Photosensitive resin composition, photosensitive element, method for forming resist pattern, and method for producing circuit board

MYPI2025004247A0Undetermined Publication Date: 2024-09-17RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025004247
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-17
Filing Date
2024-02-20
Publication Date
2024-09-17

AI Technical Summary

Technical Problem

Conventional photosensitive resin compositions undergo discoloration during long-term storage, affecting their stability and usability in manufacturing wiring boards.

Method used

A photosensitive resin composition is developed using a solvent system comprising ketone solvents with an alicyclic skeleton, such as cyclopentanone and cyclohexanone, and aromatic ether solvents like anisole, replacing toluene to enhance storage stability and prevent discoloration.

Benefits of technology

The new solvent system effectively suppresses discoloration over time, providing improved storage stability and environmental friendliness by eliminating the need for toluene, a regulated substance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025004247_DRAWING_001
    Figure PI2025004247_DRAWING_001
  • Figure PI2025004247_DRAWING_002
    Figure PI2025004247_DRAWING_002
Patent Text Reader

Abstract

A photosensitive resin composition contains a binder polymer, a photopolymerizable compound, a photopolymerization initiator, and a solvent, in which the solvent contains at least one selected from the group consisting of a ketone-based solvent having an alicyclic skeleton and an aromatic ether-based solvent.
Need to check novelty before this filing date? Find Prior Art

Description

Photosensitive resin composition, photosensitive element, method for forming resist pattern, and method for manufacturing wiring board

[0001] The present disclosure relates to a photosensitive resin composition, a photosensitive element, a method for forming a resist pattern, and a method for producing a wiring board.

[0002] In the manufacture of wiring boards, a resist pattern is formed to obtain desired wiring. Photosensitive resin compositions are widely used to form resist patterns. Photosensitive resin compositions can be prepared by dissolving components such as a binder polymer, a photopolymerizable compound, and a photopolymerization initiator in a solvent such as toluene (see, for example, Patent Document 1).

[0003] International Publication No. 2007 / 004619

[0004] Conventional photosensitive resin compositions may discolor after long-term storage, and therefore, there is a need for improved storage stability. Therefore, the present disclosure aims to provide a photosensitive resin composition and a photosensitive element that can suppress discoloration after long-term storage, as well as a method for forming a resist pattern and a method for producing a wiring board using the same.

[0005] As a result of intensive research to solve the above problems, the present inventors have found that discoloration of a photosensitive resin composition after long-term storage can be suppressed by using a specific organic solvent as a solvent used in producing the photosensitive resin composition, and have thus completed the present invention.

[0006] The present disclosure provides the following photosensitive resin composition, photosensitive element, method for forming a resist pattern, and method for manufacturing a wiring board. [1] A photosensitive resin composition containing a binder polymer, a photopolymerizable compound, a photopolymerization initiator, and a solvent, wherein the solvent contains at least one solvent selected from the group consisting of a ketone solvent having an alicyclic skeleton and an aromatic ether solvent. [2] The photosensitive resin composition according to [1] above, wherein the ketone solvent having an alicyclic skeleton contains at least one solvent selected from the group consisting of cyclopentanone and cyclohexanone. [3] The photosensitive resin composition according to [1] above, wherein the aromatic ether solvent contains anisole. [4] The photosensitive resin composition according to any one of [1] to [3] above, wherein the solvent does not contain toluene. [5] A photosensitive element comprising a support and a photosensitive layer formed on the support using the photosensitive resin composition according to any one of [1] to [4] above. [6] A method for forming a resist pattern, comprising the steps of: forming a photosensitive layer on a substrate using the photosensitive resin composition according to any one of [1] to [4] above or the photosensitive element according to [5] above; photocuring a portion of the photosensitive layer; and removing the uncured portion of the photosensitive layer by development. [7] The method for forming a resist pattern according to [6] above, wherein an inorganic alkaline developer is used in the development. [8] A method for producing a wiring board, comprising the step of etching or plating a substrate on which a resist pattern has been formed by the method for forming a resist pattern according to [6] or [7] above, to form a conductor pattern.

[0007] According to the present disclosure, it is possible to provide a photosensitive resin composition and a photosensitive element that can suppress discoloration after long-term storage, as well as a method for forming a resist pattern and a method for manufacturing a wiring board using the same. Furthermore, according to the present disclosure, it is possible to provide an environmentally friendly photosensitive resin composition and a photosensitive element that do not require the use of toluene, an environmentally regulated substance, as a solvent, as well as a method for forming a resist pattern and a method for manufacturing a wiring board using the same.

[0008] 1A to 1C are schematic cross-sectional views showing a photosensitive element according to an embodiment of the present invention; 1B to 1C are schematic cross-sectional views showing a method for manufacturing a wiring board according to an embodiment of the present invention;

[0009] Hereinafter, embodiments of the present disclosure will be described in detail.

[0010] In this specification, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes as long as the intended effect of the process is achieved. A numerical range indicated using "to" indicates a range that includes the numerical values ​​before and after "to" as the minimum and maximum values, respectively. The term "layer" encompasses not only a structure that is formed over the entire surface when observed in a plan view, but also a structure that is formed on only a portion of the surface. "(Meth)acrylic acid" means at least one of "acrylic acid" and the corresponding "methacrylic acid." The same applies to other similar expressions such as (meth)acrylate.

[0011] In this specification, "(poly)oxyethylene group" means an oxyethylene group or a polyoxyethylene group in which two or more ethylene groups are linked by ether bonds. "(poly)oxypropylene group" means an oxypropylene group or a polyoxypropylene group in which two or more propylene groups are linked by ether bonds. "EO-modified" means a compound having a (poly)oxyethylene group. "PO-modified" means a compound having a (poly)oxypropylene group. "EO-PO-modified" means a compound having a (poly)oxyethylene group and / or a (poly)oxypropylene group.

[0012] In this specification, when a composition contains a plurality of substances corresponding to each component, the amount of each component refers to the total amount of the plurality of substances present in the composition, unless otherwise specified. In this specification, the term "solid content" refers to the non-volatile content of the photosensitive resin composition excluding volatile substances. In other words, the term "solid content" refers to components other than the solvent that remain without volatilizing during drying of the photosensitive resin composition, as described below, and includes components that are liquid, syrup-like, or waxy at room temperature (25°C).

[0013] <Photosensitive Resin Composition> The photosensitive resin composition according to this embodiment contains a binder polymer (hereinafter also referred to as "component (A)"), a photopolymerizable compound (hereinafter also referred to as "component (B)"), a photopolymerization initiator (hereinafter also referred to as "component (C)"), and a solvent (hereinafter also referred to as "component (D)"). Here, component (D) includes at least one solvent selected from the group consisting of ketone solvents and aromatic ether solvents having an alicyclic skeleton. Each component will be described below.

[0014] Component (A): Binder Polymer The photosensitive resin composition contains one or more types of component (A). Examples of component (A) include acrylic resins, styrene resins, epoxy resins, amide resins, amide-epoxy resins, alkyd resins, and phenolic resins.

[0015] From the viewpoint of alkali developability, the component (A) may contain an acrylic resin. The acrylic resin is a resin having structural units (monomer units) derived from a (meth)acryloyl group-containing compound.

[0016] The (meth)acryloyl group-containing compound is a compound containing a (meth)acryloyl group. Examples of the (meth)acryloyl group-containing compound include hydroxyalkyl (meth)acrylate, (meth)acrylic acid, (meth)acrylic acid alkyl ester, (meth)acrylic acid aryl ester, (meth)acrylic acid cycloalkyl ester, acrylamide such as diacetone acrylamide, (meth)acrylic acid tetrahydrofurfuryl ester, (meth)acrylic acid dimethylaminoethyl ester, (meth)acrylic acid diethylaminoethyl ester, (meth)acrylic acid glycidyl ester, 2,2,2-trifluoroethyl (meth)acrylate, 2,2,3,3-tetrafluoropropyl (meth)acrylate, α-bromoacrylic acid, α-chloroacrylic acid, β-furyl (meth)acrylic acid, and β-styryl (meth)acrylic acid.

[0017] The acrylic resin may be, for example, a polymer (a) having at least one unit selected from the group consisting of a hydroxyalkyl (meth)acrylate unit, a (meth)acrylic acid unit, a (meth)acrylic acid alkyl ester unit, and a (meth)acrylic acid aryl ester unit.

[0018] The hydroxyalkyl (meth)acrylate unit is a structural unit derived from a hydroxyalkyl (meth)acrylate. Examples of the hydroxyalkyl (meth)acrylate include hydroxymethyl (meth)acrylate, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, hydroxypentyl (meth)acrylate, and hydroxyhexyl (meth)acrylate. When the alkyl moiety in the hydroxyalkyl (meth)acrylate unit has 3 or more carbon atoms, the hydroxyalkyl (meth)acrylate unit may have a branched structure.

[0019] When the polymer (a) has a hydroxyalkyl (meth)acrylate unit, the content of the hydroxyalkyl (meth)acrylate unit, based on the total amount of monomer units constituting the polymer (a), may be 0.5 mass% or more, 0.75 mass% or more, 1.0 mass% or more, 1.5 mass% or more, or 2.0 mass% or more from the viewpoint of dispersibility, and may be 20 mass% or less, 15 mass% or less, 8 mass% or less, 5 mass% or less, or 4 mass% or less from the viewpoint of water absorbency.

[0020] The (meth)acrylic acid unit is a structural unit derived from (meth)acrylic acid. When the polymer (a) has the (meth)acrylic acid unit, the content of the (meth)acrylic acid unit may be 1% by mass or more, 5% by mass or more, 10% by mass or more, 15% by mass or more, 20% by mass or more, or 25% by mass or more, or may be 50% by mass or less, 45% by mass or less, 40% by mass or less, 35% by mass or less, or 30% by mass or less, based on the total amount of the monomer units constituting the polymer (a), from the viewpoints of resolution and adhesion.

[0021] The (meth)acrylic acid alkyl ester unit is a structural unit derived from a (meth)acrylic acid alkyl ester. The alkyl group of the (meth)acrylic acid alkyl ester may be, for example, a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, a dodecyl group, or a structural isomer thereof, or may be an alkyl group having 1 to 4 carbon atoms from the viewpoint of release properties.

[0022] When the polymer (a) has a (meth)acrylic acid alkyl ester unit, the content of the (meth)acrylic acid alkyl ester unit may be 1 mass % or more, 2 mass % or more, or 3 mass % or more, based on the total amount of monomer units constituting the polymer (a), from the viewpoint of release properties, and may be 80 mass % or less, 60 mass % or less, or 50 mass % or less, from the viewpoint of resolution and adhesion.

[0023] The (meth)acrylic acid aryl ester unit is a structural unit derived from a (meth)acrylic acid aryl ester. Examples of the (meth)acrylic acid aryl ester include benzyl (meth)acrylate, phenyl (meth)acrylate, and naphthyl (meth)acrylate. When the polymer (a) has a (meth)acrylic acid aryl ester unit, the content of the (meth)acrylic acid aryl ester unit may be 1% by mass or more, 5% by mass or more, 10% by mass or more, 15% by mass or more, or 18% by mass or more, or 50% by mass or less, 45% by mass or less, 40% by mass or less, 35% by mass or less, 30% by mass or less, 25% by mass or less, or 23% by mass or less, based on the total amount of the monomer units constituting the polymer (a), from the viewpoint of resolution and adhesion.

[0024] The polymer (a) may further have a structural unit derived from a monomer other than the (meth)acryloyl group-containing compound. The other monomer may be one type or two or more types.

[0025] Examples of other monomers include styrene or styrene derivatives, acrylonitrile, vinyl alcohol ethers such as vinyl n-butyl ether, maleic acid, maleic anhydride, maleic acid monoesters such as monomethyl maleate, monoethyl maleate, and monoisopropyl maleate, fumaric acid, cinnamic acid, α-cyanocinnamic acid, itaconic acid, crotonic acid, and propiolic acid. Examples of styrene derivatives include vinyltoluene and α-methylstyrene.

[0026] When polymer (a) has a structural unit derived from styrene or a styrene derivative (hereinafter also referred to as a "styrene or styrene derivative unit"), the content of the styrene or styrene derivative unit, based on the total amount of monomer units constituting polymer (a), may be 20% by mass or more, 30% by mass or more, 40% by mass or more, 45% by mass or more, 47% by mass or more, or 50% by mass or more from the viewpoint of resolution, and may be 90% by mass or less, 85% by mass or less, 80% by mass or less, 70% by mass or less, or 60% by mass or less from the viewpoint of developability.

[0027] The polymer (a) may be a polymer (a1) having hydroxyalkyl (meth)acrylate units, (meth)acrylic acid units, styrene or styrene derivative units, and (meth)acrylic acid aryl ester units.

[0028] The component (A) may contain a binder polymer other than the polymer (a), or may consist solely of the polymer (a). From the viewpoints of adhesion and resolution, the content of the polymer (a) in the component (A) may be 50 to 100 mass % or 80 to 100 mass % based on the total amount of the component (A).

[0029] The acid value of polymer (a) may be 100 mgKOH / g or more, 120 mgKOH / g or more, 140 mgKOH / g or more, or 150 mgKOH / g or more from the viewpoint of developability, and may be 250 mgKOH / g or less, 240 mgKOH / g or less, or 230 mgKOH / g or less from the viewpoint of adhesion (developer resistance) of the cured product of the photosensitive resin composition. The acid value of polymer (a) can be adjusted by the content of structural units (e.g., (meth)acrylic acid units) constituting polymer (a). When component (A) contains a binder polymer other than polymer (a), the acid value of the other binder polymer may also be within the above range.

[0030] The weight average molecular weight (Mw) of the polymer (a) may be 10,000 or more, 15,000 or more, 20,000 or more, 25,000 or more, or 30,000 or more from the viewpoint of adhesion (developer resistance) of the cured product of the photosensitive resin composition, and may be 100,000 or less, 80,000 or less, 60,000 or less, or 40,000 or less from the viewpoint of developability. The dispersity (Mw / Mn) of the polymer (a) may be, for example, 1.0 or more or 1.5 or more, and from the viewpoint of adhesion and resolution, may be 3.0 or less or 2.5 or less. When the component (A) contains a binder polymer other than the polymer (a), the Mw of the other binder polymer may also be within the above range.

[0031] The weight average molecular weight and dispersity can be measured, for example, by gel permeation chromatography (GPC) using a calibration curve of standard polystyrene. More specifically, they can be measured under the conditions described in the Examples. For compounds with low molecular weights, if it is difficult to measure the weight average molecular weight using the above-mentioned method, the molecular weight can be measured by another method and the average can be calculated.

[0032] The content of the component (A), based on the total solid content of the photosensitive resin composition, may be 20% by mass or more, 30% by mass or more, or 40% by mass or more from the viewpoint of film formability, and may be 90% by mass or less, 80% by mass or less, 70% by mass or less, or 65% by mass or less from the viewpoint of sensitivity and resolution.

[0033] The content of the (A) component may be 30 parts by mass or more, 35 parts by mass or more, or 40 parts by mass or more, relative to 100 parts by mass of the total amount of the (A) component and the (B) component, from the viewpoint of film formability, and may be 70 parts by mass or less, 65 parts by mass or less, or 60 parts by mass or less, from the viewpoint of sensitivity and resolution.

[0034] Component (B): Photopolymerizable Compound The photosensitive resin composition contains one or more types of component (B). Component (B) may be any compound that polymerizes when exposed to light, and may be, for example, a compound having an ethylenically unsaturated bond. Component (B) may contain a polyfunctional monomer having two or more reactive groups that react with radicals. From the viewpoints of alkali developability, resolution, and release properties after curing, component (B) may contain a bisphenol A type (meth)acrylate compound.

[0035] Examples of bisphenol A type (meth)acrylate compounds include 2,2-bis(4-((meth)acryloxypolyethoxy)phenyl)propane, 2,2-bis(4-((meth)acryloxypolypropoxy)phenyl)propane, 2,2-bis(4-((meth)acryloxypolybutoxy)phenyl)propane, and 2,2-bis(4-((meth)acryloxypolyethoxypolypropoxy)phenyl)propane. From the viewpoints of resolution and release properties, component (B) may contain 2,2-bis(4-((meth)acryloxypolyethoxy)phenyl)propane. Examples of 2,2-bis(4-((meth)acryloxypolyethoxy)phenyl)propane include (2,2-bis(4-((meth)acryloxypentaethoxy)phenyl)propane). As the 2,2-bis(4-((meth)acryloxypolyethoxy)phenyl)propane, a compound having 10 or more oxyethylene groups may be used, or a compound having less than 10 oxyethylene groups may be used, or a compound having 10 or more oxyethylene groups and a compound having less than 10 oxyethylene groups may be used in combination.

[0036] When the component (B) contains a bisphenol A type (meth)acrylate compound, the content of the bisphenol A type (meth)acrylate compound may be 20 mass % or more, 40 mass % or more, 60 mass % or more, 80 mass % or more, 85 mass % or more, or 90 mass % or more, and may be 100 mass % or less, or 95 mass % or less, based on the total amount of the component (B), from the viewpoint of resist resolution.

[0037] From the viewpoint of resolution and flexibility, component (B) may contain an α,β-unsaturated ester compound obtained by reacting a polyhydric alcohol with an α,β-unsaturated carboxylic acid. Examples of the α,β-unsaturated ester compound include polyalkylene glycol di(meth)acrylates such as polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, and EO-modified polypropylene glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, EO-modified trimethylolpropane tri(meth)acrylate, PO-modified trimethylolpropane tri(meth)acrylate, EO-PO-modified trimethylolpropane tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, and tetramethylolmethane tetra(meth)acrylate.

[0038] From the viewpoint of sensitivity and adhesion, the component (B) may contain a compound having three or more (meth)acryloyl groups. Examples of such a compound include trimethylolpropane tri(meth)acrylate, EO-modified trimethylolpropane tri(meth)acrylate, PO-modified trimethylolpropane tri(meth)acrylate, EO-PO-modified trimethylolpropane tri(meth)acrylate, EO-modified pentaerythritol tetra(meth)acrylate, EO-modified ditrimethylolpropane tetra(meth)acrylate, and EO-modified dipentaerythritol hexa(meth)acrylate.

[0039] When the component (B) includes an α,β-unsaturated ester compound, the content of the α,β-unsaturated ester compound, based on the total amount of the component (B), may be 1% by mass or more, 3% by mass or more, 5% by mass or more, or 8% by mass or more from the viewpoint of flexibility, and may be 20% by mass or less, 15% by mass or less, or 10% by mass or less from the viewpoint of resolution.

[0040] The photosensitive resin composition may contain, as component (B), a photopolymerizable compound other than the bisphenol A (meth)acrylate compound and the α,β-unsaturated ester compound.

[0041] Examples of other photopolymerizable compounds include nonylphenoxy polyethyleneoxy acrylate, phthalic acid compounds, (meth)acrylic acid alkyl esters, and photopolymerizable compounds having at least one cationically polymerizable cyclic ether group in the molecule (such as oxetane compounds). From the viewpoints of resolution, adhesion, resist shape, and release properties after curing, the other photopolymerizable compound may be at least one selected from the group consisting of nonylphenoxy polyethyleneoxy acrylate and phthalic acid compounds.

[0042] Examples of nonylphenoxy polyethyleneoxyacrylates include nonylphenoxytriethyleneoxyacrylate, nonylphenoxytetraethyleneoxyacrylate, nonylphenoxypentaethyleneoxyacrylate, nonylphenoxyhexaethyleneoxyacrylate, nonylphenoxyheptaethyleneoxyacrylate, nonylphenoxyoctaethyleneoxyacrylate, nonylphenoxynonaethyleneoxyacrylate, nonylphenoxydecaethyleneoxyacrylate, and nonylphenoxyundecaethyleneoxyacrylate.

[0043] Examples of phthalic acid compounds include γ-chloro-β-hydroxypropyl-β'-(meth)acryloyloxyethyl-o-phthalate (also known as 3-chloro-2-hydroxypropyl-2-(meth)acryloyloxyethyl phthalate), β-hydroxyethyl-β'-(meth)acryloyloxyethyl-o-phthalate, and β-hydroxypropyl-β'-(meth)acryloyloxyethyl-o-phthalate.

[0044] When the component (B) contains other photopolymerizable compounds, the content of the other photopolymerizable compounds may be 1% by mass or more, 3% by mass or more, or 5% by mass or more, and may be 30% by mass or less, 25% by mass or less, or 20% by mass or less, based on the total amount of the component (B), from the viewpoints of resolution, adhesion, resist shape, and release properties after curing.

[0045] From the viewpoints of adhesion and resolution, the component (B) may include, among the above-mentioned compounds, a compound having a total of 2 to 40 oxyethylene groups (EO groups) and / or oxypropylene groups (PO groups) in the molecule. From the viewpoints of adhesion and resolution, the total number of EO groups and / or PO groups may be 2 to 40 or 2 to 30.

[0046] Component (B) may contain a compound having a urethane group. Examples of compounds having a urethane group include compounds having 1 to 3 urethane groups in the molecule. The compound having a urethane group does not necessarily have to contain a compound having 4 or more urethane groups in the molecule.

[0047] The content of the component (B) may be 3% by mass or more, 10% by mass or more, or 25% by mass or more, based on the total solid content of the photosensitive resin composition, from the viewpoint of sensitivity and resolution, and may be 70% by mass or less, 60% by mass or less, or 50% by mass or less, from the viewpoint of film formability.

[0048] Component (C): Photopolymerization Initiator The photosensitive resin composition contains one or more kinds of component (C). Examples of component (C) include hexaarylbiimidazole compounds; oxime ester compounds such as 1,2-octanedione-1-[4-(phenylthio)phenyl]-2-(o-benzoyloxime), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone-1-(o-acetyloxime), and 1-phenyl-1,2-propanedione-2-[o-(ethoxycarbonyl)oxime]; benzophenone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, and 4-(2-hydroxybenzoyl)-1-methylbenzoyl aromatic ketones such as 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propanone-1; quinones such as alkyl anthraquinones; benzoin ether compounds such as benzoin alkyl ethers; benzoin compounds such as benzoin and alkylbenzoins; benzyl derivatives such as benzyl dimethyl ketal; bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide; bis(2,6-dimethylbenzoyl)-2,4,4-trimethyl-pentylphosphine oxide; and (2,4,6-trimethylbenzoyl)ethoxyphenylphosphine oxide.

[0049] The component (C) may include at least one selected from the group consisting of a hexaarylbiimidazole compound and an oxime ester compound, or may include a hexaarylbiimidazole compound. The aryl group in the hexaarylbiimidazole compound may be a phenyl group or the like. The hydrogen atom bonded to the aryl group in the hexaarylbiimidazole compound may be substituted with a halogen atom (e.g., a chlorine atom) or an alkoxy group (e.g., a methoxy group).

[0050] The hexaarylbiimidazole compound may be a 2,4,5-triarylimidazole dimer, such as 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer, 2-(o-chlorophenyl)-4,5-bis-(m-methoxyphenyl)imidazole dimer, and 2-(p-methoxyphenyl)-4,5-diphenylimidazole dimer.

[0051] From the viewpoint of sensitivity and adhesion, the content of the (C) component may be 0.1 parts by mass or more, 0.5 parts by mass or more, 1 part by mass or more, 3 parts by mass or more, 5 parts by mass or more, 6 parts by mass or more, 7 parts by mass or more, or 7.5 parts by mass or more, relative to 100 parts by mass of the total amount of the (A) component and the (B) component, and may be 20 parts by mass or less, 15 parts by mass or less, 10 parts by mass or less, 9 parts by mass or less, or 8.5 parts by mass or less.

[0052] Component (D): Solvent The photosensitive resin composition contains one or more types of component (D). The component (D) contains at least one solvent selected from the group consisting of a ketone solvent having an alicyclic skeleton (hereinafter also referred to as "component (d1)") and an aromatic ether solvent (hereinafter also referred to as "component (d2)"). By using such components (d1) and (d2) as component (D), the photosensitive resin composition can suppress discoloration after long-term storage.

[0053] The components (d1) and (d2) can achieve solubility and appropriate viscosity equivalent to or greater than that of toluene, which has traditionally been used in preparing photosensitive resin compositions, and can therefore be used as alternative solvents to toluene. The component (D) does not need to contain toluene, making it possible to produce an environmentally friendly photosensitive resin composition.

[0054] Examples of the component (d1) include cyclopentanone and cyclohexanone. Examples of the component (d2) include anisole. From the viewpoint of achieving superior discoloration suppression, the component (D) preferably contains at least one selected from the group consisting of cyclopentanone, cyclohexanone, and anisole, and more preferably contains at least one selected from the group consisting of cyclopentanone and cyclohexanone.

[0055] The component (d1) can improve the solubility of components other than the component (D) (e.g., the component (C)) contained in the photosensitive resin composition, and therefore may be used alone. The use of the component (d1) can reduce the number of solvents used, which is advantageous in terms of environmental friendliness and workability.

[0056] Component (D) may contain other solvents, such as methanol and acetone, as long as the effects of the present disclosure are not impaired.

[0057] The content of the (D) component may be 20 parts by mass or more, or 30 parts by mass or more, and may be 70 parts by mass or less, 60 parts by mass or less, 50 parts by mass or less, or 40 parts by mass or less, relative to 100 parts by mass of the total amount of the (A) component and the (B) component.

[0058] When the (D) component contains the (d1) component, the content of the (d1) component may be 10 parts by mass or more, 20 parts by mass or more, 25 parts by mass or more, 30 parts by mass or more, or 35 parts by mass or more, and may be 70 parts by mass or less, 60 parts by mass or less, 50 parts by mass or less, or 40 parts by mass or less, relative to 100 parts by mass of the total amount of the (A) component and the (B) component. When the (D) component contains the (d1) component, the content of the (d1) component may be 50% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, 90% by mass or more, or 100% by mass, based on the total amount of the (D) component. When the (D) component contains the (d1) component, the content of the (d1) component may be 2.5 times or more, 3.0 times or more, 3.5 times or more, 4.0 times or more, or 4.5 times or more than the content of the (C) component.

[0059] When the (D) component contains the (d2) component, the content of the (d2) component may be 10 parts by mass or more, 15 parts by mass or more, or 20 parts by mass or more, and may be 70 parts by mass or less, 60 parts by mass or less, 50 parts by mass or less, 40 parts by mass or less, or 30 parts by mass or less, relative to 100 parts by mass of the total amount of the (A) component and the (B) component. When the (D) component contains the (d2) component, the content of the (d2) component may be 40% by mass or more, 45% by mass or more, 50% by mass or more, or 55% by mass or more, and may be 70% by mass or less, or 60% by mass or less, based on the total amount of the (D) component. When the (D) component contains the (d2) component, the content of the (d2) component may be 2.5 times or more, 3.0 times or more, 3.5 times or more, 4.0 times or more, or 4.5 times or more the content of the (C) component.

[0060] Component (E): Photosensitizer The photosensitive resin composition may further contain a photosensitizer as component (E). Component (E) is not particularly limited, and known photosensitizers can be used. Examples of component (E) include anthracene-based sensitizers. Examples of anthracene-based sensitizers include 9,10-dibutoxyanthracene, 9,10-diphenylanthracene, and 9,10-diethoxyanthracene. From the viewpoints of adhesion and resolution, the anthracene-based sensitizer may be 9,10-dibutoxyanthracene.

[0061] When the photosensitive resin composition contains the component (E), the content of the component (E) may be 0.2 parts by mass or more, 0.3 parts by mass or more, 0.4 parts by mass or more, or 0.5 parts by mass or more, relative to 100 parts by mass of the total of the component (A) and the component (B), from the viewpoints of sensitivity, adhesion, and resolution, and may be 1.5 parts by mass or less, 1.0 parts by mass or less, 0.8 parts by mass or less, 0.75 parts by mass or less, or 0.7 parts by mass or less, from the viewpoint of the resist pattern shape.

[0062] Component (F): Polymerization Inhibitor The photosensitive resin composition may further contain a polymerization inhibitor as component (F). Examples of the polymerization inhibitor include t-butylcatechol and 4-hydroxy-2,2,6,6-tetramethylpiperidine-N-oxyl.

[0063] When the photosensitive resin composition contains the component (F), the content of the component (F) may be 0.001 part by mass or more, 0.005 part by mass or more, 0.008 part by mass or more, 0.01 part by mass or more, or 0.015 part by mass or more, relative to 100 parts by mass of the total amount of the component (A) and the component (B), from the viewpoints of sensitivity and resolution; and may be 0.1 part by mass or less, 0.05 part by mass or less, or 0.03 part by mass or less, from the viewpoints of sensitivity and adhesion.

[0064] Component (G): Dye The photosensitive resin composition may further contain a dye as component (G). The component (G) is not particularly limited, and any known dye can be used. Examples of component (G) include leuco dyes, phthalocyanine green, crystal violet, methyl orange, Nile blue 2B, Victoria blue, malachite green, basic blue 20, and diamond green. Examples of leuco dyes include leuco crystal violet and fluoran dyes.

[0065] When the photosensitive resin composition contains the component (G), the content of the component (G) may be 0.01 parts by mass or more, 0.05 parts by mass or more, 0.10 parts by mass or more, 0.20 parts by mass or more, 0.30 parts by mass or more, 0.40 parts by mass or more, or 0.50 parts by mass or more, relative to 100 parts by mass of the total amount of the components (A) and (B).

[0066] The photosensitive resin composition may further contain one or more other components in addition to the components described above. Examples of other components include hydrogen donors (such as bis[4-(dimethylamino)phenyl]methane, bis[4-(diethylamino)phenyl]methane, and N-phenylglycine), tribromophenyl sulfone, thermal color-development inhibitors, plasticizers (such as p-toluenesulfonamide), pigments, fillers, antifoaming agents, flame retardants, stabilizers, adhesion promoters, leveling agents, release promoters, antioxidants, fragrances, imaging agents, and thermal crosslinkers. The content of these other components may be 0.005 parts by mass or more, or 0.01 parts by mass or more, or may be 20 parts by mass or less, per 100 parts by mass of the total amount of component (A) and component (B).

[0067] The photosensitive resin composition can be suitably used in the method for forming a resist pattern and the method for producing a wiring board, which will be described later.

[0068] <Photosensitive Element> The photosensitive element according to this embodiment includes a support and a photosensitive layer formed on the support using the above-described photosensitive resin composition. The photosensitive element may further include a protective layer on the photosensitive layer.

[0069] 1 is a schematic cross-sectional view showing a photosensitive element according to one embodiment. As shown in FIG. 1, the photosensitive element 1 includes a support 2, a photosensitive layer 3 provided on the support 2, and a protective layer 4 provided on the side of the photosensitive layer 3 opposite the support 2.

[0070] The support may be a polymer film having heat resistance and solvent resistance, such as polyester films such as polyethylene terephthalate film, polybutylene terephthalate film, and polyethylene-2,6-naphthalate film, and polyolefin films such as polyethylene film and polypropylene film.

[0071] The haze of the support may be 0.01 to 5.0%, 0.01 to 1.5%, 0.01 to 1.0%, or 0.01 to 0.5%. Haze can be measured using a commercially available haze meter (turbidity meter) in accordance with the method specified in JIS K7105. Haze can be measured, for example, using a commercially available turbidity meter such as NDH-5000 (trade name, manufactured by Nippon Denshoku Industries Co., Ltd.).

[0072] The thickness of the support may be 1 μm or more, 5 μm or more, or 10 μm or more from the viewpoint of easily preventing damage to the support when peeling the support from the photosensitive layer, and may be 100 μm or less, 50 μm or less, 30 μm or less, or 20 μm or less from the viewpoint of easily and suitably performing exposure when exposing through the support.

[0073] The protective layer may be a polymer film having heat resistance and solvent resistance, and for example, a polyolefin film such as a polyethylene film or a polypropylene film can be used. In particular, by using a polyethylene film as the protective layer, misalignment of the photosensitive element during winding can be suppressed, and static electricity is less likely to be generated when the protective layer is peeled off from the photosensitive layer, thereby suppressing damage to the photosensitive layer.

[0074] The thickness of the protective layer may be 1 μm or more, 5 μm or more, 10 μm or more, or 15 μm or more from the viewpoint of easily suppressing damage to the protective layer when the photosensitive layer and the support are laminated onto the substrate while peeling off the protective layer, or may be 100 μm or less, 50 μm or less, 40 μm or less, or 30 μm or less from the viewpoint of easily improving productivity.

[0075] The photosensitive layer is formed using the photosensitive resin composition described above. The thickness of the photosensitive layer after drying (after volatilizing the solvent) may be 1 μm or more, 5 μm or more, 10 μm or more, or 15 μm or more from the viewpoints of facilitating coating and improving productivity, and may be 100 μm or less, 50 μm or less, 40 μm or less, or 30 μm or less from the viewpoints of adhesion and resolution.

[0076] The photosensitive element 1 can be obtained, for example, as follows. First, a photosensitive layer 3 is formed on a support 2. The photosensitive layer 3 can be formed, for example, by applying a photosensitive resin composition to form a coating layer and drying this coating layer. Next, a protective layer 4 is formed on the surface of the photosensitive layer 3 opposite to the support 2.

[0077] The coating layer is formed by a known method such as roll coating, comma coating, gravure coating, air knife coating, die coating, bar coating, etc. The coating layer is dried so that the amount of solvent remaining in the photosensitive layer 3 is, for example, 2% by mass or less, and specifically, for example, at 70 to 150°C for about 5 to 30 minutes.

[0078] In another embodiment, the photosensitive element may further include other layers such as a cushion layer, an adhesive layer, a light absorbing layer, and a gas barrier layer.

[0079] The photosensitive element 1 may be, for example, in the form of a sheet, or in the form of a photosensitive element roll wound around a core. In the photosensitive element roll, the photosensitive element 1 is preferably wound with the support 2 facing outward. The core is formed of, for example, polyethylene, polypropylene, polystyrene, polyvinyl chloride, acrylonitrile-butadiene-styrene copolymer, or the like. An end separator may be provided on the end face of the photosensitive element roll from the viewpoint of end face protection, or a moisture-proof end face separator may be provided from the viewpoint of edge fusion resistance. The photosensitive element 1 may be wrapped, for example, in a black sheet with low moisture permeability.

[0080] The photosensitive element according to this embodiment can be suitably used in the method for forming a resist pattern and the method for manufacturing a wiring board, which will be described later.

[0081] <Method of Forming Resist Pattern> The method of forming a resist pattern according to this embodiment includes a step of forming a photosensitive layer on a substrate using the photosensitive resin composition or the photosensitive element (hereinafter also referred to as a "photosensitive layer forming step"), a step of photocuring a portion of the photosensitive layer (hereinafter also referred to as an "exposure step"), and a step of removing an uncured portion of the photosensitive layer by development (hereinafter also referred to as a "development step"), and may further include other steps as necessary. The resist pattern can also be referred to as a photocured product pattern of the photosensitive resin composition or a relief pattern.

[0082] (Photosensitive layer forming step) In the photosensitive layer forming step, a photosensitive layer is formed on a substrate using a photosensitive resin composition or a photosensitive element. The substrate is not particularly limited, but typically, a circuit-forming substrate having an insulating layer and a conductor layer formed on the insulating layer, or a die pad (substrate for lead frame) such as an alloy substrate is used.

[0083] For example, the photosensitive layer can be formed on the substrate by removing the protective layer from the photosensitive element and then pressing the photosensitive layer of the photosensitive element onto the substrate while heating, thereby obtaining a laminate having the substrate, photosensitive layer, and support in this order.

[0084] The photosensitive layer forming step may be carried out under reduced pressure from the viewpoint of adhesion and followability. Heating during pressure bonding may be carried out at a temperature of 70 to 130°C, and pressure bonding may be carried out at 0.1 to 1.0 MPa (1 to 10 kgf / cm 2 These conditions can be appropriately selected as needed. Note that if the photosensitive layer of the photosensitive element is heated to 70 to 130°C, it is not necessary to preheat the substrate, but the substrate can be preheated in order to further improve the adhesion and followability.

[0085] In the exposure step, the photosensitive layer may be exposed to actinic rays through the support, or the support may be peeled off and then the photosensitive layer may be exposed to actinic rays. As a result, the exposed area irradiated with actinic rays is photocured to form a photocured area (latent image).

[0086] As the exposure method, known exposure methods can be applied, for example, a method of irradiating an actinic ray in an imagewise manner through a negative or positive mask pattern called artwork (mask exposure method), an LDI (laser direct imaging) exposure method, and a method of irradiating an actinic ray projected from a photomask image through a lens in an imagewise manner (projection exposure method). Among them, from the viewpoint of resolution, the LDI exposure method or the projection exposure method may be used. The projection exposure method can also be said to be an exposure method using an actinic ray with attenuated energy.

[0087] The light source of actinic rays is not particularly limited as long as it is a commonly used known light source, and examples thereof include those that effectively emit ultraviolet rays, such as carbon arc lamps, mercury vapor arc lamps, ultra-high pressure mercury lamps, high pressure mercury lamps, xenon lamps, gas lasers such as argon lasers, solid-state lasers such as YAG lasers, and semiconductor lasers such as gallium nitride blue-violet lasers. Among these, from the viewpoint of improving the resolution and alignment in a well-balanced manner, a light source capable of emitting i-line monochromatic light with an exposure wavelength of 365 nm, a light source capable of emitting h-line monochromatic light with an exposure wavelength of 405 nm, or a light source capable of emitting actinic rays with an exposure wavelength of cross-linked i, h, and g may be used. Alternatively, a light source capable of emitting i-line monochromatic light with an exposure wavelength of 365 nm or h-line monochromatic light with an exposure wavelength of 405 nm may be used. Examples of light sources capable of emitting i-line monochromatic light with an exposure wavelength of 365 nm include ultra-high pressure mercury lamps. Examples of light sources capable of emitting h-line monochromatic light with an exposure wavelength of 405 nm include blue-violet laser diodes with a wavelength of 405 nm.

[0088] In the method for forming a resist pattern according to this embodiment, from the viewpoint of adhesion, post-exposure baking (PEB) may be performed after the exposure step and before the development step. The temperature when performing PEB may be 50 to 100° C. Heating may be performed using a heater such as a hot plate, a box dryer, or a heating roll.

[0089] (Development Step) In the development step, the uncured portions of the photosensitive layer are removed from the substrate. When the photosensitive layer is exposed through the support, the support and the uncured portions of the photosensitive layer are removed from the substrate. In the development step, a resist pattern consisting of photocured portions of the photosensitive layer is formed on the substrate. The development method may be wet development or dry development, and wet development is preferred.

[0090] In the case of wet development, development can be carried out by a known wet development method using a developer suitable for the photosensitive resin composition. Examples of wet development methods include dipping, puddling, high-pressure spraying, brushing, scrubbing, and swinging immersion. These wet development methods may be used alone or in combination of two or more methods.

[0091] The developer is appropriately selected depending on the constitution of the photosensitive resin composition, and may be, for example, an alkaline developer or an organic solvent developer.

[0092] From the viewpoints of safety, stability, and ease of use, an alkaline developer may be used as the developer. The alkaline developer may be an aqueous solution containing a base such as an alkali hydroxide such as lithium, sodium, or potassium hydroxide; an alkali carbonate such as lithium, sodium, potassium, or ammonium carbonate or bicarbonate; an alkali metal phosphate such as potassium phosphate or sodium phosphate; an alkali metal pyrophosphate such as sodium pyrophosphate or potassium pyrophosphate; borax; sodium metasilicate; tetramethylammonium hydroxide; ethanolamine; ethylenediamine; diethylenetriamine; 2-amino-2-hydroxymethyl-1,3-propanediol; 1,3-diamino-2-propanol; or morpholine.

[0093] From the viewpoint of environmental friendliness, an inorganic alkaline developer may be used, such as a dilute solution of 0.1 to 5 mass % sodium carbonate, a dilute solution of 0.1 to 5 mass % potassium carbonate, a dilute solution of 0.1 to 5 mass % sodium hydroxide, or a dilute solution of 0.1 to 5 mass % sodium tetraborate.

[0094] The pH of the alkaline developer used for development may be in the range of 9 to 11, and the temperature of the alkaline developer can be adjusted according to the developability of the photosensitive layer. The alkaline developer may contain, for example, a surfactant, an antifoaming agent, or a small amount of an organic solvent to promote development. Examples of organic solvents used in the alkaline developer include 3-acetone alcohol, acetone, ethyl acetate, an alkoxyethanol having an alkoxy group having 1 to 4 carbon atoms, ethyl alcohol, isopropyl alcohol, butyl alcohol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, and diethylene glycol monobutyl ether.

[0095] Examples of organic solvents used in the organic solvent developer include 1,1,1-trichloroethane, N-methyl-2-pyrrolidone, N,N-dimethylformamide, cyclohexanone, methyl isobutyl ketone, and γ-butyrolactone. From the viewpoint of preventing ignition, these organic solvents may be used as the organic solvent developer by adding water in a range of 1 to 20% by mass.

[0096] (Other Steps) In the method for forming a resist pattern according to this embodiment, after removing the uncured portion in the development step, heating at 60 to 250° C. or irradiating with 0.2 to 10 J / cm 2 is performed as necessary. 2 The method may further include a step of further hardening the resist pattern by exposing the resist pattern to light at an exposure dose of 1000 nm or more.

[0097] <Method of manufacturing wiring board> The method of manufacturing a wiring board according to this embodiment includes a step of forming a conductor pattern (wiring layer) by etching or plating a substrate on which a resist pattern has been formed by the above-described method of forming a resist pattern, and may also include other steps such as a resist pattern removal step as necessary.

[0098] In the etching process, a resist pattern formed on a substrate having a conductive layer is used as a mask to etch away the conductive layer of the substrate that is not covered with the resist, thereby forming a conductive pattern.

[0099] The etching method is appropriately selected depending on the conductor layer to be removed. Examples of the etching solution include a cupric chloride solution, a ferric chloride solution, an alkaline etching solution, and a hydrogen peroxide-based etching solution. From the viewpoint of a good etch factor, a ferric chloride solution may be used as the etching solution.

[0100] In the plating process, a resist pattern formed on a substrate having a conductor layer is used as a mask to plate copper, solder, etc. on the conductor layer of the substrate that is not covered with the resist. After the plating process, the resist is removed by removing the resist pattern as described below, and the conductor layer that was covered with the resist is then etched to form the conductor pattern.

[0101] The plating method may be electrolytic plating or electroless plating, and examples thereof include copper plating such as copper sulfate plating and copper pyrophosphate plating; solder plating such as high-throw solder plating; nickel plating such as Watts bath (nickel sulfate-nickel chloride) plating and nickel sulfamate plating; and gold plating such as hard gold plating and soft gold plating.

[0102] After the etching or plating process, the resist pattern on the substrate is removed. The resist pattern can be removed, for example, with an aqueous solution that is more strongly alkaline than the alkaline developer used in the development step. Examples of such strongly alkaline aqueous solutions include a 1 to 10% by mass aqueous solution of sodium hydroxide and a 1 to 10% by mass aqueous solution of potassium hydroxide. Of these, a 1 to 5% by mass aqueous solution of sodium hydroxide or potassium hydroxide may also be used.

[0103] Methods for removing the resist pattern include, for example, a dipping method and a spray method, which may be used alone or in combination.

[0104] When the resist pattern is removed after plating, the conductor layer covered with the resist is further etched by etching to form a conductor pattern, thereby manufacturing a desired wiring board. The etching method used in this process is appropriately selected depending on the conductor layer to be removed. For example, the above-mentioned etching solution can be used.

[0105] The method for manufacturing a wiring board according to this embodiment can be applied to the manufacture of not only single-layer wiring boards but also multi-layer wiring boards, and can also be applied to the manufacture of wiring boards having small-diameter through holes.

[0106] The method for manufacturing a wiring board according to this embodiment can be suitably used for manufacturing high-density packaging substrates, particularly for manufacturing wiring boards using a semi-additive process. An example of a manufacturing process for a wiring board using a semi-additive process is shown in FIG.

[0107] In (a) of FIG. 2, a substrate (circuit-forming substrate) is prepared in which a conductor layer 40 is formed on an insulating layer 50. The conductor layer 40 is, for example, a copper layer. In (b) of FIG. 2, the photosensitive layer forming step described above forms a photosensitive layer 30 and a support 20 on the conductor layer 40 of the substrate. In (c) of FIG. 2, the exposure step described above irradiates the photosensitive layer 30 with active light 80, which projects a photomask image onto the photosensitive layer 30 through the support 20, to form a photocured portion in the photosensitive layer 30. In (d) of FIG. 2, the development step removes from the substrate areas other than the photocured portion formed in the exposure step, thereby forming a resist pattern 32, which is a photocured portion, on the substrate.

[0108] 2(e), a plating layer 60 is formed on the conductor layer 40 of the substrate that is not covered with resist by a plating process using the resist pattern 32, which is the photocured portion, as a mask. The conductor layer 40 and the plating layer 60 may be made of the same material or different materials. When the conductor layer 40 and the plating layer 60 are made of the same material, the conductor layer 40 and the plating layer 60 may be integrated.

[0109] In FIG. 2( f ), the photocured resist pattern 32 is peeled and removed using a strong alkaline aqueous solution. The strong alkaline developer may be, for example, a 1 to 10% by weight sodium hydroxide aqueous solution or a 1 to 10% by weight potassium hydroxide aqueous solution. Next, a flash etching process is performed to remove the conductor layer 40 masked by the resist pattern 32, forming a conductor pattern 70 including the etched plating layer 62 and the etched conductor layer 42. The etching solution is appropriately selected depending on the type of conductor layer 40, and may be, for example, a cupric chloride solution, a ferric chloride solution, an alkaline etching solution, a hydrogen peroxide etching solution, or the like. While FIG. 2 illustrates a projection exposure method, the resist pattern 32 may also be formed using a combination of a mask exposure method and an LDI exposure method. By using the photosensitive element according to this embodiment, a wiring board having a fine conductor pattern can be produced.

[0110] Although the preferred embodiments of the present disclosure have been described above, the present disclosure is not limited to the above-described embodiments.

[0111] The present disclosure will be explained in more detail below using examples, but the present disclosure is not limited to these examples.

[0112] <Synthesis of Component (A)> 27 parts by mass of methacrylic acid, 50 parts by mass of styrene, 3 parts by mass of 2-hydroxyethyl methacrylate, and 20 parts by mass of benzyl methacrylate were mixed with 0.9 parts by mass of azobisisobutyronitrile to prepare solution (a). 0.5 parts by mass of azobisisobutyronitrile was dissolved in 50 parts by mass of a mixed solution (x) consisting of 30 parts by mass of 1-methoxy-2-propanol and 20 parts by mass of toluene to prepare solution (b). 500 g of mixed solution (x) was placed in a flask equipped with a stirrer, reflux condenser, thermometer, dropping funnel, and nitrogen gas inlet tube, and the mixture was stirred while blowing nitrogen gas into the flask and heated to 80°C. Solution (a) was added dropwise to the mixed solution in the flask at a constant dropping rate over 4 hours, followed by stirring at 80°C for 2 hours. Next, the solution (b) was added dropwise to the solution in the flask at a constant rate over 10 minutes, and the solution in the flask was stirred at 80°C for 3 hours. The solution in the flask was then heated to 90°C over 30 minutes and maintained at 90°C for 2 hours. The stirring was then stopped and the solution was cooled to room temperature (25°C), yielding a solution of binder polymer A1. The non-volatile content (solid content) of the binder polymer A1 solution was 49.8% by mass. The weight-average molecular weight of binder polymer A1 was 35,000.

[0113] The weight average molecular weight was measured by gel permeation chromatography (GPC) and calculated by conversion using a calibration curve of standard polystyrene. The GPC conditions are as follows. (GPC conditions) Pump: Hitachi L-6000 type (trade name, manufactured by Hitachi, Ltd.) Column: a total of three columns: Gelpack GL-R420, Gelpack GL-R430, and Gelpack GL-R440 (all manufactured by Resonac Corporation, trade names) Eluent: tetrahydrofuran Measurement temperature: 40°C Flow rate: 2.05 mL / min Detector: Hitachi L-3300 type RI (trade name, manufactured by Hitachi, Ltd.)

[0114] <Preparation of Photosensitive Resin Compositions> Each photosensitive resin composition was prepared by mixing the components shown in Tables 1 and 2 in the amounts (parts by mass) shown in the tables. The amounts (parts by mass) of components other than the solvent shown in Tables 1 and 2 are the mass of non-volatile components (solid content). Details of each component shown in Tables 1 and 2 are as follows.

[0115] (Binder polymer) A1: Binder polymer A1 synthesized above (Photopolymerizable compound) FA-321M(70): 70% propylene glycol monomethyl ether solution of 2,2-bis(4-(methacryloxyethoxy)phenyl)propane (ethylene oxide adduct of an average of 10 mol) (manufactured by Resonac Corporation) FA-024M: (PO)(EO)(PO) modified dimethacrylate (manufactured by Resonac Corporation, ethylene oxide adduct of an average of 6 mol and propylene oxide adduct of an average of 12 mol (total value)) BP-2EM: 2,2-bis(4-(methacryloxypolyethoxy)phenyl)propane (manufactured by Kyoeisha Chemical Co., Ltd., EO groups: 5.2 (total value)) (Photopolymerization initiator) B-CIM: 2,2'-bis(o-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole (manufactured by Hampford Chemical Industry Co., Ltd.) TR-HABI-102: 2,2',4-tris-(o-chlorophenyl)-5-(3,4-dimethoxyphenyl)-4',5'-diphenylbiimidazole (trade name, manufactured by Changzhou Strong Electronic New Materials Co., Ltd.) OXE-01: 1,2-octanedione-1-[4-(phenylthio)phenyl]-2-(o-benzoyloxime) (trade name: IRGACURE OXE-01, manufactured by BASF Japan Ltd.) (photosensitizer) DBA: 9,10-dibutoxyanthracene (manufactured by Kawasaki Chemical Industries, Ltd.) (polymerization inhibitor) TBC: 4-t-butylcatechol (manufactured by DIC Corporation, trade name "DIC-TBC") (dye) LCV: Leuco Crystal Violet (manufactured by Yamada Chemical Co., Ltd.) MKG: Malachite Green (manufactured by Osaka Organic Chemical Industry Ltd.) (solvent) Cyclopentanone (HSP value: 7.3) Cyclohexanone (HSP value: 5.2) Anisole (HSP value: 6.7) Toluene (HSP value: 5.6) MEK: Methyl ethyl ketone (HSP value: 7.9) MFG: 1-methoxy-2-propanol (HSP value: 12.6) PGMEA: Propylene glycol 1-monomethyl ether 2-acetate (HSP value: 11.2) Mesitylene (HSP value: 6.3) Acetone (HSP value: 10.2) Methanol (HSP value: 23.7)

[0116] The HSP value (Hansen solubility parameter) referred to here is the HSP value (δD 1 , δP 1 , δH 1 ) and the HSP value of the solvent (δD 2 , δP 2 , δH 2 ) and was calculated using the following formula: where δD represents the energy derived from intermolecular dispersion forces, δP represents the energy derived from intermolecular polar forces, and δH represents the energy derived from intermolecular hydrogen bonding forces.

[0117]

[0118] <Evaluation of Photosensitive Resin Compositions> (Discoloration Resistance) The photosensitive resin compositions of Examples 1 to 9 and Comparative Examples 1 to 5 were each transferred to a plastic bottle, and the sealed plastic bottle was then stored for 7 days in a completely light-shielded state under storage conditions of a temperature of 20°C and a humidity of 60% RH. The color change of the photosensitive resin composition after storage for 7 days was visually observed, and the discoloration resistance was evaluated according to the following criteria. A: No discoloration was observed even after storage for 7 days. B: Slight discoloration was observed after storage for 7 days. C: Significant discoloration was observed after storage for 7 days.

[0119]

[0120]

[0121] DESCRIPTION OF SYMBOLS 1... photosensitive element, 2, 20... support, 3, 30... photosensitive layer, 4... protective layer, 32... resist pattern, 40... conductor layer, 42... conductor layer after etching treatment, 50... insulating layer, 60... plating layer, 62... plating layer after etching treatment, 70... conductor pattern, 80... actinic light.

Claims

1. A photosensitive resin composition comprising a binder polymer, a photopolymerizable compound, a photopolymerization initiator, and a solvent, the solvent including at least one selected from the group consisting of ketone-based solvents having an alicyclic skeleton and aromatic ether-based solvents.

2. The photosensitive resin composition according to claim 1, wherein the ketone solvent having an alicyclic skeleton includes at least one selected from the group consisting of cyclopentanone and cyclohexanone.

3. The photosensitive resin composition according to claim 1, wherein the aromatic ether solvent comprises anisole.

4. The photosensitive resin composition according to claim 1, wherein the solvent does not contain toluene.

5. A photosensitive element comprising: a support; and a photosensitive layer formed on the support using the photosensitive resin composition according to any one of claims 1 to 4.

6. A method for forming a resist pattern, comprising the steps of: forming a photosensitive layer on a substrate using the photosensitive resin composition according to any one of claims 1 to 4; photocuring a portion of the photosensitive layer; and removing an uncured portion of the photosensitive layer by development.

7. The method for forming a resist pattern according to claim 6, wherein an inorganic alkaline developer is used in the development.

8. A method for forming a resist pattern, comprising the steps of: forming a photosensitive layer on a substrate using the photosensitive element according to claim 5; photocuring a portion of the photosensitive layer; and removing an uncured portion of the photosensitive layer by development.

9. The method for forming a resist pattern according to claim 8, wherein an inorganic alkaline developer is used in the development.

10. A method for manufacturing a wiring board, comprising the step of etching or plating a substrate on which a resist pattern has been formed by the method for forming a resist pattern according to claim 6, to form a conductor pattern.

11. A method for manufacturing a wiring board, comprising the step of etching or plating a substrate on which a resist pattern has been formed by the method for forming a resist pattern according to claim 8, to form a conductor pattern.