AI Technical Summary
The hot stamping process faces challenges in achieving high-quality shear surfaces and efficient processing due to increased processing time with laser equipment and deteriorated quality with press molds, particularly in determining optimal hot piercing timing considering material thickness and forming start temperature.
Deriving the maximum delay time for hot piercing using a mathematical equation that considers the thickness of the blank, forming start temperature, and other environmental and press mold-related factors, allowing for flexible process design and improved quality control.
This approach enables flexible process design and enhances the quality control of hot stamping parts by optimizing the hot piercing timing, reducing hydrogen embrittlement and ensuring uniform shear surface quality.
Smart Images

Figure PI2025003950_DRAWING_001 
Figure PI2025003950_DRAWING_002 
Figure PI2025003950_DRAWING_003
Abstract
Description
Method for manufacturing hot stamping parts
[0001] The present invention relates to a method for manufacturing a hot stamping part.
[0002] As environmental and fuel efficiency regulations tighten globally, the need for lighter vehicle materials is increasing. Consequently, research and development on ultra-high-strength steel and hot-stamping steel is actively underway.
[0003] Hot stamping is a process for manufacturing high-strength parts by heating steel plates to high temperatures in a furnace, then forming and rapidly cooling them within a press. Additionally, a piercing process may be performed to cut and machine holes within the high-strength parts.
[0004] The piercing process uses laser equipment or press molds, but when laser equipment is used, processing time may increase, and when press molds are used, the cross-sectional quality may deteriorate.
[0005] As a technology related to this, there is Korean Patent Publication No. 10-2020-0080721 (Title of invention: Hot stamping part manufacturing device and hot stamping part manufacturing method using the same).
[0006] Embodiments of the present invention are characterized by deriving a maximum hot piercing delay time considering blank thickness, forming start temperature, etc.
[0007] One embodiment of the present invention comprises a heating step of heating a blank; a transfer step of transferring the heated blank to a press mold including a punch; and a forming and piercing step of hot-forming the transferred blank into a shape of a hot stamping part and hot-piercing the transferred blank to form a piercing portion in the hot stamping part; wherein a hot piercing delay time in the forming and piercing step is λ 0 seconds or more from the time when the press mold reaches the bottom dead point. max Below, the above λ maxA method for manufacturing a hot stamping part is provided, which is derived by the following mathematical formula.
[0008] <Mathematical formula>
[0009]
[0010] (In the above mathematical formula, λ max is the maximum delay time for hot piercing (s), α p is a correction factor considering the forming start temperature and hot piercing environment, T is the forming start temperature (℃), b p is a correction factor considering the pressing force of the press mold, c p is a correction factor that takes into account the thickness sensitivity of the material, and t is the thickness of the material (mm).
[0011] In this embodiment, α in the above mathematical formula p has a value greater than 0 and less than or equal to 0.001, and b p has a value greater than about 0 and less than or equal to 0.65, and c p can have a value of about 1 or more and about 1.2 or less.
[0012] In the present embodiment, in the step of transporting the blank, the heated blank can be air-cooled at room temperature.
[0013] In the present embodiment, the step of heating the blank may include a multi-stage heating step of heating the blank step by step; and a crack heating step of heating the blank to a temperature of Ac3 to 1000°C.
[0014] In the present embodiment, the step of heating the blank is performed in a heating furnace, and the heating furnace may have a plurality of sections having different temperature ranges.
[0015] In the present embodiment, the blank can be cooled within the press mold during the forming and piercing steps.
[0016] In this embodiment, at least two piercing portions may be formed.
[0017] Other aspects, features and advantages other than those described above will become apparent from the following detailed description, claims and drawings for carrying out the invention.
[0018] According to one embodiment of the present invention, as described above, by deriving the maximum hot piercing delay time considering the blank thickness, forming start temperature, etc., flexible process design is possible and quality control of manufactured hot stamping parts is facilitated. Of course, the scope of the present invention is not limited by these effects.
[0019] FIG. 1 is a perspective view schematically illustrating a hot stamping part according to one embodiment of the present invention.
[0020] FIG. 2 is a flowchart schematically illustrating a method for manufacturing a hot stamping part according to one embodiment of the present invention.
[0021] FIG. 3 is a flowchart schematically illustrating a preparation step of a method for manufacturing a hot stamping part according to one embodiment of the present invention.
[0022] Figure 4 is a plan view schematically illustrating a blank according to one embodiment of the present invention.
[0023] FIG. 5 is a flowchart schematically illustrating a heating step of a method for manufacturing a hot stamping part according to one embodiment of the present invention.
[0024] FIG. 6 is a drawing illustrating a heating furnace having a plurality of sections in a heating step of a method for manufacturing a hot stamping part according to one embodiment of the present invention.
[0025] FIGS. 7 and 8 are cross-sectional views illustrating a forming / piercing step of a manufacturing process of a hot stamping part according to one embodiment of the present invention.
[0026] Figure 9 is a diagram illustrating a process window derived according to the thickness of the material, the forming start temperature, and the hot piercing delay time.
[0027] The present invention is capable of various modifications and embodiments. Specific embodiments are illustrated in the drawings and described in detail in the detailed description. The effects and features of the present invention, as well as the methods for achieving them, will become clearer with reference to the embodiments described in detail below, along with the drawings. However, the present invention is not limited to the embodiments disclosed below and can be implemented in various forms.
[0028] In the examples below, the terms first, second, etc. are not used in a limiting sense, but are used for the purpose of distinguishing one component from another.
[0029] In the examples below, singular expressions include plural expressions unless the context clearly indicates otherwise.
[0030] In the following examples, terms such as “include” or “have” mean that a feature or component described in the specification is present, and do not preclude the possibility that one or more other features or components may be added.
[0031] For convenience of explanation, the sizes of components in the drawings may be exaggerated or reduced. For example, the sizes and thicknesses of each component shown in the drawings are arbitrarily shown for convenience of explanation, and the present invention is not necessarily limited to what is shown.
[0032] In some embodiments, where implementations are otherwise feasible, specific process sequences may be performed in a different order than described. For example, two processes described in succession may be performed substantially simultaneously, or in a reverse order from the described order.
[0033] In this specification, “A and / or B” refers to the case where it is A, or B, or both A and B. And, “at least one of A and B” refers to the case where it is A, or B, or both A and B.
[0034] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings. When describing with reference to the drawings, identical or corresponding components are given the same drawing reference numerals, and redundant descriptions thereof will be omitted.
[0035] FIG. 1 is a perspective view schematically illustrating a hot stamping part according to one embodiment of the present invention.
[0036] Referring to FIG. 1, a hot stamping part (10) according to one embodiment of the present invention may include a piercing portion (110). In one embodiment, the hot stamping part (10) may include two piercing portions (110). The piercing portions (110) may include a first piercing portion (110a) and a second piercing portion (110b). However, the present invention is not limited thereto. The hot stamping part (10) may include one piercing portion (110) or three or more piercing portions (110).
[0037] Although not shown, the hot stamping part (10) may include an additional piercing part in addition to the piercing part (110). In this case, the piercing part (110) may be formed through hot piercing, and the additional piercing part may be formed through cold piercing or laser piercing. The hot stamping part (10) may be provided with one or more additional piercing parts.
[0038] In one embodiment, an additional piercing portion may be formed using the piercing portion (110). This will be described in more detail below.
[0039] Additionally, although not shown, the hot stamping part (10) may include an edge portion. In this case, the edge portion of the hot stamping part (10) may mean a surface extending along the long side of the hot stamping part (10).
[0040] FIG. 2 is a flowchart schematically illustrating a method for manufacturing a hot stamping part according to one embodiment of the present invention.
[0041] Referring to FIG. 2, a method for manufacturing a hot stamping part according to one embodiment may include a preparation step (S100), a heating step (S200), a transfer step (S300), and a forming / piercing step (S400).
[0042] FIG. 3 is a flowchart schematically illustrating a preparation step of a method for manufacturing a hot stamping part according to one embodiment of the present invention, and FIG. 4 is a plan view schematically illustrating a blank according to one embodiment of the present invention.
[0043] Referring to FIGS. 3 and 4, the preparation step (S100) may be a step of preparing a blank (100) for hot stamping. In one embodiment, the preparation step (S100) may include a hot rolling step (S110), a cooling / coiling step (S120), a cold rolling step (S130), an annealing step (S140), a plating step (S150), and a cutting step (S160).
[0044] First, a reheating step of the steel slab may be performed. In the reheating step of the steel slab, the steel slab obtained through the continuous casting process is reheated to a predetermined temperature, so that the components segregated during casting can be re-dissolved. In one embodiment, the slab reheating temperature (SRT) may be about 1,200°C to about 1,400°C. If the slab reheating temperature (SRT) is lower than about 1,200°C, the components segregated during casting may not be sufficiently re-dissolved, making it difficult to significantly see the homogenization effect of the alloy elements and the solid solution effect of titanium (Ti). A higher slab reheating temperature (SRT) is advantageous for homogenization, but if the slab reheating temperature (SRT) exceeds about 1,400°C, the austenite grain size increases, making it difficult to secure strength, and the manufacturing cost of the steel plate may increase due to the excessive heating process.
[0045] In the hot rolling step (S110), the reheated plate may be hot rolled at a predetermined finishing rolling temperature. A hot-rolled steel plate may be manufactured through the hot rolling step (S110). In one embodiment, the finishing rolling temperature (Finishing Delivery Temperature: FDT) may be about 880°C to about 950°C. At this time, if the finishing rolling temperature (FDT) is lower than about 880°C, it is difficult to secure the workability of the steel plate due to the occurrence of a mixed grain structure caused by abnormal region rolling, and not only may the workability be reduced due to microstructural non-uniformity, but also a problem of sheet passing during hot rolling may occur due to a rapid phase change. If the finishing rolling temperature (FDT) exceeds about 950°C, the austenite grains may become coarser, and the TiC precipitates may become coarser, which may deteriorate the performance of the hot stamping part.
[0046] In the cooling / coiling step (S120), the hot-rolled hot-rolled steel sheet may be cooled to a predetermined coiling temperature (Coiling Temperature, CT) and coiled. In one embodiment, the coiling temperature of the cooling / coiling step (S120) may be about 550°C to about 800°C. The coiling temperature affects the redistribution of carbon, and when the coiling temperature is lower than about 550°C, the low-temperature phase fraction due to overcooling may increase, which may increase the strength, and there is a concern that the rolling load may be intensified during cold rolling, and the ductility may rapidly decrease. Conversely, when the coiling temperature exceeds about 800°C, abnormal crystal grain growth or excessive crystal grain growth may cause formability deterioration and strength deterioration.
[0047] In the cold rolling step (S130), the coiled hot-rolled steel sheet may be uncoiled, pickled, and then cold rolled. The pickling process may be performed to remove scale from the coiled hot-rolled steel sheet, i.e., the hot-rolled coil manufactured through the hot rolling process. Through the cold rolling step (S130), a cold-rolled steel sheet may be manufactured.
[0048] The annealing step (S140) may anneal the cold-rolled cold-rolled steel sheet at a temperature of about 700°C or higher. For example, the annealing step (S140) may include heating the cold-rolled cold-rolled steel sheet and cooling the heated cold-rolled steel sheet at a predetermined cooling rate. The cold-rolled steel sheet may be annealed in the annealing step (S140). The annealing step (S140) may be performed in an annealing furnace.
[0049] In one embodiment, the annealing temperature of the cold-rolled steel sheet may be between about 750°C and about 900°C. If the annealing temperature of the cold-rolled steel sheet is lower than about 750°C, the desired structure may not be obtained, and recrystallization may not be sufficiently completed. On the other hand, if the annealing temperature of the cold-rolled steel sheet exceeds about 900°C, the annealing temperature may be too high, reducing the efficiency of the manufacturing process. Therefore, if the annealing temperature of the cold-rolled steel sheet satisfies the range of about 750°C to about 900°C, the desired structure may be obtained, recrystallization may be sufficiently completed, and the efficiency of the manufacturing process may be improved.
[0050] The plating step (S150) may be a step of forming a plating layer on an annealed cold-rolled steel sheet. In one embodiment, a plating layer may be formed on the annealed cold-rolled steel sheet through the plating step (S150). At this time, the plating layer may include a zinc (Zn)-based plating layer or an aluminum (Al)-based plating layer.
[0051] Specifically, in the plating step (S150), the annealed cold-rolled steel sheet can be immersed in a plating bath. At this time, the plating bath can maintain a temperature of about 400°C to about 700°C. The plating amount is about 40 g / m on both sides of the base material of the cold-rolled steel sheet. 2 About 200 g / m 2 It can be done. After the plating step (S150), the cold rolled steel sheet with the plating layer formed can be wound into a coil shape.
[0052] Although Fig. 3 illustrates that a cold rolling step (S130), an annealing step (S140), and a plating step (S150) are performed after the cooling / coiling step (S120), the present invention is not limited thereto. At least one of the cold rolling step (S130), the annealing step (S140), and the plating step (S150) may be omitted. For example, the cold rolling step (S130) and the annealing step (S140) may be omitted. In this case, the hot-rolled steel sheet on which a plating layer is formed after the plating step (S150) may be coiled into a coil shape.
[0053] Thereafter, in the cutting step (S160), a steel plate (e.g., a cold-rolled steel plate or a hot-rolled steel plate) wound in a coil shape is uncoiled, and then the steel plate can be cut into a blank (100) using a laser or a cold press mold. At this time, the blank (100) may include an outer portion (or edge) of the coil. For example, the blank (100) may include an outer portion (or edge) of the steel plate.
[0054] Referring to FIG. 2, after the preparation step (S100) of preparing a blank (100), a heating step (S200) of heating the blank (100) may be performed. The heat source method in the heating step (S200) may be direct heating or indirect heating. The heat source method in the heating step (S200) may use either direct heating or indirect heating, or a combination of direct heating and indirect heating.
[0055] In one embodiment, in the heating step (S200), the blank (100) may be heated within a heating furnace. The heating furnace may be provided with one section having one temperature range (or, a single temperature), or may be provided with multiple sections having different temperature ranges. When the heating furnace is provided with one section having one temperature range, the blank (100) may be heated within the heating furnace to a target temperature within one temperature range. At this time, the target temperature may be Ac3 to about 1,000°C. That is, the blank (100) may be heated within a heating furnace having a temperature range of Ac3 to about 1,000°C until the temperature of the blank (100) reaches Ac3 to about 1,000°C.
[0056] On the other hand, if the furnace is equipped with multiple sections having different temperature ranges, the blank (100) within the furnace can be heated to the target temperature in different temperature ranges.
[0057] FIG. 5 is a flowchart schematically illustrating a heating step of a method for manufacturing a hot stamping part according to one embodiment of the present invention, and FIG. 6 is a drawing illustrating a heating furnace having a plurality of sections in the heating step of a method for manufacturing a hot stamping part according to one embodiment of the present invention.
[0058] Referring to FIGS. 5 and 6, in the heating step (S200), the blank (100, see FIG. 4) may be heated in a heating furnace having multiple sections having different temperature ranges. As illustrated in FIG. 5, the heating step (S200) may include a multi-stage heating step (S210) and a soaking heating step (S220). The multi-stage heating step (S210) and the soaking heating step (S220) may be steps in which the blank (100) is heated while passing through multiple sections provided in the heating furnace.
[0059] In one embodiment, the overall temperature of the furnace may be about 680°C to about 1,000°C. Specifically, the overall temperature of the furnace in which the multi-stage heating step (S210) and the soaking heating step (S220) are performed may be about 680°C to about 1,000°C. At this time, the temperature of the furnace in which the multi-stage heating step (S210) is performed may be about 680°C to about Ac3, and the temperature of the furnace in which the soaking heating step (S220) is performed may be about Ac3 to about 1,000°C.
[0060] In the multi-stage heating step (S210), the blank (100) may be heated (or heated) in stages while passing through multiple sections provided in the heating furnace. There may be multiple sections among the multiple sections provided in the heating furnace in which the multi-stage heating step (S210) is performed, and the temperature is set for each section so that the temperature increases from the inlet of the heating furnace into which the blank (100) is introduced toward the outlet of the heating furnace from which the blank (100) is taken out, so that the blank (100) may be heated (or heated) in stages.
[0061] After the multi-stage heating step (S210), a soaking heating step (S220) may be performed. In the soaking heating step (S220), the multi-stage heated blank may be heated (or soaked heated) while passing through a section of a heating furnace set to a temperature of about Ac3 to about 1,000°C. Among the multiple sections provided in the heating furnace, at least one section may be used for the soaking heating step (S220).
[0062] According to one embodiment, a heating furnace may have a plurality of sections having different temperature ranges. Specifically, the heating furnace may have a first section (P1) having a first temperature range (T1), a second section (P2) having a second temperature range (T2), a third section (P3) having a third temperature range (T3), a fourth section (P4) having a fourth temperature range (T4), a fifth section (P5) having a fifth temperature range (T5), a sixth section (P6) having a sixth temperature range (T6), and a seventh section (P7) having a seventh temperature range (T7).
[0063] In one embodiment, in the multi-stage heating step (S210), the blank may be heated stepwise while passing through the first section (P1) to the fourth section (P4) defined within the heating furnace. Additionally, in the crack heating step (S220), the blank that has been multi-stage heated in the first section (P1) to the fourth section (P4) may be crack heated while passing through the fifth section (P5) to the seventh section (P7).
[0064] The first section (P1) to the seventh section (P7) may be arranged sequentially within the furnace. The first section (P1) having the first temperature range (T1) may be adjacent to the inlet of the furnace into which the blank is fed, and the seventh section (P7) having the seventh temperature range (T7) may be adjacent to the outlet of the furnace from which the blank is taken out. Accordingly, the first section (P1) having the first temperature range (T1) may be the first section of the furnace, and the seventh section (P7) having the seventh temperature range (T7) may be the last section of the furnace.
[0065] The temperatures of the plurality of sections provided in the furnace, for example, the temperatures of the first section (P1) to the seventh section (P7), may increase from the inlet of the furnace into which the blank is fed to the outlet of the furnace from which the blank is taken out. However, the temperatures of the fifth section (P5), the sixth section (P6), and the seventh section (P7) may be the same. In addition, the temperature difference between two adjacent sections among the plurality of sections provided in the furnace may be greater than 0°C and less than or equal to 100°C. For example, the temperature difference between the first section (P1) and the second section (P2) may be greater than 0°C and less than or equal to 100°C.
[0066] The furnace temperature of the soaking heating step (S220) may be Ac3 to about 1,000°C. If the furnace temperature of the soaking heating step (S220) is less than Ac3, the manufactured hot stamping part may not have the desired material. On the other hand, if the furnace temperature of the soaking heating step (S220) exceeds about 1,000°C, carbide-forming elements or nitride-forming elements such as Ti, V, Nb, and Mo in the blank (100) are dissolved into the parent material, making it difficult to suppress grain coarsening.
[0067] Although FIG. 6 illustrates a heating furnace according to one embodiment as having seven sections with different temperature ranges, the present invention is not limited thereto. The heating furnace may also have five, six, or eight sections with different temperature ranges.
[0068] In one embodiment, the heating step (S200) is provided with a multi-stage heating step (S210) and a crack heating step (S220), so that the temperature of the heating furnace can be set in stages, thereby improving the energy efficiency of the heating furnace.
[0069] In one embodiment, the furnace may have a length of about 20 m to about 40 m along the transport path of the blank (100). The furnace may have a plurality of sections having different temperature ranges, and a ratio of the length of a section in which the blank is multi-heated among the plurality of sections to the length of a section in which the blank is crack-heated among the plurality of sections may satisfy about 1:1 to about 4:1. If the length of the section in which the blank is crack-heated within the furnace increases so that the ratio of the length of the section in which the blank is multi-heated to the length of the section in which the blank is crack-heated exceeds about 1:1, the amount of hydrogen penetrating into the blank in the crack-heating section may increase, which may increase delayed fracture. On the other hand, if the length of the section in which the blank is crack-heated decreases so that the ratio of the length of the section in which the blank is multi-heated to the length of the section in which the blank is crack-heated is less than about 4:1, the crack-heating section (or time) may not be sufficiently secured, which may result in uneven strength of the manufactured hot stamped part. For example, the length of a uniform heating section among the plurality of sections provided in the furnace may be about 20% to about 50% of the total length of the furnace.
[0070] In one embodiment, the total heating time for which the heating step (S200) is performed may be about 2 min to about 20 min. That is, the total time for which the blank remains in the heating furnace may be about 2 min to about 20 min. If the total heating time for which the heating step (S200) is performed is about 2 min or less, the heating time may be insufficient, and the manufactured hot stamping part may not have a desired material. On the other hand, if the total heating time for which the heating step (S200) is performed is about 20 min or more, the heating time may be too long, which may lower the production speed and reduce economic efficiency. Therefore, if the total heating time for which the heating step (S200) is performed satisfies about 2 min to about 20 min, the manufactured hot stamping part may have a desired material, and at the same time, the reduction in economic efficiency of the manufacturing process may be prevented or minimized.
[0071] Referring to FIG. 2, a transfer step (S300) may be performed after the heating step (S200). In the transfer step (S300), the heated blank (100) may be transferred to a press mold (400, see FIG. 7). For example, the heated blank (100) may be taken out from the heating furnace and then transferred to the press mold (400).
[0072] In the transport step (S300), the heated blank (100) may be cooled to ambient temperature (or room temperature). That is, the heated blank (100) may be air-cooled at ambient temperature during transport. If the heated blank (100) is not air-cooled, the mold entry temperature (e.g., molding start temperature) may increase, causing wrinkles (or bends) to occur on the surface of the manufactured hot stamping part. In addition, since the use of a refrigerant may affect the subsequent process (hot stamping), it may be desirable for the heated blank (100) to be air-cooled during transport.
[0073] FIGS. 7 and 8 are cross-sectional views illustrating a forming / piercing step in a manufacturing process of a hot stamping part according to one embodiment of the present invention. Specifically, FIG. 7 is a cross-sectional view of a blank and a press mold before the forming / piercing step is performed, and FIG. 8 is a cross-sectional view of a blank and a press mold during the forming / piercing step.
[0074] Referring to FIGS. 2, 7, and 8, a forming / piercing step (S400) may be performed after the transfer step (S300). The forming / piercing step (S400) may be a step of hot-forming the transferred blank (100) into the shape of a hot stamping part and forming a piercing portion (110) in the transferred blank (100) through hot piercing.
[0075] In one embodiment, the forming / piercing step (S400) may be performed in a press mold (400). The press mold (400) may include a lower mold (410), an upper mold (420), and a punch (430). The lower mold (410) may have a bottom surface shape of a hot stamping part. The upper mold (420) faces the lower mold (410) and may have a top surface shape of a hot stamping part. The upper mold (420) may be raised and lowered between a top dead center and a bottom dead center. At this time, the top dead center may refer to a position at which the upper mold (420) moves to the highest position, and the bottom dead center may refer to a lowest point at which the upper mold (420) moves toward the lower mold (410) to form the blank (100). Although not shown, the upper mold (420) may be raised and lowered between the top dead center and the bottom dead center using a separately provided hydraulic cylinder. However, the present invention is not limited thereto.
[0076] The press mold (400) may be equipped with at least one punch (430), preferably at least two punches (430). In one embodiment, the punches (430) may include a first punch and a second punch. However, the present invention is not limited thereto. For example, the press mold (400) may be equipped with only one punch (430), or may be equipped with three or more punches (430), and various modifications are possible.
[0077] Although not shown, when the press mold (400) is equipped with only one punch (430), a foam bead may be formed at the edge of the blank (100) during molding of the blank (100).
[0078] For example, as will be described later, a laser process or a cold piercing process may be performed using the piercing portion (110) formed through hot piercing. Specifically, the piercing portions (110) formed through hot piercing may be used as guide patterns (or reference points) to secure the blank (100) to a tool, and then subsequent processes may be performed. Accordingly, the number of piercing portions (110) formed on the blank (100) through hot piercing may be at least two.
[0079] In one embodiment, the clearance between the punch (430) and the mold (e.g., the lower mold (410) and / or the upper mold (420)) may be from about 2% to about 30%. If the clearance is less than about 2%, the punch (430) may become stuck in the mold due to thermal expansion of the mold. On the other hand, if the clearance is greater than about 30%, there is a risk that the punch (430) may fluctuate significantly, resulting in uneven quality of the cross-section. For example, the uniformity of the cross-section quality may deteriorate, such as when many short-circuit lines are formed only in a portion of the cross-section. Accordingly, when the clearance between the punch (430) and the mold (e.g., the lower mold (410) and / or the upper mold (420)) is about 2% to about 30%, the punch (430) can be prevented from being caught in the mold due to thermal expansion, and the short-circuit lines formed around the shear surface can be uniformly formed.
[0080] In one embodiment, the blank (100) may be hot formed (or hot pressed) in the forming / piercing step (S400). The conveyed (or heated) blank (100) may be hot formed into the shape of a hot stamping part using a press mold (400) including a lower mold (410) and an upper mold (420). Specifically, the blank (100) may be formed into the shape of a hot stamping part by pressing (e.g., hot pressing) the lower mold (410) having the shape of the bottom surface of the hot stamping part with the upper mold (420) having the shape of the top surface of the hot stamping part. For example, the press mold may reach the bottom dead center, and at the bottom dead center, the blank (100) may be formed into the shape of the hot stamping part (10). Specifically, the upper mold (420) can be lowered to reach the bottom dead point, and after reaching the bottom dead point, the blank (100) can be formed into the shape of a hot stamping part (10) at the bottom dead point.
[0081] In one embodiment, the forming start temperature of the blank (100) during hot forming in the forming / piercing step (S400) may be equal to or higher than the Ms temperature. Specifically, the forming start temperature is the temperature at which forming of the blank (100) is initiated, and the forming start temperature of the blank (100) during hot forming in the forming / piercing step (S400) may be equal to or higher than the Ms temperature and equal to or lower than the heating furnace ejection temperature of the blank (100). If the blank (100) is hot formed below the Ms temperature, a large load may be generated during hot forming, which may cause damage to the press die (400), the formability of the blank (100) may deteriorate, and the manufactured hot stamping part may not have the targeted structure and properties. On the other hand, since the blank (100) is air-cooled during the process of being taken out of the heating furnace and transferred to the press mold (400), the temperature of the blank (100) when hot forming is performed cannot but be lower than the temperature at which the blank (100) is taken out of the heating furnace. Therefore, when the forming start temperature is about Ms or higher and lower than the temperature at which the blank (100) is taken out of the heating furnace, the formability of the blank can be improved, and the manufactured hot stamping part can have the targeted structure and properties.
[0082] In one embodiment, in the forming / piercing step (S400), hot piercing may be performed on the blank (100) after the hot forming of the blank (100) is completed. Specifically, after the hot forming of the blank (100) is completed, the punch (430) included in the press die (400) may be lowered to perform hot piercing on the blank (100) to form a piercing portion (110) on the hot stamping part (10) (or blank (100)). For example, after the upper die (420) reaches the bottom dead center and the hot forming of the blank (100) is completed, the punch (430) may be lowered to perform hot piercing on the blank (100) to form a piercing portion (110) on the hot stamping part (10) (or blank (100)). That is, hot piercing can be performed after the press die (or upper die) reaches the bottom dead center. Although not shown, the punch (430) can be raised and lowered using a hydraulic cylinder. However, the present invention is not limited thereto.
[0083] In one embodiment, after hot forming of the blank (100) is completed using the press mold (400), the first punch and the second punch included in the press mold (400) may be lowered to form at least two piercing portions (110a, 110b) in the blank (100). Specifically, after hot forming of the blank (100) is completed by pressing the lower mold (410) and the blank (100) with the upper mold (420), the first punch and the second punch may be lowered to form the first piercing portion (110a) and the second piercing portion (110b) in the hot stamping part (10).
[0084] In one embodiment, hot piercing may be performed after hot forming has occurred.
[0085] Although FIGS. 7 and 8 illustrate that a punch (430) included in a press mold (400) is lowered to form a piercing portion (110) in a blank (100), the present invention is not limited thereto. Although not illustrated, a piercing portion (110) may also be formed in a blank (100) through a separately provided external device.
[0086] In one embodiment, the temperature of the blank (100) when hot piercing is performed in the forming / piercing step (S400) may be higher than the Mf temperature. If the temperature of the blank (100) when hot piercing is performed is lower than the Mf temperature, hot piercing may be performed at too low a temperature, which may cause phase transformation in the blank (or hot stamping part) and increase shear stress. In addition, this may result in poor shear quality and hydrogen embrittlement. In addition, a large load may be generated during hot piercing, which may cause damage to the press die (400) and / or the punch (430).
[0087] In one embodiment, the blank (100) may be cooled while being formed into the final part shape in the press mold (400) (or during hot forming). The press mold (400) may be provided with cooling channels (440) through which a coolant circulates therein. For example, the interiors of the lower mold (410) and the upper mold (420) may each have cooling channels (440). Specifically, the cooling channels (440) may be arranged within the lower mold (410) and the upper mold (420) along the surface of the lower mold (410) and the surface of the upper mold (420). The blank (100), which has been heated by the circulation of the coolant supplied through the cooling channels (440) provided in the press mold (400), may be rapidly cooled. At this time, in order to prevent a spring back phenomenon of the plate material and to maintain a desired shape, the rapid cooling may be performed while applying pressure in a closed state. When forming and cooling a heated blank (100), the average cooling rate can be at least 10°C / s or more to the martensite end temperature. Preferably, the cooling can be at least 20°C / s or more.
[0088] The blank (100) may be held in the press mold (400) for 3 to 20 seconds. For example, the engagement state of the press mold (400) may be held for 3 to 20 seconds. If the holding time in the press mold (400) is less than 3 seconds, sufficient cooling of the blank (100) may not occur, resulting in thermal deformation due to residual heat and temperature deviations between sections, which may deteriorate the dimensional quality. On the other hand, if the holding time in the press mold (400) exceeds 20 seconds, the holding time in the press mold (400) may become longer, which may deteriorate productivity.
[0089] In one embodiment, the hot forming, hot piercing, and cooling processes of the heated blank (100) may be performed within the press die (400). For example, the hot forming of the blank (100) and the cooling of the blank (100) may be performed from the time when the forming of the blank (100) is initiated, and the hot piercing of the blank (100) may be performed thereafter. That is, the hot forming of the blank (100) and the cooling of the blank (100) may be performed while the press die (400) is closed (or engaged), and the hot piercing of the blank (100) may be performed after a certain period of time has elapsed. However, the present invention is not limited thereto.
[0090] As described above, hot piercing may be a process of punching out a blank (100) during a cooling process of a heated, high-temperature blank (100). Hot piercing may be applied between the time when the press die (or upper die) reaches the bottom dead point and the time when cooling (or rapid cooling) of the blank (100) is completed. In other words, hot piercing may be applied between the time when hot forming is completed and the time when cooling (or rapid cooling) of the blank (100) is completed.
[0091] When hot piercing is performed on the blank (100) while the blank (100) is being cooled (or rapidly cooled), the quality of the hot stamping part manufactured may be affected depending on the temperature of the blank (100), so it is necessary to control the timing of performing the hot piercing. For example, if the temperature of the blank (100) is too low during hot piercing, the shear surface quality and shear load may be inferior, and thus hydrogen embrittlement may occur. In addition, since the cooling behavior of the blank (100) differs depending on the thickness of the blank (100), even when hot piercing is performed after the same amount of time has passed since the press die (400) has reached the bottom dead center, the shear surface quality and dimensions may differ for each hot stamping part (10). Therefore, it may be difficult to secure the shear surface quality and dimensions under the target conditions.
[0092] In addition, since the temperature behavior (or cooling behavior) of the blank (100) is different depending on the thickness of the blank (or material) and the forming start temperature, it is necessary to control the hot piercing time differentially for each blank by taking this into consideration.
[0093] Therefore, it is necessary to control the hot piercing timing in the forming / piercing step (S400). However, to control the hot piercing timing in the forming / piercing step (S400), various variables must be considered, such as the forming start temperature and material thickness, as well as the hot piercing environment, the press mold pressure, and the material thickness sensitivity. In this case, the material may refer to a blank.
[0094] Accordingly, the inventors of the present invention, through repeated experiments, have derived a mathematical formula that can easily control the hot piercing timing in the forming / piercing step (S400). In one embodiment, the maximum hot piercing delay time in the forming / piercing step (S400) can satisfy the following mathematical formula.
[0095] <Mathematical formula>
[0096]
[0097] λ in mathematical formula max is the maximum delay time for hot piercing (s), α p is a correction factor considering the forming start temperature and hot piercing environment, T is the forming start temperature (℃), b p is a correction factor considering the pressing force of the press mold, c p is a correction factor that takes into account the thickness sensitivity of the material, and t is the thickness of the material (mm). In this case, the material can mean a blank, and the unit of the maximum delay time at the hot piercing point, s, can mean seconds.
[0098] First, the cooling behavior of a material (e.g., a blank) may vary depending on the forming initiation temperature of the blank and the hot piercing environment. Specifically, the cooling behavior of a material may vary depending on the forming initiation temperature, the temperature of the atmosphere in which hot piercing is performed, the design structure of the material placement in the press die, the layout of the press die, etc. α p is a correction factor that takes into account the forming start temperature and hot piercing environment, and can have a value greater than about 0 and less than 0.001. In this case, α p can have units of s / (℃ x mm).
[0099] Depending on the pressure applied by the press die to the material, heat transfer (or amount of heat transfer) from the material to the press die may vary. For example, if the press die presses the material with a large pressure, heat transfer from the material to the press die may increase. Therefore, the cooling behavior of the material may vary depending on the pressure applied by the press die to the material. b p is a correction factor that takes into account the pressing force of the press mold, b p can have a value greater than about 0 and less than or equal to 0.65. In this case, b p can have units of s / mm.
[0100] Additionally, the thermal conductivity (or amount of heat transfer) transmitted within the material may vary depending on the thickness of the material. c p c is a correction factor that takes into account the difference in thermal conductivity (or heat transfer amount) depending on the thickness of the material. p can have a value of about 1 or more and about 1.2 or less.
[0101] The forming initiation temperature (T) is the temperature at which the forming of the material begins, and may be higher than the Ms temperature. Specifically, the forming initiation temperature (T) is the temperature at which the forming of the material begins, and may be higher than the Ms temperature and lower than the ejection temperature of the material after heating. In addition, the material thickness (t) may be about 1 mm or more and about 2.3 mm or less.
[0102] In one embodiment, the maximum delay time of hot piercing in the forming / piercing step (S400) can be derived by the mathematical formula described above. Therefore, the delay time of hot piercing in the forming / piercing step (S400) is λ 0 seconds or more from the time when the bottom dead center of the press mold (or upper mold) is reached. max It may be as follows. At this time, the hot piercing delay time may be the time between the time when the press mold (or upper mold) reaches the bottom dead center and the time when hot piercing is performed on the blank (100).
[0103] In other words, the hot piercing delay time in the forming / piercing step (S400) is λ 0 seconds or more from the time when the upper mold reaches the bottom dead center and forming is completed. maxIt may be below. If the hot piercing time in the forming / piercing step (S400) is 0 seconds, it may mean that the hot piercing is performed simultaneously as soon as the hot forming is completed. In other words, the hot piercing delay time in the forming / piercing step (S400) is 0 seconds, it may mean that the hot piercing is performed immediately as soon as the hot forming is completed. If the hot piercing is performed before the hot forming, the dimensional quality of the piercing portion (110) formed by the hot piercing may be inferior. In addition, if the hot piercing delay time in the forming / piercing step (S400) is λ from the time when the bottom dead point of the press mold is reached, max If exceeded, hot piercing may occur at too low a temperature, which may complete the phase transformation in the blank (or hot stamped part), resulting in increased shear stress. This may also result in poor shear quality and hydrogen embrittlement.
[0104] Therefore, the hot piercing delay time in the forming / piercing step (S400) is λ more than 0 seconds from the time the press die reaches the bottom dead center. max If the following is satisfied, the quality of the cross-section of the piercing portion (110) formed through hot piercing can be uniformly managed. For example, the hot piercing delay time in the forming / piercing step (S400) is λ 0 seconds or more from the time of reaching the bottom dead center of the press mold. max When the following is satisfied, the hydrogen embrittlement resistance of the manufactured hot stamping part can be improved, and the dimensional quality of the manufactured hot stamping part can be maintained uniformly.
[0105] In one embodiment, the hot piercing delay time in the forming / piercing step (S400) is λ 0 seconds or more from the time the press die reaches the bottom dead center. max If the following is satisfied, the amount of activated hydrogen in the manufactured hot stamping part may be 0.5 ppm or less.
[0106] Figure 9 is a diagram illustrating a process window derived from the thickness of the material, the forming start temperature, and the maximum hot piercing delay time. In this case, in Figure 9, the material refers to a blank, and Ta refers to the heating furnace extraction temperature of the blank (100).
[0107] Referring to FIGS. 2 and 9, a method for manufacturing a hot stamping part may include a preparation step (S100), a heating step (S200), a transfer step (S300), and a forming / piercing step (S400). In addition, as described above, the maximum delay time (λ) of hot piercing considering the thickness of the material and the forming start temperature is calculated through a mathematical formula. max ) can be derived, and the hot piercing delay time during hot piercing of the material is 0 seconds or more λ max It could be as follows:
[0108] Therefore, a process window can be derived using forming start temperature, material thickness, and hot piercing delay time as parameters. At this time, in the process window, the forming number temperature can be higher than the Ms temperature and lower than the Ta (blank ejection temperature) temperature, the material thickness can be higher than or equal to about 1.0 mm and lower than or equal to about 2.3 mm, and the hot piercing delay time can be higher than or equal to 0 seconds λ. max It could be as follows:
[0109] In one embodiment, by deriving a parameter window (or process window) for hot piercing in the forming / piercing step (S400) using the thickness of the material, the forming start temperature, and the hot piercing delay time, flexible process design can be enabled, the quality of the manufactured hot stamping part can be improved, and the quality control of the manufactured hot stamping part can be made easier.
[0110] Although not shown, a trimming step may be performed after the forming / piercing step (S400). The trimming step may be a step of cutting an outer portion of a formed hot stamping part (10) using at least two piercing portions (110a, 110b) formed on the hot stamping part (10). In other words, the trimming step may be a step of cutting an outer portion of a hot stamping part (10) using two piercing portions (110a, 110b) formed on the hot stamping part (10) through hot piercing.
[0111] In one embodiment, in the trimming step, the edge of the hot stamping part (10) can be cut using at least two piercing portions (110a, 110b) formed through hot piercing as reference points (or, guide patterns). In other words, the hot stamping part (10) can be secured to a tool using at least two piercing portions (110a, 110b) formed on the molded hot stamping part (10), and the edge of the hot stamping part (10) can be cut. For example, after inserting a fixing pin into each of the at least two piercing portions (110a, 110b) formed on the hot stamping part (10), the outer portion of the hot stamping part (10) can be cut.
[0112] In one embodiment, the trimming step may be performed using a laser or a press die (e.g., a cold press die).
[0113] A method for manufacturing a hot stamping part according to one embodiment of the present invention may include forming a piercing portion (110) in a blank (100) through hot piercing, and then additionally cutting the outer portion of the hot stamping part (10) through cold trimming or laser trimming. That is, a method for manufacturing a hot stamping part according to one embodiment of the present invention may perform a hot piercing process on a blank (100), cool the blank (100), and then perform cold trimming or laser trimming.
[0114] In one embodiment, a second piercing step may be performed after the forming / piercing step (S400). The second piercing step may be a step of forming an additional piercing portion in the hot stamping part (10) using at least two piercing portions (110a, 110b) formed in the hot stamping part (10). In other words, the second piercing step may be a step of forming an additional piercing portion (e.g., an additional piercing portion) in the hot stamping part (10) using two piercing portions (110a, 110b) formed in the hot stamping part (10) through hot piercing.
[0115] In one embodiment, the second piercing step may be performed during the trimming step. For example, the second piercing step and the trimming step may be performed simultaneously. Alternatively, the second piercing step may be performed before or after the trimming step. For example, the second piercing step and the trimming step may be performed sequentially.
[0116] A method for manufacturing a hot stamping part according to one embodiment of the present invention can form a piercing portion (110) in a hot stamping part (10) through hot piercing, and then additionally form a piercing portion (e.g., an additional piercing portion) in the hot stamping part (10) through cold piercing or laser piercing. That is, a method for manufacturing a hot stamping part according to one embodiment of the present invention can perform a hot piercing process on a blank (100), cool the blank (100) on which the hot piercing process has been performed, and then perform a cold piercing process or a laser piercing process.
[0117] In one embodiment, a portion of the perimeter of the manufactured hot stamped part may be an edge of the coil raw material. That is, a portion of the perimeter of the manufactured hot stamped part may be an edge of the coil raw material without being cut.
[0118] In one embodiment, after the trimming step and / or the second piercing step are performed, a step of removing burrs formed in the blank may be performed. This may remove burrs formed during processes such as hot piercing, cold piercing, and cold trimming.
[0119] Experimental example
[0120] Hereinafter, the present invention will be described in more detail through experimental examples. However, the following experimental examples are intended to further illustrate the present invention, and the scope of the present invention is not limited by the following experimental examples. The following experimental examples may be appropriately modified or altered by those skilled in the art within the scope of the present invention.
[0121] Composition (wt%) CSiMnPSCrBTi0.220.31.50.020.0150.250.00250.05
[0122] Material thickness (t, mm) Molding start temperature (T, ℃)λ max (s)Hot piercing delay time (s)Activation hydrogen amount (ppm)Example 11.26931.671.60.429Example 21.26661.641.50.431Example 31.26591.631.60.415Comparative example 11.26931.671.70.719Comparative example 21.26661.641.70.721Comparative example 31.26591.631.80.704
[0123] Examples 1 to 3 and Comparative Examples 1 to 3 are specimens in which blanks having the same composition as in Table 1 were heated in a heating furnace with a maximum temperature of 950°C for 360 seconds, and then hot-formed, cooled, and hot-pierced according to the conditions in Table 2. At this time, a multi-stage heating furnace was used, which is configured to include a plurality of heating zones in which the temperature is gradually increased from the inlet of the heating furnace into which the blank (e.g., a plated steel sheet) is fed toward the outlet of the heating furnace from which the blank is taken out.
[0124] Also, in Table 2, the maximum delay time for hot piercing (λ max) in the mathematical formula for deriving a p , b p , c p are 0.001, 0.65, and 1.2, respectively.
[0125] Hydrogen embrittlement was evaluated using TDS (Thermal Desorption Spectroscopy) equipment for the specimens of Examples 1 to 3 and Comparative Examples 1 to 3 manufactured according to the conditions of Tables 1 and 2. Specifically, for the specimens of Examples 1 to 3 and Comparative Examples 1 to 3 manufactured according to the conditions of Tables 1 and 2, the amount of hydrogen released from the specimens of Examples 1 to 3 and Comparative Examples 1 to 3 was measured at 350°C or lower while the temperature was increased from room temperature to 500°C at a heating rate of 20°C / min.
[0126] Referring to Table 2, the maximum hot piercing delay time (λ) is 0 seconds or more. max ) If the following is satisfied, it can be confirmed that the amount of activated hydrogen in the manufactured hot stamping part is 0.5 ppm or less.
[0127] On the other hand, in the case of Comparative Examples 1 to 3, the material thickness and the molding start temperature satisfy the range of the present invention, but the hot piercing delay time is the maximum hot piercing delay time (λ max ) is exceeded, it can be confirmed that the amount of activated hydrogen in the manufactured hot stamping part exceeds 0.5 ppm.
[0128] Therefore, the hot piercing delay time in the forming / piercing step (S400) is λ more than 0 seconds from the time the press die reaches the bottom dead center. max If the following is satisfied, the amount of activated hydrogen in the manufactured hot stamping part may be 0.5 ppm or less.
[0129] While the present invention has been described with reference to the embodiments illustrated in the drawings, these are merely exemplary, and those skilled in the art will appreciate that various modifications and equivalent alternative embodiments are possible. Therefore, the true scope of technical protection of the present invention should be determined by the technical spirit of the appended claims.
Claims
1. Heating step for heating the blank; A transfer step of transferring the heated blank to a press mold including a punch; and A forming and piercing step of hot forming the transferred blank into the shape of a hot stamping part and hot piercing the transferred blank to form a piercing portion in the hot stamping part; Including, The hot piercing delay time in the above forming and piercing step is λ 0 seconds or more from the time the lower dead point of the press mold is reached. max Below, Above λ max A method for manufacturing a hot stamping part, the method being derived by the following mathematical formula. <Mathematical formula> (In the above mathematical formula, λ max is the maximum delay time for hot piercing (s), α p is a correction factor considering the forming start temperature and hot piercing environment, T is the forming start temperature (℃), b p is a correction factor considering the pressing force of the press mold, c p is a correction factor that takes into account the thickness sensitivity of the material, and t is the thickness of the material (mm).
2. In paragraph 1, In the above mathematical formula, α p has a value greater than 0 and less than or equal to 0.001, and b p has a value greater than about 0 and less than or equal to 0.65, and c p A method for manufacturing a hot stamping part, wherein the value is about 1 or more and about 1.2 or less.
3. In paragraph 1, In the step of transferring the above blank, A method for manufacturing a hot stamping part, wherein the heated blank is cooled to room temperature.
4. In paragraph 1, The step of heating the above blank is: A multi-stage heating step for heating the blank step by step; and A crack heating step of heating the blank to a temperature of Ac3 to 1000°C; A method for manufacturing a hot stamping part, comprising:
5. In paragraph 1, The step of heating the above blank is performed in a heating furnace, A method for manufacturing a hot stamping part, wherein the above heating furnace has a plurality of sections having different temperature ranges.
6. In paragraph 1, A method for manufacturing a hot stamping part, wherein the blank is cooled within the press mold in the above forming and piercing steps.
7. In paragraph 6, A method for manufacturing a hot stamping part, wherein at least two of the above piercing parts are formed.