab containing manganese (Mn): 10 to 45% by weight, carbon (C): a range satisfying 24×[C]+[Mn]≥25 and 33.5×[C]-[Mn]≤18, chromium (Cr): 10% or less (excluding 0%), and at least one of Cu: 5% or less (excluding 0%), Si: 5% or less (excluding 0%), Al: 5% or less (excluding 0%), Mo: 5% or less (excluding 0%), and B: 0.5% or less (excluding 0%), the remainder iron (Fe) and unavoidable impurities, at 1000 to 1300°C; A step of obtaining a hot-rolled steel sheet by finishing hot rolling the above-mentioned heated slab at 800 to 1050°C; and A method for manufacturing an austenitic steel, comprising the step of welding the hot-rolled steel sheet.