Photosensitive resin composition, photosensitive element, cured product, method for forming resist pattern, and method for manufacturing printed wiring board

MYPI2025004238A0Undetermined Publication Date: 2024-09-10RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025004238
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-10
Filing Date
2024-03-01
Publication Date
2024-09-10

AI Technical Summary

Technical Problem

Conventional photosensitive resin compositions used in manufacturing printed wiring boards often result in resist line widths that deviate from the designed value, requiring costly corrections and affecting the precision of the manufacturing process.

Method used

A photosensitive resin composition comprising a binder polymer, a photopolymerizable compound with ethylenically unsaturated bonds, and an oxime ester photopolymerization initiator, which reduces the deviation of resist line widths by optimizing the curing process and adhesion properties.

Benefits of technology

The proposed composition allows for the formation of resist patterns with line widths closer to the designed value, reducing the need for corrections and enhancing the efficiency of the exposure process in both mask exposure and direct writing methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025004238_DRAWING_001
    Figure PI2025004238_DRAWING_001
  • Figure PI2025004238_DRAWING_002
    Figure PI2025004238_DRAWING_002
Patent Text Reader

Abstract

A photosensitive resin composition, containing: a binder polymer (A); a photopolymerizable compound (B) having at least one ethylenically unsaturated bond; and a photopolymerization initiator (C), in which the photopolymerization initiator (C) includes an oxime ester-based photopolymerization initiator, and a content of the oxime ester-based photopolymerization initiator is 0.3 parts by mass or more, with respect to a total of 100 parts by mass of the binder polymer (A) and the photopolymerizable compound (B).
Need to check novelty before this filing date? Find Prior Art

Description

Photosensitive resin composition, photosensitive element, cured product, method for forming resist pattern, and method for manufacturing printed wiring board

[0001] The present disclosure relates to a photosensitive resin composition, a photosensitive element, a cured product, a method for forming a resist pattern, and a method for producing a printed wiring board.

[0002] In the field of printed wiring board manufacturing, photosensitive elements comprising a layer (hereinafter referred to as a "photosensitive resin layer") formed on a support using a photosensitive resin composition are widely used as resist materials for etching, plating, and the like.

[0003] Conventionally, printed wiring boards have been manufactured using the above-mentioned photosensitive element, for example, by the following procedure. That is, first, a photosensitive resin layer of the photosensitive element is laminated onto a circuit-forming substrate (such as a copper-clad laminate). At this time, the photosensitive resin layer is laminated so as to be in close contact with the surface of the circuit-forming substrate on which the conductor pattern (circuit) is formed. The lamination is also performed by heating and pressing the photosensitive resin layer onto the underlying circuit-forming substrate (atmospheric pressure lamination method).

[0004] Next, desired regions of the photosensitive resin layer are exposed to light through a mask film or the like (mask exposure method). At this time, the support (support film or the like) is peeled off either before or after exposure. Thereafter, the unexposed portions of the photosensitive resin layer are dissolved or dispersed and removed in a developer, forming a resist pattern consisting of the cured portions of the photosensitive resin layer. Next, an etching process or a plating process is performed to form a conductor pattern, and then the resist pattern is finally peeled off and removed.

[0005] Recently, as a method for the above-mentioned pattern exposure, a direct imaging method (such as an LDI (Laser Direct Imaging) method) has become popular, which does not require a mask film and directly images circuit data created by CAD using laser light.

[0006] The direct imaging method (such as the LDI method) has many advantages, such as the fact that it does not use a mask film, thereby reducing the cost of the mask film, that it has high accuracy in aligning the opening of the resist, making scaling correction easy, and that it is not necessary to manage the adhesion of foreign matter, dirt, or scratches on the mask.

[0007] As a photosensitive resin composition that can be used in such a direct imaging method, for example, a photosensitive resin composition containing a specific binder polymer and a specific photopolymerization initiator has been proposed (see, for example, Patent Documents 1 and 2 listed below).

[0008] JP 2010-217400 A International Publication No. 2012 / 014580 JP 11-327137 A

[0009] In both the mask exposure method and the direct writing method, it is necessary to form a resist pattern with high precision in order to form fine wiring. However, when a resist pattern is formed using a conventional photosensitive resin composition, there is a problem that the resist line width after exposure and development tends to be wider than the designed value.

[0010] Therefore, an object of the present disclosure is to provide a photosensitive resin composition that can reduce deviation of the resulting resist line width from the designed value when a resist pattern is formed. Another object of the present disclosure is to provide a photosensitive element, a cured product, a method for forming a resist pattern, and a method for producing a printed wiring board using the photosensitive resin composition.

[0011] In order to solve the above problems, the present disclosure provides the following photosensitive resin composition, photosensitive element, cured product, method for forming a resist pattern, and method for producing a printed wiring board.

[0012] [1] A photosensitive resin composition comprising (A) a binder polymer, (B) a photopolymerizable compound having at least one ethylenically unsaturated bond, and (C) a photopolymerization initiator, wherein the (C) photopolymerization initiator comprises an oxime ester photopolymerization initiator, and the content of the oxime ester photopolymerization initiator is 0.3 parts by mass or more per 100 parts by mass of the (A) binder polymer and the (B) photopolymerizable compound combined. [2] The photosensitive resin composition according to [1], wherein the (A) binder polymer has structural units derived from (meth)acrylic acid and structural units derived from benzyl (meth)acrylate or a benzyl (meth)acrylate derivative. [3] The photosensitive resin composition according to [1] or [2], wherein the (C) photopolymerization initiator consists solely of the oxime ester photopolymerization initiator. [4] The photosensitive resin composition according to any one of [1] to [3] above, wherein the oxime ester photopolymerization initiator comprises a compound having a carbazole structure. [5] The photosensitive resin composition according to any one of [1] to [4] above, wherein the oxime ester photopolymerization initiator comprises a compound having a phenyl sulfide structure. [6] The photosensitive resin composition according to any one of [1] to [5] above, wherein the oxime ester photopolymerization initiator comprises a compound having a fluorene structure. [7] The photosensitive resin composition according to any one of [1] to [6] above, wherein the content of the oxime ester photopolymerization initiator is 3.0 parts by mass or less per 100 parts by mass of the total of the (A) binder polymer and the (B) photopolymerizable compound. [8] The photosensitive resin composition according to any one of [1] to [7] above, wherein the photosensitive resin composition is used in a direct imaging system. [9] A photosensitive element comprising a support and a photosensitive resin layer disposed on the support, wherein the photosensitive resin layer comprises the photosensitive resin composition according to any one of [1] to [8] above or a cured product thereof.

[10] A cured product of the photosensitive resin composition according to any one of [1] to [8] above.

[11] The cured product according to

[10] above, which is a resist pattern.

[12] A method for forming a resist pattern, comprising the steps of: forming a photosensitive resin layer on a substrate using the photosensitive resin composition according to any one of [1] to [8] above; irradiating at least a portion of the photosensitive resin layer with actinic rays to cure the photosensitive resin layer; and removing the uncured portion of the photosensitive resin layer from the substrate to form a resist pattern.

[13] A method for forming a resist pattern, comprising the steps of: forming a photosensitive resin layer on a substrate using the photosensitive element according to [9] above; irradiating at least a portion of the photosensitive resin layer with actinic rays to cure the photosensitive resin layer; and removing the uncured portion of the photosensitive resin layer from the substrate to form a resist pattern.

[14] A method for producing a printed wiring board, comprising the steps of forming a resist pattern on the substrate by the method for forming a resist pattern according to

[12] or

[13] above; and plating or etching the substrate and a member having the resist pattern.

[0013] According to the present disclosure, it is possible to provide a photosensitive resin composition that can reduce deviation of the resulting resist line width from the designed value when a resist pattern is formed. The present disclosure also provides a photosensitive element, a cured product, a method for forming a resist pattern, and a method for producing a printed wiring board, which use the photosensitive resin composition.

[0014] 1 is a schematic cross-sectional view showing a photosensitive element according to an embodiment of the present disclosure; 2 is a perspective view showing a schematic example of a manufacturing process for a printed wiring board by a semi-additive process;

[0015]

[0030] Hereinafter, embodiments of the present disclosure will be described in detail. It should be understood that other embodiments are contemplated and may be made without departing from the scope and spirit of the present disclosure. Therefore, the following description of the "Description of the Preferred Embodiments" should not be interpreted in a limiting sense.

[0016] As used herein, the term "process" refers not only to an independent process, but also to processes that are not clearly distinguishable from other processes, as long as the process achieves its intended effect. Numerical ranges indicated using "to" indicate ranges that include the numerical values ​​before and after "to" as the minimum and maximum values, respectively. In numerical ranges described in stages in this specification, the upper or lower limit of a certain numerical range may be replaced with the upper or lower limit of a numerical range of another stage. In numerical ranges described in this specification, the upper or lower limit of that numerical range may be replaced with a value shown in the examples. The term "layer" encompasses not only a structure that is formed over the entire surface when observed in a plan view, but also a structure that is formed only on a portion of the surface. "(Meth)acrylic acid" refers to at least one of "acrylic acid" and its corresponding "methacrylic acid." The same applies to other similar expressions, such as (meth)acrylate.

[0017] When referring to the amount of each component in a composition herein, if the composition contains multiple substances corresponding to each component, the total amount of the multiple substances present in the composition is referred to unless otherwise specified. In this specification, "room temperature" refers to 25°C. In this specification, "solid content" refers to the non-volatile content of a photosensitive resin composition excluding volatile substances (water, solvents, etc.). In other words, it refers to components other than water, organic solvents, and other solvents that remain without volatilizing during the drying process, and includes liquid, starch syrup-like, and wax-like substances at around room temperature (25°C).

[0018] "(Poly)oxyethylene group" means an oxyethylene group or a polyoxyethylene group in which two or more ethylene groups are linked by ether bonds. "(Poly)oxypropylene group" means an oxypropylene group or a polyoxypropylene group in which two or more propylene groups are linked by ether bonds. "EO-modified" means a compound having a (poly)oxyethylene group. "PO-modified" means a compound having a (poly)oxypropylene group. "EO-PO-modified" means a compound having both a (poly)oxyethylene group and a (poly)oxypropylene group.

[0019] <Photosensitive Resin Composition and Cured Product Thereof> The photosensitive resin composition according to this embodiment contains (A) a binder polymer (hereinafter also referred to as component (A)), (B) a photopolymerizable compound having at least one ethylenically unsaturated bond (hereinafter also referred to as component (B)), and (C) a photopolymerization initiator (hereinafter also referred to as component (C)). In the photosensitive resin composition according to this embodiment, the (C) photopolymerization initiator includes an oxime ester-based photopolymerization initiator. In the photosensitive resin composition according to this embodiment, the content of the oxime ester-based photopolymerization initiator is 0.3 parts by mass or more relative to a total of 100 parts by mass of the (A) binder polymer and the (B) photopolymerizable compound.

[0020] The photosensitive resin composition according to this embodiment contains an oxime ester-based photopolymerization initiator as component (C) in an amount of 0.3 parts by mass or more per 100 parts by mass of the total of components (A) and (B). In both mask exposure and direct writing, when a resist pattern is formed, the resulting resist line width can be prevented from becoming wider or narrower than the design value, thereby reducing deviations in the resulting resist line width from the design value. Conventionally, when the resulting resist line width significantly deviates from the design value, it has been necessary to correct the writing data or mask film to account for the resulting resist line width becoming wider or narrower than the design value. However, by using the photosensitive resin composition according to this embodiment, a resist line width close to the design value can be obtained without correction. Therefore, correction of the design value is not necessary in the exposure process, or only a small correction is required, enabling the exposure process to be carried out efficiently.

[0021] The cured product according to this embodiment is a cured product of the photosensitive resin composition according to this embodiment. The cured product according to this embodiment may be a resist pattern.

[0022] (Component (A): Binder Polymer) Examples of the component (A) that can be used in the photosensitive resin composition according to this embodiment include (meth)acrylic resins (resins having structural units derived from (meth)acrylic acid), styrene-based resins, epoxy-based resins, amide-based resins, amide-epoxy-based resins, alkyd-based resins, and phenol-based resins. From the viewpoint of further improving alkaline developability, the photosensitive resin composition according to this embodiment may contain a (meth)acrylic resin, and the component (A) may have a structural unit derived from (meth)acrylic acid. Furthermore, the component (A) may have a structural unit derived from a polymerizable monomer other than (meth)acrylic acid. Examples of such structural units include a structural unit derived from styrene or a styrene derivative, a structural unit derived from an alkyl (meth)acrylate, and a structural unit derived from benzyl (meth)acrylate or a benzyl (meth)acrylate derivative. From the viewpoint of improving resolution and adhesion, the component (A) preferably has at least a structural unit derived from (meth)acrylic acid and a structural unit derived from benzyl (meth)acrylate or a benzyl (meth)acrylate derivative. In addition, from the viewpoint of further improving resolution and adhesion, the (A) component may have a structural unit derived from a hydroxyalkyl (meth)acrylate. Furthermore, the (A) component may be composed of at least one structural unit selected from the group consisting of a structural unit derived from (meth)acrylic acid, a structural unit derived from styrene or a styrene derivative, a structural unit derived from an alkyl (meth)acrylate, a structural unit derived from benzyl (meth)acrylate or a benzyl (meth)acrylate derivative, and a structural unit derived from a hydroxyalkyl (meth)acrylate. The (A) component can be produced, for example, by radical polymerization of a polymerizable monomer.

[0023] Examples of the polymerizable monomer other than (meth)acrylic acid include styrene; polymerizable styrene derivatives substituted at the α-position or at the aromatic ring, such as vinyltoluene and α-methylstyrene; alkyl (meth)acrylate; benzyl (meth)acrylate; benzyl (meth)acrylate derivatives; acrylamides such as diacetone acrylamide; acrylonitrile; esters of vinyl alcohol such as vinyl-n-butyl ether; cycloalkyl (meth)acrylate; furfuryl (meth)acrylate; tetrahydrofurfuryl (meth)acrylate; isobornyl (meth)acrylate; adamantyl (meth)acrylate. acrylate; dicyclopentanyl (meth)acrylate; dimethylaminoethyl (meth)acrylate; diethylaminoethyl (meth)acrylate; glycidyl (meth)acrylate; 2,2,2-trifluoroethyl (meth)acrylate; 2,2,3,3-tetrafluoropropyl (meth)acrylate; β-furyl (meth)acrylic acid; β-styryl (meth)acrylic acid; maleic acid; maleic anhydride; maleic acid monoesters such as monomethyl maleate, monoethyl maleate, and monoisopropyl maleate; fumaric acid; cinnamic acid; α-cyanocinnamic acid; itaconic acid; crotonic acid; and propiolic acid.

[0024] Examples of benzyl (meth)acrylate derivatives include compounds in which the aromatic ring of a benzyl group is substituted with an alkoxy group having 1 to 6 carbon atoms (the number of carbon atoms; the same applies hereinafter), a halogen atom, and / or an alkyl group having 1 to 6 carbon atoms. Examples of benzyl (meth)acrylate derivatives include ethoxybenzyl (meth)acrylate, methoxybenzyl (meth)acrylate, chlorobenzyl (meth)acrylate, methylbenzyl (meth)acrylate, and ethylbenzyl (meth)acrylate.

[0025] From the viewpoint of further improving resolution and adhesion, the component (A) may contain at least one structural unit derived from styrene or a styrene derivative. In this case, the resolution is further improved, thereby enabling the production of an even better resist shape. The component (A) may contain a structural unit derived from styrene and a structural unit derived from a styrene derivative.

[0026] Examples of hydroxyalkyl (meth)acrylates include hydroxymethyl (meth)acrylate, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, hydroxypentyl (meth)acrylate, hydroxyhexyl (meth)acrylate, etc. In addition, when the number of carbon atoms in the alkyl moiety in the hydroxyalkyl (meth)acrylate unit is 3 or more, the hydroxyalkyl (meth)acrylate unit may have a branched structure.

[0027] From the viewpoint of improving alkaline developability and release properties, component (A) may have at least one structural unit derived from alkyl (meth)acrylate. Examples of the alkyl group of the alkyl (meth)acrylate include methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, and dodecyl. Each structural isomer can be used as the alkyl group. Examples of the alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, and dodecyl (meth)acrylate. From the viewpoint of further improving release properties, the alkyl group may have 1 to 4 carbon atoms. The alkyl (meth)acrylates can be used alone or in any combination of two or more.

[0028] The content of each structural unit constituting the component (A) is not particularly limited. The content of the structural unit derived from (meth)acrylic acid may be such that the acid value of the component (A) falls within the following range. From the viewpoint of preventing the development time from becoming long, the acid value of the component (A) may be 100 mgKOH / g or more, 120 mgKOH / g or more, 140 mgKOH / g or more, 150 mgKOH / g or more, or 160 mgKOH / g or more. From the viewpoint of further improving the developer resistance (e.g., adhesion) of the cured product of the photosensitive resin composition, the acid value of the component (A) may be 250 mgKOH / g or less, 240 mgKOH / g or less, or 230 mgKOH / g or less. From these viewpoints, the acid value of the component (A) may be 100 to 250 mgKOH / g, 120 to 240 mgKOH / g, 140 to 230 mgKOH / g, 150 to 230 mgKOH / g, or 160 to 230 mgKOH / g. When solvent development is performed, the amount of a polymerizable monomer having a carboxy group (monomer, such as (meth)acrylic acid) may be adjusted to a small amount from the viewpoint of excellent developability.

[0029] When the component (A) has a structural unit derived from benzyl (meth)acrylate or a benzyl (meth)acrylate derivative, the content of the structural unit may be in the following ranges based on the total amount (total mass) of solids in the component (A). From the viewpoint of improving the chemical resistance of the resin, the content may be 1% by mass or more, 15% by mass or more, or 20% by mass or more. From the viewpoint of suppressing an increase in the peel time, the content may be 80% by mass or less, 50% by mass or less, or 40% by mass or less. From these viewpoints, the content may be 1 to 80% by mass, 15 to 50% by mass, or 20 to 40% by mass.

[0030] When component (A) has a structural unit derived from styrene or a styrene derivative, the content of the structural unit may be in the following ranges based on the total solids content (total mass) of component (A). From the viewpoint of further improving resolution, the content may be 5% by mass or more, 10% by mass or more, 20% by mass or more, 25% by mass or more, 30% by mass or more, 35% by mass or more, 40% by mass or more, or 45% by mass or more. From the viewpoint of suppressing the size of peeled pieces and suppressing an increase in peel time, the content may be 65% by mass or less, 55% by mass or less, or 50% by mass or less. From these viewpoints, the content may be 5 to 65% by mass, 10 to 55% by mass, 20 to 50% by mass, 25 to 50% by mass, 30 to 50% by mass, 35 to 50% by mass, 40 to 50% by mass, or 45 to 50% by mass.

[0031] The component (A) may have a structural unit derived from benzyl (meth)acrylate or a benzyl (meth)acrylate derivative, and a structural unit derived from styrene or a styrene derivative, in which case a resist with even better adhesion can be obtained.

[0032] When the component (A) has a structural unit derived from an alkyl (meth)acrylate, the content of the structural unit may be in the following ranges based on the total amount (total mass) of solids in the component (A). From the viewpoints of preventing peeled pieces from becoming large and preventing the peeling time from becoming long, the content may be 1% by mass or more, 2% by mass or more, or 3% by mass or more. From the viewpoints of further improving resolution and adhesion, the content may be 80% by mass or less, 60% by mass or less, or 50% by mass or less. From these viewpoints, the content may be 1 to 80% by mass, 2 to 60% by mass, or 3 to 50% by mass.

[0033] The weight average molecular weight (Mw) of component (A) may be 10,000 or more, 20,000 or more, or 25,000 or more, from the viewpoint that the developer resistance (e.g., adhesion) of the cured product of the photosensitive resin composition tends to be even better. The weight average molecular weight (Mw) of component (A) may be 100,000 or less, 80,000 or less, or 60,000 or less, from the viewpoint that the development time tends to be excellent. From these viewpoints, the weight average molecular weight (Mw) of component (A) may be 10,000 to 100,000, 20,000 to 80,000, or 25,000 to 60,000. The weight average molecular weight of component (A) is measured by gel permeation chromatography (GPC) (converted using a calibration curve using standard polystyrene). For low molecular weight compounds, if it is difficult to measure the weight average molecular weight using the above-mentioned method, the molecular weight can be measured by another method and the average can be calculated.

[0034] The dispersity (Mw / Mn) of component (A) is not particularly limited, but may be from 1.0 to 3.0, or from 1.5 to 2.5. When the dispersity is 3.0 or less, adhesion and resolution are further improved.

[0035] Component (A) may optionally have in its molecule a characteristic group (such as a nitro group) that is photosensitive to light having a wavelength in the range of 350 to 440 nm.

[0036] In the photosensitive resin composition according to this embodiment, as component (A), one type of binder polymer may be used alone, or two or more types of binder polymers may be used in any combination. When two or more types of binder polymers are used in combination, examples of component (A) include two or more types of binder polymers composed of different copolymerization components (binder polymers containing different monomer units as copolymerization components), two or more types of binder polymers with different weight-average molecular weights, and two or more types of binder polymers with different dispersities. As component (A), a polymer having a multimodal molecular weight distribution as described in JP-A-11-327137 (Patent Document 3) can also be used.

[0037] The content of the component (A) may be in the following ranges based on the total amount (total mass) of solids in the photosensitive resin composition. From the viewpoint of tending to provide excellent film formability, the content of the component (A) may be 20% by mass or more, 30% by mass or more, 40% by mass or more, or 50% by mass or more. From the viewpoint of tending to provide even better sensitivity and resolution, the content of the component (A) may be 90% by mass or less, 80% by mass or less, 65% by mass or less, or 60% by mass or less. From these viewpoints, the content of the component (A) may be 20 to 90% by mass, 30 to 80% by mass, 40 to 65% by mass, or 50 to 60% by mass.

[0038] The content of the component (A) may be within the following ranges, relative to 100 parts by mass of the total of the components (A) and (B). From the viewpoint of further improving film formability, the content of the component (A) may be 30 parts by mass or more, 35 parts by mass or more, 40 parts by mass or more, or 50 parts by mass or more. From the viewpoint of further improving sensitivity and resolution, the content of the component (A) may be 70 parts by mass or less, 65 parts by mass or less, or 60 parts by mass or less. From these viewpoints, the content of the component (A) may be 30 to 70 parts by mass, 35 to 65 parts by mass, 40 to 60 parts by mass, or 50 to 60 parts by mass.

[0039] (Component (B): Photopolymerizable Compound) The component (B) is a compound having at least one ethylenically unsaturated bond. The component (B) may be used alone or in any combination of two or more. From the viewpoint of further improving the alkali developability, resolution, and release properties after curing, the component (B) may contain at least one bisphenol A type (meth)acrylate compound.

[0040] Examples of bisphenol A type (meth)acrylate compounds include 2,2-bis(4-((meth)acryloxypolyethoxy)phenyl)propane, 2,2-bis(4-((meth)acryloxypolypropoxy)phenyl)propane, 2,2-bis(4-((meth)acryloxypolybutoxy)phenyl)propane, and 2,2-bis(4-((meth)acryloxypolyethoxypolypropoxy)phenyl)propane. Of these, component (B) may contain 2,2-bis(4-((meth)acryloxypolyethoxy)phenyl)propane from the viewpoint of further improving resolution and release properties. The bisphenol A type (meth)acrylate compounds may be used alone or in any combination of two or more.

[0041] Of these, 2,2-bis(4-(methacryloxydiethoxy)phenyl)propane is commercially available as BPE-200 (trade name, manufactured by Shin-Nakamura Chemical Co., Ltd.). 2,2-bis(4-(methacryloxypentaethoxy)phenyl)propane is commercially available as BPE-500 (trade name, manufactured by Shin-Nakamura Chemical Co., Ltd.) or FA-321M (trade name, manufactured by Resonac Corporation).

[0042] In the photosensitive resin composition according to this embodiment, the content of the bisphenol A (meth)acrylate compound may be in the following ranges based on the total solid content (total mass) of the component (B), from the viewpoint of further improving the resolution of the resist pattern. The content may be 20% by mass or more, 40% by mass or more, 60% by mass or more, or 70% by mass or more. The content may be 100% by mass or less, or 95% by mass or less. From these viewpoints, the content may be 20 to 100% by mass, 40 to 100% by mass, 60 to 100% by mass, or 70 to 100% by mass, or may be 20 to 95% by mass, 40 to 95% by mass, 60 to 95% by mass, or 70 to 95% by mass.

[0043] From the viewpoint of improving resolution and flexibility in a balanced manner, component (B) may contain a compound obtained by reacting a polyhydric alcohol with an α,β-unsaturated carboxylic acid. Examples of compounds obtained by reacting a polyhydric alcohol with an α,β-unsaturated carboxylic acid include polyethylene glycol di(meth)acrylate having 2 to 14 ethylene groups, polypropylene glycol di(meth)acrylate having 2 to 14 propylene groups, alkylene glycol di(meth)acrylate having both a (poly)oxyethylene group and a (poly)oxypropylene group, trimethylolpropane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, EO-modified trimethylolpropane tri(meth)acrylate, PO-modified trimethylolpropane tri(meth)acrylate, EO-PO-modified trimethylolpropane tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, and tetramethylolmethane tetra(meth)acrylate. These compounds may be used alone, but from the viewpoint of further improving the resolution, two or more compounds selected from the group of compounds obtained by reacting the above-mentioned polyhydric alcohol with an α,β-unsaturated carboxylic acid may be used in combination, which further improves the resolution.

[0044] The content (total amount) of the compound obtained by reacting a polyhydric alcohol with an α,β-unsaturated carboxylic acid may be in the following ranges based on the total amount (total mass) of solids in component (B). From the viewpoint of improving flexibility, the content may be 5% by mass or more. From the viewpoint of further improving resolution, the content may be 20% by mass or less or 15% by mass or less. From these viewpoints, the content may be 5 to 20% by mass or 5 to 15% by mass.

[0045] The photosensitive resin composition in this embodiment may further contain, as component (B), a polymerizable compound other than the bisphenol A (meth)acrylate compound and the compound obtained by reacting a polyhydric alcohol with an α,β-unsaturated carboxylic acid.

[0046] Other polymerizable compounds include nonylphenoxy polyethyleneoxy (meth)acrylate, phthalic acid compounds, alkyl (meth)acrylate, photopolymerizable compounds having at least one cationically polymerizable cyclic ether group in the molecule (oxetane compounds, etc.), etc. Among these, from the viewpoint of achieving a balanced improvement in resolution, adhesion, resist shape, and release properties after curing, at least one selected from the group consisting of nonylphenoxy polyethyleneoxy (meth)acrylate and phthalic acid compounds is preferred.

[0047] Examples of the nonylphenoxy polyethyleneoxy (meth)acrylate include nonylphenoxy triethyleneoxy (meth)acrylate, nonylphenoxy tetraethyleneoxy (meth)acrylate, nonylphenoxy pentaethyleneoxy (meth)acrylate, nonylphenoxy hexaethyleneoxy (meth)acrylate, nonylphenoxy heptaethyleneoxy (meth)acrylate, nonylphenoxy octaethyleneoxy (meth)acrylate, nonylphenoxy nonaethyleneoxy (meth)acrylate, nonylphenoxy decaethyleneoxy (meth)acrylate, and nonylphenoxy undecaethyleneoxy (meth)acrylate. The nonylphenoxy polyethyleneoxy (meth)acrylate can be used alone or in any combination of two or more.

[0048] Examples of phthalic acid compounds include γ-chloro-β-hydroxypropyl-β'-(meth)acryloyloxyethyl-o-phthalate, β-hydroxyethyl-β'-(meth)acryloyloxyethyl-o-phthalate, and β-hydroxypropyl-β'-(meth)acryloyloxyethyl-o-phthalate. Of these, γ-chloro-β-hydroxypropyl-β'-(meth)acryloyloxyethyl-o-phthalate is preferred as the phthalic acid compound. γ-Chloro-β-hydroxypropyl-β'-methacryloyloxyethyl-o-phthalate is commercially available as FA-MECH (trade name, manufactured by Resonac Corporation). The phthalic acid compounds can be used alone or in any combination of two or more.

[0049] When the photosensitive resin composition according to this embodiment contains the other photopolymerizable compound as the component (B), the content of the photopolymerizable compound may be 1 to 30 mass %, 3 to 25 mass %, or 5 to 20 mass % based on the total amount (total mass) of solids in the component (B), from the viewpoint of improving the resolution, adhesion, resist shape, and release properties after curing in a balanced manner.

[0050] The content of the (B) component may be in the following ranges based on the total amount (total mass) of solids in the photosensitive resin composition. From the viewpoint of tending to achieve even better sensitivity and resolution, the content of the (B) component may be 3 mass% or more, 10 mass% or more, 25 mass% or more, 30 mass% or more, or 40 mass% or more. From the viewpoint of tending to achieve excellent film formability, the content of the (B) component may be 70 mass% or less, 60 mass% or less, or 50 mass% or less. From these viewpoints, the content of the (B) component may be 3 to 70 mass%, 10 to 60 mass%, 25 to 50 mass%, 30 to 50 mass%, or 40 to 50 mass%.

[0051] The content of the (B) component may be in the following ranges relative to 100 parts by mass of the total amount of the (A) component and the (B) component. From the viewpoint of further improving sensitivity and resolution, the content of the (B) component may be 5 parts by mass or more, 10 parts by mass or more, 15 parts by mass or more, 20 parts by mass or more, 30 parts by mass or more, or 40 parts by mass or more. From the viewpoint of further improving film formability, the content of the (B) component may be 70 parts by mass or less, 65 parts by mass or less, 60 parts by mass or less, 50 parts by mass or less, or 45 parts by mass or less. From these viewpoints, the content of the (B) component may be 5 to 70 parts by mass, 10 to 70 parts by mass, 15 to 65 parts by mass, 20 to 60 parts by mass, 30 to 50 parts by mass, or 40 to 45 parts by mass.

[0052] (Component (C): Photopolymerization Initiator) The photosensitive resin composition according to this embodiment contains an oxime ester-based photopolymerization initiator as component (C). This makes it possible to reduce deviations of the resulting resist line width from the designed value when forming a resist pattern, whether using a mask exposure method or a direct writing method.

[0053] The oxime ester photopolymerization initiator is not particularly limited as long as it is a photopolymerization initiator having an oxime ester group, but is preferably a compound having at least one of a carbazole structure, a phenyl sulfide structure, and a fluorene structure. This makes it possible to further reduce deviations from the design value of the resist line width obtained when a resist pattern is formed, in both the mask exposure method and the direct writing method. The oxime ester photopolymerization initiator can be used alone or in any combination of two or more types.

[0054] Examples of the oxime ester photopolymerization initiator having a carbazole structure include 1-propanone, 3-cyclopentyl-1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(o-acetyloxime) (trade name "TR-PBG-304", manufactured by Changzhou New Power Electronic Materials Co., Ltd.), 1-propanone, 3-cyclopentyl-1-[2-(2-pyrimidinylthio)-9H-carbazol-3-yl]-, 1-(o-acetyloxime) (trade name "TR-PBG-314", manufactured by Changzhou New Power Electronic Materials Co., Ltd.), and 2-(acetoxyimino)-1-(6-(2-(acetoxyimino)-3-cyclohexylpropionyl)-9-ethylcarbazol-3-yl)n-octan-1-one. Commercially available products include TR-PBG-304, TR-PBG-314, and TR-PBG-345 (all manufactured by Changzhou Strong Electronic New Materials Co., Ltd.).

[0055] Examples of oxime ester photopolymerization initiators having a phenyl sulfide structure include 1-[4-(phenylthio)phenyl]-3-cyclopentylpropane-1,2-dione-2-(o-benzoyloxime) (trade name "TR-PBG-305", manufactured by Changzhou Strong Electronic New Materials Co., Ltd.). Commercially available products include TR-PBG-305 and TR-PBG-3057 (both manufactured by Changzhou Strong Electronic New Materials Co., Ltd.).

[0056] Examples of oxime ester photopolymerization initiators having a fluorene structure include (Z)-[3-cyclohexyl-1-(9,9-dibutyl-7-nitrofluoren-2-yl)propylidene]amino)acetate, etc. Commercially available products include TR-PBG-358 (manufactured by Changzhou Strong Electronic New Materials Co., Ltd.).

[0057] The oxime ester photopolymerization initiator may be a compound that does not have any of a carbazole structure, a phenyl sulfide structure, and a fluorene structure. Examples of such oxime ester photopolymerization initiators include 1-phenyl-1,2-propanedione-2-o-benzoyloxime.

[0058] The content of the oxime ester photopolymerization initiator is 0.3 parts by mass or more relative to 100 parts by mass of the total of the components (A) and (B). This reduces deviation of the resulting resist line width from the design value when forming a resist pattern, whether using a mask exposure method or a direct writing method. From the viewpoint of further enhancing the above effect, the content of the oxime ester photopolymerization initiator may be 0.35 parts by mass or more, or 0.4 parts by mass or more, relative to 100 parts by mass of the total of the components (A) and (B). Furthermore, from the viewpoint of obtaining appropriate sensitivity, the content of the oxime ester photopolymerization initiator may be 3.0 parts by mass or less, 2.5 parts by mass or less, or 2.0 parts by mass or less, relative to 100 parts by mass of the total of the components (A) and (B). From these viewpoints, the content of the oxime ester photopolymerization initiator may be 0.3 to 3.0 parts by mass, 0.35 to 2.5 parts by mass, or 0.4 to 2.0 parts by mass, relative to 100 parts by mass of the total of the components (A) and (B).

[0059] From the viewpoint of obtaining appropriate sensitivity, the content of the oxime ester photopolymerization initiator may be in the following ranges based on the total mass of the component (C). The content of the oxime ester photopolymerization initiator may be 50% by mass or more, 60% by mass or more, 65% by mass or more, 70% by mass or more, or 75% by mass or more. The content of the oxime ester photopolymerization initiator may be 100% by mass. That is, the photopolymerization initiator (C) may consist solely of the oxime ester photopolymerization initiator. From these viewpoints, the content may be 50 to 100% by mass, 60 to 100% by mass, 65 to 100% by mass, 70 to 100% by mass, or 75 to 100% by mass.

[0060] The photosensitive resin composition according to this embodiment may further contain a photopolymerization initiator other than the oxime ester-based photopolymerization initiator. Examples of other photopolymerization initiators include hexaarylbiimidazole derivatives. From the viewpoint of further improving sensitivity and adhesion, the photopolymerization initiator is preferably at least one type of 2,4,5-triarylimidazole dimer. The structure of the 2,4,5-triarylimidazole dimer may be symmetric or asymmetric.

[0061] Examples of the 2,4,5-triarylimidazole dimer include 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer (also known as 2,2'-bis(o-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole), 2-(o-chlorophenyl)-4,5-bis-(m-methoxyphenyl)imidazole dimer, and 2-(p-methoxyphenyl)-4,5-diphenylimidazole dimer. Of these, 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer is preferred.

[0062] Other photopolymerization initiators include aromatic ketones such as benzophenone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1,2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, 4-(2-hydroxyethoxy)phenyl-2-(hydroxy-2-propyl)ketone, and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propanone-1; quinones such as thiaquinone; benzoin ether compounds such as benzoin alkyl ether; benzoin compounds such as benzoin and alkylbenzoin; benzyl derivatives such as benzyl dimethyl ketal; bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide; bis(2,6-dimethylbenzoyl)-2,4,4-trimethyl-pentylphosphine oxide; (2,4,6-trimethylbenzoyl)ethoxyphenylphosphine oxide, and the like.

[0063] When the photosensitive resin composition according to this embodiment contains the other photopolymerization initiator, the content of the photopolymerization initiator may be 0.01 to 10 parts by mass, 0.01 to 8 parts by mass, or 0.01 to 5 parts by mass, relative to 100 parts by mass of the total of the component (A) and the component (B).

[0064] From the viewpoint of further improving sensitivity and adhesion, the content of the component (C) may be in the following ranges based on the total amount (total mass) of solids in the photosensitive resin composition. The content of the component (C) may be 0.1 mass% or more, 0.2 mass% or more, 0.3 mass% or more, or 0.35 mass% or more. The content of the component (C) may be 20 mass% or less, 10 mass% or less, 3 mass% or less, 1 mass% or less, 0.5 mass% or less, or 0.4 mass% or less. From these viewpoints, the content of the component (C) may be 0.1 to 20 mass%, 0.1 to 10 mass%, or 0.1 to 3 mass%.

[0065] (Component (D): Hydrogen Donor) The photosensitive resin composition according to this embodiment may further contain a hydrogen donor capable of donating hydrogen during the reaction of the exposed area. This further improves the sensitivity of the photosensitive resin composition.

[0066] Examples of the component (D) include bis[4-(dimethylamino)phenyl]methane, bis[4-(diethylamino)phenyl]methane, leucocrystal violet, and N-phenylglycine. The component (D) can be used alone or in any combination of two or more.

[0067] When the photosensitive resin composition according to this embodiment contains the component (D), the content of the component (D) may be in the following ranges relative to 100 parts by mass of the total of the components (A) and (B). From the viewpoint of further improving sensitivity, the content of the component (D) may be 0.01 parts by mass or more, 0.05 parts by mass or more, 0.1 parts by mass or more, 0.3 parts by mass or more, 0.5 parts by mass or more, or 0.6 parts by mass or more. From the viewpoint of suppressing the precipitation of excess component (D) as foreign matter after film formation, the content of the component (D) may be 10 parts by mass or less, 5 parts by mass or less, 2 parts by mass or less, or 1 part by mass or less. From these viewpoints, the content of the component (D) may be 0.01 to 10 parts by mass, 0.05 to 5 parts by mass, or 0.1 to 2 parts by mass.

[0068] (Sensitizing dye) The photosensitive resin composition according to this embodiment may further contain a sensitizing dye. This further improves the sensitivity of the photosensitive resin composition. Examples of sensitizing dyes include dialkylaminobenzophenones, pyrazolines, anthracenes, coumarins, xanthones, oxazoles, benzoxazoles, thiazoles, benzothiazoles, triazoles, stilbenes, triazines, thiophenes, naphthalimides, and triarylamines. The sensitizing dyes may be used alone or in any combination of two or more.

[0069] In particular, when the photosensitive resin layer is exposed to actinic rays having a wavelength of 390 to 420 nm, the sensitizing dye may contain at least one selected from the group consisting of pyrazolines, anthracenes, coumarins, and triarylamines, from the viewpoint of achieving even better sensitivity and adhesion, and may particularly contain at least one selected from the group consisting of pyrazolines, anthracenes, and triarylamines.

[0070] When the photosensitive resin composition according to this embodiment contains a sensitizing dye, the content of the sensitizing dye may be 0.01 to 10 parts by mass, 0.05 to 5 parts by mass, or 0.1 to 3 parts by mass, relative to 100 parts by mass of the total amount of the components (A) and (B). When the content of the sensitizing dye is 0.01 parts by mass or more, sensitivity and resolution are further improved. When the content of the sensitizing dye is 10 parts by mass or less, the resist shape is further prevented from becoming an inverted trapezoid, and adhesion is further improved.

[0071] (Other Components) In addition to the above components, the photosensitive resin composition according to this embodiment may contain other components as needed. Examples of other components include dyes (e.g., malachite green), tribromophenyl sulfone, photocoloring agents, thermal color-developing inhibitors, plasticizers (e.g., p-toluenesulfonamide), pigments, fillers, antifoaming agents, flame retardants, stabilizers, adhesion promoters, leveling agents, release promoters, antioxidants, fragrances, imaging agents, and thermal crosslinking agents. These may be used alone or in any combination of two or more.

[0072] The content of each of these components is preferably about 0.01 to 20 parts by mass per 100 parts by mass of the total amount of components (A) and (B).

[0073] The content of coloring matter such as dyes and pigments may be less than 0.5% by mass and may be 0.45% by mass or less based on the solid content (total mass) of the photosensitive resin composition.

[0074] The photosensitive resin composition according to this embodiment may contain at least one organic solvent to adjust the viscosity, if necessary. As the organic solvent, any commonly used organic solvent may be used without any particular limitation. Examples of the organic solvent include methanol, ethanol, acetone, methyl ethyl ketone, methyl cellosolve, ethyl cellosolve, toluene, N,N-dimethylformamide, propylene glycol monomethyl ether, and mixed solvents thereof.

[0075] The photosensitive resin composition according to this embodiment can be used, for example, by dissolving at least the components (A), (B), and (C) in the organic solvent to form a solution having a solid content of about 30 to 60 mass % (hereinafter referred to as a "coating liquid").

[0076] The coating liquid can be used to form a photosensitive resin layer, for example, as follows. The coating liquid is applied to the surface of a support (such as a support film or a metal plate) described below, and then dried, thereby forming a photosensitive resin layer derived from the photosensitive resin composition on the support. Examples of metal plates include copper, copper-based alloys, nickel, chromium, iron, and iron-based alloys (such as stainless steel), and preferably copper, copper-based alloys, and iron-based alloys.

[0077] The thickness of the photosensitive resin layer varies depending on the application, but may be about 1 to 100 μm after drying.

[0078] The photosensitive resin composition according to this embodiment can be suitably used, for example, in the method for forming a resist pattern described below. In particular, it is suitable for application to a method for forming a conductor pattern (circuit) by plating treatment.

[0079] <Photosensitive Element> The photosensitive element according to this embodiment includes a support and a photosensitive resin layer disposed on the support. The photosensitive resin layer includes the photosensitive resin composition according to this embodiment or a cured product thereof. The photosensitive resin layer is formed using the photosensitive resin composition according to this embodiment, and the photosensitive resin composition may be in an uncured state (coating film). The photosensitive element may include other layers, such as a protective layer, as needed. For example, the surface (surface) of the photosensitive resin layer opposite to the surface facing the support may be covered with a protective layer (protective film, etc.).

[0080] FIG. 1 shows one embodiment of a photosensitive element. In the photosensitive element 1 shown in FIG. 1 , a support 2, a photosensitive resin layer 3, and a protective layer 4 are laminated in this order. The photosensitive element 1 can be obtained, for example, as follows. A coating liquid that is a photosensitive resin composition is applied to the support 2 to form a coating layer, and the coating layer is then dried to form the photosensitive resin layer 3. Next, the surface of the photosensitive resin layer 3 opposite the support 2 is covered with the protective layer 4, thereby obtaining a photosensitive element 1 that includes the support 2, the photosensitive resin layer 3 formed on the support 2, and the protective layer 4 laminated on the photosensitive resin layer 3. The photosensitive element 1 does not necessarily have to include the protective layer 4.

[0081] As the support, a polymer film having heat resistance and solvent resistance, such as a polyethylene terephthalate film, a polyethylene film, a polypropylene film, or a polyester film, can be used.

[0082] The thickness of the support (such as a support film) may be 1 to 100 μm, 5 to 50 μm, or 5 to 30 μm. When the thickness of the support is 1 μm or more, it is possible to easily prevent the support from being torn when peeled off. When the thickness of the support is 100 μm or less, it is possible to easily prevent a decrease in resolution when exposure is performed through the support.

[0083] The protective layer (protective film, etc.) preferably has a smaller adhesive strength to the photosensitive resin layer than the adhesive strength of the support to the photosensitive resin layer, and is preferably a film with few fisheyes. Here, "fisheyes" refers to foreign matter, undissolved matter, oxidized degradation products, etc., of the material that constitutes the protective film that is introduced into the film when the film is produced by thermally melting the material and then kneading, extrusion, biaxial stretching, casting, etc. In other words, "few fisheyes" means that the film contains few such foreign matter.

[0084] Specifically, the protective layer can be a polymer film having heat resistance and solvent resistance, such as a polyethylene terephthalate film, a polyethylene film, a polypropylene film, or a polyester film. Commercially available polymer films include polypropylene films manufactured by Oji Paper Co., Ltd. (e.g., Alphan MA-410 and E-200C) and Shin-Etsu Film Co., Ltd.; and polyethylene terephthalate films such as PS-25 manufactured by Teijin Limited (e.g., PS series). The protective layer may be made of the same type of material as the support, or may be made of a different type of material.

[0085] The thickness of the protective layer may be 1 to 100 μm, 5 to 50 μm, 5 to 30 μm, or 15 to 30 μm. When the thickness of the protective layer is 1 μm or more, tearing of the protective layer can be suppressed when the photosensitive resin layer and the support are laminated onto a base material (substrate, etc.) while peeling off the protective layer. When the thickness of the protective layer is 100 μm or less, productivity is improved.

[0086] The photosensitive element according to this embodiment can be produced, for example, by a production method including the steps of dissolving at least the components (A), (B), and (C) in an organic solvent to prepare a coating solution having a solids content of about 30 to 60% by mass, applying the coating solution to a support to form a coating layer, and drying the coating layer to form a photosensitive resin layer.

[0087] The coating solution can be applied to a support by known methods such as roll coating, comma coating, gravure coating, air knife coating, die coating, and bar coating. The drying method for the coating layer is not particularly limited as long as it can remove at least a portion of the organic solvent from the coating layer. For example, drying may be performed at 70 to 150°C for approximately 5 to 30 minutes. The amount of organic solvent remaining in the photosensitive resin layer after drying may be 2% by mass or less, from the viewpoint of preventing the organic solvent from diffusing in subsequent steps.

[0088] The thickness of the photosensitive resin layer in the photosensitive element according to this embodiment can be appropriately selected depending on the application, and may be 1 to 100 μm, 1 to 50 μm, or 5 to 40 μm after drying. When the thickness of the photosensitive resin layer is 1 μm or more, industrial coating becomes easy and productivity improves. When the thickness of the photosensitive resin layer is 100 μm or less, adhesion and resolution are further improved.

[0089] The photosensitive element according to this embodiment may further include known intermediate layers such as a cushion layer, an adhesive layer, a light absorbing layer, and a gas barrier layer, as needed.

[0090] The form of the photosensitive element according to this embodiment is not particularly limited. The photosensitive element may be, for example, in the form of a sheet or in the form of a roll wound around a core.

[0091] The photosensitive element according to this embodiment can be suitably used, for example, in the method of forming a resist pattern described below, and is particularly suitable for application to a method of forming a conductor pattern (circuit) by plating.

[0092] <Method of Forming a Resist Pattern> The method of forming a resist pattern according to this embodiment includes: (i) a step of forming a photosensitive resin layer on a substrate (such as a substrate) using the photosensitive resin composition or the photosensitive element (photosensitive resin layer formation step); (ii) a step of irradiating at least a portion of the photosensitive resin layer with actinic rays to cure the photosensitive resin layer (exposure step); and (iii) a step of removing uncured portions of the photosensitive resin layer from the substrate to form a resist pattern (development step), and may include other steps as necessary. The resist pattern can also be referred to as a relief pattern. The method of forming a resist pattern according to this embodiment can also be referred to as a method of manufacturing a substrate having a resist pattern.

[0093] (i) Photosensitive Resin Layer Forming Step In the photosensitive resin layer forming step, a photosensitive resin layer is formed on a substrate (substrate or the like) using the photosensitive resin composition or the photosensitive element. The substrate is not particularly limited, but examples thereof include substrates having a conductor layer. As the substrate having a conductor layer, a circuit-forming substrate having an insulating layer and a conductor layer formed on the insulating layer, or a die pad (substrate for a lead frame, alloy substrate or the like) can be used.

[0094] A method for forming a photosensitive resin layer on a substrate (such as a substrate) includes, for example, removing a protective layer from the photosensitive element, and then pressing the photosensitive resin layer of the photosensitive element onto the substrate while heating. This results in a laminate consisting of the substrate, the photosensitive resin layer, and the support, which are laminated in this order. Alternatively, the photosensitive resin layer may be formed by applying and drying the photosensitive resin composition.

[0095] This photosensitive resin layer forming step is preferably carried out under reduced pressure from the viewpoint of achieving even better adhesion and conformability. The photosensitive resin layer and / or the base material (substrate, etc.) may be heated at a temperature of 70 to 130°C during pressure bonding. The pressure bonding is carried out at a pressure of about 0.1 to 1.0 MPa (1 to 10 kgf / cm 2 The heating may be performed at a pressure of about 1000 psi (approximately 1000 psi). These conditions can be appropriately selected as needed. It is not necessary to preheat the substrate if the photosensitive resin layer is heated to 70 to 130°C. However, the substrate may be preheated in order to further improve adhesion and conformability.

[0096] (ii) Exposure Step) In the exposure step, at least a part of the photosensitive resin layer formed on the base material (substrate or the like) is irradiated with actinic rays, whereby the part irradiated with the actinic rays is cured to form a latent image.

[0097] In this case, when the support present on the photosensitive resin layer is transparent to actinic rays, the actinic rays can be irradiated through the support, whereas when the support is light-shielding, the actinic rays can be irradiated onto the photosensitive resin layer after removing the support.

[0098] The exposure method may be a method of irradiating an actinic ray in an imagewise manner by a direct writing exposure method such as an LDI (Laser Direct Imaging) exposure method or a DLP (Digital Light Processing) exposure method, or a method of irradiating an actinic ray in an imagewise manner through a negative or positive mask pattern called artwork (a mask exposure method), or these may be used in combination.

[0099] Known light sources can be used as the light source for actinic rays. For example, light sources that effectively emit ultraviolet or visible light, such as carbon arc lamps, mercury vapor arc lamps, high-pressure mercury lamps, xenon lamps, gas lasers (argon lasers, etc.), solid-state lasers (YAG lasers, etc.), and semiconductor lasers, can be used. Examples of dominant wavelengths of actinic rays include 355 nm and 405 nm. The dominant wavelength refers to the set wavelength of the actinic rays, and for example, light with a dominant wavelength of 355 nm can include light with a wavelength of 352 to 358 nm.

[0100] ((iii) Development Step) In the development step, the uncured portions of the photosensitive resin layer are removed from the base material (substrate or the like), thereby forming a resist pattern on the base material, which is made of a cured product of the photosensitive resin layer that has been photocured. If a support is present on the photosensitive resin layer, the support is removed, and then the unexposed portions other than the exposed portions are removed (developed). Development methods include wet development and dry development, with wet development being widely used.

[0101] When wet development is used, development can be performed by a known development method using a developer suitable for the photosensitive resin composition. Development methods include dipping, puddling, spraying, brushing, slapping, scrubbing, and swinging immersion, and from the viewpoint of further improving resolution, the high-pressure spraying method is most suitable. Development can also be performed by combining two or more of these methods.

[0102] The composition of the developer can be appropriately selected depending on the composition of the photosensitive resin composition. Examples of the developer include an alkaline aqueous solution and an organic solvent developer.

[0103] When used as a developer, the alkaline aqueous solution is safe, stable, and easy to handle. Examples of the base for the alkaline aqueous solution include alkali hydroxides such as lithium, sodium, or potassium hydroxide; alkali carbonates such as carbonates or bicarbonates of lithium, sodium, potassium, or ammonium; alkali metal phosphates such as potassium phosphate and sodium phosphate; alkali metal pyrophosphates such as sodium pyrophosphate and potassium pyrophosphate; borax; sodium metasilicate; tetramethylammonium hydroxide; ethanolamine; ethylenediamine; diethylenetriamine; 2-amino-2-hydroxymethyl-1,3-propanediol; 1,3-diamino-2-propanol; and morpholine.

[0104] The alkaline aqueous solution is preferably a dilute solution of 0.1 to 5 mass % sodium carbonate, a dilute solution of 0.1 to 5 mass % potassium carbonate, a dilute solution of 0.1 to 5 mass % sodium hydroxide, or a dilute solution of 0.1 to 5 mass % sodium tetraborate. The pH of the alkaline aqueous solution is preferably 9 to 11. The temperature of the alkaline aqueous solution is adjusted according to the alkaline developability of the photosensitive resin layer. The alkaline aqueous solution may contain a surfactant, an antifoaming agent, a small amount of an organic solvent to promote development, or the like.

[0105] Examples of organic solvents include acetone, ethyl acetate, alkoxyethanols having an alkoxy group having 1 to 4 carbon atoms, ethyl alcohol, isopropyl alcohol, butyl alcohol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, and diethylene glycol monobutyl ether. These organic solvents may be used singly or in any combination of two or more. The content of the organic solvent in the aqueous developer is usually preferably 2 to 90% by mass, and the temperature can be adjusted according to the alkali developability.

[0106] Examples of organic solvent developers include 1,1,1-trichloroethane, N-methylpyrrolidone, N,N-dimethylformamide, cyclohexanone, methyl isobutyl ketone, γ-butyrolactone, etc. To prevent ignition, it is preferable to add water to the organic solvent in an amount of 1 to 20% by mass.

[0107] In this embodiment, after removing the unexposed portion in the development step, the film is heated to about 60 to 250° C. or 0.2 to 10 J / cm 2 as needed. 2 The resist pattern may be further hardened by exposing it to light.

[0108] <Method for manufacturing printed wiring board> The method for manufacturing a printed wiring board according to this embodiment includes the steps of forming a resist pattern on a substrate (such as a board) by the method for forming a resist pattern described above, and plating or etching the substrate (such as a board) and a member having the resist pattern (substrate on which a resist pattern has been formed, substrate with a resist pattern) to form a conductor pattern. Furthermore, the method for manufacturing a printed wiring board according to this embodiment may include other steps, such as a step of removing the resist pattern, as necessary.

[0109] In this embodiment, for example, a resist pattern formed on a base material (such as a substrate) can be used as a mask to perform plating or etching on the base material (for example, a conductor layer provided on the base material).

[0110] The plating method in the method for producing a printed wiring board may be either or both of electrolytic plating and electroless plating, and electroless plating is preferred. Examples of electroless plating include copper plating such as copper sulfate plating and copper pyrophosphate plating, solder plating such as high-throw solder plating, Watts bath (nickel sulfate-nickel chloride) plating, nickel plating such as nickel sulfamate, and gold plating.

[0111] In the step of removing the resist pattern, the resist pattern can be stripped using, for example, an aqueous solution that is more strongly alkaline than the aqueous alkaline solution used in the developing step. Examples of such strongly alkaline aqueous solutions include a 1 to 10% by mass aqueous solution of sodium hydroxide and a 1 to 10% by mass aqueous solution of potassium hydroxide. Methods for this include an immersion method and a spray method, which may be used alone or in combination.

[0112] The etching method can be appropriately selected depending on the conductor layer (metal layer) to be removed. Examples of etching solutions include cupric chloride solution, ferric chloride solution, alkaline etching solution, and hydrogen peroxide etching solution. Among these, ferric chloride solution is preferred from the viewpoint of a good etch factor.

[0113] The printed wiring board manufactured by the method for manufacturing a printed wiring board according to this embodiment may be a multilayer printed wiring board, and may have small-diameter through holes.

[0114] The printed wiring board according to this embodiment can be manufactured by a manufacturing method including a step of forming a conductor pattern by performing an etching process or an etching process on a substrate on which a resist pattern has been formed by the method for forming a resist pattern according to this embodiment. An example of a manufacturing process for a printed wiring board by the semi-additive method will be described below with reference to FIG.

[0115] In FIG. 2( a), a substrate (circuit-forming substrate) is prepared in which a conductor layer 10 is formed on an insulating layer 15. The conductor layer 10 is, for example, a metallic copper layer. In FIG. 2( b), a photosensitive resin layer 32 is formed on the conductor layer 10 of the substrate by the photosensitive resin layer formation process. In FIG. 2( c), a mask 20 is placed on the photosensitive resin layer 32, and actinic light 50 is irradiated to expose areas other than the area where the mask 20 is placed, thereby forming a photocured portion. In FIG. 2( d), areas other than the photocured portion formed by the exposure process are removed from the substrate by a development process, thereby forming a resist pattern 30, which is a photocured portion, on the substrate. In FIG. 2( e), a plating layer 42 is formed on the conductor layer 10 by a plating process using the resist pattern 30, which is a photocured portion, as a mask. 2( f), the photocured resist pattern 30 is stripped with a strong alkaline aqueous solution, and then a flash etching process is performed to remove a portion of the plating layer 42 and the conductor layer 10 that was masked by the resist pattern 30, thereby forming the conductor pattern 40. The conductor layer 10 and the plating layer 42 may be made of the same material or different materials. When the conductor layer 10 and the plating layer 42 are made of the same material, the conductor layer 10 and the plating layer 42 may be integrated. Note that although a method of forming the resist pattern 30 using the mask 20 is described in FIG. 2, the resist pattern 30 may also be formed by a direct writing exposure method without using the mask 20.

[0116] The present disclosure will be described in more detail below with reference to examples, although the present disclosure is not limited to these examples.

[0117] [Examples 1 to 7 and Comparative Examples 1 to 6] <Preparation of Photosensitive Resin Composition> The materials shown in Tables 1 and 2 were mixed in the amounts (unit: parts by mass) shown in the tables to prepare solutions of photosensitive resin compositions. The amounts (parts by mass) of components other than the solvent shown in Tables 1 and 2 are the masses of non-volatile components (solid content). Details of each component shown in Tables 1 and 2 are as follows.

[0118] ((A) Binder Polymer) A-1: ​​A solution of a copolymer of methacrylic acid / styrene / benzyl methacrylate / 2-hydroxyethyl methacrylate (mass ratio: 27 / 50 / 20 / 3, Mw: 35,000, acid value: 176.1 mg KOH / g, Tg: 106.8°C) in propylene glycol monomethyl ether / toluene (mass ratio 3 / 4) (solid content: 49.6% by mass) A-2: A solution of a copolymer of methacrylic acid / methyl methacrylate / styrene / benzyl methacrylate (mass ratio: 27 / 5 / 45 / 23, Mw: 51,000, acid value: 176.1 mg KOH / g, Tg: 107.0°C) in propylene glycol monomethyl ether / toluene (mass ratio 3 / 4) (solid content: 47% by mass)

[0119] ((B) Photopolymerizable Compound) FA-321M: 2,2-bis(4-(methacryloxypentaethoxy)phenyl)propane (manufactured by Resonac Corporation, number of EO groups: 10 (average value)) BP-2EM: 2,2-bis(4-(methacryloxypolyethoxy)phenyl)propane (EO groups: 2.6 (total value), manufactured by Kyoeisha Chemical Co., Ltd.) BPE-200: 2,2-bis(4-(methacryloxydiethoxy)phenyl)propane (manufactured by Shin-Nakamura Chemical Co., Ltd.) FA-024M: polyalkylene glycol dimethacrylate (manufactured by Resonac Corporation, number of EO groups: 12 (average value), number of PO groups: 6 (average value)) FA-023M: polyalkylene glycol dimethacrylate (manufactured by Resonac Corporation, number of EO groups: 6 (average value), number of PO groups: 12 (average value)) FA-MECH: γ-chloro-β-hydroxypropyl-β'-methacryloyloxyethyl-o-phthalate (manufactured by Resonac Co., Ltd.)

[0120] ((C) Photopolymerization initiator) B-CIM: 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenylbiimidazole (manufactured by Changzhou New Power Electronic Materials Co., Ltd.) TR-PBG-304: Oxime ester photopolymerization initiator having a carbazole structure represented by the following formula (1) (manufactured by Changzhou New Power Electronic Materials Co., Ltd.) TR-PBG-305: an oxime ester photopolymerization initiator having a phenyl sulfide structure represented by the following formula (2) (manufactured by Changzhou Strong Electronic New Materials Co., Ltd.) TR-PBG-314: an oxime ester photopolymerization initiator having a carbazole structure represented by the following formula (3) (manufactured by Changzhou Strong Electronic New Materials Co., Ltd.) TR-PBG-345: an oxime ester photopolymerization initiator having a carbazole structure represented by the following formula (4) (manufactured by Changzhou Strong Electronic New Materials Co., Ltd.) TR-PBG-358: an oxime ester-based photopolymerization initiator having a fluorene structure represented by the following formula (5) (manufactured by Changzhou Strong Electronic New Materials Co., Ltd.) TR-PBG-365: Oxime ester-based photopolymerization initiator having a fluorene structure (manufactured by Changzhou Strong Electronic New Materials Co., Ltd.) TR-PBG-3057: Oxime ester-based photopolymerization initiator having a phenyl sulfide structure represented by the following formula (6) (manufactured by Changzhou Strong Electronic New Materials Co., Ltd.)

[0121] (Other components) DBA: 9,10-dibutoxyanthracene (manufactured by Kawasaki Chemical Industries, Ltd.) TBC: 4-tert-butylcatechol (manufactured by DIC Corporation) (polymerization inhibitor) LCV: Leuco Crystal Violet (manufactured by Yamada Chemical Industry Co., Ltd.) (color former) MKG: Malachite Green (manufactured by Osaka Organic Chemical Industry Ltd.) (dye) LA-7RD: 4-hydroxy-2,2,6,6-tetramethylpiperidine-N-oxyl (manufactured by Adeka Corporation) FA-711MM: 1,2,2,6,6-pentamethylpiperidin-4-yl methacrylate (manufactured by Resonac Corporation) SF-808H: mixture of carboxybenzotriazole, 5-amino-1H-tetrazole, and methoxypropanol (manufactured by Sanwa Chemical Industries, Ltd.)

[0122] <Preparation of Photosensitive Element> Each of the photosensitive resin compositions obtained above was applied to a 16 μm thick polyethylene terephthalate film (support, product name "FS-31", manufactured by Toray Industries, Inc.) so as to have a uniform thickness. The film was then dried in a hot air convection dryer at 80°C and 120°C to form a photosensitive resin layer having a thickness of 25 μm after drying. A polyethylene film (protective layer, product name "NF-15", manufactured by Tamapoly Corporation) was laminated onto this photosensitive resin layer, and photosensitive elements were obtained in which the support, photosensitive resin layer, and protective layer were laminated in this order.

[0123] <Preparation of Laminate> A copper-clad laminate (substrate, manufactured by Resonac Corporation, product name "MLC-E-67"), a glass epoxy material with copper foil (thickness: 35 μm) laminated on both sides, was washed with water, pickled, and washed with water in that order, and then dried with an air flow. This copper-clad laminate was heated to 80°C. While peeling off the protective layer, the photosensitive element obtained above was laminated onto each of the copper-clad laminates so that the photosensitive resin layer was in contact with the copper surface. This resulted in each laminate having the copper-clad laminate, photosensitive resin layer, and support layered in this order. The obtained laminate was used as a test piece in the evaluation test for the precision of the resist line width described below. Lamination was performed using a heat roll at 110°C, a compression pressure of 0.4 MPa, and a roll speed of 1.0 m / min.

[0124] <Measurement of Minimum Development Time> The laminate was cut into a square (5 cm × 5 cm), and the support was peeled off to obtain a test piece. Next, the unexposed photosensitive resin layer of the test piece was spray-developed at a pressure of 0.18 MPa using a 1% by mass aqueous solution of sodium carbonate at 30°C (nozzle: full cone type, distance between the treatment object and the nozzle tip: 6 cm), and the shortest time at which it was visually confirmed that the unexposed photosensitive resin layer had been removed was obtained as the minimum development time (MD).

[0125] <Evaluation of Resist Line Width Accuracy (Mask Exposure Method)> A 41-step tablet (manufactured by Resonac Co., Ltd.) and a photomask (a photomask capable of producing lines with a line width of 10 μm) were placed on the support of the test piece. Using a parallel beam exposure machine (manufactured by Oak Manufacturing Co., Ltd., product name: EXM1201), ultraviolet light was irradiated from above the photomask surface perpendicularly with an energy amount such that the number of remaining steps on the 41-step tablet was 15. The support was then peeled off, and the resulting resist was spray-developed for twice the minimum development time obtained by the above method to remove the unexposed portions. This resulted in a resist pattern, a photocured product of the photosensitive resin composition, being formed on the copper-clad laminate. The line width of the resulting resist pattern was measured at three locations, and the average value was taken as the actual line width (unit: μm). The ratio (actual value / design value) of the actual line width to the design value (10 μm) of the photomask line width was calculated. This ratio (actual value / design value) is shown in Tables 1 and 2 as the resist line width accuracy. The closer this value is to 1, the less deviation the resulting resist line width has from the design value.

[0126]

[0127]

[0128] [Examples 8 to 12 and Comparative Examples 7 to 10] <Preparation of Photosensitive Resin Composition> The materials shown in Table 3 were mixed in the amounts (unit: parts by mass) shown in the same table to prepare solutions of photosensitive resin compositions. The amounts (parts by mass) of components other than the solvent shown in Table 3 are the masses of non-volatile components (solid content). Details of each component shown in Table 3 are as follows. However, details of the same components as those shown in Tables 1 and 2 are as described above.

[0129] (A) Binder Polymer) A-3: A solution of a copolymer of methacrylic acid / methyl methacrylate / styrene / benzyl methacrylate (mass ratio: 27 / 5 / 45 / 23, Mw: 47000, acid value: 176.1 mg KOH / g, Tg: 107.0°C) in acetone / propylene glycol monomethyl ether (mass ratio 6 / 1) (solid content: 47% by mass)

[0130] ((C) Photopolymerization initiator) C-1: Oxime ester photopolymerization initiator having a carbazole structure represented by the following formula (7) (manufactured by Japan Chemical Research Institute Co., Ltd.)

[0131] <Preparation of Photosensitive Element> Each of the photosensitive resin compositions obtained above was applied to a 16 μm thick polyethylene terephthalate film (support, product name "FS-31", manufactured by Toray Industries, Inc.) so as to have a uniform thickness. The film was then dried in a hot air convection dryer at 80°C and 120°C to form a photosensitive resin layer having a thickness of 25 μm after drying. A polyethylene film (protective layer, product name "NF-15", manufactured by Tamapoly Corporation) was laminated onto this photosensitive resin layer, and photosensitive elements were obtained in which the support, photosensitive resin layer, and protective layer were laminated in this order.

[0132] <Preparation of Laminate> A copper-clad laminate (substrate, manufactured by Resonac Corporation, product name "MLC-E-679"), a glass epoxy material with copper foil (thickness: 35 μm) laminated on both sides, was washed with water, pickled, and washed with water in that order, and then dried with an air flow. This copper-clad laminate was heated to 80°C. While peeling off the protective layer, the photosensitive element obtained above was laminated onto each of the copper-clad laminates so that the photosensitive resin layer was in contact with the copper surface. This resulted in each laminate having the copper-clad laminate, photosensitive resin layer, and support layered in this order. The obtained laminate was used as a test piece in the evaluation test for the precision of the resist line width described below. Lamination was performed using a heat roll at 110°C, a compression pressure of 0.4 MPa, and a roll speed of 1.0 m / min.

[0133] <Evaluation of Resist Line Width Accuracy (Direct Writing Method)> A 41-step step tablet (manufactured by Resonac Co., Ltd.) was placed on the support of the test piece. Next, using an LDI exposure machine (dominant wavelength 405 nm, manufactured by ADTEC Engineering Co., Ltd., product name "DE-1UH"), exposure was performed with an energy amount such that the number of remaining steps on the 41-step step tablet was 15. The support was then peeled off, and spray development was performed for twice the minimum development time obtained by the above method to remove the unexposed portions. This resulted in a resist pattern (design line width: 10 μm) that was a photocured product of the photosensitive resin composition formed on the copper-clad laminate. The line width of the resulting resist pattern was measured at three locations, and the average value was taken as the actual measured line width (unit: μm). The ratio (actual value / design value) of the actual measured value to the design line width of the photomask (10 μm) was calculated. This ratio (actual value / design value) is shown in Table 3 as the resist line width accuracy. The closer this value is to 1, the less deviation the resulting resist line width has from the design value.

[0134]

[0135] DESCRIPTION OF SYMBOLS 1... photosensitive element, 2... support, 3, 32... photosensitive resin layer, 4... protective layer, 10... conductor layer, 15... insulating layer, 20... mask, 30... resist pattern, 40... conductor pattern, 42... plating layer, 50... actinic light.

Claims

1. A photosensitive resin composition comprising: (A) a binder polymer; (B) a photopolymerizable compound having at least one ethylenically unsaturated bond; and (C) a photopolymerization initiator, wherein the (C) photopolymerization initiator contains an oxime ester-based photopolymerization initiator, and the content of the oxime ester-based photopolymerization initiator is 0.3 parts by mass or more per 100 parts by mass of the combined total of the (A) binder polymer and the (B) photopolymerizable compound.

2. The photosensitive resin composition according to claim 1, wherein the binder polymer (A) has a structural unit derived from (meth)acrylic acid and a structural unit derived from benzyl (meth)acrylate or a benzyl (meth)acrylate derivative.

3. The photosensitive resin composition according to claim 1, wherein the photopolymerization initiator (C) consists solely of the oxime ester-based photopolymerization initiator.

4. The photosensitive resin composition according to claim 1, wherein the oxime ester photopolymerization initiator comprises a compound having a carbazole structure.

5. The photosensitive resin composition according to claim 1, wherein the oxime ester photopolymerization initiator comprises a compound having a phenyl sulfide structure.

6. The photosensitive resin composition according to claim 1, wherein the oxime ester photopolymerization initiator comprises a compound having a fluorene structure.

7. The photosensitive resin composition according to claim 1, wherein the content of the oxime ester photopolymerization initiator is 3.0 parts by mass or less per 100 parts by mass of the total of the binder polymer (A) and the photopolymerizable compound (B).

8. The photosensitive resin composition according to claim 1, which is used in a direct imaging system.

9. A photosensitive element comprising a support and a photosensitive resin layer disposed on the support, the photosensitive resin layer comprising the photosensitive resin composition according to any one of claims 1 to 8 or a cured product thereof.

10. A cured product of the photosensitive resin composition according to any one of claims 1 to 8.

11. The cured product according to claim 10, which is a resist pattern.

12. A method for forming a resist pattern, comprising the steps of: forming a photosensitive resin layer on a substrate using the photosensitive resin composition according to any one of claims 1 to 8; irradiating at least a portion of the photosensitive resin layer with active light rays to harden the photosensitive resin layer; and removing an unhardened portion of the photosensitive resin layer from the substrate to form a resist pattern.

13. A method for forming a resist pattern, comprising the steps of: forming a photosensitive resin layer on a substrate using the photosensitive element according to claim 9; irradiating at least a portion of the photosensitive resin layer with active light rays to harden the photosensitive resin layer; and removing the unhardened portion of the photosensitive resin layer from the substrate to form a resist pattern.

14. A method for manufacturing a printed wiring board, comprising: a step of forming a resist pattern on the substrate by the resist pattern forming method described in claim 12; and a step of subjecting the substrate and a member having the resist pattern to a plating process or an etching process.

15. A method for manufacturing a printed wiring board, comprising: a step of forming a resist pattern on the substrate by the resist pattern forming method described in claim 13; and a step of subjecting the substrate and a member having the resist pattern to a plating process or an etching process.