Process for production of iron ore agglomerate for use in direct reduction reactors and the agglomerated product
Patent Information
- Application Number
- MYPI2025003931
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-12-06
- Filing Date
- 2023-12-26
- Publication Date
- 2024-07-06
AI Technical Summary
Current agglomeration technologies for iron ore in direct reduction reactors fail to produce agglomerates with specific metallurgical characteristics necessary for optimized performance, as they lack control over porosity, packaging degree, and high iron content, leading to high disintegration and low metallization, and are not sustainable in terms of CO2 emissions.
A process involving the dispersion of nanomaterials in binders with iron ore fines and additives, followed by agglomeration via briquetting or extrusion, curing, and surface coating to control porosity and packaging, resulting in high iron content, low disintegration, and high metallization, while reducing CO2 emissions through low-temperature curing.
The process produces agglomerates with high physical resistance, low fine generation, and high metallization, optimizing performance in direct reduction reactors and reducing CO2 emissions by controlling porosity and packaging, and achieving efficient metallurgical properties.
Smart Images

Figure PI2025003931_DRAWING_001 
Figure PI2025003931_DRAWING_002 
Figure PI2025003931_DRAWING_003
Abstract
Description
IRON ORE AGGLOMERATE PRODUCTION PROCESS FOR USE IN DIRECT REDUCTION REACTORS AND THE AGGLOMERATED PRODUCT FIELD OF INVENTION
[0001] The present invention is part of the field of mining-metallurgical technologies and refers to a process for producing iron ore agglomerate, for use in direct reduction (DR) reactors, replacing pellets and granulates traditionally used. BACKGROUND OF THE INVENTION
[0002] Direct reduction reactors are characterized by the ability to reduce iron ore to metallic iron without melting the reactor feed. The metallic product, obtained in the solid phase, is called sponge iron (or DRI - Direct Reduced Iron), which can be briquetted hot, producing HBI - Hot Briquetted Iron.
[0003] The direct reduction process is an alternative to using a blast furnace to produce an intermediate product with the same basic functions as the pig iron produced by the blast furnace. Both intermediate products (pig iron and sponge iron) are intended for use in steelmaking, with sponge iron used in electric furnaces. The best-known direct reduction processes are Midrex, HyL (Hayata y Lamina), Armco, H. Iron, SL-RN, and Purofer.
[0004] To ensure optimized performance of direct reduction reactors, as well as a quality final product (sponge iron), the iron ore agglomerate to be fed must have specific physical, chemical, and metallurgical characteristics.
[0005] The state of the art presents some ore agglomeration technologies for use in reduction furnaces. However, none of these technologies allows the production of agglomerates with specific metallurgical characteristics for a optimized performance in a direct reduction reactor, as obtained by the present invention.
[0006] Patent BR102019023195-5, registered in the name of Vale SA, describes an agglomerate of iron ore fines for replacing metal charges in blast furnaces, unlike the present invention, which produces agglomerates with specific characteristics for feeding direct reduction reactors, such as Midrex and HyL. Furthermore, patent BR102019023195-5 uses fluxes and other inputs different from those of the present invention. Furthermore, the aforementioned patent does not include coating application steps, as required by the present invention.
[0007] Patent BR112014005488-6, also in the name of Vale SA, describes a process for obtaining agglomerates that differs from the present invention in several aspects, including (i) raw materials used; (ii) it does not have a coating step; (iii) it applies to agglomerates obtained by pelletizing technology, for example mini pellets, and (iv) the product subject to the patent does not have physical and chemical requirements for application in the direct reduction process.
[0008] Patent application BR102022006033-9, also registered with Vale SA, describes a process for producing agglomerates that differs from the present invention in terms of (i) the raw materials used, (ii) the use of microwaves for reduction, (iii) the use of biomass as a reductant, among other differences. Document BR102022006033-9 describes a process for producing reduced material using microwave technology and biomass. The pre-reduced agglomerate (metallic Fe >60%) obtained is merely an intermediate step for future application in different reactors.
[0009] The master's dissertation entitled "Development of self-reducing briquettes with coating agent", published in 2019 by Kleiton Gonçalves Lovati, describes a process for obtaining self-reducing briquettes using coating agents such as dolomitic limestone, bentonite, serpentinite, and steel slag. The present invention differs from this document because it deals with a different product and cannot be considered a self-reducing briquette. Self-reducing briquettes are composed of iron ore and a significant amount of carbonaceous material, enabling the self-reduction characteristic. They are specifically used in Reduction and Fusion technologies (e.g., Corex, Finex, Hismelt, Tecnored, Oxicup), unlike the present invention, which focuses on Direct Reduction technologies (e.g., Midrex, HyL, Fastmet, Jindal, etc.).
[0010] The master's dissertation entitled "Development of a methodology for evaluating the reoxidation tendency of iron ore pellets reduced in a direct gas reduction process," published in 2010 by Renata Gonçalves Penna, describes the effect of iron ore pellet degradation in a direct reduction process. This document differs from the present invention due to the different agglomerate. That is, the document describes pellets produced by a hot agglomeration process (>1300°C), while the present invention addresses cold agglomerate, produced at temperatures of around 250°C.
[0011] In direct reduction agglomerates, the iron content (>60%) and the deleterious content (NazO, SiCh, and Al2O3) must be lower (<10%) when compared to the blast furnace process. Furthermore, it is essential that direct reduction agglomerates have low disintegration and a high metallization content (>90%) when compared to the blast furnace product.
[0012] The present invention relates to a process for the production of cold iron ore agglomerate, for use in direct reduction (DR) reactors, which presents the following advantages in comparison to the processes known in the prior art: 1. Control of agglomerate porosity via incorporation of organic additives and curing at slightly higher temperatures (burning of the added organic materials); 2. Control of the degree of packaging by reducing compaction pressure and apparent density of the agglomerate; 3. Use of necessarily richer feeds (feeding ore with a higher iron content); 4. Individual use or a combination of binders; 5. Obtaining final agglomerate with standardized size, which influences the properties of the final product; 6. Obtaining final agglomerate with high physical resistance to handling and transportation over long distances, including resistance to weathering; 7. Obtaining a final agglomerate that allows low generation of fines in the reduction reactors and a high degree of metallization; 8. Reduction in CO2 emissions, as curing is carried out at room temperature or low temperature.
[0013] Porosity for this type of agglomerate is crucial for its subsequent application in direct reduction reactors. To this end, porosity control and the degree of packing are the distinguishing and essential elements capable of promoting the product's necessary properties for use in direct reduction reactors.
[0014] Porosity control, for example, allows gases to enter and exit the agglomerate's internal structure during the direct reduction process without compromising its physical quality, i.e., causing it to disintegrate. If this doesn't occur, the product's strength is severely impacted, and it fails to meet the minimum performance requirements.
[0015] Particleboard packaging can be controlled in a number of ways, such as adjusting process conditions, improving the particleboard finish, and using additives (chemical or mineral) to ensure ideal porosity.
[0016] Thus, the present invention has a major difference in relation to the documents known in the state of the art, since the importance of porosity for this direct reduction product was confirmed in bench-scale tests, as well as in basket tests in direct reduction process customers.
[0017] Regarding inputs, it is important to note that the possibility of using a combination of different binders aims, among others, to reduce the presence of deleterious substances (NazO, SiOz and AI2O3) in the agglomerated product. OBJECTIVES OF THE INVENTION
[0018] The present invention has the general objective of providing a new process for producing iron ore agglomerate with high metallurgical performance to replace granules and pellets in direct reduction reactors. The main characteristics of the agglomerate obtained are high physical strength, low generation of fines, and a high degree of metallization during operation in direct reduction reactors.
[0019] Another objective of the present invention is to provide a more sustainable process, which allows the reduction of CO2 emissions in the mining-metallurgical production chain. SUMMARY OF THE INVENTION
[0020] The present invention, in its preferred embodiment, discloses a process for producing iron ore agglomerate to replace granulate and pellets in direct reduction furnaces comprising the following steps: a) dispersing 0.05-2% by weight of nanomaterial in agglomerate in order to obtain a mixture called "agglomerate mixture"; b) mixing 1-10% of the agglomerate mixture from step a) with 70-99% of iron ore fines and / or steel co-products, 0-5% of chemical and / or mineral additives with properties to promote plasticity and / or improve the porosity of the agglomerate; c) adjust the humidity in such a way as to obtain the quantity of 0-25% by weight of water in the mixture; d) carry out the agglomeration process via briquetting or extrusion; e) cure the agglomerate; f) apply a coating to the surface of the agglomerate in order to reduce the sticking effect in the RD reactors; BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The present invention is described in detail based on the respective figures:
[0022] Figure 1 illustrates a simplified block diagram of the process for producing pellets for use in direct reduction reactors in accordance with the present invention.
[0023] Figure 2 presents a comparison showing the evolution of the disintegration results of the obtained clusters.
[0024] Figure 3 shows an image of the agglomerates obtained from the process of the present invention after application of the coating used to mitigate the effect of gluing.
[0025] Figure 4 shows an image of the agglomerates (DRI) obtained after performing a basket test in a direct reduction furnace on an industrial scale.
[0026] Figure 5 presents a graph containing agglomerate metallization and carburization (DRI) data obtained with the various briquette samples subjected to basket tests in Midrex and HyL reactors.
[0027] Figure 6 presents a graph containing disintegration under agglomerate reduction (DRI) data obtained with the various briquette samples subjected to basket tests in Midrex and HyL reactors. DETAILED DESCRIPTION OF THE INVENTION
[0028] Although the present invention may be susceptible to different embodiments, preferred embodiments are shown in the figures and in the following detailed discussion with the understanding that the present description should be considered an exemplification of the principles of the invention and is not intended to limit the present invention to what has been illustrated and described herein.
[0029] The subject matter required in the present invention will be detailed hereinafter by way of example and not limitation, since the materials and methods disclosed herein may include different details and procedures, without departing from the scope of the invention. Unless otherwise indicated, all parts and percentages disclosed below are by weight.
[0030] The main approach of this invention is related to a process for producing iron ore agglomerate to replace granulate and pellets in direct reduction furnaces comprising the following steps: a) dispersing 0.05-2% by weight of nanomaterial in binder in order to obtain a mixture called "binder mixture"; b) mixing 1-10% of the binder mixture from step a) with 70-99% of iron ore fines and / or steel co-products, 0-5% of chemical and / or mineral additives with properties to promote plasticity and / or improve the porosity of the agglomerate; c) adjust the humidity in such a way as to obtain the amount of 0-25% by weight of water in the mixture; d) carry out the agglomeration process via briquetting or extrusion; e) cure the agglomerate; f) apply a coating to the surface of the agglomerate (coating) in order to reduce the sticking effect in the RD reactors.
[0031] The agglomerate production process, represented by the block diagram in Figure 1, preferably begins with the dispersion of the nanomaterial in the binder(s) under mechanical agitation, at a dosage of 0.05 to 2% by weight relative to the amount of binder used in the mixture. The nanomaterials used in step a) can be carbon nanotubes, exfoliated graphite, functionalized microsilicate, tubular nanosilica, tubular halloysite, carbon nanofiber, graphene, among others.
[0032] The binders used in step a) may consist of sodium silicate, vegetable tar, pitch, starch, phenolic resins, molasses, among others. These binders, which bind particles together through adhesion and / or chemical interaction, can be used individually or in combination to achieve greater strength of the agglomerated product.
[0033] Step b) of the process of the present invention consists of adding 1 to 10% of the agglomerating mixture obtained in step a) to 70 to 99% by weight of iron ore fines and / or steel by-products, and 0 to 5% by weight of chemical and / or mineral additives, and then carrying out the mixing process in an intensive mixer for a maximum time of 4 minutes. The additives used as plasticizing agents consist of bentonite, pitch, tar, starch, and hydrated lime, and have the property of increasing plastic conformation during the subsequent agglomeration step. Additives containing some porosity-forming substances, such as pitch, tar, phenolic resins, glucose, starch, molasses, glycerin, CMC (carboxymethyl cellulose), and biomass, are also used, which promote greater porosity in the agglomerate after curing.
[0034] The iron ore fines and steel co-products used in step b) of the process of the present invention preferably have Fe contents to tai >60%, SiO2 <5%, AI2O3 <2%, particle size 98% <6mm, and maximum moisture content of 25%. The steelmaking co-products used may consist of pellet fines, DRI (Direct Reduced Iron) fines, sludge, scale (scale), among others. The quality of these co-products may vary depending on the mill and, therefore, their use as raw material is subject to compliance with the levels previously mentioned and through prior laboratory tests.
[0035] Step c) of this process consists of adjusting the moisture content of the mixture by adding water to obtain the optimum moisture content of 0 to 25%, desired for the agglomeration step.
[0036] Step d) of the present invention refers to the agglomeration process that can be carried out by means of briquetting or extrusion.
[0037] For extrusion agglomeration, the optimum moisture content should be in the range of 8-25%. In addition to the addition of binders and additives, the strength and porosity of the green agglomerate are also adjusted during the production process by controlling the negative pressure in equipment called extruders. The resulting extrudates are cylindrical tubes measuring 5-50 mm in diameter and 50-200 mm in length.
[0038] For agglomeration by briquetting, the mixture should preferably contain between 1-7% moisture. The briquetting process takes place in a roller press with cavities designed to produce pillow-shaped briquettes with dimensions of 15-50 mm x 10-40 mm x 5-25 mm. This geometry and adequate control of these dimensions, combined with the raw materials and process conditions used, allow for the production of agglomerates with greater mechanical strength, generating excellent performance results.
[0039] During the briquetting process, it is essential to control the pressure and speed of the rolls, control the distance between rolls (maintaining the minimum gap, avoiding the generation of open and / or burr-like briquettes), and control the feed rate, in order to obtain a briquette with an apparent density of less than 3.8 g / cm 3 and packaging degree of the order or less than 50%, aiming to meet metallurgical properties.
[0040] The pressure and speed of the rollers are controlled by changing the amperage of the briquette machine, with each machine having a different type of Different adjustments. It is not possible to define predetermined amperage ranges, as these can vary significantly depending on the type, brand, and capacity of the briquette machine. Therefore, a control that is best applied and can be replicated across different machines is through the calculation of linear force, the recommended value of which is 15 to 30 kN / cm. The higher the amperage, the greater the force of particle approximation and, consequently, the greater the compaction (packing and apparent density), and the lower the porosity. However, it is necessary to achieve an optimum between packing, apparent density, porosity, and the physical quality of the agglomerate.
[0041] Step e) of this production process involves curing the agglomerate, which can be performed using gas, electric, infrared, electromagnetic, or room-temperature ovens. The temperature and curing time in the various types of ovens will be determined by the type of binder or binder mixture used. If the binder is pure sodium silicate, 10 to 30 minutes at a temperature of 100 to 550°C can be used in electric, infrared, or gas ovens. For microwave-based electromagnetic ovens, the time would be 2 to 15 minutes. For room-temperature curing, the time can be up to 15 days.
[0042] Step f) consists of applying another layer of chemical or mineral agent through immersion, spraying, or other technology to reduce the adhesion of agglomerates in direct reduction reactors. These additives can include bauxite, betonite, serpentinite, cement, magnesium hydroxide, limestone, and combinations thereof. The dosage of coating agent per ton of agglomerate can vary from 1 to 10 kg. For application, the coating is suspended in water.
[0043] The iron ore agglomerate obtained through the process of the present invention has physical, chemical and metallurgical properties to replace pellets and granulated in direct reduction furnaces, bringing gains in efficiency and productivity in the metallurgical chain. The characteristics of the final agglomerate obtained are: • High iron content (Fe> 60%) • Low deleterious content (NazO, SiCh and AI2O3 < 5%) • Low disintegration value (<10%, reaching values <5%) • High metallization content (> 90%, reaching values of 99.5%)
[0044] The high performance of the agglomerates obtained by the present invention in direct reduction reactors is only possible due to three key factors that are controlled during the process: • Packaging degree < 50% • Apparent density < 3.8 g / cm3 • Porosity > 40%, with network of connected pores
[0045] Porosity for this type of agglomerate is crucial for its subsequent application in direct reduction reactors. Porosity control allows gases to enter and exit the agglomerate's internal structure during the direct reduction process without compromising its physical quality. Failure to do so can severely impact the product's strength during reduction, resulting in the product failing to meet the minimum performance requirements. This results in fines being generated through disintegration, which is detrimental to the direct reduction reactor process.
[0046] Figure 2 presents a comparison showing the evolution of the disintegration results obtained throughout the research and development (R&D) process aimed at optimizing the present invention. Figure 2A shows agglomerates obtained using processes known in the prior art, showing high disintegration values, in the order of 40 to 65%. Figure 2B presents an initial evolution obtained throughout the R&D process, showing disintegration values. between 20 and 30%. Figure 2C shows agglomerates obtained through the process described in the present invention, whose disintegration value is below 10%.
[0047] The degree of particle packing (or compaction) directly influences the level of agglomerate disintegration in direct reduction reactors, in addition to improving the degree of metallization. Less dense agglomerates have greater porosity, allowing more homogeneous (less abrupt) gas entry and exit during metallurgical operations within a direct reduction reactor, as mentioned previously.
[0048] The present invention allows achieving optimal parameters of packaging degree and porosity through adjustments in the agglomeration conditions, improvement of the agglomerate finish and use of additives (chemical or mineral) to improve porosity. EXAMPLE
[0049] Iron ore fines agglomerates for specific use in direct reduction reactors were produced according to the process described by the present invention.
[0050] Iron ore fines containing 96% by weight of pellet feed containing 68.5% Fe and a particle size <0.15 mm were used as the iron ore fines. Sodium silicate and nanomaterial were used as binders. Starch and hydrated lime were used as additives. The agglomeration process chosen was briquetting, and pillow-shaped briquettes with the following dimensions were produced: 25x20x15 mm.
[0051] The amperage used in the briquetting machine varied between 30 and 40 Å, corresponding to a linear force in the order of 15.7 to 29.4 kN / cm. The briquettes were cured in a gas oven for 30 min, at a temperature range of 250-350°C. After curing, the briquettes underwent a coating step using sprayed cement.
[0052] The briquettes obtained, as shown in Figure 3, were subjected to chemical-physical-metallurgical tests to attest to the quality of the final agglomerate obtained. The chemical and physical quality results for various briquette samples are presented in Table 1 below: [
[0053] The image of the DRI agglomerates obtained after performing basket tests in Midrex and HyL industrial reactors is presented in Figure 4, and the quality data of these DRI agglomerates are shown in Figure 5 (metallization and carburization) and Figure 6 (disintegration under reduction).
[0054] Thus, although only some embodiments of the present invention have been shown, it will be understood that various omissions, substitutions, and changes may be made by one skilled in the art without departing from the spirit and scope of the present invention. The described embodiments should be considered in all respects only as illustrative and not restrictive.
[0055] It is expressly intended that all combinations of the elements that perform the same function in substantially the same manner to achieve the same results are within the scope of the invention. Substitutions of elements from one described embodiment to another are also fully intended and contemplated.
Claims
CLAIMS 1. Process for producing iron ore agglomerate for use in direct reduction furnaces, comprising the following steps: a) dispersing 0.05-2% by weight of nanomaterial in binder to obtain an agglomerating mixture; b) mixing 1-10% of the agglomerating mixture from step a) with 70-99% of iron ore fines and / or steel co-products and 0-5% of additives in an intensive mixer; c) adjusting the humidity so as to obtain the amount of 0-25% by weight of water in the mixture; d) carrying out the agglomeration process via briquetting or extrusion; e) curing the agglomerate; f) applying a coating to the surface of the agglomerate (coating) in order to reduce the sticking effect in direct reduction furnaces.
2. Process, according to claim 1, characterized by the fact that the nanomaterial used in step a) is selected from the group consisting of carbon nanotube, exfoliated graphite, functionalized microsilicate, tubular nanosilica, tubular halloysite, carbon nanofiber and graphene.
3. Process, according to claim 1, characterized by the fact that the binder used in step a) is selected from the group consisting of sodium silicate, vegetable tar, pitch, starch, phenolic resins and molasses.
4. Process, according to claim 1, characterized by the fact that the iron ore fines and steel co-products used in step b) have Fetotai contents >60%, SiCh <5%, AI2O3 <2% and particle size 98% <6mm.
5. Process, according to claim 1, characterized by the fact that the additives used in step b) are selected from the group consisting of bentonite, pitch, tar, hydrated lime, phenolic resins, glucose, starch, molasses, glycerin, CMC (carboxy methyl cellulose) and biomass.
6. Process, according to claim 1, characterized by the fact that the mixing in step b) is carried out in an intensive mixer for a maximum time of 4 minutes.
7. Process, according to claim 1, characterized by the fact that the agglomeration in step d) is carried out in extruders producing extrudates in the shape of cylindrical tubes of size 5-50 mm in diameter and 50-200 mm in length.
8. Process, according to claim 1, characterized by the fact that the agglomeration in step d) is carried out in a roller press producing pillow-shaped briquettes with dimensions of 15-50 mm x 10-40 mm x 5-25 mm.
9. Process, according to claim 1, characterized by the fact that the agglomeration in step d) is carried out in a roller press producing briquettes with a degree of packaging < 50%, apparent density < 3.8 g / cm3, and porosity > 40%, with connected pores.
10. Process, according to claim 1, characterized by the fact that the agglomeration in step d) is carried out in a briquetting machine controlling the linear force in the range of 15 to 30 KN / cm.
11. Process, according to claim 1, characterized by the fact that the curing in step e) can be carried out in gas, electric, infrared, electromagnetic or room temperature ovens.
12. Process, according to claim 11, characterized by the fact that curing in gas, electric or infrared ovens is carried out at a temperature of 100 to 550°C, for 10 to 30 minutes.
13. Process, according to claim 11, characterized by the fact that curing in electromagnetic ovens is carried out for 2 to 15 minutes.
14. Process, according to claim 11, characterized by the fact that curing at room temperature is carried out for up to 15 days.
15. Process, according to claim 1, characterized by the fact that the application of coating agent in step f) consists of the application by immersion or spray of a chemical or mineral additive with surface coating properties selected from the group consisting of bauxite, bentonite, serpentinites, cement, magnesium hydroxide, limestones and combinations thereof.
16. Process, according to claim 1, characterized by the fact that, in step f), the dosage of coating agent is 1 to 10 kg per ton of agglomerate.
17. Iron ore agglomerate produced from the process described in claims 1 to 16, characterized by having ideal physical, chemical and metallurgical properties to replace pellets and granulates in direct reduction furnaces, namely Fe> 60%, deleterious (Na2O, SiO2 and AI2O3) < 10%, disintegration <10%, metallization content > 90%, degree of packing < 50%, apparent density < 3.8 g / cm3 and porosity > 40%, with connected pores.
18. Agglomerate, according to claim 17, characterized by having Fe content in the range of 65.1 to 67.5%, deleterious content (Na2O, SiO2 and AI2O3) <5%, disintegration <5%, and metallization content in the range of 91.2 - 99.5%.