Chloroprene-based polymer , chloroprene-based polymer latex, and dip-molded article

MYPI2025004024A0Undetermined Publication Date: 2024-07-31DENKA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025004024
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-01-31
Filing Date
2024-01-24
Publication Date
2024-07-31

AI Technical Summary

Technical Problem

Conventional chloroprene-based polymers fail to produce dip-molded products with sufficient tensile strength and flexibility, especially when cut, and these products lose flexibility over long-term storage.

Method used

A chloroprene-based polymer containing 12 to 30% 2,3-dichloro-1,3-butadiene monomer units, with a toluene insoluble content of 60 to 87%, and a specific ratio of abietic acid and its salts, which is molded using a dip coagulation method and heat-treated to achieve low-temperature hardness change ΔH1 of 29 or less, maintaining flexibility after storage.

Benefits of technology

The resulting dip-molded products exhibit excellent tensile strength and flexibility at cutting, and retain flexibility even after long-term storage, suitable for applications like industrial gloves, medical gloves, balloons, and catheters.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a chloroprene-based polymer capable of yielding a dip-molded article that has sufficient tensile strength at break and flexibility, and that can maintain flexibility even after long-term storage. According to the present invention, there is provided a chloroprene-based polymer comprising a chloroprene monomer unit and a 2,3-dichloro-1,3-butadiene monomer unit, wherein the chloroprene-based polymer contains 12 to 30% by mass of the 2,3-dichloro-1,3-butadiene monomer unit with respect to 100% by mass of a total of the chloroprene monomer unit and the 2,3-dichloro-1,3-butadiene monomer unit, the chloroprene-based polymer has a toluene-insoluble content of 60 to 87% by mass, a low-temperature hardness change ΔH1 of a test dip-molded article is 29 or less, wherein the test dip-molded article is obtained by molding a test chloroprene-based polymer latex composition comprising the chloroprene-based polymer by a dip coagulation method and heat-drying a molded body resulting therefrom at 130°C for 30 minutes; the low-temperature hardness change ΔH1 is represented by HB1-HA1; HA1 represents a Shore hardness measured at 23°C using the durometer type A after heat-treating the test dip-molded article at 70°C for 30 minutes and then stacking the test dip-molded article to a thickness of 6.00 ± 0.20 mm, and HB1 represents a Shore hardness measured at -10°C using the durometer type A after heat-treating the test dip-molded article at 70°C for 30 minutes, further storing the test dip-molded article at -10°C for 168 hours, and then stacking the test dip-molded article to a thickness of 6.00 ± 0.20 mm, and a ratio RB / RA is 0.10 or more and 0.70 or less, wherein the ratio RB / RA is a ratio of a total peak area RB of abietic acid, neoabietic acid, palustric acid, levopimaric acid, and salts thereof to a total peak area RA of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid, and salts thereof, obtained from a gas chromatography analysis of an extract extracted from the test dip-molded article with an ethanol and toluene azeotropic mixture specified in JIS K 6229.
Need to check novelty before this filing date? Find Prior Art

Description

Chloroprene polymers, chloroprene polymer latexes and dip-molded products

[0001] The present invention relates to a chloroprene polymer, a chloroprene polymer latex, and a dip-molded product.

[0002] Chloroprene polymers are known as materials for dip-molded products such as medical surgical gloves, medical examination gloves, industrial gloves, balloons, catheters, and rubber boots.

[0003] Various techniques have been proposed for chloroprene polymer latexes for dip-molded products and dip-molded articles of chloroprene polymers. Patent Document 1 describes a polychloroprene latex with a pH of 7 to 14 that contains 100 parts by mass of modified polychloroprene obtained by copolymerizing chloroprene and methacrylic acid, 90 to 150 parts by mass of water, 1 to 5 parts by mass of an emulsifier, and 0.5 to 2.5 parts by mass of potassium ions, for use in dip-molded products. Patent Document 2, relating to applications for dip-molded products, describes a mercaptan-modified polychloroprene latex obtained by copolymerizing chloroprene and 2,3-dichloro-1,3-butadiene, in which the peak areas (A) at 126.2 to 127.6 ppm, (B) at 122.0 to 126.2 ppm, and (C) at 129.9 to 130.3 ppm in the C-solid-state NMR spectrum of the polychloroprene are within the ranges represented by the following general formula (I): Patent Document 3, relating to applications for dip-molded products, describes a chloroprene polymer latex that contains high-molecular-weight and low-molecular-weight components, thereby achieving both excellent flexibility and mechanical properties in the vulcanized rubber produced by dip molding. Patent Document 4, relating to applications for dip-molded products, describes a chloroprene polymer latex that exhibits excellent flexibility and mechanical properties even under mild vulcanization conditions, obtained by copolymerizing a chloroprene monomer with an isoprene monomer, which is a raw material for isoprene rubber. Patent Document 5 describes a dip-molded product of an isoprene / chloroprene polymer that exhibits excellent flexibility without containing a diphenylguanidine vulcanization accelerator by mixing an isoprene polymer latex with a chloroprene polymer latex. Patent Document 6 describes a dip-molded product that exhibits excellent mechanical properties by mixing a nitrile-butadiene polymer (NBR) latex or an isoprene polymer latex with a chloroprene polymer latex.

[0004]

[0005] Japanese Patent Application Laid-Open No. 2014-114342 International Publication No. 2019 / 009038 Japanese Patent Application Laid-Open No. 2019-143002 International Publication No. 2021-132460 Special Publication No. 2017-508840 Japanese Patent Application Laid-Open No. 2020-189963

[0006] However, with conventional chloroprene polymers, it has not been possible to obtain a dip-molded product that has sufficient tensile strength at break and flexibility and that can maintain its flexibility even after long-term storage.

[0007] The present invention has been made in view of the above circumstances, and provides a chloroprene polymer from which a dip-molded product can be obtained which has sufficient tensile strength at break and flexibility and which can maintain its flexibility even after long-term storage.

[0008] According to the present invention, there is provided a chloroprene polymer containing chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units, wherein the chloroprene polymer contains 12 to 30 mass% of 2,3-dichloro-1,3-butadiene monomer units relative to 100 mass% in total of the chloroprene monomer units and the 2,3-dichloro-1,3-butadiene monomer units, the chloroprene polymer has a toluene-insoluble content of 60 to 87 mass%, a test chloroprene polymer latex composition containing the chloroprene polymer is molded by a dip coagulation method and then heated and dried at 130°C for 30 minutes, and the low-temperature hardness change ΔH1 of a test dip molded product is 29 or less, and the low-temperature hardness change ΔH1 is represented by HB1-HA1, HA1 represents the Shore hardness measured by stacking the test dip-molded products to a thickness of 6.00±0.20 mm using a durometer type A in an environment of 23°C after heat-treating the test dip-molded products at 70°C for 30 minutes and then storing the test dip-molded products at -10°C for 168 hours, and then stacking the test dip-molded products to a thickness of 6.00±0.20 mm using a durometer type A in an environment of -10°C. HB1 represents the Shore hardness measured by stacking the test dip-molded products to a thickness of 6.00±0.20 mm using a durometer type A in an environment of -10°C after heat-treating the test dip-molded products at 70°C for 30 minutes and then storing the test dip-molded products at -10°C for 168 hours. The present invention provides a chloroprene-based polymer, in which the ratio RB / RA, of the total amount RB of the peak areas of abietic acid, neoabietic acid, palustric acid, levopimaric acid and their salts to the total amount RA of the peak areas of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid and their salts, obtained by gas chromatography analysis of an extract extracted with an ethanol / toluene azeotropic mixture specified in JP 6229, is 0.10 or more and 0.70 or less.

[0009] The present inventors have conducted extensive studies and have found that, by adjusting the content of 2,3-dichloro-1,3-butadiene monomer units, the toluene-insoluble content, the change in low-temperature hardness of a test dip-molded product obtained from the chloroprene polymer, and the ratio RB / RA of the total amount RB of the peak areas of abietic acid, neoabietic acid, palustric acid, levopimaric acid, and salts thereof to the total amount RA of the peak areas of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid, and salts thereof, within specific numerical ranges, a chloroprene polymer can be obtained that has sufficient tensile strength at break and flexibility and from which dip-molded products that can maintain their flexibility even after long-term storage can be obtained, thereby completing the present invention.

[0010] Various embodiments of the present invention will be exemplified below. The embodiments shown below can be combined with each other. [1] A chloroprene polymer containing chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units, wherein the chloroprene polymer contains 12 to 30 mass% of 2,3-dichloro-1,3-butadiene monomer units relative to 100 mass% in total of the chloroprene monomer units and the 2,3-dichloro-1,3-butadiene monomer units, and the chloroprene polymer has a toluene-insoluble content of 60 to 87 mass%, and the low-temperature hardness change ΔH of a test dip-molded product obtained by molding a test chloroprene polymer latex composition containing the chloroprene polymer by a dip coagulation method and heating and drying it at 130°C for 30 minutes is The low-temperature hardness change ΔH1 is expressed as HB1-HA1, and HA1 represents the Shore hardness obtained by stacking the test dip-molded products to a thickness of 6.00±0.20 mm after heat treatment at 70°C for 30 minutes and measuring the Shore hardness using a durometer type A in an environment at 23°C. HB1 represents the Shore hardness obtained by stacking the test dip-molded products to a thickness of 6.00±0.20 mm after heat treatment at 70°C for 30 minutes and storing the test dip-molded products at -10°C for 168 hours and measuring the Shore hardness using a durometer type A in an environment at -10°C. A chloroprene polymer having a ratio RB / RA of 0.10 or more and 0.70 or less of the total amount RB of peak areas of abietic acid, neoabietic acid, palustric acid, levopimaric acid, and their salts to the total amount RA of peak areas of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid, and their salts, as obtained by gas chromatography analysis of an extract extracted with an ethanol / toluene azeotropic mixture as defined in JIS K 6229. [2] The chloroprene polymer according to [1], wherein in a 13C-solid state NMR spectrum of the chloroprene polymer, the peak area from 126.2 to 127.6 ppm is PA, the peak area from 122.0 to 126.2 ppm is PB, and the peak area from 129.9 to 130.3 ppm is PC, the following formula (1) is satisfied:Formula (1): 4.4≦PA / (PB−PC)×100≦5.0 [3] A chloroprene polymer latex comprising the chloroprene polymer according to [1] or 2 and water. [4] A dip-molded product of a chloroprene polymer latex composition comprising the chloroprene polymer latex according to [3]. [5] The dip-molded product according to [4], which is an industrial glove, a glove for general household use, a medical glove, a balloon, a catheter, or a boot. [6] A dip-molded product according to [4] or [5], wherein the low-temperature hardness change ΔH2 is 29 or less, and the low-temperature hardness change ΔH2 is expressed as HB2-HA2, where HA2 represents the Shore hardness measured in an environment of 23°C after heat-treating the dip-molded product under conditions of 70°C and 30 minutes, stacking the dip-molded products to a thickness of 6.00±0.20 mm, and using a durometer type A; and HB2 represents the Shore hardness measured in an environment of -10°C after heat-treating the dip-molded product under conditions of 70°C and 30 minutes, storing the dip-molded product at -10°C for 168 hours, stacking the dip-molded products to a thickness of 6.00±0.20 mm, and using a durometer type A. [7] A dip-molded product of a chloroprene polymer latex composition containing a chloroprene polymer, wherein the dip-molded product has a low-temperature hardness change ΔH2 of 29 or less, and the low-temperature hardness change ΔH2 is expressed as HB2-HA2, where HA2 represents a Shore hardness obtained by stacking the dip-molded products to a thickness of 6.00±0.20 mm using a durometer type A under an environment of 23°C after heat-treating the dip-molded product under conditions of 70°C and 30 minutes, and further storing the dip-molded product at -10°C for 168 hours, and then stacking the dip-molded products to a thickness of 6.00±0.20 mm using a durometer type A under an environment of -10°C, and the dip-molded product has a Shore hardness measured according to JIS K The dip-molded product has a tensile strength at break of 20.0 MPa or more and a modulus at 500% elongation of 2.00 MPa or less, as measured in accordance with JIS No. 6251.

[0011] The chloroprene polymer of the present invention can provide a dip-molded product that has sufficient tensile strength at break and flexibility and can maintain its flexibility even after long-term storage. Specifically, it can provide a dip-molded product that has excellent tensile strength at break, a sufficiently low modulus at 500% elongation, and a sufficiently low modulus at 500% elongation after 6 months of storage at 23°C. Furthermore, the obtained dip-molded product can be used to its full potential as various components that require excellent tensile strength at break, flexibility, and flexibility after long-term storage. Specifically, it can be used as industrial gloves, general household gloves, medical gloves, balloons, catheters, or boots.

[0012] The present invention will be described in detail below by illustrating embodiments of the present invention. The present invention is not limited by these descriptions. The features of the embodiments of the present invention described below can be combined with each other. Furthermore, each feature can be an invention independently.

[0013] 1. Chloroprene-Based Polymer The chloroprene-based polymer according to the present invention refers to a polymer containing monomer units derived from 2-chloro-1,3-butadiene (hereinafter also referred to as chloroprene). The chloroprene-based polymer according to the present invention contains chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units. The chloroprene-based polymer according to one embodiment of the present invention may contain chloroprene monomer units, 2,3-dichloro-1,3-butadiene monomer units, and other monomer units copolymerizable therewith. Examples of such other monomers include 1-chloro-1,3-butadiene, isoprene, styrene, methacrylic acid, acrylonitrile, and sulfur. The other monomer may include one or more of these.

[0014] The chloroprene polymer according to the present invention contains 12 to 30 mass% of 2,3-dichloro-1,3-butadiene monomer units, preferably 14 to 27 mass%, based on 100 mass% of the total of chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units. The content of 2,3-dichloro-1,3-butadiene monomer units is, for example, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or 30 mass%, and may be within a range between any two of the values ​​exemplified here. By controlling the content of 2,3-dichloro-1,3-butadiene monomer units within the above range, a dip-molded article obtained from the chloroprene polymer exhibits excellent flexibility and maintains its flexibility even after long-term storage.

[0015] A chloroprene polymer according to one embodiment of the present invention may contain 0 to 30% by mass of other monomer units other than chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units, based on 100% by mass of the chloroprene polymer. The content of the other monomer units may be, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or 30, or may be within a range between any two of the values ​​exemplified here. A chloroprene polymer according to one embodiment of the present invention may also be composed of chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units.

[0016] When the chloroprene polymer is a mixture of two or more different chloroprene polymers, the content of each monomer unit means the total amount of each monomer unit in all chloroprene polymers contained in the chloroprene polymer latex composition.

[0017] The content of 2,3-dichloro-1,3-butadiene monomer units in a chloroprene polymer can be calculated by measuring a test piece of the chloroprene polymer obtained by freeze-drying a latex containing the chloroprene polymer by pyrolysis gas chromatography, determining the area ratio of the peak derived from chloroprene to the peak derived from 2,3-dichloro-1,3-butadiene, and using a calibration curve of the 2,3-dichloro-1,3-butadiene content. Specifically, the content can be calculated by the method described in the Examples.

[0018] The content of 2,3-dichloro-1,3-butadiene monomer units in the chloroprene polymer can be controlled by adjusting the production conditions of the chloroprene polymer, for example, the types and amounts of raw materials blended.

[0019] The chloroprene polymer according to one embodiment of the present invention has a toluene-insoluble content of 60 to 87% by mass, preferably 75 to 87% by mass, and may be, for example, 60, 61, 62, 63, 64, 65, 66, 67, 68, 69, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, or 87% by mass, or may be within a range between any two of the values ​​exemplified here.

[0020] The toluene-insoluble content can be calculated by the following formula, specifically by the method described in the Examples: Toluene-insoluble content (gel content) = B / A × 100 (%), where Ag is the chloroprene-based polymer obtained by freeze-drying a latex containing a chloroprene-based polymer, the resulting chloroprene-based polymer is immersed in toluene for 16 hours, and the chloroprene-based polymer after freeze-drying is taken as Ag and Bg is the gel content (insoluble content) separated from the toluene-dissolved mixture.

[0021] The toluene-insoluble content can be controlled by adjusting the production conditions of the chloroprene polymer, specifically, the polymerization recipe, the type and amount of the chain transfer agent, the polymerization temperature, the polymerization time, the polymerization conversion rate, etc. By controlling the toluene-insoluble content within the above-mentioned range, the dip-molded product obtained from the chloroprene polymer will have excellent tensile strength at break and flexibility.

[0022] In a chloroprene rubber composition according to one embodiment of the present invention, when the peak area from 126.2 to 127.6 ppm is PA, the peak area from 122.0 to 126.2 ppm is PB, and the peak area from 129.9 to 130.3 ppm is PC in a 13C-solid state NMR spectrum, the formula (1) is satisfied: 4.4≦PA / (PB−PC)×100≦5.0.

[0023] The 13C solid-state NMR spectrum is used to analyze the microstructure of a polymer, and the molar ratios of the microstructures of a chloroprene-based polymer, including 1,4-trans bonds, 1,4-cis bonds, 1,2-bonds, isomerized 1,2-bonds, 3,4-bonds, and isomerized 3,4-bonds, correspond to the areas of the peaks in the 13C solid-state NMR spectrum. The peak at 126.2 to 127.6 ppm is thought to be a signal attributable to the carbon of the -CH= group in the 1,4-cis bond, a bonding unit between chloroprene monomers. Furthermore, the peaks at 122.0 to 126.2 ppm are mostly signals attributable to the carbon of -CH= in the 1,4-trans bond of the bonding unit between chloroprene monomer units, but are also thought to include signals (123.6 to 123.9 ppm) attributable to the carbon of -CH= in the chloroprene monomer unit and the 2,3-dichloro-1,3-butadiene monomer unit. The peaks at 129.9 to 130.3 ppm are thought to be signals attributable to the carbon of -CCl= in the chloroprene monomer unit and the 2,3-dichloro-1,3-butadiene monomer unit. Therefore, by subtracting the peak area PC from 129.9 to 130.3 ppm from the peak area PB from 122.0 to 126.2 ppm, only the signal components attributable to the carbon of -CH= in the 1,4-trans bond of the bonding unit between chloroprene monomer units can be obtained. Therefore, the relationship PA / (PB-PC) represented by the peak area PA from 126.2 to 127.6 ppm, the peak area PB from 122.0 to 126.2 ppm, and the peak area PC from 129.9 to 130.3 ppm indicates the molar ratio of 1,4-cis bonds to 1,4-trans bonds.

[0024] The value of PA / (PB-PC)×100 is, for example, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, or 5.0, and may be within a range between any two of the values ​​exemplified here. The C-solid state NMR spectrum is measured on a chloroprene polymer obtained by freeze-drying a chloroprene polymer latex, and the measurement data is based on a signal at 135.0 ppm attributable to the carbon of the 1,4-trans bond -CCl=, which shows the maximum peak intensity in the C-solid state NMR spectrum. Specifically, the measurement can be performed using the method described in the Examples. Note that when the resolution of the C-solid state NMR spectrum is low, the measurement error of the peak area may be large. However, when the rise of the measured peak is higher than the baseline of the NMR spectrum chart, the measurement error of the peak area can be reduced by subtracting the area between the baseline and the rise of the peak from the measured peak area. The value of PA / (PB-PC)×100 can be controlled by adjusting the polymerization conditions for the chloroprene polymer, particularly the polymerization temperature.

[0025] By setting the value of PA / (PB-PC)×100 within the above range, the dip-molded article obtained from the chloroprene polymer will have a better tensile strength at break.

[0026] The chloroprene polymer according to the present invention is a dip-molded test product obtained by molding a test chloroprene polymer latex composition containing the chloroprene polymer by a dip coagulation method and then subjecting the resultant to a heat drying treatment at 130°C for 30 minutes, and the low-temperature hardness change ΔH1 of the dip-molded test product is 29 or less.

[0027] The low-temperature hardness change ΔH1 is, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, or 29, and may be within a range between any two of the values ​​exemplified here.

[0028] The low-temperature hardness change ΔH1 is expressed as HB1 - HA1. The low-temperature hardness change ΔH1 can be determined by storing a test dip-molded product at -10°C for 168 hours and subtracting the hardness before low-temperature storage from the hardness after low-temperature storage. Specifically, HA1 represents the Shore hardness measured using a durometer type A at 23°C after heat-treating the test dip-molded product at 70°C for 30 minutes (before storing it at -10°C for 168 hours), stacking the test dip-molded products to a thickness of 6.00 ± 0.20 mm. HB1 represents the Shore hardness measured using a durometer type A at -10°C after a test dip-molded specimen is heated at 70°C for 30 minutes (before storing it at -10°C for 168 hours) and then stored at -10°C for 168 hours, after which the test dip-molded specimens are stacked to a thickness of 6.00±0.20 mm. The low-temperature hardness change ΔH1 can be measured by the method described in the Examples. The heat treatment at 70°C for 30 minutes is intended to melt the crystalline structure contained in the test dip-molded specimen before storing it at -10°C for 168 hours, and it is believed that the crystalline structure is melted by performing the heat treatment at 70°C for 30 minutes. The low-temperature hardness change ΔH1 can be controlled by adjusting the production conditions of the chloroprene polymer.

[0029] By setting the low-temperature hardness change ΔH1 within the above range, the dip-molded article obtained from the chloroprene polymer will have excellent flexibility even after long-term storage.

[0030] The chloroprene polymer according to the present invention has a ratio RB / RA of 0.10 or more and 0.70 or less, where RB is the total peak area of ​​abietic acid, neoabietic acid, palustric acid, levopimaric acid, and their salts to RA is the total peak area of ​​dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid, and their salts, as determined by gas chromatography of an extract obtained from a dip-molded test specimen with an ethanol / toluene azeotropic mixture as specified in JIS K 6229. RB / RA is preferably 0.15 to 0.50. RB / RA may be, for example, 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, or 0.70, and may be within a range between any two of the values ​​exemplified herein.

[0031] RB / RA can be determined by extracting a test immersion molding with an ethanol / toluene azeotropic mixture (ETA solution) specified in JIS K 6229, treating the extract with hydrochloric acid, analyzing the resulting extract by gas chromatography, and calculating the ratio RB / RA ((conjugated resin acid component b) / (non-conjugated resin acid component a)) of the total amount RB of the peak areas of abietic acid, neoabietic acid, palustric acid, levopimaric acid, and their salts to the total amount RA of the peak areas of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid, and their salts. Specifically, it can be determined by the method described in the Examples.

[0032] The RB / RA can be controlled by adjusting the type and amount of an emulsifier (particularly a rosin acid and / or a rosin acid salt) used during emulsion polymerization of the polymer contained in the chloroprene polymer. By controlling the RB / RA within the above range, the dip-molded product obtained from the chloroprene polymer will have excellent tensile strength at break.

[0033] In the chloroprene polymer according to one embodiment of the present invention, a test dip-molded product prepared from the test chloroprene polymer latex composition preferably has a tensile strength at break of 20.0 MPa or more, more preferably 23.0 MPa or more, as measured in accordance with JIS K 6251. The tensile strength at break is, for example, 20.0, 21.0, 22.0, 23.0, 24.0, 25.0, 26.0, 27.0, 28.0, 29.0, 30.0, 31.0, 32.0, 33.0, 34.0, 35.0, 36.0, 37.0, 38.0, 39.0, or 40.0 MPa, and may be within a range between any two of the values ​​exemplified here.

[0034] In the chloroprene polymer according to one embodiment of the present invention, a modulus at 500% elongation measured in accordance with JIS K 6251 on a dip-molded test specimen prepared from the chloroprene polymer latex composition is preferably 2.00 MPa or less, more preferably 1.80 MPa or less, and may be, for example, 1.00, 1.10, 1.20, 1.30, 1.40, 1.50, 1.60, 1.70, 1.80, 1.90, or 2.00 MPa, or may be within a range between any two of the values ​​exemplified here.

[0035] In the chloroprene polymer according to one embodiment of the present invention, a test dip-molded product prepared from the test chloroprene polymer latex composition preferably has a modulus at 500% elongation of 2.50 MPa or less after storage at 23° C. for 6 months, as measured in accordance with JIS K 6251. The modulus at 500% elongation is, for example, 1.00, 1.10, 1.20, 1.30, 1.40, 1.50, 1.60, 1.70, 1.80, 1.90, 2.00, 2.10, 2.20, 2.30, 2.40, or 2.50 MPa, and may be within a range between any two of the values ​​exemplified here.

[0036] The tensile strength at break, the modulus at 500% elongation, and the modulus at 500% elongation measured according to JIS K 6251 after storage at 23°C for 6 months can be measured by the methods described in the examples.

[0037] The dip-molded test specimen can be obtained by molding a test chloroprene polymer latex composition having a solids concentration of 30% by mass, which is prepared so that the composition contains, relative to 100 parts by mass of the solids content of the chloroprene polymer, 2 parts by mass of zinc oxide, 2 parts by mass of a butylated reaction product of p-cresol and dicyclopentadiene, 0.1 parts by mass of a sodium salt of a β-naphthalenesulfonic acid-formalin condensate, and water, by a dip coagulation method, and then subjecting the composition to a heat-drying treatment at 130°C for 30 minutes.

[0038] 2. Method for Producing Chloroprene Polymer The method for producing a chloroprene polymer according to one embodiment of the present invention is not particularly limited. The method for producing a chloroprene polymer according to one embodiment of the present invention may include a polymerization step of polymerizing raw material monomers including chloroprene and 2,3-dichloro-1,3-butadiene to obtain a chloroprene polymer.

[0039] When producing a chloroprene polymer, raw material monomers are polymerized by a polymerization method such as emulsion polymerization, solution polymerization, suspension polymerization, or bulk polymerization. Among these polymerization methods, emulsion polymerization is preferred because it offers various advantages, such as ease of control, ease of polymer isolation from the polymerization-terminated liquid, and a relatively fast polymerization rate. A production method according to one embodiment of the present invention may include an emulsion polymerization step in which raw material monomers including chloroprene and 2,3-dichloro-1,3-butadiene are polymerized in the presence of an emulsifier to obtain a chloroprene polymer latex containing a chloroprene polymer. In the emulsion polymerization step, raw material monomers including chloroprene and 2,3-dichloro-1,3-butadiene are emulsion-polymerized using an emulsifier, a dispersant, a polymerization initiator, a chain transfer agent, a reducing agent, and the like, as appropriate. When a desired conversion rate is reached, a polymerization terminator is added to obtain a chloroprene polymer latex. Furthermore, unreacted monomers may be removed by a concentration method such as vacuum distillation.

[0040] (Raw Material Monomers) In the polymerization step, the monomers include chloroprene and 2,3-dichloro-1,3-butadiene, and may also include other monomers copolymerizable with chloroprene and 2,3-dichloro-1,3-butadiene. The other monomers are as described above as the monomer units that the chloroprene polymer may contain. The type and amount of each monomer charged are preferably adjusted so that the content of each monomer unit in the resulting chloroprene polymer falls within the above-described numerical range.

[0041] (Emulsifier) ​​The emulsifier preferably contains rosin acid and / or a rosin acid salt. Examples of rosin acid salts include alkali metal salts such as sodium salts and potassium salts. The amount of rosin acid and rosin acid salt added may be 3.0 to 10.0 parts by mass per 100 parts by mass of the raw material monomer used. The amount of rosin acid and rosin acid salt added may be, for example, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, 7.0, 7.5, 8.0, 8.5, 9.0, or 10.0 parts by mass, and may be within a range between any two of the values ​​exemplified here.

[0042] The rosin acid and / or rosin acid salt may contain a conjugated resin acid component and a non-conjugated resin acid component. Examples of the conjugated resin acid component include abietic acid, neoabietic acid, palustric acid, levopimaric acid, and salts thereof. Examples of the non-conjugated resin acid component include dehydroabietic acid, pimaric acid, isopimaric acid, dihydropimaric acid, dihydroabietic acid, and salts thereof.

[0043] The rosin acid and rosin acid salts used in the emulsion polymerization step can have a ratio RB / RA of 0.10 or more and 0.70 or less, where RB is the total peak area of ​​abietic acid, neoabietic acid, palustric acid, levopimaric acid, and their salts relative to RA, the total peak area of ​​dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid, and their salts, as determined by gas chromatography analysis of an extract extracted with an ethanol / toluene azeotrope as specified in JIS K 6229. The RB / RA of the rosin acid and rosin acid salts can be, for example, 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, or 0.70, or can be within a range between any two of the values ​​exemplified here. The RB / RA of the resulting chloroprene polymer test specimens can be adjusted by adjusting the type and amount of rosin acid and / or rosin acid salt.

[0044] The emulsifier may also include emulsifiers and dispersants other than rosin acid and rosin acid salts. Examples of emulsifiers and dispersants other than rosin acid and rosin acid salts include cationic, anionic, and nonionic emulsifiers and dispersants. In one embodiment of the present invention, the emulsifier used in the emulsion polymerization process may include rosin acid and / or rosin acid salts, together with an anionic emulsifier and dispersant. As anionic emulsifiers and dispersants, sulfate- or sulfonate-based anionic emulsifiers and dispersants are preferably used in combination to stabilize the chloroprene polymer latex when a pH adjuster is added. Specific examples include alkyl sulfonates having 8 to 20 carbon atoms, alkyl aryl sulfates, condensates of sodium β-naphthalene sulfonate and formaldehyde, and sodium alkyl diphenyl ether disulfonates. The amount of anionic emulsifier or dispersant added may be 0.05 to 5.0 parts by mass per 100 parts by mass of the raw material monomers. The amount of anionic emulsifier or dispersant added is, for example, 0.05, 0.1, 0.2, 0.3, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, or 5.0 parts by mass relative to 100 parts by mass of the raw material monomer, and may be within a range between any two of the numerical values ​​exemplified here.

[0045] (Chain Transfer Agent) In the emulsion polymerization step, it is preferable to add a chain transfer agent to adjust the molecular weight, molecular weight distribution, and toluene insoluble content of the chloroprene polymer. The chain transfer agent may be added at the beginning of polymerization or during polymerization. Preferred chain transfer agents are long-chain alkyl mercaptans such as n-dodecyl mercaptan and t-dodecyl mercaptan, and dialkyl xanthogen disulfides such as diisopropyl xanthogen disulfide and diethyl xanthogen disulfide. Long-chain alkyl mercaptans are more preferable because they facilitate control of the molecular weight and toluene insoluble content. The chain transfer agent can be used alone or in combination of two or more. The total amount of chain transfer agent added during emulsion polymerization is preferably 0.005 to 0.12 parts by mass per 100 parts by mass of the chloroprene monomer and the monomer copolymerizable with the chloroprene monomer. The total amount of chain transfer agent added is, for example, 0.005, 0.01, 0.05, 0.10, 0.11, or 0.12 parts by mass, and may be within a range between any two of the numerical values ​​exemplified here.

[0046] (Initiator) As the polymerization initiator, a conventional radical polymerization initiator can be used. Specifically, organic or inorganic peroxides such as benzoyl peroxide, potassium persulfate, ammonium persulfate, etc., and azo compounds such as azobisisobutyronitrile, etc., can be used. Furthermore, a co-catalyst such as anthraquinone sulfonate, potassium sulfite, sodium sulfite, etc. can be used in combination as appropriate.

[0047] (Potassium hydroxide and sodium hydroxide) In the emulsion polymerization step, sodium hydroxide and / or potassium hydroxide can be used. The amount of sodium hydroxide and potassium hydroxide can be 0.01 to 2.0 parts by mass per 100 parts by mass of the raw material monomers.

[0048] (Reducing Agent) In the emulsion polymerization step, a reducing agent can be added. Examples of the reducing agent include potassium pyrosulfite, potassium sulfite, potassium hydrogen sulfite, potassium phosphate, potassium hydrogen phosphate, sodium hydrogen sulfite, sodium sulfate, and thiourea dioxide. The amount of the reducing agent added can be 0.005 to 3.0 parts by mass per 100 parts by mass of the raw material monomers used in the polymerization step.

[0049] (Polymerization Conversion Rate) The polymerization conversion rate of raw material monomers during emulsion polymerization of chloroprene-based polymers and the like is preferably 50% by mass or more but less than 90% by mass. The polymerization conversion rate (mass%) is calculated by [(polymer mass / total monomer mass) × 100]. Hereinafter, the polymerization conversion rate may also be simply referred to as the polymerization rate.

[0050] (Polymerization Temperature) The chloroprene polymer can be polymerized, for example, in the range of 0 to 45°C, and is preferably polymerized at a low temperature of 5 to 20°C. The polymerization temperature is, for example, 0, 5, 10, 15, 20, 25, 30, 35, 40, or 45°C, and may be within a range between any two of the values ​​exemplified here. By adjusting the polymerization temperature, the microstructure in the chloroprene polymer can be adjusted, and in particular, the value of PA / (PB-PC) x 100 can be controlled. For example, by lowering the polymerization temperature, the value of PA / (PB-PC) x 100 can be reduced.

[0051] (Polymerization Terminator) Generally, in the production of chloroprene polymers, a polymerization terminator is added to terminate the reaction when a predetermined polymerization rate is reached in order to obtain a polymer with a desired molecular weight and distribution. The polymerization terminator is not particularly limited, but examples thereof include phenothiazine, p-t-butylcatechol, hydroquinone, hydroquinone monomethyl ether, and diethylhydroxylamine.

[0052] (Solid Content Concentration) The method for producing a chloroprene polymer latex according to one embodiment of the present invention may include a step of removing unreacted monomers by a concentration method such as vacuum distillation. The solid content concentration of the chloroprene polymer latex is not particularly limited, but can be adjusted to 40 to 65 mass%. The solid content concentration of the chloroprene polymer latex can be controlled by adjusting the blending ratio including a solvent such as water during emulsion polymerization of the chloroprene polymer, or by a concentration step such as vacuum distillation.

[0053] Furthermore, after polymerization, a composition (e.g., latex) containing a chloroprene polymer obtained by the production method of one embodiment of the present invention may optionally contain a freeze stabilizer, an emulsion stabilizer, a viscosity modifier, an antioxidant, a preservative, and the like, within a range that does not impair the effects of the present invention.

[0054] In the polymerization process for a chloroprene-based polymer, all of the raw material monomers and chemicals to be used in the polymerization process can be charged into a polymerization vessel before the start of polymerization, and then the polymerization can be started. Alternatively, at least a portion of the raw material monomers and / or chemicals to be used in the polymerization process can be charged into a polymerization vessel before the start of polymerization, and the remainder can be added in portions after the start of polymerization.

[0055] When at least a portion of the raw material monomers and chemicals are charged into a polymerization vessel before the initiation of polymerization, and the remaining raw material monomers and / or chemicals are added after the initiation of polymerization, the remaining raw material monomers and / or chemicals can be added in one or more divided portions, or can be added continuously at a constant flow rate. In one embodiment of the present invention, at least a portion of the raw material monomers can be added in divided portions after the initiation of polymerization. For example, when chloroprene and 2,3-dichloro-1,3-butadiene are used as raw material monomers, a portion of the 2,3-dichloro-1,3-butadiene can be added in divided portions after the initiation of polymerization.

[0056] 3. Chloroprene Polymer Latex The chloroprene polymer latex according to one embodiment of the present invention may contain a chloroprene polymer and water. A latex containing a chloroprene polymer obtained after chloroprene polymer polymerization may be referred to as a chloroprene polymer latex. When the polymer contained in the chloroprene polymer according to the present invention is obtained by emulsion polymerization, the chloroprene polymer latex may further contain raw materials used in the emulsion polymerization step, such as an emulsifier.

[0057] 4. Dip-molded product (dip-molded coating / film) A dip-molded product according to one embodiment of the present invention can be a dip-molded product of a chloroprene polymer latex composition containing a chloroprene polymer latex.

[0058] A dip-molded product according to one embodiment of the present invention can be obtained by dip-molding a chloroprene polymer latex composition described below by a dip coagulation method, followed by heating and drying at 130°C for 30 minutes. The dip-molded product according to the present invention has high tensile strength at break, a low modulus at 500% elongation, and a low modulus at 500% elongation after long-term storage. The dip-molded product according to one embodiment of the present invention can be suitably used as industrial gloves, general household gloves, medical gloves, balloons, catheters, or boots.

[0059] The dip-molded product according to the present invention may contain components contained in the chloroprene polymer latex composition described below. The dip-molded product may contain a chloroprene polymer as a base polymer, and may contain 70% by mass or more of the chloroprene polymer, preferably 80% by mass or more, and more preferably 90% by mass or more, of the chloroprene polymer, based on 100% by mass of the dip-molded product. The content of the chloroprene polymer in the dip-molded product, based on 100% by mass of the dip-molded product, may be, for example, 70, 75, 80, 85, 90, 95, 96, 97, 98, 99, or 100% by mass, or may be within a range between any two of the values ​​exemplified here.

[0060] The dip-molded article containing the chloroprene polymer according to the present invention has high tensile strength at break, low modulus at 500% elongation, and low modulus at 500% elongation after long-term storage, regardless of whether a vulcanizing agent and a vulcanization accelerator are added. The dip-molded article according to one embodiment of the present invention may be free of a vulcanizing agent and a vulcanization accelerator, and may be free of sulfur and vulcanization accelerators such as thiuram, dithiocarbamate, thiourea, guanidine, xanthogenate, and thiazole.

[0061] 4.1 Characteristics of Dip-Molded Product The dip-molded product according to one embodiment of the present invention preferably has a low-temperature hardness change ΔH2 of 29 or less. The low-temperature hardness change ΔH2 may be, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, or 29, and may be within a range between any two of the values ​​exemplified here. The low-temperature hardness change ΔH2 is expressed as HB2 - HA2, where HA2 represents the Shore hardness measured in an environment of 23°C using a durometer type A after the dip-molded product has been heat-treated at 70°C for 30 minutes, and then the dip-molded product has been stacked to a thickness of 6.00 ± 0.20 mm. HB2 represents the Shore hardness measured in an environment of -10°C using a durometer type A after the dip-molded product has been heat-treated at 70°C for 30 minutes and further stored at -10°C for 168 hours, and then the dip-molded product has been stacked to a thickness of 6.00 ± 0.20 mm.

[0062] In the dip-molded product according to one embodiment of the present invention, the ratio RB / RA of the total amount RB of peak areas of abietic acid, neoabietic acid, palustric acid, levopimaric acid, and their salts to the total amount RA of peak areas of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid, and their salts, obtained by gas chromatography analysis of an extract extracted with an ethanol / toluene azeotropic mixture as specified in JIS K 6229, is preferably 0.10 or more and 0.70 or less. RB / RA is, for example, 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, or 0.70, and may be within a range between any two of the values ​​exemplified here.

[0063] The dip-molded article according to one embodiment of the present invention may contain 12 to 30 mass% of 2,3-dichloro-1,3-butadiene monomer units, preferably 14 to 27 mass%, based on 100 mass% of the total of chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units. The content of 2,3-dichloro-1,3-butadiene monomer units is, for example, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or 30 mass%, and may be within a range between any two of the values ​​exemplified here.

[0064] The dip-molded product according to one embodiment of the present invention preferably has a tensile strength at break of 20.0 MPa or more, and more preferably 23.0 MPa or more, measured in accordance with JIS K 6251. The tensile strength at break may be, for example, 20.0, 21.0, 22.0, 23.0, 24.0, 25.0, 26.0, 27.0, 28.0, 29.0, 30.0, 31.0, 32.0, 33.0, 34.0, 35.0, 36.0, 37.0, 38.0, 39.0, or 40.0 MPa, or may be within a range between any two of the values ​​exemplified here.

[0065] The dip-molded product according to one embodiment of the present invention preferably has a modulus at 500% elongation of 2.00 MPa or less, more preferably 1.80 MPa or less, measured in accordance with JIS K 6251. The modulus at 500% elongation may be, for example, 1.00, 1.10, 1.20, 1.30, 1.40, 1.50, 1.60, 1.70, 1.80, 1.90, or 2.00 MPa, or may be within a range between any two of the values ​​exemplified here.

[0066] The dip-molded product according to one embodiment of the present invention preferably has a modulus at 500% elongation of 2.50 MPa or less, as measured according to JIS K6251, after storage at 23° C. for 6 months. The modulus at 500% elongation is, for example, 1.00, 1.10, 1.20, 1.30, 1.40, 1.50, 1.60, 1.70, 1.80, 1.90, 2.00, 2.10, 2.20, 2.30, 2.40, or 2.50 MPa, and may be within a range between any two of the values ​​exemplified here.

[0067] The low-temperature hardness change ΔH2, RB / RA, tensile strength at break, modulus at 500% elongation, and modulus at 500% elongation after storage at 23°C for 6 months of the dip-molded product were measured by the methods described above in the section on chloroprene-based polymers.

[0068] A dip-molded product according to one embodiment of the present invention can have a low-temperature hardness change ΔH2 of 29 or less, a tensile strength at break of 20.0 MPa or more, and a 500% modulus of 2.00 MPa or less, as measured in accordance with JIS K 6251. Furthermore, a dip-molded product according to one embodiment of the present invention can satisfy the above-mentioned requirements for any three or more, four or more, or all of the low-temperature hardness change ΔH2, RB / RA, tensile strength at break, modulus at 500% elongation, and modulus at 500% elongation after storage at 23°C for six months.

[0069] The dip-molded product according to one embodiment of the present invention contains a chloroprene polymer and may further contain an antioxidant and a metal oxide. The dip-molded product may also contain a vulcanizing agent, a vulcanization accelerator, and a crosslinking agent. The dip-molded product may be produced as described in the Examples.

[0070] The low-temperature hardness change ΔH2, RB / RA, tensile strength at break, modulus at 500% elongation, and modulus at 500% elongation after storage at 23°C for 6 months of the dip-molded product can be controlled by adjusting the production method for the chloroprene polymer, for example, the types and amounts of raw materials used, the types and amounts of agents used, and polymerization conditions.

[0071] 4.2 Shape of Dip-Molded Product The thickness (e.g., minimum thickness) of the dip-molded product may be 0.01 to 0.50 mm. The thickness of the dip-molded product may be, for example, 0.01, 0.05, 0.10, 0.20, 0.30, 0.40, or 0.50 mm, and may be within a range between any two of the values ​​exemplified here. The thickness of the dip-molded product can be adjusted by the time for immersing the mold in the chloroprene polymer latex composition, the solids concentration of the chloroprene polymer latex composition, and the like. To reduce the thickness of the dip-molded product, the immersion time may be shortened or the solids concentration of the chloroprene polymer latex composition may be reduced.

[0072] The dip-molded product may contain sulfur or a vulcanization accelerator. However, the dip-molded product according to one embodiment of the present invention can have mechanical properties equivalent to or superior to those of vulcanized dip-molded products obtained from a chloroprene polymer latex composition containing a conventional chloroprene polymer, even if it does not contain sulfur or a vulcanization accelerator. Therefore, the chloroprene polymer according to the present invention is suitably used as a raw material for the dip-molded product (dip-molded article) of the chloroprene polymer of this embodiment.

[0073] 5. Method for Producing Dip-Molded Product A method for producing a dip-molded product according to one embodiment of the present invention may include: a dip-molding step of dip-molding a chloroprene polymer latex composition containing the above-described chloroprene polymer to obtain a dip-molded product; and a drying step of heating and drying the dip-molded product to obtain a dip-molded product.

[0074] 5.1 Chloroprene Polymer Latex Composition The chloroprene polymer latex composition according to one embodiment of the present invention contains the chloroprene polymer described above. The chloroprene polymer latex composition according to one embodiment of the present invention may contain, in addition to the chloroprene polymer, a metal oxide, an antioxidant, and other necessary chemicals. The chloroprene polymer latex composition according to one embodiment of the present invention may not contain a vulcanizing agent or a vulcanization accelerator, and may not contain sulfur or a vulcanization accelerator such as a thiuram, dithiocarbamate, thiourea, guanidine, xanthogenate, or thiazole.

[0075] 5.1.1 Metal Oxide The chloroprene polymer latex composition according to one embodiment of the present invention may contain a metal oxide. The metal oxide is not particularly limited, and examples thereof include zinc oxide, lead oxide, trilead tetroxide, magnesium oxide, aluminum oxide, iron oxide, beryllium oxide, and titanium oxide. The metal oxide preferably contains zinc oxide. Zinc oxide is generally believed to function as a scavenger for dechlorinated atoms in the chloroprene polymer. These metal oxides may be used alone or in combination of two or more.

[0076] The amount of metal oxide added is preferably 0.5 to 15.0 parts by mass per 100 parts by mass of the solid content of the chloroprene polymer contained in the chloroprene polymer latex composition. When the amount of metal oxide added is 0.5 parts by mass or more, an improvement in tensile strength at break is expected due to the crosslinking effect between polymers. When the amount of metal oxide added is 15.0 parts by mass or less, a dip-molded product with excellent flexibility can be obtained. Furthermore, from the viewpoint of the balance of physical properties between flexibility and tensile strength at break of the obtained dip-molded product, the amount of metal oxide added is more preferably 0.5 to 5.0 parts by mass.

[0077] 5.1.2 Antioxidant The chloroprene polymer latex composition according to one embodiment of the present invention may contain an antioxidant. The antioxidant is not particularly limited, and phenolic antioxidants, amine-based antioxidants, heat-resistant oxidation (aging) inhibitors, ozone-resistant antioxidants, etc. can be used. When the obtained dip-molded product is used as a medical glove, a phenolic antioxidant can be used from the viewpoint of the color tone, texture, and hygiene of the dip-molded product. In particular, hindered phenolic antioxidants have a strong effect. Examples of hindered phenol-based antioxidants include 2,2'-methylenebis(4-ethyl-6-t-butylphenol), 2,2'-methylenebis(4-methyl-6-t-butylphenol), 4,4'-butylidene(3-methyl-6-t-butylphenol), 4,4'-thiobis(3-methyl-6-t-butylphenol), butylated reaction products of p-cresol and dicyclopentadiene, 2,5'-di-t-butylhydroquinone, and 2,5'-di-t-amylhydroquinone. Among these, butylated reaction products of p-cresol and dicyclopentadiene are desirable from the viewpoint of general dispersibility in aqueous materials. Furthermore, these compounds may be used alone or in combination of two or more.

[0078] The amount of antioxidant added is preferably 0.5 to 10.0 parts by mass per 100 parts by mass of the solid content of the chloroprene polymer contained in the chloroprene polymer latex composition. The amount of antioxidant added is, for example, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, or 10.0 parts by mass, and may be within a range between any two of the values ​​exemplified here. When the amount of antioxidant added is 0.5 parts by mass or more, the effect of suppressing color change in the dip-molded product can be obtained. When the amount of antioxidant added is 10.0 parts by mass or less, the stability of the chloroprene polymer latex composition can be ensured. Furthermore, from the viewpoint of the balance of physical properties between the flexibility and tensile strength at break of the obtained dip-molded product, the amount of antioxidant added is more preferably 0.5 to 5.0 parts by mass.

[0079] 5.1.3 Vulcanizing Agent and Vulcanization Accelerator The chloroprene polymer latex composition according to one embodiment of the present invention may contain a vulcanizing agent and / or a vulcanization accelerator. The chloroprene polymer latex composition according to one embodiment of the present invention may not contain sulfur or the aforementioned thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthogenate-based, thiazole-based, or other vulcanization accelerators. That is, the chloroprene polymer latex composition includes one containing a vulcanizing agent but not a vulcanization accelerator, one containing a vulcanization accelerator but not a vulcanizing agent, one containing a vulcanization accelerator and a vulcanization accelerator, and one containing a vulcanizing agent and a vulcanization accelerator and not a vulcanization accelerator. Whether a vulcanizing agent and a vulcanization accelerator are added may be determined depending on the desired dip-molded product.

[0080] Examples of vulcanizing agents include, but are not limited to, sulfur. The amount of vulcanizing agent added can be 0 to 10.0 parts by mass per 100 parts by mass of the solid content of the chloroprene polymer contained in the chloroprene polymer latex composition. The amount of vulcanizing agent added is, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 parts by mass, and may be within a range between any two of the values ​​exemplified here.

[0081] A vulcanization accelerator is a chemical added during the vulcanization of raw rubber to act with the vulcanizing agent to increase the vulcanization speed, thereby shortening the vulcanization time, lowering the vulcanization temperature, reducing the amount of vulcanizing agent, and improving the physical properties of the vulcanized rubber. It usually refers to a chemical that accelerates the sulfur vulcanization reaction.

[0082] Examples of vulcanization accelerators include, but are not limited to, thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthogenate-based, thiazole-based, etc. These may be used alone or in combination of two or more types as required.

[0083] Examples of thiuram vulcanization accelerators include tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, tetrakis(2-ethylhexyl)thiuram disulfide, tetramethylthiuram monosulfide, and dipentamethylenethiuram tetrasulfide.

[0084] Examples of the dithiocarbamate vulcanization accelerator include sodium dibutyldithiocarbamate, zinc dimethyldithiocarbamate, zinc diethyldithiocarbamate, zinc N-ethyl-N-phenyldithiocarbamate, zinc N-pentamethylenedithiocarbamate, copper dimethyldithiocarbamate, ferric dimethyldithiocarbamate, and tellurium diethyldithiocarbamate, and zinc dibutyldithiocarbamate is particularly preferred.

[0085] Examples of the thiourea-based vulcanization accelerator include ethylene thiourea, N,N'-diethyl thiourea, trimethyl thiourea, and N,N'-diphenyl thiourea.

[0086] Examples of the guanidine vulcanization accelerator include 1,3-diphenylguanidine, 1,3-di-o-tolylguanidine, 1-o-tolylbiguanide, and di-o-tolylguanidine salts of dicatechol borate.

[0087] Examples of xanthogenate-based vulcanization accelerators include zinc butylxanthogenate and zinc isopropylxanthogenate.

[0088] Examples of the thiazole vulcanization accelerator include 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, 2-mercaptobenzothiazole zinc salt, 2-mercaptobenzothiazole cyclohexylamine salt, and 2-(4'-morpholinodithio)benzothiazole.

[0089] The amount of the vulcanization accelerator added may be 0 to 5.0 parts by mass relative to 100 parts by mass of the solid content of the chloroprene polymer contained in the chloroprene polymer latex composition, and may be, for example, 0, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, or 5.0, or may be within a range between any two of the numerical values ​​exemplified here.

[0090] A method for producing a chloroprene polymer latex composition according to one embodiment of the present invention may include a raw material mixing step of mixing raw materials containing a chloroprene polymer, a metal oxide, an antioxidant, and other required chemicals. In the mixing step, an aqueous dispersion containing the metal oxide, the antioxidant, and other required chemicals may be prepared in advance, and the chloroprene polymer and the aqueous dispersion may be mixed. The mixing step may be performed using a known mixing device such as a ball mill.

[0091] 5.2 Dip-molding step A method for producing a dip-molded product according to one embodiment of the present invention may include a dip-molding step of dip-molding a chloroprene polymer latex composition containing the chloroprene polymer obtained by the above-described method for producing a chloroprene polymer to obtain a dip-molded product.

[0092] Examples of the dip-molding method according to one embodiment of the present invention include the dip-coagulation method, the simple dip-coagulation method, the thermal dip-coagulation method, and the electrodeposition method. The dip-coagulation method can be used from the viewpoints of ease of production and the ease of obtaining a dip-molded product of a uniform thickness. Specifically, a ceramic mold coated with a calcium-based coagulation liquid is immersed in a chloroprene polymer latex composition to coagulate the chloroprene polymer latex composition. After removing water-soluble impurities by leaching, the composition is dried, and then heated and vulcanized to form a dip-molded film (rubber film), which is then demolded. This allows for the production of a film-like dip-molded product.

[0093] 5.3 Drying Step The method for producing a dip-molded product according to one embodiment of the present invention may include a drying step of heating and drying the dip-molded product to obtain a dip-molded product.

[0094] The heating temperature may be set appropriately depending on the composition of the chloroprene polymer, and may be 120 to 180°C. The heating temperature is preferably 120 to 150°C. The heating temperature may be, for example, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, or 220°C, or may be within a range between any two of the values ​​exemplified here. The heating time may be set appropriately depending on the composition of the chloroprene polymer, the shape of the unvulcanized molded body, and the like, and may be 10 to 300 minutes. The heating time may be, for example, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, or 300 minutes, or may be within a range between any two of the values ​​exemplified here. As an example, a dip-molded product according to one embodiment of the present invention may be one that has been subjected to a heat drying treatment at 130°C for 30 minutes.

[0095] The present invention will be described in more detail below based on examples, but the present invention should not be construed as being limited to these examples.

[0096] Example 1 A 30 L polymerization vessel was charged with 80 parts by mass of chloroprene (monomer), 20 parts by mass of 2,3-dichloro-1,3-butadiene, 90 parts by mass of pure water, 4.6 parts by mass of conjugated resin acid-based rosin acid (trade name "Harthall R-WW" manufactured by Harima Chemicals Co., Ltd.), 0.03 parts by mass of n-dodecyl mercaptan, 1.6 parts by mass of potassium hydroxide, 0.5 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "Demol N" manufactured by Kao Corporation), 0.5 parts by mass of sodium hydrogen sulfite, and 0.03 parts by mass of thiourea dioxide. Polymerization was carried out at a polymerization temperature of 15°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous solution of potassium persulfate as a polymerization initiator. When the polymerization rate reached 83%, 0.1 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization, yielding a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and the resulting mixture was concentrated to obtain a chloroprene polymer latex having a solid content of 60% by mass.

[0097] For measuring the physical properties, 200 mL of the obtained chloroprene polymer latex was sampled, and the remaining latex was used to prepare a dip-molded test product.

[0098] Using the sampled chloroprene polymer latex, the 2,3-dichloro-1,3-butadiene content of the chloroprene polymer was measured. Furthermore, the toluene-insoluble portion of the chloroprene polymer was measured. Furthermore, the nuclear magnetic resonance (13C-solid NMR) spectrum of the chloroprene polymer was measured. The analytical results are shown in Table 1. The measurement method will be described later.

[0099] Example 2 Polymerization was carried out in the same manner as in Example 1, except that the amounts of chloroprene (monomer) and 2,3-dichloro-1,3-butadiene were changed to 85 parts by mass and 15 parts by mass, respectively. The obtained polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a chloroprene polymer latex having a solid content of 60% by mass. Using the obtained latex, a dip-molded test article was prepared in the same manner as in Example 1. Furthermore, the 2,3-dichloro-1,3-butadiene content of the chloroprene polymer, the toluene-insoluble content, and the nuclear magnetic resonance (C-solid state NMR) spectrum were measured in the same manner as in Example 1. The analytical results are shown in Table 1.

[0100] Example 3 To a 30 L polymerization vessel were added 87 parts by mass of chloroprene (monomer), 7 parts by mass of 2,3-dichloro-1,3-butadiene, 90 parts by mass of pure water, 4.6 parts by mass of conjugated resin acid-based rosin acid (trade name "Harthall R-WW" manufactured by Harima Chemicals Co., Ltd.), 0.03 parts by mass of n-dodecyl mercaptan, 1.6 parts by mass of potassium hydroxide, 0.5 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "Demol N" manufactured by Kao Corporation), 0.5 parts by mass of sodium hydrogen sulfite, and 0.03 parts by mass of thiourea dioxide. Polymerization was carried out at a polymerization temperature of 15°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous solution of potassium persulfate as a polymerization initiator. When the conversion of the charged monomers reached 15%, 6 parts by mass of 2,3-dichloro-1,3-butadiene was continuously added over 120 minutes. When the conversion of the initially charged monomer and the continuously added monomer reached 83%, 0.1 parts by mass of diethylhydroxylamine, a polymerization terminator, was added to terminate the polymerization, yielding a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomer, and then concentrated to yield a chloroprene polymer latex with a solids concentration of 60% by mass. Using the obtained latex, a dip-molded test specimen was prepared in the same manner as in Example 1. Furthermore, the 2,3-dichloro-1,3-butadiene content of the chloroprene polymer, the toluene-insoluble content, and the nuclear magnetic resonance (C-solid state NMR) spectrum were measured in the same manner as in Example 1. The analytical results are shown in Table 1.

[0101] Example 4 Polymerization was carried out in the same manner as in Example 1, except that the polymerization was terminated at a polymerization rate of 70%. The obtained polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and further concentrated to obtain a chloroprene polymer latex with a solid content of 60% by mass. Using the obtained latex, a dip-molded test article was prepared in the same manner as in Example 1. Furthermore, the 2,3-dichloro-1,3-butadiene content of the chloroprene polymer, the toluene-insoluble content, and the nuclear magnetic resonance (13C-solid state NMR) spectrum were measured in the same manner as in Example 1. The analytical results are shown in Table 1.

[0102] Example 5 Polymerization was carried out in the same manner as in Example 1, except that the polymerization was terminated at a polymerization rate of 64%. The obtained polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a chloroprene polymer latex with a solid content of 60% by mass. The obtained latex was subjected to dip-molding for testing in the same manner as in Example 1. Furthermore, the 2,3-dichloro-1,3-butadiene content of the chloroprene polymer, the toluene-insoluble content, and the nuclear magnetic resonance (13C-solid state NMR) spectrum were measured in the same manner as in Example 1. The analytical results are shown in Table 1.

[0103] Example 6 A 30 L polymerization vessel was charged with 80 parts by mass of chloroprene (monomer), 20 parts by mass of 2,3-dichloro-1,3-butadiene, 90 parts by mass of pure water, 2.2 parts by mass of conjugated resin acid-based rosin acid (trade name "Harthall R-WW", manufactured by Harima Chemicals Co., Ltd.), 9.6 parts by mass of gum rosin-based disproportionated potassium rosinate (aqueous solution) (trade name "Londis K-25", manufactured by Arakawa Chemical Industries, Ltd.), 0.03 parts by mass of n-dodecyl mercaptan, 1.6 parts by mass of potassium hydroxide, 0.5 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "Demol N", manufactured by Kao Corporation), 0.5 parts by mass of sodium hydrogensulfite, and 0.03 parts by mass of thiourea dioxide. Polymerization was carried out at a polymerization temperature of 15°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous solution of potassium persulfate as a polymerization initiator. When the polymerization rate reached 83%, 0.1 parts by mass of diethylhydroxylamine, a polymerization terminator, was added to terminate the polymerization, yielding a polymerization solution. The polymerization solution was distilled under reduced pressure to remove unreacted monomers, and then concentrated to yield a chloroprene polymer latex with a solids concentration of 60% by mass. The resulting polymerization solution was distilled under reduced pressure to remove unreacted monomers, and then concentrated to yield a chloroprene polymer latex with a solids concentration of 60% by mass. The resulting latex was subjected to dip-molding for testing in the same manner as in Example 1. Furthermore, the 2,3-dichloro-1,3-butadiene content of the chloroprene polymer, the toluene-insoluble content, and the nuclear magnetic resonance (13C-solid state NMR) spectrum were measured in the same manner as in Example 1. The analytical results are shown in Table 1.

[0104] Example 7 Polymerization was carried out in the same manner as in Example 1, except that the amount of conjugated resin acid-based rosin acid in Example 1 was changed to 9 parts by mass. The obtained polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a chloroprene polymer latex with a solid content of 60% by mass. The obtained latex was subjected to dip-molding for testing in the same manner as in Example 1. Furthermore, the 2,3-dichloro-1,3-butadiene content of the chloroprene polymer, the toluene-insoluble content, and the nuclear magnetic resonance (C-solid state NMR) spectrum were measured in the same manner as in Example 1. The analytical results are shown in Table 1.

[0105] Example 8 A 30 L polymerization vessel was charged with 90 parts by mass of chloroprene (monomer), 10 parts by mass of 2,3-dichloro-1,3-butadiene, 90 parts by mass of pure water, 4.6 parts by mass of conjugated resin acid-based rosin acid (trade name "Harthall R-WW" manufactured by Harima Chemicals Co., Ltd.), 0.03 parts by mass of n-dodecyl mercaptan, 1.6 parts by mass of potassium hydroxide, 0.5 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "Demol N" manufactured by Kao Corporation), and 0.5 parts by mass of sodium hydrogen sulfite. Polymerization was carried out at a polymerization temperature of 40°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous solution of potassium persulfate as a polymerization initiator. When the polymerization rate reached 70%, 0.1 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization, yielding a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a chloroprene polymer latex with a solids concentration of 60% by mass. The obtained polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a chloroprene polymer latex with a solids concentration of 60% by mass. The obtained latex was subjected to dip-molding for testing in the same manner as in Example 1. Furthermore, the 2,3-dichloro-1,3-butadiene content of the chloroprene polymer, the toluene-insoluble content, and the nuclear magnetic resonance (13C-solid state NMR) spectrum were measured in the same manner as in Example 1. The analytical results are shown in Table 1.

[0106] Example 9 A 30 L polymerization vessel was charged with 85 parts by mass of chloroprene (monomer), 15 parts by mass of 2,3-dichloro-1,3-butadiene, 90 parts by mass of pure water, 4.3 parts by mass of a conjugated resin acid-based rosin acid (trade name "Harthall R-WW", manufactured by Harima Chemicals Co., Ltd.), 0.5 parts by mass (based on solids content) of a gum rosin-based disproportionated potassium rosinate aqueous solution (trade name "Londis K-25", manufactured by Arakawa Chemical Industries, Ltd.), 0.03 parts by mass of n-dodecyl mercaptan, 1.5 parts by mass of potassium hydroxide, and 0.5 parts by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "Demol N", manufactured by Kao Corporation). Polymerization was carried out at a polymerization temperature of 20°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous potassium persulfate solution as a polymerization initiator. When the polymerization rate reached 83%, 0.1 parts by mass of diethylhydroxylamine, a polymerization terminator, was added to terminate the polymerization, yielding a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to yield a chloroprene polymer latex with a solid content of 60% by mass. The obtained latex was subjected to dip-molding for testing in the same manner as in Example 1. Furthermore, the 2,3-dichloro-1,3-butadiene content of the chloroprene polymer, the toluene-insoluble content, and the nuclear magnetic resonance (13C-solid state NMR) spectrum were measured in the same manner as in Example 1. The analytical results are shown in Table 1.

[0107] Comparative Example 1 Polymerization was carried out in the same manner as in Example 1, except that the amounts of chloroprene (monomer) and 2,3-dichloro-1,3-butadiene were changed to 90 parts by mass and 10 parts by mass, respectively. The obtained polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a chloroprene polymer latex having a solid content of 60% by mass. The obtained latex was subjected to dip-molding for testing in the same manner as in Example 1. Furthermore, the 2,3-dichloro-1,3-butadiene content of the chloroprene polymer, the toluene-insoluble content, and the nuclear magnetic resonance (C-solid state NMR) spectrum were measured in the same manner as in Example 1. The analytical results are shown in Table 2.

[0108] Comparative Example 2 Polymerization was carried out in the same manner as in Example 1, except that the amounts of chloroprene (monomer) and 2,3-dichloro-1,3-butadiene were changed to 93 parts by mass and 7 parts by mass, respectively. The obtained polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a chloroprene polymer latex having a solid content of 60% by mass. The obtained latex was subjected to dip-molding for testing in the same manner as in Example 1. Furthermore, the 2,3-dichloro-1,3-butadiene content of the chloroprene polymer, the toluene-insoluble content, and the nuclear magnetic resonance (C-solid state NMR) spectrum were measured in the same manner as in Example 1. The analytical results are shown in Table 2.

[0109] Comparative Example 3 Polymerization was carried out in the same manner as in Example 1, except that the amount of conjugated resin acid-based rosin acid was changed to 11 parts by mass. The obtained polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a chloroprene polymer latex with a solid content of 60% by mass. The obtained latex was subjected to dip-molding for testing in the same manner as in Example 1. Furthermore, the 2,3-dichloro-1,3-butadiene content of the chloroprene polymer, the toluene-insoluble content, and the nuclear magnetic resonance (C-solid state NMR) spectrum were measured in the same manner as in Example 1. The analytical results are shown in Table 2.

[0110] Comparative Example 4 To a 30 L polymerization vessel were added 80 parts by mass of chloroprene (monomer), 20 parts by mass of 2,3-dichloro-1,3-butadiene, 90 parts by mass of purified water, 18.4 parts by mass of gum rosin-based disproportionated potassium rosinate (aqueous solution) (trade name "LONDIS K-25" manufactured by Arakawa Chemical Industries, Ltd.), 0.03 parts by mass of n-dodecyl mercaptan, 0.8 parts by mass of potassium hydroxide, 0.5 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N" manufactured by Kao Corporation), 0.5 parts by mass of sodium hydrogen sulfite, and 0.03 parts by mass of thiourea dioxide. Polymerization was carried out at a polymerization temperature of 15°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous solution of potassium persulfate as a polymerization initiator. When the polymerization rate reached 83%, 0.1 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization, yielding a polymerization solution. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and the resulting solution was concentrated to obtain a chloroprene polymer latex having a solids concentration of 60% by mass. The resulting polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and the resulting solution was concentrated to obtain a chloroprene polymer latex having a solids concentration of 60% by mass. The resulting latex was subjected to dip-molding for testing in the same manner as in Example 1. Furthermore, the 2,3-dichloro-1,3-butadiene content of the chloroprene polymer, the toluene-insoluble content, and the nuclear magnetic resonance (13C-solid state NMR) spectrum were measured in the same manner as in Example 1. The analytical results are shown in Table 2.

[0111] Comparative Example 5 Polymerization was carried out in the same manner as in Example 1, except that the polymerization rate at which the polymerization was terminated was set to 50%. The obtained polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a chloroprene polymer latex with a solid content of 60% by mass. The obtained latex was subjected to dip molding for testing in the same manner as in Example 1. Furthermore, the 2,3-dichloro-1,3-butadiene content of the chloroprene polymer, the toluene insoluble content, and the nuclear magnetic resonance (C-solid state NMR) spectrum were measured in the same manner as in Example 1. The analytical results are shown in Table 2.

[0112] Comparative Example 6 To a 30 L polymerization vessel were added 80 parts by mass of chloroprene (monomer), 20 parts by mass of 2,3-dichloro-1,3-butadiene, 90 parts by mass of pure water, 4.8 parts by mass of conjugated resin acid-based rosin acid (trade name "Harthall R-WW", manufactured by Harima Chemicals Co., Ltd.), 0.03 parts by mass of n-dodecyl mercaptan, 1.5 parts by mass of potassium hydroxide, and 0.5 parts by mass of a sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "Demol N", manufactured by Kao Corporation). Polymerization was carried out at a polymerization temperature of 10°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous solution of potassium persulfate as a polymerization initiator. When the polymerization rate reached 89%, 0.1 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization, yielding a polymerization liquid. The polymerization solution was distilled under reduced pressure to remove unreacted monomers, and the resulting solution was concentrated to obtain a chloroprene polymer latex with a solid content of 60% by mass. The obtained latex was subjected to dip molding for testing in the same manner as in Example 1. Furthermore, the 2,3-dichloro-1,3-butadiene content of the chloroprene polymer, the toluene insoluble content, and the nuclear magnetic resonance (C-solid state NMR) spectrum were measured in the same manner as in Example 1. The analytical results are shown in Table 2.

[0113] Comparative Example 7 Polymerization was carried out in the same manner as in Comparative Example 1, except that the polymerization temperature in Comparative Example 6 was 17°C and the conversion at which the polymerization was terminated was 87%. The obtained polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and then concentrated to obtain a chloroprene polymer latex with a solid content of 60% by mass. The obtained latex was subjected to dip-molding for testing in the same manner as in Example 1. Furthermore, the 2,3-dichloro-1,3-butadiene content of the chloroprene polymer, the toluene-insoluble content, and the nuclear magnetic resonance (C-solid state NMR) spectrum were measured in the same manner as in Example 1. The analytical results are shown in Table 2.

[0114] Comparative Example 8 To a 30 L polymerization vessel were added 85 parts by mass of chloroprene (monomer), 15 parts by mass of 2,3-dichloro-1,3-butadiene, 100 parts by mass of pure water, 4.8 parts by mass of a conjugated resin acid-based rosin acid (trade name "Harthall R-WW", manufactured by Harima Chemicals Co., Ltd.), 1.5 parts by mass of potassium hydroxide, and 0.4 parts by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "Demol N", manufactured by Kao Corporation). Polymerization was carried out at a polymerization temperature of 15°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous solution of potassium persulfate as a polymerization initiator. When the polymerization rate reached 67%, 0.1 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization, yielding a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomer, and then concentrated to yield a chloroprene polymer latex with a solids concentration of 60% by mass. The obtained latex was subjected to dip molding for testing in the same manner as in Example 1. Furthermore, the 2,3-dichloro-1,3-butadiene content of the chloroprene polymer, the toluene insoluble matter, and the nuclear magnetic resonance analysis (13C-solid NMR) spectrum were measured in the same manner as in Example 1. The analytical results are shown in Table 2.

[0115] <Measurement of 2,3-dichloro-1,3-butadiene Content in Chloroprene Polymer> A chloroprene polymer obtained by freeze-drying a chloroprene polymer latex was cut into a 0.05 mg test piece and analyzed by pyrolysis gas chromatography to determine the area ratio of the peak derived from chloroprene to the peak derived from 2,3-dichloro-1,3-butadiene. Using a calibration curve of the area ratio of the peak derived from chloroprene to the peak derived from 2,3-dichloro-1,3-butadiene and the 2,3-dichloro-1,3-butadiene content, the content (% by mass) of 2,3-dichloro-1,3-butadiene monomer units relative to 100% by mass of the total of chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units was determined. The results are shown in Tables 1 and 2.

[0116] [Conditions for pyrolysis gas chromatography measurement] Device name: HP5890-II Column: DB-5 0.25 mmφ×30 m (film thickness 1.0 μm) Column temperature: 50°C (5 min) → 10°C / min → 150°C → 25°C / min → 300°C Injection port temperature: 250°C Detector temperature: 280°C Detector: FID

[0117] <Toluene-insoluble content> A chloroprene polymer obtained by freeze-drying a chloroprene polymer latex was cut into 2 mm squares to obtain a test piece. The test piece was placed in a conical beaker and dissolved in 80 g of toluene for 16 hours. Subsequently, after centrifugation, the gel content (insoluble content) was separated using a 200-mesh wire netting. The gel content was then dried and the mass of the dried product was measured. The toluene-insoluble content of the chloroprene polymer was calculated using the following formula, where Ag represents the chloroprene polymer after freeze-drying and B g represents the gel content (insoluble content) separated from the mixture dissolved in toluene. The results are shown in Tables 1 and 2. Toluene-insoluble content (gel content) = B / A × 100 (%)

[0118] <Calculation of PA / (PB-PC)×100 Based on Nuclear Magnetic Resonance Analysis (13C-Solid State NMR) Spectrum> A chloroprene polymer obtained by freeze-drying a chloroprene polymer latex was analyzed using a JNM-ECX-400 (400 MHz, FT type) manufactured by JEOL Ltd. In the obtained 13C-Solid State NMR spectrum, the peak area PA at 126.2 to 127.6 ppm, the peak area PB at 122.0 to 126.2 ppm, and the peak area PC at 129.9 to 130.3 ppm were determined based on the signal at 135.0 ppm attributable to carbon of the 1,4-trans bond -CCl=, which shows the maximum peak intensity. The peak areas PA and PC were calculated by determining the peak areas when the peak area PB from 122.0 to 126.2 ppm was set to 100, and then calculating PA / (PB-PC) x 100. The results are shown in Tables 1 and 2.

[0119] <Measurement conditions for nuclear magnetic resonance analysis (13C-solid NMR)> Nuclear magnetic resonance analysis (13C-solid NMR) was carried out under the following measurement conditions: Measurement mode: magic angle spinning Flip angle: 90 degrees Waiting time: 5.0 seconds Sample rotation speed: 15 Hz Window processing: exponential function Number of accumulations: 10,000

[0120] A test chloroprene polymer latex composition containing the above-mentioned chloroprene polymer-containing latex was prepared by the following method, and the composition was dip-molded to obtain a dip-molded product. The dip-molded product was then subjected to a heat-drying treatment to prepare a test dip-molded product, which was then evaluated.

[0121] <Preparation of Dip-Molded Articles> 100 parts by mass of the solid content of each chloroprene polymer was mixed with an aqueous dispersion, and water was further added to adjust the overall solid content of the blend to 30% by mass to prepare a test chloroprene polymer latex composition. The aqueous dispersion was prepared by mixing 2 parts by mass of two types of zinc oxide, 2 parts by mass of a butylated reaction product of p-cresol and dicyclopentadiene (trade name "Nocrac PBK", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 0.1 part by mass of a sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "Demol N", manufactured by Kao Corporation), and 11 parts by mass of water in a ceramic ball mill at 20°C for 16 hours. The obtained test chloroprene polymer latex composition contained, relative to 100 parts by mass of the solid content of the chloroprene polymer, 2 parts by mass of two types of zinc oxide, 2 parts by mass of a butylated reaction product of p-cresol and dicyclopentadiene (trade name "Nocrac PBK", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 0.1 part by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "Demol N", manufactured by Kao Corporation), and water.

[0122] A ceramic cylindrical mold (manufactured by Shinko Co., Ltd.) with an outer diameter of 50 mm was immersed for 1 second in a coagulation solution containing 62 parts by mass of water, 35 parts by mass of potassium nitrate tetrahydrate, and 3 parts by mass of calcium carbonate, and then removed. After drying for 3 minutes, the molded product was immersed for 2 minutes in the chloroprene polymer latex composition for testing prepared by the above-described procedure. The molded product was then washed with running water at 45°C for 1 minute and dried at 130°C for 30 minutes to prepare a dipping-molded film for testing.

[0123] (Film Thickness) Using a test piece thickness gauge (manufactured by Kobunshi Keiki Co., Ltd., product name: ASKER SDA-12), the thickness (film thickness) of the dip-molded film for evaluation of tensile properties was measured at three points in the center, and the minimum thickness was taken as the thickness of the dip-molded film for test. The results are shown in Tables 1 and 2.

[0124] (Measurement of Tensile Properties) Using dip-molded test films for evaluating tensile properties, the modulus at 500% elongation and the tensile strength at break were measured in accordance with JIS K 6251. Furthermore, the test chloroprene polymer latex compositions of each Example and Comparative Example were stored at 23°C for 6 months, and the modulus at 500% elongation was measured in accordance with JIS K 6251. The results are shown in Tables 1 and 2.

[0125] (Change in low-temperature hardness) The test dip-molded specimens were stored at −10° C. for 168 hours, and the change in low-temperature hardness was determined from the hardness of the test dip-molded specimens before and after storage. The results are shown in Table 1. Formula (2): ΔH=HB−HA In formula (2), HA represents the Shore hardness measured using a durometer type A in an environment at 23°C after the test dip-molded specimens before storage at −10°C for 168 hours were subjected to a heat treatment for crystallization at 70°C for 30 minutes, and then the test dip-molded specimens were stacked to a thickness of 6.00±0.20 mm; and HB represents the Shore hardness measured using a durometer type A in an environment at −10°C after the test dip-molded specimens before storage at −10°C for 168 hours were heat-treated for crystallization at 70°C for 30 minutes, and then further stored at −10°C for 168 hours, and then the test dip-molded specimens were stacked to a thickness of 6.00±0.20 mm.

[0126] (The ratio RB / RA of the total peak area RB of abietic acid, neoabietic acid, palustric acid, levopimaric acid, and their salts to the total peak area RA of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid, and their salts.) 3 g of the above-mentioned immersion-molded test specimen was cut into 2 mm square pieces to obtain test specimens. The test specimens were placed in an eggplant-shaped flask equipped with a condenser, extracted with an ethanol / toluene azeotropic mixture (ETA solution) specified in JIS K 6229, and then treated with hydrochloric acid. Gas chromatography was performed under the following conditions using the extract. From the gas chromatography measurement results, the total peak area RA of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid, and their salts was determined. In addition, the total amount RB of the peak areas of abietic acid, neoabietic acid, palustric acid, levopimaric acid, and their salts was determined, and the ratio RB / RA ((conjugated resin acid component b) / (non-conjugated resin acid component a)) of the total amount RB of the peak areas of abietic acid, neoabietic acid, palustric acid, levopimaric acid, and their salts to the total amount RA of the peak areas of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid, and their salts in the test dip-molded product was calculated.

[0127] [Gas chromatography measurement conditions] Column used: FFAP 0.32 mmφ×25 m (film thickness 0.3 μm) Detector: FID Column temperature: 200° C. (hold for 90 min) → 250° C. Heating rate: 10° C. / min Injection port temperature: 270° C. Detector temperature: 270° C. Injection volume: 2 μL

[0128]

[0129]

Claims

1. A chloroprene-based polymer containing chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units, wherein the chloroprene-based polymer contains 12 to 30% by mass of 2,3-dichloro-1,3-butadiene monomer units based on a total of 100% by mass of the chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units; the chloroprene-based polymer has a toluene-insoluble content of 60 to 87% by mass; a test chloroprene-based polymer latex composition containing the chloroprene-based polymer is formed by an immersion coagulation method and heat-dried at 130° C. for 30 minutes, and a low-temperature hardness change ΔH1 of a test immersion molded product obtained is 29 or less; the low-temperature hardness change ΔH1 is represented by HB1−HA1; HA1 represents the Shore hardness measured in an environment of 23° C. using a durometer type A after the test immersion molded product is heat-treated under the conditions of 70° C. for 30 minutes and the test immersion molded products are stacked to a thickness of 6.00±0.20 mm; HB1 represents the Shore hardness measured in an environment of −10° C. using a durometer type A after the test immersion molded product is heat-treated under the conditions of 70° C. for 30 minutes and further stored at −10° C. for 168 hours and the test immersion molded products are stacked to a thickness of 6.00±0.20 mm; and a ratio RB / RA of a total amount RB of peak areas of abietic acid, neoabietic acid, palustric acid, levopimaric acid and salts thereof to a total amount RA of peak areas of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid and salts thereof obtained from gas chromatography analysis of an extract extracted from the test immersion molded product with an ethanol / toluene azeotropic mixture specified in JIS K 6229 is 0.10 or more and 0.70 or less.

2. The chloroprene-based polymer according to claim 1, wherein in a 13C-solid NMR spectrum of the chloroprene-based polymer, when a peak area of 126.2 to 127.6 ppm is PA, a peak area of 1,22.0 to 126.2 ppm is PB, and a peak area of 129.9 to 130.3 ppm is PC, formula (1) is satisfied. Formula (1): 4.4≦PA / (PB−PC)×100≦5.0 3. A chloroprene-based polymer latex containing the chloroprene-based polymer according to claim 1 or 2 and water.

4. A dip-molded product of a chloroprene polymer latex composition containing the chloroprene polymer latex according to claim 3.

5. The dip-molded product according to claim 4, which is an industrial glove, a glove for general household use, a glove for medical use, a balloon, a catheter, or a boot.

6. A dip-molded product according to claim 4, wherein the low-temperature hardness change ΔH2 is 29 or less, and the low-temperature hardness change ΔH2 is expressed as HB2-HA2, where HA2 represents the Shore hardness measured in an environment of 23°C using a durometer type A after the dip-molded product has been heat-treated at 70°C for 30 minutes and then stacked to a thickness of 6.00±0.20 mm, and HB2 represents the Shore hardness measured in an environment of -10°C using a durometer type A after the dip-molded product has been heat-treated at 70°C for 30 minutes and then stored at -10°C for 168 hours and then stacked to a thickness of 6.00±0.20 mm.

7. A dip-molded product of a chloroprene polymer latex composition containing a chloroprene polymer, wherein the dip-molded product has a low-temperature hardness change ΔH2 of 29 or less, and the low-temperature hardness change ΔH2 is expressed as HB2-HA2, and HA2 represents the Shore hardness measured by stacking the dip-molded products to a thickness of 6.00±0.20 mm using a durometer type A in an environment of 23°C after heat-treating the dip-molded product under conditions of 70°C and 30 minutes, and HB2 represents the Shore hardness measured by stacking the dip-molded products to a thickness of 6.00±0.20 mm using a durometer type A in an environment of -10°C after heat-treating the dip-molded product under conditions of 70°C and 30 minutes and storing the dip-molded product at -10°C for 168 hours, and the dip-molded product is a dip-molded product having a low-temperature hardness change ΔH2 of 29 or less, and the low-temperature hardness change ΔH2 is expressed as HB2-HA2, and HA2 represents the Shore hardness measured by stacking the dip-molded products to a thickness of 6.00±0.20 mm using a durometer type A in an environment of -10°C after heat-treating the dip-molded product under conditions of 70°C and 30 minutes and storing the dip-molded product at -10°C for 168 hours, and The dip-molded product has a tensile strength at break of 20.0 MPa or more and a modulus at 500% elongation of 2.00 MPa or less, as measured in accordance with JIS No. 6251.