Method for converting ethanol, zeolite-containing catalyst, method for producing zeolite-containing catalyst, and method for producing hydrocarbon and the like

MYPI2025004107A0Undetermined Publication Date: 2024-07-30ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025004107
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-01-30
Filing Date
2024-01-29
Publication Date
2024-07-30

AI Technical Summary

Technical Problem

The existing methods for converting ethanol to hydrocarbons using zeolite catalysts face challenges due to catalyst deterioration caused by water vapor and coke deposition, leading to decreased catalytic activity and productivity over time, especially in fixed bed reactors where catalyst replacement is not feasible.

Method used

A method utilizing a zeolite-containing catalyst with a specific oxygen 10-membered ring structure, controlled acidity, and a Na/Al molar ratio of 0.0050 to 0.25, along with a steaming step to produce a catalyst with reduced sodium content and optimized silica/alumina ratio, which suppresses structural collapse and coke deposition, maintaining catalytic activity and productivity.

Benefits of technology

This approach stabilizes the yield of target compounds like propylene and aromatic compounds by preventing catalyst deterioration, ensuring consistent ethylene conversion rates and extending catalyst lifespan.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025004107_DRAWING_001
    Figure PI2025004107_DRAWING_001
  • Figure PI2025004107_DRAWING_002
    Figure PI2025004107_DRAWING_002
Patent Text Reader

Abstract

A method for converting ethanol, comprising a reaction step of feeding a mixed raw material containing ethanol into a reactor having a fixed bed filled with a zeolite-containing catalyst to obtain a reaction gas containing an olefin having 3 or more carbon atoms and water, wherein a zeolite contained in the zeolite-containing catalyst has an oxygen 10-membered ring structure, a molar ratio of Na / Al of the zeolite-containing catalyst is from 0.0050 to 0.25, and an acid content per weight of the zeolite-containing catalyst determined from an amount of ammonia desorbed at from 100 to 650C in ammonia temperature-programmed desorption measurement of the zeolite-containing catalyst is 75 μmol / g or less. Fig. 1
Need to check novelty before this filing date? Find Prior Art

Description

Ethanol conversion method, zeolite-containing catalyst, method for producing zeolite-containing catalyst, and method for producing hydrocarbons, etc.

[0001] The present invention relates to a method for converting ethanol, a zeolite-containing catalyst, a method for producing a zeolite-containing catalyst, and a method for producing hydrocarbons, etc.

[0002] Hydrocarbons such as lower olefins and aromatic compounds are important core raw materials in the chemical industry, and in particular, the development and improvement of production methods for propylene, for which demand is expected to increase, has been actively pursued. Among these, a commonly known method for producing propylene is a method in which naphtha and olefins are brought into contact with a catalyst using zeolite as the active species.

[0003] In addition to olefins, the recent rise in environmental awareness has led to the production of chemical products such as lower olefins and aromatic compounds using biomass-derived alcohols as raw materials, which has attracted attention. In particular, since ethanol is a compound for which a production method from biomass raw materials has been established, there are high hopes for the early development of an efficient method for converting ethanol.

[0004] For example, Patent Documents 1 and 2 disclose methods for producing a phosphorus-modified zeolite catalyst that promotes the conversion reaction from ethanol to propylene. Patent Document 3 discloses a method for producing propylene from a water-containing ethylene raw material using a zeolite catalyst.

[0005] China Patent Publication No. 107649173A Patent No. 6229274 Patent No. 5116043

[0006] When ethanol is converted to obtain hydrocarbons such as propylene and aromatic compounds, the dehydration reaction of ethanol produces a by-product of water in an amount equimolar to the feedstock ethanol. Generally, water (steam) at temperatures above 400°C causes structural collapse due to dealumination of the zeolite catalyst, reducing the catalytic performance of the zeolite. In other words, when ethanol is converted by contacting a feedstock containing ethanol with zeolite, the by-product water reduces catalytic activity, resulting in a decrease in the yield of the target compound over time. In particular, when a fixed-bed reactor is used, catalyst replacement or additional loading is not possible during the reaction, and catalyst degradation leads to a significant decrease in productivity.

[0007] Patent Documents 1 and 2 each disclose a method for producing a zeolite catalyst that converts an ethanol feedstock into propylene, but show that the catalytic activity decreases with the passage of reaction time. Patent Document 3 discloses a method for converting a water-containing ethylene feedstock into propylene by contacting it with a zeolite catalyst, but shows that the propylene selectivity decreases within a few hours of the start of the reaction.

[0008] Therefore, an object of the present invention is to provide a method for converting ethanol that suppresses deterioration of catalyst performance due to water vapor and suppresses coke deposition, a zeolite-containing catalyst, a method for producing a zeolite-containing catalyst, and a method for producing hydrocarbons, etc.

[0009] As a result of extensive research to achieve the above object, the present inventors have found that the use of a catalyst containing a 10-membered oxygen ring zeolite with specific composition and physical properties prevents the structural collapse of the zeolite and the deposition of coke on the catalyst due to side reactions, even in ethanol conversion accompanied by the by-production of water, thereby suppressing a decrease in catalytic activity and enabling the production of target compounds in stable yields. That is, the present invention encompasses the following embodiments.

[0010] <1> A method for converting ethanol, comprising a reaction step of supplying an ethanol-containing mixed raw material to a reactor having a fixed bed packed with a zeolite-containing catalyst to obtain a reaction gas containing olefins having 3 or more carbon atoms and water, wherein the zeolite contained in the zeolite-containing catalyst has a 10-membered oxygen ring structure, the Na / Al molar ratio of the zeolite-containing catalyst is 0.0050 to 0.25, and the acid amount per weight of the zeolite-containing catalyst, calculated from the amount of ammonia desorption at 100 to 650°C in an ammonia temperature-programmed desorption measurement of the zeolite-containing catalyst, is 75 μmol / g or less. <2> The method for converting ethanol according to <1>, wherein the acid amount Ac (unit: μmol / g) per weight of the zeolite-containing catalyst satisfies the following formula (1): Ac ≦ 25 − 60 × [Na / Al molar ratio] (1). <3> The method for converting ethanol according to <1> or <2>, wherein the acid amount per weight of the zeolite-containing catalyst is 0.5 μmol / g or more. <4> The method for converting ethanol according to any one of <1> to <3>, wherein the acid amount per weight of the zeolite, calculated from the amount of ammonia desorption at 100 to 650°C in ammonia temperature-programmed desorption measurement of the zeolite-containing catalyst, is 75 μmol / g or less. <5> The method for converting ethanol according to any one of <1> to <4>, wherein the amount of sodium contained in the zeolite-containing catalyst is 100 ppm by mass or less. <6> The method for converting ethanol according to any one of <1> to <5>, wherein the mass ratio of Si / Al in the zeolite-containing catalyst is 300 to 3,000. <7> The method for converting ethanol according to any one of <1> to <6>, wherein the molar ratio of silica / alumina of the zeolite in the zeolite-containing catalyst is 600 to 2,000. <8> The method for converting ethanol according to any one of <1> to <7>, wherein the zeolite-containing catalyst contains at least one doping element selected from the group consisting of phosphorus and Group 11 elements. <9> The method for converting ethanol according to <8>, wherein the content of the doping element is 2.0 mass% or less, based on the total amount of the zeolite-containing catalyst. <10> The method for converting ethanol according to any one of <1> to <9>, wherein the content of aluminum is 0.01 mass% to 1 mass%, based on the total amount of the zeolite-containing catalyst.<11> The method for converting ethanol according to any one of <1> to <10>, wherein the mixed feedstock contains ethylene. <12> The method for converting ethanol according to any one of <1> to <11>, wherein the ethanol content in the mixed feedstock is 30% by mass or more relative to the mixed feedstock. <13> The method for converting ethanol according to any one of <1> to <12>, wherein the molar ratio of ethylene / ethanol in the mixed feedstock is 0.20 to 2.50. <14> The method for converting ethanol according to any one of <1> to <13>, comprising a regeneration step of contacting the zeolite-containing catalyst subjected to the reaction step with an oxygen-containing gas heated to 400°C or higher, and then subjecting the catalyst to the reaction step again. <15> A method for producing propylene, comprising a propylene separation step of separating a fraction mainly containing propylene from the reaction gas obtained by the method for converting ethanol according to any one of <1> to <14>. <16> A method for producing aromatic compounds, comprising: an aromatic compound separation step of separating a fraction mainly containing aromatic compounds from a reaction gas obtained by the ethanol conversion method according to any one of <1> to <14>. <17> A zeolite-containing catalyst, wherein the zeolite contained in the zeolite-containing catalyst has a 10-membered oxygen ring structure, the zeolite-containing catalyst has a Na / Al molar ratio of 0.0050 to 0.25, and the acid amount per weight of the zeolite-containing catalyst, calculated from the amount of ammonia desorption at 100 to 650°C in an ammonia temperature-programmed desorption measurement of the zeolite-containing catalyst, is 75 μmol / g or less. <18> The zeolite-containing catalyst according to <17>, wherein the Si / Al mass ratio in the zeolite-containing catalyst is 300 to 3000. <19> The zeolite-containing catalyst according to <17> or <18>, which is a catalyst for producing olefins having 3 or more carbon atoms from a mixed feedstock containing ethanol. <20> The zeolite-containing catalyst according to any one of <17> to <19>, which contains at least one doping element selected from the group consisting of phosphorus and Group 11 elements. <21> The zeolite-containing catalyst according to <20>, in which the content of the doping element is 2.0 mass% or less based on the total amount of the zeolite-containing catalyst.<22> The zeolite-containing catalyst according to any one of <17> to <21>, wherein the aluminum content is 0.01% by mass to 1% by mass relative to the total amount of the zeolite-containing catalyst. <23> A method for producing a zeolite-containing catalyst, wherein the zeolite contained in the zeolite-containing catalyst is a zeolite having a 10-membered oxygen ring structure, the zeolite-containing catalyst has a Na / Al molar ratio of 0.0050 to 0.25, the zeolite-containing catalyst has an acid amount per weight of 75 μmol / g or less, as determined from the amount of ammonia desorption at 100 to 650°C in an ammonia temperature-programmed desorption measurement of the zeolite-containing catalyst, and the method for producing a zeolite-containing catalyst includes a steaming step of contacting the zeolite-containing catalyst with steam at a steaming temperature of 450°C or higher. <24> A method for producing hydrocarbons, comprising a reaction step of supplying a raw material containing ethanol to a reactor having a fixed bed packed with a zeolite-containing catalyst, and obtaining a reaction gas containing olefins having 3 or more carbon atoms and water, wherein the zeolite contained in the zeolite-containing catalyst is a zeolite having a 10-membered oxygen ring structure, the Na / Al molar ratio of the zeolite-containing catalyst is 0.0050 to 0.25, and the acid amount per weight of the zeolite-containing catalyst, calculated from the amount of ammonia desorption at 100 to 650°C in ammonia temperature-programmed desorption measurement of the zeolite-containing catalyst, is 75 μmol / g or less.

[0011] According to the present invention, it is possible to provide a method for converting ethanol, a zeolite-containing catalyst, a method for producing a zeolite-containing catalyst, and a method for producing hydrocarbons, etc., which suppress deterioration of catalyst performance due to water vapor and suppress coke deposition.

[0012] Figure 1 shows a schematic diagram of an embodiment of a fixed-bed single-stage adiabatic reactor. Figure 2 shows a schematic diagram of an embodiment of an ethanol conversion apparatus. Figure 3 shows a schematic diagram of an embodiment of an ethanol conversion apparatus. Figure 4 shows the reaction results of Example 1.

[0013] The present invention will be described in detail below. Note that the present invention is not limited to the following embodiments (present embodiments) and can be practiced in various modifications within the scope of the gist thereof. In this specification, a numerical range indicated using "to" indicates a range that includes the numerical values ​​before and after "to" as the minimum and maximum values, respectively. In the numerical ranges described in stages in this specification, the upper limit or lower limit of a numerical range of a certain stage can be arbitrarily combined with the upper limit or lower limit of a numerical range of another stage.

[0014] [Method for Conversion of Ethanol] The method for converting ethanol according to this embodiment includes a reaction step of supplying an ethanol-containing mixed feedstock to a reactor having a fixed bed packed with a zeolite-containing catalyst, and obtaining a reaction gas containing olefins having 3 or more carbon atoms and water, wherein the zeolite contained in the zeolite-containing catalyst has a 10-membered oxygen ring structure (also simply referred to as a "10-membered ring structure"); the Na / Al molar ratio of the zeolite-containing catalyst is 0.0050 to 0.25; and the acid amount per weight of the zeolite-containing catalyst (hereinafter also referred to as "TPD acid amount per catalyst weight"), calculated from the amount of ammonia desorption at 100 to 650°C in a temperature-programmed ammonia desorption measurement of the zeolite-containing catalyst, is 75 μmol / g or less. According to this embodiment, by using the above-mentioned zeolite-containing catalyst, it is possible to provide an ethanol conversion method, a zeolite-containing catalyst, a method for producing a zeolite-containing catalyst, a method for producing hydrocarbons, a method for producing propylene, and a method for producing aromatic compounds, which suppress deterioration of catalytic performance due to water vapor and suppress coke deposition. In other words, by controlling the acidity of zeolite and reducing the affinity of zeolite with water (steam), it is believed that the catalytic activity of zeolite can be maintained even under reaction conditions in the presence of steam, and that the activity of the zeolite-containing catalyst can be prevented from decreasing over reaction time. Furthermore, by controlling the amount of sodium in the zeolite-containing catalyst, it is believed that the structural collapse of the zeolite and the deposition of coke on the catalyst due to side reactions can be prevented, and that the activity of the zeolite-containing catalyst can be prevented from decreasing even under reaction conditions in the presence of ethanol. Furthermore, the zeolite-containing catalyst can also be prevented from deteriorating in catalytic activity during a catalyst regeneration process that involves the generation of steam.

[0015] Furthermore, according to the present embodiment, ethanol can be converted into target compounds such as propylene, aromatic compounds, etc. with high yield. Furthermore, according to the present embodiment, the ethylene conversion rate can be kept constant, and ethylene can be produced stably.

[0016] [Reactor] In this embodiment, a zeolite-containing catalyst is packed into a reactor having a fixed bed (hereinafter also referred to as a "fixed-bed reactor") to carry out the reaction step. The fixed-bed reactor may be either an adiabatic reactor or an isothermal reactor. Among these, it is preferable to use a fixed-bed adiabatic reactor from the viewpoint of excellent operability. If necessary, a heating device for heating the raw materials can be provided before the reactor.

[0017] (Fixed-Bed Adiabatic Reactor) For details of fixed-bed adiabatic reactors, reference can be made to the description in Adiabatic Fixed-Bed Reactors (Elsevier, 2014, Ch. 1, P. 4, L. 5-24 ISBN: 978-0-12-801306-9). Among fixed-bed adiabatic reactors, a fixed-bed single-stage adiabatic reactor having only one fixed catalyst bed is more preferred. Since carbonaceous matter (coke) accumulates on the catalyst as the reaction proceeds, a multi-column switching type fixed-bed single-stage adiabatic reactor is preferred, as it is capable of burning off and removing this carbonaceous matter while the reaction is continuing.

[0018] 1 is a schematic diagram of a fixed-bed, single-stage adiabatic reactor. The fixed-bed, single-stage adiabatic reactor 10a includes a reaction casing 12 with a heat insulating material 121 provided on the outer periphery, a catalyst bed 13, a reactor inlet 14, and a reactor outlet 15. The reaction casing 12 is provided with the heat insulating material 121 on the outer periphery, thereby preventing heat from escaping from the reactor to the outside. In the production method according to this embodiment, the temperature inside the reactor can be controlled by the heat generation and heat absorption caused by the reaction.

[0019] The catalyst bed 13 is filled with a catalyst, which will be described later. A first sheathed thermocouple 161 is provided in the catalyst bed 13 immediately before it contacts the catalyst bed inlet 131. A second sheathed thermocouple 162 is provided in the catalyst bed 13 immediately after it passes through the catalyst bed outlet 132. These thermocouples measure the temperature of the mixed raw material immediately before it contacts the catalyst bed inlet 131 and the reaction gas immediately after it passes through the catalyst bed outlet 132. The positions of these thermocouples can be changed as necessary. The catalyst bed 13 may be of a multi-stage type, but is preferably of a single stage type as shown in FIG. 1.

[0020] In the fixed-bed single-stage adiabatic reactor 10 a , a raw material is introduced through a reactor inlet 14 and brought into contact with a catalyst bed 13 , and a reaction gas is taken out through a reactor outlet 15 .

[0021] [Zeolite-Containing Catalyst] A zeolite-containing catalyst is used in the reaction step of this embodiment. The zeolite-containing catalyst contains zeolite. The zeolite-containing catalyst exhibits catalytic activity for converting ethanol and olefins into target compounds such as propylene. A common problem in conventional olefin production using ethanol as a raw material with zeolite is the deterioration of zeolite due to steam. According to the ethanol conversion method of this embodiment, it is believed that the acidity of the zeolite-containing catalyst can be controlled to reduce the affinity of the zeolite-containing catalyst with water (steam), thereby making it easier to maintain the yield of the target compound for a long period of time.

[0022] The zeolite-containing catalyst may be a molded body made of zeolite alone, but a molded body containing zeolite and a silica binder is preferred in terms of excellent crushing strength.

[0023] In the conversion method of this embodiment, the zeolite has a 10-membered oxygen ring structure. Examples of such zeolites include ZSM-5, ZSM-8, ZSM-11, ZSM-12, ZSM-21, ZSM-23, ZSM-35, and ZSM-38. Among them, MFI zeolite is preferred, and ZSM-5 is more preferred, from the viewpoint of excellent catalytic performance (catalytic activity and durability against coking).

[0024] The zeolite synthesis method of this embodiment is not particularly limited, but can be produced by optimizing various conditions of a conventionally known hydrothermal synthesis method for MFI zeolite. Generally, methods for efficiently obtaining MFI zeolite by hydrothermal synthesis include hydrothermal synthesis using an appropriate organic structure-directing agent (SDA), hydrothermal synthesis using hydrothermally synthesized MFI zeolite as seed crystals, or hydrothermal synthesis using seed slurry in the crystalline stage. Examples of organic structure-directing agents used here include ammonium salts, urea compounds, amines, and alcohols. It is known that not only organic SDAs but also inorganic cations and anions are involved in the structure, and zeolite synthesis depends on the combined functions of each component. In the hydrothermal synthesis method for MFI zeolite described above, a suitable catalyst can be obtained by appropriately optimizing synthesis conditions such as the type of raw materials and additives (SDA), the amount of additives, pH, silica / alumina molar ratio, raw material charge composition (e.g., medium, cation, and anion abundance ratio), synthesis temperature, and synthesis time.

[0025] Specific examples include the synthesis method using a seed slurry described in Japanese Patent No. 5,426,983 and the method exemplified in The Hydrothermal Synthesis of Zeolites (Chemical Reviews, 2003, 103, 663-702).

[0026] Furthermore, commercially available zeolites can also be used as long as they are MFI zeolites having the above-mentioned specific physical properties and composition.

[0027] (TPD Acid Amount per Catalyst Weight) The ethanol conversion method of this embodiment uses a zeolite-containing catalyst having an acid amount per zeolite-containing catalyst weight of 75 μmol / g or less, as determined from the amount of ammonia desorption from the zeolite-containing catalyst at 100 to 650°C in ammonia temperature-programmed desorption measurement. Having a TPD acid amount within this range can suppress deterioration of catalytic performance due to steam. While zeolite acid sites contribute to catalytic activity, they also function as autocatalysts, promoting hydrolysis of the zeolite structure. Therefore, in a reactor containing ethanol as a reaction raw material and coexisting with high-temperature steam, catalysts with excessive acid amounts tend to undergo structural collapse of the zeolite. Therefore, controlling the TPD acid amount within a specific range is believed to contribute to maintaining the zeolite structure and catalytic function. Furthermore, excessive active sites can lead to excessive polymerization reactions and coke deposition on the catalyst surface. Therefore, controlling the acid amount below the upper limit helps to keep the amount of coke within an appropriate range. However, this is not a limiting factor.

[0028] The amount of TPD acid per catalyst weight is preferably 40 μmol / g or less, more preferably 30 μmol / g or less, and even more preferably 25 μmol / g or less. In order to achieve excellent catalytic activity per catalyst weight, the amount of TPD acid per catalyst weight is preferably 0.5 μmol / g or more, more preferably 1.5 μmol / g or more, and even more preferably 5.0 μmol / g or more.

[0029] Furthermore, as a result of repeated experiments and investigations, it was found that sodium, which has conventionally been used to adjust the acid amount of a catalyst, accelerates catalyst deterioration in the reaction step of this embodiment. Therefore, in the ethanol conversion method of this embodiment, it is preferable to control the amount of sodium in addition to the amount of acid, and from the viewpoint of further improving the durability of the catalyst, it is preferable that the TPD acid amount Ac (unit: μmol / g) per catalyst weight satisfies the following formula (1): Ac ≦ 25 − 60 × [molar ratio of Na / Al] (1). The molar ratio of Na / Al is the molar ratio of the amounts of sodium and aluminum contained in the zeolite-containing catalyst.

[0030] Under the conditions of the reaction process of this embodiment, the sodium contained in the zeolite-containing catalyst exhibits strong basicity when coexisting with water or ethanol, promoting structural collapse of zeolites with poor base resistance and accelerating catalyst degradation. Furthermore, sodium is both basic and Lewis acidic, promoting coke deposition on the catalyst. Therefore, in order to stably produce the target compound, it is necessary to control the amount of sodium in addition to controlling the acid content of the zeolite-containing catalyst. In other words, a zeolite-containing catalyst with a high sodium content will tolerate a smaller amount of acid, and the relationship in which the upper limit of the suitable acid content decreases with increasing sodium is expressed as Equation (1). The first term, 25, on the right side of Equation (1) represents the acid content per catalyst weight suitable for achieving excellent durability of the zeolite structure. The second term on the right side of Equation (1) represents the effect of sodium on catalyst durability by multiplying the Na / Al molar ratio of the zeolite-containing catalyst by a coefficient of 10. In the second term, the Na / Al molar ratio of the zeolite-containing catalyst was used as a variable instead of the amount of sodium relative to the zeolite-containing catalyst. This is because, even if the amount of sodium relative to the zeolite-containing catalyst is the same, the number of acid sites in the zeolite-containing catalyst, i.e., the catalyst with a higher aluminum content, can reduce the adverse effects of sodium. The coefficient of 60 was determined from an example that showed favorable catalytic performance in experimental studies.

[0031] The structural collapse of zeolite due to dealumination by steam is caused by the acidity of zeolite, and the reaction step can be carried out while suppressing dealumination by controlling the acidity of the zeolite-containing catalyst, although the cause is not limited to this.

[0032] Among the above-mentioned zeolite-containing catalysts, the zeolite structure has excellent durability, and therefore the acid amount per zeolite weight (hereinafter referred to as "TPD acid amount per zeolite weight"), determined from the amount of ammonia desorption at 100 to 650°C in an ammonia temperature-programmed desorption measurement of the zeolite-containing catalyst, is preferably 75 μmol / g or less, more preferably 40 μmol / g or less, and even more preferably 30 μmol / g or less. The TPD acid amount per zeolite weight is preferably 0.5 μmol / g or more, more preferably 1.5 μmol / g or more, and even more preferably 5.0 μmol / g or more.

[0033] The TPD acid amount per catalyst weight can be calculated using a calibration curve method from a desorption spectrum obtained by passing diluted ammonia gas through a degassed zeolite-containing catalyst to adsorb ammonia, and then raising the temperature. The area value of the spectrum obtained by measurement from 100°C to 650°C is used to derive the TPD acid amount. More specifically, the method described in the Examples is used. The TPD acid amount per zeolite weight is calculated by dividing the TPD acid amount per zeolite-containing catalyst weight obtained by the above method by the weight ratio of zeolite in the zeolite-containing catalyst. Here, the TPD acid amount means the acid amount before (initial) the zeolite-containing catalyst is used in the reactor.

[0034] The acid amount retention rate of the zeolite-containing catalyst, represented by the following formula, is preferably 50% or more, more preferably 60% or more, and even more preferably 70% or more. The upper limit of the acid amount retention rate is not particularly limited, but it may be 98% or less.

[0035] Acid amount maintenance rate (%) = 6.0 hr Acid amount after STM treatment (μmol / g) / 1.0 hr Acid amount after STM treatment (μmol / g) × 100

[0036] The acid amount after 6.0-hour STM treatment is the TPD acid amount of the zeolite-containing catalyst after 6 hours of steam treatment, and the acid amount after 1.0-hour STM treatment is the TPD acid amount of the zeolite-containing catalyst after 1 hour of steam treatment.

[0037] The steam treatment was carried out by bubbling helium gas at a flow rate of 50 mL / min into water heated to 80°C, lowering the temperature to 75°C using a condenser, preparing a zeolite-containing catalyst heated to 650°C, and bringing the steam into contact with the zeolite-containing catalyst.

[0038] (Mesopore Volume of Zeolite-Containing Catalyst) In the ethanol conversion method of this embodiment, from the viewpoint of excellent raw material adsorption characteristics, it is preferable to use a zeolite-containing catalyst having a mesopore volume of 0.15 cc / g or more, and more preferably 0.20 cc / g or more. The mesopore volume can be measured by mercury intrusion porosimetry using a mercury porosimeter.

[0039] (Composition of Zeolite-Containing Catalyst) The silica / alumina (SiO 2 / Al 2 O 3 The silica / alumina molar ratio can be appropriately selected, but from the viewpoint of excellent catalyst durability, it is preferably 20 to 3000, more preferably 200 to 2500, and even more preferably 600 to 2000. The silica / alumina molar ratio of the zeolite can be measured by a known method, for example, by completely dissolving the zeolite in an alkaline aqueous solution and analyzing the resulting solution by plasma emission spectrometry or the like.

[0040] The mass ratio of silicon (Si) to aluminum (Al) (Si / Al mass ratio) contained in the zeolite-containing catalyst of this embodiment can be selected as appropriate. From the viewpoint of excellent catalyst durability, the Si / Al mass ratio is preferably 125 to 3000, and more preferably 300 to 3000. The Si / Al mass ratio can be measured by a known method, for example, by completely dissolving the zeolite-containing catalyst in an alkaline aqueous solution and analyzing the resulting solution using plasma emission spectroscopy or the like. By controlling the Si / Al mass ratio of the zeolite-containing catalyst, the affinity of the zeolite-containing catalyst with water can be reduced, and the reaction step can be carried out while maintaining catalytic performance even under hydrothermal conditions. However, factors are not limited to these. To achieve excellent catalytic activity, the Si / Al mass ratio is preferably 3000 or less, more preferably 2500 or less, and even more preferably 2000 or less. Furthermore, to suppress deterioration of catalytic performance due to water vapor, the Si / Al mass ratio is preferably 125 or more, more preferably 300 or more, and even more preferably 500 or more.

[0041] The molar ratio of sodium to aluminum (Na / Al molar ratio) contained in the zeolite-containing catalyst of this embodiment is 0.0050 to 0.25, preferably 0.0050 to 0.20, and more preferably 0.005 to 0.15. A Na / Al molar ratio of 0.25 or less suppresses deterioration of catalytic performance due to steam, and a Na / Al molar ratio of 0.0050 or more suppresses coke deposition. To achieve excellent durability against catalyst deterioration due to higher-temperature steam, the Na / Al molar ratio is preferably 0.20 or less, and more preferably 0.15 or less. Furthermore, to further suppress coke formation, the Na / Al molar ratio is preferably 0.0060 or more, and more preferably 0.0070 or more.

[0042] Because sodium is used as part of the raw materials in the zeolite synthesis process and catalyst molding process, the Na / Al molar ratio of the zeolite-containing catalyst is generally greater than 0.5. To adjust the sodium content of the zeolite-containing catalyst to the above range, it is effective to remove sodium by washing the zeolite-containing catalyst with an acid (hereinafter also referred to as "acid washing"). The type of acid used in acid washing is not particularly limited; for example, the Na / Al molar ratio can be adjusted by washing with an aqueous nitric acid solution. The acid concentration of the washing solution used in acid washing is preferably 0.010 to 10 N to achieve excellent washing efficiency. Furthermore, to suppress zeolite deactivation during acid washing, the acid concentration of the washing solution is more preferably 0.01 to 2.0 N, and even more preferably 0.05 to 1.5 N. Acid washing does not require heating or cooling, but from the perspective of excellent washing efficiency, it is preferably performed at 10 to 90°C, and more preferably 20 to 70°C. Acid washing is carried out, for example, by immersing the zeolite-containing catalyst in a washing solution, and the immersion time is preferably 0.10 to 10 hours, more preferably 0.50 to 6.0 hours, because this provides excellent washing efficiency. The weight of the washing solution used in one acid washing is preferably 500 parts by mass or less, more preferably 250 parts by mass or less, per 10 parts by mass of zeolite, because this facilitates waste liquid treatment. Although the sodium removal rate can be increased by performing acid washing multiple times, it is preferably performed only once during catalyst production because this facilitates waste liquid treatment.

[0043] Another effective method for removing sodium held at the cation sites is cation exchange, for example, by ion exchange treatment using an aqueous silver nitrate solution, the sodium content in the zeolite-containing catalyst can be reduced and the Na / Al molar ratio can be adjusted. Alternatively, the sodium content in the raw materials used for zeolite synthesis can be reduced by acid washing, thereby adjusting the amount of sodium in the zeolite-containing catalyst.

[0044] Sodium contained in the zeolite-containing catalyst forms basic sites in the presence of water or ethanol, causing the zeolite to collapse and produce coke, thereby accelerating catalyst degradation. Therefore, in the reaction process of this embodiment, it is desirable to reduce the sodium content in the zeolite to prevent catalyst degradation. Sodium is a component that is easily mixed in during zeolite synthesis and catalyst molding processes, and therefore requires particular management. Therefore, controlling the Na / Al molar ratio is believed to prevent the formation of basic sites during the reaction and to prevent the activity of the zeolite-containing catalyst from decreasing over the reaction time, even under reaction conditions in which water vapor coexists.

[0045] The sodium content of the zeolite-containing catalyst of this embodiment is preferably 1,000 ppm by mass or less, more preferably 100 ppm by mass or less, and even more preferably 10 ppm by mass or less, based on the total amount of the zeolite-containing catalyst. Furthermore, from the viewpoint of suppressing coke generation due to side reactions, it is preferably 100 ppm by mass or less. In this embodiment, the sodium content in the zeolite-containing catalyst is a value measured by XRF analysis.

[0046] (Doping element in zeolite-containing catalyst) The zeolite-containing catalyst in this embodiment may contain at least one doping element selected from the group consisting of phosphorus and elements belonging to Group 11 of the periodic table (hereinafter, these elements are collectively referred to as "dopant element"). Among these, the zeolite-containing catalyst preferably contains phosphorus or silver.

[0047] The form of phosphorus includes a polymer of phosphorus (e.g., polyphosphoric acid), an oxide of phosphorus (e.g., P 2 O 5), compounds in which phosphorus is added to the aluminum of zeolite, etc. may also be included. When the zeolite contains aluminum, phosphorus has the effect of suppressing dealumination of the zeolite. In the method according to this embodiment, water is generated in the reactor, and the raw material ethanol may also contain water, so the reactor becomes a high-temperature steam atmosphere that causes dealumination. When the zeolite-containing catalyst contains phosphorus, dealumination of the zeolite is suppressed, and the durability of the catalyst can be further improved.

[0048] Examples of elements belonging to Group 11 of the periodic table include copper, silver, and gold. By containing an element belonging to Group 11 of the periodic table, dealumination of the zeolite is suppressed, and the durability of the catalyst is improved. Among these elements belonging to Group 11 of the periodic table, silver is preferred from the viewpoint of excellent support efficiency.

[0049] The content of the doping element contained in the zeolite-containing catalyst may be 2.0% by mass or less, preferably 0.01 to 2.0% by mass, and more preferably 0.05 to 1.0% by mass, based on the total amount of the zeolite-containing catalyst, from the viewpoint of further suppressing dealumination.

[0050] In this embodiment, the content of the doping element in the zeolite-containing catalyst is a value measured using an X-ray fluorescence analyzer. The content of phosphorus, copper, silver, or gold can be measured using a commercially available X-ray fluorescence analyzer under normal conditions in accordance with the instruction manual. For example, when using a Rigaku product under the trade name "RIX3000," the measurement conditions can be P-Kα radiation, a tube voltage of 50 kV, and a tube current of 50 mA.

[0051] In this embodiment, phosphoric acid and / or a phosphate (hereinafter also referred to as a "phosphorus raw material") may be used as a source of phosphorus contained in the zeolite-containing catalyst. Phosphates are more preferred as the phosphorus raw material, and among phosphates, compounds showing a solubility of 1 g or more in 100 g of water at 25°C are more preferred.

[0052] Examples of phosphoric acid include phosphoric acid and pyrophosphoric acid, and examples of phosphates include ammonium phosphate salts such as ammonium phosphate, diammonium hydrogen phosphate, ammonium dihydrogen phosphate, and sodium ammonium hydrogen phosphate, as well as potassium hydrogen phosphate, aluminum hydrogen phosphate, sodium phosphate, and potassium phosphate. Among these, ammonium phosphate salts having relatively high solubility in water are preferred, and more preferred is at least one selected from the group consisting of ammonium phosphate, diammonium hydrogen phosphate, and ammonium dihydrogen phosphate. These may be used alone or in combination of two or more.

[0053] In this embodiment, metal nitrate salts such as copper nitrate and silver nitrate may be used as raw materials for the elements belonging to Group 11 of the periodic table contained in the zeolite-containing catalyst. A zeolite-containing catalyst containing sodium as a counter cation can be ion-exchanged with a metal nitrate salt and then sintered to obtain a zeolite-containing catalyst containing an element belonging to Group 11 of the periodic table. The ion exchange between sodium, the counter cation in the zeolite, and the metal nitrate salt can be performed by immersing the zeolite or the zeolite-containing catalyst in an aqueous solution of the metal nitrate salt and then washing with water. The ion exchange rate can be improved by performing the immersion and washing multiple times. Furthermore, because residual sodium in the catalyst as described above impairs the degradation resistance of the zeolite, it is preferable to prepare a zeolite-containing catalyst containing an element belonging to Group 11 of the periodic table using a proton-type or ammonium-type zeolite-containing catalyst.

[0054] (Method for Molding Zeolite-Containing Catalyst) The zeolite-containing catalyst of this embodiment can be produced by molding a zeolite having the specific physical properties and composition described above, for example, as follows. The molding method is not particularly limited, and a general method can be used. Specific examples include a method of compression molding or extrusion molding of the catalyst component, and a spray-dry molding method that is optimal for a fluidized bed reaction system.

[0055] A binder can be used for molding. The binder is not particularly limited, and for example, silica, alumina, and kaolin can be used alone or in combination. Commercially available binders can be used. The mass ratio of zeolite to binder is preferably in the range of 10 / 90 to 90 / 10, more preferably 20 / 80 to 80 / 20. Since the conversion method of this embodiment requires precise control of the acid sites on the catalyst, it is preferable that the catalyst does not contain any compounds exhibiting acidic properties other than zeolite. However, binders such as alumina and kaolin exhibit acidic properties. Therefore, it is preferable to use a binder that does not exhibit acidic properties. Among these, it is more preferable to use a silica binder from the viewpoint of excellent coking resistance. The total content of zeolite and binder may be 80 to 100% by mass, or 90 to 100% by mass, based on the total amount of the zeolite-containing catalyst. The aluminum content in the zeolite-containing catalyst is preferably 0.01 mass % to 1 mass %, more preferably 0.03 mass % to 0.5 mass %, and even more preferably 0.05 mass % to 0.1 mass %, based on the total amount of the zeolite-containing catalyst.

[0056] (Pretreatment step of zeolite-containing catalyst) In the ethanol conversion method of this embodiment, after optionally molding, the zeolite-containing catalyst may be subjected to a pretreatment step prior to contacting the zeolite-containing catalyst with the raw material. A preferred pretreatment step is a steaming step in which the catalyst is heated in the presence of steam at a temperature of 450°C or higher. Pretreatment tends to more significantly suppress catalyst degradation and improve selectivity. In the above method, the catalyst is preferably treated at a temperature of 450°C or higher and 900°C or lower in a mixed gas of steam (water vapor) and an inert gas such as air or nitrogen, although the atmosphere is not particularly limited, under conditions of a water vapor partial pressure of 0.01 atmosphere or higher. The heat treatment temperature is more preferably 500°C or higher and 700°C or lower. This pretreatment step can be carried out using a reactor for converting ethanol and ethylene.

[0057] (Zeolite-Containing Catalyst Shape) In the ethanol conversion method of this embodiment, zeolite-containing catalysts having various shapes, such as cylindrical or ring-shaped, can be used. However, from the viewpoint of excellent ease of handling, it is preferable to use a cylindrical zeolite-containing catalyst. Among these, from the viewpoint of excellent catalyst strength, it is preferable to use a cylindrical molded body having a diameter of 1.6 mm or more and a length of 0.1 to 10.0 cm.

[0058] [Mixed Raw Material] In the reaction step of this embodiment, a mixed raw material containing ethanol is used. From the viewpoint of excellent environmental friendliness, the ethanol is preferably derived from biomass. Note that biomass refers to organic resources other than fossil resources originating from animals and plants, and biomass-derived refers to a compound produced using biomass as a raw material.

[0059] From the viewpoint of excellent production efficiency of the target compound, the ethanol content in the mixed raw material is preferably 30% by mass or more, more preferably 40% by mass or more, and even more preferably 50% by mass or more.

[0060] In the reaction process of this embodiment, ethanol is first converted to ethylene. Ethanol is more reactive than olefins having four or more carbon atoms, and increasing the ethanol content in the mixed feedstock improves the production efficiency of the target compounds, light olefins such as propylene and ethylene. The high reactivity of ethanol is due to the ease with which these substrates can access the zeolite reaction active sites. In other words, ethanol and ethylene, which have two carbon atoms, have smaller molecular sizes than olefins having four or more carbon atoms, and are less susceptible to steric hindrance within the zeolite pores. The high reactivity of ethanol is also due to the fact that ethanol has a functional group containing a heteroatom, i.e., the electron imbalance within the molecule.

[0061] Although a similar effect can be expected by using a large amount of ethylene as the mixed feedstock, from the viewpoint of stable operation of the apparatus, it is preferable to increase the ratio of raw materials with a carbon number of 2 in the mixed feedstock by using ethanol. This is because the process of converting ethylene to the target compound is an exothermic reaction, and if ethylene is contained in excess, the temperature inside the reactor will rise, accelerating coking of the catalyst.

[0062] The mixed feedstock may contain ethylene in addition to ethanol, from the viewpoint of ease of changing the feedstock composition. Ethylene produced by various production methods can be used. For example, ethylene obtained by thermal decomposition of naphtha and / or ethane, direct or oxidative dehydrogenation of ethane, or dehydration of ethanol can be used. Among these, the mixed feedstock preferably contains ethylene and water, such as gas obtained through the dehydration of ethanol. Ethylene generally contains water because water is by-produced in the process of converting ethanol to ethylene. From the viewpoint of excellent environmental friendliness, it is preferable to use ethylene obtained by dehydrating biomass-derived ethanol. The molar ratio of ethylene / ethanol in the mixed feedstock is preferably 0.20 to 2.50, more preferably 0.40 to 2.0, from the viewpoint of excellent ease of reaction control.

[0063] The mixed feedstock may further contain hydrocarbons having 4 to 6 carbon atoms. Examples of hydrocarbons having 4 to 6 carbon atoms include olefins having 4 to 6 carbon atoms and saturated hydrocarbons having 4 to 6 carbon atoms. Among these, olefins having 4 to 6 carbon atoms, like ethylene and ethanol, can produce target compounds such as propylene by contacting them with a zeolite-containing catalyst. Examples of hydrocarbons having 4 to 6 carbon atoms include butene, pentene, hexene, butane, pentane, and hexane. In the mixed feedstock, the molar ratio of olefins having 4 to 6 carbon atoms to ethylene is preferably 3.0 or less, more preferably 1.0 or less, and even more preferably 0.14 to 1.0. The term "olefin" as used above includes linear, branched, and cyclic olefins as well as cycloparaffins.

[0064] In the ethanol conversion method of this embodiment, the mixed feedstock may further contain an oxygenated compound having 1 to 6 carbon atoms other than ethanol. Similar to ethylene and ethanol, the oxygenated compound having 1 to 6 carbon atoms can provide a target compound such as propylene by contacting it with a catalyst. Examples of oxygenated compounds having 1 to 6 carbon atoms other than ethanol include methanol, propanol, dimethyl ether, and diethyl ether. In the mixed feedstock, the molar ratio of the oxygenated compound having 1 to 6 carbon atoms to ethylene is preferably 1.0 or less, and more preferably 0.5 or less.

[0065] Ethylene, ethanol, olefins having 4 to 6 carbon atoms, and oxygen-containing compounds having 1 to 6 carbon atoms other than ethanol are also collectively referred to as "effective raw materials."

[0066] The mixed feedstock may contain, in addition to the above-mentioned effective raw materials, saturated aliphatic hydrocarbons such as paraffin, olefins having 7 or more carbon atoms, and oxygen-containing compounds having 7 or more carbon atoms. These saturated aliphatic hydrocarbons, olefins having 7 or more carbon atoms, and oxygen-containing compounds having 7 or more carbon atoms can be converted into target compounds by contacting them with a conversion catalyst, similar to ethylene and ethanol, but have lower reactivity than the above-mentioned effective raw materials.

[0067] The mixed feedstock may contain an inert gas such as nitrogen in addition to the above-mentioned feedstocks that can be converted to propylene by the reaction step. The mixed feedstock may also contain hydrogen or methane as a diluent gas, but it is preferable not to dilute with hydrogen. Hydrogen is sometimes used to suppress catalyst coking deterioration, but at the same time, hydrogenation reactions of the produced propylene and the like occur, which has the adverse effect of reducing the propylene purity (propylene / (propylene + propane)) [mol / mol]. In the method of this embodiment, it is preferable not to dilute with hydrogen because the rate of catalyst coking deterioration is low and stable operation is possible even when hydrogen dilution is not performed.

[0068] The total content of ethylene and ethanol in the mixed raw material is preferably 30 to 100 mass %, more preferably 40 to 100 mass %, and even more preferably 50 to 100 mass %, based on the total amount of effective raw materials, provided that the mass of ethanol is calculated as ethylene.

[0069] The total content of olefins having 4 to 6 carbon atoms in the mixed raw material is preferably 65 mass % or less, more preferably 10 to 55 mass %, based on the total amount of effective raw materials.

[0070] The mixed raw material may contain diethyl ether, but preferably does not contain diethyl ether. The content of diethyl ether in the active ingredients is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 1% by mass or less.

[0071] In the conversion method of this embodiment, water can be included in the mixed feedstock. Since the ethylene and ethanol contained in the feedstock are produced by various production methods, they contain "water generated during the production process." Here, "water generated during the production process" refers to moisture that is generated during the production process of ethylene and / or ethanol and has not been removed. In the conversion method of this embodiment, water can be included in the mixed feedstock in addition to "water generated during the production process." Water has the effect of suppressing coking deterioration by lowering the olefin partial pressure and improving the yield of lower olefins. On the other hand, from the viewpoint of excellent production efficiency of the target compound per feedstock flow rate, it is preferable not to include water in the mixed feedstock in addition to "water generated during the production process."

[0072] [Reaction Conditions] The reaction temperature in the reaction step is preferably 400 to 600°C, more preferably 450 to 580°C, and even more preferably 480 to 550°C, from the viewpoint of achieving a high yield of the target compound.

[0073] When an adiabatic reactor is used, the reaction temperature is as follows. The inlet temperature of the catalyst bed is the temperature of the raw material immediately before the raw material fluid comes into contact with the catalyst bed packed in the adiabatic reactor. The outlet temperature of the catalyst bed is the temperature of the reaction gas immediately after it has passed through the catalyst bed. The temperatures of the raw material and reaction gas referred to here refer to temperatures between 0d and 0.8d in a plane perpendicular to the fluid flow direction, where 0 is the center of the reactor and d is the distance from the center of the reactor to the inner wall surface of the reactor. The average inlet and outlet reaction temperature is a value (hereinafter simply referred to as the "reaction temperature") calculated by measuring the inlet temperature of the catalyst bed and the outlet temperature of the catalyst bed, as shown in FIG. 1, and using the formula: [inlet temperature of the catalyst bed + outlet temperature of the catalyst bed] / 2. When an adiabatic reactor is used, the inlet temperature of the catalyst bed is preferably 480°C to 550°C, and the outlet temperature of the catalyst bed is preferably 480°C to 550°C. The temperature difference between the outlet temperature of the catalyst bed and the inlet temperature of the catalyst bed is preferably -80K to 80K, more preferably -60K to 60K.

[0074] The reaction pressure in the reaction step is preferably 0.01 to 3.0 MPaG, more preferably 0.01 to 1.0 MPaG.

[0075] The feed rate of the effective raw material is preferably 0.1 to 1000 hr in terms of the mass hourly space velocity (WHSV) of the zeolite-containing catalyst. -1 and more preferably 0.1 to 100 hours. -1 , more preferably 0.5 to 50 hours -1 In the reaction step, the WHSV is calculated by converting ethanol into ethylene as shown in the following formula: From the viewpoint of excellent productivity of the target compound, the mass flow rate of the effective raw material supply is preferably 1 kg / hr or more, more preferably 10 kg / hr or more, and even more preferably 1 t / hr or more.

[0076] WHSV (hr -1 ) = effective raw material supply flow rate (kg / hr) / catalyst amount (kg)

[0077] Effective raw material flow rate (kg / hr) = ethylene flow rate (kg / hr) + ethylene-equivalent ethanol flow rate (kg / hr) + C4-C6 olefin flow rate (kg / hr) + C1-C6 oxygen-containing compound flow rate (kg / hr) other than ethanol

[0078] Ethylene-equivalent ethanol flow rate (kg / hr) = ethanol flow rate (kg / hr) × ethylene molecular weight (g / mol) / ethanol molecular weight (g / mol)

[0079] [Regeneration Step] The ethanol conversion method of this embodiment may include a regeneration step (hereinafter also referred to as the "regeneration step") in which the zeolite-containing catalyst subjected to the reaction step is contacted with an oxygen-containing gas heated to 400°C or higher and then subjected to the reaction step again. When a zeolite-containing catalyst is used in a reaction for a long period of time, coke accumulates on the catalyst, causing coking degradation. The regeneration step allows the coke deposited on the zeolite-containing catalyst to be burned. Examples of the oxygen-containing gas used in the regeneration step include air and a mixture of air or oxygen and an inert gas. The oxygen concentration in the contact gas is preferably 0.1 to 2.0% by volume. The contact temperature with the gas is preferably at least 20°C higher (preferably 30°C higher, more preferably 40°C higher) than the temperature in the reaction step. Specifically, the contact temperature may be 400 to 700°C. In the regeneration step, the zeolite catalyst used in the reaction step contains water derived from the steam generated in the reaction step, and water is generated by burning the coke. Therefore, in the regeneration step, the zeolite catalyst comes into contact with water vapor under temperature conditions of 400°C or higher, which promotes the structural collapse of zeolite. However, as shown in this embodiment, by controlling the amount of TPD acid in a specific zeolite-containing catalyst, the affinity between zeolite and water (water vapor) can be reduced, thereby suppressing deterioration of catalytic activity. It is possible to employ either of the following regeneration methods: out-of-reactor regeneration, in which the catalyst is extracted from the reactor and regenerated outside the reactor, or in-reactor regeneration, in which the catalyst is regenerated within the reactor without being extracted from the reactor. Furthermore, by employing a switching reactor, reaction-regeneration switching operation can be performed.

[0080] (Reaction-regeneration switching operation) Reaction-regeneration switching operation is an operation in which a reaction step and a regeneration step are carried out simultaneously using a two-tower or multi-tower switching reactor. For example, in the case of a three-tower switching reactor, two towers are used for the reaction step, and at the same time, the remaining tower is used for catalyst regeneration. Thereafter, the reaction step in one of the towers used for the reaction step is stopped to perform catalyst regeneration, and the reaction step is carried out in the one tower used for catalyst regeneration, thereby enabling catalyst regeneration while maintaining the production capacity of the two towers. This type of reaction format is also called a merry-go-round system, and is preferred from the viewpoint of excellent production efficiency because it does not require stopping the production process for catalyst regeneration.

[0081] [Product: Reaction Gas Containing Olefins Having 3 or More Carbon Atoms] In the conversion method of this embodiment, a reaction gas containing olefins having 3 or more carbon atoms is obtained by contacting a raw material with a zeolite-containing catalyst. The reaction gas may contain ethylene. The reaction gas may contain hydrogen, aliphatic hydrocarbons having 1 to 3 carbon atoms, aliphatic hydrocarbons having 4 to 6 carbon atoms, aromatic compounds, and hydrocarbons having 9 or more carbon atoms. In the conversion method of this embodiment, the aliphatic hydrocarbons having 1 to 3 carbon atoms, aliphatic hydrocarbons having 4 to 6 carbon atoms, aromatic compounds, and hydrocarbons having 9 or more carbon atoms are referred to as target compounds.

[0082] [Separation Step] In the conversion method according to this embodiment, a separation step is provided, and various separation operations are carried out to efficiently purify the target compound. Among these, it is preferable to include a step of separating the reaction gas obtained in the above-described reaction step into a fraction A containing mainly hydrocarbons having 2 to 3 carbon atoms and a fraction B containing mainly hydrocarbons having 4 to 6 carbon atoms using a separation device. By separating the reaction gas into each fraction in this manner, the target compound can be efficiently separated. Examples of separation devices used in the separation step include a distillation column, a quench column, and a decanter.

[0083] The reaction gas obtained in the above-mentioned reaction step or a fraction separated from the reaction gas (hereinafter also referred to as a "connected fraction") may be introduced into a purification system of an ethylene plant to separate target compounds such as ethylene, propylene, aromatic compounds, etc.

[0084] The method according to this embodiment may be carried out in an apparatus having a reactor 1 and a first distillation column 2, as shown in FIG. 2. The reaction gas obtained in the reaction step carried out in the reactor 1 is separated in the first distillation column 2 into a fraction A mainly containing hydrocarbons having 1 to 3 carbon atoms and a fraction B mainly containing hydrocarbons having 4 to 6 carbon atoms. Ethylene is separated from fraction A in a distillation column (not shown), and propylene is further separated in a distillation column (not shown), thereby efficiently separating ethylene and propylene from the reaction gas. Furthermore, although not shown, at least a portion of the reaction gas and / or fraction A may be introduced into a purification system of an ethylene plant, and target compounds such as ethylene and propylene may be separated from the reaction gas in the purification system.

[0085] As shown in FIG. 3 , the method according to this embodiment can be carried out using an apparatus including a reactor 1, a cooler 3, an oil-water separator 4, and a first distillation column 2. The reaction gas obtained in the reaction step carried out in the reactor 1 is separated in the cooler 3 into a fraction C mainly containing hydrocarbons having 1 to 6 carbon atoms and a fraction D mainly containing water, hydrocarbons having 7 or more carbon atoms, and aromatic compounds. The phrase "mainly containing water, hydrocarbons having 7 or more carbon atoms, and aromatic compounds" in fraction D means that the total amount of water, hydrocarbons having 7 or more carbon atoms, and aromatic compounds is more than 50 mass% of the total amount of fraction D. In the first distillation column 2, fraction C is separated into a fraction A mainly containing hydrocarbons having 1 to 3 carbon atoms and a fraction B mainly containing hydrocarbons having 4 to 6 carbon atoms. In the oil-water separator 4, fraction D is separated into a fraction E mainly containing hydrocarbons having 7 or more carbon atoms and aromatic compounds, and a fraction F mainly containing water. By introducing fraction E into a purification system, aromatic compounds can be efficiently purified. In this way, target compounds such as propylene and aromatic compounds can be efficiently purified by separating the reaction gas into fraction A, fraction B, and fraction E. At least a portion of fraction A, fraction B, and fraction E may be introduced into a purification system of an ethylene plant, and target compounds such as ethylene, propylene, and aromatic compounds may be separated from the reaction gas in the purification system.

[0086] The term "mainly comprises" in each fraction means that the total mass of the components described as "mainly comprises" exceeds 50 mass% of each fraction. These separation steps can be carried out by combining various known methods such as distillation and extraction.

[0087] As described above, various hydrocarbons can be obtained by the ethanol conversion method of this embodiment. In other words, from another aspect, the ethanol conversion method of this embodiment is a method for producing hydrocarbons. The hydrocarbons may be either saturated hydrocarbons or unsaturated hydrocarbons. Examples of unsaturated hydrocarbons include olefins and aromatic hydrocarbon compounds.

[0088] [Method for Producing Hydrocarbons, etc.] Various chemical products can be obtained by separating target compounds from the reaction gas obtained by this embodiment. That is, the method for producing hydrocarbons according to this embodiment includes contacting a mixed feedstock containing ethylene and ethanol with a catalyst in an adiabatic reactor to obtain a reaction gas containing olefins having three or more carbon atoms. Details of this production method are as described above for the ethanol conversion method, and preferred embodiments thereof are also the same.

[0089] Examples of hydrocarbons obtainable by this production method include aliphatic unsaturated hydrocarbons such as olefins such as propylene, ethylene, butene, pentene, hexene, and heptene, dienes such as 1,3-butadiene and isoprene, aromatic hydrocarbons such as benzene and toluene, and aliphatic saturated hydrocarbons such as ethane, propane, butane, and pentane. The aromatic hydrocarbons preferably have a boiling point of 500° C. or lower at normal pressure.

[0090] By introducing the obtained hydrocarbons into the cracker's purification system, the target hydrocarbon compounds can be efficiently purified. The hydrocarbon production method according to this embodiment includes: a cracking step for cracking hydrocarbons having two or more carbon atoms; and a purification step for purifying the components obtained in the cracking step. In the purification step, the reaction gas or its purified fraction obtained by the above-described ethanol conversion method is combined. With the above configuration, the target hydrocarbons can be obtained from ethanol resources using a conventional cracker. For example, bio-derived hydrocarbons can be produced by using bioethanol as a raw material in the ethanol conversion method.

[0091] Examples of hydrocarbons having two or more carbon atoms include ethylene, propylene, butene, paraffin, and aromatic hydrocarbons. Naphtha may also be used as the hydrocarbon having two or more carbon atoms.

[0092] As the cracker, a thermal cracking furnace used in an ethane cracker, naphtha cracker, etc. may be used.

[0093] In the purification step, a purification system used in a conventional ethane cracker or naphtha cracker may be used, and distillation may be carried out using equipment equipped with, for example, a distillation column, a quench column, etc.

[0094] The reaction gas or purified fraction thereof obtained by the above-mentioned method for converting ethanol is joined in the above-mentioned purification step, and the joining point is appropriately selected depending on the components to be joined.

[0095] The method for producing a monomer according to this embodiment includes an unsaturated hydrocarbon separation step of separating a fraction mainly containing unsaturated hydrocarbons from the reaction gas obtained by the above-described ethanol conversion method. Examples of unsaturated hydrocarbons include aliphatic unsaturated hydrocarbons such as olefins such as propylene, ethylene, butene, butane, pentene, hexene, and heptene, and dienes such as 1,3-butadiene and isoprene.

[0096] The olefin production method according to this embodiment includes an olefin separation step of separating a fraction mainly containing olefins from the reaction gas obtained by the above-described ethanol conversion method.

[0097] The propylene production method according to this embodiment includes a propylene separation step of separating a fraction mainly containing propylene from the reaction gas obtained by the above-described ethanol conversion method.

[0098] The ethylene production method according to this embodiment includes an ethylene separation step of separating a fraction mainly containing ethylene from the reaction gas obtained by the above-described ethanol conversion method.

[0099] The diene production method according to this embodiment includes a diene separation step of separating a fraction mainly containing dienes from the reaction gas obtained by the above-described ethanol conversion method.

[0100] The method for producing a monomer according to this embodiment may further include a step of converting the unsaturated hydrocarbon.

[0101] The method for producing an acrylic monomer according to this embodiment includes: an unsaturated hydrocarbon separation step of separating a fraction mainly containing unsaturated hydrocarbons from the reaction gas obtained by the above-described ethanol conversion method; and an acrylic monomer production step of obtaining an acrylic monomer from the unsaturated hydrocarbons obtained by the unsaturated hydrocarbon separation step. In the acrylic monomer production step, a known method for introducing an acrylic monomer from an unsaturated hydrocarbon is used.

[0102] The method for producing acrylonitrile according to this embodiment includes: a propylene separation step of separating a fraction mainly containing propylene from the reaction gas obtained by the above-mentioned ethanol conversion method; and an acrylonitrile production step of obtaining acrylonitrile from the propylene obtained by the propylene separation step. In the acrylic monomer production step, a known method of introducing an acrylic monomer from an unsaturated hydrocarbon is used.

[0103] The method for producing styrene according to this embodiment includes an ethylene separation step of separating a fraction mainly containing ethylene from the reaction gas obtained by the above-described method for converting ethanol, and a styrene production step of obtaining styrene from the ethylene obtained by the ethylene separation step.

[0104] The monomer obtained by the above-mentioned production method may be further polymerized. The method for producing a polymer according to this embodiment includes the step of polymerizing the monomer obtained by the above-mentioned method for producing a monomer. The step of polymerizing the monomer can be carried out using a conventional polymerization method, and various initiators and polymerization catalysts can be used for the polymerization.

[0105] The method for producing an olefin polymer according to the present embodiment includes a step of polymerizing a polymerizable composition containing an olefin obtained by the above-described method for producing an olefin. Here, the polymerizable composition may contain an olefin alone as a monomer, or may contain another monomer having an unsaturated bond.

[0106] The method for producing a polypropylene-based polymer according to the present embodiment includes a step of polymerizing a polymerizable composition containing propylene obtained by the above-described method for producing propylene. Here, the polymerizable composition may contain propylene alone as a monomer, or may contain other monomers having an unsaturated bond.

[0107] The method for producing a polyethylene polymer according to the present embodiment includes a step of polymerizing a polymerizable composition containing ethylene obtained by the above-described method for producing ethylene. Here, the polymerizable composition may contain ethylene alone as a monomer, or may contain another monomer having an unsaturated bond.

[0108] The method for producing a diene polymer according to the present embodiment includes a step of polymerizing a polymerizable composition containing a diene obtained by the above-described method for producing a diene. The polymerizable composition may contain only a diene as a monomer, or may contain another monomer having an unsaturated bond.

[0109] The method for producing an acrylic monomer-based polymer according to this embodiment includes a step of polymerizing a polymerizable composition containing an acrylic monomer obtained by the above-described method for producing an acrylic monomer. Here, the polymerizable composition may contain only the acrylic monomer as the monomer, or may contain another monomer having an unsaturated bond.

[0110] The method for producing an acrylonitrile polymer according to the present embodiment includes a step of polymerizing a polymerizable composition containing acrylonitrile obtained by the above-mentioned method for producing acrylonitrile. Here, the polymerizable composition may contain acrylonitrile alone as a monomer, or may contain other monomers having an unsaturated bond.

[0111] The method for producing a styrene-based polymer according to the present embodiment includes a step of polymerizing a polymerizable composition containing styrene obtained by the above-described method for producing styrene. Here, the polymerizable composition may contain styrene alone as a monomer, or may contain other monomers having an unsaturated bond.

[0112] Aromatic compounds may be separated from the reaction gas obtained by the above-described ethanol conversion method. The method for producing an aromatic compound according to this embodiment includes an aromatic compound separation step of separating a fraction mainly containing aromatic compounds from the reaction gas obtained by the above-described ethanol conversion method. Examples of aromatic hydrocarbons include benzene, toluene, and xylene.

[0113] The present embodiment will be described in more detail below with reference to examples, but the present embodiment is not limited to the following examples.

[0114] [Methods for Measuring Catalyst Properties] Various physical properties of the catalyst were measured as follows.

[0115] (1) Silica / Alumina Molar Ratio of Zeolite Zeolite was completely dissolved in a sodium hydroxide solution to prepare a solution. The amounts of Si and Al contained in the solution were measured using an inductively coupled plasma (ICP) emission spectrometer (Rigaku, product name "JY138") in a standard manner, and the silica / alumina molar ratio was derived from the results. The measurement conditions were set as follows: high-frequency power: 1 kW, plasma gas: 13 L / min, sheath gas: 0.15 L / min, nebulizer gas: 0.25 L / min, Si measurement wavelength: 251.60 nm, and Al measurement wavelength: 396.152 nm.

[0116] (2) Al Content and Si Content in Zeolite-Containing Catalyst A solution was prepared by completely dissolving the zeolite-containing catalyst in a sodium hydroxide solution, and the amount of aluminum (Al) in the zeolite-containing catalyst was measured and calculated in the same manner as in (1).

[0117] (3) Content of Doping Element in Zeolite-Containing Catalyst The content of the doping element in the zeolite-containing catalyst was measured by a conventional method using an X-ray fluorescence analyzer (manufactured by Rigaku, trade name "RIX3000").

[0118] (4) Structural Type of Zeolite The structural type of zeolite in the zeolite-containing catalyst was identified by measuring the X-ray diffraction pattern of the zeolite using an X-ray analyzer (manufactured by Bruker, trade name "D8 Advance") and referring to the diffraction patterns of known zeolites. The measurement conditions were as follows: Cu cathode, tube voltage: 40 kV, tube current: 40 mA, scan speed: 6 deg / min.

[0119] (5) TPD Acid Amount Per Zeolite-Containing Catalyst Weight and TPD Acid Amount Per Zeolite Weight The TPD acid amount of a zeolite-containing catalyst, "the acid amount determined from the amount of ammonia desorbed at 100 to 650°C in ammonia temperature-programmed desorption measurement," was measured using a BELCAT II temperature-programmed desorption spectrometer by the following method. As a pretreatment, 1.0 g of a catalyst sample was heated to 650°C in He gas and then cooled to 100°C. Next, while the catalyst sample was heated to 100°C, 5 vol% ammonia gas diluted with helium gas was passed through to adsorb ammonia onto the catalyst sample. After that, while the catalyst sample was heated to 100°C, helium gas containing saturated water vapor at 80°C was passed through to remove the ammonia physically adsorbed onto the catalyst. Helium gas was passed through the catalyst at a flow rate of 50 mL / min. After the catalyst was held at 100°C for 90 minutes, the temperature was increased from 100°C to 850°C at a heating rate of 5°C / min to measure the amount of ammonia desorption. Mass spectrometry at m / z = 16 was used to detect the desorbed ammonia. The area of ​​the mass spectrum obtained from the measurement was calculated from the point where the temperature began to rise from 100°C to 850°C until the point where 650°C was reached. The TPD acid amount per zeolite-containing catalyst weight was calculated using the calibration curve method. The TPD acid amount per zeolite weight was calculated from the TPD acid amount per zeolite-containing catalyst weight and the weight ratio of the zeolite. (Acid Amount Retention Rate) In this example, the zeolite-containing catalyst was subjected to steam treatment (STM treatment) and the acid amount was observed over time to calculate the acid amount retention rate. The steam treatment for calculating the acid amount retention rate was carried out by bubbling helium gas at a flow rate of 50 mL / min into water heated to 80°C, lowering the temperature to 75°C using a condenser, and then contacting the water with a zeolite-containing catalyst heated to 650°C. The acid amount retention rate, which indicates the deterioration resistance of the zeolite-containing catalyst under hydrothermal conditions, was calculated using the following formula: Acid amount retention rate (%) = Acid amount after 6.0 hr STM treatment (µmol / g) / Acid amount after 1.0 hr STM treatment (µmol / g) × 100

[0120] (6) Mesopore Volume of Zeolite-Containing Catalyst The mesopore volume of the zeolite-containing catalyst was measured using a mercury intrusion porosimeter (Autopore 9500 manufactured by MicroMeritics) by the following method. First, as a pretreatment, the zeolite-containing catalyst was coarsely crushed and sieved to adjust the particle size. After the particle size adjustment, the sample was dried, and then 0.5 g of the sample was introduced into a measurement cell, filled with mercury, and pressurized. The mesopore volume was calculated from the amount of mercury intrusion obtained.

[0121] (7) Sodium Content in Zeolite-Containing Catalyst The sodium content in the zeolite-containing catalyst was measured by a conventional method using an X-ray fluorescence analyzer (manufactured by Rigaku, product name "RIX3000") (hereinafter also simply referred to as "XRF analysis").

[0122] (Na / Al Molar Ratio) The Na / Al molar ratio was calculated using the following formula: Na / Al molar ratio of zeolite-containing catalyst = [sodium content (mass%) / atomic weight of sodium] / [(aluminum content (mass%) / atomic weight of aluminum]

[0123] (8) Strength of Zeolite-Containing Catalyst The strength of the zeolite-containing catalyst was calculated using a digital hardness tester (manufactured by Fujiwara Seisakusho, product name "KHT-40"). Catalyst samples were prepared by drying at 120°C for 3 hours or more, and the crushing strength in the diameter direction was measured using a hardness tester equipped with a 3 mm diameter indenter (unit: N). 30 samples were measured, and the average value was divided by 3 to obtain a value (unit: N / mm) that was defined as the strength of the zeolite-containing catalyst.

[0124] (9) Coke Amount The coke amount was calculated by the following method. After the reaction, the zeolite-containing catalyst was crushed, and the weight loss rate was measured in the temperature range of 500°C to 700°C using a thermogravimetric differential thermal analyzer. The weight loss rate was divided by the effective raw material supply mass, and the resulting value (unit: mass ppm) was defined as the coke amount. Effective raw material supply mass (kg) = Effective raw material supply mass flow rate (kg / hr) × Time from start to finish of reaction (hr) [Analysis conditions for thermogravimetric differential thermal analyzer] Apparatus: TG-DTA8122 manufactured by Rigaku Sample container: Pt pan (φ5 mm × 2.5 mmh) Reference sample: α-alumina Atmosphere: Air (500 cc / min) Temperature: (1) Heat from room temperature to 120°C at 20°C / min (2) Hold at 120°C for 10 minutes (3) Heat from 120°C to 900°C at 10°C / min

[0125] [Method for Conversion of Ethanol] (Reactor) In the following examples and comparative examples, evaluations were carried out using a fixed-bed single-stage adiabatic reactor 1 shown in FIG.

[0126] (Temperature Measurement) The temperatures at the catalyst bed inlet and catalyst bed outlet were measured using thermocouples inserted from outside the reactor. Specifically, as shown in Figure 1, in a plane perpendicular to the fluid flow direction, the center of the reactor is defined as 0, and the distance from the center of the reactor to the inner wall surface of the reactor is defined as d, and the temperatures were measured at 0.5d to 0.6d. Note that the effect of heat radiation due to the insertion of the thermocouples was negligibly small. Furthermore, the thermocouple was moved in the fluid flow direction as necessary to measure the lowest temperature inside the reactor.

[0127] (Feedstock) The following examples were carried out using a feedstock containing ethanol. The feedstock may contain ethylene, 1-butene, and water in addition to ethanol. The molar ratio of ethylene / ethanol and the molar ratio of C4-C6 olefins / ethylene in the feedstock were calculated using the following formulas.

[0128] Ethylene / ethanol molar ratio (-) = ethylene molar flow rate (mol / hr) / ethanol molar flow rate (mol / hr)

[0129] Molar ratio of C4-C6 olefin / ethylene (-)=flow rate of C4-C6 olefin (mol / hr) / molar flow rate of ethylene (mol / hr) (Reaction evaluation of reaction step)

[0130] According to the following examples and comparative examples, reactions were carried out so that the average inlet and outlet reaction temperature was 530°C or 500°C. A portion of the gas at the reactor outlet was sampled every 3 hours from the start of the reaction and introduced into a gas chromatograph (TCD (Thermal Conductivity Detector), FID (Flame Ionization Detector) detector) to analyze the reaction gas composition. The reaction was stopped 48 hours after the start of the reaction. The average value of the GC analysis results from the start of the reaction to the end of the reaction was calculated. The average inlet and outlet reaction temperature was calculated according to the following formula: Average inlet and outlet reaction temperature (°C) = [Catalyst bed inlet temperature (°C) + Catalyst bed outlet temperature (°C)] / 2

[0131] [Gas chromatograph analysis conditions] (Reaction gas analysis) Apparatus: GC-2030 manufactured by Shimadzu Corporation Column: Custom capillary column SPB-1 manufactured by SUPELCO, USA (inner diameter 0.25 mm, length 60 m, film thickness 3.0 μm) Sample gas amount: 1 mL (sampling line kept at 200° C. to 300° C.) Heating program: held at 40° C. for 12 minutes, then heated to 200° C. at 5° C. / min, and then held at 200° C. for 22 minutes. Split ratio: 200:1 Carrier gas (nitrogen) flow rate: 120 mL / min FID detector: Air supply pressure 50 kPa (approximately 500 mL / min), hydrogen supply pressure 60 kPa (approximately 50 mL / min) Measurement method: The TCD detector and FID detector were connected in series, and composition analysis was performed based on data detected by the TCD detector for hydrogen and data detected by the FID detector for oxygenated substances such as hydrocarbons and ethanol, and the calibration curve method was used to determine the concentration of each component in the reaction gas and the mass per hour produced by the reaction.

[0132] (Ethylene Yield) The ethylene yield represents the selectivity to ethylene in the reaction step, and was calculated by the following formula: Ethylene yield (mass %) = Mass of ethylene produced per hour in the reaction step (kg / hr) / Effective raw material supply mass flow rate (kg / hr) × 100

[0133] (Ethylene Conversion Rate) Although the raw material in this embodiment does not necessarily contain ethylene, ethylene is produced in the reaction step in this embodiment, and since ethylene is the smallest olefin, the ethylene conversion rate derived from the mass of ethylene per hour in the reaction gas was used as an index for evaluating catalytic activity. The ethylene conversion rate was calculated using the following formula: Ethylene conversion rate (mass %) = (effective raw material supply mass flow rate (kg / hr) - ethylene mass per hour in the reaction gas (kg / hr)) / effective raw material supply mass flow rate (kg / hr) × 100

[0134] Effective raw material supply mass flow rate (kg / hr) = ethylene flow rate (kg / hr) + ethylene-equivalent ethanol flow rate (kg / hr) + C4-C6 olefin flow rate (kg / hr) + C1-C6 oxygen-containing compound flow rate (kg / hr)

[0135] Ethylene-equivalent ethanol flow rate (kg / hr) = ethanol flow rate (kg / hr) × ethylene molecular weight (g / mol) / ethanol molecular weight (g / mol)

[0136] (Propylene Yield) The propylene yield represents the selectivity to propylene in the reaction step and was calculated by the following formula.

[0137] Propylene yield (mass%) = propylene mass produced per hour in the reaction step (kg / hr) / effective raw material supply mass flow rate (kg / hr) × 100

[0138] (Aromatic Yield) The aromatic yield represents the selectivity to aromatic compounds in the reaction step, and was calculated by the following formula.

[0139] Aromatic yield (mass%) = mass of aromatics produced in the reaction step per hour (kg / hr) / effective raw material supply mass flow rate (kg / hr) × 100

[0140] Effective raw material supply mass flow rate (kg / hr) = ethylene flow rate (kg / hr) + ethylene-equivalent ethanol flow rate (kg / hr) + C4-C6 olefin flow rate (kg / hr) + C1-C6 oxygen-containing compound flow rate (kg / hr)

[0141] Ethylene-equivalent ethanol flow rate (kg / hr) = ethanol flow rate (kg / hr) × ethylene molecular weight (g / mol) / ethanol molecular weight (g / mol)

[0142] (Yield Maintenance Rate) In Examples 1 to 6 and Comparative Example 1, a 48-hour reaction was defined as one cycle, and the maintenance rate of ethylene conversion after 24 hours, the maintenance rate of ethylene conversion after 48 hours, the maintenance rate of propylene yield after 24 hours, the maintenance rate of propylene yield after 48 hours, the maintenance rate of aromatics yield after 24 hours, and the maintenance rate of aromatics yield after 48 hours were calculated by the following formulas.

[0143] In Examples 7 to 14 and Comparative Examples 3 to 5, the catalyst was further regenerated after the first cycle to remove accumulated coke, and a second cycle was carried out under the same conditions. The maintenance rates of the ethylene conversion rate after regeneration, the propylene yield after regeneration, and the aromatics yield after regeneration were calculated using the following formulas.

[0144] Maintenance rate of ethylene conversion after 24 hours (mass%)=ethylene conversion rate (mass%) at 24 hours after the start of the reaction in the first cycle / ethylene conversion rate (mass%) at 3 hours after the start of the reaction in the first cycle×100

[0145] Maintenance rate of ethylene conversion after 48 hours (mass%)=ethylene conversion rate (mass%) at 48 hours after the start of the reaction in the first cycle / ethylene conversion rate (mass%) at 3 hours after the start of the reaction in the first cycle×100

[0146] Maintenance rate of ethylene conversion rate after regeneration (mass%)=ethylene conversion rate (mass%) at 3 hours after the start of the reaction in the second cycle / ethylene conversion rate (mass%) at 3 hours after the start of the reaction in the first cycle×100

[0147] Maintenance rate of propylene yield after 24 hours (mass%) = Propylene yield (mass%) at 24 hours after the start of the reaction in the first cycle / Propylene yield (mass%) at 3 hours after the start of the reaction in the first cycle × 100

[0148] Maintenance rate of propylene yield after 48 hours (mass%) = Propylene yield (mass%) at 48 hours after the start of the reaction in the first cycle / Propylene yield (mass%) at 3 hours after the start of the reaction in the first cycle × 100

[0149] Maintenance rate of propylene yield after regeneration (mass%) = Propylene yield (mass%) at 3 hours after the start of the reaction in the second cycle / Propylene yield (mass%) at 3 hours after the start of the reaction in the first cycle × 100

[0150] Maintenance rate of aromatic yield after 24 hours (mass%) = aromatic yield (mass%) at 24 hours after the start of the first cycle reaction / aromatic yield (mass%) at 3 hours after the start of the first cycle reaction × 100

[0151] Maintenance rate of aromatic yield after 48 hours (mass%) = aromatic yield (mass%) at 48 hours after the start of the first cycle reaction / aromatic yield (mass%) at 3 hours after the start of the first cycle reaction × 100

[0152] Maintenance rate of aromatic yield after regeneration (mass%)=aromatic yield (mass%) at 3 hours after the start of the reaction in the second cycle / aromatic yield (mass%) at 3 hours after the start of the reaction in the first cycle×100

[0153] [Production Example 1: Preparation of Zeolite-Containing Catalyst 1] Clay obtained from 70 parts by mass of proton-type ZSM-5 (silica / alumina molar ratio 980), a medium pore diameter zeolite, and 89 parts by mass of colloidal silica liquid equivalent to 30 parts by mass of silica (silica 33.8% by mass, sodium content relative to the total amount of colloidal silica liquid 28 ppm by mass) was kneaded and then extrusion-molded to obtain an extruded molded body adjusted to a diameter of 2.1 mm and a length of 4 to 6 mm. The obtained molded body was calcined at 600 ° C. for 5 hours to obtain zeolite-containing catalyst 1. At this time, the content of sodium element contained in the zeolite-containing catalyst was 55 ppm by mass.

[0154] [Production Example 2: Preparation of Zeolite-Containing Catalyst 2] Clay obtained from 70 parts by mass of proton-type ZSM-5 (silica / alumina molar ratio 980), a medium pore size zeolite, and 89 parts by mass of colloidal silica equivalent to 30 parts by mass (silica 33.8% by mass, sodium content 28 ppm by mass relative to the total amount of colloidal silica liquid) was kneaded and then extrusion-molded to obtain an extruded molded body adjusted to a diameter of 2.1 mm and a length of 4 to 6 mm. The obtained molded body was calcined at 600 ° C. for 5 hours to obtain a catalyst precursor. The obtained catalyst precursor was stirred in a 0.1 N aqueous sodium nitrate solution for 1 hour, filtered and washed, and calcined at 600 ° C. for 5 hours to obtain a sodium-exchanged body. The sodium-exchanged body was stirred in a 0.01 N aqueous silver nitrate solution for 1 hour, and then the filtration and washing process was repeated three times, followed by calcination at 600 ° C. for 5 hours to obtain a silver-exchanged body. A steam-air mixed gas containing 80% by volume of steam was supplied to and circulated through the silver-exchanged body under conditions of a pressure of 0.1 MPa and a temperature of 600°C for 24 hours to obtain zeolite-containing catalyst 2. At this time, the silver content in the zeolite-containing catalyst was 0.16% by mass, and the sodium content was 46 ppm by mass.

[0155] [Production Example 3: Method for preparing zeolite-containing catalyst 3] Clay obtained from 70 parts by mass of proton-type ZSM-5 (silica / alumina molar ratio 980), a medium pore size zeolite, and 89 parts by mass of colloidal silica equivalent to 30 parts by mass (silica 33.8% by mass, sodium content 28 ppm by mass relative to the total amount of colloidal silica liquid) was kneaded and then extrusion-molded to obtain an extruded molded product adjusted to a diameter of 2.1 mm and a length of 4 to 6 mm. A predetermined amount of diammonium hydrogen phosphate aqueous solution was supported on the obtained molded product to obtain a phosphorus-supported product. The obtained phosphorus-supported product was calcined at 600 °C for 5 hours in an air atmosphere. The calcined product was charged into a reactor, and a steam-nitrogen mixed gas containing 80% by volume of steam was supplied and circulated for 24 hours under conditions of a pressure of 0.1 MPa and a temperature of 600 °C, to obtain zeolite-containing catalyst 3. At this time, the content of elemental phosphorus contained in the zeolite-containing catalyst was 0.032 mass %, and the content of elemental sodium was 76 mass ppm.

[0156] [Production Example 4: Preparation of Zeolite-Containing Catalyst 4] Clay obtained from 70 parts by mass of proton-type ZSM-5 (silica / alumina molar ratio 212), a medium pore size zeolite, and 89 parts by mass of colloidal silica equivalent to 30 parts by mass (silica 33.8% by mass, sodium content 28 ppm by mass relative to the total amount of colloidal silica liquid) was kneaded and then extrusion-molded to obtain an extruded molded product adjusted to a diameter of 1.6 mm and a length of 4 to 6 mm. A predetermined amount of diammonium hydrogen phosphate aqueous solution was supported on the obtained molded product to obtain a phosphorus-supported product. The obtained phosphorus-supported product was calcined for 5 hours at 600 °C in an air atmosphere. The calcined product was loaded into a reactor, and a steam-nitrogen mixed gas containing 80% by volume of steam was supplied and circulated for 24 hours under conditions of a pressure of 0.1 MPa and a temperature of 600 °C, to obtain zeolite-containing catalyst 4. At this time, the content of elemental phosphorus contained in the zeolite-containing catalyst was 0.14 mass %, and the content of elemental sodium was 253 mass ppm.

[0157] [Production Example 5: Preparation of Zeolite-Containing Catalyst 5] Clay obtained from 70 parts by mass of proton-type ZSM-5 (silica / alumina molar ratio 302), a medium pore size zeolite, and 89 parts by mass of colloidal silica equivalent to 30 parts by mass (silica 33.8% by mass, sodium content 28 ppm by mass relative to the total amount of colloidal silica liquid) was kneaded and then extrusion-molded to obtain an extruded molded product adjusted to a diameter of 1.6 mm and a length of 4 to 6 mm. A predetermined amount of diammonium hydrogen phosphate aqueous solution was supported on the obtained molded product to obtain a phosphorus-supported product. The obtained phosphorus-supported product was calcined at 600 °C for 5 hours in an air atmosphere. The calcined product was charged into a reactor, and a steam-nitrogen mixed gas containing 80% by volume of steam was supplied and circulated for 24 hours under conditions of a pressure of 0.1 MPa and a temperature of 600 °C, to obtain zeolite-containing catalyst 5. At this time, the content of elemental phosphorus contained in the zeolite-containing catalyst was 0.085 mass %, and the content of elemental sodium was 98 mass ppm.

[0158] [Production Example 6: Preparation of Zeolite-Containing Catalyst 6] After kneading clay obtained from 70 parts by mass of proton-type ZSM-5 (silica / alumina molar ratio 150), which is a medium pore size zeolite, and 89 parts by mass of colloidal silica equivalent to 30 parts by mass (silica 33.8 mass%, sodium content 28 mass ppm relative to the total amount of colloidal silica liquid), extrusion molding was carried out to obtain an extruded molded body adjusted to a diameter of 1.6 mm and a length of 4 to 6 mm. The obtained molded body was dried at 350 ° C. for 5 hours and then calcined at 600 ° C. for 5 hours to obtain zeolite-containing catalyst 6. At this time, the content of sodium element contained in the zeolite-containing catalyst was 141 mass ppm.

[0159] [Production Example 7: Preparation of Zeolite-Containing Catalyst 7] After kneading clay obtained from 80 parts by mass of proton-type ZSM-5 (silica / alumina molar ratio 850), which is a medium pore size zeolite, and 59 parts by mass of colloidal silica equivalent to 20 parts by mass (silica 33.8% by mass, sodium content 28 mass ppm relative to the total amount of colloidal silica liquid), extrusion molding was carried out to obtain an extruded molded body adjusted to a diameter of 2.6 mm and a length of 4 to 6 mm. The obtained molded body was calcined at 600 ° C. for 5 hours to obtain a catalyst precursor. The obtained catalyst precursor was stirred in a 0.01 N silver nitrate aqueous solution for 1 hour, and then the filtration and washing process was repeated three times, followed by calcination at 600 ° C. for 5 hours to obtain zeolite-containing catalyst 7. At this time, the silver content contained in the zeolite-containing catalyst was 0.2339 mass%, and the sodium content was 10 mass ppm.

[0160] [Production Example 8: Preparation of zeolite-containing catalyst 8] A steam-air mixed gas containing 80% by volume of steam was supplied to and circulated through the zeolite-containing catalyst 7 under conditions of a pressure of 0.1 MPa and a temperature of 600°C for 24 hours, thereby obtaining a zeolite-containing catalyst 8.

[0161] [Production Example 9: Preparation of Zeolite-Containing Catalyst 9] After kneading clay obtained from 80 parts by mass of proton-type ZSM-5 (silica / alumina molar ratio 850), which is a medium pore size zeolite, and 59 parts by mass of colloidal silica equivalent to 20 parts by mass (silica 33.8% by mass, sodium content 28 mass ppm relative to the total amount of colloidal silica liquid), extrusion molding was carried out to obtain an extruded molded body adjusted to a diameter of 2.6 mm and a length of 4 to 6 mm. The obtained molded body was calcined at 600 ° C. for 5 hours to obtain a catalyst precursor. The obtained molded body was stirred in a 0.002 N silver nitrate aqueous solution for 1 hour, and then the filtration and washing process was repeated three times, followed by calcination at 600 ° C. for 5 hours to obtain zeolite-containing catalyst 9. At this time, the content of silver element contained in the zeolite-containing catalyst was 0.1360 mass%, and the content of sodium element was 14 mass ppm.

[0162] [Production Example 10: Preparation of zeolite-containing catalyst 10] A steam-air mixed gas containing 80% by volume of steam was supplied to and circulated through zeolite-containing catalyst 9 under conditions of a pressure of 0.1 MPa and a temperature of 600°C for 24 hours, thereby obtaining zeolite-containing catalyst 10.

[0163] [Production Example 11: Preparation of Zeolite-Containing Catalyst 11] Clay obtained from 80 parts by mass of proton-type ZSM-5 (silica / alumina molar ratio 850), a medium pore size zeolite, and 59 parts by mass of colloidal silica equivalent to 20 parts by mass (silica 33.8% by mass, sodium content 28 mass ppm relative to the total amount of colloidal silica liquid) was kneaded and then extrusion-molded to obtain an extruded molded body adjusted to a diameter of 2.6 mm and a length of 4 to 6 mm. The obtained molded body was calcined at 600 ° C. for 5 hours to obtain a catalyst precursor. The obtained catalyst precursor was stirred in a 0.1 N aqueous sodium nitrate solution for 1 hour, filtered and washed, and calcined at 600 ° C. for 5 hours to obtain a sodium-exchanged body. The sodium-exchanged body was stirred in a 0.01 N aqueous silver nitrate solution for 1 hour, and then the filtration and washing process was repeated three times, followed by calcination at 600 ° C. for 5 hours to obtain a silver-exchanged body. A steam-air mixed gas containing 80% by volume of steam was supplied to and circulated through the silver-exchanged body under conditions of a pressure of 0.1 MPa and a temperature of 600°C for 24 hours to obtain zeolite-containing catalyst 11. At this time, the silver content in the zeolite-containing catalyst was 0.2641% by mass, and the sodium content was 38 ppm by mass.

[0164] [Production Example 12: Preparation of Zeolite-Containing Catalyst 12] After kneading clay obtained from 80 parts by mass of proton-type ZSM-5 (silica / alumina molar ratio 850) which is a medium pore size zeolite and 59 parts by mass of colloidal silica equivalent to 20 parts by mass of silica (silica 33.8% by mass, sodium content 28 mass ppm relative to the total amount of colloidal silica liquid), extrusion molding was carried out, and an extruded molded body adjusted to a diameter of 2.6 mm and a length of 4 to 6 mm was obtained. The obtained molded body was calcined at 600 ° C. for 5 hours, stirred for 1 hour in a 0.001 N silver nitrate aqueous solution, and then filtered and washed three times. Zeolite-containing catalyst 12 was obtained by calcining for 5 hours at 600 ° C. At this time, the content of silver element contained in the zeolite-containing catalyst was 0.1899 mass%, and the content of sodium element was 61 mass ppm.

[0165] [Production Example 13: Preparation of Zeolite-Containing Catalyst 13] After kneading clay obtained from 70 parts by mass of proton-type ZSM-5 (silica / alumina molar ratio 980) which is a medium pore size zeolite and 89 parts by mass of colloidal silica equivalent to 30 parts by mass (silica 33.8% by mass, sodium content 28 mass ppm relative to the total amount of colloidal silica liquid), extrusion molding was carried out to obtain an extruded molded body adjusted to a diameter of 2.1 mm and a length of 4 to 6 mm. The obtained molded body was calcined at 600 ° C. for 5 hours, and immersed in 100 parts by mass of 0.1 N nitric acid per 10 parts by mass of the molded body for 1 hour at room temperature, followed by washing with water to obtain zeolite-containing catalyst 13. At this time, the content of sodium element contained in the zeolite-containing catalyst was 18 mass ppm.

[0166] [Production Example 14: Preparation of Zeolite-Containing Catalyst 14] After kneading clay obtained from 80 parts by mass of proton-type ZSM-5 (silica / alumina molar ratio 850) which is a medium pore size zeolite and 59 parts by mass of colloidal silica equivalent to 20 parts by mass (silica 33.8 mass%, sodium content 28 mass ppm relative to the total amount of colloidal silica liquid), extrusion molding was carried out to obtain an extruded molded body adjusted to a diameter of 2.6 mm and a length of 4 to 6 mm. The obtained molded body was calcined at 600 ° C. for 5 hours, and immersed in 100 parts by mass of 0.1 N nitric acid per 10 parts by mass of the molded body for 1 hour at room temperature, followed by washing with water to obtain a catalyst precursor. The obtained precursor was filled into a reactor, and a steam-nitrogen mixed gas containing 80% by volume of steam was supplied and circulated for 48 hours under conditions of a pressure of 0.1 MPa and a temperature of 600 ° C., to obtain a zeolite-containing catalyst 14. At this time, the content of elemental sodium contained in the zeolite-containing catalyst was 21 ppm by mass.

[0167] [Production Example 15: Preparation of Zeolite-Containing Catalyst 15] After kneading clay obtained from 80 parts by mass of proton-type ZSM-5 (silica / alumina molar ratio 850), which is a medium pore size zeolite, and 59 parts by mass of colloidal silica equivalent to 20 parts by mass (silica 33.8% by mass, sodium content 28 ppm by mass relative to the total amount of colloidal silica liquid), extrusion molding was carried out to obtain an extruded molded body adjusted to a diameter of 2.6 mm and a length of 4 to 6 mm. The obtained molded body was calcined at 600 ° C. for 5 hours, and immersed in 100 parts by mass of 0.1 N nitric acid per 10 parts by mass of the molded body for 1 hour at room temperature, followed by washing with water to obtain a catalyst precursor. A predetermined amount of diammonium hydrogen phosphate aqueous solution was supported on the obtained precursor to obtain a phosphorus-supported product. The obtained phosphorus-supported product was calcined at 600 ° C. for 5 hours in an air atmosphere to obtain zeolite-containing catalyst 15. At this time, the content of elemental phosphorus contained in the zeolite-containing catalyst was 0.1687 mass %, and the content of elemental sodium was 18 mass ppm.

[0168] [Production Example 16: Preparation of Zeolite-Containing Catalyst 16] After kneading clay obtained from 80 parts by mass of proton-type ZSM-5 (silica / alumina molar ratio 850), which is a medium pore size zeolite, and 59 parts by mass of colloidal silica equivalent to 20 parts by mass (silica 33.8% by mass, sodium content 28 mass ppm relative to the total amount of colloidal silica liquid), extrusion molding was carried out to obtain an extruded molded body adjusted to a diameter of 2.6 mm and a length of 4 to 6 mm. The obtained molded body was calcined at 600 ° C. for 5 hours, and immersed in 100 parts by mass of 0.1 N nitric acid per 10 parts by mass of the molded body for 1 hour at room temperature, followed by washing with water to obtain a catalyst precursor. A predetermined amount of diammonium hydrogen phosphate aqueous solution was supported on the obtained precursor to obtain a phosphorus-supported product. The obtained phosphorus-supported product was calcined at 600 ° C. for 5 hours in an air atmosphere to obtain zeolite-containing catalyst 16. At this time, the content of elemental phosphorus contained in the zeolite-containing catalyst was 0.0371 mass %, and the content of elemental sodium was 7 mass ppm.

[0169] [Production Example 17: Preparation of Zeolite-Containing Catalyst 17] After kneading clay obtained from 80 parts by mass of proton-type ZSM-5 (silica / alumina molar ratio 850), which is a medium pore size zeolite, and 59 parts by mass of colloidal silica equivalent to 20 parts by mass (silica 33.8 mass%, sodium content 28 mass ppm relative to the total amount of colloidal silica liquid), extrusion molding was carried out to obtain an extruded molded body adjusted to a diameter of 2.6 mm and a length of 4 to 6 mm. The obtained molded body was calcined at 600 ° C. for 5 hours to obtain a catalyst precursor. The obtained catalyst precursor was stirred in a 0.1 N aqueous sodium nitrate solution for 1 hour, filtered and washed, and calcined at 600 ° C. for 5 hours to obtain a sodium-exchanged body. The sodium-exchanged body was stirred in a 0.002 N aqueous silver nitrate solution for 1 hour, filtered and washed, and calcined at 600 ° C. for 5 hours to obtain a zeolite-containing catalyst 17. At this time, the silver content in the zeolite-containing catalyst was 0.1291 mass %, and the sodium content was 339 mass ppm.

[0170] [Production Example 18: Preparation of Zeolite-Containing Catalyst 18] After kneading clay obtained from 70 parts by mass of proton-type ZSM-5 (silica / alumina molar ratio 980), which is a medium pore diameter zeolite, and 89 parts by mass of colloidal silica equivalent to 30 parts by mass (silica 33.8 mass%, sodium content 28 mass ppm relative to the total amount of colloidal silica liquid), extrusion molding was carried out to obtain an extruded molded body adjusted to a diameter of 2.1 mm and a length of 4 to 6 mm. The obtained molded body was calcined at 600 ° C. for 5 hours to obtain zeolite-containing catalyst 18. At this time, the content of sodium element contained in the zeolite-containing catalyst was 156 mass ppm.

[0171] Example 1 (Evaluation of Catalyst Properties) The initial TPD acid amount of zeolite-containing catalyst 1 was 10.7 μmol / g, and the acid amount retention rate was 78.1%. The physical properties of the catalyst obtained by characterization are shown in Table 1. (Reaction Step) A mixed feedstock containing 19.2 mass% ethylene, 48.1 mass% ethanol, 18.1 mass% water, and 14.6 mass% 1-butene was supplied to a reactor packed with zeolite-containing catalyst 1 so as to achieve a WHSV of 2.2, a pressure of 0.15 MPaG, and a catalyst bed inlet temperature of 530°C, and a 48-hour reaction step was carried out. Three hours after the start of the reaction, the propylene yield was 18.4 mass%, and the aromatics yield was 3.5 mass%. After 48 hours, the propylene yield retention rate was 91.7%, and the aromatics yield retention rate was 60.2%. The reaction results are shown in Table 1 and FIG. 4.

[0172] [Example 2] (Regeneration Step) While the zeolite-containing catalyst 1 used in the reaction step in Example 1 was still packed in the reactor, the flow gas was switched from the raw material to nitrogen-diluted gas, and the regeneration step was carried out under the following conditions 1 to 5. The regenerated zeolite-containing catalyst 1 (regenerated catalyst) was used again in the reaction step. Procedure 1) Temperature: 480°C, Oxygen concentration: 1%, 1 hour Procedure 2) Temperature: 520°C, Oxygen concentration: 1%, 3 hours Procedure 3) Temperature: 550°C, Oxygen concentration: 1%, 3 hours Procedure 4) Temperature: 550°C, Oxygen concentration: 5%, 1 hour Procedure 5) Temperature: 580°C, Oxygen concentration: 5%, 2 hours (Reaction Step: Second Cycle) The reaction step was carried out in the same manner as in Example 1, except that a regenerated catalyst was used. After 48 hours, the propylene yield retention rate was 91.8%, and the aromatics yield retention rate was 63.1%. The reaction results are shown in Figure 4. (Reaction step: 3rd cycle) After the 2nd cycle reaction step was carried out, the regeneration step was carried out in the same manner as above, and the 3rd cycle reaction step was carried out. After 48 hours, the propylene yield was maintained at 92.4%, and the aromatics yield was maintained at 57.1%. The reaction results are shown in FIG. 4.

[0173] Example 3 The same procedure as in Example 1 was carried out except that zeolite-containing catalyst 2 was used. The initial TPD acid amount of zeolite-containing catalyst 2 was 10.3 μmol / g, and the acid amount retention rate was 93.5%. After 48 hours, the propylene yield retention rate was 93.6%, and the aromatics yield retention rate was 61.4%. The physical properties and reaction results of the catalyst obtained by characterization are shown in Table 1.

[0174] Example 4 The same procedure as in Example 1 was carried out except that zeolite-containing catalyst 3 was used. The initial TPD acid amount of zeolite-containing catalyst 3 was 11.3 μmol / g, and the acid amount retention rate was 81.5%. After 48 hours, the propylene yield retention rate was 92.1%, and the aromatics yield retention rate was 61.2%. The physical properties and reaction results of the catalyst obtained by characterization are shown in Table 1.

[0175] Example 5 The same procedure as in Example 1 was carried out except that zeolite-containing catalyst 4 was used. The initial TPD acid amount of zeolite-containing catalyst 4 was 40.9 μmol / g, and the acid amount retention rate was 73.1%. After 48 hours, the propylene yield retention rate was 79.4%, and the aromatics yield retention rate was 50.1%. The physical properties and reaction results of the catalyst obtained by characterization are shown in Table 1.

[0176] Example 6 The same procedure as in Example 1 was carried out except that zeolite-containing catalyst 5 was used. The initial TPD acid amount of zeolite-containing catalyst 5 was 32.1 mol / g, and the acid amount maintenance rate was 73.1%. After 48 hours, the propylene yield maintenance rate was 78.1%, and the aromatics yield maintenance rate was 52.1%. The physical properties and reaction results of the catalyst obtained by characterization are shown in Table 1.

[0177] Comparative Example 1 The same procedure as in Example 1 was carried out except that zeolite-containing catalyst 6 was used. The initial TPD acid amount of zeolite-containing catalyst 6 was 86.2 μmol / g, and the acid amount maintenance rate was 44.8%. Three hours after the start of the reaction, the propylene yield was 18.2 mass% and the aromatics yield was 3.1 mass%. After 48 hours, the propylene yield maintenance rate was 54.7% and the aromatics yield maintenance rate was 42.9%. The physical properties of the catalyst obtained by characterization and the reaction results are shown in Table 1.

[0178] Comparison of the Examples and Comparative Examples revealed that zeolite-containing catalysts exhibiting an initial TPD acid content of a certain amount or more significantly reduced the acid content retention rate. Furthermore, it was found that zeolite-containing catalysts with low acid content retention rates reduced the average yield of the target compound and could not be maintained.

[0179] The zeolite-containing catalyst 6 used in Comparative Example 1 was subjected to the regeneration step in the same manner as in Example 2. When the reaction step was carried out again using the obtained regenerated catalyst, the propylene yield was 12.2 mass % and the aromatics yield was 1.1 mass %, which were significantly lower than those of Comparative Example 1, 3 hours after the start of the reaction.

[0180]

[0181] [Example 7] (Evaluation of Catalyst Properties) The physical properties of zeolite-containing catalyst 7 obtained by characterization are shown in Table 2. (Reaction Evaluation) A mixed feedstock containing 28.1 mass% ethylene, 57.1 mass% ethanol, and 14.8 mass% water was supplied to a reactor packed with zeolite-containing catalyst 7 so as to achieve a WHSV of 2.2, a pressure of 0.15 MPaG, and an average catalyst bed temperature of 500°C, and a 48-hour reaction process was carried out. Three hours after the start of the reaction, the ethylene yield was 22.6 mass% (ethylene conversion rate 77.4 mass%), the propylene yield was 21.5 mass%, and the aromatics yield was 7.9 mass%. After 24 hours, the ethylene yield was 26.5 mass% (ethylene conversion rate 73.5 mass%), the propylene yield was 21.3 mass%, and the aromatics yield was 6.3 mass%. Subsequently, the zeolite-containing catalyst 7 used in the 48-hour reaction evaluation was removed from the reactor and calcined at 580°C for 3 hours under air flow to regenerate the catalyst. Using the resulting regenerated catalyst, a reaction evaluation was carried out under the same conditions as in the above reaction evaluation. Three hours after the start of the reaction, the ethylene yield was 30.2% by mass (ethylene conversion rate 69.8% by mass), the propylene yield was 21.3% by mass, and the aromatics yield was 5.2% by mass. The retention rates of each yield are shown in Table 2.

[0182] Examples 8 to 16, Comparative Examples 3 to 5 The physical properties and reaction characteristics of each catalyst were evaluated in the same manner as in Example 7, except that the catalysts listed in Table 2 were used. The results are shown in Table 2. Comparing Comparative Example 3 with the Examples, it was found that when the TPD acid content of the zeolite was high, the ethylene conversion rate 24 hours after the start of the reaction and the propylene yield 24 hours after the start of the reaction could not be maintained, resulting in large fluctuations in the product composition. Comparing Comparative Examples 4 and 5 with the Examples, it was found that when the sodium content of the zeolite-containing catalyst was high or the Na / Al molar ratio was high, the ethylene conversion rate 24 hours after the start of the reaction, the propylene yield 24 hours after the start of the reaction, the ethylene conversion rate after regeneration, and the propylene yield after regeneration could not be maintained, and the amount of coke produced was large.

[0183]

[0184] 1... reactor, 2... first distillation column, 3... cooler, 4... oil-water separator

Claims

1. A method for converting ethanol, comprising a reaction step of supplying a mixed raw material containing ethanol to a reactor having a fixed bed packed with a zeolite-containing catalyst to obtain a reaction gas containing olefins having 3 or more carbon atoms and water, wherein the zeolite contained in the zeolite-containing catalyst has a 10-membered oxygen ring structure, the Na / Al molar ratio of the zeolite-containing catalyst is 0.0050 to 0.25, and the amount of acid per weight of the zeolite-containing catalyst, calculated from the amount of ammonia desorption at 100 to 650°C in ammonia temperature-programmed desorption measurement of the zeolite-containing catalyst, is 75 μmol / g or less.

2. The method for converting ethanol according to claim 1, wherein the acid amount Ac (unit: μmol / g) per weight of the zeolite-containing catalyst satisfies the following formula (1): Ac≦25−60×[Na / Al molar ratio]...(1).

3. The method for converting ethanol according to claim 1, wherein the amount of acid per weight of the zeolite-containing catalyst is 0.5 μmol / g or more.

4. The method for converting ethanol according to claim 1, wherein the amount of acid per weight of zeolite, as determined from the amount of ammonia desorption at 100 to 650°C in ammonia temperature-programmed desorption measurement of the zeolite-containing catalyst, is 75 μmol / g or less.

5. The method for converting ethanol according to claim 1, wherein the zeolite-containing catalyst has a sodium content of 100 ppm by mass or less.

6. The method for converting ethanol according to claim 1, wherein the Si / Al mass ratio in the zeolite-containing catalyst is 300-3000.

7. The process for the conversion of ethanol according to claim 1, wherein the silica / alumina molar ratio of the zeolite in the zeolite-containing catalyst is 600-2000.

8. The method for converting ethanol according to claim 1, wherein the zeolite-containing catalyst contains at least one doping element selected from the group consisting of phosphorus and group 11 elements.

9. The method for converting ethanol according to claim 8, wherein the content of the doping element is not more than 2.0% by mass, based on the total amount of the zeolite-containing catalyst.

10. The process for converting ethanol according to claim 1, wherein the aluminum content is 0.01% by mass to 1% by mass based on the total amount of the zeolite-containing catalyst.

11. The method for converting ethanol according to claim 1, wherein the mixed feedstock contains ethylene.

12. The method for converting ethanol according to claim 1, wherein the ethanol content in the mixed feedstock is 30 mass% or more based on the mixed feedstock.

13. The method for converting ethanol according to claim 1, wherein the molar ratio of ethylene / ethanol in the mixed feedstock is 0.20 to 2.

50.

14. The method for converting ethanol according to claim 1, further comprising a regeneration step of contacting the zeolite-containing catalyst subjected to the reaction step with an oxygen-containing gas heated to 400°C or higher, and subjecting the catalyst to the reaction step again.

15. A method for producing propylene, comprising: a propylene separation step of separating a fraction mainly containing propylene from the reaction gas obtained by the ethanol conversion method according to any one of claims 1 to 14.

16. A method for producing aromatic compounds, comprising: an aromatic compound separation step of separating a fraction mainly containing aromatic compounds from a reaction gas obtained by the ethanol conversion method according to any one of claims 1 to 14.

17. A zeolite-containing catalyst, wherein the zeolite contained in the zeolite-containing catalyst has a 10-membered oxygen ring structure, the Na / Al molar ratio of the zeolite-containing catalyst is 0.0050 to 0.25, and the acid amount per weight of the zeolite-containing catalyst, calculated from the amount of ammonia desorption at 100 to 650°C in ammonia temperature-programmed desorption measurement of the zeolite-containing catalyst, is 75 μmol / g or less.

18. The zeolite-containing catalyst according to claim 17, wherein the mass ratio of Si / Al in the zeolite-containing catalyst is 300 to 3,000.

19. The zeolite-containing catalyst according to claim 17, which is a catalyst for obtaining olefins having 3 or more carbon atoms from a mixed feedstock containing ethanol.

20. The zeolite-containing catalyst of claim 17, wherein the zeolite-containing catalyst contains at least one doping element selected from the group consisting of phosphorus and Group 11 elements.

21. The zeolite-containing catalyst according to claim 20, wherein the content of the doping element is 2.0 mass % or less based on the total amount of the zeolite-containing catalyst.

22. The zeolite-containing catalyst according to claim 17, wherein the aluminum content is 0.01% by mass to 1% by mass based on the total amount of the zeolite-containing catalyst.

23. A method for producing a zeolite-containing catalyst, comprising: a zeolite contained in the zeolite-containing catalyst having a 10-membered oxygen ring structure; a Na / Al molar ratio of the zeolite-containing catalyst being 0.0050 to 0.25; an acid amount per weight of the zeolite-containing catalyst being 75 μmol / g or less, as determined from the amount of ammonia desorption at 100 to 650°C in an ammonia temperature-programmed desorption measurement of the zeolite-containing catalyst; and a steaming step of contacting the zeolite-containing catalyst with water vapor at a steaming temperature of 450°C or higher.

24. A method for producing hydrocarbons, comprising a reaction step of supplying a raw material containing ethanol to a reactor having a fixed bed packed with a zeolite-containing catalyst to obtain a reaction gas containing olefins having 3 or more carbon atoms and water, wherein the zeolite contained in the zeolite-containing catalyst is a zeolite having a 10-membered oxygen ring structure, the Na / Al molar ratio of the zeolite-containing catalyst is 0.0050 to 0.25, and the acid amount per weight of the zeolite-containing catalyst, calculated from the amount of ammonia desorption at 100 to 650°C in ammonia temperature-programmed desorption measurement of the zeolite-containing catalyst, is 75 μmol / g or less.