Method for producing polymer, method for producing curable composition, method for producing cured product, and method for producing contact lens using curable composition

MYPI2025003792A0Undetermined Publication Date: 2024-06-23SEED CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025003792
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-10-20
Filing Date
2023-12-20
Publication Date
2024-06-23

AI Technical Summary

Technical Problem

Conventional methods for producing silicone hydrogel contact lenses face challenges in removing unreacted silicon-containing monomers and impurities without using flammable organic solvents, which are hazardous and increase manufacturing costs, while also compromising oxygen permeability and comfort.

Method used

A method involving the polymerization of specific monomers followed by purification using subcritical or supercritical fluids to produce a high-purity polymer, allowing for the removal of poorly water-soluble silicon-containing compounds without hazardous solvents, thereby enhancing the manufacturing efficiency and safety.

Benefits of technology

This method enables the production of high-purity silicone hydrogel contact lenses with improved oxygen permeability and reduced manufacturing costs, ensuring both safety and effectiveness in removing impurities without using hazardous solvents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025003792_DRAWING_001
    Figure PI2025003792_DRAWING_001
  • Figure PI2025003792_DRAWING_002
    Figure PI2025003792_DRAWING_002
  • Figure PI2025003792_DRAWING_003
    Figure PI2025003792_DRAWING_003
Patent Text Reader

Abstract

The present invention provides: a method for producing a high-purity polymer (A); and a method for producing a silicone hydrogel lens at a low cost. A method for producing a polymer (A) according to the present invention comprises: (step 1) a step of obtaining a polymer (A1) by polymerizing a first monomer (a) that has one ethylenically unsaturated group; (step 2) a step of obtaining a polymer (A2) by having the polymer (A1) react with a second monomer that has an ethylenically unsaturated group; and (step 3) a step of obtaining a polymer (A) by purifying the polymer (A2) with use of a subcritical or supercritical fluid. The first monomer is selected from one of the first group consisting of hydroxyl group-containing monomers, and the second group consisting of isocyanate compounds of (meth)acrylic acids, anhydrides of (meth)acrylic acids, and halides of (meth)acrylic acids. The second monomer is selected from the other of the first group and the second group. Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing polymer, method for producing curable composition, method for producing cured product, and method for producing contact lens using the curable composition

[0001] The present invention relates to a method for producing a polymer, a method for producing a curable composition containing the polymer, a method for producing a cured product obtained by curing the curable composition, and a method for producing a hydrogel contact lens using the curable composition.

[0002] Because there are no blood vessels in the eye, the oxygen needed to maintain healthy eye cells cannot be supplied via the blood but is instead supplied directly from the atmosphere via the cornea. Wearing contact lenses prevents oxygen from reaching the cornea, and prolonged contact lens wear can cause corneal oxygen deficiency, leading to eye diseases such as hyperemia, corneal edema, and vascular infiltration. Therefore, oxygen permeability, one of the physical properties of contact lenses, is an important property that affects the amount of oxygen supplied to eye cells.

[0003] Contact lenses are broadly classified into hard contact lenses (HCLs) and soft contact lenses (SCLs). HCLs have excellent optical properties and oxygen permeability, but have the drawback of being prone to foreign body sensation when worn due to the hardness of the material. SCLs have excellent wearing comfort, but have the drawback of having low oxygen permeability due to the material.

[0004] In recent years, silicone hydrogel contact lenses (SHGCLs), which combine the high oxygen permeability of HCLs with the excellent wearing comfort of SCLs, have been developed and are becoming widely used.

[0005] However, the production cost of SHGCL is significantly higher than that of SCL that does not contain a silicon-containing monomer. This is because the production of SHGCL requires the use of large amounts of organic solvents such as isopropanol or methyl ethyl ketone (several to several hundred times the dry weight of the lens) to remove unreacted silicon-containing monomer from the cured product after curing. Furthermore, flammable organic solvents such as isopropanol and methyl ethyl ketone (hazardous materials under the Fire Service Act of Japan) pose a high risk of fire and other disasters, and explosion-proof equipment is required as a disaster prevention measure, resulting in enormous equipment costs.

[0006] Therefore, various studies have been conducted with the aim of efficiently removing unreacted monomers and impurities in the production of contact lenses, particularly silicone hydrogel contact lenses.

[0007] For example, a method for producing a vinyl monomer containing a tris(trimethylsilyloxy)silyl group (hereinafter referred to as a TRIS group) by reacting a vinyl monomer containing a TRIS group having a solubility or dispersibility of at least about 5% by weight in water with an actinic radiation-crosslinkable silicone-containing prepolymer made thereof has been disclosed, with the aim of improving the solubility of the vinyl monomer containing a tris(trimethylsilyloxy)silyl group in water (hereinafter referred to as a TRIS group) (see Patent Document 1).

[0008] Also disclosed is a method for producing a silicone hydrogel lens by subjecting a polymerizable composition containing a copolymerizable siloxane compound, first and second hydrophilic monomers, and first and second crosslinkable monomers as its constituent components to two-stage ultraviolet irradiation, and then extracting unreacted components using only an aqueous solution (see Patent Document 2).

[0009] Furthermore, a method has been disclosed in which a contact lens composition containing an alcohol group-containing polysiloxane dimethacrylate is polymerized in a contact lens mold made of polyethylene vinyl alcohol resin to obtain a polymer, and then the polymer is treated under low pressure with supercritical carbon dioxide, or with supercritical carbon dioxide and an extraction aid (entrainer), thereby removing unpolymerized monomers and impurities (see Patent Document 3).

[0010] Japanese Patent No. 6065988 Japanese Patent No. 6906556 Japanese Patent No. 3640934

[0011] However, the vinyl monomer containing a TRIS group obtained by the method described in Patent Document 1 does not have sufficient solubility or dispersibility in water due to the TRIS group, and it is therefore thought to be difficult to extract the unreacted vinyl monomer containing a TRIS group with water from a silicone-containing prepolymer that contains this monomer as a constituent component.

[0012] According to the method described in Patent Document 2, siloxane compounds that are poorly soluble in water are polymerized completely without remaining. However, it is unlikely that 100% of the siloxane compounds are polymerized. Furthermore, raw materials for silicon-containing monomers that exist as impurities in siloxane compounds are not incorporated into the polymer network and have low solubility in water, so organic solvents must be used to remove the raw materials for silicon-containing monomers.

[0013] In Patent Document 3, when a supercritical fluid is used for treatment under a high pressure exceeding 20 MPa, the object is less easily separable from the mold and is more likely to have minute defects on the surface of the object. Therefore, treatment is performed under a low pressure of 6 MPa to 16 MPa. However, while treatment with a supercritical fluid under low pressure reduces the adverse effects on the object, it naturally reduces the effectiveness of removing unreacted materials and impurities. Therefore, there is room for further study on a method for effectively removing impurities and the like without reducing workability or causing defects in the object.

[0014] As described above, with conventional techniques, it has been difficult to effectively remove silicon-containing compounds from the polymer network of silicone hydrogel, which contains poorly water-soluble silicon-containing compounds as its constituent components, without using flammable organic solvents (hazardous materials under the Fire Service Act of Japan) and without causing adverse effects on the material being treated.

[0015] The present invention has been made in view of these circumstances, and aims to provide a manufacturing method for obtaining a highly pure polymer (with low impurity content), as well as an inexpensive method for manufacturing a silicone hydrogel lens containing the polymer.

[0016] That is, the present invention relates to the following [1] to

[18] . Note that in this application, "(Numerical value 1) to (Numerical value 2)" indicates that the upper and lower limits are included. [1] A method for producing polymer (A), comprising: (Step 1) a step of polymerizing a first monomer (a) having an ethylenically unsaturated group to obtain polymer (A1); (Step 2) a step of reacting polymer (A1) with a second monomer having an ethylenically unsaturated group to obtain polymer (A2); and (Step 3) a step of purifying polymer (A2) using a subcritical or supercritical fluid to obtain polymer (A), wherein the first monomer is selected from one of a first group consisting of hydroxyl group-containing monomers, or a second group consisting of isocyanate compounds of (meth)acrylic acid, anhydrides of (meth)acrylic acid, and halides of (meth)acrylic acid, and the second monomer is selected from the other of the first group and the second group. [2] The method for producing polymer (A) according to the preceding item [1], wherein in step 1, a silicon-containing monomer (b) having one ethylenically unsaturated group is polymerized together with the first monomer (a). [3] The method for producing polymer (A) according to the preceding item [2], wherein in step 1, an amide group-containing monomer (c) is further polymerized. [4] The method for producing polymer (A) according to the preceding item [3], wherein in step 1, an alkyl group-containing monomer (d) having one ethylenically unsaturated group and having 1 to 18 carbon atoms is polymerized together with the first monomer (a), the silicon-containing monomer (b), and the amide group-containing monomer (c). [5] The method for producing polymer (A) according to any one of the preceding items [1] to [4], wherein the first monomer is a hydroxyl group-containing monomer. [6] The method for producing polymer (A) according to the preceding item [5], wherein the second monomer is an isocyanate compound of (meth)acrylic acid. [7] The method for producing polymer (A) according to the above item [5], wherein the second monomer is an anhydride of (meth)acrylic acid. [8] The method for producing polymer (A) according to the above item [5], wherein the second monomer is a halide of (meth)acrylic acid.[9] A method for producing polymer (A) according to any one of the preceding items [1] to [4], wherein the first monomer is an isocyanate compound of (meth)acrylic acid, and the second monomer is a hydroxyl group-containing monomer.

[10] A method for producing polymer (A) according to any one of the preceding items [1] to [9], wherein carbon dioxide alone is used as the subcritical or supercritical fluid.

[11] A method for producing polymer (A) according to any one of the preceding items [1] to [9], wherein a mixture of carbon dioxide and an entrainer is used as the subcritical or supercritical fluid.

[12] A method for producing polymer (A) according to the preceding item

[11] , wherein the mixture of carbon dioxide and an entrainer consists of 80.0 to 99.9% by weight of carbon dioxide and 0.1 to 20.0% by weight of an entrainer.

[13] A method for producing polymer (A) according to the preceding item

[11] or

[12] , wherein the entrainer is one or more selected from methanol, ethanol, 1-propanol, 2-propanol, 2-methoxyethanol, and 1,4-dioxane.

[14] A method for producing polymer (A) according to any one of the preceding items [1] to

[13] , wherein the polymer (A) has a weight-average molecular weight of 5,000 to 300,000.

[15] A method for producing a curable composition containing polymer (A) according to any one of the preceding items [1] to

[14] , a hydrophilic monomer (B), and a radical polymerization initiator (C).

[16] A method for producing a cured product obtained from the curable composition according to the preceding item

[15] .

[17] A method for producing the curable composition according to the preceding item

[15] , which is used for a contact lens.

[18] A method for producing a silicone hydrogel contact lens using the curable composition for contact lenses according to the preceding item

[17] .

[0017] The manufacturing method of the present invention can produce high-purity polymers and silicone hydrogel contact lenses containing the polymers. Furthermore, the cured product of the curable composition comprising the high-purity polymer, hydrophilic monomer, and polymerization initiator obtained by the method of the present invention, or the silicone hydrogel lens, can be easily cleaned, allowing for inexpensive production. The water-insoluble silicon-containing compounds present in the hydrophilic polymer network can be removed without using flammable organic solvents (a hazardous material under the Fire Service Act of Japan), improving operational safety and efficiency. Furthermore, since the method of the present invention uses the polymer as a constituent component of the silicone hydrogel contact lens, the process of extracting impurities after contact lens formation is simplified, which is expected to reduce manufacturing costs.

[0018] 1 is a GPC chart of polymer (P-5), a GPC chart of polymer (P-6), and a GPC chart of FM-0711.

[0019] In this specification, "(meth)acrylic" means "acrylic" and / or "methacrylic," and "(meth)acrylate" means "acrylate" and / or "methacrylate." Furthermore, in this specification, "%" and "parts" are all expressed by weight unless otherwise specified.

[0020] The method for producing polymer (A) of the present invention comprises the following steps (Step 1) to (Step 3): (Step 1) a step of polymerizing a first monomer (a) having an ethylenically unsaturated group to obtain polymer (A1); (Step 2) a step of reacting polymer (A1) with a second monomer having an ethylenically unsaturated group to obtain polymer (A2); and (Step 3) a step of purifying polymer (A2) using a subcritical or supercritical fluid to obtain polymer (A).

[0021] The first monomer is selected from either the first group or the second group below, and the second monomer is selected from the other of the first group or the second group: First group: hydroxyl group-containing monomers Second group: isocyanate compounds of (meth)acrylic acid, anhydrides of (meth)acrylic acid, and halides of (meth)acrylic acid Hereinafter, each component of the first group and the second group will be described.

[0022] First Group: Hydroxyl Group-Containing Monomer The hydroxyl group-containing monomer is a hydroxyl group-containing monomer having one ethylenically unsaturated group and not containing silicon. The ethylenically unsaturated group in the present invention is a curable substituent, and examples thereof include a styryl group, a vinyl group, an allyl group, a maleimide group, a (meth)acryloyl group, and a (meth)acrylamide group. Examples of hydroxyl group-containing monomers include acrylic acid, methacrylic acid, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, glycerol (meth)acrylate, butoxyethylene glycol (meth)acrylate, caprolactone-modified 2-hydroxyethyl (meth)acrylate, N-(4-hydroxyphenyl)maleimide, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, polytetramethylene glycol mono(meth)acrylate, and N-(2-hydroxyethyl)acrylamide.

[0023] Second Group: Isocyanate Compounds of (Meth)acrylic Acid The isocyanate compounds of (meth)acrylic acid are acrylic acid esters or methacrylic acid esters having an isocyanate group. Examples of the isocyanate compounds of (meth)acrylic acid include 2-isocyanatoethyl methacrylate (trade name: Karenz MOI, manufactured by Resonac Corporation), 2-isocyanatoethyl acrylate (trade name: Karenz AOI, manufactured by Resonac Corporation), 2-(2-methacryloyloxyethyloxy)ethyl isocyanate (trade name: Karenz MOI-EG, manufactured by Resonac Corporation), and 1,1-(bisacryloyloxymethyl)ethyl isocyanate (trade name: Karenz BEI, manufactured by Resonac Corporation).

[0024] When a hydroxyl group-containing monomer is used as the first monomer (a) and an isocyanate compound of (meth)acrylic acid is used as the second monomer, polymer (A2) can be obtained by reacting polymer (A1) obtained in step 1 with the isocyanate compound of (meth)acrylic acid in step 2. Specifically, this reaction involves adding an isocyanate compound having a (meth)acrylate group to the hydroxyl groups of polymer (A1), and the reaction temperature is preferably 70 to 100° C. The isocyanate compound having a (meth)acrylate group is mixed and reacted so that the amount of isocyanate groups per equivalent of hydroxyl groups in polymer (A1) is preferably 1.0 to 1.2 equivalents, more preferably 1.05 to 1.1 equivalents.

[0025] On the other hand, when an isocyanate compound of (meth)acrylic acid is used as the first monomer (a) and a hydroxyl group-containing monomer is used as the second monomer, polymer (A2) can be obtained by reacting polymer (A1) obtained in step 1 with the hydroxyl group-containing monomer in step 2. Specifically, this is a reaction in which the hydroxyl group-containing monomer is added to the isocyanate groups of polymer (A1), and the reaction temperature is preferably 70 to 100° C. The hydroxyl group-containing monomer is mixed and reacted so that the amount of hydroxyl groups per equivalent of isocyanate groups in polymer (A1) is preferably 1.0 to 1.2 equivalents, more preferably 1.05 to 1.1 equivalents.

[0026] It is preferable to use a catalyst such as dibutyltin dilaurate to promote the addition reaction between the hydroxyl group and the isocyanate group in step 2. Furthermore, a polymerization inhibitor such as paramethoxyphenol, methylhydroquinone, or dibutylhydroxytoluene can also be used to prevent polymerization during the reaction.

[0027] Second Group: (Meth)acrylic Anhydride The (meth)acrylic anhydride refers to acrylic anhydride and / or methacrylic anhydride. When a hydroxyl group-containing monomer is used as the first monomer (a) and (meth)acrylic anhydride is used as the second monomer, polymer (A2) can be obtained by reacting polymer (A1) obtained in step 1 with acrylic anhydride and / or methacrylic anhydride. Specifically, this reaction involves adding acrylic anhydride and / or methacrylic anhydride to the hydroxyl groups of polymer (A1), and the reaction temperature is preferably 80 to 120°C. The acrylic anhydride and / or methacrylic anhydride are mixed and reacted in an amount of preferably 1.0 to 1.2 equivalents, more preferably 1.05 to 1.1 equivalents, per equivalent of the hydroxyl groups of polymer (A1). In order to promote the reaction, it is preferable to use a catalyst such as triphenylphosphine, 2,4,6-tris(dimethylaminomethyl)phenol, triethanolamine, tetraethylammonium chloride, trimethylglycine, etc. Furthermore, in order to prevent polymerization during the reaction, a polymerization inhibitor such as paramethoxyphenol, methylhydroquinone, dibutylhydroxytoluene, etc. may also be used.

[0028] Second Group: Halides of (Meth)acrylic Acid Specific examples of the halides of (meth)acrylic acid include (meth)acrylic acid fluoride, (meth)acrylic acid chloride, (meth)acrylic acid bromide, and (meth)acrylic acid iodide.

[0029] When a hydroxyl group-containing monomer is used as the first monomer (a) and a (meth)acrylic acid halide is used as the second monomer, polymer (A2) can be obtained by reacting polymer (A1) obtained in step 1 with the (meth)acrylic acid halide. Specifically, this is a dehydrohalogenation reaction between the hydroxyl groups of polymer (A1) and the halogen groups of the (meth)acrylic acid halide. The reaction temperature is preferably 30 to 100°C. The (meth)acrylic acid halide is preferably used in an amount equivalent to the hydroxyl groups of polymer (A1). Furthermore, a polymerization inhibitor, such as paramethoxyphenol, methylhydroquinone, or dibutylhydroxytoluene, can be used to prevent polymerization during the reaction.

[0030] Since the reaction between the polymer (A1) and a halide of (meth)acrylic acid is a dehydrohalogenation reaction, it is preferable to add a tertiary amine to the reaction solution in advance in order to trap the generated hydrogen halide and further promote the reaction. Examples of tertiary amines include triethylamine, pyridine, and 1-methylimidazole. The amount of the tertiary amine used is preferably equimolar to 2 times, and more preferably equimolar to 1.5 times, the amount of (meth)acrylic acid chloride.

[0031] The content of the first monomer (a) (hereinafter also referred to as "component (a)") in polymer (A1) is not particularly limited, but is, for example, 0.01 to 100 wt %, preferably 0.1 to 30 parts by weight, more preferably 0.1 to 10 wt %, and even more preferably 0.2 to 5 wt %, based on the total weight of all comonomer components. Here, "total comonomer components" refers to all comonomer components that are raw materials for polymer (A1). That is, it includes component (a), component (b) and component (c) described below, but does not include polymerization initiators, etc. If the amount of component (a) is less than 0.01 wt %, reactivity will be poor. Note that component (a) can be used alone or in a mixture of two or more types in any ratio.

[0032] In step 1, polymer (A1) may be obtained by polymerizing a silicon-containing monomer (b) having one ethylenically unsaturated group (hereinafter also referred to as "component (b)") together with component (a). Component (b) is a component that contributes to the flexibility of polymer (A).

[0033] Component (b) is a silicon-containing monomer having one ethylenically unsaturated group. Component (b) is not particularly limited, but examples include α-(meth)acryloxy-ω-butylpolydimethylsiloxane, (meth)acryloxypropyltris(trimethylsiloxy)silane, (meth)acrylamide silicone, (meth)acryloxyethylcarbamoyloxysilicone, and silicone (meth)acrylate represented by the following formula (1). The silicone (meth)acrylate represented by the following formula (1) is commercially available as FM-0711 (manufactured by JNC Corporation, molecular weight 1,000). Component (b) can be used alone or in combination of two or more types in any ratio.

[0034]

[0035] The content of component (b) in polymer (A1) is not particularly limited, but is, for example, 20 to 90 wt %, preferably 30 to 80 wt %, and more preferably 40 to 70 wt %, based on the total weight of all comonomer components. If the blending amount is less than 20 wt %, the oxygen permeability and flexibility of the resulting cured product will be reduced. On the other hand, if the blending amount is more than 90 wt %, the surface lubricity of the cured product will be poor.

[0036] In step 1, polymer (A1) may be obtained by polymerizing an amide group-containing monomer (c) (hereinafter also referred to as "component (c)") having one ethylenically unsaturated group together with components (a) and (b). Component (c) is a monomer that has no hydroxyl group or silicon, has an amide group, and is soluble in water at any ratio. Component (c) is a component that contributes to improving the hydrophilicity of polymer (A).

[0037] Examples of component (c) include, but are not limited to, acryloylmorpholine, N,N-dimethylacrylamide, N,N-diethylacrylamide, N-vinylpyrrolidone, N-vinyl-N-methylacetamide, N-vinyl-N-ethylacetamide, N-vinyl-N-ethylformamide, and N-vinylformamide. In the production process of a curable composition containing polymer (A), from the viewpoint of improving the compatibility between polymer (A) and hydrophilic monomer (B) and contributing to improving the transparency of the cured product, component (c) is preferably N,N-dimethylacrylamide, N,N-diethylacrylamide, or N-vinylpyrrolidone.

[0038] The content of component (c) in polymer (A1) is not particularly limited, but is, for example, 1 to 50 wt %, preferably 3 to 40 wt %, and more preferably 5 to 30 wt %, based on the total weight of all comonomer components. If the blending amount is less than 1 wt %, the compatibility with the hydrophilic monomer used in the curable composition will be poor, causing the curable composition to become cloudy. If the blending amount is more than 50 wt %, the viscosity of the polymer will increase, making it difficult to work with. Note that component (c) can be used alone or in a mixture of two or more types in any ratio.

[0039] In step 1, polymer (A1) may be obtained by polymerizing an alkyl group-containing monomer (d) (hereinafter also referred to as "component (d)") having one ethylenically unsaturated group and having 1 to 18 carbon atoms together with components (a) to (c). Component (d) does not contain a hydroxyl group, an amide group, or silicon. Component (d) is a component that contributes to the compatibility of component (b) and component (c).

[0040] Examples of the component (d) include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, t-butyl (meth)acrylate, n-butoxyethyl (meth)acrylate, n-butoxydiethylene glycol (meth)acrylate, pentyl (meth)acrylate, trimethylcyclohexyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, and hexyl (meth)acrylate. acrylate, 2-ethylhexyl (meth)acrylate, cyclohexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, methoxydiethylene glycol (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, 3-methyltridecyl (meth)acrylate, 6-methyl Tridecyl (meth)acrylate, 7-methyltridecyl (meth)acrylate, 2,1,1-dimethyldodecyl (meth)acrylate, 2,7-dimethyl-4,5-diethyloctyl (meth)acrylate, pentadecyl (meth)acrylate, stearyl (meth)acrylate, i-stearyl (meth)acrylate, allyl (meth)acrylate, tricyclodecane (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate

[0043] Examples of the alkyl (meth)acrylate include linear, branched, or cyclic alkyl (meth)acrylates such as dicyclopentadieneoxyethyl (meth)acrylate, 1-adamantyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, 2-ethyl-2-adamantyl (meth)acrylate, and 1-adamantyl (meth)acrylate. From the viewpoint of flexibility of the cured product, however, n-butyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and lauryl (meth)acrylate are preferred.

[0041] It is also preferable to use an alkyl group-containing monomer (d-1) (hereinafter also referred to as "component (d-1)") having one ethylenically unsaturated group and a urethane bond and having 1 to 18 carbon atoms as component (d). Component (d-1) does not contain a hydroxyl group, an amide group, or silicon. Component (d-1) contributes to the compatibility of component (b) and component (c) and also has the effect of improving the strength of the cured product.

[0042] The method for obtaining component (d-1) is not particularly limited, and examples thereof include a method of reacting an alcohol compound (I) having from 1 to 18 carbon atoms (hereinafter also simply referred to as "component (I)") with an isocyanate compound (II) having one (meth)acrylate group (hereinafter also simply referred to as "component (II)"), or a method of reacting an isocyanate compound (III) having from 1 to 18 carbon atoms (hereinafter also simply referred to as "component (III)") with a (meth)acrylate compound (IV) having one hydroxyl group (hereinafter also simply referred to as "component (IV)").

[0043] When reacting component (I) with component (II), the target component (d-1) can be obtained by mixing component (II) with component (I) so that the amount of isocyanate groups per equivalent of hydroxyl groups in component (I) is 1.0 to 1.2 equivalents, preferably 1.05 to 1.1 equivalents, and reacting at a reaction temperature of 70 to 90° C. When reacting component (III) with component (IV), the target component (d-1) can be obtained by mixing component (III) with component (IV) so that the amount of hydroxyl groups per equivalent of isocyanate is 1.0 to 1.2 equivalents, preferably 1.05 to 1.1 equivalents, and reacting at a reaction temperature of 70 to 90° C.

[0044] Examples of component (I) include methyl alcohol, ethyl alcohol, butyl alcohol, hexyl alcohol, octyl alcohol, tridecanol, lauryl alcohol, myristyl alcohol, cetyl alcohol, and stearyl alcohol.

[0045] Examples of component (II) include 2-isocyanatoethyl methacrylate (Karenz (registered trademark) MOI, manufactured by Resonac Corporation), 2-isocyanatoethyl acrylate (Karenz (registered trademark) AOI, manufactured by Resonac Corporation), and 2-(2-methacryloyloxyethyloxy)ethyl isocyanate (Karenz (registered trademark) MOI-EG, manufactured by Resonac Corporation).

[0046] Examples of component (III) include methyl isocyanate, ethyl isocyanate, butyl isocyanate, hexyl isocyanate, heptyl isocyanate, octyl isocyanate, nonyl isocyanate, decyl isocyanate, dodecyl isocyanate, and octadecyl isocyanate (Millionate O, manufactured by Hodogaya Chemical Co., Ltd.).

[0047] Examples of component (IV) include hydroxy C2-C4 alkyl (meth)acrylates such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxybutyl (meth)acrylate, dimethylolcyclohexyl mono(meth)acrylate, hydroxycaprolactone (meth)acrylate, hydroxyl group-terminated polyalkylene glycol (meth)acrylate, and glycerin mono(meth)acrylate.

[0048] Component (d-1) is commercially available as 2-[[(butylamino)carbonyl]oxy]ethyl acrylate (manufactured by Sigma-Aldrich) represented by the following formula (2).

[0049]

[0050] The content of component (d) in polymer (A1) is not particularly limited, but is, for example, 1 to 50 wt %, preferably 3 to 40 wt %, and more preferably 5 to 30 wt %, based on the total weight of all comonomer components. If the blending amount is less than 1 wt %, the effect of improving the compatibility between components (b) and (c) cannot be obtained. If the blending amount is more than 50 wt %, a cured product with high strength cannot be obtained.

[0051] Materials other than components (a) to (d) may be added arbitrarily to improve the performance of polymer (A). Examples of materials other than components (a) to (d) are listed below, but are not limited to these.

[0052] In order to impart an ultraviolet-shielding function to the polymer (A), a monomer that absorbs ultraviolet light can be used. Examples of the ultraviolet-absorbing monomer include 2-(2'-hydroxy-5'-methacryloyloxyethylphenyl)-2H-benzotriazole (trade name: RUVA-93, manufactured by Otsuka Chemical Co., Ltd.), 2-hydroxy-4-(meth)acryloyloxybenzophenone, 2-hydroxy-4-(meth)acryloyloxy-5-t-butylbenzophenone, 2-(2'-hydroxy-5'-(meth)acryloyloxyethylphenyl)-5-chloro-2H-benzotriazole, and 2-hydroxy-4-methacryloyloxymethylphenyl benzoate.

[0053] In order to make polymer (A) have antifouling function against components such as protein and lipid in tear fluid in the cured product, the monomer having fluoroalkyl group can be used.As the monomer having fluoroalkyl group, for example, trifluoroethyl (meth) acrylate, tetrafluoroethyl (meth) acrylate, trifluoropropyl (meth) acrylate, tetrafluoropropyl (meth) acrylate, pentafluoropropyl (meth) acrylate, hexafluorobutyl (meth) acrylate, hexafluoroisopropyl (meth) acrylate, heptafluorobutyl (meth) acrylate, octafluoropentyl (meth) acrylate, nonafluoropentyl (meth) acrylate, dodecafluoropentyl (meth) acrylate, dodecafluoroheptyl (meth) acrylate, dodecafluorooctyl (meth) acrylate and tridecafluoroheptyl (meth) acrylate can be mentioned. Trifluoroethyl (meth)acrylate, tetrafluoroethyl (meth)acrylate, hexafluoroisopropyl (meth)acrylate, octafluoropentyl (meth)acrylate, and dodecafluorooctyl (meth)acrylate are preferably used, and trifluoroethyl (meth)acrylate is most preferred.

[0054] To improve the storage stability of the polymer (A), a monomer having a polymerization inhibitor effect can be used. Examples of the monomer having a polymerization inhibitor effect include 4-hydroxyphenyl methacrylate (trade name: PQMA, manufactured by Showa Denko Materials Co., Ltd.), 4-hydroxyphenyl acrylamide (trade name: HMAd, manufactured by Osaka Organic Chemical Industry Co., Ltd.), 4-allyl-2,6-di-t-butylphenol (trade name: TRIAM-100, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl acrylate (trade name: Sumilizer GS, manufactured by Sumitomo Chemical Co., Ltd.), and 2,4-di-t-amyl-6-[1-(3,5-di-t-amyl-2-hydroxyphenyl)ethyl]phenyl acrylate (trade name: Sumilizer GM, manufactured by Sumitomo Chemical Co., Ltd.).

[0055] The polymer (A1) can be obtained by a conventionally known method such as solution polymerization, bulk polymerization, suspension polymerization, etc. For example, in the case of solution polymerization, the polymer (A1) can be obtained by adding dropwise a monomer solution prepared by mixing a comonomer in a predetermined ratio in an organic solvent and a polymerization initiator under a nitrogen gas flow at a reaction temperature of 80 to 150°C to cause a polymerization reaction.

[0056] Examples of the polymerization initiator include a cationic polymerization initiator, an anionic polymerization initiator, and a radical polymerization initiator, and a radical polymerization initiator is preferred.

[0057] Examples of the radical polymerization initiator include various azo compounds or peroxides as thermal radical polymerization initiators. Specific examples include 2,2'-azobisisobutyronitrile, 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), dimethyl 2,2'-azobisbutyrate, 2,2'-azobis(2,4,4-trimethylpentane)diisobutylyl peroxide, di(3,5,5-trimethylhexanoyl)peroxide, and dilauroyl peroxide. Side, distearoyl peroxide, di-n-propyl peroxydicarbonate, diisopropyl peroxydicarbonate, di(4-tert-butylcyclohexyl) peroxydicarbonate, di(2-ethoxyethyl) peroxydicarbonate, di(2-ethylhexyl) peroxydicarbonate, di(3-methoxybutyl) peroxydicarbonate, cumyl peroxyneodecanoate, 1,1,3,3-tetramethylbutyl peroxyneodecanoate, 1-cyclohexyl-1-methylethyl Peroxyneodecanoate, tert-hexylperoxyneodecanoate, tert-butylperoxyneodecanoate, tert-hexylperoxypivalate, tert-butylperoxypivalate, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, 2,5-dimethyl-2,5-di(2-hexanoyl)peroxyhexane, tert-hexylperoxy-2-ethylhexanoate, tert-butylperoxy-2-ethylhexanoate, tert- Butyl peroxyisobutyrate, tert-hexylperoxyisopropyl carbonate, tert-butylperoxymaleic acid, tert-butylperoxy-3,5,5-trimethylhexanoate, tert-butylperoxylaurate, 2,5-dimethyl-2,5-di(3-methylbenzoylperoxy)hexane, tert-butylperoxyisopropyl carbonate, tert-butylperoxy-2-ethylhexyl carbonate, tert-hexylperoxybenzoate, 2,Examples of the radical polymerization initiator include 5-dimethyl-2,5-di(benzoylperoxy)hexane, tertiary butylperoxyacetic acid, and tertiary butylperoxybenzoate. One or more radical polymerization initiators can be used in any combination.

[0058] Examples of cationic polymerization initiators include inorganic acids such as sulfuric acid and hydrochloric acid, CF 3 COOH and CCl 3 Organic acids such as COOH, CF 3 SO3H and HClO 4 Examples of super strong acids include:

[0059] Examples of the anionic polymerization initiator include butyllithium, Na-naphthalene complex, alkali metals, alkyllithium compounds, sodium amide, Grignard reagents, and lithium alkoxides.

[0060] The amount of the polymerization initiator is not particularly limited, but is, for example, 0.01 to 10.0 wt %, preferably 0.05 to 9.0 wt %, and more preferably 0.1 to 8.0 wt %, relative to the total weight of the comonomers. If the amount of the polymerization initiator is less than 0.01 wt %, the molecular weight of the polymer (A1) becomes high, making it difficult to apply the curable composition. If the amount of the polymerization initiator is 10.0 wt % or more, the molecular weight of the polymer (A1) becomes low, making it difficult to obtain a cured product with appropriate strength.

[0061] Examples of organic solvents used in the polymerization reaction include aromatics such as toluene and xylene, ketones such as acetone, methyl ethyl ketone and methyl isobutyl ketone, and esters such as ethyl acetate, n-butyl acetate and propyl acetate, which may be used alone or in combination. Toluene is preferred because it has good solubility for the polymer (A1).

[0062] Next, step 3 will be described.

[0063] The polymer (A) of the present invention is obtained by purifying the polymer (A2) by removing impurities such as the solvent, unpolymerized monomer, monomer raw material, polymerization initiator, and decomposition products of the polymerization initiator from the polymer (A2) using a subcritical or supercritical fluid.

[0064] The purification method involves contacting the polymer before purification with a subcritical or supercritical fluid in a pressure vessel and controlling the pressure and temperature inside the pressure vessel so that the subcritical or supercritical fluid extracts impurities from the polymer. Specifically, the pressure and temperature inside the pressure vessel are controlled so that the polymer becomes insoluble in the subcritical or supercritical fluid and the subcritical or supercritical fluid dissolves the impurities. Next, the subcritical or supercritical fluid with the dissolved impurities is discharged from the pressure vessel, and the purified polymer remaining in the pressure vessel is recovered. The impurities are separated from the subcritical or supercritical fluid by reducing the pressure of the subcritical or supercritical fluid discharged from the pressure vessel.

[0065] The subcritical or supercritical fluid used in the present invention is not particularly limited, and examples thereof include carbon dioxide, nitrous oxide, sulfur hexafluoride, xenon, trifluoromethane, and monofluoromethane. Carbon dioxide is preferred because it does not remain in the polymer (A) after purification and is highly safe and easy to handle.

[0066] Furthermore, in order to adjust the polarity and improve the removal efficiency of the target substance, an extraction aid (hereinafter referred to as an entrainer) can be used together with the subcritical or supercritical fluid. Examples of entrainers include water, methanol, ethanol, 1-propanol, 2-propanol, 1-hexanol, 2-methoxyethanol, tetrahydrofuran, 1,4-dioxane, and acetonitrile. However, in consideration of ease of handling, methanol, ethanol, 1-propanol, 2-propanol, 2-methoxyethanol, and 1,4-dioxane are preferably used, and one or more of them can be mixed in any ratio and used.

[0067] When carbon dioxide is selected as the subcritical or supercritical fluid, the ratio of carbon dioxide to entrainer is not particularly limited, but is preferably 80 to 99.9% by weight of carbon dioxide and 0.1 to 20% by weight of entrainer, more preferably 78 to 99.8% by weight of carbon dioxide and 0.2 to 22% by weight of entrainer, and particularly preferably 75 to 99.8% by weight of carbon dioxide and 0.2 to 25% by weight of entrainer. If the carbon dioxide content is less than 75% by weight, not only impurities but also the polymer (A2) will be removed, resulting in a poor yield.

[0068] Subcritical or supercritical fluids are used at various temperatures and pressures depending on the properties of the fluid, but when carbon dioxide is used, subcritical fluids are used at temperatures of 16°C to 31°C and a pressure of at least 4.9 MPa, and supercritical fluids are used at temperatures of 31°C to 120°C and a pressure of at least 7.4 MPa, preferably 10 MPa or more, more preferably 20 MPa or more, and particularly preferably 25 MPa or more. The fluid to be contacted may be in either a subcritical state or a supercritical state, or treatment may be performed with a fluid in both states.

[0069] The polymer (A) of the present invention preferably has a weight average molecular weight (Mw) of 5,000 to 300,000, more preferably 30,000 to 250,000, and particularly preferably 50,000 to 200,000. In the present invention, the weight average molecular weight (Mw) is measured by the GPC (gel permeation chromatography) method described in the examples below.

[0070] [Curable Composition] The curable composition of the present invention contains a polymer (A) (hereinafter also referred to as "component (A)"), a hydrophilic monomer (B) (hereinafter also referred to as "component (B)"), and a radical polymerization initiator (C) (hereinafter also referred to as "component (C)").

[0071] In the curable composition of the present invention, component (A) can be used alone or in a mixture of two or more types in any ratio. The content of component (A) is preferably 30 to 99 wt %, more preferably 50 to 99 wt %, even more preferably 60 to 95 wt %, particularly preferably 70 to 90 wt %, and most preferably 75 to 90 wt % of the total amount of the curable composition of the present invention. If it is less than 30 wt %, a cured product with high oxygen permeability cannot be obtained. If it is more than 99 wt %, the viscosity of the curable composition becomes too high, resulting in poor workability.

[0072] The hydrophilic monomer (B) is not particularly limited, and examples thereof include 2-hydroxyethyl(meth)acrylate, 2-hydroxypropyl(meth)acrylate, 3-hydroxypropyl(meth)acrylate, 2-hydroxybutyl(meth)acrylate, 4-hydroxybutyl(meth)acrylate, glycerol(meth)acrylate, butoxyethylene glycol(meth)acrylate, caprolactone-modified 2-hydroxyethyl(meth)acrylate, acryloylmorpholine, hydroxyethyl(meth)acrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide, N-vinylpyrrolidone, acrylic acid, methacrylic acid, polyethylene glycol mono(meth)acrylate, N-vinyl-N-methylacetamide, N-vinyl-N-ethylacetamide, N-vinyl-N-ethylformamide, N-vinylformamide, and N-(4-hydroxyphenyl)maleimide, but are not limited thereto. N,N-dimethylacrylamide, N,N-diethylacrylamide, N-vinylpyrrolidone, and 2-hydroxyethyl methacrylate are preferred.

[0073] The hydrophilic monomer (B) may be any monomer that dissolves in water in any proportion, and may be the same as or different from the hydroxyl group-containing monomer of the first group and the amide group-containing monomer (c) having one ethylenically unsaturated group.

[0074] In the curable composition of the present invention, component (B) can be used alone or in a mixture of two or more types in any ratio. The content of component (B) is preferably 1 to 70 wt % of the total amount of the curable composition of the present invention, more preferably 1 to 50 wt %, even more preferably 5 to 40 wt %, particularly preferably 10 to 30 wt %, and most preferably 10 to 25 wt %. If it is less than 1 wt %, the viscosity of the curable composition becomes too high, resulting in poor workability. If it is more than 70 wt %, a cured product with high oxygen permeability cannot be obtained.

[0075] The radical polymerization initiator (C) used in the curable composition of the present invention includes a thermal radical polymerization initiator and a photoradical polymerization initiator.

[0076] The thermal radical polymerization initiator is not particularly limited, and examples thereof include various azo compounds or peroxides. Specific examples thereof include 2,2'-azobisisobutyronitrile, 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), dimethyl 2,2'-azobisbutyrate, 2,2'-azobis(2,4,4-trimethylpentane)diisobutylyl peroxide, di(3,5,5-trimethylhexanoyl)peroxide, and dilauroyl peroxide. Distearoyl peroxide, di-n-propyl peroxydicarbonate, diisopropyl peroxydicarbonate, di(4-tert-butylcyclohexyl)peroxydicarbonate, di(2-ethoxyethyl)peroxydicarbonate, di(2-ethylhexyl)peroxydicarbonate, di(3-methoxybutyl)peroxydicarbonate, cumyl peroxyneodecanoate, 1,1,3,3-tetramethylbutylperoxyneodecanoate, 1-cyclohexyl-1-methylethylperoxide Cineodecanoate, tert-hexylperoxyneodecanoate, tert-butylperoxyneodecanoate, tert-hexylperoxypivalate, tert-butylperoxypivalate, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, 2,5-dimethyl-2,5-di(2-hexanoyl)peroxyhexane, tert-hexylperoxy-2-ethylhexanoate, tert-butylperoxy-2-ethylhexanoate, tert-butylperoxy peroxyisobutyrate, tert-hexylperoxyisopropyl carbonate, tert-butylperoxymaleic acid, tert-butylperoxy-3,5,5-trimethylhexanoate, tert-butylperoxylaurate, 2,5-dimethyl-2,5-di(3-methylbenzoylperoxy)hexane, tert-butylperoxyisopropyl carbonate, tert-butylperoxy-2-ethylhexyl carbonate, tert-hexylperoxybenzoate, 2,5-dimethyl-2,Examples include 5-di(benzoylperoxy)hexane, tertiary butylperoxyacetic acid, and tertiary butylperoxybenzoate.

[0077] The photoradical polymerization initiator is not particularly limited, but examples thereof include various benzoin derivatives. Specific examples include 2,2-dimethoxy-1,2-diphenylethan-1-one, 1-hydroxy-cyclohexyl-phenyl-ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-[4-(2hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-[4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl]-2-methyl-propan-1-one, phenylglyoxylic acid methyl ester, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, 2-benzyl -2-dimethylamino-1-(4-morpholinylphenyl)-butanone-1,2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 1,2-octanedione 1-[4-(phenylthio)-2-(O-benzoyloxime)], ethanone 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-1-(O-acetyloxime), and the like.

[0078] In the curable composition of the present invention, component (C) can be used alone or in a mixture of two or more types in any ratio. The content of component (C) is preferably 0.01 to 1.0 wt %, more preferably 0.05 to 0.5 wt %, of the total amount of the curable composition of the present invention. If it is less than 0.01 wt %, the polymerization reaction will be insufficient and a cured product with appropriate strength will not be obtained. If it is more than 1.0 wt %, the polymerization rate will be too fast, resulting in a non-uniform reaction, and a cured product with appropriate strength will not be obtained.

[0079] To improve transparency, the curable composition of the present invention may contain an alkyl group-containing monomer (D) (hereinafter also referred to as "component (D)") having one ethylenically unsaturated group and 1 to 18 carbon atoms. Component (D) is not particularly limited, and the monomers exemplified as component (d) of polymer (A) can be used. The content of component (D) in the curable composition of the present invention is not particularly limited, but for example, the content of component (D) relative to the total amount of the curable composition of the present invention is 1.0 to 30.0 wt%, preferably 3.0 to 18.0 wt%. If the blending amount is less than 1.0 wt%, the transparency improvement effect is not achieved. Furthermore, if the blending amount exceeds 20.0 wt%, the crosslinked structure becomes dense, and the flexibility of the cured product tends to decrease.

[0080] A crosslinkable monomer may be used in the curable composition of the present invention for the purpose of reinforcing the strength of the cured product. The crosslinkable monomer is not particularly limited as long as it is a compound having two or more (meth)acrylic groups or vinyl groups in the molecule. Specific examples of the crosslinkable monomer include ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, triethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, and dipentaerythritol. Examples of crosslinkable monomers include, but are not limited to, (meth)acrylate crosslinkable monomers such as hexa(meth)acrylate; vinyl crosslinkable monomers such as allyl methacrylate, diallyl maleate, diallyl fumarate, diallyl succinate, diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, diethylene glycol bisallyl carbonate, triallyl phosphate, triallyl trimellitate, diallyl ether, N,N-diallyl melamine, and divinylbenzene; and α,ω-methacryloxypropyl polydimethylsiloxane. These crosslinkable monomers can be used alone or in combination of two or more.

[0081] The content of the crosslinking monomer in the curable composition of the present invention is not particularly limited, but for example, the content of the crosslinking monomer in the total amount of the curable composition of the present invention is 0.1 to 5.0 wt %, preferably 0.3 to 3.0 wt %. If the blending amount is less than 0.1 wt %, the reinforcing effect on the strength of the cured product is not obtained. On the other hand, if the blending amount is more than 5 wt %, the crosslinked structure becomes dense, and the flexibility of the cured product tends to decrease.

[0082] [Silicone Hydrogel Contact Lens] The silicone hydrogel contact lens of the present invention can be obtained by polymerizing the curable composition of the present invention. As a method for producing the silicone hydrogel contact lens of the present invention, known methods can be used, such as a method of polymerizing the curable composition of the present invention using a mold in the shape of a contact lens, or a method of polymerizing the curable composition of the present invention in a tubular container and then cutting and polishing the cured product into the shape of a lens.

[0083] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. Unless otherwise specified, "parts" and "%" in the text are by weight.

[0084] Example 1 (Step 1) 67.2 g of toluene was placed in a flask equipped with a stirrer, a dropping funnel, a condenser, and a thermometer, and the temperature was raised to 95°C under a nitrogen stream. A mixed solution of 0.61 g of 2-hydroxyethyl methacrylate, 51.1 g of silicone methacrylate (FM-0711 manufactured by JNC Corporation, molecular weight 1,000), 24.3 g of N,N-dimethylacrylamide, 12.2 g of n-butyl acrylate, 1.83 g of 2-(2'-hydroxy-5'-methacryloyloxyethylphenyl)-2H-benzotriazole (trade name: RUVA-93 manufactured by Otsuka Chemical Co., Ltd.), 7.2 g of toluene, and 0.9 g of azobisisobutyronitrile was placed in the dropping funnel and added dropwise at a constant rate over 2 hours, and the mixture was then aged at the same temperature for 3 hours. (Step 2) Next, 0.04 g of dibutyltin dilaurate as a reaction catalyst and 0.45 g of dibutylhydroxytoluene as a polymerization inhibitor were added, followed by addition of 0.69 g of 2-isocyanatoethyl methacrylate, and the mixture was reacted for 10 hours at 95° C. The isocyanate content after the reaction was determined by adding an excess of amine and back titrating with hydrochloric acid. It was confirmed that the value was less than 0.05% of the residual isocyanate amount calculated from the calculated value, and a pre-purification polymer (P-1) was obtained.

[0085] Example 2 (Step 3: Purification with Supercritical Carbon Dioxide) 20.0 g of the unpurified polymer (P-1) obtained in Example 1 was placed in a pressure vessel with an internal volume of approximately 140 mL and sealed. Carbon dioxide was passed through the vessel at 70°C and a pressure of 25 MPa for 3 hours to dissolve the impurities in the carbon dioxide supercritical fluid, and the supercritical fluid containing the dissolved impurities was then discharged from the pressure vessel. The vessel was returned to normal pressure, and the polymer (P-2) remaining in the vessel was obtained as polymer (A) of the present invention. The molecular weight of the obtained polymer (P-2) was measured, and the weight average molecular weight was found to be 25,000.

[0086] Comparative Example 1: Purification under reduced pressure 20.0 g of the unpurified polymer (P-1) obtained in Example 1 was treated using a rotary evaporator at a reduced pressure of -0.01 kPa and 75°C for 3 hours to volatilize and remove impurities. The pressure inside the vessel was returned to normal pressure, and polymer (P-3) was obtained. The molecular weight of the obtained polymer (P-3) was measured, and the weight average molecular weight was found to be 24,000.

[0087] [Example 3] A flask equipped with a stirrer, dropping funnel, condenser, and thermometer was charged with 111.9 g of toluene, and the temperature was raised to 90 ° C. under a nitrogen stream. A mixed solution of 1.40 g of 4-hydroxybutyl acrylate, 84.0 g of silicone methacrylate (FM-0711 manufactured by JNC Corporation, molecular weight 1,000), 14.0 g of N,N-dimethylacrylamide, 25.2 g of n-butyl acrylate, 14 g of toluene, and 1.24 g of azobisisobutyronitrile was charged into the dropping funnel and added dropwise at a constant rate over 2 hours, and then aged at the same temperature for 3 hours. Next, 0.13 g of triphenylphosphine as a reaction catalyst and 0.13 g of dibutylhydroxytoluene as a polymerization inhibitor were added, and the mixture was heated to 95 ° C., and 1.50 g of methacrylic anhydride was added, and the mixture was reacted at 95 ° C. for 5 hours to obtain a polymer (P-4) before purification.

[0088] [Example 4]: Purification with supercritical carbon dioxide 20.0 g of the unpurified polymer (P-4) obtained in Example 3 was placed in a pressure vessel with an internal volume of approximately 140 mL, which was then sealed and treated with carbon dioxide at 40°C and a pressure of 25 MPa for 3 hours. The pressure inside the vessel was returned to normal pressure, and a reactive polymer (P-5) of the present invention was obtained. The molecular weight of the obtained polymer was measured, and the weight average molecular weight was found to be 64,000.

[0089] Comparative Example 2: Purification under reduced pressure 20.0 g of the unpurified polymer (P-4) obtained in Example 3 was treated using a rotary evaporator at a reduced pressure of -0.01 kPa and 75°C for 3 hours. The pressure inside the vessel was returned to normal pressure, and polymer (P-6) was obtained. The molecular weight of the obtained polymer was measured, and the weight average molecular weight was 54,000.

[0090] The GPC chart of polymer (P-5) is shown in FIG. 1, the GPC chart of polymer (P-6) is shown in FIG. 2, and the GPC chart of FM-0711 is shown in FIG.

[0091] Example 5 (Step 1) A flask equipped with a stirrer, a dropping funnel, a condenser, and a thermometer was charged with 63.8 g of toluene, and the temperature was raised to 95°C under a nitrogen stream. A mixed solution of 1.36 g of 2-isocyanatoethyl methacrylate, 48.0 g of silicone methacrylate (FM-0711 manufactured by JNC Corporation, molecular weight 1,000), 22.9 g of N,N-dimethylacrylamide, 11.4 g of n-butyl acrylate, 1.71 g of 2-(2'-hydroxy-5'-methacryloyloxyethylphenyl)-2H-benzotriazole (trade name: RUVA-93 manufactured by Otsuka Chemical Co., Ltd.), 6.8 g of toluene, and 0.9 g of azobisisobutyronitrile was charged into the dropping funnel and added dropwise at a constant rate over 2 hours, and the mixture was then aged at the same temperature for 3 hours. (Step 2) Next, 0.04 g of dibutyltin dilaurate as a reaction catalyst and 0.45 g of dibutylhydroxytoluene as a polymerization inhibitor were added, followed by 1.20 g of 2-hydroxyethyl methacrylate, and the mixture was reacted for 10 hours at 95° C. The isocyanate content after the reaction was determined by adding an excess of amine and back titrating with hydrochloric acid. It was confirmed that the value was less than 0.05% of the residual isocyanate amount calculated from the calculated value, and a pre-purification polymer (P-7) was obtained.

[0092] Example 6 (Step 3: Purification with Supercritical Carbon Dioxide) 20.0 g of the unpurified polymer (P-7) obtained in Example 1 was placed in a pressure vessel with an internal volume of approximately 140 mL and sealed, and carbon dioxide was passed through the vessel at 70°C and a pressure of 25 MPa for 3 hours to dissolve the impurities in the carbon dioxide supercritical fluid, while the supercritical fluid in which the impurities had been dissolved was discharged from the pressure vessel. The vessel was returned to normal pressure, and the polymer (P-8) remaining in the vessel was obtained as polymer (A) of the present invention. The molecular weight of the obtained polymer (P-8) was measured, and the weight average molecular weight was found to be 29,000.

[0093] Comparative Example 3: Purification under reduced pressure 20.0 g of the unpurified polymer (P-7) obtained in Example 5 was treated using a rotary evaporator at a reduced pressure of -0.01 kPa and 75°C for 3 hours to volatilize and remove impurities. The pressure inside the vessel was returned to normal pressure, and polymer (P-9) was obtained. The molecular weight of the obtained polymer (P-9) was measured, and the weight average molecular weight was found to be 28,000.

[0094] [Example 7] (Step 1) 61.3 g of toluene was charged into a flask equipped with a stirrer, a dropping funnel, a condenser, and a thermometer, and the temperature was raised to 95°C under a nitrogen stream. A mixed solution of 2.22 g of 2-hydroxyethyl methacrylate, 46.6 g of silicone methacrylate (FM-0711 manufactured by JNC Corporation, molecular weight 1,000), 22.2 g of N,N-dimethylacrylamide, 11.1 g of n-butyl acrylate, 6.5 g of toluene, and 0.82 g of azobisisobutyronitrile was charged into the dropping funnel and added dropwise at a constant rate over 2 hours, followed by aging at the same temperature for 3 hours. (Step 2) Next, 1.74 g of triethylamine and 0.42 g of dibutylhydroxytoluene as a polymerization inhibitor were added, and the temperature was lowered to 60°C. 1.78 g of methacrylic acid chloride was added dropwise with stirring, and the mixture was allowed to react for 2 hours. The reaction solution was pressure filtered through a filter paper with a particle size of 1 micron to remove triethylamine hydrochloride, thereby obtaining a polymer (P-10) before purification.

[0095] Example 8 (Step 3: Purification with Supercritical Carbon Dioxide) 20.0 g of the unpurified polymer (P-10) obtained in Example 7 was placed in a pressure vessel with an internal volume of approximately 140 mL and sealed. A mixed fluid of 98 wt % carbon dioxide and 2 wt % 2-propanol was passed through the vessel at 70°C and a pressure of 25 MPa for 3 hours to dissolve impurities in the supercritical fluid of carbon dioxide and 2-propanol, and the supercritical fluid in which the impurities had been dissolved was then discharged from the pressure vessel. Next, carbon dioxide was passed through the vessel at 70°C and a pressure of 25 MPa for 2 hours, and the 2-propanol was discharged from the pressure vessel. The vessel was returned to normal pressure, and the polymer (P-11) remaining in the vessel was obtained as polymer (A) of the present invention. The molecular weight of the obtained polymer (P-11) was measured, and the weight average molecular weight was found to be 37,000.

[0096] Comparative Example 4: Purification under reduced pressure 20.0 g of the unpurified polymer (P-10) obtained in Example 1 was treated using a rotary evaporator at a reduced pressure of -0.01 kPa and 75°C for 3 hours to volatilize and remove impurities. The pressure inside the vessel was returned to normal pressure, and polymer (P-12) was obtained. The molecular weight of the obtained polymer (P-12) was measured, and the weight average molecular weight was 36,000.

[0097] In each of the examples and comparative examples, the physical properties were measured as follows.

[0098] (Weight-average molecular weight) The weight-average molecular weight (Mw) was measured by gel permeation chromatography (GPC) under the following conditions: Analytical device: GPC HLC-8320GPC manufactured by Tosoh Corporation Column: SuperMultiporeHZ-H (two columns) manufactured by Tosoh Corporation Column temperature: 40°C Flow rate: 0.35 ml / min Eluent: tetrahydrofuran Detector: differential refractometer Standard sample: polystyrene

[0099] (Quantitative Analysis of Silicone Methacrylate Monomer FM-0711) The amount of silicone methacrylate monomer FM-0711 contained in the polymer was quantified by LC-MS (liquid chromatography mass spectrometry). Analytical device: UltiMate 3000 manufactured by Thermo Fisher Science Column: CORTECS C18 Column temperature: 40°C Mobile phase A: acetonitrile / THF (50 / 50) Mobile phase B: 5 mM aqueous ammonium acetate solution Detector: photodiode array (PDA) detector 190-800 nm, electrospray ionization (ESI) ± (Mass Range 150-2250)

[0100] (Quantitative Analysis of Toluene, Monomer, and Initiator) The toluene, monomer, and initiator remaining in the polymers (P-2), (P-3), (P-5), and (P-6) were quantified by GC-MS (gas chromatography mass spectrometry) using tridecane as an internal standard. Analytical apparatus: GC-2010 manufactured by Shimadzu Corporation. Column: HP-5MS 30 m - 0.25 mm - 0.25 μm. Carrier gas: He 1.2 mL / min. Oven: 50°C (2 min) - 10°C / min - 300°C (33 min). Inlet: split (30:1), 250°C. Detector: Flame Ionization Detector (FID).

[0101] The amounts of impurities contained in the polymers (P-2) and (P-3) were measured, and the results are shown in Table 1.

[0102]

[0103] The abbreviations for the compounds in Table 1 are as follows: FM-0711: Silicone methacrylate (manufactured by JNC Corporation) 2-HEMA: 2-hydroxyethyl methacrylate nBA: n-butyl acrylate DMA: N,N-dimethylacrylamide RUVA-93: 2-(2'-hydroxy-5'-methacryloyloxyethylphenyl)-2H-benztriazole MOI: 2-isocyanatoethyl methacrylate AIBN: Azobisisobutyronitrile

[0104] The amounts of impurities contained in the polymers (P-5) and (P-6) were measured, and the results are shown in Table 2.

[0105]

[0106] The impurities in FM-0711 are thought to be by-products produced during the production of FM-0711, but have not been accurately identified. In Table 2, MAA (methacrylic acid) is a component eliminated after the reaction of the polymer with methacrylic anhydride.

[0107] The abbreviations for the compounds in Table 2 are as follows: FM-0711: Silicone methacrylate (manufactured by JNC Corporation) 4-HBA: 4-hydroxybutyl acrylate nBA: n-butyl acrylate DMA: N,N-dimethylacrylamide MAAH: Methacrylic anhydride MAA: Methacrylic acid AIBN: Azobisisobutyronitrile

[0108] The toluene, monomer, and initiator remaining in the polymers (P-8) and (P-9) were quantified by GC (gas chromatography) using tridecane as an internal standard. Analytical equipment: Agilent Agilent 7890 Column: HP-5MS 30 m - 0.25 mm - 0.25 μm Carrier gas: He 1.2 mL / min Oven: 80°C (2 min) - 10°C / min - 300°C (21 min) Injection port: split (30:1), 300°C Detector: Hydrogen flame ionization detector (FID)

[0109] The amounts of impurities contained in the polymers (P-8) and (P-9) were measured, and the results are shown in Table 3.

[0110] The abbreviations for the compounds in Table 3 are as follows: FM-0711: Silicone methacrylate (manufactured by JNC Corporation) 2-HEMA: 2-hydroxyethyl methacrylate nBA: n-butyl acrylate DMA: N,N-dimethylacrylamide RUVA-93: 2-(2'-hydroxy-5'-methacryloyloxyethylphenyl)-2H-benztriazole MOI: 2-isocyanatoethyl methacrylate AIBN: Azobisisobutyronitrile

[0111] The toluene and 2-propanol monomer remaining in the polymers (P-11) and (P-12) were quantified by GC (gas chromatography) using tridecane as an internal standard. Analytical equipment: Agilent Agilent 7890 Column: HP-5MS 30 m - 0.25 mm - 0.25 μm Carrier gas: He 1.2 mL / min Oven: 40°C (5 min) - 10°C / min - 220°C (18 min) Injection port: split (30:1), 200°C Detector: Flame ionization detector (FID)

[0112] The amount of initiator remaining in the polymers (P-11) and (P-12) was quantified by GC (gas chromatography) using tridecane as an internal standard. Analytical equipment: Agilent Agilent 7890 Column: HP-5MS 30 m - 0.25 mm - 0.25 μm Carrier gas: He 1.2 mL / min Oven: 80°C (2 min) - 10°C / min - 300°C (21 min) Injection port: split (30:1), 300°C Detector: Flame ionization detector (FID)

[0113] The triethylamine remaining in the polymers (P-11) and (P-12) was quantified by GC (gas chromatography) using tridecane as an internal standard. Analytical apparatus: Agilent 8890 Column: InterCap for Amines 30 m - 0.32 mm Carrier gas: He 1.2 mL / min Oven: 50°C (3 min) -10°C / min -220°C (10 min) Injection port: split (30:1), 260°C Detector: Flame ionization detector (FID)

[0114] The amounts of impurities contained in the resulting polymers (P-11) and (P-12) were measured, and the results are shown in Table 4.

[0115]

[0116] The abbreviations for the compounds in Table 4 are as follows: FM-0711: Silicone methacrylate (manufactured by JNC Corporation) nBA: n-butyl acrylate DMA: N,N-dimethylacrylamide 2-HEMA: 2-hydroxyethyl methacrylate AIBN: Azobisisobutyronitrile

[0117] In Table 4, methacrylic acid is the reaction product of methacrylic acid chloride and water, and 2-propanol is the entrainer used in the purification with supercritical carbon dioxide.

[0118] [Preparation of Curable Composition] [Example 9] 7.2 g of polymer (P-2) as polymer (A); 0.9 g of N-vinylpyrrolidone, 0.6 g of N,N-diethylacrylamide, 0.4 g of methacrylic acid, and 0.3 g of 4-hydroxybutyl acrylate as hydrophilic monomers (B); 0.6 g of lauryl acrylate as alkyl group-containing monomer (D) having from 1 to 18 carbon atoms; and 0.05 g of 1,1'-azobis(cyclohexane-1-carbonitrile) as radical polymerization initiator (C) were prepared in a glass bottle and mixed using a planetary centrifugal mixer, thereby obtaining the curable composition of Example 9.

[0119] Example 10 8.0 g of polymer (P-5) as the polymer (A), 2.0 g of N,N-diethylacrylamide and 0.01 g of ethylene glycol dimethacrylate as the hydrophilic monomer (B), and 0.05 g of azobisisobutyronitrile as the radical polymerization initiator (C) were prepared in a glass bottle and mixed using a planetary centrifugal mixer, thereby obtaining a curable composition of Example 10.

[0120] Example 11 In a glass bottle were prepared 7.2 g of polymer (P-8) as polymer (A); 0.9 g of N-vinylpyrrolidone, 0.6 g of N,N-diethylacrylamide, 0.4 g of methacrylic acid, and 0.3 g of 4-hydroxybutyl acrylate as hydrophilic monomers (B); 0.6 g of lauryl acrylate as alkyl group-containing monomer (D) having from 1 to 18 carbon atoms; and 0.05 g of 1,1′-azobis(cyclohexane-1-carbonitrile) as radical polymerization initiator (C), and the mixture was mixed using a planetary centrifugal mixer to obtain a curable composition of Example 11.

[0121] [Preparation of Silicone Hydrogel Contact Lenses] The curable compositions obtained in Examples 9 to 11 were placed in the female mold of a polypropylene contact lens, and the corresponding male and female molds were mated. The mated contact lens mold was polymerized and cured in a nitrogen atmosphere at 105°C for 2 hours.

[0122] After polymerization was complete, the male and female molds were separated, and the female (male) mold with the cured product attached was immersed in a pure water / ethanol mixture (volume ratio 90 / 10) at 60°C for 1 hour to release the cured product from the female (male) mold. The resulting cured product was then immersed in physiological saline for 1 hour, followed by high-pressure steam sterilization at 121°C for 30 minutes to obtain a silicone hydrogel contact lens.

[0123] When the resulting silicone hydrogel contact lenses were observed from directly above, they all had a perfect circular shape. When their light transmittance was measured using a spectrophotometer, they all had a transparency of 90% or more.

[0124] Example 12 7.2 g of polymer (P-11) as the polymer (A); 2.3 g of N,N-diethylacrylamide as the hydrophilic monomer (B); 0.6 g of n-butyl acrylate as the alkyl group-containing monomer (D) having from 1 to 18 carbon atoms; and 0.05 g of azobisisobutyronitrile as the radical polymerization initiator (C) were prepared in a glass bottle and mixed using a planetary centrifugal mixer, thereby obtaining a curable composition of Example 12.

[0125] Example 13 Preparation of Silicone Hydrogel Contact Lens The curable composition obtained in Example 12 was poured into a female mold for a polypropylene contact lens, and the corresponding male and female molds were mated. The mated contact lens mold was polymerized and cured in a nitrogen atmosphere at 105°C for 2 hours.

[0126] After polymerization was complete, the male and female molds were separated, and the female (male) mold with the cured product attached was immersed in a pure water / ethanol mixture (volume ratio 95 / 5) at 60°C for 1 hour. The cured product was then released from the female (male) mold, and then transferred to physiological saline and immersed therein for 1 hour to obtain a swollen body. The resulting swollen body was sterilized by high-pressure steam at 121°C for 30 minutes to obtain the silicone hydrogel contact lens of Example 13.

[0127] When observed from directly above, the resulting silicone hydrogel contact lens of Example 13 was found to have a perfect circle. Furthermore, when light transmittance was measured using a spectrophotometer, it was found to have a transparency of 90% or more.

[0128] Example 14 Preparation of Silicone Hydrogel Contact Lens The curable composition obtained by the same method as in Example 12 was polymerized and cured by the same method as in Example 13, and then the male and female molds were separated. The female (male) mold with the cured product attached was immersed in a pure water / IPA (isopropanol) mixture (volume ratio: 50 / 50) at 60°C for 1 hour. The cured product was then released from the female (male) mold, and then transferred to physiological saline and immersed for 1 hour to obtain a swollen body. The obtained swollen body was further sterilized by high-pressure steam at 121°C for 30 minutes to obtain the silicone hydrogel contact lens of Example 14.

[0129] When observed from directly above, the resulting silicone hydrogel contact lens of Example 14 was found to have a perfect circular shape. Furthermore, when light transmittance was measured using a spectrophotometer, it was found to have a transparency of 90% or more.

[0130] Comparative Example 5 Preparation of Curable Composition Preparation Using Monomers The following substances were prepared in a glass bottle and mixed using a planetary centrifugal mixer: 4.2 g of silicone methacrylate (FM-0711 manufactured by JNC Corporation, molecular weight 1,000) as component (b); 2.3 g of N,N-diethylacrylamide and 2.0 g of N,N-dimethylacrylamide as hydrophilic monomers (B); 1.5 g of n-butyl acrylate as alkyl group-containing monomer (D) having from 1 to 18 carbon atoms; 0.2 g of ethylene glycol di(meth)acrylate as a crosslinking monomer; and 0.05 g of azobisisobutyronitrile as radical polymerization initiator (C). The curable composition of Comparative Example 5 was obtained by mixing the mixture in a planetary centrifugal mixer.

[0131] Comparative Example 6 Preparation of a Silicone Hydrogel Contact Lens The resulting curable composition was poured into a female mold for a polypropylene contact lens, and the corresponding male and female molds were mated together. The mated contact lens mold was polymerized and cured at 105°C for 2 hours in a nitrogen atmosphere.

[0132] After polymerization was complete, the male and female molds were separated, and the female (male) mold with the cured product attached was immersed in a pure water / ethanol mixture (volume ratio 95 / 5) at 60°C for 1 hour. The cured product was then released from the female (male) mold, and then transferred to physiological saline and immersed therein for 1 hour to obtain a swollen body. The obtained swollen body was sterilized by high-pressure steam at 121°C for 30 minutes to obtain the silicone hydrogel contact lens of Comparative Example 6.

[0133] The light transmittance of the obtained silicone hydrogel contact lens of Comparative Example 6 was measured using a spectrophotometer. Although the lens had a transparency of 90% or more, when observed from directly above, it was found that the lens did not have a perfect circular shape and was distorted.

[0134] Comparative Example 7 Preparation of Silicone Hydrogel Contact Lens The curable composition obtained by the same method as in Comparative Example 2 was polymerized and cured by the same method as in Comparative Example 7, and then the male and female molds were separated. The female (male) mold with the cured product attached was immersed in a pure water / IPA mixture (volume ratio 50 / 50) at 60°C for 1 hour. The cured product was then released from the female (male) mold, and then transferred to physiological saline and immersed for 1 hour to obtain a swollen body. The obtained swollen body was further sterilized by high-pressure steam at 121°C for 30 minutes to obtain the silicone hydrogel contact lens of Comparative Example 7.

[0135] The light transmittance of the obtained silicone hydrogel contact lens of Comparative Example 7 was measured using a spectrophotometer. Although the lens had a transparency of 90% or more, when observed from directly above, it was found that the lens did not have a perfect circular shape and was distorted.

[0136] Twenty-five silicone hydrogel contact lenses each obtained in Examples 13 and 14 and Comparative Examples 6 and 7 were immersed in 5 mL of acetone and shaken at room temperature for 72 hours to prepare an acetone extract.

[0137] The silicone monomer FM-0711 in the resulting acetone extract was quantified using LC-MS (liquid chromatography mass spectrometry). The standard solution concentrations were calculated as sample concentrations, and calibration curves corresponding to 0.1, 0.5, 1.5, and 10 ppm were prepared. The results are shown in Table 5.

[0138] The silicone monomer FM-0711 in the resulting acetone extract was quantified by LC-MS (liquid chromatography mass spectrometry). The standard solution concentrations were calculated as sample concentrations, and calibration curves equivalent to 0.1, 0.5, 1.5, and 10 ppm were prepared. The results are shown in Table 5. Analytical equipment: Thermo Fisher Science Q-Exactive Column: CORTECS C18 Column temperature: 40°C Mobile phase A: acetonitrile / THF (50 / 50) Mobile phase B: 5 mM ammonium acetate aqueous solution Gradient: A / B = 50 / 50 - (5) - 95 / 5 (10) Detector: photodiode array (PDA) detector 190-800 nm, electrospray ionization (ESI) ± (mass range 200-2500)

[0139]

[0140] This application claims priority based on Japanese Patent Application No. 2022-206597 filed on December 23, 2022, Japanese Patent Application No. 2023-146954 filed on September 11, 2023, and Japanese Patent Application No. 2023-181047 filed on October 20, 2023.

[0141] The polymer of the present invention has high purity, and after a curable composition using the polymer is cured, no silicon-containing monomer remains. This eliminates the need for washing using a large amount of organic solvent, making it possible to provide inexpensive contact lenses.

Claims

1. A method for producing polymer (A), comprising: (Step 1) polymerizing a first monomer (a) having an ethylenically unsaturated group to obtain polymer (A1); (Step 2) reacting polymer (A1) with a second monomer having an ethylenically unsaturated group to obtain polymer (A2); and (Step 3) purifying polymer (A2) using a subcritical or supercritical fluid to obtain polymer (A), wherein the first monomer is selected from either a first group consisting of hydroxyl group-containing monomers or a second group consisting of isocyanate compounds of (meth)acrylic acid, (meth)acrylic anhydride, and (meth)acrylic acid halide; and the second monomer is selected from the other of the first group or the second group.

2. The method for producing polymer (A) according to claim 1, wherein in step 1, a silicon-containing monomer (b) having one ethylenically unsaturated group is polymerized together with the first monomer (a).

3. The method for producing polymer (A) according to claim 2, wherein in the step 1, an amide group-containing monomer (c) is further polymerized.

4. A method for producing polymer (A) according to claim 3, wherein in (Step 1), the first monomer (a), the silicon-containing monomer (b), and the amide group-containing monomer (c) are polymerized with an alkyl group-containing monomer (d) having one ethylenically unsaturated group and having 1 to 18 carbon atoms.

5. A method for producing polymer (A) according to any one of claims 1 to 4, wherein the first monomer is a hydroxyl group-containing monomer.

6. The method for producing polymer (A) according to claim 5, wherein the second monomer is an isocyanate compound of (meth)acrylic acid.

7. The method for producing polymer (A) according to claim 5, wherein the second monomer is an anhydride of (meth)acrylic acid.

8. The method for producing polymer (A) according to claim 5, wherein the second monomer is a halide of (meth)acrylic acid.

9. A method for producing polymer (A) according to any one of claims 1 to 4, wherein the first monomer is an isocyanate compound of (meth)acrylic acid, and the second monomer is a hydroxyl group-containing monomer.

10. The method for producing polymer (A) according to any one of claims 1 to 9, wherein carbon dioxide alone is used as the subcritical or supercritical fluid.

11. The method for producing polymer (A) according to any one of claims 1 to 9, wherein a mixture of carbon dioxide and an entrainer is used as the subcritical or supercritical fluid.

12. The method for producing polymer (A) according to claim 11, wherein the mixture of carbon dioxide and entrainer comprises 80.0 to 99.9% by weight of carbon dioxide and 0.1 to 20.0% by weight of entrainer.

13. The method for producing polymer (A) according to claim 11 or 12, wherein the entrainer is at least one selected from the group consisting of methanol, ethanol, 1-propanol, 2-propanol, 2-methoxyethanol, and 1,4-dioxane.

14. A method for producing polymer (A) according to any one of claims 1 to 13, wherein the polymer (A) has a weight average molecular weight of 5,000 to 300,000.

15. A method for producing a curable composition comprising the polymer (A) according to any one of claims 1 to 14, a hydrophilic monomer (B), and a radical polymerization initiator (C).

16. A method for producing a cured product obtained from the curable composition according to claim 15.

17. A method for producing the curable composition according to claim 15 for use in contact lenses.

18. A method for producing a silicone hydrogel contact lens using the curable composition for contact lenses according to claim 17.