Hot-stamped component

MYPI2025003945A0Undetermined Publication Date: 2024-06-30HYUNDAE STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025003945
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-12-30
Filing Date
2023-03-17
Publication Date
2024-06-30

Smart Images

  • Figure PI2025003945_DRAWING_001
    Figure PI2025003945_DRAWING_001
  • Figure PI2025003945_DRAWING_002
    Figure PI2025003945_DRAWING_002
  • Figure PI2025003945_DRAWING_003
    Figure PI2025003945_DRAWING_003
Patent Text Reader

Abstract

The present disclosure provides a hot-stamped component having a pierced portion formed therein, the hot-stamped component including: a base material; an interdiffusion layer arranged on the base material; and a plating layer arranged on the interdiffusion layer, wherein the hot-stamped component includes a shearing-processed surface formed at an edge of the pierced portion, the shearing-processed surface includes a rollover surface, a shear surface, and a fracture surface, and a thickness th1 of the fracture surface and a thickness th2 of the shearing-processed surface satisfy Equation 1 (th1 / th2 ≤ 0.6).
Need to check novelty before this filing date? Find Prior Art

Description

Hot stamping parts

[0001] The present invention relates to a hot stamping part.

[0002] As environmental and fuel efficiency regulations tighten globally, the need for lighter vehicle materials is increasing. Consequently, research and development on ultra-high-strength steel and hot-stamping steel is actively underway.

[0003] Hot stamping is a process that manufactures high-strength parts by heating steel plates to high temperatures in a furnace, then forming them in a press and rapidly cooling them simultaneously. Additionally, a piercing process may be performed to cut and machine holes within the high-strength parts.

[0004] The piercing process uses laser equipment or press molds, but when laser equipment is used, processing time may increase, and when press molds are used, the cross-sectional quality may deteriorate.

[0005] As a technology related to this, there is Korean Patent Publication No. 10-2020-0080721 (Title of invention: Hot stamping part manufacturing device and hot stamping part manufacturing method using the same).

[0006] Embodiments of the present invention can provide a hot stamping part having excellent hydrogen embrittlement resistance.

[0007] One embodiment of the present invention provides a hot stamping part having a piercing portion formed thereon, comprising: a base material; a mutual diffusion layer disposed on the base material; and a plating layer disposed on the mutual diffusion layer; wherein the hot stamping part includes a shearing surface formed on an edge of the piercing portion, the shearing surface includes a rollover surface, a shearing surface, and a fracture surface, and a thickness (th1) of the fracture surface and a thickness (th2) of the shearing surface satisfy the following equation 1.

[0008] <Formula 1>

[0009] th1 / th2 ≤ 0.6

[0010] In the present embodiment, the rollover surface, the shear surface, and the fracture surface may be sequentially provided in the thickness direction of the hot stamping part.

[0011] In this embodiment, the thickness of the shear processing surface may be the sum of the thickness of the fracture surface, the thickness of the shear surface, and the thickness of the rollover surface.

[0012] In the present embodiment, the thickness of the fracture surface may be the shortest distance in the thickness direction of the hot stamping part from the start point of the fracture surface to the end point of the fracture surface.

[0013] In the present embodiment, the thickness of the sheared surface may be the shortest distance in the thickness direction of the hot stamping part from the starting point of the rollover surface to the end point of the fracture surface.

[0014] In the present embodiment, the hot stamping part may further include a plating layer peel-off surface in which at least a portion of the upper surface of the intermixing layer is exposed.

[0015] In this embodiment, the width (w1) of the plating layer peeling surface and the width (w2) of the rollover surface can satisfy the following equation 2.

[0016] <Formula 2>

[0017] w1 / w2 ≤ 0.6

[0018] In this embodiment, at least two piercing parts may be provided.

[0019] Other aspects, features and advantages other than those described above will become apparent from the following detailed description, claims and drawings for carrying out the invention.

[0020] According to one embodiment of the present invention, which is achieved as described above, a hot stamping part with excellent hydrogen embrittlement resistance can be provided. Of course, the scope of the present invention is not limited by these effects.

[0021] FIG. 1 is a perspective view schematically illustrating a hot stamping part according to one embodiment of the present invention.

[0022] FIG. 2 is a cross-sectional view schematically illustrating a hot stamping part according to one embodiment of the present invention.

[0023] Figure 3 is an enlarged view of part A of Figure 2.

[0024] FIG. 4a is a side view of a piercing portion of a hot stamping part according to one embodiment of the present invention.

[0025] FIG. 4b is a drawing of a piercing portion of a hot stamping part according to one embodiment of the present invention when viewed from the front.

[0026] Figure 4c is an enlarged view of a portion of Figure 4a.

[0027] Figure 5a is a drawing of the piercing portion of a hot stamping part according to a comparative example when viewed from the side.

[0028] Figure 5b is a drawing of the piercing portion of a hot stamping part according to a comparative example when viewed from the front.

[0029] Figure 5c is an enlarged view of a portion of Figure 5a.

[0030] Figure 6 is a flowchart schematically illustrating a method for manufacturing a hot stamping part according to one embodiment of the present invention.

[0031] Figure 7 is a flowchart schematically illustrating a preparation step of a method for manufacturing a hot stamping part according to one embodiment of the present invention.

[0032] Figure 8 is a plan view schematically illustrating a blank according to one embodiment of the present invention.

[0033] FIG. 9 is a flowchart schematically illustrating a heating step of a method for manufacturing a hot stamping part according to one embodiment of the present invention.

[0034] FIG. 10 is a drawing illustrating a heating furnace having a plurality of sections in a heating step of a method for manufacturing a hot stamping part according to one embodiment of the present invention.

[0035] FIGS. 11 and 12 are cross-sectional views illustrating a forming / piercing step of a manufacturing process of a hot stamping part according to one embodiment of the present invention.

[0036] The present invention is capable of various modifications and embodiments. Specific embodiments are illustrated in the drawings and described in detail in the detailed description. The effects and features of the present invention, as well as the methods for achieving them, will become clearer with reference to the embodiments described in detail below, along with the drawings. However, the present invention is not limited to the embodiments disclosed below and can be implemented in various forms.

[0037] In the examples below, the terms first, second, etc. are not used in a limiting sense, but are used for the purpose of distinguishing one component from another.

[0038] In the examples below, singular expressions include plural expressions unless the context clearly indicates otherwise.

[0039] In the following examples, terms such as “include” or “have” mean that a feature or component described in the specification is present, and do not preclude the possibility that one or more other features or components may be added.

[0040] For convenience of explanation, the sizes of components in the drawings may be exaggerated or reduced. For example, the sizes and thicknesses of each component shown in the drawings are arbitrarily shown for convenience of explanation, and the present invention is not necessarily limited to what is shown.

[0041] In some embodiments, where implementations are otherwise feasible, specific process sequences may be performed in a different order than described. For example, two processes described in succession may be performed substantially simultaneously, or in a reverse order from the described order.

[0042] In this specification, “A and / or B” refers to the case where it is A, or B, or both A and B. And, “at least one of A and B” refers to the case where it is A, or B, or both A and B.

[0043] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings. When describing with reference to the drawings, identical or corresponding components are given the same reference numerals and redundant descriptions thereof will be omitted.

[0044] FIG. 1 is a perspective view schematically illustrating a hot stamping part according to one embodiment of the present invention.

[0045] Referring to FIG. 1, a hot stamping part (10) according to one embodiment of the present invention may include a piercing portion (110). In one embodiment, the hot stamping part (10) may include two piercing portions (110). The piercing portions (110) may include a first piercing portion (110a) and a second piercing portion (110b). However, the present invention is not limited thereto. The hot stamping part (10) may include one piercing portion (110) or three or more piercing portions (110).

[0046] Although not shown, the hot stamping part (10) may include an additional piercing part in addition to the piercing part (110). In this case, the piercing part (110) may be formed through hot piercing, and the additional piercing part may be formed through cold piercing or laser piercing. The hot stamping part (10) may be provided with one or more additional piercing parts.

[0047] In one embodiment, an additional piercing portion may be formed using the piercing portion (110). This will be described in more detail below.

[0048] Additionally, although not shown, the hot stamping part (10) may include an edge portion. In this case, the edge portion of the hot stamping part (10) may mean a surface extending along the long side of the hot stamping part (10).

[0049] Fig. 2 is a cross-sectional view schematically illustrating a hot stamping part according to one embodiment of the present invention, and Fig. 3 is an enlarged view of portion A of Fig. 2. Specifically, Fig. 2 is a cross-sectional view schematically illustrating a piercing portion of a hot stamping part according to one embodiment of the present invention.

[0050] Referring to FIGS. 2 and 3, a hot stamping part (10) according to one embodiment may include a base material (200), a mutual diffusion layer (210), and a plating layer (220). The base material (200), the mutual diffusion layer (210), and the plating layer (220) may be sequentially provided in the thickness direction of the hot stamping part (10). At this time, the thickness direction of the hot stamping part (10) may be defined as a vertical direction, and the direction intersecting the thickness direction of the hot stamping part (10) may be defined as a horizontal direction.

[0051] In one embodiment, the hot stamping part (10) may include a shearing surface (300) formed on the edge of the piercing portion (110). The shearing surface (300) may include a rollover surface (301), a shearing surface (302), and a fracture surface (303).

[0052] In one embodiment, the rollover surface (301) may be a surface where sagging or pressing occurs. As described below, when the punch is lowered during shearing (or hot piercing), the blank may be plastically deformed and sagging may occur, which may cause curvature to occur on the uppermost surface of the parent material (200) forming the upper surface in the horizontal direction. At this time, the surface of the uppermost surface of the parent material (200) where the curvature occurs may correspond to the rollover surface (301). The rollover surface (301) may correspond to the point where the curvature begins to occur on the uppermost surface of the parent material (200) to the point where the shear surface (302) begins.

[0053] In one embodiment, the shear plane (302) may be a plane that extends and is formed in the vertical direction or at a predetermined angle with the vertical direction. As described below, as the punch continues to descend in the vertical direction, the sagging of the blank ends and the punch and the blank come into direct contact, so that shearing (or piercing) may proceed, and as the shearing (or piercing) proceeds, the shear plane (302) may be formed along the vertical direction. For example, the curvature that occurred at the top surface of the base material (200) may disappear, and a straight shear plane (302) may be formed along the vertical direction or at a predetermined angle with the vertical direction. The shear plane (302) may correspond to a point from which the rollover plane (301) ends to a point at which the fracture plane (303) begins.

[0054] In one embodiment, the fracture surface (303) may be a surface formed as the blank is fractured. As will be described below, as the punch is lowered in the vertical direction, at least a portion of the blank may fracture, thereby forming the fracture surface (303). Since the fracture surface (303) is formed by the fracture of at least a portion of the blank, it may be irregular compared to the shear surface (302). The fracture surface (303) may correspond to a point from which the irregular formation compared to the shear surface (302) begins to occur, to a point at which the fracture surface (303) ends or to an end point of the parent material (200).

[0055] In one embodiment, the shear surface (302) is a portion that directly rubs against the punch, and when viewed from the front, the shear surface (302) may have a glossy surface due to direct friction with the punch. In addition, the fracture surface (303) is a portion where the blank is irregularly removed, and may have a rough surface. Therefore, since the shear surface (302) has a smooth surface and the fracture surface (303) has an irregular surface, it may be easy to distinguish the boundary point between the shear surface (302) and the fracture surface (303).

[0056] In one embodiment, the plating layer detachment surface (304) may be a surface from which at least a portion of the plating layer (220) is removed. A mutual diffusion layer (210) may be formed due to alloying of the base material (200) and the plating layer (220) during hot stamping heat treatment. At this time, at least a portion of the plating layer (220) disposed on the upper surface of the mutual diffusion layer (210) may be detached (or removed) during hot piercing. The plating layer detachment surface (304) may be defined as a surface from which at least a portion of the plating layer (220) disposed on the upper surface of the mutual diffusion layer (210) is detached (or removed). The plating layer detachment surface (304) may correspond to a point from which the upper surface of the mutual diffusion layer (210) exposed by removing at least a portion of the plating layer (220) and the plating layer (220) meet to a point from which the shear surface (302) begins.

[0057] In one embodiment, the thickness (th1) of the fracture surface (303) may be defined as the shortest vertical distance from the boundary point of the shear surface (302) and the fracture surface (303) to the end point of the parent material (200). In other words, the thickness (th1) of the fracture surface (303) may be defined as the shortest distance between a first virtual line (or, first virtual plane) extending horizontally through the boundary point of the shear surface (302) and the fracture surface (303) and a second virtual line (or, second virtual plane) extending horizontally through the end point of the parent material (200). In this case, the end point of the parent material (200) may mean the end point of the fracture surface (303).

[0058] In one embodiment, the thickness (th3) of the shear surface (302) may be defined as the shortest vertical distance from the boundary point of the rollover surface (301) and the shear surface (302) to the boundary point of the shear surface (302) and the fracture surface (303). In other words, the thickness (th3) of the shear surface (302) may be defined as the shortest distance between a third virtual line (or second virtual line) extending horizontally through the starting point of the shear surface (302) and a fourth virtual line (or fourth virtual line) extending horizontally through the boundary point of the shear surface (302) and the fracture surface (303).

[0059] In one embodiment, the thickness (th4) of the rollover surface (301) may be defined as the shortest distance in the vertical direction from the point where the curvature of the parent material (200) begins to the point where the shear surface (302) begins. In other words, the thickness (th4) of the rollover surface (301) may be defined as the shortest distance between a fifth virtual line (or fifth virtual plane) extending horizontally and contacting the upper surface of the parent material (200) and a sixth virtual line (or sixth virtual plane) extending horizontally and passing through the point where the shear surface (302) begins.

[0060] In one embodiment, the thickness (th2) of the shearing surface (300) may be defined as the shortest vertical distance from the point where the curvature of the base material (200) begins to the end point of the base material (200). In other words, the thickness (th2) of the shearing surface (300) may be defined as the shortest distance between a fifth virtual line (or fifth virtual plane) that is in contact with the upper surface of the base material (200) and extends in the horizontal direction and a second virtual line (or second virtual plane) that passes through the end point of the base material (200) and extends in the horizontal direction. For example, the thickness (th2) of the shearing surface (300) may be the sum of the thickness (th1) of the fracture surface (303), the thickness (th3) of the shearing surface (302), and the thickness (th4) of the rollover surface (301).

[0061] In one embodiment, the width (w1) of the plating layer detachment surface (304) may be defined as the shortest distance in the horizontal direction from the point where the upper surface of the mutually diffusion layer (210) exposed by removing at least a portion of the plating layer (220) and the plating layer (220) meet to the point where the shear plane (302) begins. In other words, the width (w1) of the plating layer detachment surface (304) may be defined as the shortest distance between a seventh virtual line (or seventh virtual plane) extending in the vertical direction through the point where the upper surface of the mutually diffusion layer (210) exposed by removing at least a portion of the plating layer (220) and the plating layer (220) meet and an eighth virtual line (or eighth virtual plane) extending in the vertical direction through the point where the shear plane (302) begins.

[0062] In one embodiment, the width (w2) of the rollover surface (301) may be defined as the shortest distance in the horizontal direction from the point where the curvature of the parent material (200) begins to the point where the shear surface (302) begins. In other words, the width (w2) of the rollover surface (301) may be defined as the shortest distance between a ninth virtual line (or, ninth virtual plane) that passes through the point where the curvature of the parent material (200) begins and extends in the vertical direction and an eighth virtual line (or, eighth virtual plane) that passes through the point where the shear surface (302) begins and extends in the vertical direction.

[0063] Increasing the temperature of the blank can reduce the flow stress, and decreasing the stress acting on the blank can improve the hydrogen embrittlement resistance.

[0064] In one embodiment, as described below, hot piercing at a relatively high temperature can reduce the shear stress acting on the blank compared to cold piercing where shearing is performed at about 30°C (e.g., room temperature), thereby improving hydrogen embrittlement resistance.

[0065] FIG. 4a is a side view of a piercing portion of a hot stamping part according to one embodiment of the present invention, FIG. 4b is a front view of a piercing portion of a hot stamping part according to one embodiment of the present invention, and FIG. 4c is an enlarged view of a portion of FIG. 4a.

[0066] In addition, Fig. 5a is a drawing of a piercing portion of a hot stamping part according to a comparative example when viewed from the side, Fig. 5b is a drawing of a piercing portion of a hot stamping part according to a comparative example when viewed from the front, and Fig. 5c is an enlarged drawing of a portion of Fig. 5a.

[0067] Specifically, FIGS. 4a, 4b, and 4c correspond to cases where hot piercing is performed, and FIGS. 5a, 5b, and 5c correspond to cases where cold piercing is performed.

[0068] Referring to FIGS. 4a, 4b, 4c, 5a, 5b, and 5c, it can be confirmed that the width (w2) of the rollover surface (301) when hot piercing is performed is larger than the width (w2') of the rollover surface (301') when cold piercing is performed. In addition, it can be confirmed that the width (w1) of the plating layer peeling surface (304) when hot piercing is performed is smaller than the width (w1') of the plating layer peeling surface (304') when cold piercing is performed. Therefore, when hot piercing is performed, the width (w2) of the rollover surface (301) may increase, and the width (w1) of the plating layer peeling surface (304) may decrease, compared to when cold piercing is performed. That is, when piercing is performed when the temperature of the blank is high, the width (w2) of the rollover surface (301) may be larger and the width (w1) of the plating layer peeling surface (304) may be smaller compared to when piercing is performed when the temperature of the blank is low.

[0069] It can be confirmed that when hot piercing is performed, the shear surface fraction is larger and the fracture surface fraction is smaller compared to when cold piercing is performed. Specifically, it can be confirmed that the thickness (th3) of the shear surface (302) when hot piercing is performed is larger than the thickness (th3') of the shear surface (302') when cold piercing is performed. In addition, it can be confirmed that the thickness (th1) of the fracture surface (303) when hot piercing is performed is smaller than the thickness (th1') of the fracture surface (303') when cold piercing is performed. Through this, it can be confirmed that when hot piercing is performed, the ratio of the shear surface (302) among the shear processing surface (300) is larger and the ratio of the fracture surface (303) is smaller compared to when cold piercing is performed.

[0070] It can be confirmed that in the case of performing hot piercing, the ratio of the rollover surface (301) to the shearing surface (300) is larger than in the case of performing cold piercing. Specifically, it can be confirmed that the thickness (th4) of the rollover surface (301) in the case of performing hot piercing is larger than the thickness (th4') of the rollover surface (301') in the case of performing cold piercing. Through this, it can be confirmed that in the case of performing hot piercing, the thickness (th4) of the rollover surface (301) increases compared to in the case of performing cold piercing.

[0071] As the shear stress applied to the blank (100) during piercing increases, the proportion of the fracture surface (303) among the sheared surface (300) may increase. Specifically, as the shear stress applied to the blank (100) increases, the thickness (th1) of the fracture surface (303) may increase, and the thickness (th3) of the shear surface (302) may decrease. A large thickness (th1) of the fracture surface (303) may mean that the shear stress applied to the blank is large, and hydrogen embrittlement may be induced in the piercing portion (110) due to the large shear stress. Therefore, in order to improve the hydrogen embrittlement resistance of the hot stamping part (10), it is necessary to reduce the thickness (th1) of the fracture surface (303) below a certain level.

[0072] In addition, as the shear stress applied to the blank increases, the width (w1) of the plating layer peeling surface (304) may increase and the width (w2) of the rollover surface (301) may decrease. Therefore, in order to improve the hydrogen embrittlement resistance of the hot stamping part (10), it is necessary to reduce the width (w1) of the plating layer peeling surface (304) and increase the width (w2) of the rollover surface (301).

[0073] Accordingly, the inventors of the present invention have derived Equations 1 and 2 through excessively repeated experiments to enable a hot stamping part (10) to have excellent hydrogen embrittlement resistance. In one embodiment, the hot stamping part (10) can satisfy Equations 1 and 2. Specifically, in the hot stamping part (10), the thickness (th1) of the fracture surface (303) and the thickness (th2) of the sheared surface (300) can satisfy Equation 1, and in the hot stamping part (10), the width (w1) of the plating layer peeling surface (304) and the width (w2) of the rollover surface (301) can satisfy Equation 2.

[0074] <Formula 1>

[0075] th1 / th2 ≤ 0.6

[0076] <Formula 2>

[0077] w1 / w2 ≤ 0.6

[0078] In one embodiment, the value of the thickness (th1) of the fracture surface (303) / the thickness (th2) of the shear-processed surface (300) may be an average value of the values ​​of the thickness (th1) of the fracture surface (303) / the thickness (th2) of the shear-processed surface (300) measured at at least four points at equal angles from the center of the piercing portion (110).

[0079] In one embodiment, the value of the width (w1) of the plating layer peeling surface (304) / the width (w2) of the rollover surface (301) may be an average value of the values ​​of the width (w1) of the plating layer peeling surface (304) / the width (w2) of the rollover surface (301) measured at at least four points at equal angles from the center of the piercing portion (110).

[0080] In the case of cold piercing, if the clearance decreases, the fraction of the fracture surface may also decrease. That is, in the case of cold piercing, if the clearance decreases, the ratio of the thickness (th1) of the fracture surface (303) to the thickness (th2) of the shear-processed surface (300) may decrease. However, if the clearance decreases, the shear stress acting on the blank may increase. Therefore, the shear stress and the fraction of the fracture surface may be inversely proportional.

[0081] In the case of hot piercing, piercing is performed at a relatively high temperature compared to cold piercing, so the shear stress acting on the blank can be reduced, and the fraction of the fracture surface can also be reduced.

[0082] In addition, when piercing is performed at a high temperature, the length of the plating layer (220) that is peeled off around the piercing portion (110) may decrease. In addition, as the temperature of the blank increases and the clearance increases, the stress acting on the blank may decrease, which may increase the area of ​​the rollover surface (301), and may also increase the width (w1) of the rollover surface (301).

[0083] If the fraction of the fracture surface (303) is large, it can be seen that a large shear stress is applied to the piercing portion (110) during hot piercing, and if a large shear stress is applied to the piercing portion (110), hydrogen embrittlement may occur in the portion adjacent to the piercing portion (110) of the hot stamping part (10). That is, if the thickness (th1) of the fracture surface (303) is large, it can be seen that a large shear stress is applied to the piercing portion (110) during hot piercing, and if a large shear stress is applied to the piercing portion (110), hydrogen embrittlement may occur in the portion adjacent to the piercing portion (110).

[0084] If the thickness (th1) of the fracture surface (303) of the hot stamping part (10) and the thickness (th2) of the shear-processed surface do not satisfy Equation 1, hydrogen embrittlement may occur in a portion adjacent to the piercing portion (110). Specifically, if the value of the thickness (th1) of the fracture surface (303) / the thickness (th2) of the shear-processed surface (300) of the hot stamping part (10) exceeds 0.6, this may mean that the fraction of the fracture surface (303) among the shear-processed surface (300) is large, which means that a large shear stress is applied to the piercing portion (110) during piercing, and as a result, hydrogen embrittlement may occur in a portion adjacent to the piercing portion (110) of the hot stamping part (10).

[0085] Therefore, when the thickness (th1) of the fracture surface (303) of the hot stamping part (10) and the thickness (th2) of the sheared surface (300) satisfy Equation 1, hydrogen embrittlement can be prevented or minimized from occurring in the area adjacent to the piercing portion (110).

[0086] If the shear stress applied to the blank during piercing increases, hydrogen embrittlement may occur around the piercing portion (110). In addition, if the shear stress applied to the blank during piercing increases, the plating layer (220) peeled off around the piercing portion (110) may increase, and the length (or area) of the rollover surface (301) may decrease. Specifically, if the shear stress applied to the blank during piercing increases, the width (w1) of the plating layer peeled-off surface (304) may increase, and the width (w2) of the rollover surface (301) may decrease.

[0087] If the width (w1) of the plating layer peeling surface (304) of the hot stamping part (10) and the width (w2) of the rollover surface (301) do not satisfy Equation 2, hydrogen embrittlement may occur in a portion adjacent to the piercing portion (110). Specifically, in order for the value of the width (w1) of the plating layer peeling surface (304) / the width (w2) of the rollover surface (301) of the hot stamping part (10) to exceed 0.6, the width (w1) of the plating layer peeling surface (304) must increase or the width (w2) of the rollover surface (301) must decrease. An increase in the width (w1) of the plating layer peeling surface (304) or a decrease in the width (w2) of the rollover surface (301) means that a large shear stress is applied to the piercing portion (110). Therefore, when the value of the width (w1) of the plating layer peeling surface (304) / width (w2) of the rollover surface (301) of the hot stamping part (10) exceeds 0.6, this means that a large shear stress is applied to the piercing portion (110) during piercing, and this may cause hydrogen embrittlement to occur in a portion adjacent to the piercing portion (110) of the hot stamping part (10).

[0088] Therefore, when the width (w1) of the plating layer peeling surface (304) of the hot stamping part (10) and the width (w2) of the rollover surface (301) satisfy Equation 2, hydrogen embrittlement can be prevented or minimized from occurring in the area adjacent to the piercing portion (110).

[0089] Below, the manufacturing method of hot stamping parts will be described.

[0090] Figure 6 is a flowchart schematically illustrating a method for manufacturing a hot stamping part according to one embodiment of the present invention.

[0091] Referring to FIG. 6, a method for manufacturing a hot stamping part according to one embodiment may include a preparation step (S100), a heating step (S200), a transfer step (S300), and a forming / piercing step (S400).

[0092] FIG. 7 is a flowchart schematically illustrating a preparation step of a method for manufacturing a hot stamping part according to one embodiment of the present invention, and FIG. 8 is a plan view schematically illustrating a blank according to one embodiment of the present invention.

[0093] Referring to FIGS. 7 and 8, the preparation step (S100) may be a step of preparing a blank (100) for hot stamping. In one embodiment, the preparation step (S100) may include a hot rolling step (S110), a cooling / coiling step (S120), a cold rolling step (S130), an annealing step (S140), a plating step (S150), and a cutting step (S160).

[0094] First, a reheating step of the steel slab may be performed. In the reheating step of the steel slab, the steel slab obtained through the continuous casting process is reheated to a predetermined temperature, so that the components segregated during casting can be re-dissolved. In one embodiment, the slab reheating temperature (SRT) may be about 1,200°C to about 1,400°C. If the slab reheating temperature (SRT) is lower than about 1,200°C, the components segregated during casting may not be sufficiently re-dissolved, making it difficult to significantly see the homogenization effect of the alloy elements and the solid solution effect of titanium (Ti). A higher slab reheating temperature (SRT) is advantageous for homogenization, but if the slab reheating temperature (SRT) exceeds about 1,400°C, the austenite crystal grain size increases, making it difficult to secure strength, and the manufacturing cost of the steel plate may increase due to the excessive heating process.

[0095] In the hot rolling step (S110), the reheated plate may be hot rolled at a predetermined finishing rolling temperature. A hot-rolled steel plate may be manufactured through the hot rolling step (S110). In one embodiment, the finishing rolling temperature (Finishing Delivery Temperature: FDT) may be about 880°C to about 950°C. At this time, if the finishing rolling temperature (FDT) is lower than about 880°C, it is difficult to secure the workability of the steel plate due to the occurrence of a mixed grain structure caused by abnormal region rolling, and not only may the workability be reduced due to microstructural non-uniformity, but also a problem of sheet passing during hot rolling may occur due to a rapid phase change. If the finishing rolling temperature (FDT) exceeds about 950°C, the austenite grains may become coarser, and the TiC precipitates may become coarser, which may deteriorate the performance of the hot stamping part.

[0096] In the cooling / coiling step (S120), the hot-rolled hot-rolled steel sheet may be cooled to a predetermined coiling temperature (Coiling Temperature, CT) and coiled. In one embodiment, the coiling temperature of the cooling / coiling step (S120) may be about 550°C to about 800°C. The coiling temperature affects the redistribution of carbon, and when the coiling temperature is lower than about 550°C, the low-temperature phase fraction due to overcooling may increase, which may increase the strength, and there is a concern that the rolling load may be intensified during cold rolling, and the ductility may rapidly decrease. Conversely, when the coiling temperature exceeds about 800°C, abnormal crystal grain growth or excessive crystal grain growth may cause formability deterioration and strength deterioration.

[0097] In the cold rolling step (S130), the coiled hot-rolled steel sheet may be uncoiled, pickled, and then cold rolled. The pickling process may be performed to remove scale from the coiled hot-rolled steel sheet, i.e., the hot-rolled coil manufactured through the hot rolling process. Through the cold rolling step (S130), a cold-rolled steel sheet may be manufactured.

[0098] The annealing step (S140) may anneal the cold-rolled cold-rolled steel sheet at a temperature of about 700°C or higher. For example, the annealing step (S140) may include heating the cold-rolled cold-rolled steel sheet and cooling the heated cold-rolled steel sheet at a predetermined cooling rate. The cold-rolled steel sheet may be annealed in the annealing step (S140). The annealing step (S140) may be performed in an annealing furnace.

[0099] In one embodiment, the annealing temperature of the cold-rolled steel sheet may be between about 750°C and about 900°C. If the annealing temperature of the cold-rolled steel sheet is lower than about 750°C, the desired structure may not be obtained, and recrystallization may not be sufficiently completed. On the other hand, if the annealing temperature of the cold-rolled steel sheet exceeds about 900°C, the annealing temperature may be too high, reducing the efficiency of the manufacturing process. Therefore, if the annealing temperature of the cold-rolled steel sheet satisfies the range of about 750°C to about 900°C, the desired structure may be obtained, recrystallization may be sufficiently completed, and the efficiency of the manufacturing process may be improved.

[0100] The plating step (S150) may be a step of forming a plating layer on an annealed cold-rolled steel sheet. In one embodiment, a plating layer may be formed on the annealed cold-rolled steel sheet through the plating step (S150). At this time, the plating layer may include a zinc (Zn)-based plating layer or an aluminum (Al)-based plating layer.

[0101] Specifically, in the plating step (S150), the annealed cold-rolled steel sheet can be immersed in a plating bath. At this time, the plating bath can maintain a temperature of about 400°C to about 700°C. The plating amount is about 40 g / m on both sides of the base material of the cold-rolled steel sheet. 2 About 200 g / m 2 It can be done. After the plating step (S150), the cold rolled steel sheet with the plating layer formed can be wound into a coil shape.

[0102] Although Fig. 7 illustrates that a cold rolling step (S130), an annealing step (S140), and a plating step (S150) are performed after a cooling / coiling step (S120), the present invention is not limited thereto. At least one of the cold rolling step (S130), the annealing step (S140), and the plating step (S150) may be omitted. For example, the cold rolling step (S130) and the annealing step (S140) may be omitted. In this case, the hot-rolled steel sheet on which a plating layer is formed after the plating step (S150) may be coiled into a coil shape.

[0103] Thereafter, in the cutting step (S160), a steel plate (e.g., a cold-rolled steel plate or a hot-rolled steel plate) wound in a coil shape is uncoiled, and then the steel plate can be cut into a blank (100) using a laser or a cold press mold. At this time, the blank (100) may include an outer portion (or edge) of the coil. For example, the blank (100) may include an outer portion (or edge) of the steel plate.

[0104] Referring to Fig. 6, after the preparation step (S100) of preparing a blank (100), a heating step (S200) of heating the blank (100) may be performed. The heat source method in the heating step (S200) may be direct heating or indirect heating. The heat source method in the heating step (S200) may use either direct heating or indirect heating, or a combination of direct heating and indirect heating.

[0105] In one embodiment, in the heating step (S200), the blank (100) may be heated within a heating furnace. The heating furnace may be provided with one section having one temperature range (or, a single temperature), or may be provided with multiple sections having different temperature ranges. When the heating furnace is provided with one section having one temperature range, the blank (100) may be heated within the heating furnace to a target temperature within one temperature range. At this time, the target temperature may be Ac3 to about 1,000°C. That is, the blank (100) may be heated within a heating furnace having a temperature range of Ac3 to about 1,000°C until the temperature of the blank (100) reaches Ac3 to about 1,000°C.

[0106] On the other hand, if the furnace is equipped with multiple sections having different temperature ranges, the blank (100) can be heated to the target temperature in different temperature ranges within the furnace.

[0107] FIG. 9 is a flowchart schematically illustrating a heating step of a method for manufacturing a hot stamping part according to one embodiment of the present invention, and FIG. 10 is a drawing illustrating a heating furnace having a plurality of sections in the heating step of a method for manufacturing a hot stamping part according to one embodiment of the present invention.

[0108] Referring to FIGS. 9 and 10, in the heating step (S200), the blank (100, see FIG. 8) may be heated in a heating furnace having multiple sections having different temperature ranges. As illustrated in FIG. 9, the heating step (S200) may include a multi-stage heating step (S210) and a soaking heating step (S220). The multi-stage heating step (S210) and the soaking heating step (S220) may be steps in which the blank (100) is heated while passing through multiple sections provided in the heating furnace.

[0109] In one embodiment, the overall temperature of the furnace may be about 680°C to about 1,000°C. Specifically, the overall temperature of the furnace in which the multi-stage heating step (S210) and the soaking heating step (S220) are performed may be about 680°C to about 1,000°C. At this time, the temperature of the furnace in which the multi-stage heating step (S210) is performed may be about 680°C to about Ac3, and the temperature of the furnace in which the soaking heating step (S220) is performed may be about Ac3 to about 1,000°C.

[0110] In the multi-stage heating step (S210), the blank (100) may be heated (or heated) in stages while passing through multiple sections provided in the heating furnace. There may be multiple sections among the multiple sections provided in the heating furnace in which the multi-stage heating step (S210) is performed, and the temperature is set for each section so that the temperature increases from the inlet of the heating furnace into which the blank (100) is introduced toward the outlet of the heating furnace from which the blank (100) is taken out, so that the blank (100) may be heated (or heated) in stages.

[0111] After the multi-stage heating step (S210), a soaking heating step (S220) may be performed. In the soaking heating step (S220), the multi-stage heated blank may be heated (or soaked heated) while passing through a section of a heating furnace set to a temperature of about Ac3 to about 1,000°C. Among the multiple sections provided in the heating furnace, at least one section may be used for the soaking heating step (S220).

[0112] According to one embodiment, a heating furnace may have a plurality of sections having different temperature ranges. Specifically, the heating furnace may have a first section (P1) having a first temperature range (T1), a second section (P2) having a second temperature range (T2), a third section (P3) having a third temperature range (T3), a fourth section (P4) having a fourth temperature range (T4), a fifth section (P5) having a fifth temperature range (T5), a sixth section (P6) having a sixth temperature range (T6), and a seventh section (P7) having a seventh temperature range (T7).

[0113] In one embodiment, in the multi-stage heating step (S210), the blank may be heated stepwise while passing through the first section (P1) to the fourth section (P4) defined within the heating furnace. Additionally, in the crack heating step (S220), the blank that has been multi-stage heated in the first section (P1) to the fourth section (P4) may be crack heated while passing through the fifth section (P5) to the seventh section (P7).

[0114] The first section (P1) to the seventh section (P7) may be arranged sequentially within the furnace. The first section (P1) having the first temperature range (T1) may be adjacent to the inlet of the furnace into which the blank is fed, and the seventh section (P7) having the seventh temperature range (T7) may be adjacent to the outlet of the furnace from which the blank is taken out. Accordingly, the first section (P1) having the first temperature range (T1) may be the first section of the furnace, and the seventh section (P7) having the seventh temperature range (T7) may be the last section of the furnace.

[0115] The temperatures of the plurality of sections provided in the furnace, for example, the temperatures of the first section (P1) to the seventh section (P7), may increase from the inlet of the furnace into which the blank is fed to the outlet of the furnace from which the blank is taken out. However, the temperatures of the fifth section (P5), the sixth section (P6), and the seventh section (P7) may be the same. In addition, the temperature difference between two adjacent sections among the plurality of sections provided in the furnace may be greater than 0°C and less than or equal to 100°C. For example, the temperature difference between the first section (P1) and the second section (P2) may be greater than 0°C and less than or equal to 100°C.

[0116] The furnace temperature of the soaking heating step (S220) may be Ac3 to about 1,000°C. If the furnace temperature of the soaking heating step (S220) is less than Ac3, the manufactured hot stamping part may not have the desired material. On the other hand, if the furnace temperature of the soaking heating step (S220) exceeds about 1,000°C, carbide-forming elements or nitride-forming elements such as Ti, V, Nb, and Mo in the blank (100) are dissolved into the parent material, making it difficult to suppress grain coarsening.

[0117] Although FIG. 10 illustrates a heating furnace according to one embodiment as having seven sections with different temperature ranges, the present invention is not limited thereto. The heating furnace may also have five, six, or eight sections with different temperature ranges.

[0118] In one embodiment, the heating step (S200) is provided with a multi-stage heating step (S210) and a crack heating step (S220), so that the temperature of the heating furnace can be set in stages, thereby improving the energy efficiency of the heating furnace.

[0119] In one embodiment, the furnace may have a length of about 20 m to about 40 m along the transport path of the blank (100). The furnace may have a plurality of sections having different temperature ranges, and a ratio of the length of a section in which the blank is multi-heated among the plurality of sections to the length of a section in which the blank is crack-heated among the plurality of sections may satisfy about 1:1 to about 4:1. If the length of the section in which the blank is crack-heated within the furnace increases so that the ratio of the length of the section in which the blank is multi-heated to the length of the section in which the blank is crack-heated exceeds about 1:1, the amount of hydrogen penetrating into the blank in the crack-heating section may increase, which may increase delayed fracture. On the other hand, if the length of the section in which the blank is crack-heated decreases so that the ratio of the length of the section in which the blank is multi-heated to the length of the section in which the blank is crack-heated is less than about 4:1, the crack-heating section (or time) may not be sufficiently secured, which may result in uneven strength of the manufactured hot stamped part. For example, the length of a uniform heating section among the plurality of sections provided in the furnace may be about 20% to about 50% of the total length of the furnace.

[0120] In one embodiment, the total heating time for which the heating step (S200) is performed may be about 2 min to about 20 min. That is, the total time for which the blank remains in the heating furnace may be about 2 min to about 20 min. If the total heating time for which the heating step (S200) is performed is about 2 min or less, the heating time may be insufficient, and the manufactured hot stamping part may not have a desired material. On the other hand, if the total heating time for which the heating step (S200) is performed is about 20 min or more, the heating time may be too long, which may lower the production speed and reduce economic efficiency. Therefore, if the total heating time for which the heating step (S200) is performed satisfies about 2 min to about 20 min, the manufactured hot stamping part may have a desired material, and at the same time, the reduction in economic efficiency of the manufacturing process may be prevented or minimized.

[0121] Referring to FIG. 6, a transfer step (S300) may be performed after the heating step (S200). In the transfer step (S300), the heated blank (100) may be transferred to a press mold (400, see FIG. 11). For example, the heated blank (100) may be taken out from the heating furnace and then transferred to the press mold (400).

[0122] In the transport step (S300), the heated blank (100) may be cooled to ambient temperature (or room temperature). That is, the heated blank (100) may be air-cooled at ambient temperature during transport. If the heated blank (100) is not air-cooled, the mold entry temperature (e.g., molding start temperature) may increase, causing wrinkles (or bends) to occur on the surface of the manufactured hot stamping part. In addition, since the use of a refrigerant may affect the subsequent process (hot stamping), it may be desirable for the heated blank (100) to be air-cooled during transport.

[0123] FIGS. 11 and 12 are cross-sectional views illustrating a forming / piercing step in a manufacturing process of a hot stamping part according to one embodiment of the present invention. Specifically, FIG. 11 is a cross-sectional view of a blank and a press mold before the forming / piercing step is performed, and FIG. 12 is a cross-sectional view of a blank and a press mold during the forming / piercing step.

[0124] Referring to FIGS. 6, 11, and 12, a forming / piercing step (S400) may be performed after the transfer step (S300). The forming / piercing step (S400) may be a step of hot-forming the transferred blank (100) into the shape of a hot stamping part and forming a piercing portion (110) in the transferred blank (100).

[0125] In one embodiment, the forming / piercing step (S400) may be performed in a press mold (400). The press mold (400) may include a lower mold (410), an upper mold (420), and a punch (430). The lower mold (410) may have a shape of a bottom surface of a hot stamping part. The upper mold (420) may face the lower mold (410) and have a shape of a top surface of a hot stamping part. The press mold (400) may be provided with at least one punch (430), preferably at least two punches (430). In one embodiment, the punches (430) may include a first punch and a second punch. However, the present invention is not limited thereto. For example, the press mold (400) may be provided with only one punch (430), or with three or more punches (430), and various modifications are possible.

[0126] Although not shown, when the press mold (400) is equipped with only one punch (430), a foam bead may be formed at the edge of the blank (100) during molding of the blank (100).

[0127] For example, as will be described later, a laser process or a cold piercing process may be performed using the piercing portion (110) formed through hot piercing. Specifically, the piercing portions (110) formed through hot piercing may be used as guide patterns (or reference points) to secure the blank (100) to a tool, and then subsequent processes may be performed. Accordingly, the number of piercing portions (110) formed on the blank (100) through hot piercing may be at least two.

[0128] In one embodiment, the clearance between the punch (430) and the mold (e.g., the lower mold (410) and / or the upper mold (420)) may be greater than or equal to about 5% and less than or equal to about 15%. If the clearance is less than about 5%, the punch (430) may become stuck in the mold due to thermal expansion of the mold. On the other hand, if the clearance exceeds about 15%, the vibration of the punch (430) may become severe, which may lead to uneven quality, including flow lines on the cross-section. For example, the uniformity of flow lines may deteriorate, such as when many flow lines are formed only on a portion of the cross-section. Accordingly, when the clearance between the punch (430) and the mold (e.g., the lower mold (410) and / or the upper mold (420)) is about 5% to about 15%, the punch (430) can be prevented from being caught in the mold due to thermal expansion, and the short-circuit lines formed around the shear surface can be uniformly formed.

[0129] In one embodiment, the blank (100) can be hot formed in the forming / piercing step (S400). The blank (100) that has been transferred (or heated) can be hot formed using a press mold (400) including a lower mold (410) and an upper mold (420) to form it into the shape of a hot stamping part. Specifically, the blank (100) can be formed into the shape of a hot stamping part by pressing (e.g., hot pressing) the lower mold (410) that has the shape of the bottom surface of the hot stamping part with the upper mold (420) that has the shape of the top surface of the hot stamping part.

[0130] In one embodiment, in the forming / piercing step (S400), hot forming and hot piercing may be performed simultaneously or sequentially. In one embodiment, in the forming / piercing step (S400), hot piercing may be performed on the blank (100) after hot forming of the blank (100) is completed (or started). Specifically, when hot forming the blank (100) (or after hot forming is completed), a punch (430) included in the press die (400) may be lowered to perform hot piercing on the blank (100), thereby forming a piercing portion (110) on the hot stamping part (10) (or blank (100)). For example, after the upper mold (420) reaches the bottom dead center and hot forming of the blank (100) is completed (or hot forming is initiated), the punch (430) may be lowered to perform hot piercing on the blank (100) to form a piercing portion (110) on the hot stamping part (10) (or blank (100)). That is, the hot piercing may be performed after hot forming is completed (or initiated). Alternatively, the hot forming and hot piercing may be performed simultaneously.

[0131] Although not shown, the punch (430) can be raised and lowered using a hydraulic cylinder. However, the present invention is not limited thereto.

[0132] In one embodiment, the forming start temperature at which forming of the blank (100) is initiated when the blank (100) is hot formed in the forming / piercing step (S400) may be equal to or higher than the Ms temperature and equal to or lower than 750°C. If the blank (100) is hot formed at a temperature lower than the Ms temperature, a large load may be generated during the hot forming, which may cause damage to the press die (400), the formability of the blank (100) may be reduced, and the manufactured hot stamping part may not have the targeted structure and properties. On the other hand, if the forming start temperature exceeds about 750°C, wrinkles (or bends) may occur on the surface of the manufactured hot stamping part. In addition, the plating layer may adhere to the die. Therefore, when the forming initiation temperature is about Ms temperature or higher and about 750°C or lower, the formability of the hot stamping steel sheet can be improved, the manufactured hot stamping part can have the target structure and properties, and the occurrence of wrinkles (or bends) on the surface of the manufactured hot stamping part can be prevented or minimized.

[0133] In one embodiment, the temperature of the blank (100) when hot piercing is performed on the blank (100) in the forming / piercing step (S400) may be about 200°C or more and about 700°C or less. If the temperature of the blank (100) during hot piercing is less than about 200°C, a large load may be generated during hot piercing, which may cause damage to the press die (400) and / or the punch (430). On the other hand, since the blank (100) is air-cooled during the process of taking the heated blank (100) out of the heating furnace and being transferred to the press die (400), the temperature of the blank (100) before hot piercing is performed may be about 700°C or less. In addition, since hot piercing is performed after hot forming of the heated blank (100) is completed (or initiated), the temperature of the blank (100) when hot piercing is performed may be lower than the temperature of the blank (100) when hot forming is performed. Therefore, when hot piercing is performed when the temperature of the blank (100) is about 200°C or higher and about 700°C or lower in the forming / piercing step (S400), the piercing portion (110) can be formed in the blank (100) without damaging the press mold (400) and / or the punch (430).

[0134] In one embodiment, when hot forming a blank (100) using a press mold (400), a first punch and a second punch included in the press mold (400) may be lowered to form at least two piercing portions (110a, 110b) in the blank (100). Specifically, in the process of hot forming the blank (100) by pressing the lower mold (410) and the blank (100) with the upper mold (420), the first punch and the second punch may be lowered to form a first piercing portion (110a) and a second piercing portion (110b) in the hot stamping part (10).

[0135] Although FIGS. 11 and 12 illustrate that a punch (430) included in a press mold (400) is lowered to form a piercing portion (110) in a blank (100), the present invention is not limited thereto. Although not illustrated, a piercing portion (110) may also be formed in a blank (100) through a separately provided external device.

[0136] In one embodiment, the blank (100) may be cooled while being formed into the final part shape in the press mold (400) (or during hot forming). The press mold (400) may be provided with cooling channels (440) through which a coolant circulates therein. For example, cooling channels (440) may be provided within the interiors of the lower mold (410) and the upper mold (420), respectively. Specifically, the cooling channels (440) may be arranged within the interiors of the lower mold (410) and the upper mold (420) along the surface of the lower mold (410) and the surface of the upper mold (420). The blank (100), which has been heated by the circulation of the coolant supplied through the cooling channels (440) provided in the press mold (400), may be rapidly cooled. At this time, in order to prevent a spring back phenomenon of the plate material and to maintain a desired shape, rapid cooling may be performed while applying pressure in a closed state. When forming and cooling a heated blank (100), the average cooling rate can be at least 10°C / s or more to the martensite end temperature. Preferably, the cooling can be at least 20°C / s or more.

[0137] The blank (100) may be held within the press mold (400) for 3 to 20 seconds. For example, the engagement state of the press mold (400) may be held for 3 to 20 seconds. If the holding time within the press mold (400) is less than 3 seconds, sufficient cooling of the blank (100) may not occur, resulting in thermal deformation due to residual heat and temperature deviations between sections, which may deteriorate dimensional quality. On the other hand, if the holding time within the press mold (400) exceeds 20 seconds, the holding time within the press mold (400) may become longer, which may deteriorate productivity.

[0138] In one embodiment, hot forming of the blank (100) and cooling of the blank (100) can be performed with the press mold (400) in a closed state (or in an interlocked state), and hot piercing of the blank (100) can be performed after a certain period of time.

[0139] In one embodiment, hot forming, hot piercing, and cooling of the heated blank (100) can be performed simultaneously within the press die (400). For example, hot forming, hot piercing, and cooling of the blank (100) can be performed simultaneously (or together) with the press die (400) in a closed (or interlocked) state.

[0140] Although not shown, a trimming step may be performed after the forming / piercing step (S400). The trimming step may be a step of cutting an outer portion of the formed hot stamping part (10) using at least two piercing portions (110a, 110b) formed on the formed hot stamping part (10). In other words, the trimming step may be a step of cutting an outer portion of the hot stamping part (10) using two piercing portions (110a, 110b) formed on the hot stamping part (10) through hot piercing.

[0141] In one embodiment, in the trimming step, the edge of the hot stamping part (10) can be cut using at least two piercing portions (110a, 110b) formed through hot piercing as reference points (or, guide patterns). In other words, the hot stamping part (10) can be secured to a tool using at least two piercing portions (110a, 110b) formed on the molded hot stamping part (10), and the edge of the hot stamping part (10) can be cut. For example, after inserting a fixing pin into each of the at least two piercing portions (110a, 110b) formed on the hot stamping part (10), the outer portion of the hot stamping part (10) can be cut.

[0142] In one embodiment, the trimming step may be performed using a laser or a press die (e.g., a cold press die).

[0143] A method for manufacturing a hot stamping part according to one embodiment of the present invention may include forming a piercing portion (110) in a blank (100) through hot piercing, and then additionally cutting the outer portion of the hot stamping part (10) through cold trimming or laser trimming. That is, a method for manufacturing a hot stamping part according to one embodiment of the present invention may perform a hot piercing process on a blank (100), cool the blank (100), and then perform cold trimming or laser trimming.

[0144] In one embodiment, a second piercing step may be performed after the forming / piercing step (S400). The second piercing step may be a step of forming an additional piercing portion in the hot stamping part (10) using at least two piercing portions (110a, 110b) formed in the hot stamping part (10). In other words, the second piercing step may be a step of forming an additional piercing portion (e.g., an additional piercing portion) in the hot stamping part (10) using two piercing portions (110a, 110b) formed in the hot stamping part (10) through hot piercing.

[0145] In one embodiment, the second piercing step may be performed during the trimming step. For example, the second piercing step and the trimming step may be performed simultaneously. Alternatively, the second piercing step may be performed before or after the trimming step. For example, the second piercing step and the trimming step may be performed sequentially.

[0146] A method for manufacturing a hot stamping part according to one embodiment of the present invention can form a piercing portion (110) in a hot stamping part (10) through hot piercing, and then additionally form a piercing portion (e.g., an additional piercing portion) in the hot stamping part (10) through cold piercing or laser piercing. That is, a method for manufacturing a hot stamping part according to one embodiment of the present invention can perform a hot piercing process on a blank (100), cool the blank (100) on which the hot piercing process has been performed, and then perform a cold piercing process or a laser piercing process.

[0147] In one embodiment, a portion of the perimeter of the manufactured hot stamped part may be an edge of the coil raw material. That is, a portion of the perimeter of the manufactured hot stamped part may be an edge of the coil raw material without being cut.

[0148] In one embodiment, after the trimming step and / or the second piercing step are performed, a step of removing burrs formed in the blank may be performed. This may remove burrs formed during processes such as hot piercing, cold piercing, or cold trimming.

[0149] Experimental example

[0150] Hereinafter, the present invention will be described in more detail through experimental examples. However, the following experimental examples are intended to further illustrate the present invention, and the scope of the present invention is not limited by the following experimental examples. The following experimental examples may be appropriately modified or altered by those skilled in the art within the scope of the present invention.

[0151] Composition (wt%) CSiMnPSCrBTi0.220.31.50.020.0150.250.00250.05

[0152] Blank thickness (mm) Clearance (%) Blank temperature at piercing (℃) th1 / th2 w1 / w2 Hydrogen brittle fracture result Example 1 1.25 6000.228 0.058 Non-broken Example 2 1.25 4000.23 10.054 Non-broken Example 3 1.25 2000.225 0.043 Non-broken Example 4 1.21 0 6000.27 30.153 Non-broken Example 5 1.21 0 4000.25 5 0.123 Non-broken Example 6 1.21 0 200 0.2180.125 Unbroken Example 71.2156000.2310.196 Unbroken Example 81.2154000.2630.125 Unbroken Example 91.2152000.2860.073 Unbroken Example 102127000.3290.078 Unbroken Example 112124000.4480.171 Unbroken

[0153] Blank thickness (mm) Clearance (%) Piercing blank temperature (℃) th1 / th2 w1 / w2 Hydrogen brittleness evaluation result comparison example 11.25 190 0.26 40.6 12 Fracture comparison example 21.25 100 0.65 20.59 1 Fracture comparison example 31.25 Room temperature 0.77 01.3 15 Fracture comparison example 41.210 190 0.49 40.7 18 Fracture comparison example 51.210 100 0.65 70.85 6 Fracture comparison example 61.210 Room temperature 0.78 42.7 52 Breakage Comparison Example 71.215 100 0.72 6 0.332 Breakage Comparison Example 81.215 Room Temperature 0.72 4 0.733 Breakage Comparison Example 924 190 0.30 14.365 Breakage Comparison Example 1024 Room Temperature 0.80 0 3.250 Breakage Comparison Example 112 12 190 0.69 4 2.249 Breakage Comparison Example 122 12 Room Temperature 0.77 8 2.695 Breakage

[0154] Examples 1 to 11 and Comparative Examples 1 to 12 are specimens manufactured from blanks having a composition as shown in Table 1 under the conditions of slab reheating temperature (SRT): 1,230°C, finish rolling temperature (FDT): 900°C, reduction ratio during hot rolling: 95%, coiling temperature (CT): 700°C, annealing heat treatment temperature: 780°C, and plating immersion temperature: 660°C, which were heated at 950°C for 270 seconds and then hot formed, hot pierced, and cooled in a press mold. In Tables 2 and 3, th1 is the thickness of the fracture surface (303), th2 is the thickness of the sheared surface (300), w1 is the width of the plating layer peeling surface (304), and w2 is the width of the rollover surface (301). In Tables 2 and 3, the values ​​(th1 / th2) of Equation 1 and the values ​​(w1 / w2) of Equation 2 may be averages of values ​​measured at at least four points at equal angles from the center of the piercing portion (110). In addition, in Table 3, room temperature may mean 30°C.

[0155] Hydrogen embrittlement evaluation was performed on the hot stamping parts (e.g., specimens) of Examples 1 to 11 and Comparative Examples 1 to 12 through a 4-point bending test according to the ASTM G39-99 standard. The 4-point bending test is a test method that reproduces the condition of exposing the specimen to a corrosive environment, applies a stress below the elastic limit to a specific point of the manufactured specimen, and checks whether stress corrosion cracking occurs. Here, stress corrosion cracking refers to cracking that occurs when corrosion and continuous tensile stress are applied simultaneously. Specifically, the hydrogen embrittlement evaluation results in Tables 2 and 3 are the results of checking whether fracture occurred by applying a stress of 1,000 MPa in air for 100 hours to each specimen.

[0156] Referring to Table 2, when the value of the thickness (th1) of the fracture surface (303) / the thickness (th2) of the shear-processed surface (300) is 0.6 or less, and at the same time, the value of the width (w1) of the plating layer peeling surface (304) / the width (w2) of the roll-over surface (301) is 0.6 or less, it can be confirmed that fracture does not occur during the hydrogen embrittlement evaluation. That is, when the thickness (th1) of the fracture surface (303) and the thickness (th2) of the shear-processed surface (300) satisfy Equation 1 (th1 / th2 ≤ 0.6), and the width (w1) of the plating layer peeling surface (304) and the width (w2) of the roll-over surface (301) satisfy Equation 2 (w1 / w2 ≤ 0.6), it can be confirmed that fracture does not occur during the hydrogen embrittlement evaluation.

[0157] However, referring to Table 3, if the value of the thickness (th1) of the fracture surface (303) / the thickness (th2) of the shear-processed surface (300) exceeds 0.6, or the value of the width (w1) of the plating layer peeling surface (304) / the width (w2) of the roll-over surface (301) exceeds 0.6, it can be confirmed that fracture occurred during the hydrogen embrittlement evaluation. That is, if the thickness (th1) of the fracture surface (303) and the thickness (th2) of the shear-processed surface (300) do not satisfy Equation 1 (th1 / th2 ≤ 0.6), or the width (w1) of the plating layer peeling surface (304) and the width (w2) of the roll-over surface (301) do not satisfy Equation 2 (w1 / w2 ≤ 0.6), it can be confirmed that fracture does not occur during the hydrogen embrittlement evaluation.

[0158] Therefore, when the value of the thickness (th1) of the fracture surface (303) / the thickness (th2) of the shear-processed surface (300) of the hot stamping part (10) is 0.6 or less, and the value of the width (w1) of the plating layer peeling surface (304) / the width (w2) of the roll-over surface (301) is 0.6 or less, it can be confirmed that the hydrogen embrittlement resistance is excellent because no fracture occurs during the hydrogen embrittlement evaluation. That is, when the thickness (th1) of the fracture surface (303) and the thickness (th2) of the shear-processed surface (300) satisfy Equation 1 (th1 / th2 ≤ 0.6), and the width (w1) of the plating layer peeling surface (304) and the width (w2) of the roll-over surface (301) satisfy Equation 2 (w1 / w2 ≤ 0.6), it can be confirmed that the hydrogen embrittlement resistance is excellent because no fracture occurs during the hydrogen embrittlement evaluation.

[0159] While the present invention has been described with reference to the embodiments illustrated in the drawings, these are merely exemplary, and those skilled in the art will appreciate that various modifications and equivalent alternative embodiments are possible. Therefore, the true scope of technical protection of the present invention should be determined by the technical spirit of the appended claims.

Claims

1. As a hot stamping part with a piercing part formed, Mother material; a mutual diffusion layer disposed on the above-mentioned parent material; and A plating layer disposed on the above mutual diffusion layer; Including, The above hot stamping part includes a shearing surface formed on the edge of the piercing portion, The above shear processing surface includes a rollover surface, a shear surface, and a fracture surface, A hot stamping part, wherein the thickness (th1) of the above fracture surface and the thickness (th2) of the above shear processing surface satisfy the following equation 1. <Formula 1> th1 / th2 ≤ 0.6 2. In paragraph 1, A hot stamping part, wherein the rollover surface, the shear surface, and the fracture surface are sequentially provided in the thickness direction of the hot stamping part.

3. In paragraph 1, A hot stamping part, wherein the thickness of the above sheared surface is the sum of the thickness of the fractured surface, the thickness of the sheared surface, and the thickness of the rollover surface.

4. In paragraph 1, A hot stamping part, wherein the thickness of the above fracture surface is the shortest distance in the thickness direction of the hot stamping part from the starting point of the above fracture surface to the ending point of the above fracture surface.

5. In paragraph 1, A hot stamping part, wherein the thickness of the above sheared surface is the shortest distance in the thickness direction of the hot stamping part from the starting point of the rollover surface to the end point of the fracture surface.

6. In paragraph 1, A hot stamping part, wherein the hot stamping part further includes a plating layer peel-off surface in which at least a portion of the upper surface of the intermixing layer is exposed.

7. In paragraph 6, A hot stamping part in which the width (w1) of the above plating layer peeling surface and the width (w2) of the above rollover surface satisfy the following equation 2. <Formula 2> w1 / w2 ≤ 0.6 8. In paragraph 1, A hot stamping part having at least two of the above piercing parts.