Hot-dip plated steel sheet

MYPI2025004216A0Undetermined Publication Date: 2024-09-30NIPPON STEEL CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025004216
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2023-10-03
Publication Date
2024-09-30

AI Technical Summary

Technical Problem

Current methods for displaying patterns on hot-dip galvanized steel sheets, such as printing or grinding, increase costs and time, compromise corrosion resistance, and reduce durability, while also altering the metallic appearance.

Method used

A hot-dip plated steel sheet with a controlled composition of Al, Mg, and Zn, featuring a patterned and non-patterned area with specific phase area ratios and inclusion of elements like Si, Ni, and rare earth metals, formed through a hot-dip plating process that maintains corrosion resistance and visual distinction.

Benefits of technology

The solution provides improved durability and corrosion resistance while maintaining the metallic appearance, with clear visual distinction between patterned and non-patterned areas, and prevents deterioration of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025004216_DRAWING_001
    Figure PI2025004216_DRAWING_001
Patent Text Reader

Abstract

ABSTRACT HOT-DIP PLATED STEEL SHEET This hot-dip plated steel sheet includes: a steel sheet; and a hot-dip plating layer formed on a surface of the steel sheet, wherein the hot-dip plating layer contains Al: 0.1 to 70 mass% and Mg: 0.1 to 10.0 mass% in terms of average composition, and a remainder includes Zn and impurities, a pattern part arranged to have a predetermined shape and a non-pattern part are formed on at least one surface side of the steel sheet among the hot-dip plating layers, and an area fraction of an Mg2Zn11 phase on a surface of the non-pattern part is more than 0%, and a ratio (pattern part / non-pattern part) of an area fraction of an Mg2Zn11 phase on a surface of the pattern part to the area fraction of the Mg2Zn11 phase on the surface of the non-pattern part is in a range of 0 or more and less than 0.90 or in a range of 1.10 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Hot-dip galvanized steel sheet

[0001] This application claims priority to Japanese Patent Application No. 2023-054635, filed on March 30, 2023, the contents of which are incorporated herein by reference.

[0002] Zn-Al-Mg hot-dip coated steel sheets, which have higher corrosion resistance than hot-dip galvanized steel sheets, are widely used in various manufacturing industries, such as in the fields of building materials, home appliances, and automobiles, and their usage has been increasing in recent years.

[0003] Incidentally, in order to make characters, patterns, designs, etc. appear on the surface of the hot-dip plated layer of a hot-dip plated steel sheet, the hot-dip plated layer may be subjected to a process such as printing or painting, thereby making characters, patterns, designs, etc. appear on the surface of the hot-dip plated layer.

[0004] However, when processes such as printing and painting are performed on the hot-dip plated layer, there are problems such as increased costs and time required to apply letters, designs, etc. Furthermore, when letters, designs, etc. are displayed on the surface of the plated layer by printing or painting, not only is the metallic luster appearance that is highly popular among consumers lost, but there is also the risk of the letters, designs, etc. disappearing over time due to problems such as deterioration of the coating film itself and deterioration of the adhesion of the coating film over time. Furthermore, when letters, designs, etc. are displayed on the surface of the plated layer by stamping ink, although the cost and time are relatively low, there is a concern that the corrosion resistance of the hot-dip plated layer may be reduced by the ink. Furthermore, when designs, etc. are displayed by grinding the hot-dip plated layer, although the durability of the design, etc. is excellent, the thickness of the hot-dip plated layer at the grinding point is significantly reduced, inevitably reducing corrosion resistance and raising concerns about deterioration of plating properties.

[0005] Therefore, as shown in Patent Document 1 below, a technique has been proposed for producing letters, designs, etc. on the surface of the plating layer of a Zn—Al—Mg hot-dip plated steel sheet without using ink application or grinding.

[0006] Japanese Patent No. 6648871

[0007] The Zn-Al-Mg hot-dip plated steel sheet described in Patent Document 1 is formed by adhering solidification nuclei to an original sheet to be plated and then hot-dip plating, thereby controlling the exposed ratio of the Al phase on the surface of the plated layer or by controlling the surface roughness Ra on the surface of the plated layer, and further improvements to the patterned portion are being studied.

[0008] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a hot-dip plated steel sheet having an improved pattern portion.

[0009] In order to solve the above problems, the present invention employs the following configuration: [1] A steel sheet and a hot-dip galvanized layer formed on a surface of the steel sheet, wherein the hot-dip galvanized layer contains, on an average composition, Al: 0.1 to 70 mass %, Mg: 0.1 to 10.0 mass %, and the balance contains Zn and impurities, and the hot-dip galvanized layer has a patterned portion and a non-patterned portion arranged to have a predetermined shape on at least one side of the steel sheet, and the Mg on the surface of the non-patterned portion is 2 Zn 11 The area ratio of the Mg phase is more than 0%, and the Mg 2 Zn 11 The area ratio of the phase and the Mg on the surface of the non-patterned portion 2 Zn 11 [2] A hot-dip galvanized steel sheet, comprising a steel sheet and a hot-dip galvanized layer formed on a surface of the steel sheet, wherein the hot-dip galvanized layer contains, on an average composition, Al: 0.1 to 70 mass%, Mg: 0.1 to 10.0 mass%, and the balance contains Zn and impurities, and the hot-dip galvanized layer has a pattern portion and a non-pattern portion that are arranged to have a predetermined shape on at least one side of the steel sheet, and the ratio of the area ratio of the Mg phase to the area ratio of the pattern portion (pattern portion / non-pattern portion) is in the range of 0 to less than 0.90, or in the range of 1.10 or more. 2 Zn 11 The area ratio of the phase and the Mg on the surface of the non-patterned portion 2 Zn 11[3] A hot-dip galvanized steel sheet, comprising a steel sheet and a hot-dip galvanized layer formed on a surface of the steel sheet, wherein the hot-dip galvanized layer contains, in average composition, Al: 0.1 to 70 mass %, Mg: 0.1 to 10.0 mass %, and the balance containing Zn and impurities, and the hot-dip galvanized layer has a pattern portion and a non-pattern portion that are arranged to have a predetermined shape on at least one side of the steel sheet, and only one of the pattern portion and the non-pattern portion contains Mg. 2 Zn 11 phase, and the Mg on the surface of the patterned portion or the surface of the non-patterned portion is included. 2 Zn 11 [4] The hot-dip galvanized steel sheet according to any one of [1] to [3], wherein the hot-dip galvanized layer further contains one or two elements selected from the group consisting of Group A and Group B below: [Group A] Si: 0.0001 to 2.0 mass% [Group B] One or more elements selected from Ni, Ti, Zr, Sr, Fe, Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, REM, Hf, and C, in total 0.0001 to 2.0 mass% [5] The hot-dip galvanized steel sheet according to any one of [1] to [3], wherein the patterned portion is arranged to form one or more of a straight line portion, a curved line portion, a dot portion, a figure, a number, a symbol, a design, or a letter, or a combination of two or more of these. [6] The hot-dip galvanized steel sheet according to [4], characterized in that the pattern portion is arranged so as to have one or a combination of two or more of a straight line portion, a curved line portion, a dot portion, a figure, a number, a symbol, a design, or a letter. [7] The area of ​​one continuous pattern portion is 1 mm 2 [8] The hot-dip galvanized steel sheet according to any one of [1] to [3], characterized in that the area of ​​one continuous pattern portion is 1 mm or more. 2[9] The patterned portion is arranged so as to have a shape of one of straight line portions, curved line portions, dot portions, figures, numbers, symbols, designs, and letters, or a combination of two or more of these, and the area of ​​one continuous patterned portion is 1 mm 2

[10] The hot-dip galvanized steel sheet according to any one of [1] to [3], characterized in that the patterned portion is arranged so as to have a shape of one or a combination of two or more of a straight line portion, a curved line portion, a dot portion, a figure, a number, a symbol, a design, or a letter, and the area of ​​one continuous patterned portion is 1 mm or more or 2

[11] The hot-dip galvanized steel sheet according to [4], characterized in that the coating weight of the hot-dip galvanized layer is 30 to 600 g / m on both sides of the steel sheet in total. 2

[12] The hot-dip galvanized steel sheet according to any one of [1] to [3], characterized in that the hot-dip galvanized layer has an average composition containing, by mass%, the Group A.

[13] The hot-dip galvanized steel sheet according to [4], characterized in that the hot-dip galvanized layer has an average composition containing, by mass%, the Group B.

[14] The hot-dip galvanized steel sheet according to [4], characterized in that the Mg 2 Zn 11 The phase is composed of massive [Mg 2 Zn 11 phase] or [Al / Zn / Mg 2 Zn 11

[15] The hot-dip galvanized steel sheet according to any one of [1] to [3], wherein the hot-dip galvanized layer contains either one or both of the above-mentioned ternary eutectic structure of the pattern portion and the above-mentioned non-pattern portion.

[16] The hot-dip galvanized steel sheet according to any one of [1] to [3], wherein the difference between the static friction coefficient of the pattern portion and the static friction coefficient of the non-pattern portion is less than 0.2.

[0010] According to the present invention, a hot-dip galvanized steel sheet having an improved pattern portion can be provided.

[0011] FIG. 2 is a schematic diagram showing a wavy line pattern formed on a hot-dip plated layer in an example.

[0012] The hot-dip galvanized steel sheet according to the present embodiment includes a steel sheet and a hot-dip galvanized layer formed on the surface of the steel sheet, the hot-dip galvanized layer containing, on average, 0.1 to 70 mass% Al, 0.1 to 10.0 mass% Mg, and the balance including Zn and impurities, and the hot-dip galvanized layer has, on at least one surface of the steel sheet, a patterned portion and a non-patterned portion arranged in a predetermined shape, and the Mg on the surface of the non-patterned portion is 2 Zn 11 The area ratio of the Mg phase is more than 0%, and the Mg 2 Zn 11 The area ratio of the phase and the Mg on the surface of the non-patterned portion 2 Zn 11 The ratio of the area ratio of the patterned portion to the non-patterned portion is in the range of 0 or more and less than 0.90, or in the range of 1.10 or more.

[0013] The hot-dip plated steel sheet of this embodiment includes a steel sheet and a hot-dip plated layer formed on the surface of the steel sheet. The hot-dip plated layer contains, on an average composition, Al: 0.1 to 70 mass%, Mg: 0.1 to 10.0 mass%, and the balance contains Zn and impurities. In the hot-dip plated layer, a patterned portion and a non-patterned portion are formed on at least one side of the steel sheet, and the Mg on the surface of the patterned portion is 2 Zn 11 The area ratio of the phase and Mg on the surface of the non-patterned part 2 Zn 11 The difference between the area ratio of the Cr-based and Cr-based phases is 5% or more.

[0014] The hot-dip plated steel sheet of this embodiment includes a steel sheet and a hot-dip plated layer formed on the surface of the steel sheet, the hot-dip plated layer containing, on an average composition, Al: 0.1 to 70 mass %, Mg: 0.1 to 10.0 mass %, with the balance containing Zn and impurities, and the hot-dip plated layer has a patterned portion and a non-patterned portion arranged to have a predetermined shape on at least one side of the steel sheet, and only one of the patterned portion and the non-patterned portion contains Mg. 2 Zn 11 phase, and Mg on the surface of the patterned portion or the surface of the non-patterned portion.2 Zn 11 The area ratio of the phase is 1% or more.

[0015] There are no particular restrictions on the material of the steel sheet that serves as the base for the hot-dip layer. As will be described in detail later, general steel and the like can be used as the material without any particular restrictions, and Al-killed steel and some high-alloy steels can also be applied, and there are no particular restrictions on the shape. The hot-dip layer according to this embodiment is formed by applying a hot-dip galvanizing method, which will be described later, to the steel sheet. The hot-dip layer is formed on the surface of the steel sheet. That is, the hot-dip layer is formed on both one side and the other side of the steel sheet.

[0016] Next, the chemical composition of the hot-dip galvanized layer will be described. The hot-dip galvanized layer contains, on average, 0.1 to 70 mass% Al, 0.1 to 10.0 mass% Mg, with the balance being Zn and impurities. More preferably, the hot-dip galvanized layer contains, on average, 0.1 to 70 mass% Al, 0.1 to 10.0 mass% Mg, with the balance being Zn and impurities.

[0017] Furthermore, the hot-dip plated layer may contain one or two elements selected from the group consisting of the following Group A and Group B: [Group A] Si: 0.0001 to 2 mass% [Group B] One or more of Ni, Ti, Zr, Sr, Fe, Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, REM, Hf, and C, in a total of 0.0001 to 2 mass%

[0018] The content of Al is in the range of 0.1 to 70 mass% in the average composition. Al is preferably contained to ensure corrosion resistance. If the content of Al in the hot-dip coating layer is 0.1 mass% or more, the effect of improving corrosion resistance is further enhanced. If the content of Al exceeds 70 mass%, the effect of improving corrosion resistance may not only saturate but may also decrease. Furthermore, by containing Al in the range of 0.1 to 70 mass%, Mg 2 Zn 11 From the viewpoint of corrosion resistance, the content is preferably 0.5 to 55 mass %, and more preferably 1 to 30 mass %.

[0019] The Mg content is in the range of 0.1 to 10.0 mass% in terms of average composition. Mg is preferably added to improve corrosion resistance. If the Mg content in the hot-dip coating layer is 0.1 mass% or more, the effect of improving corrosion resistance is further enhanced. However, if the Mg content exceeds 10.0 mass%, dross generation in the coating bath becomes significant and corrosion resistance decreases, so the Mg content is set to 10.0 mass% or less. Furthermore, by including Mg in the range of 0.1 to 10.0 mass%, Mg 2 Zn 11 The phase can be formed. 2 Zn 11 From the viewpoint of the balance of the amounts of phases formed, the Mg content is preferably set to 0.5 to 10.0 mass %, more preferably to the range of 1 to 8.0 mass %.

[0020] The hot-dip plated layer may contain 0.0001 to 2.0 mass% Si in its average composition. Si is an element effective for improving the adhesion of the hot-dip plated layer. The effect of improving adhesion is achieved by adding 0.0001 mass% or more of Si to the hot-dip plated layer, so it is preferable to add 0.0001 mass% or more of Si. On the other hand, even if the hot-dip plated layer contains Si at a content exceeding 2.0 mass%, the effect of improving coating adhesion saturates. Therefore, even when Si is added to the hot-dip plated layer, the Si content is set to 2.0 mass% or less. From the viewpoint of coating adhesion, the Si content in the hot-dip plated layer may be 0.0010 to 1.0 mass%, or 0.0100 to 0.8 mass%.

[0021] The hot-dip coating layer may contain, in terms of average composition, one or more of Ni, Ti, Zr, Sr, Fe, Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, REM, Hf, and C in a total amount of 0.0001 to 2.0 mass%. The inclusion of these elements can further improve the corrosion resistance of the hot-dip coating layer. REM is one or more of the rare earth elements having atomic numbers 57 to 71 in the periodic table.

[0022] The remainder of the chemical composition of the hot-dip coating is zinc and impurities. The impurities include those that are inevitably contained in zinc and other base metals, and those that are contained when the steel is dissolved in the coating bath.

[0023] The average composition of the hot-dip plated layer can be measured by the following method. First, the surface coating film is removed with a coating remover that does not corrode the coating (e.g., Neo River SP-751 manufactured by Sansai Kako Co., Ltd.), and then the hot-dip plated layer is dissolved with hydrochloric acid containing an inhibitor (e.g., Hibilon manufactured by Sugimura Chemical Industry Co., Ltd.), and the resulting solution is subjected to inductively coupled plasma (ICP) atomic emission spectrometry. Furthermore, if there is no surface coating film, the step of removing the surface coating film can be omitted.

[0024] Next, the structure of the hot-dip plated layer will be described. The hot-dip plated layer of this embodiment may have a structure as described below, for example, when the hot-dip plated layer contains, in average composition, 4 to 22 mass% Al, 1 to 10.0 mass% Mg, and 0 to 2 mass% Si. This gives the surface of the hot-dip plated layer a mat finish, i.e., an appearance in which fine irregularities are uniformly formed, resulting in an overall aesthetically excellent appearance. Note that the structure of the hot-dip plated layer described below can be obtained as long as it is plated with the above-mentioned chemical composition, and therefore there is no need to limit the structure of the hot-dip plated layer in the present invention.

[0025] The hot-dip coating layer containing Al, Mg and Zn contains [Al phase] and [Al / Zn / MgZn 2 ternary eutectic structure] and Mg 2 Zn 11 phase. Mg 2 Zn 11 The phase is composed of massive [Mg 2 Zn 11 phase], and [Al / Zn / Mg 2 Zn 11 Furthermore, the hot-dip coating layer may contain [MgZn ternary eutectic structure]. 2 In addition, when Si is contained in the hot-dip plating layer, [Mg 2 Si phase] may be contained.

[0026] [Al / Zn / MgZn 2 ternary eutectic structure] [Al / Zn / MgZn 2The ternary eutectic structure is composed of an Al phase, a Zn phase and an intermetallic compound MgZn. 2 The Al phase forming this ternary eutectic structure corresponds to the "Al" phase (an Al solid solution that dissolves Zn and contains a small amount of Mg) at high temperatures in the Al-Zn-Mg ternary equilibrium phase diagram. This Al" phase at high temperatures usually appears separated into a fine Al phase and a fine Zn phase at room temperature. The Zn phase in this ternary eutectic structure is a Zn solid solution that dissolves a small amount of Al and, in some cases, a small amount of Mg. The MgZn in this ternary eutectic structure 2 The phase is an intermetallic compound phase that exists in the vicinity of Zn: approximately 84 mass% in the Zn-Mg binary equilibrium phase diagram. As far as the phase diagram is concerned, it is thought that other added elements are not dissolved in each phase, or even if they are dissolved, the amount is extremely small. However, since the amount cannot be clearly distinguished by normal analysis, the ternary eutectic structure consisting of these three phases is referred to in this specification as [Al / Zn / MgZn 2 ternary eutectic structure].

[0027] [Al Phase] The [Al phase] is a phase that appears as islands with clear boundaries in the matrix of the ternary eutectic structure. This corresponds to, for example, the "Al" phase (an Al solid solution that dissolves Zn and contains a small amount of Mg) at high temperatures in an Al-Zn-Mg ternary equilibrium phase diagram. The amount of Zn and Mg dissolved in this Al" phase at high temperatures varies depending on the Al and Mg concentrations in the plating bath. This Al" phase at high temperatures usually separates into a fine Al phase and a fine Zn phase at room temperature, but the island-like shape seen at room temperature is thought to be due to the shape of the Al" phase at high temperatures. Judging from the phase diagram, it is thought that this phase does not contain any other added elements as solid solution, or if it does, only a very small amount. However, since a clear distinction cannot be made by ordinary analysis, this phase derived from the Al" phase at high temperatures and shaped like the Al" phase is referred to as the [Al phase] in this specification. The [Al phase] can be clearly distinguished from the Al phase that forms the ternary eutectic structure by microscopic observation.

[0028] Mg 2 Zn 11 Phase ([Mg 2 Zn 11 phase], [Al / Zn / Mg2 Zn 11 ternary eutectic structure) Mg 2 Zn 11 The phase is [Mg 2 Zn 11 phase] or [Al / Zn / Mg 2 Zn 11 The hot-dip coating layer contains [Mg 2 Zn 11 phase] and [Al / Zn / Mg 2 Zn 11 The ternary eutectic structure of Mg may be contained. 2 Zn 11 The visibility of the patterned portion is improved by including the Mg phase in either or both of the patterned portion and the non-patterned portion at a predetermined area ratio. 2 Zn 11 The phases are described in more detail below in the description of the patterned and non-patterned portions.

[0029] [Al / Zn / Mg 2 Zn 11 ternary eutectic structure] [Al / Zn / Mg 2 Zn 11 The ternary eutectic structure is composed of an Al phase, a Zn phase, and an intermetallic compound Mg 2 Zn 11 The Al phase forming this ternary eutectic structure corresponds to the "Al" phase (an Al solid solution that dissolves Zn and contains a small amount of Mg) at high temperatures in the Al-Zn-Mg ternary equilibrium phase diagram. This Al" phase at high temperatures usually appears separated into a fine Al phase and a fine Zn phase at room temperature. The Zn phase in this ternary eutectic structure is a Zn solid solution that dissolves a small amount of Al and, in some cases, a small amount of Mg. The Mg in this ternary eutectic structure 2 Zn 11 The phase is an intermetallic compound phase that exists in the vicinity of Zn: approximately 94 mass% in the Zn-Mg binary equilibrium phase diagram. As far as the phase diagram is concerned, it is thought that other added elements are not dissolved in each phase, or even if they are dissolved, the amount is extremely small. However, since the amount cannot be clearly distinguished by normal analysis, the ternary eutectic structure consisting of these three phases is referred to in this specification as [Al / Zn / Mg 2 Zn11 ternary eutectic structure].

[0030] [Mg 2 Zn 11 Phase] [Mg 2 Zn 11 phase] is [Al / Zn / MgZn 2 ternary eutectic structure] or [Al / Zn / Mg 2 Zn 11 It is a phase that appears as islands with clear boundaries in the matrix of the ternary eutectic structure of Mg, and in fact may contain a small amount of solid solution of Al. As far as the phase diagram is concerned, it is thought that this phase does not contain any other added elements in solid solution, or even if it does, it is in a very small amount. 2 Zn 11 phase] and [Al / Zn / Mg 2 Zn 11 Mg forming a ternary eutectic structure 2 Zn 11 The hot-dip plating layer according to this embodiment contains the [Mg 2 Zn 11 Although there are cases where the [phase] is not contained, it is contained in the hot-dip plating layer under most manufacturing conditions.

[0031] [Zn phase] [Zn phase] is [Al / Zn / MgZn 2 ternary eutectic structure] or [Al / Zn / Mg 2 Zn 11 It is a phase that appears as an island with a clear boundary in the matrix of the ternary eutectic structure of [Zn phase] and may actually contain a small amount of solid solution of Al and Mg. As far as the phase diagram is concerned, it is thought that this phase does not contain any other added elements, or even if it does, it is in a very small amount. 2 ternary eutectic structure] or [Al / Zn / Mg 2 Zn 11 The Zn phase can be clearly distinguished from the Zn phase forming the ternary eutectic structure (Zn phase) by microscopic observation. The hot-dip coating layer according to this embodiment may contain the Zn phase depending on the manufacturing conditions, but the influence of the Zn phase on the corrosion resistance was hardly observed. Therefore, there is no particular problem even if the hot-dip coating layer contains the Zn phase.

[0032] [MgZn 2 Phase] [MgZn 2 phase] is [Al / Zn / MgZn 2 ternary eutectic structure] or [Al / Zn / Mg 2 Zn 11 It is a phase that appears as islands with clear boundaries in the matrix of the ternary eutectic structure of MgZn, and in fact may contain a small amount of solid solution of Al. As far as the phase diagram is concerned, it is thought that this phase does not contain any other added elements in solid solution, or even if it does, it is in a very small amount. 2 phase] and [Al / Zn / MgZn 2 MgZn forming a ternary eutectic structure 2 The hot-dip plating layer according to this embodiment contains the [MgZn 2 Although there are cases where the [phase] is not contained, it is contained in the hot-dip plating layer under most manufacturing conditions.

[0033] [Mg 2 Si phase] [Mg 2 The [Mg Si phase] is a phase that appears as islands with clear boundaries in the solidification structure of the Si-added coating layer. 2 It is believed that Zn, Al and other additive elements are not dissolved in the [Mg Si phase], or even if they are dissolved, the amount is extremely small. 2 The Si phase can be clearly distinguished from other phases in the hot-dip coating layer when observed under a microscope.

[0034] The hot-dip coating layer of this embodiment is formed by immersing the steel sheet in a coating bath, then pulling it out, and then solidifying the molten metal that has adhered to the steel sheet surface. 2 Zn 11 Phase, [Al / Zn / MgZn 2 Depending on the chemical composition of the hot-dip coating layer (i.e., the chemical composition of the coating bath), a ternary eutectic structure such as [Al / Zn / MgZn 2 ternary eutectic structure] in the matrix of [Mg 2 Si phase], [MgZn 2 In some cases, the Al / Zn / Mg phase or the Zn phase may be formed. 2 Zn11 In some cases, a ternary eutectic structure (combined ternary eutectic structure) may be formed.

[0035] Next, the patterned portion and non-patterned portion on the surface of the hot-dip plated layer will be described. The hot-dip plated layer of this embodiment has patterned portions and non-patterned portions arranged in a predetermined shape. Either the patterned portion or the non-patterned portion consists of a region with a relatively low metallic luster and a white or gray color. Such regions are low-smooth regions with fine irregularities on the surface, as seen in Zn-Al-Mg hot-dip plated steel sheets, and have a matte appearance. Therefore, the patterned portion and the non-patterned portion can be visually distinguished with the naked eye, a magnifying glass, or a microscope. The patterned portion is preferably arranged to have a shape consisting of one or a combination of two or more of straight lines, curved portions, dots, figures, numbers, symbols, patterns, and letters. The patterned portion may also have a randomly arranged shape. The non-patterned portion is a region other than the patterned portion. The shape of the patterned portion is acceptable even if it is partially missing, such as a missing dot, as long as it is recognizable as a whole. The non-patterned portion may also have a shape that outlines the boundary of the patterned portion.

[0036] The patterned portion and the non-patterned portion may be formed on the surface of either one of the hot-dip galvanized layers formed on one side and the other side of the steel sheet, and in this case, the surface of the hot-dip galvanized layer on the other side may have no patterned portion but a non-patterned portion.

[0037] Furthermore, the patterned portion and the non-patterned portion may be formed on the surface of both the hot-dip plated layers formed on one side and the other side of the steel sheet.

[0038] When the surface of the hot-dip plated layer is provided with one or a combination of two or more of the following shapes: straight line portions, curved line portions, dot portions, figures, numbers, symbols, patterns, or letters, these areas can be defined as patterned areas, and other areas can be defined as non-patterned areas.

[0039] The patterned portion is preferably formed to a size that allows its presence to be discerned with the naked eye, under a magnifying glass, or under a microscope. The non-patterned portion is a region that occupies the majority of the hot-dip plated layer (the surface of the hot-dip plated layer), and the patterned portion may be disposed within the non-patterned portion.

[0040] The patterned portion is arranged in a predetermined shape within the non-patterned portion. Specifically, the patterned portion is arranged within the non-patterned portion to form one or a combination of two or more of straight lines, curved lines, figures, dots, figures, numbers, symbols, patterns, or letters. By intentionally adjusting the shape of the patterned portion, one or a combination of two or more of straight lines, curved lines, figures, dots, figures, numbers, symbols, patterns, or letters appears on the surface of the hot-dip plated layer. For example, the surface of the hot-dip plated layer may appear as a character string, a number string, a symbol, a mark, a line drawing, a design, or a combination thereof, consisting of the patterned portion. This shape is intentionally or artificially formed by the manufacturing method described below and is not naturally formed. Therefore, the area of ​​one continuous patterned portion is larger than that of a naturally formed portion. The area of ​​one continuous patterned portion may be large enough to be distinguishable from the surrounding non-patterned portions. The area of ​​a single continuous pattern portion is 1 mm2 because the larger the area, the more easily it can be distinguished from the surrounding non-patterned portions with the naked eye or under a magnifying glass without using a microscope. 2 More preferably, it is equal to or greater than this.

[0041] As described above, either the patterned portion or the non-patterned portion consists of a region with a relatively low metallic luster on the surface and exhibiting a white or gray color. Such a region is a region with low smoothness having fine irregularities on the surface found in Zn-Al-Mg hot-dip coated steel sheets, and has a matte appearance. Hereinafter, such a region will be referred to as a matte appearance region. Meanwhile, the other of the patterned portion or the non-patterned portion is a region with a relatively high surface smoothness and exhibiting a dark gray or black color compared to the matte appearance region. Hereinafter, such a region will be referred to as a discolored region. Due to this difference in appearance, the patterned portion and the non-patterned portion can be distinguished with the naked eye.

[0042] The patterned portion and the non-patterned portion can be distinguished under a microscope. Specifically, the shape formed by the patterned portion can be distinguished under a microscope even at a magnification of 50 times or less due to differences in the surface condition. In this embodiment, the patterned portion and the non-patterned portion are formed by a manufacturing method described below, and therefore the area of ​​one continuous patterned portion is larger than that of a naturally formed portion. Therefore, the patterned portion and the non-patterned portion can be distinguished under a microscope at a magnification of preferably 20 times or less, more preferably 10 times or less, and even more preferably 5 times or less.

[0043] Next, the difference in the metal structure between the patterned portion and the non-patterned portion will be described in detail. In the following description, as an example, a case will be described in which the non-patterned portion is a matte appearance region and the patterned portion is a discolored region.

[0044] Compared with the matte appearance area constituting the non-pattern area, the discolored area constituting the pattern area is characterized by Mg in the metal structure. 2 Zn 11 The area ratio of the Mg phase is high. 2 Zn 11 The region with a relatively large amount of Mg 2 Zn 11 Phase-poor regions or Mg 2 Zn 11 In order to be able to clearly distinguish the patterned and non-patterned areas with the naked eye, the Mg phase in the metal structure must be clearly distinguished. 2 Zn11 The area ratio of the phase may have at least one of the following configurations (a) to (c). Two or more of the configurations (a) to (c) may be included, or all of the configurations (a) to (c) may be included.

[0045] (a) Mg on the surface of the non-patterned area 2 Zn 11 The area ratio of the Mg phase is more than 0%, and the Mg 2 Zn 11 The area ratio of the phase and Mg on the surface of the non-patterned part 2 Zn 11 The ratio of the area ratio of the phase (patterned portion / non-patterned portion) is in the range of 0 to 0.90, or in the range of 1.10 or more.

[0046] (b) Mg on the surface of the patterned portion 2 Zn 11 The area ratio of the phase and Mg on the surface of the non-patterned part 2 Zn 11 The difference from the area ratio of the phase is 5% or more.

[0047] (c) Mg is added only to either the patterned portion or the non-patterned portion. 2 Zn 11 phase, and Mg on the surface of the patterned portion or the surface of the non-patterned portion. 2 Zn 11 The area ratio of the phase is 1% or more.

[0048] Regarding (a), Mg in the metal structure of the plating layer 2 Zn 11 As the proportion of the Mg phase increases, the appearance of the plating layer becomes dark gray or black. 2 Zn 11 The area ratio of the phase and Mg on the surface of the non-patterned part 2 Zn 11When the ratio of the area ratio of the patterned portion to the non-patterned portion (patterned portion / non-patterned portion) is in the range of 0 to less than 0.90 or 1.10 or more, the difference in color between the patterned portion and the non-patterned portion on the plating layer surface becomes clear, making it possible to distinguish the patterned portion and the non-patterned portion with the naked eye, under a magnifying glass, or under a microscope. However, when the area ratio ratio (patterned portion / non-patterned portion) is 0.90 or more and less than 1.10, the difference in color between the patterned portion and the non-patterned portion becomes unclear, making it difficult to distinguish the patterned portion. Furthermore, there is no need to specify an upper limit for the area ratio ratio (patterned portion / non-patterned portion).

[0049] Regarding (b), Mg in the metal structure of the plating layer 2 Zn 11 As the proportion of the Mg phase increases, the appearance of the plating layer becomes dark gray or black. 2 Zn 11 When the phase is included, or when Mg is present in both the patterned and non-patterned parts, 2 Zn 11 When the Mg phase is included, the Mg 2 Zn 11 The area ratio of the phase and Mg on the surface of the non-patterned part 2 Zn 11 If the difference in area ratio between the Mg phase and the non-patterned portion is 5% or more, the difference in color between the patterned portion and the non-patterned portion on the surface of the plating layer becomes clear, and the patterned portion and the non-patterned portion can be distinguished with the naked eye, under a magnifying glass, or under a microscope. 2 Zn 11 The difference in area ratio between the phases may be 10% or more, or 15% or more. There is no particular need to specify the upper limit of the difference in area ratio, but it may be, for example, 50% or less.

[0050] Regarding (c), Mg in the metal structure of the plating layer 2 Zn 11 As the proportion of the Mg phase increases, the appearance of the plating layer becomes dark gray or black. 2 Zn 11 phase, and Mg on the surface of the patterned portion or the surface of the non-patterned portion. 2 Zn11 If the area ratio of the Mg phase is 1% or more, the difference in color between the patterned portion and the non-patterned portion on the surface of the plating layer becomes clear, and the patterned portion and the non-patterned portion can be distinguished with the naked eye, under a magnifying glass, or under a microscope. 2 Zn 11 The area ratio of the phase may be 5% or more, or 10% or more. There is no particular need to specify the upper limit of the area ratio, but it may be, for example, 50% or less.

[0051] Mg contained in the patterned and non-patterned parts 2 Zn 11 The area ratio of the phase is determined as follows: First, the boundary between the patterned portion and the non-patterned portion is identified by observing the surface of the hot-dip plated layer with the naked eye. If it is difficult to identify the boundary with the naked eye, a magnifying glass or a magnified image using an optical microscope is used.

[0052] Next, the surface of the hot-dip galvanized layer formed on the steel sheet is mirror-polished to a depth of 0.1 μm from the surface to remove the native oxide film on the surface. The removal of the native oxide film is performed on both the patterned portion and the non-patterned portion.

[0053] Next, a backscattered electron image was taken with a scanning electron microscope (SEM) of the surface of the hot-dip plating layer from which the native oxide film had been removed, and Mg 2 Zn 11 Identify the phase: Mg 2 Zn 11 The phases are classified into two types: one that exists in a block form and one that exists in a [Al / Zn / Mg 2 Zn 11 The ternary eutectic structure of Mg is identified. 2 Zn 11 When identifying the phase, elemental analysis using an energy dispersive X-ray elemental analyzer attached to the SEM is also used to confirm the distribution of Zn, Al, and Mg. 2 Zn 11 The total area fraction of the phase is calculated. The observation field is 0.2 mm. 2 The above areas.

[0054] As described above, Mg contained in the patterned portion and the non-patterned portion 2 Zn 11Furthermore, the area ratio ratio (Mg in the non-patterned area) 2 Zn 11 Mg in the pattern area relative to the area ratio of the phase 2 Zn 11 The area ratio of the Mg phase (patterned portion / non-patterned portion) is calculated. 2 Zn 11 The area ratio of the phase and Mg in the non-patterned area 2 Zn 11 The difference between the area ratio of the phase is calculated.

[0055] The static friction coefficients of the plating layer surface of the patterned portion and the plating layer surface of the non-patterned portion are preferably equivalent. Specifically, the difference in the static friction coefficients of the plating layer surfaces of the patterned portion and the non-patterned portion is preferably less than 0.2. More preferably, the difference in the static friction coefficients of the plating layer surfaces of the patterned portion and the non-patterned portion is less than 0.1.

[0056] If the difference in static friction coefficient between the plating layer surface of the patterned portion and the plating layer surface of the non-patterned portion is within the above range, partial deterioration of corrosion resistance can be prevented.

[0057] The static friction coefficient can be measured, for example, using the following method. A hot-dip galvanized steel sheet is cut to prepare a rectangular plate-shaped test piece having a width of 150 mm, a length of 100 mm, and a thickness of 0.6 mm, and a disc-shaped test piece having a diameter of 20 mm and a thickness of 0.6 mm. However, if the length in the plate width direction of the region sprayed with the water jet is, for example, less than 20 mm, a disc-shaped test piece having a diameter of that length is collected. A disc-shaped test piece is placed on top of the rectangular plate-shaped test piece, and the plating layer surfaces of the rectangular plate-shaped test piece and the plating layer surfaces of the disc-shaped test piece are brought into contact with each other. For example, the rectangular plate-shaped test piece and the disc-shaped test piece may be combined such that the plate width direction of the rectangular plate-shaped test piece and the disc-shaped test piece are aligned and the sliding direction is the sheet passing direction. Furthermore, a load (vertical load) is applied from above to below the disc-shaped test piece, and while the disc-shaped test piece is pressed against the rectangular plate-shaped test piece, a horizontal load (horizontal load) is applied to the rectangular plate-shaped test piece, causing the rectangular plate-shaped test piece to slide against the disc-shaped test piece. The value obtained by dividing the horizontal load when the rectangular plate-shaped test piece first starts to move by the vertical load is taken as the static friction coefficient. Note that the test conditions are a vertical load of 3.14 kN, a sliding speed of the rectangular plate-shaped test piece of 150 mm / sec, and a sliding distance of the rectangular plate-shaped test piece of 45 mm. Note that a high-load reciprocating friction and wear tester is used for the above test.

[0058] Next, a method for manufacturing a hot-dip plated steel sheet according to this embodiment will be described. The hot-dip plated steel sheet according to this embodiment is produced by hot-dip plating a steel sheet manufactured through steelmaking, casting, and hot rolling. After the hot rolling, pickling, hot-rolled sheet annealing, cold rolling, and cold-rolled sheet annealing may be further carried out, followed by hot-dip plating. The hot-dip plating is a continuous hot-dip plating method in which the steel sheet is continuously passed through a hot-dip plating bath.

[0059] The hot-dip galvanizing bath preferably contains 0.1 to 70 mass% Al, 0.1 to 10.0 mass% Mg, and the balance Zn and impurities. Alternatively, the hot-dip galvanizing bath may contain 0.1 to 70 mass% Al, 0.1 to 10.0 mass% Mg, and the balance Zn and impurities. Furthermore, the hot-dip galvanizing bath may contain 0.0001 to 2 mass% Si, and may contain a total of 0.0001 to 2 mass% of one or more of Ni, Ti, Zr, Sr, Fe, Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, REM, Hf, and C. The average composition of the hot-dip galvanizing layer in this embodiment is substantially the same as the composition of the hot-dip galvanizing bath.

[0060] The temperature of the hot-dip galvanizing bath varies depending on the composition, but is preferably in the range of 400 to 500°C, for example. This is because a desired hot-dip galvanized layer can be formed if the temperature of the hot-dip galvanizing bath is in this range. The coating weight of the hot-dip galvanized layer can be adjusted by means of gas wiping or the like on the steel sheet pulled out of the hot-dip galvanizing bath. The coating weight of the hot-dip galvanized layer should be 30 to 600 g / m2 in total on both sides of the steel sheet. 2 It is preferable to adjust the amount of adhesion so that it is in the range of 30 g / m 2 If the coating weight is less than 600 g / m, the corrosion resistance of the hot-dip galvanized steel sheet will decrease, which is not preferable. 2 If the coating weight exceeds 15 to 300 g / m, the molten metal adhering to the steel sheet will drip, making it impossible to smooth the surface of the hot-dip plated layer, which is not preferable. 2 The range is.

[0061] After adjusting the deposition amount by gas wiping, the patterned and non-patterned portions are formed. Formation of the patterned and non-patterned portions involves locally spraying a water stream onto the molten metal while cooling the entire steel sheet. The water stream spray position is preferably continuously moved to trace the shape of the patterned portion to be formed. To enable high-speed drawing, it is preferable to fix the position of the water stream nozzle and change the spray position by changing the angle of the water stream nozzle and the pressure of the water stream. The patterned portion is formed along the trajectory of the sprayed water stream. Simply spraying mist-like water is not preferable because it has a lower cooling effect than a water stream. If the amount of water stream is excessive, there may be areas in the sprayed area where the heat recovery described below does not occur sufficiently, and the patterned and non-patterned portions may not be formed. The appropriate amount of water stream varies depending on the thickness of the hot-dip galvanized steel sheet, and is therefore preferably adjusted experimentally. Continuous spraying of water streams tends to result in excessive water streams, so spraying in pulses is recommended. It is also possible to spray cooling gas, but gas spraying has a lower heat removal effect than water spraying, and 2 Zn 11 This is not preferable because it is not sufficient as a means for increasing the proportion of the phase present.

[0062] In order to form the patterned portion into a predetermined shape, the hot-dip plated layer is cooled at an average cooling rate of 10°C / sec or more from the bath temperature to 345°C to form the non-patterned portion. Then, to form the patterned portion, a part of the hot-dip plated layer is sprayed with a water jet while the temperature of the plated layer is in the range of 360°C to 345°C. When the temperature of the plated layer exceeds 360°C, the plated layer is not fully solidified. If the water jet is sprayed when the plated layer is not fully solidified, the surface of the plated layer becomes wavy, and as the plated layer solidifies while maintaining this state, irregularities are formed. It is known that the static friction coefficient is higher in the area where irregularities are formed than in the surrounding area. Additionally, if the water jet is sprayed at a plated layer temperature of more than 360°C, Mg is deposited on the surface of the plated layer. 2 Zn 11 The Mg phase does not crystallize on the surface of the plating layer in the pattern area. 2 Zn 11If the phase does not crystallize, the difference in appearance between the patterned and non-patterned areas will not be sufficiently apparent. For this reason, it is necessary to spray the water jet at a plating layer temperature of 360°C or less. By spraying the water jet at 360°C or less, no irregularities will be formed on the plating layer surface, the thickness of the plating layer will be kept uniform, and partial deterioration of corrosion resistance will not occur. In addition, by spraying the water jet at 345°C or more, Mg 2 Zn 11 The amount of crystallization of the phase can be controlled. Here, the plating layer temperature refers to the surface temperature of the plating layer. The surface temperature of the plating layer can be measured using a radiation thermometer or a contact thermometer.

[0063] By spraying the water flow, the temperature of the hot-dip coating layer is locally reduced. After that, heat flows in from the area where the water flow is not being sprayed, causing reheating and raising the temperature of the coating layer. This series of temperature changes causes Mg 2 Zn 11 The proportion of the phase increases, forming a pattern portion.

[0064] As described above, spraying the water jet at a predetermined temperature can prevent the occurrence of unevenness on the plating layer surface, thereby making the static friction coefficients of the plating layer surfaces of the patterned and non-patterned portions equivalent.

[0065] Furthermore, when a chemical conversion treatment layer is formed on the surface of the hot-dip plated layer, a chemical conversion treatment is performed on the hot-dip plated steel sheet after the hot-dip plated layer has been formed. The type of chemical conversion treatment is not particularly limited, and known chemical conversion treatments can be used. Furthermore, when a coating layer is formed on the surface of the hot-dip plated layer or the surface of the chemical conversion treatment layer, a painting treatment is performed on the hot-dip plated steel sheet after the hot-dip plated layer has been formed or the chemical conversion treatment layer has been formed. The type of painting treatment is not particularly limited, and known painting treatments can be used.

[0066] Next, examples of the present invention will be described. After cold rolling, the steel sheet was degreased and washed with water, and then annealed in an inert atmosphere at a soaking temperature of 800°C for 1 minute. The steel sheet was then immersed in a coating bath and pulled out. While controlling the coating weight of the coating layer and forming a pattern, the entire coating layer was cooled from the bath temperature to 345°C at an average cooling rate of 10°C / second or more. In this manner, hot-dip coated steel sheets Nos. 1 to 18 and 21 to 45 shown in Tables 1 to 6 were produced.

[0067] The pattern portion was formed by spraying a water jet onto a portion of the hot-dip coating layer while the coating layer temperature was in the range of 360°C to 345°C. The water jet was sprayed in a pattern such that a wavy line pattern was formed at intervals of 50 mm. Figure 1 shows the wavy line pattern. The wavy line pattern is a pattern in which multiple wavy lines are arranged at equal intervals, with the intervals between the wavy lines being 50 mm.

[0068] Furthermore, Zn-Al-Mg hot-dip plated steel sheets Nos. 19 and 20 were produced in the same manner as above, except that in forming the pattern portion, a water jet was sprayed onto a part of the hot-dip plated layer at a plated layer temperature of more than 360°C or less than 345°C.

[0069] In addition, Zn—Al—Mg hot-dip plated steel sheets Nos. 46 to 48 were produced in the same manner as above, except that an attempt was made to form a pattern by mist spraying instead of water jet spraying.

[0070] Furthermore, a hot-dip plated steel sheet was produced in the same manner as above, except that no pattern was formed. A wavy line pattern was printed at 50 mm intervals on the surface of the hot-dip plated layer of this steel sheet by an inkjet method. The shape of the pattern is as shown in Figure 1. In this way, No. 49 Zn-Al-Mg hot-dip plated steel sheet was produced.

[0071] Furthermore, a hot-dip galvanized steel sheet was produced in the same manner as above, except that no pattern was formed. The surface of the hot-dip galvanized layer was then ground to form a wavy line pattern spaced at 50 mm intervals. The shape of the pattern is as shown in Figure 1 . In this manner, No. 50 hot-dip galvanized steel sheet was produced.

[0072] The Mg content in the patterned and non-patterned parts of the obtained hot-dip plated steel sheet was 2 Zn 11 The area ratio of the phase was determined. First, the boundary between the patterned portion and the non-patterned portion was identified by observing the surface of the hot-dip plated layer with the naked eye. When it was difficult to identify the boundary with the naked eye, a magnifying glass or a magnified image using an optical microscope was used.

[0073] Next, the surface of the hot-dip galvanized layer formed on the steel sheet was mirror-polished to a depth of 0.1 μm from the surface to remove the native oxide film on the surface. The removal of the native oxide film was performed on both the patterned portion and the non-patterned portion.

[0074] Next, a backscattered electron image was taken with a scanning electron microscope (SEM) of the surface of the hot-dip plating layer from which the native oxide film had been removed, and Mg 2 Zn 11 The phase was identified. 2 Zn 11 The phases are classified into two types: one that exists in a block form and one that exists in a [Al / Zn / Mg 2 Zn 11 The ternary eutectic structure of Mg was identified. 2 Zn 11 When identifying the phase, elemental analysis was performed using an energy dispersive X-ray elemental analyzer attached to the SEM, and the distribution of Zn, Al, and Mg was confirmed and identified. 2 Zn 11 The total area fraction of the phases was calculated. 2 Then, Mg in the observation field 2 Zn 11 The total area fraction of the phases was determined.

[0075] As described above, Mg contained in the patterned portion and the non-patterned portion 2 Zn 11 The area ratio of the Mg phase was calculated. 2 Zn 11 Phase area ratio (Mg in non-patterned area) 2 Zn 11 Mg in the pattern area relative to the area ratio of the phase 2 Zn 11The area ratio of the Mg phase (patterned portion / non-patterned portion) was calculated. 2 Zn 11 The area ratio of the phase and Mg in the non-patterned area 2 Zn 11 The difference between the area ratio of the phase and the area ratio of the phase was calculated.

[0076] [Distinguishing property] The test plates with the patterned portions were visually evaluated based on the following criteria, both in the initial state immediately after production and in the aged state after six months of outdoor exposure. For both the initial state and the aged state, AA to B were considered to be acceptable.

[0077] AA: The pattern portion can be seen from 5 m away. A: The pattern portion cannot be seen from 5 m away, but visibility is high from 3 m away. B: The pattern portion cannot be seen from 3 m away, but visibility is high from 1 m away. C: The pattern portion cannot be seen from 1 m away.

[0078] [Corrosion Resistance] The test plates were cut into 150 x 70 mm pieces and subjected to 30 cycles of accelerated corrosion testing (CCT) in accordance with JASO-M609. The state of rust formation was then examined and evaluated based on the following criteria: AA to B were considered pass.

[0079] AA: No rusting has occurred, and both the patterned and non-patterned parts maintain a beautiful design appearance. A: No rusting has occurred, but a very slight change in the design appearance is observed in the patterned and non-patterned parts. B: Slight rusting has occurred, and the design appearance has been slightly impaired, but the patterned and non-patterned parts can be distinguished visually. C: Rust has occurred, and the appearance quality of the patterned and non-patterned parts has deteriorated significantly, making them indistinguishable visually.

[0080] [Static friction coefficient] A hot-dip plated steel sheet was cut to prepare a rectangular plate-shaped test piece having a width of 150 mm, a length of 100 mm, and a thickness of 0.6 mm, and a disc-shaped test piece having a diameter of 20 mm and a thickness of 0.6 mm. The disc-shaped test piece was placed on top of the rectangular plate-shaped test piece, and the plating layer surfaces of the rectangular plate-shaped test piece and the disc-shaped test piece were brought into contact with each other and slid against each other to measure the static friction coefficient.

[0081] The static friction coefficients of the patterned and non-patterned portions were measured, and the difference in static friction coefficient between the patterned and non-patterned portions was evaluated based on the following criteria: AA: The difference in static friction coefficient between the patterned and non-patterned portions was less than 0.1 A: The difference in static friction coefficient between the patterned and non-patterned portions was 0.1 or more and less than 0.2 B: The difference in static friction coefficient between the patterned and non-patterned portions was 0.2 or more and less than 0.3 C: The difference in static friction coefficient between the patterned and non-patterned portions was 0.3 or more

[0082] As shown in Tables 1 to 6, the Zn-Al-Mg hot-dip coated steel sheets Nos. 1 to 9, 12 to 16 and 21 to 45 had chemical compositions of the hot-dip coated layer within the range of the present invention, and after the steel sheets were pulled out of the coating bath, patterned portions and non-patterned portions were formed in the hot-dip coated layer. 2 Zn 11 The ratio of the area ratio of the phase (pattern portion / non-pattern portion) is 0 or more and less than 0.90 or 1.10 or more, or the Mg 2 Zn 11 Area ratio of the phase and Mg in the non-patterned area 2 Zn 11 The difference between the area ratio of the patterned and non-patterned portions is 5% or more, or Mg is present only in either the patterned or non-patterned portions. 2 Zn 11 phase, and Mg in the patterned or non-patterned portion 2 Zn 11 The area ratio of the phase was 1% or more. Therefore, Nos. 1 to 9, 12 to 16, and 21 to 45 were excellent in both the discriminability and the corrosion resistance.

[0083] The hot-dip galvanized steel sheet No. 10 had reduced corrosion resistance because the hot-dip galvanized layer did not contain Al, and the hot-dip galvanized steel sheet No. 11 had reduced corrosion resistance because the hot-dip galvanized layer contained excessive Al.

[0084] No. 17 hot-dip plated steel sheet did not contain Mg in the hot-dip plated layer. 2 Zn 11No phase was formed, making it difficult to distinguish between patterned and non-patterned areas. The hot-dip plated steel sheet No. 18 had an excessive Mg content in the hot-dip plated layer, resulting in reduced corrosion resistance.

[0085] The hot-dip galvanized steel sheets Nos. 19 and 20 had inferior distinguishability because the conditions for forming the pattern portion were outside the preferred range. The hot-dip galvanized steel sheet No. 19 had a low temperature of the coating layer when the water jet was sprayed, so Mg 2 Zn 11 Furthermore, in the case of the hot-dip galvanized steel sheet No. 20, the temperature of the coating layer when the water jet was sprayed was high, which resulted in the formation of irregularities on the surface of the coating layer and the generation of thin portions of the coating layer, resulting in a decrease in corrosion resistance.

[0086] For hot-dip galvanized steel sheets Nos. 46 to 48, the pattern was formed by mist spraying instead of water jetting. 2 Zn 11 The ratio of the area ratio of the Mg phase (pattern portion / non-pattern portion) is 0.90 or more and less than 1.10, and the Mg 2 Zn 11 Area ratio of the phase and Mg in the non-patterned area 2 Zn 11 The difference in area ratio between the patterned and non-patterned portions is less than 5%, and further, Mg 2 Zn 11 The inclusion of phases resulted in poor discrimination.

[0087] For No. 49, which had a square pattern printed using the inkjet method, the pattern thinned after six months of outdoor exposure, reducing its discernibility. For No. 50, which had a square pattern formed by grinding, the plating layer thickness decreased in the ground areas, reducing the corrosion resistance of the ground areas.

[0088]

[0089]

[0090]

[0091]

[0092]

[0093]

Claims

1. A method for manufacturing a steel plate comprising the steps of: a steel plate; and a hot-dip plating layer formed on a surface of the steel plate, the hot-dip plating layer containing, in average composition, Al: 0.1 to 70 mass%, Mg: 0.1 to 10.0 mass%, and the balance containing Zn and impurities; a pattern portion and a non-pattern portion arranged to have a predetermined shape are formed on at least one side of the steel plate in the hot-dip plating layer; and Mg on the surface of the non-pattern portion is 2 Zinc 11 The area ratio of the Mg phase is more than 0% on the surface of the pattern portion. 2 Zinc 11 The area ratio of the phase and the Mg 2 Zinc 11 A hot-dip galvanized steel sheet having an area ratio of a phase (pattern portion / non-pattern portion) in the range of 0 to less than 0.90, or in the range of 1.10 or more.

2. A method for manufacturing a steel plate having a hot-dip plating layer formed on a surface of the steel plate, the hot-dip plating layer containing, in average composition, Al: 0.1 to 70 mass%, Mg: 0.1 to 10.0 mass%, and the balance containing Zn and impurities, the hot-dip plating layer has a pattern portion and a non-pattern portion arranged to have a predetermined shape on at least one side of the steel plate, and the Mg on the surface of the pattern portion is 2 Zinc 11 The area ratio of the phase and the Mg 2 Zinc 11 The difference between the area ratio of the first and second phases is 5% or more.

3. A steel sheet and a hot-dip plating layer formed on the surface of the steel sheet, the hot-dip plating layer containing, in average composition, Al: 0.1 to 70 mass%, Mg: 0.1 to 10.0 mass%, and the balance containing Zn and impurities, the hot-dip plating layer has a pattern portion and a non-pattern portion arranged to have a predetermined shape on at least one side of the steel sheet, and only one of the pattern portion and the non-pattern portion contains Mg. 2 Zinc 11 phase, and the Mg phase on the surface of the patterned portion or the surface of the non-patterned portion is 2 Zinc 11 A hot-dip galvanized steel sheet having an area ratio of 1% or more of the phase.

4. The hot-dip plated steel sheet according to any one of claims 1 to 3, wherein the hot-dip plated layer further contains one or two selected from the group consisting of the following groups A and B. [Group A] Si: 0.0001 to 2.0 mass% [Group B] One or more of Ni, Ti, Zr, Sr, Fe, Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, REM, Hf, and C, in a total content of 0.0001 to 2.0 mass% 5. The hot-dip galvanized steel sheet according to any one of claims 1 to 3, characterized in that the pattern portion is arranged so as to have a shape that is one or a combination of two or more of the following: straight line portion, curved portion, dot portion, figure, number, symbol, design, or letter.

6. The hot-dip galvanized steel sheet according to claim 4, characterized in that the pattern portion is arranged so as to form one or a combination of two or more of the following: straight line portion, curved portion, dot portion, figure, number, symbol, design or letter.

7. The area of ​​one continuous pattern portion is 1 mm 2 The hot-dip plated steel sheet according to any one of claims 1 to 3, characterized in that 8. The area of ​​one continuous pattern portion is 1 mm 2 The hot-dip galvanized steel sheet according to claim 4, characterized in that 9. The pattern portion is arranged to have a shape that is one of straight lines, curved lines, dots, figures, numbers, symbols, patterns, or letters, or a combination of two or more of these, and the area of ​​one continuous pattern portion is 1 mm 2 The hot-dip plated steel sheet according to any one of claims 1 to 3, characterized in that 10. The pattern portion is arranged so as to have a shape that is one of straight lines, curved lines, dots, figures, numbers, symbols, patterns, or letters, or a combination of two or more of these, and the area of ​​one continuous pattern portion is 1 mm 2 The hot-dip galvanized steel sheet according to claim 4, characterized in that 11. The coating weight of the hot-dip coating layer is 30 to 600 g / m2 on both sides of the steel sheet in total. 2 The hot-dip plated steel sheet according to any one of claims 1 to 3, characterized in that 12. The hot-dip plated steel sheet according to claim 4, wherein the hot-dip plated layer has an average composition containing, in mass %, the Group A elements.

13. The hot-dip plated steel sheet according to claim 4, wherein the hot-dip plated layer has an average composition containing, in mass %, the B group.

14. The above Mg 2 Zinc 11 The phase is composed of massive [Mg 2 Zinc 11 phase] or [Al / Zn / Mg 2 Zinc 11 The hot-dip plated steel sheet according to claim 1 , wherein either one or both of the above two components are contained in the hot-dip plated layer.

15. A hot-dip plated steel sheet according to any one of claims 1 to 3, wherein the difference between the static friction coefficient of the patterned portion and the static friction coefficient of the non-patterned portion is less than 0.2.