Geopolymer composition, geopolymer cured body, and production method for geopolymer cured body

MYPI2025004077A0Undetermined Publication Date: 2024-07-05SIKA TECH AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025004077
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-01-05
Filing Date
2023-12-27
Publication Date
2024-07-05

AI Technical Summary

Technical Problem

Existing geopolymer compositions face challenges in maintaining fluidity over a long period while reducing silica fume content to lower manufacturing costs, as silica fume is costly and its reduction affects both fluidity and short-term strength development, leading to difficulties in handling and achieving desired strength without increasing water content or using expensive steam curing.

Method used

A geopolymer composition that includes an active filler with a high percentage of pulverized blast furnace slag powder and coal ash, along with a polycondensate-based dispersant containing polyalkylene glycol monophenyl ether, and controlled water content, which allows for good fluidity and high strength development in a short period without silica fume or with minimal silica fume content.

Benefits of technology

The solution achieves both good fluidity over a long period and high strength development in a short period using a simple method, reducing manufacturing costs and eliminating the need for steam curing, while effectively utilizing industrial by-products like blast furnace slag powder and untreated coal ash.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025004077_DRAWING_001
    Figure PI2025004077_DRAWING_001
  • Figure PI2025004077_DRAWING_002
    Figure PI2025004077_DRAWING_002
Patent Text Reader

Abstract

The present invention provides a geopolymer composition capable of achieving both good fluidity over a long period of time and high strength development of a cured body in a short period of time by a simple technique while suppressing the mixing amount of silica fume. The geopolymer composition is a geopolymer composition containing an active filler, aggregate, an activator, a dispersant, and added water, wherein the geopolymer composition contains no silica fume or contains silica fume in an amount of less than 1 mass% based on a total mass of the geopolymer composition, a total moisture content of the geopolymer composition is from 10 mass% to 13 mass%, the active filler contains coal ash and 35 mass% or more of ground granulated blast-furnace slag based on the total mass of the active filler, and the dispersant is a polycondensate-based dispersant that contains polyalkylene glycol monophenyl ether as a substructure. Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Geopolymer composition, hardened geopolymer, and method for producing hardened geopolymer

[0001] The present invention relates to a geopolymer composition, a geopolymer hardened body which is a hardened product thereof, and a method for producing the same.

[0002] Hardened materials such as concrete, mortar, artificial stone, and hardened building materials generally contain cement. However, cement releases a large amount of CO when fired. 2 Therefore, methods for producing hardened materials such as concrete that do not use cement and are environmentally friendly are attracting attention. In particular, methods for producing hardened materials using the geopolymer method are being actively researched.

[0003] In the geopolymer method, powders containing silicon and aluminum as the main components are used as binders to bond the powders together to produce artificial rocks. The hardened geopolymer formed by the geopolymer method is produced by causing a geopolymer reaction using an activated filler as an aluminosilicate source and an alkaline aqueous solution as an activator. Activated fillers that can be used include natural products such as kaolin and clay, as well as fly ash, silica fume, blast furnace slag, and rice husk ash. The alkaline aqueous solution can be an aqueous solution of sodium hydroxide, water glass (sodium silicate), or the like.

[0004] The primary role of active fillers is to form a hardened geopolymer and improve its strength. Among active fillers, silica fume not only significantly contributes to short-term strength improvement of the hardened geopolymer, but also imparts good long-term fluidity to the geopolymer composition immediately after mixing. Therefore, silica fume is widely used in the production of hardened geopolymers due to its excellent workability. For example, Patent Document 1 describes a geopolymer composition containing ground granulated blast furnace slag and fly ash as powdered raw materials, fine aggregate, silica fume, potassium hydroxide or sodium hydroxide as an alkali source, and water, in which the volume ratio of ground granulated blast furnace slag to the powdered raw materials (BFS / P) is 35-80%, the molar ratio of silicon contained in the silica fume to the alkali source (Si / A) is 0.05-0.35, and the molar ratio of the alkali source to water (A / W) is 0.1-0.3.

[0005] Japanese Patent Application Laid-Open No. 2021-066613

[0006] The present invention aims to provide a geopolymer composition that can achieve both good fluidity over a long period of time and high strength of the hardened body in a short period of time using a simple method while reducing the amount of silica fume blended.

[0007] The present inventors have conducted extensive research to solve the above problems and have arrived at the present invention. That is, the present invention includes the following preferred embodiments.

[0008] A geopolymer composition according to a first aspect of the present invention is a geopolymer composition comprising an active filler, an aggregate, an activator, a dispersant, and added water, wherein the geopolymer composition does not contain silica fume or contains less than 1% by mass of silica fume relative to the total mass of the geopolymer composition, the total water content of the geopolymer composition is 10% to 13% by mass, the active filler comprises 35% by mass or more of ground granulated blast furnace slag and coal ash relative to the total mass of the active filler, and the dispersant is a polycondensate-based dispersant containing polyalkylene glycol monophenyl ether as a partial structure.

[0009] A hardened geopolymer according to a second aspect of the present invention is a hardened product of the geopolymer composition according to the first aspect described above.

[0010] A method for producing a hardened geopolymer according to a third aspect of the present invention includes a step of mixing and kneading the geopolymer composition according to the first aspect described above, and then hardening the mixture.

[0011] Figure 1 is a graph showing the fluidity test results of the geopolymer composition in the examples. Figure 2 is a graph showing the uniaxial compressive strength test results of the hardened geopolymer composition in the examples.

[0012] Silica fume is included as an active filler in most geopolymer compositions currently being manufactured and developed. The geopolymer composition described in Patent Document 1 also contains silica fume as an essential active filler component. However, silica fume has a higher material cost than other active fillers. Therefore, silica fume is a cause of the high cost when manufacturing hardened geopolymer compositions.

[0013] If no silica fume or only a small amount of silica fume is included in the geopolymer composition, the fluidity of the geopolymer composition immediately after mixing will decrease, and it will be difficult to obtain a hardened body with the desired strength in a short period of time.

[0014] If the fluidity of a geopolymer composition immediately after mixing decreases, handling of the geopolymer composition at the manufacturing site for the hardened product becomes difficult. One possible solution to this problem is to increase the amount of water contained in the activator or the amount of water added separately. However, increasing the total water content in the geopolymer composition can lead to problems such as the need for long-term curing to achieve the hardened product strength, bleeding in the composition or hardened product, or insufficient strength of the hardened product. Another possible solution is to replace conventional curing (water, wet, or air) with steam curing to achieve the desired strength in a shorter period of time. However, steam curing is expensive, significantly increasing production costs.

[0015] Thus, if the amount of silica fume in the geopolymer composition is reduced in order to reduce manufacturing costs, various problems arise in terms of both the fluidity of the composition immediately after mixing and the strength of the hardened body.

[0016] The inventors of the present invention have conducted extensive research into geopolymer compositions that can maintain high fluidity for a long period of time while minimizing the amount of silica fume used, and can produce high-strength hardened products in a short period of time using simple methods. They then focused on the type and amount of active filler and dispersant used in the geopolymer composition, as well as the total water content of the geopolymer composition, and completed the present invention.

[0017] According to the present invention, it is possible to provide a geopolymer composition that can achieve both good fluidity over a long period of time and high strength of the hardened body in a short period of time using a simple method while reducing the amount of silica fume blended.

[0018] Specifically, the geopolymer composition in this embodiment contains an active filler, an aggregate, an activator, a dispersant, and added water. The geopolymer composition does not contain silica fume or contains less than 1% by weight of silica fume relative to the total weight of the geopolymer composition. The dispersant is a polycondensate-based dispersant containing polyalkylene glycol monophenyl ether as a substructure. By including this specific type of dispersant in the geopolymer composition, the total water content of the geopolymer composition required to ensure high fluidity for a long period of time can be reduced, even if the silica fume content is 0% by weight or less than 1% by weight.

[0019] In addition, the geopolymer composition of this embodiment contains 35% by mass or more of ground granulated blast furnace slag as an active filler, based on the total mass of the active filler. As will be described in detail later, ground granulated blast furnace slag contributes significantly to improving the strength of the hardened body compared to other active fillers other than silica fume. Therefore, by including a large amount of ground granulated blast furnace slag, a high-strength hardened body can be obtained in a short period of time through normal curing, without complex processes such as steam curing. In other words, the geopolymer composition of this embodiment contains a specific type of dispersant, and the amount of ground granulated blast furnace slag as an active filler and the total moisture content of the composition are adjusted to an appropriate amount. As a result, even if the amount of silica fume, which causes cost increases, is reduced, favorable effects can be maintained in both the fluidity of the composition after kneading and the strength of the hardened body. Coal ash is also included as an active filler. As the coal ash, coal ash that has been subjected to special pretreatment to make its quality uniform (specifically, treatment to conform to the standard for fly ash for concrete specified in JIS A 6201: 2015) may be used. However, even if coal ash that has not been subjected to such special pretreatment is used as coal ash, the effect of the geopolymer composition according to this embodiment can be obtained.

[0020] As used herein, "water" refers to all water contained in the geopolymer composition of this embodiment, including water contained in the activator, water contained in the dispersant, optionally added water, and water contained in other materials. Furthermore, as used herein, "total water content" (mass%) refers to the total amount (mass%) of this "water" in the geopolymer composition of this embodiment. This "total water content" (mass%) can be calculated by using a moisture analyzer to determine the total solids content (mass%) of the water-containing components and subtracting this from the total solution volume (mass%), as described in the Examples below.

[0021] In this specification, "added water" refers to water that is added separately from the water contained in the activator, the water contained in the dispersant, and the water contained in other optional materials. Specifically, added water is added separately to the geopolymer composition of this embodiment for the purpose of adjusting the fluidity of the geopolymer composition, promoting the migration of various ions that contribute to the geopolymer reaction, etc. Examples of added water include, but are not limited to, tap water, ion-exchanged water, etc.

[0022] Hereinafter, embodiments of the present invention will be described in detail. Note that the scope of the present invention is not limited to the embodiments described here, and various modifications can be made without departing from the spirit of the present invention.

[0023] 1. Geopolymer Composition The geopolymer composition in this embodiment includes an active filler, an aggregate, an activator, a dispersant, and added water. The dispersant is a polycondensate-based dispersant containing polyalkylene glycol monophenyl ether as a partial structure.

[0024] In this embodiment, the aggregate contained in the geopolymer composition includes fine aggregate and / or coarse aggregate. That is, the geopolymer composition in this embodiment can be applied to both geopolymer mortar compositions containing fine aggregate but not coarse aggregate, and geopolymer concrete compositions containing fine aggregate and coarse aggregate.

[0025] The function of each component, its amount, the total water content of the geopolymer composition, and the method for preparing the geopolymer composition are described in detail below. The amounts and ratios of the components of the geopolymer composition described below primarily refer to the amounts and ratios when the geopolymer composition is used as a geopolymer mortar composition, unless otherwise specified. However, the amounts and ratios of the components can be adjusted as needed even when the geopolymer composition is used as a geopolymer concrete composition.

[0026] <Activated Filler> Activated filler is a powder containing aluminosilicate as its main component. Aluminosilicate is active against alkali. When an activator, added water, etc., described below, is added to the activated filler, the silicon and aluminum in the activated filler are partially dissolved or ionized. After dissolution, the silica component, which exists in a state close to a monomer in the alkaline silica solution, captures metal ions. As a result, a dehydration condensation reaction occurs, producing a hardened polymer compound (polymer), which becomes the hardened geopolymer composition.

[0027] In the geopolymer composition of this embodiment, the active filler is not particularly limited as long as it includes 35% by mass or more of ground granulated blast furnace slag and coal ash relative to the total mass of the active filler. The type of coal ash is not particularly limited, and coal ash that has not been treated to comply with the JIS A 6201:2015 standard for fly ash for concrete may be used, or coal ash that has been treated may be used. For example, the active filler may include, in addition to ground granulated blast furnace slag and coal ash, one or more of any active fillers known to those skilled in the art that have the above-mentioned functions. The geopolymer composition of this embodiment may also include silica fume as an active filler, but the amount of silica fume is less than 1% by mass relative to the total mass of the geopolymer composition. These active fillers are described in detail below.

[0028] (Coal ash) Coal ash is mainly composed of silicon dioxide (SiO 2 ), alumina (Al 2 O 3) and the like. As described above, in this embodiment, the type of coal ash is not particularly limited. Specifically, the coal ash may include coal ash produced as an industrial by-product that has not been treated to conform to the standard for fly ash for concrete specified in JIS A 6201:2015 (hereinafter also referred to as "untreated coal ash"), coal ash that has been subjected to such treatment, or a mixture of these coal ashes. Of these, the coal ash preferably includes untreated coal ash. Untreated coal ash refers to coal ash that has not been subjected to any treatment other than normal crushing for the purpose of transportation from the production site, or raw powder coal ash. Using untreated coal ash as an activated filler allows the industrial by-product coal ash to be efficiently and effectively utilized as a resource without being treated. Furthermore, production costs can be reduced. Such untreated coal ash can be obtained, for example, as an industrial by-product produced during coal combustion from thermal power plants, boilers, etc.

[0029] In this specification, "coal ash that has not been treated to conform to the standard for fly ash for concrete specified in JIS A 6201:2015" refers to coal ash that has not been subjected to a crushing treatment and / or particle size adjustment (preferably particle size adjustment). Alternatively, for example, "coal ash that has not been treated to conform to the standard for fly ash for concrete specified in JIS A 6201:2015" refers to coal ash that has not been subjected to a crushing treatment and / or particle size adjustment (preferably particle size adjustment). 2 / g to 6000 cm 2The coal ash has a Blaine specific surface area of ​​about 1 / g and has not been subjected to pulverization and / or particle size adjustment (preferably particle size adjustment). Alternatively, for example, "coal ash that has not been treated to conform to the standard for fly ash for concrete specified in JIS A 6201:2015" is, in other words, preferably coal ash (untreated coal ash) produced as an industrial by-product from at least one of a thermal power plant and a boiler. Note that, in one embodiment, "coal ash that has not been treated to conform to the standard for fly ash for concrete specified in JIS A 6201:2015" may be coal ash that does not conform to the standard for fly ash for concrete specified in JIS A 6201:2015, or may include coal ash that does not conform to the standard.

[0030] Specifically, coal ash, preferably untreated coal ash, includes, for example, fly ash captured from flue gas by a dust collector, bottom ash obtained by pulverizing lumps of ash at the bottom of a boiler, etc. Coal ash, preferably untreated coal ash, may be used in combination of two or more types of coal ash.

[0031] The geopolymer composition of this embodiment can achieve the effects of high fluidity of the geopolymer composition itself over a long period of time and high strength of the hardened body in a short period of time. In particular, the same effects can be achieved even when untreated coal ash is used as an active filler. In other words, the above-mentioned effects can be achieved even when the size, composition, etc. of the coal ash used are not uniform and the quality varies to some extent.

[0032] The amount of coal ash relative to the total mass of the activated filler is not particularly limited as long as it satisfies the conditions for the amount of ground granulated blast furnace slag described below. For example, the amount of coal ash is preferably 3% to 65% by mass relative to the total mass of the activated filler. Even when the coal ash contains untreated coal ash, the amount of untreated coal ash relative to the total mass of the activated filler is preferably 3% to 65% by mass. When the amount of untreated coal ash is 3% by mass or more, untreated coal ash generated as an industrial by-product can be effectively utilized as a resource, resulting in a geopolymer composition that is environmentally and cost-effectively suitable. Furthermore, when the amount of untreated coal ash is 65% by mass or less, the amount of ground granulated blast furnace slag is not insufficient, and a hardened body with the desired high strength can be obtained in a short period of time.

[0033] The amount of coal ash relative to the total mass of the activated filler is more preferably 23% by mass or more, and even more preferably 50% by mass or more. Even when the coal ash contains untreated coal ash, the amount of untreated coal ash relative to the total mass of the activated filler is more preferably 23% by mass or more, and even more preferably 50% by mass or more. When the coal ash contains both untreated coal ash and coal ash that has been treated to comply with the JIS A 6201:2015 fly ash standard for concrete as the activated filler, the amount of the treated coal ash is preferably, for example, about 5% by mass relative to the total mass of the activated filler.

[0034] (Ground granulated blast furnace slag) Ground granulated blast furnace slag contains calcium oxide (CaO), silicon dioxide (SiO 2 ), alumina (Al 2 O 3 ) etc.

[0035] Any ground granulated blast furnace slag known to those skilled in the art can be used as the ground granulated blast furnace slag. For example, ground granulated blast furnace slag can be obtained by pulverizing granulated blast furnace slag. Granulated blast furnace slag is obtained as a by-product when refining iron in a blast furnace. Alternatively, commercially available ground granulated blast furnace slag may be used. For example, commercially available ground granulated blast furnace slag that meets the JIS A 6206 Ground Granulated Blast Furnace Slag 4000 standard can be used. Such commercially available ground granulated blast furnace slag includes, for example, "K-MENT" sold by Kobe Steel Slag Products Co., Ltd. and "ESMENT" manufactured by Nippon Steel Blast Furnace Cement Co., Ltd.

[0036] In the geopolymer composition of this embodiment, the amount of ground granulated blast furnace slag relative to the total mass of the active filler is 35% by mass or more. By using 35% by mass or more of ground granulated blast furnace slag, the impact on the strength of the hardened body caused by reducing the amount of silica fume can be compensated for. As a result, even with a simple method, high strength of the hardened body can be achieved in a short period of time. Furthermore, industrial by-products can be effectively utilized as resources, resulting in a geopolymer composition that is environmentally and cost-effective.

[0037] The amount of ground granulated blast furnace slag mixed relative to the total mass of the active filler is preferably 36 mass % or more, and more preferably 37 mass % or more.

[0038] The present inventors have confirmed that increasing the blend ratio of ground granulated blast furnace slag to the total amount of active filler can improve the strength of the hardened body compared to increasing the blend ratio of other types of active filler, such as coal ash (preferably untreated coal ash). Experiments by the present inventors have shown that this is not due to differences in the structure of the final hardened body. More specifically, the present inventors used geopolymer compositions containing different blend ratios of coal ash (preferably untreated coal ash) and ground granulated blast furnace slag, and compared the structure around the Si atoms of hardened bodies containing a higher amount of ground granulated blast furnace slag powder with that containing a higher amount of coal ash (preferably untreated coal ash) by NMR analysis. The results showed no differences in the peak position or width of the spectra. However, the peak intensity of the spectrum was higher for hardened bodies containing a higher amount of ground granulated blast furnace slag powder. Therefore, it was found that changing the blend ratio of coal ash and ground granulated blast furnace slag powder produced hardened bodies with similar structures, but the amounts of the products differed.

[0039] From these results, it is predicted that the reason why ground granulated blast furnace slag has a greater effect on the strength of the hardened body is because ground granulated blast furnace slag is more reactive than other types of active fillers such as coal ash (preferably untreated coal ash). This prediction can be estimated, for example, from the vitrification rate, which can be one indicator of reactivity. Specifically, the vitrification rate of commonly used ground granulated blast furnace slag is 99%, while the vitrification rate of coal ash (preferably untreated coal ash) is approximately 70% to 80%. Therefore, the vitrification rate of the ground granulated blast furnace slag contained in the geopolymer composition of this embodiment is preferably 99% or more, and the vitrification rate of coal ash (preferably untreated coal ash) is preferably 70% to 80%.

[0040] The upper limit of the amount of ground granulated blast furnace slag relative to the total mass of the active filler is not particularly limited. For example, the amount of ground granulated blast furnace slag may be 100%. The amount of ground granulated blast furnace slag relative to the total mass of the active filler is preferably 77% by mass or less, more preferably 50% by mass or less. By setting the amount of ground granulated blast furnace slag to 77% by mass or less, excessive early strengthening of the geopolymer composition can be prevented.

[0041] (Silica fume) Silica fume is a material that contains silicon dioxide (SiO 2 Specifically, silica fume is a highly pure silicon dioxide (SiO 2 ) amorphous spherical fine particles.

[0042] Any silica fume known to those skilled in the art can be used. For example, silica fume can be obtained as a by-product of collecting dust in exhaust gas generated during the production of ferrosilicon, metallic silicon, electrolytic zirconia, etc. Commercially available silica fume may also be used.

[0043] Silica fume not only functions as a typical active filler, i.e., it initiates the dehydration condensation polymerization reaction, which leads to improved strength of the hardened body, but also enhances the fluidity of the prepared geopolymer composition. This is due to the spherical shape of silica fume.

[0044] The geopolymer composition of this embodiment does not contain silica fume or contains less than 1% by mass of silica fume relative to the total mass of the geopolymer composition. By using less than 1% by mass of silica fume, the manufacturing cost of the geopolymer composition can be reduced. Furthermore, the geopolymer composition of this embodiment can reduce the amount of silica fume used while more effectively utilizing industrial by-products such as ground granulated blast furnace slag (and untreated coal ash) as a substitute. This allows for a geopolymer composition that is favorable from both an environmental and cost perspective.

[0045] The amount of silica fume relative to the total mass of the geopolymer composition is preferably 0.5% by mass or less, more preferably 0.1% by mass or less. In particular, it is more preferable that the geopolymer composition in this embodiment does not contain silica fume.

[0046] (Other active fillers) Other active fillers that can be included in the geopolymer composition of this embodiment include, for example, red mud, feldspars, micas, zeolites, perlite, clay minerals, kaolin, metakaolin, sewage sludge, and the like.

[0047] The total amount (mass%) of active filler relative to the total mass of the geopolymer composition can be determined by the ratio to the amount of activator in the geopolymer composition. Specifically, when using an alkaline aqueous solution of, for example, about 8 mol / L to 10 mol / L as the activator, the ratio of the amount of activator to the total amount of active filler (i.e., activator (mass) / active filler (total mass)) is preferably 5% to 30%. In this case, if the activator (mass) / active filler (total mass) ratio is 5% or more, the dehydration condensation reaction of the active filler can be sufficiently generated, and ultimately, a geopolymer hardened body with sufficient strength can be obtained. In addition, in this case, if the activator (mass) / active filler (total mass) ratio is 30% or less, false setting due to excessive amounts of activator can be prevented.

[0048] Likewise, in this case, the activator (mass) / active filler (total mass) ratio is preferably 10% or more, and more preferably 15% or more, and more preferably 25% or less, and even more preferably 20% or less.

[0049] The above-mentioned preferable ratio varies somewhat depending on the type and concentration of the activator, but the activator (mass) / active filler (total mass) may be adjusted appropriately within a range in which the active filler reacts sufficiently and no false coagulation occurs.

[0050] In addition, the total amount (mass%) of active filler relative to the total mass of the geopolymer composition varies depending on the type of geopolymer hardened body, which is the final product. Therefore, the total amount of active filler can be adjusted appropriately to suit the type of desired geopolymer hardened body. For example, the total amount of active filler is approximately 20% to 60% by mass relative to the total mass of the geopolymer composition. Examples of types of geopolymer hardened bodies include mortar and concrete, as mentioned above.

[0051] <Aggregate> Any aggregate known to those skilled in the art can be used as the aggregate. For example, commonly known aggregates used in the production of concrete, mortar, artificial stone, etc. can be used.

[0052] The aggregate may be either coarse or fine aggregate. At least 85% of the coarse aggregate has a diameter of 5 mm or more. At least 85% of the fine aggregate has a diameter of 5 mm or less. The type of aggregate may be selected appropriately depending on the intended use of the final product, the hardened geopolymer body. For example, two or more types of aggregate, such as a combination of coarse and fine aggregates, may be used.

[0053] Examples of fine aggregate include blast furnace slag fine aggregate and fine aggregate such as general silica sand, which is a natural aggregate. Of these, it is preferable to use blast furnace slag fine aggregate. Blast furnace slag fine aggregate has latent hydraulic properties. The latent hydraulic properties are due to the silicon dioxide (SiO 2 ), alumina (Al 2 O 3 ) and other factors, which produces hydrates, which increases the strength of the hardened material. Therefore, by using blast furnace slag fine aggregate as an aggregate, the long-term strength of the final product, the hardened geopolymer, can be increased.

[0054] Blast furnace slag fine aggregate is specified in JIS A 5011-1:2018. Alternatively, commercially available blast furnace slag fine aggregate may be used. Examples of commercially available blast furnace slag fine aggregate include "Shinko Sand" sold by Kobelco Slag Products Co., Ltd. and blast furnace slag fine aggregate manufactured by JFE Mineral Co., Ltd.

[0055] As the coarse aggregate, it is preferable to use blast furnace slag coarse aggregate made from blast furnace slag. When blast furnace slag coarse aggregate and / or the above-mentioned blast furnace slag fine aggregate are used as the aggregate, industrial by-products can be effectively utilized as resources, and a highly environmentally friendly geopolymer composition can be obtained. Furthermore, production costs can be reduced.

[0056] The amount of aggregate (preferably fine aggregate) relative to the total mass of the geopolymer composition is not particularly limited and may be adjusted according to the intended use of the hardened geopolymer body, which is the final product. For example, the amount of aggregate (preferably fine aggregate) relative to the total mass of the geopolymer composition is preferably 30% to 70% by mass. When the amount of aggregate (preferably fine aggregate) is 30% by mass or more, separation of the aggregate and the geopolymer composition paste can be prevented, making it easier to form a uniform hardened body. When the amount of aggregate (preferably fine aggregate) is 70% by mass or less, it becomes easier to maintain good fluidity of the geopolymer composition over a long period of time.

[0057] The amount of aggregate (preferably fine aggregate) relative to the total mass of the geopolymer composition is preferably 40% by mass or more, and even more preferably 50% by mass or more. The amount of aggregate (preferably fine aggregate) relative to the total mass of the geopolymer composition is preferably 65% ​​by mass or less, and even more preferably 60% by mass or less.

[0058] <Added water> The type of added water is not particularly limited, and examples include tap water, ion-exchanged water, etc. Furthermore, the pH, temperature, etc. of the added water are also optional, and can be adjusted to general values ​​as appropriate according to the types and amounts of each component contained in the geopolymer composition.

[0059] The added water contributes to the fluidity of the geopolymer composition. The geopolymer composition in this embodiment contains a specific type of dispersant that significantly increases the fluidity of the composition, as described below. Therefore, the amount of added water can be very small.

[0060] On the other hand, in the geopolymer composition of this embodiment, because the amount of silica fume is reduced, the total water content must be adjusted to 10% to 13% by mass, as described in detail below. Therefore, the amount of added water relative to the total mass of the geopolymer composition must be appropriately adjusted so that the total water content is within the range of 10% to 13% by mass, depending on the amount of water (% by mass) contained in the activator and the amount of water (% by mass) contained in the dispersant. Specifically, the amount of added water relative to the total mass of the geopolymer composition is preferably 4.5% by mass or more, more preferably 5% by mass or more, and even more preferably 6% by mass or more. Furthermore, the amount of added water is preferably 7.8% by mass or less, more preferably 7.6% by mass or less, and even more preferably 7.3% by mass or less.

[0061] <Activator> The activator is a component that initiates polymerization by a dehydration condensation reaction of the activated filler. Specifically, the activator is an aqueous alkaline solution that comes into contact with the aluminosilicate in the activated filler and dissolves silicon and aluminum. The activator is not particularly limited as long as it is a commonly used activator, and for example, an aqueous solution of sodium hydroxide, water glass (sodium silicate), potassium silicate, etc. can be used. Alternatively, a commercially available activator containing an alkali source may be used as the activator. Examples of such commercially available activators include the Mastercrete AC series manufactured by Pozzolith Solutions.

[0062] The concentration of the alkaline aqueous solution serving as the activator must be adjusted appropriately depending on the type and amount of the activator, but is preferably 6 mol / L to 12 mol / L, for example. When the activator concentration is 6 mol / L or higher, the dehydration condensation reaction in the activated filler can be sufficiently induced. When the activator concentration is 12 mol / L or lower, the generation of excessive heat of fusion due to high concentrations can be avoided.

[0063] The concentration of the aqueous alkaline solution serving as the activator must be adjusted appropriately depending on the type and amount of the activator, but is preferably 7 mol / L or more, and more preferably 8 mol / L or more.The concentration of the aqueous alkaline solution serving as the activator must be adjusted appropriately depending on the type and amount of the activator, but is more preferably 11 mol / L or less, and more preferably 10 mol / L or less.

[0064] The amount of activator (mass%) relative to the total mass of the geopolymer composition can be determined in the same manner as described above from the ratio to the total amount (mass%) of active filler in the geopolymer composition.

[0065] At the same time, the amount of water (mass%) contained in the activator can be appropriately adjusted depending on the amount of added water (mass%) and the amount of water (mass%) contained in the dispersant so that the total water content is within the range of 10 mass% to 13 mass%.

[0066] <Dispersant> The geopolymer composition in this embodiment contains a polycondensate-based dispersant containing polyalkylene glycol monophenyl ether as a partial structure. Specifically, this dispersant is a polycondensate-based dispersant containing polyalkylene glycol monophenyl ether as a partial structure in the state of an aqueous solution (in this specification, even in the state of an aqueous solution, it is also simply referred to as "dispersant").

[0067] The inclusion of this dispersant in the geopolymer composition disperses particles in the geopolymer composition, slowing the curing reaction of the composition. In addition, the curing reaction retardation effect of this dispersant disappears within a few hours. Therefore, when the geopolymer composition contains this dispersant, it can achieve both high fluidity over a long period of time and high strength development in a short period of time.

[0068] In this specification, the term "polycondensate dispersant containing polyalkylene glycol monophenyl ether as a partial structure (specifically, a polycondensate dispersant in the state of an aqueous solution containing polyalkylene glycol monophenyl ether as a partial structure)" is not particularly limited as long as it is an aqueous solution of a polymer having the above-mentioned action and a specified structure. Examples of such dispersants include aqueous solutions of polymers containing polycondensates containing the following structural units A, B, C, and D.

[0069] Structural unit A: At least one polyethylene glycol monophenyl ether represented by the following formula (1). [wherein, m is an integer of 3 to 280]

[0070] Structural unit B: a cyclic compound having at least one hydroxyl group and a derivative thereof, for example, at least one aromatic compound selected from the group consisting of benzene-1,2-diol, benzene-1,2,3-triol, 2-hydroxybenzoic acid, 2,3-dihydroxybenzoic acid, 3,4-dihydroxybenzoic acid, 3,4,5-trihydroxybenzoic acid, 3-hydroxyphthalic acid, 2,3-dihydroxybenzenesulfonic acid, 3,4-dihydroxybenzenesulfonic acid, 1,2-dihydroxynaphthalene, 2,3-dihydroxynaphthalene, 1,2-dihydroxynaphthalene-5-sulfonic acid, 1,2-dihydroxynaphthalene-6-sulfonic acid, 2,3-dihydroxynaphthalene-5-sulfonic acid, 2,3-dihydroxynaphthalene-6-sulfonic acid, and mixtures thereof.

[0071] Structural unit C: phenol, polyethylene glycol monophenyl ether having 1 or 2 ethylene oxide repeating units, or a phenoxyethyl derivative containing a phosphate or phosphonate, such as at least one other aromatic compound selected from the group consisting of phenol, 2-phenoxyethanol, 2-phenoxyethyl phosphate, 2-phenoxyethyl phosphonate, 2-phenoxyacetic acid, 2-(2-phenoxyethoxy)ethanol, 2-(2-phenoxyethoxy)ethyl phosphate, 2-(2-phenoxyethoxy)ethyl phosphonate, 2-[4-(2-hydroxyethoxy)phenoxy]ethyl phosphate, 2-[4-(2-hydroxyethoxy)phenoxy]ethyl phosphonate, 2-[4-(2-phosphonatooxyethoxy)phenoxy]ethyl phosphate, 2-[4-(2-phosphonatooxyethoxy)phenoxy]ethyl phosphonate, methoxyphenol, and mixtures thereof.

[0072] Structural unit D: aldehydes, for example, at least one aldehyde selected from the group consisting of formaldehyde, paraformaldehyde, glyoxylic acid, benzaldehyde, benzaldehyde sulfonic acid, benzaldehyde disulfonic acid, vanillin, isovanillin, and mixtures thereof.

[0073] The amount (mass%) of dispersant (aqueous solution) relative to the total mass of the geopolymer composition is adjusted appropriately depending on the type, concentration, etc., but is preferably 0.5% to 3.5% by mass. When the amount (mass%) of dispersant (aqueous solution) is 0.5% by mass or more, the above-mentioned dispersant's action can be effectively exerted, more reliably achieving both high fluidity over a long period of time and high strength in a short period of time. When the amount (mass%) of dispersant (aqueous solution) is 3.5% by mass or less, separation and bleeding of the geopolymer composition due to the addition of excessive dispersant can be suppressed.

[0074] The amount (mass%) of the dispersant (aqueous solution) relative to the total mass of the geopolymer composition is preferably 0.8% by mass or more, more preferably 0.85% by mass or more. The amount (mass%) of the dispersant (aqueous solution) is preferably 2.5% by mass or less, more preferably 2.0% by mass or less.

[0075] The concentration of the dispersant (aqueous solution concentration) and its blending amount (mass%) can be adjusted appropriately so that the total water content of the geopolymer composition in this embodiment is within the range of 10% to 13% by mass. In other words, the amount of water (mass%) contained in the dispersant can be adjusted appropriately so that the total water content is within the range of 10% to 13% by mass depending on the blending amount (mass%) of added water and the amount (mass%) of water contained in the activator.

[0076] <Other Materials> The geopolymer composition in this embodiment may contain any material that can be generally added as a raw material for mortar, concrete, etc., as long as it does not impair the effects of improving fluidity and strength. For example, it may contain an inert filler, which is a powder that is not active against alkali, various additives, etc. Examples of inert fillers include cement and calcium carbonate. The various additives are not particularly limited, but include conventionally known components such as fluidizers, shrinkage reducing agents, rust inhibitors, waterproofing agents, antifoaming agents, dust reducing agents, and pigments.

[0077] <Total Water Content of Geopolymer Composition> The total water content of the geopolymer composition in this embodiment is 10% by mass to 13% by mass. By setting the total water content to 10% by mass or more, it is possible to compensate for the impact on the fluidity of the composition caused by reducing the amount of silica fume blended. As a result, the geopolymer composition can maintain good fluidity for a long period of time. By setting the total water content to 13% by mass or less, it is possible to reduce the occurrence of bleeding, and it is possible to obtain a hardened body with the desired high strength in a short period of time.

[0078] The total water content is preferably 10.5% by mass or more, more preferably 11% by mass or more, even more preferably 11.5% by mass or more, and particularly preferably 11.8% by mass or more, and is preferably 12.8% by mass or less, more preferably 12.5% ​​by mass or less, and even more preferably 12.3% by mass or less.

[0079] As mentioned above, the total water content of the geopolymer composition can be adjusted to a range of 10% to 13% by weight by adjusting the amount of added water (% by weight), the amount of water contained in the activator (% by weight), and the amount of water contained in the dispersant (% by weight). In particular, the total water content can be easily adjusted within this range by appropriately varying the amount of added water (% by weight).

[0080] <Method for Preparing Geopolymer Composition> The geopolymer composition of this embodiment can be prepared by any method known to those skilled in the art. For example, the method for preparing the geopolymer composition includes a powder mixing step and a subsequent kneading step. In the powder mixing step, the main powder raw material, an activated filler (for example, an activated filler including coal ash (preferably including untreated coal ash) and ground granulated blast furnace slag) and aggregate are mixed in a predetermined blending amount. In the subsequent kneading step, water, an activator, and a dispersant are further added to the powder mixture in predetermined blending amounts, and the mixture is mixed and kneaded. The mixing and kneading methods are not particularly limited, and any method known to those skilled in the art using a mixer or the like may be used.

[0081] In addition, in the method for preparing the geopolymer composition described above, a powder mixture containing the main powder raw material, an active filler (for example, an active filler containing coal ash (preferably untreated coal ash) and blast furnace slag powder), and aggregate in a predetermined blending amount can be prepared in advance, and the prepared powder mixture can be used as a premixed geopolymer composition. Specifically, before construction, work, etc., water, an activator, and a dispersant are added to the premixed geopolymer composition in a predetermined blending amount, and then mixed and kneaded. This allows any desired amount of geopolymer composition to be easily prepared on site.

[0082] The geopolymer composition of this embodiment can achieve both good fluidity over a long period of time and high strength in a hardened body in a short period of time using a simple method. Ensuring good fluidity over a long period of time allows the geopolymer composition to be easily handled at the manufacturing site of hardened products. The ability to achieve high strength in a hardened body in a short period of time using a simple method means that hardened bodies of equivalent strength can be obtained using conventional curing methods, such as air curing or sealing, without the need for long-term curing or expensive steam curing. Additionally, the geopolymer composition of this embodiment can efficiently and effectively utilize granulated blast furnace slag, an industrial by-product, while reducing the amount of silica fume that causes cost increases. This is advantageous from the perspectives of reducing production costs and environmental impact.

[0083] 2. Hardened Geopolymer and Manufacturing Method Thereof The hardened geopolymer in this embodiment is a hardened product of the geopolymer composition in the previous embodiment. The hardened geopolymer has any shape that can be formed by any molding method, construction method, etc. Briefly, as described above, such hardened geopolymer can be manufactured by a method including mixing and kneading the geopolymer composition in the previous embodiment, followed by hardening. Specifically, the hardened geopolymer can be manufactured by the following method. First, the mixed, kneaded, and prepared geopolymer composition is molded or constructed using any method known to those skilled in the art, such as molding using a formwork, troweling in plastering work, spraying, or pasting. Then, the molded or constructed geopolymer composition can be subjected to conventional curing, such as air curing or sealing, without the need for complex processes such as steam curing, to produce a high-strength hardened geopolymer in a short period of time.

[0084] In addition, when producing a hardened geopolymer body using a formwork from the geopolymer composition in the above-described embodiment, it is preferable to apply a release agent or the like to the formwork in advance. The release agent is not particularly limited as long as it is any release agent known to those skilled in the art that imparts release properties to the hardened geopolymer composition (i.e., the hardened geopolymer body).

[0085] The geopolymer hardened body in this embodiment is not particularly limited, but includes, for example, road or bank blocks, blocks for storm water channels or irrigation channels, tiles, bricks, sewer pipes, piles, poles, precast products such as sleepers, cast-in-place concrete, sprayed concrete, concrete repair, dam concrete, and other cast-in-place products.

[0086] As described above, this specification discloses various aspects of the technology, the main aspects of which are summarized below.

[0087] A geopolymer composition according to a first aspect of the present invention is a geopolymer composition comprising an active filler, an aggregate, an activator, a dispersant, and added water, wherein the geopolymer composition does not contain silica fume or contains less than 1% by mass of silica fume relative to the total mass of the geopolymer composition, the total water content of the geopolymer composition is 10% to 13% by mass, the active filler comprises 35% by mass or more of ground granulated blast furnace slag and coal ash relative to the total mass of the active filler, and the dispersant is a polycondensate-based dispersant containing polyalkylene glycol monophenyl ether as a partial structure.

[0088] In the above geopolymer composition, it is preferred that the geopolymer composition does not contain silica fume.

[0089] A hardened geopolymer according to a second aspect of the present invention is a hardened product of the geopolymer composition according to the first aspect described above.

[0090] A method for producing a hardened geopolymer according to a third aspect of the present invention includes a step of mixing and kneading the geopolymer composition according to the first aspect described above, and then hardening the mixture.

[0091] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to these examples in any way.

[0092] In this example, various geopolymer compositions were actually prepared by changing the blending ratio of raw materials, and the geopolymer compositions were evaluated (flowability test of geopolymer composition, bleeding test of geopolymer composition, and uniaxial compressive strength test of hardened geopolymer composition).

[0093] 1. Preparation of Geopolymer Compositions The raw materials and preparation methods of the geopolymer compositions of the Examples and Comparative Examples are described in detail below.

[0094] [Raw materials for geopolymer composition] The raw materials for the geopolymer composition used in the examples and comparative examples are as follows. Coal ash (untreated coal ash): Coal ash, an industrial by-product collected at thermal power plants, was used as is. Specifically, a mixture of fly ash captured by an electrostatic precipitator and bottom ash that had adhered and grown inside a boiler and was then crushed by a crusher was used. In other words, untreated coal ash was used as is without undergoing strict pretreatment to make the quality uniform (in other words, treatment to conform to the standard for fly ash for concrete specified in JIS A 6201:2015). Blast furnace slag ground powder: "K-MENT" (specific surface area 4700 cm), manufactured by Kobe Steel Slag Products Co., Ltd. 2 / g) Silica fume: "Mastercrete SF 5000" manufactured by Pozzolith Solutions, bulk density: 2.2 g / cm 3 Aggregate (fine blast furnace slag aggregate): Shinko Sand manufactured by Kobelco Slag Products Co., Ltd. (maximum particle size 2.5 mm, sieve passing mass fraction 55% when the nominal sieve size is 0.6 mm) Added water: tap water Activator (aqueous solution): Mastercrete AC 5025 manufactured by Pozzolith Solutions Dispersant (aqueous solution): aqueous solution of the compound described in Example 5 of Japanese Patent No. 6290176 (This aqueous solution of the compound can be produced by the following method. First, 300 parts by weight of poly(ethylene oxide) monophenyl ether (average molecular weight 2000 g / mol), 46.2 parts by weight of 3,4-dihydroxybenzoic acid, 33 parts by weight of 2-phenoxyethyl phosphate, and 19.9 parts by weight of paraformaldehyde are added to a heatable reactor equipped with a stirrer and a metering pump. The mixture is charged under nitrogen at 90°C. The reaction mixture is then heated to 110°C with stirring, and 41 parts by weight of methanesulfonic acid (70%) is then added within 25 minutes, ensuring that the reaction temperature does not exceed 115°C. After metering, the reaction mixture is stirred at 110°C for a further 2.5 hours. The reaction mixture is then cooled and mixed with 350 parts by weight of water, and the mixture is heated at 100°C for 30 minutes. Finally, the mixture is neutralized with 50% caustic soda solution to a pH of approximately 7.0.

[0095] [Method for preparing geopolymer compositions] The raw materials shown in Table 1 below were blended in the respective mass % (relative to the total mass of the composition) to prepare the geopolymer compositions in Examples 1 and 2 and Comparative Examples 1 to 4. Specifically, first, coal ash (untreated coal ash) and blast furnace slag ground powder were mixed as active fillers in the respective blending amounts shown in Table 1 below. In Comparative Example 1, silica fume was also added as an active filler and mixed. Next, blast furnace slag fine aggregate was further added as aggregate to this mixed powder and mixed. Finally, tap water, an activator (aqueous solution), and a dispersant (aqueous solution) were added as additive water to the mixture in the respective blending amounts, and mixed using a Hobart mixer.

[0096] The total water content in the geopolymer composition was calculated by adding the amount of tap water (% by mass) used as added water, the amount of water (% by mass) contained in the activator, and the amount of water (% by mass) contained in the dispersant. The amount of water (% by mass) contained in the activator and the dispersant was determined by subtracting the solid content (% by mass) of each from the amount (% by mass) of the aqueous solution of the activator or dispersant, respectively. The solid content (% by mass) was determined by evaporating to dryness at 110°C for approximately 15 minutes using an A&D Moisture Analyzer ("MX-50").

[0097]

[0098] 2. Evaluation of Geopolymer Compositions Using each geopolymer composition prepared as described above, a fluidity test, a bleeding test, and a uniaxial compressive strength test of the hardened geopolymer composition were performed. The test methods and test results are described in detail below.

[0099] [Fluidity test of geopolymer composition] The fluidity of the geopolymer composition was measured in accordance with the flow test specified in JIS R 5201:2015 (Physical test method for cement). However, the flow test was performed without tamping.

[0100] [Geopolymer Composition Bleeding Test] The geopolymer composition bleeding test was performed as follows. After kneading the raw materials of the geopolymer composition with a total volume of 1.5 L, the kneaded composition was left for 1 hour. After 1 hour, the water floating on the surface of the left-standing composition was extracted with a dropper. Then, the volume of the extracted water was measured using a measuring cylinder, and the degree of bleeding was evaluated.

[0101] The fluidity (mm) measurement results and bleeding test results for the geopolymer composition at each elapsed time (min) are summarized in Table 2 below. Furthermore, the graph in Figure 1 shows the fluidity test results for the geopolymer composition shown in Table 2 below. In Figure 1, the target fluidity is 200 mm, which is the standard of fluidity generally desired for geopolymer compositions.

[0102]

[0103] [Uniaxial compressive strength test of hardened geopolymer composition] The uniaxial compressive strength of the hardened geopolymer composition was measured by the following method. Each prepared geopolymer composition was placed in a cylindrical mold with a diameter of 5 cm and a height of 10 cm, and the molded product was sealed and cured until the age shown in Table 2 below. After demolding, the uniaxial compressive strength of the molded product was measured in accordance with JIS A 1108:2018.

[0104] The results of the unconfined compressive strength test at each age (strength measurement date) are shown in Table 3 below. Furthermore, the graph in Figure 2 shows the unconfined compressive strength test results for the cured geopolymer composition shown in Table 3 below. The target strength in Figure 2 is 18 MPa, which is the standard for high strength generally desired for cured geopolymer compositions.

[0105]

[0106] [Discussion] As shown in Table 1 above, the geopolymer composition of Comparative Example 1 contains a large amount of silica fume. Therefore, as shown in Tables 2 and 3 above and Figures 1 and 2, the geopolymer composition of Comparative Example 1 exceeded the target fluidity of 200 mm except at the 5-minute mark, no bleeding occurred, and the strength of the hardened product exceeded the target strength by 28 days. However, since the geopolymer composition of Comparative Example 1 contains a large amount of expensive silica fume, producing various hardened products using such a geopolymer composition increases production costs. In addition, it would be preferable if the geopolymer composition had better fluidity.

[0107] The geopolymer composition of Comparative Example 2 does not contain silica fume compared to the geopolymer composition of Comparative Example 1, and there is no significant difference in the blending ratio of other components. Specifically, the blending ratio of ground granulated blast furnace slag in the active filler and the total moisture content in the geopolymer composition of Comparative Example 2 are generally similar to those of the geopolymer composition of Comparative Example 1. However, the geopolymer composition of Comparative Example 2 was unable to reach the target fluidity of 200 mm, and the strength of the cured product also failed to reach the target strength.

[0108] On the other hand, the geopolymer compositions of Examples 1 and 2, like the geopolymer composition of Comparative Example 2, do not contain silica fume. However, as shown in Tables 2 and 3 and Figures 1 and 2 above, the geopolymer compositions of Examples 1 and 2 far exceeded the target fluidity of 200 mm over a long period of time, no bleeding occurred, and the strength of the cured product exceeded the target strength by 28 days. In particular, the fluidity of the geopolymer compositions of Examples 1 and 2 exceeded 300 mm over a long period of time, which was unexpectedly significantly superior even when compared to the conventional geopolymer composition of Comparative Example 1, which contains a high amount of silica fume. This is presumably because the geopolymer compositions of Examples 1 and 2 contain a specific type of dispersant, have a high proportion of blast furnace slag powder in the active filler, and have an appropriate total moisture content.

[0109] That is, in the above-mentioned Comparative Example 2, the silica fume content was not as high as in Comparative Example 1, and in addition, the mixing ratio of the ground granulated blast furnace slag in the activated filler was small, and the total water content was also small, so it is assumed that the effects of fluidity and strength were not obtained.

[0110] The geopolymer compositions of Comparative Examples 3 and 4 also did not contain silica fume. In the geopolymer composition of Comparative Example 3, the blending ratio of ground granulated blast furnace slag in the activated filler was high, as in Example 1, but the total moisture content was excessively high. As a result, although the target fluidity of 200 mm was exceeded, bleeding occurred, and the strength of the hardened product did not reach the target strength. In the geopolymer composition of Comparative Example 4, the blending ratio of ground granulated blast furnace slag in the activated filler was high, as in Example 1, but the total moisture content was high. As a result, although the target fluidity of 200 mm was exceeded and bleeding did not occur, the strength of the hardened product did not reach the target strength.

[0111] This application is based on Japanese Patent Application No. 2023-000433 filed on January 5, 2023, the contents of which are incorporated herein by reference.

[0112] The embodiments and examples disclosed herein should be understood to be illustrative in all respects and not restrictive. The scope of the present invention is defined by the claims, not by the above description, and is intended to include all modifications within the meaning and scope of the claims.

[0113] According to an embodiment of the present invention, a geopolymer composition can be obtained that achieves both good flowability over a long period of time and high strength in a hardened body in a short period of time using a simple method while reducing the amount of silica fume blended. This reduces the manufacturing cost of the geopolymer composition. In particular, the same effects can be achieved even if the active filler contains coal ash, an industrial by-product that has not been treated to comply with the JIS A 6201:2015 fly ash standard for concrete, which is environmentally preferable.

Claims

1. A geopolymer composition comprising an active filler, an aggregate, an activator, a dispersant, and added water, wherein the geopolymer composition does not contain silica fume or contains less than 1% by weight of silica fume relative to the total weight of the geopolymer composition, the total water content of the geopolymer composition is 10% to 13% by weight, the active filler contains 35% or more by weight of ground granulated blast furnace slag and coal ash relative to the total weight of the active filler, and the dispersant is a polycondensate-based dispersant containing polyalkylene glycol monophenyl ether as a partial structure. A geopolymer composition.

2. The geopolymer composition of claim 1, wherein the geopolymer composition does not contain silica fume.

3. A hardened geopolymer, which is a hardened product of the geopolymer composition according to claim 1 or 2.

4. A method for producing a hardened geopolymer, comprising the steps of mixing and kneading the geopolymer composition according to claim 1 or 2, and then hardening the composition.