Plated steel sheet having excellent corrosion resistance, and manufacturing method therefor
Patent Information
- Application Number
- MYPI2025003676
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-12-19
- Filing Date
- 2023-12-18
- Publication Date
- 2024-06-19
AI Technical Summary
Conventional zinc-based plated steel sheets lack sufficient corrosion resistance in complex environments, particularly in acidic and alkaline atmospheres, limiting their application in diverse industrial settings.
A coated steel sheet with an Al-Mg-Zn-based plating layer, comprising 4.00-7.00% Mg, 8.000-20.000% Al, 0.002-0.050% Fe, and a balance of Zn, is developed, featuring a specific microstructure with MgZn2 and Al phases, which provides excellent corrosion resistance through controlled phase distribution and composition.
The coated steel sheet exhibits superior corrosion resistance in both acidic and alkaline environments, ensuring durability in complex corrosive conditions, as demonstrated by enhanced performance in neutral, acidic, and alkaline tests.
Smart Images

Figure PI2025003676_DRAWING_001
Abstract
Description
Coated steel sheet with excellent corrosion resistance and manufacturing method thereof
[0001] The present invention relates to a plated steel sheet having excellent corrosion resistance even under a complex corrosion environment and a method for manufacturing the same.
[0002] Zinc-plated steel exhibits a sacrificial nature. When exposed to a corrosive environment, zinc, with a lower redox potential than iron, corrodes first, inhibiting corrosion of the steel. Furthermore, as the zinc in the plating layer oxidizes, it forms a dense corrosion product on the steel surface, shielding it from the oxidizing environment and enhancing its corrosion resistance. Thanks to these advantageous properties, zinc-plated steel has recently been expanding its application to include building materials, home appliances, and automotive steel.
[0003] However, the corrosive environment is gradually worsening due to increased air pollution resulting from industrial advancement. Furthermore, as industries diversify, steel plates are exposed to increasingly complex corrosive environments. This has led to a growing need for steel materials with superior corrosion resistance in diverse corrosive environments than conventional zinc-plated steel plates.
[0004] For example, steel sheets used on the interior of buildings may be placed inside livestock sheds or in contact with cement, while steel sheets used on the exterior of buildings may be exposed to acidic, corrosive environments due to acid rain. In these complex corrosive environments, galvanized steel sheets with superior corrosion resistance in both acidic and alkaline environments are required. However, conventional zinc-based galvanized steel sheet technology has not yet been developed to provide sufficient corrosion resistance in both acidic and alkaline environments.
[0005] [Prior Art Literature]
[0006] [Patent Document]
[0007] (Patent Document 1) Korean Publication No. 2013-0133358
[0008] According to one aspect of the present invention, it is an object to provide a plated steel sheet having excellent corrosion resistance even under a complex corrosion environment and a method for manufacturing the same.
[0009] According to another aspect of the present invention, it is an object to provide a plated steel sheet having excellent corrosion resistance even in acidic and alkaline environments and a method for manufacturing the same.
[0010] According to another aspect of the present invention, it is an object to provide a plated steel sheet having excellent corrosion resistance not only in a neutral environment but also in an acidic environment and an alkaline environment, and a method for manufacturing the same.
[0011] The subject matter of the present invention is not limited to the aforementioned content. Anyone with ordinary skill in the art to which the present invention pertains will have no difficulty understanding the additional subject matter of the invention from the entire disclosure of the present invention.
[0012] One aspect of the present invention is:
[0013] steel plate; and
[0014] Including an Al-Mg-Zn based plating layer provided on at least one surface of the above steel plate,
[0015] The above plating layer has a number density of 500 to 4,000 Al phases / 0.1 mm that exist within the MgZn2 phase or in contact with the MgZn2 phase. 2 We provide people with galvanized steel sheets.
[0016]
[0017] In addition, another aspect of the present invention is
[0018] A step of hot-dip galvanizing by immersing a steel plate in a plating bath containing, by weight %, Mg: 4.00 to 7.00%, Al: 8.000 to 20.000%, Fe: 0.002 to 0.050%, the remainder Zn and other unavoidable impurities, and having a temperature of 430 to 520°C and a flow velocity of 0.03 to 0.20 m / s;
[0019] A step of performing a wiping treatment on the above molten steel plate; and
[0020] A method for manufacturing a plated steel sheet is provided, including a step of cooling the above-mentioned wiping-treated steel sheet so that an average cooling rate is 6.0°C / s or more in a range from the crystallization temperature of Al to 330°C.
[0021] According to one aspect of the present invention, a plated steel sheet having excellent corrosion resistance and a method for manufacturing the same can be provided even under a complex corrosion environment.
[0022] In addition, according to another aspect of the present invention, a plated steel sheet having excellent corrosion resistance even in acidic and alkaline environments and a method for manufacturing the same can be provided.
[0023] In addition, according to another aspect of the present invention, a plated steel sheet having excellent corrosion resistance not only in a neutral environment but also in an acidic environment and an alkaline environment and a method for manufacturing the same can be provided.
[0024] The various advantageous and beneficial effects of the present invention are not limited to the above-described contents, and will be more easily understood in the course of explaining specific embodiments of the present invention.
[0025] Figure 1 shows a photograph of a cross-sectional specimen of a plated steel sheet obtained from Invention Example B4 of the present invention, observed using a scanning electron microscope (SEM).
[0026] Figure 2 shows a photograph of a cross-sectional specimen of a plated steel sheet obtained from Comparative Example B14 of the present invention, observed using a scanning electron microscope (SEM).
[0027] The terminology used herein is for the purpose of describing specific embodiments and is not intended to limit the present invention. Furthermore, the singular forms used herein also include plural forms, unless the context clearly dictates otherwise.
[0028] The meaning of "comprising" as used in the specification is to specify a configuration and not to exclude the presence or addition of other configurations.
[0029] Unless otherwise defined, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by a person of ordinary skill in the art to which this invention pertains. Terms defined in the dictionary are to be interpreted to have meanings consistent with the relevant technical literature and the present disclosure.
[0030] Hereinafter, a plated steel sheet according to one aspect of the present invention will be described in detail. In the present invention, when indicating the content of each element, unless otherwise defined, it means weight %.
[0031]
[0032] As industries have diversified in recent years, steel plates have been placed in more complex corrosion environments, and the need for plated steel plates with excellent corrosion resistance in both acidic and alkaline environments has arisen in these complex corrosion environments.
[0033] However, in the technology related to conventional zinc-plated steel sheets, a technology has not been developed that has sufficient corrosion resistance in both acidic and alkaline atmospheres.
[0034] In addition to zinc-plated steel sheets, there are aluminum-plated steel sheets such as Al-plating and Al-Zn-plating (Galvalume). However, although aluminum-plated steel sheets have excellent corrosion resistance in acidic environments, they cannot be applied in complex corrosion environments because aluminum corrodes severely in alkaline environments.
[0035] To improve these problems, various studies are being conducted on manufacturing technologies for zinc alloy-based galvanized steel sheets that improve the corrosion resistance of steel sheets by adding elements such as aluminum (Al) and magnesium (Mg) to the zinc plating bath. A representative example is the Al-Mg-Zn zinc alloy-based galvanized steel sheet, which additionally adds Mg to the Al-Zn plating composition. By appropriately adding Mg and Al to zinc, excellent corrosion resistance can be secured even in acidic and alkaline environments. In the Al-Mg-Zn zinc alloy-based galvanized steel sheet, when the amount of Mg added to the plating layer increases, Mg dissolution is rapid in acidic environments, making corrosion easy, but in neutral (including salt water environments) and alkaline environments, stable Mg-based hydroxides are formed on the surface of the sheet, inhibiting corrosion.
[0036] On the other hand, when the amount of Al added in the plating layer increases, corrosion resistance increases because aluminum oxide on the surface is stable in acidic and neutral environments, but conversely, in an alkaline atmosphere, Al dissolution becomes severe and corrosion resistance decreases, so it is necessary to appropriately adjust the components of Mg and Al in the plating layer, and it is necessary to uniformly adjust the distribution of the components of Mg and Al in the plating layer.
[0037]
[0038] First, a plated steel sheet according to one aspect of the present invention includes: a base steel sheet; and a plated layer provided on at least one surface of the base steel sheet.
[0039] In the present invention, the type of the substrate steel sheet may not be particularly limited. For example, the substrate steel sheet may be an Fe-based substrate steel sheet used as a substrate steel sheet for a typical zinc-based galvanized steel sheet, i.e., a hot-rolled steel sheet or a cold-rolled steel sheet, but is not limited thereto. Alternatively, the substrate steel sheet may be, for example, carbon steel, ultra-low carbon steel, or high manganese steel used as a material for construction, home appliances, or automobiles, or may be stainless steel, etc. Meanwhile, in the case of the carbon steel, ultra-low carbon steel, medium-low carbon steel, low carbon steel, and carbon steel all exhibit similar effects, and there is no need to specifically limit the steel components, so it is hardly affected by components such as Mn, Si, Ti, Nb, and B, which are added in large quantities to high-strength steel and ultra-high-strength steel. Meanwhile, an example of the above-mentioned steel sheet may include, in weight %, C: more than 0% and 0.18% or less, Si: more than 0% and 1.5% or less, Mn: 0.01 to 2.7%, P: more than 0% and 0.07% or less, S: more than 0% and 0.015% or less, Al: more than 0% and 0.5% or less, Nb: 0.06% or less (including 0%), Cr: 1.1% or less (including 0%), Ti: 0.06% or less (including 0%), B: 0.03% or less (including 0%), the remainder being Fe and other unavoidable impurities. An example of the above-mentioned steel sheet may include, in weight %, C: more than 0% but not more than 0.18%, Si: more than 0% but not more than 1.5%, Mn: 0.01 to 2.7%, P: more than 0% but not more than 0.07%, S: more than 0% but not more than 0.015%, Al: more than 0% but not more than 0.5%, Nb: more than 0% but not more than 0.06%, Cr: more than 0% but not more than 1.1%, Ti: more than 0% but not more than 0.06%, B: more than 0% but not more than 0.03%, and the remainder including Fe and other unavoidable impurities.
[0040]
[0041] According to one aspect of the present invention, at least one surface of the base steel sheet may be provided with an Al-Mg-Zn-based plating layer made of an Al-Mg-Zn-based alloy as a plating layer. The plating layer may be formed on only one surface of the base steel sheet, or may be formed on both surfaces of the base steel sheet. In this case, the Al-Mg-Zn-based plating layer refers to a plating layer that includes Mg and Al and mainly includes Zn (i.e., includes Zn at 50% or more).
[0042]
[0043] According to one aspect of the present invention, the plating layer may include, in wt%, Mg: 4.00 to 7.00%, Al: 8.000 to 20.000%, Fe: 0.002 to 0.050%, the remainder Zn, and other unavoidable impurities. Meanwhile, although not particularly limited, the plating layer may optionally further include, in wt%, one or more selected from Si: 0.20% or less (including 0%) and Ca: 0.200% or less (including 0%). Each component will be described in detail below.
[0044] Mg: 4.00~7.00%
[0045] Mg is an element that improves the corrosion resistance of a plated steel sheet. In the present invention, the Mg content in the plated layer is controlled to 4.00% or more to secure the desired excellent corrosion resistance. According to one embodiment of the present invention, it may be 4.10% or more.
[0046] When the above Al-Mg-Zn plated steel sheet is exposed to a neutral, weakly acidic, or weakly alkaline corrosive environment such as salt water or rainwater, Mg in the plated layer is dissolved, resulting in LDH (Layered Double Hydroxide; (Zn,Mg)6Al2(OH) 16The higher the Mg content, the better, because (CO3)·4H2O)) is uniformly formed, improving corrosion resistance. However, in an acidic corrosive environment, Mg dissolution is too fast, so the more Mg is added, the worse the corrosion resistance in an acidic environment. In addition, if Mg is added excessively, there is a possibility that dross in the form of MgO may be generated in the plating bath, so in the present invention, the Mg content may be 7.00% or less. According to one embodiment of the present invention, it may be 6.90% or less.
[0047]
[0048] Al: 8,000~20,000%
[0049] Al is a component that improves corrosion resistance together with Mg. Since Al is strong against acid, the corrosion resistance in acidic conditions increases significantly as the Al content increases. Therefore, in order to secure the above-mentioned effect, the Al content may be 8.000% or more in the present invention. According to one embodiment of the present invention, it may be 8.200% or more. According to one embodiment of the present invention, it may be 8.500% or more. On the other hand, as the amount of Al added increases, corrosion increases in an alkaline environment. In addition, Al in the plating bath has the effect of suppressing the oxidation of Mg, so that the formation of MgO-based dross is suppressed as the amount of Al added increases. However, if the amount of Al added is too large, the melting point of the plating bath increases, so that the plating bath temperature must be maintained high, which aggravates the erosion of structures in the plating bath. Therefore, the Al content in the plating layer may be 20.000% or less. According to one embodiment of the present invention, it may be 19.800% or less.
[0050]
[0051] Fe: 0.002~0.050%
[0052] Fe plays a crucial role in the present invention. While Fe may be added directly to the plating bath, it can also be dissolved from the steel plate. Initially, when the plating bath is manufactured, its composition is adjusted by including it in the ingot being charged. However, as the plating process progresses, Fe dissolves from the steel plate. Therefore, it is periodically analyzed. If the content is low, additional ingot is added. If it exceeds the content, the content is adjusted through dilution or removal.
[0053] Typically, in a plating bath containing Al, Fe exists in the form of Fe2Al5. Since the Fe2Al5 has a lighter specific gravity than the plating bath, it floats to the surface of the plating bath, clumps together, and grows into large dross. This dross adheres to the steel plate during the plating process, causing dross adhesion defects. Furthermore, when the plating bath flow is large, coarse dross flows within the plating bath, causing dross imprinting defects on the steel plate. Therefore, it must be periodically removed. However, when the Fe2Al5 is fine, with a size (diameter) of 0.05㎛ or less, it does not float to the surface when the plating bath is fluidized, but rather flows within the plating bath, and some of it adheres to the steel plate and exists in the plating layer. In the present invention, since the Fe present in the plating layer before solidification serves as a crystal nucleation site during the solidification process, it is necessary to add at least 0.002% or more. On the other hand, when the Fe content exceeds 0.050%, the amount of dross generated on the surface of the plating bath increases, which may cause an increase in dross adhesion defects. According to one embodiment of the present invention, it may be 0.045% or less.
[0054]
[0055] Si: 0.20% or less (including 0%)
[0056] When Si is added at 0.2% or less, it can prevent the formation of a thick Fe-Al alloy layer at the interface between the base steel and the plating layer, thereby preventing a decrease in the interface strength between the plating layer and the base steel. Therefore, addition is advantageous, but since there is little effect on the corrosion resistance in the present invention even if it is not added, the lower limit is set to 0%.
[0057] However, even if the Si addition amount exceeds 0.20%, the effect of suppressing the Fe-Al alloy layer at the interface reaches saturation, and as the Si addition amount increases, the melting point of the plating bath rises, so the plating bath temperature must be maintained high, which is not good from the perspective of equipment protection. According to one embodiment of the present invention, it may be 0.18% or less.
[0058]
[0059] Ca: 0.200% or less (including 0%)
[0060] Although Ca does not necessarily need to be added, adding up to 0.200% can suppress the formation of MgO oxide in the plating bath. In addition, since small amounts are sometimes added for convenience in the production of ingots for plating bath production, small amounts may be present in the plating bath produced from such ingots. However, if the amount of Ca added exceeds 0.200%, the color of the steel sheet may darken, which is not preferred. According to one embodiment of the present invention, the amount of Ca may be 0.180% or less.
[0061]
[0062] Residual Zn and other unavoidable impurities
[0063] In addition to the aforementioned components, the plating bath is composed of inevitable impurities and zinc components that are present during the ingot manufacturing process or components eluted from the steel sheet. The inevitable impurities include Sb, Sn, Pb, Sr, Cu, etc., which are components that are inevitably mixed in small amounts during the ingot manufacturing process for preparing the plating solution. Meanwhile, components that are inevitably eluted when the steel sheet is immersed in the plating bath and exist in small amounts in the plating bath include Mn, Ti, Ni, B, Nb, etc., but other components may also exist depending on the components of the steel sheet. However, even if they are inevitably added, it is not desirable for each component to be present in an amount of more than 0.1%.
[0064]
[0065] According to one embodiment of the present invention, the plating layer may further include at least one of the following groups (a) to (h).
[0066] However, since the elements in each group below are not essential for achieving the tasks of the present invention, their lower limits of content are not limited. Therefore, even if not specifically mentioned below, the lower limit of the content of each element may be 0%.
[0067] (a) Ni: 0.5% or less
[0068] (b) La: 0.1% or less, Ce: 0.1% or less, Y: 0.1% or less, Sr: 1.0% or less, or more than one of the following
[0069] (c) Ti: 0.1% or less
[0070] (d) W: 0.5% or less
[0071] (e) Cu: 2.0% or less
[0072] (f) Cr: 0.5% or less, Mn: 0.5% or less, V: 0.5% or less, at least one of these
[0073] (g) B: 0.1% or less, P: 0.1% or less, 1 or more types
[0074] (h) Sn: 1.0% or less, Sb: 1.0% or less, Bi: 1.0% or less, or at least one of these
[0075]
[0076] (a) Ni: 0.5% or less
[0077] Ni has the effect of preventing Fe diffusion by forming an Al-Ni alloy phase, but if its content exceeds 0.5%, there may be a problem of excessive increase in the cost of raw materials.
[0078]
[0079] (b) La: 0.1% or less, Ce: 0.1% or less, Y: 0.1% or less, Sr: 1.0% or less, or more than one of the following
[0080] La, Ce, Y and Sr have the effect of preventing oxidation of Mg in the plating bath by forming an oxide film, but if their contents exceed 0.1%, 0.1%, 0.1% and 1.0%, respectively, there may be a problem of reduced plating properties due to an increase in the viscosity of the plating bath.
[0081]
[0082] (c) Ti: 0.1% or less
[0083] Ti acts as a nucleation site for Ti-Al intermetallic compounds and has the effect of refining crystal grains (spangles), but if its content exceeds 0.1%, the melting point of the plating bath may increase and there may be a problem of increased dross.
[0084]
[0085] (d) W: 0.5% or less
[0086] W forms W oxide on the surface, which improves corrosion resistance, but if its content exceeds 0.5%, there may be a problem of the melting point of the plating bath increasing.
[0087]
[0088] (e) Cu: 2.0% or less
[0089] Cu has the effect of forming an Al-Cu process structure and lowering the hardness of the plating layer, but if its content exceeds 2.0%, there may be a problem of the spangles becoming coarser.
[0090]
[0091] (f) Cr: 0.5% or less, Mn: 0.5% or less, V: 0.5% or less, at least one of these
[0092] Cr, Mn, and V have the effect of preventing electrode deterioration by suppressing alloying between zinc and the welding electrode due to rapid liquid loss, but if their contents exceed 0.5% each, there may be a problem of the melting point of the plating bath being excessively increased.
[0093]
[0094] (g) B: 0.1% or less, P: 0.1% or less, at least one of these
[0095] B and P have the effect of suppressing LME cracks in welds, but if their contents exceed 0.1% each, there may be a problem of increased dross generation.
[0096]
[0097] (h) Sn: 1.0% or less, Sb: 1.0% or less, Bi: 1.0% or less, or at least one of these
[0098] Sn, Sb, and Bi have the effect of uniformizing spangles and improving pot durability by lowering the plating bath temperature, but if their contents exceed 1.0% each, there may be a problem of coarsening of spangles.
[0099]
[0100] Hereinafter, an alloy phase in a plating layer according to an aspect of the present invention will be described. The plating layer according to an aspect of the present invention may include various phases such as a MgZn2 phase, an Al phase, an Al-Zn binary eutectic phase, a Zn-MgZn2-Al phase, and a Zn phase. In particular, according to an aspect of the present invention, the plating layer essentially includes an Al phase and a MgZn2 phase, and may further include at least one selected from an Al-Zn binary eutectic phase, a Zn-MgZn2-Al ternary eutectic phase, and a Zn phase.
[0101] At this time, in the present invention, the MgZn2 phase means a phase mainly composed of MgZn2, and may contain other components other than Mg and Zn in an atomic % of 5% or less (including 0%). In addition, the Al phase refers to a phase mainly composed of Al, specifically, a phase in which Zn is dissolved in an atomic % of less than 27% (including 0%), and the remainder is composed of Al and other impurities (the total of impurities is 2% or less (including 0%)). That is, in addition to the Al component, the Al phase may contain components such as Zn and Mg that can be included as plating layer components, and it should be noted that in the present invention, the Al phase refers only to a phase in which Zn is dissolved in an atomic % of less than 27% (including 0%).
[0102] In addition, the above Zn-MgZn2-Al ternary eutectic phase refers to a ternary eutectic phase in which a Zn phase, a MgZn2 phase, and an Al phase are all mixed, and the above Al-Zn ternary eutectic phase refers to a phase in which the Al phase and the Zn phase are arranged alternately in a lamellar or irregularly mixed form.
[0103] At this time, it is necessary to note that the Al phase within the Al-Zn binary eutectic phase and the Zn-MgZn2-Al ternary eutectic phase is not regarded as the aforementioned Al phase. Similarly, it is necessary to note that the MgZn2 within the Zn-MgZn2-Al ternary eutectic phase is not regarded as the MgZn2 phase mainly composed of the aforementioned MgZn2.
[0104] Meanwhile, the microstructure of the aforementioned plating layer may have different distributions on the surface and cross-section. Such microstructures on the surface and cross-section can be confirmed using a scanning electron microscope (SEM) or transmission electron microscope (TEM) by magnifying the plating layer for each surface or cross-section specimen.
[0105] As such, the Zn-Mg-Al plating layer contains various phases depending on the composition and manufacturing conditions of the plating layer. However, the inventors of the present invention have conducted extensive research on the distribution of phases within the plating layer in order to ensure that the Al-Mg-Zn plating steel sheet has excellent corrosion resistance not only in a corrosive environment near neutrality but also in acidic and alkaline regions. As a result, they confirmed that the MgZn2 phase has strong corrosion resistance in an alkaline region and the Al phase exhibits corrosion resistance in an acidic environment. They also discovered that by appropriately distributing these two phases, excellent corrosion resistance can be secured not only in a neutral environment but also in all atmospheres including acidic and alkaline environments, and thus completed the present invention.
[0106]
[0107] Although not particularly limited, according to one embodiment of the present invention, in the case of a Zn-Mg-Al-based plating layer that satisfies the aforementioned plating layer composition, the plating layer includes a microstructure in which an Al phase exists within a MgZn2 phase or exists in contact with a MgZn2 phase. The form in which the Al phase exists within the MgZn2 phase means a form in which one Al phase is completely contained within the MgZn2 phase. Alternatively, the form in which the Al phase exists in contact with the MgZn2 phase includes all forms in which only a part of one Al phase is contained within the MgZn2 phase or a form in which the Al phase exists in contact with the MgZn2 phase.
[0108] Meanwhile, although not particularly limited, according to one aspect of the present invention, the plating layer may include, in terms of area %, MgZn2 phase: 15.0 to 60.0% and Al phase: 3.0 to 25.0% based on a cross-section in the thickness direction (meaning the direction perpendicular to the rolling direction). By controlling the two phase fractions to satisfy this, corrosion resistance under a complex corrosion environment can be further improved.
[0109]
[0110] According to one aspect of the present invention, a plating layer includes the aforementioned MgZn2 phase, Al phase, Al-Zn binary eutectic phase, Zn-MgZn2-Al and Zn phase, etc., and when a plating steel sheet including these phases is used in an acidic corrosive atmosphere, the MgZn2 phase corrodes first, whereas the Al phase corrodes slowly in acid. On the other hand, when a plating steel sheet is used in an alkaline corrosive environment, the MgZn2 phase is relatively resistant to corrosion compared to other phases, whereas the Al phase corrodes at a fast rate. Therefore, in order to have excellent corrosion resistance in a composite corrosive environment including acid and alkali, it is necessary to appropriately control the ratio, size or distribution of these two phases. Hereinafter, the characteristics of the ratio, size or distribution between these two phases will be described in detail.
[0111] According to one aspect of the present invention, the plating layer may have a ratio of the number of Al phases present within the MgZn2 phase or in contact with the MgZn2 phase relative to the total number of Al phases of 85% or more and 100% or less. If the ratio of the number of Al phases present within the MgZn2 phase or in contact with the MgZn2 phase relative to the total number of Al phases is less than 85%, corrosion resistance in acidic and alkaline environments may decrease. At this time, it should be noted that in the present invention, the above-mentioned Al phase is intended to be at least 0.5㎛ or more based on the equivalent circle diameter, and the same applies to the description below.
[0112]
[0113] Although not particularly limited, according to one aspect of the present invention, even if the ratio of the Al phase satisfies 3.0 to 25.0% in area % based on the cross-section in the thickness direction of the plated steel sheet, as shown in Fig. 2, if the size of the Al phase is coarse based on the cross-section in the thickness direction of the plated steel sheet, when the Al phase is exposed to an alkaline corrosive environment, corrosion may occur preferentially and the corrosion substance may act as a migration path from the surface of the plated layer to the base steel sheet. As a result, even if the remaining phases including the MgZn2 phase are intact, corrosion may occur in the base steel sheet. On the other hand, as shown in Fig. 1 according to the present invention, if the Al phase is fine based on the cross-section in the thickness direction of the plated steel sheet, even if the Al phase is corroded when exposed to an alkaline corrosive environment, another phase such as the MgZn2 phase having good alkaline corrosion resistance may exist together with the Al phase, thereby blocking the migration of the corrosion substance in the depth direction (thickness direction) of the plated layer, thereby improving the corrosion resistance. Although not particularly limited, in particular, when there are a large number of fine Al phases of 5 μm or less that are stable in an acidic environment, the effect of inhibiting corrosion substances from penetrating toward the steel plate in an acidic environment can be more excellent. Therefore, although not particularly limited, according to one aspect of the present invention, the average long-axis linear length of the Al phase existing within the MgZn2 phase or in contact with the MgZn2 phase can be 5 μm or less (excluding 0 μm). In addition, since the more the aforementioned fine Al phases exist, the more the corrosion resistance under the aforementioned complex corrosion environment can be improved, according to one aspect of the present invention, the number ratio of the Al phases existing within the MgZn2 phase or in contact with the MgZn2 phase and having a long-axis linear length of 5 μm or less (excluding 0 μm) relative to the total number of Al phases can be 90.0 to 100.0%, and this is not particularly limited.
[0114]
[0115] In addition, although not particularly limited, according to one aspect of the present invention, in the plating layer, the number density (D) of the Al phase existing inside the MgZn2 phase or in contact with the MgZn2 phase al ) is 500~4,000 / 0.1mm 2 In the present invention, the aforementioned number density is 0.1 mm based on the cross-section in the thickness direction of the plating layer. 2 It refers to the number of Al phases present inside the MgZn2 phase or in contact with the MgZn2 phase per unit area. In this case, the D al The value is 500 / 0.1mm 2 If it is less than D, the gap between the Al phases is too far, so that corrosion factors can easily propagate between the Al phases, which may cause a problem in that the effect of blocking corrosion factors in an acidic atmosphere is reduced. In addition, the above D al The value is 4,000 / 0.1mm 2 If it exceeds , most of the plating layer is composed of Al phase and MgZn2 phase, so the proportion of Al-Zn binary eutectic phase and / or Zn-MgZn2-Al ternary eutectic phase, which has excellent corrosion resistance in a relatively neutral environment, decreases, which may cause problems in securing corrosion resistance in a neutral environment.
[0116]
[0117] Meanwhile, in the present invention, there are no particular limitations on the method of measuring the area ratio of each phase, the number ratio of the Al phase existing within the aforementioned MgZn2 phase or existing in contact with the MgZn2 phase, the average long-axis straight length, the number density, etc., and they can be measured using a conventional method known in the relevant technical field.
[0118] For example, the area ratio of each phase, the number ratio of the Al phase existing within the aforementioned MgZn2 phase or existing in contact with the MgZn2 phase, the average long-axis straight line length, and the number density (D al) etc., based on the cross-sectional specimen in the thickness direction of the galvanized steel sheet, the tissue photograph is taken with a field emission scanning electron microscope (FE-SEM), and then EDS (Energy Dispersive X-ray Spectroscopy) is used to analyze the components to distinguish and define each phase. After that, each phase is labeled and distinguished in the photographed image, and the area ratio, number ratio, average major axis straight length, number density, etc. of each phase can be measured using an image analyzer. At this time, considering the deviation by part of each specimen, 20 places are photographed at a magnification of 2,000 times for each specimen, and then the average value of each specimen is obtained, thereby measuring parameters such as the area ratio, number ratio, average major axis straight length, number density, etc. of each phase mentioned above.
[0119]
[0120] Next, a method for manufacturing a plated steel sheet according to another aspect of the present invention will be described in detail. However, this does not necessarily mean that the plated steel sheet of the present invention must be manufactured using the manufacturing method described below.
[0121] According to one aspect of the present invention, a step of first preparing a base steel plate may be further included, and the type of the base steel plate is not particularly limited. In this case, the aforementioned description is equally applicable to the base steel plate.
[0122] Next, the base steel sheet is immersed in a plating bath containing, in wt%, Mg: 4.00 to 7.00%, Al: 8.000 to 20.000%, Fe: 0.002 to 0.050%, the remainder Zn, and other unavoidable impurities, and hot-dip plating is performed. At this time, with respect to the reasons for adding the components in the plating bath and the reasons for limiting the contents, the description of the components of the plating layer described above can be equally applied, except for the small amount of impurity content that may flow in from the base steel sheet. Therefore, according to one aspect of the present invention, the plating bath may optionally further include, in wt%, at least one selected from Si: 0.20% or less (including 0%) and Ca: 0.200% or less (including 0%).
[0123] In order to manufacture the plating bath of the above-mentioned composition, a composite ingot containing a predetermined amount of Zn, Al, and Mg, or a Zn-Mg, Zn-Al ingot containing individual components can be used. In order to replenish the plating bath consumed by molten plating, the ingot is additionally melted and supplied. In this case, a method of directly immersing the ingot in the plating bath and melting it can be adopted, or a method of melting the ingot in a separate pot and then replenishing the molten metal to the plating bath can be adopted.
[0124] Meanwhile, when manufacturing a plating bath, 0.002 to 0.050% of Fe is included as an essential component other than Zn, Al, and Mg. The Fe in the plating bath can be manufactured by alloying Fe during the initial plating bath manufacturing process, or by adding Fe separately during the plating bath manufacturing process. However, since some of it may be eluted from the steel sheet once the plating process begins, it is necessary to analyze it periodically and manage it so that it remains within the 0.002 to 0.050% range defined in the present invention.
[0125] Fe in the plating bath reacts with Al to form Fe2Al5 phase. Fe2Al5 phase has a light specific gravity and floats to the surface of the plating bath, but when the size (diameter) is 0.05㎛ or less, it does not float to the surface when the plating bath is fluid and flows within the plating bath. Therefore, according to one aspect of the present invention, fine Fe2Al5 dross having a size of 0.05㎛ or less (excluding 0㎛) flowing within the plating bath is a key factor affecting the number of alloy phase sizes of the final plating product in the present invention, and this will be described in detail. Meanwhile, coarse dross existing on the surface of the plating bath does not correspond to 0.002 to 0.050% of Fe in the plating bath limited in the present invention. When analyzing the components of the plating bath, a sample taken from a depth of 30cm in the thickness direction from the surface is analyzed to determine the Fe content.
[0126]
[0127] In addition, although not particularly limited, according to one aspect of the present invention, fine Fe2Al5 of 0.05㎛ or less flowing in the plating bath is attached to the steel sheet together with the plating bath while the steel sheet passes through the plating bath. Thereafter, during the cooling process, it becomes a nucleation site when the plating layer is cooled. In the present invention, the phase that crystallizes first when the plating layer solidifies is the Al phase. Therefore, since the fine dross existing in the plating layer before cooling after plating becomes an Al phase crystallization nucleation site during the cooling process, the more fluid dross there is, the more Al nucleation there is, and the finer the Al phase becomes. Therefore, in the present invention, the size (average diameter) of the fluid dross in the plating bath can be made to exist as fine dross of 0.05㎛ or less (excluding 0㎛). At this time, one of the factors that refines the size of the fluid dross in the plating bath is the control of the Fe content, and if the Fe content in the plating bath is less than 0.002%, there may be no or too little Fe2Al5 fluid dross, which may cause the Al phase to coarsen due to insufficient nucleation of the Al phase. On the other hand, if the Fe content in the plating bath exceeds 0.05%, the generation of Fe2Al5 dross increases, causing the dross to clump together and coarsen, transforming into coarse dross and floating to the surface of the plating bath to interfere with the plating process or being mixed into the plating layer to cause a dross imprint defect on the steel sheet.
[0128]
[0129] Additionally, although not particularly limited, according to one aspect of the present invention, the temperature of the plating bath can be maintained at a temperature 20 to 100°C higher than the solidification initiation temperature (Ts). At this time, since the solidification initiation temperature can vary depending on the composition of the plating bath, the plating bath temperature can also be adjusted accordingly. Meanwhile, the temperature of the plating bath can be maintained in the range of 430 to 520°C.
[0130]
[0131] In addition, according to one aspect of the present invention, the flow speed of the plating bath can be controlled to 0.03 to 0.20 m / s. Even if Fe2Al5 dross of 0.05 μm or less is generated in the plating bath according to the present invention, if there is no flow in the plating bath, it is easy to float to the surface of the plating bath, and dross deviation may also occur locally in the plating bath. Therefore, the flow speed of the plating bath should be at least 0.03 m / s or more. On the other hand, if the flow speed is too fast, the flowing dross becomes too fine and attaches to the plating layer, so that the number of Al phases becomes excessive, and the effect of improving corrosion resistance in an acidic environment by the Al phase disappears.
[0132]
[0133] In addition, according to one aspect of the present invention, in order to achieve the target plating amount after plating is completed, a wiping treatment is performed on the molten steel sheet, and for example, a nitrogen (N2) or air knife may be used. At this time, the plating adhesion amount is not particularly limited, and is usually 20 to 400 g / m on one side. 2 Make it to the level.
[0134] In addition, according to one aspect of the present invention, cooling is performed after controlling the coating amount. At this time, the cooling is controlled so that the temperature of the steel sheet satisfies an average cooling rate of 6.0°C / s or more in the section from the Al phase crystallization temperature to 330°C. In the section from the Al phase crystallization temperature to 330°C, the faster the cooling, the slower the nucleus growth, and the finer the crystals become, so the cooling rate is controlled as described above. There is no need to specifically limit the upper limit of the cooling rate in the section, and it may be managed to a typical appropriate level in the relevant technical field in consideration of limitations of the cooling equipment, vibration, economic feasibility, etc. In the present invention, the Al phase crystallization nucleus generation site is a fine dross present in the plating layer before the plating layer solidification, but if the cooling rate is slow after the Al phase crystallization, the Al phase may grow and coarsen. Therefore, although several process factors are involved in controlling the number density and size of the Al phase as described above, as one of the control factors, in the range of the Al phase crystallization temperature to 330°C, cooling at an average cooling rate of 6.0°C / sec or more is required to secure the number density and size of the Al phase as intended in the present invention.
[0135] Meanwhile, since the plating layer solidification is completed when the steel plate temperature is below 330℃, the subsequent cooling speed is not very important, but considering productivity, a faster cooling speed is better.
[0136] Hereinafter, the present invention will be described in more detail through examples. However, it should be noted that the following examples are intended solely to illustrate the present invention and are not intended to limit the scope of the invention. This is because the scope of the invention is determined by the matters set forth in the patent claims and matters reasonably inferred therefrom.
[0137] (Example)
[0138] The plating bath was manufactured and used so that the composition of the components was as shown in Table 1 below. After manufacturing the plating bath, the final component confirmation was performed using ICP (Inductively Coupled Plasma Mass Spectrometry). Meanwhile, the presence of fine dross in the plating bath was confirmed by collecting a plating bath sample at a depth of 300 mm (in the thickness direction) from the plating bath surface, rapidly cooling it in water, and checking it using a TEM (Transmission Electron Microscope) at a magnification of 300,000x.
[0139] As the base steel sheet, hot-rolled steel sheet and cold-rolled steel sheet were used, and the composition of the base steel sheet was C: 0.017%, Si: 0.014%, Mn: 0.25%, P: 0.008%, S: 0.005%, Al: 0.03%, Nb: 0.02%, Cr: 0.1%, Ti: 0.02%, B: 0.015%, and the remainder was Fe and other unavoidable impurities.
[0140] The hot-rolled steel sheet was first pickled with a hydrochloric acid solution to remove iron oxides formed on the surface of the steel sheet during the hot rolling process, and then heated to 650℃ in a heating furnace under reducing conditions with a dew point temperature of -20℃, and then plating was performed under the conditions of Manufacturing Process A in Table 2 below. The cold-rolled steel sheet was first subjected to alkaline immersion and electrolytic degreasing to remove rolling oil, iron powder, and other foreign substances on the surface of the steel sheet, and then annealed at 840℃ in an annealing furnace under a reducing atmosphere, and then plating was performed under the conditions of Manufacturing Process B in Table 2 below. After plating, the plating weight was adjusted to 150g / ㎡ per side through N2 wiping.
[0141] After the plated steel plate was cut into a predetermined size for analysis, the plated layer was photographed using FE-SEM on a cross-sectional specimen in the thickness direction of the steel plate (meaning the direction perpendicular to the rolling direction), and the components were confirmed using EDS for accurate phase confirmation.
[0142] The images were taken at a magnification of 2000 times, and to ensure representativeness, 20 points were measured and analyzed from a 20 mm length of the specimen to confirm the image, and then the area ratio and number of each image were measured using an image analyzer, and the average value of the 20 images is shown in Table 3 below.
[0143] In order to evaluate corrosion resistance, the specimens were cut to a size of 80 mm x 150 mm, and three specimens were tested for each specimen and experimental condition, and then the average was calculated and evaluated based on the following criteria. The results were listed in Table 3 below.
[0144] Acid corrosion resistance
[0145] ◎: If the weight loss before and after the experiment is less than 1g / ㎡, it is evaluated as very good.
[0146] ○: If the weight loss before and after the experiment is more than 1 and less than 2 g / ㎡, it is evaluated as excellent.
[0147] △: If the weight loss before and after the experiment is more than 2 and less than 3g / ㎡, it is evaluated as defective.
[0148] ×: If the weight loss before and after the experiment exceeds 3g / ㎡, it is evaluated as very poor.
[0149] Neutral corrosion resistance
[0150] ◎: Cases where the red-blue occurrence time is 4200 hours or more are evaluated as very good.
[0151] ○: Cases where the red-rust occurrence time exceeds 3,500 hours and is less than 4,200 hours are evaluated as excellent.
[0152] △: If the red-rust occurrence time exceeds 2000 hours but is less than 3500 hours, it is evaluated as defective.
[0153] ×: If the red-and-blue occurrence time is less than 2000 hours, it is evaluated as very poor.
[0154] <Alkali corrosion resistance>
[0155] ◎: If the weight loss before and after the experiment is less than 2g / ㎡, it is evaluated as very good.
[0156] ○: If the weight loss before and after the experiment is more than 2 and less than 4 g / ㎡, it is evaluated as excellent.
[0157] △: If the weight loss before and after the experiment is more than 4 and less than 7 g / ㎡, it is evaluated as defective.
[0158] ×: If the weight loss before and after the experiment exceeds 7g / ㎡, it is evaluated as very poor.
[0159]
[0160] In addition, for the corrosion resistance test in an acidic environment, a sulfuric acid aqueous solution with a pH of 3.5 was used, for the corrosion resistance test in a neutral environment, a 3.5% NaCl aqueous solution with a pH of 6.7 was used, and for the corrosion resistance test in an alkaline environment, ammonia water with a pH of 12.5 was used.
[0161] In acid and alkaline tests, the specimens were immersed in the solution for 48 hours, then taken out and the corrosion loss was measured before and after the test. If the corrosion loss was small, it was evaluated as very good, and if the corrosion loss was large, it was evaluated as very poor.
[0162] In the neutrality test, the longer the time it takes for salt water to be sprayed on the steel plate until red rust (corrosion of the steel plate) occurs, the better the corrosion resistance is evaluated.
[0163] ClassificationAlMgFeSiCaSnSbMnC19.8204.810.003-----C213.5804.950.014-C312.5305.270.0080.12----C416.1505.460.038-0.0600.01-0.040C519.3806.100.0260.150.090-0.06-C614.2 005.260.120-0.010---C74.3604.230.003-----C810.4104.92------C919.0702.23-0.150 .010---C1018.4003.020.007-----C110.251-0.021-----C1231.1904.14-0.080.0020.008
[0164] (In Table 1 above, '-' means 0 wt%.)
[0165] Classification Manufacturing Process Plating Bath Composition (Table 1) Steel Sheet Inlet Temperature (℃) Plating Bath Temperature (℃) Plating Bath Flow Velocity (m / sec) Al Phase Crystallization Temperature ~330℃ Average Cooling rate (℃ / sec)B1AC14754650.0414.1B2C14854390.108.3B3C24704550.08 15.2B4C24554500.1311.2B5C247046108.4B6C24704700.052.7B7C248046 00.014.1B8C34704550.1012.6B9C34704600.066.7B10C34604600.013.0B 11C44904700.0810.1B12C44874650.4510.7B13C55004900.038.1B14C649 94720.049.4B15C74704600.0510.2B16C84754550.0511.8B17C94904850 .0510.7B18C114904600.059.1B19BC14804550.097.3B20C24664550.138. 4B21C248744506.8B22C34724510.1711.7B23C34814530.012.3B24C74824 510.099.2B25C94804510.042.3B26C1048045507.2B27C125105000.036.7
[0166] Classification MgZn2 Area ratio (%) Al phase Area ratio (%) Al phase Number density (number / 0.1mm) 2) Occupancy rate of Al phase with a linear length of 5㎛ or less in the long axis direction (%) Ratio of Al phase existing inside the MgZn2 phase or in contact with the MgZn2 phase (%) B125.26.670598.496 B221.35.157590.1100 B326.217.2272097.7100 B427.817.3400096.4100 B527.316.849065.697 B628.818.529972.8100 B727.817.33 5557.094B831.716.3235997.392B932.013.8198392.1100B1036.212.733251. 499B1132.820.9292593.991B1234.221.4630010089B1342.424.495086.492B14 26.916.4104291.599B1520.11.148100.0100B1624.79.734472.697B174.824. 529945.199B1800---B1922.85.250089.7100B2027.216.8293692.3100B2125.7 16.719833.295B2229.116.1300895.0100B2330.915.839929.894B2421.50.93 9100.092B251.724.120725.397B262.223.7186074.256B2719.837.040335.195
[0167] Classification Dross defect occurrence Acid corrosion resistance (pH 3.5) Neutral corrosion resistance (pH 6.7) Alkali corrosion resistance (pH 12.5) B1 None ○○◎ B2 None ○○○ B3 None ◎○○ B4 None ◎○○ B5 None ◎○△ B6 None ◎○△ B7 None ◎○X B8 None ◎◎◎ B9 None ◎◎◎ B10 None ○◎X B11 None ◎◎◎ B12 None △◎◎ B13 None ◎◎○ B14 Yes ◎◎○ B15 None X ○○ B16 None ○○△ B17 None ◎△ X B18 None XX△ B19 None ○○○ B20 None ◎○○ B21 None ◎○△ B22 None ◎◎○ B23 None ◎◎X B24 None △◎◎ B25 None ◎△ X B26 None △○△ B27 None ◎◎X
[0168] As can be seen from the experimental results in the table above, for examples B1 to B4, B8, B9, B11, B13, B19, B20, and B22 that satisfy the plating composition and manufacturing conditions of the present invention, the corrosion resistance was excellent or very excellent under all conditions of acidic, neutral, and alkaline environments. In addition, since the Fe content in the plating bath did not exceed 0.05%, which is the upper limit defined in the present invention, no dross adhesion defects occurred.
[0169]
[0170] Meanwhile, in the case of comparative examples B5 and B21, although the plating bath components and other manufacturing conditions were in accordance with the present invention, since there was no plating bath flow, the Al crystallization nucleation sites were small, and the number density of Al phases was less than 500 / 0.1㎟, which is the lower limit limited by the present invention. Therefore, since there were relatively many coarse Al phases, the corrosion resistance was excellent in acidic and neutral conditions, but poor in alkaline conditions.
[0171] Comparative Example B6 is a case where the cooling rate from the Al phase crystallization temperature to 330°C after plating is slower than 6.0°C / sec limited in the present invention. In this case, although there are many Al nuclei crystallization sites according to the present invention, it takes time until the Zn-Al binary and ternary eutectic phases other than the Al phase and MgZn2 phase crystallize, so the number density of the Al phase is less than 500 / 0.1㎟, which is the lower limit limited in the present invention, and the corrosion resistance in an alkaline environment is poor.
[0172] Comparative examples B7, B10, and B23 were cases where the plating bath flow rate was lower than the range limited in the present invention and the cooling rate from the Al phase crystallization temperature to 330°C was slower than 6°C / s limited in the present invention, the number density of the Al phase was less than 500 / 0.1㎟, which is the lower limit limited in the present invention, and the corrosion resistance in an alkaline environment was very poor.
[0173] Meanwhile, in the case of Comparative Example B12, the flow speed of the plating bath was 0.45 m / sec, which exceeded the range limited in the present invention. If the flow speed is too fast, the flowing dross becomes too fine and attaches to the plating layer, so that the number density of Al phases exceeds the upper limit limited in the present invention of 4000 / 0.1㎟, and the effect of improving corrosion resistance in an acidic environment by the Al phase disappears, resulting in poor corrosion resistance in an acidic environment.
[0174] In the case of Comparative Example B14, the Fe content in the plating bath exceeded the range limited in the present invention, and coarse dross was generated on the surface of the plating bath, resulting in a dross adhesion defect on the plated steel sheet.
[0175] Comparative examples B15 and B24 are cases where the Al content in the plating bath components is less than the range limited in the present invention, and the number density of the Al phase is outside the range limited in the present invention, so the corrosion resistance in acid is very poor.
[0176] Comparative Example B16 is a case where Fe was not present in the plating bath, and the number of Al phases was less than the range limited in the present invention, and the number of Al phases coarse and less than 5㎛ was lower than 80.0% limited in the present invention, resulting in poor corrosion resistance in an alkaline environment.
[0177] Comparative Example B17 is a case where the Mg content in the plating bath is lower than the range limited in the present invention and Fe is not added. The number density of Al phases is also low, so the corrosion resistance in an alkaline atmosphere is very poor and the corrosion resistance is also poor in neutral atmosphere.
[0178] Meanwhile, in Comparative Example B18, Mg was not added to the plating bath and Al was lower than the range limited in the present invention, so MgZn2 phase and Al phase were not crystallized in the plating layer, resulting in poor or very poor corrosion resistance in all acidic, neutral and alkaline atmospheres.
[0179] Comparative Example B25 is a case where the Mg content in the plating bath is lower than the range limited in the present invention and the cooling rate from the Al phase crystallization temperature to 330°C after plating in the plating bath without Fe addition is slower than 6.0°C / sec limited in the present invention, so the number density of Al phases in the plating layer is lower than the range limited in the present invention, and the number ratio of Al phases of 5 μm or less is also low, so that the corrosion resistance in an alkaline atmosphere is very poor and the corrosion resistance is poor even in a neutral atmosphere.
[0180] In the case of comparative example B26, the Mg content in the plating bath was lower than the range limited in the present invention and there was no plating bath flow, so the ratio of the Al phase existing inside the MgZn2 phase or in contact with the MgZn2 phase exceeded the lower limit of the present invention, and the corrosion resistance was very poor in an alkaline atmosphere and also poor in an acidic atmosphere.
[0181] In the case of comparative example B27, the Al content in the plating bath was higher than the range limited in the present invention and Fe was not added, so the number density of the Al phase was outside the range limited in the present invention, and the corrosion resistance in an alkaline atmosphere was very poor.
Claims
1. Steel plate; and Including an Al-Mg-Zn based plating layer provided on at least one surface of the above steel plate, The above plating layer has a number density of 500 to 4,000 Al phases / 0.1 mm that exist within the MgZn2 phase or in contact with the MgZn2 phase. 2 Person, galvanized steel sheet.
2. In paragraph 1, A plated steel sheet, wherein the above-mentioned plating layer contains, in weight %, Mg: 4.00 to 7.00%, Al: 8.000 to 20.000%, Fe: 0.002 to 0.050%, the remainder Zn, and other unavoidable impurities.
3. In paragraph 2, A plated steel sheet, wherein the plating layer further comprises at least one selected from, in weight %, Si: 0.2% or less (including 0%) and Ca: 0.2% or less (including 0%).
4. In paragraph 2, A plated steel sheet, wherein the plating layer further comprises at least one of the following groups (a) to (h). (a) Ni: 0.5% or less (b) La: 0.1% or less, Ce: 0.1% or less, Y: 0.1% or less, Sr: 1.0% or less, or more than one of the following (c) Ti: 0.1% or less (d) W: 0.5% or less (e) Cu: 2.0% or less (f) Cr: 0.5% or less, Mn: 0.5% or less, V: 0.5% or less, at least one of these (g) B: 0.1% or less, P: 0.1% or less, 1 or more types (h) Sn: 1.0% or less, Sb: 1.0% or less, Bi: 1.0% or less, or at least one of these 5. In paragraph 1, The above-mentioned plating layer is a plated steel sheet in which the ratio of the number of Al phases existing within the MgZn2 phase or in contact with the MgZn2 phase to the total number of Al phases is 85% or more and 100% or less.
6. In paragraph 1, A plated steel sheet in which the average longitudinal straight length of the Al phase existing within the MgZn2 phase or in contact with the MgZn2 phase is 5 ㎛ or less (excluding 0 ㎛).
7. In paragraph 1, A plated steel sheet in which the number ratio of Al phases existing within the MgZn2 phase or in contact with the MgZn2 phase and having a longitudinal straight length of 5 ㎛ or less (excluding 0 ㎛) is 90.0 to 100.0% compared to the total number of Al phases.
8. A step of hot-dip galvanizing by immersing the steel sheet in a plating bath containing, by weight%, Mg: 4.00 to 7.00%, Al: 8.000 to 20.000%, Fe: 0.002 to 0.050%, the remainder Zn and other unavoidable impurities, and having a temperature of 430 to 520°C and a flow velocity of 0.03 to 0.20 m / s; A step of performing a wiping treatment on the above molten steel plate; and A method for manufacturing a plated steel sheet, comprising: a step of cooling the above-mentioned wiping-treated steel sheet so that an average cooling rate of 6.0°C / s or more is satisfied in a range from the crystallization temperature of the Al phase to 330°C.
9. In paragraph 8, A method for manufacturing a plated steel sheet, wherein the above plating bath further includes at least one selected from the group consisting of Si: 0.20% or less (including 0%) and Ca: 0.200% or less (including 0%) in weight %.
10. In paragraph 8, A method for manufacturing a plated steel sheet, wherein the plating bath further comprises at least one of the following groups (a) to (h). (a) Ni: 0.5% or less (b) La: 0.1% or less, Ce: 0.1% or less, Y: 0.1% or less, Sr: 1.0% or less, or more than one of the following (c) Ti: 0.1% or less (d) W: 0.5% or less (e) Cu: 2.0% or less (f) Cr: 0.5% or less, Mn: 0.5% or less, V: 0.5% or less, at least one of these (g) B: 0.1% or less, P: 0.1% or less, at least one of these (h) Sn: 1.0% or less, Sb: 1.0% or less, Bi: 1.0% or less, or at least one of these 11. In paragraph 8, A method for manufacturing a plated steel sheet, wherein the temperature of the plating bath is maintained at a temperature 20 to 100°C higher than the solidification initiation temperature (Ts).
12. In paragraph 8, A method for manufacturing a plated steel sheet, wherein the average diameter of the flowing dross in the plating bath is controlled to be 0.05㎛ or less (excluding 0㎛).