Production method of electric resistance welded steel pipe and electric resistance welded steel pipe
Patent Information
- Application Number
- MYPI2025004268
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-16
- Filing Date
- 2023-10-05
- Publication Date
- 2024-09-16
AI Technical Summary
The corrosion resistance of electric resistance welded (ERW) steel pipes made from plated steel sheets deteriorates around the welds due to evaporation of plating during welding and removal of beads, which compromises the integrity of the corrosion protection.
The method involves forming inclined end faces on plated steel sheets, which are then welded to form a pipe, with the ratio of the weld bead width to the plate thickness set at 92% or less, and applying additional plating to the welded area to minimize bead removal and enhance corrosion resistance.
This approach narrows the bead width and reduces the area where corrosion resistance is compromised, thereby improving the corrosion resistance around the welded portion of ERW steel pipes.
Smart Images

Figure PI2025004268_DRAWING_001 
Figure PI2025004268_DRAWING_002 
Figure PI2025004268_DRAWING_003
Abstract
Description
Electric-resistance welded steel pipe manufacturing method and electric-resistance welded steel pipe
[0001] The present invention relates to a method for manufacturing an electric resistance welded steel pipe and an electric resistance welded steel pipe.
[0002] Plated steel sheets exhibit high corrosion resistance on the surface where the plating is coated due to the anticorrosive properties of the plating. However, when plated steel sheets are welded, the temperature near the weld becomes locally high, causing the plating components to evaporate and reducing corrosion resistance. Furthermore, when the bead created by welding, as in the case of electric resistance welded steel pipes, is removed, some of the plating in the vicinity of the bead is also removed, leaving the iron base metal exposed around the weld, which can further expand the area where corrosion resistance is reduced.
[0003] For this reason, in the manufacture of electric resistance welded steel pipes using galvanized steel sheets as base metal, the decrease in corrosion resistance around the welds is generally compensated for by performing post-repair work, such as spraying the area around the weld with the main component of the plating (e.g., Zn). However, the corrosion resistance around the repaired welds is not necessarily restored to the same level as that of other areas. Due to this decrease in corrosion resistance around the welds, in fields requiring high corrosion resistance, post-plated products that are immersed in hot dip galvanizing after processing are used, rather than pre-plated products manufactured by processing galvanized steel sheets. Under these circumstances, in order to increase productivity, there is a demand for improving the corrosion resistance around the welds of electric resistance welded steel pipes using galvanized steel sheets as base metal.
[0004] As a conventional technique for manufacturing electric resistance welded steel pipes, for example, Patent Document 1 discloses a technique in which a tapered shape is imparted to the ends of a strip material, with inclined surfaces connecting from the vertical end face of the strip material to both end faces on the outer diameter side and the inner diameter side in the thickness direction of the strip material, and then electric resistance welding is performed with the butt angle of the vertical end faces of the strip material being within a range of ±1 degree. Also, Patent Document 2 discloses a technique in which a steel strip is formed into a generally tubular shape, and both the outer and inner surfaces of both edges of an open pipe are tapered so that the angle between the inclined surfaces and the vertical end faces of the steel strip is 15 to 50 degrees, and the length of the inclined surfaces in the thickness direction from the steel strip surface is 10 to 45% of the steel strip thickness, and then electric resistance welding is performed with an upset amount of 40 to 75% of the steel strip thickness.
[0005] Furthermore, as a technique for manufacturing a welded pipe by butt-welding both widthwise ends of a plated steel strip, Patent Document 3, for example, discloses a method of butt-welding after grinding off the plated layer at both widthwise ends that will become the weld. By removing the plated layer, which has an adverse effect on the welding conditions and the structure of the weld, a weld having properties substantially similar to those of the base material can be obtained.
[0006] Japanese Patent Application Laid-Open No. 2009-45643 Japanese Patent Application Laid-Open No. 2013-139051 Japanese Patent Application Laid-Open No. 4-197516 International Publication No. 2020 / 183883
[0007] The techniques described in Patent Documents 1 and 2 are intended for electric resistance welded steel pipes used as oil country tubular goods or line pipes, which require stricter corrosion resistance, and do not anticipate the production of electric resistance welded steel pipes using coated steel sheets as the base sheet. Furthermore, the technique described in Patent Document 3 removes the coating layer from both widthwise ends that become welded parts, which raises concerns about a decrease in corrosion resistance around the welded parts.
[0008] Therefore, the present invention has been made in consideration of the above problems, and an object of the present invention is to provide a method for manufacturing an electric-resistance welded steel pipe and an electric-resistance welded steel pipe that can suppress a decrease in corrosion resistance around the weld in an electric-resistance welded steel pipe made from a plated steel sheet.
[0009] In order to solve the above-mentioned problems, according to one aspect of the present invention, there is provided a method for manufacturing an electric-resistance welded steel pipe, comprising: an end face shaping process in which an outer inclined portion that slopes in the plate thickness direction from the outer surface side toward the inner surface side is formed on each of a first end face and a second end face on both sides of the width direction of a plated steel sheet, or an outer inclined portion and an inner inclined portion that slopes in the plate thickness direction from the inner surface side toward the outer surface side, so that the first end face and the second end face have a shape in which the plate thickness decreases from the center in the width direction toward the end face; and a pipe-making process in which the shaped first end face and the second end face are butt-welded together to form a pipe.
[0010] In the end face forming step, at least a portion of the outer inclined portion may be coated with plating that continues from the outer surface side.
[0011] In the pipe-making process, the first end face and the second end face may be heated and melted, and the first end face and the second end face may be pressed together so that the ratio of the width of the weld bead on the outer surface side to the thickness of the plated steel sheet is 92% or less.
[0012] In addition, in the pipe-making process, plating may be applied to the welded portion where the first end face and the second end face are pressed together and joined.
[0013] In the end face forming process, after forming the first end face and the second end face, the plated steel sheet is wound into a coil, and in the pipe making process, the plated steel sheet wound into a coil in the end face forming process may be discharged to make a pipe.
[0014] In addition, in order to solve the above-mentioned problems, according to another aspect of the present invention, there is provided an electric-resistance welded steel pipe whose base sheet is a plated steel sheet, which has a welded portion extending in the axial direction and heat-affected zones extending in the axial direction on both circumferential sides of the welded portion, wherein the ratio of the outer surface circumferential length of the welded portion to the plate thickness of the plated steel sheet is 48% or more, and for each heat-affected zone, the ratio of the outer surface circumferential length of the heat-affected zone to the plate thickness of the plated steel sheet is 40% or less.
[0015] Furthermore, in order to solve the above-mentioned problems, according to another aspect of the present invention, there is provided an electric-resistance welded steel pipe using a plated steel sheet as a base sheet, which has a post-plated portion on its outer surface where plating is applied at least along a weld extending in the axial direction, and the ratio of the outer surface circumferential length of the post-plated portion to the plated steel sheet thickness is 172% or less.
[0016] As described above, according to the present invention, it is possible to suppress a decrease in corrosion resistance around the welded portion of an electric resistance welded steel pipe made from a plated steel sheet.
[0017] 5 is an explanatory diagram showing an example of a welding process in which both widthwise ends of a steel sheet formed into a cylindrical shape are welded in the production of an electric resistance welded steel pipe. FIG. 6 is a diagram schematically showing the shapes before and after welding, as viewed in the axial direction, of the periphery of a welded portion of an electric resistance welded steel pipe using a plated steel sheet as the base sheet. FIG. 7 is an explanatory diagram showing an example of a technique for forming a first end face and a second end face of a plated steel sheet into a shape having an outer inclined portion and an inner inclined portion, respectively, in the end face shaping process. FIG. 8 is a schematic side view of a cross section of a cut end face of a plated steel sheet cut by the technique of FIG. 3. FIG. 9 is an explanatory diagram showing an example of a technique for forming a first end face and a second end face of a plated steel sheet into a shape having an outer inclined portion, respectively, in the end face shaping process. FIG. 10 is a schematic side view of a cross section of a cut end face of a plated steel sheet cut by the technique of FIG. 5. FIG. 11 is an explanatory diagram schematically showing the shapes before and after welding, as viewed in the axial direction, of the periphery of a welded portion of a plated steel sheet in a pipe making process. FIG. 12 is an explanatory diagram showing the definitions of a weld width, a heat-affected zone width, and a bead width. FIG. 13 is a schematic explanatory diagram showing an electric resistance welded steel pipe according to the present embodiment. 1 is a simulation result showing an example of the relationship between the pressing force and bead width during welding for a steel pipe having an outer diameter of 114.3 mm; 2 is a simulation result showing an example of the relationship between the pressing force and bead width during welding for a steel pipe having an outer diameter of 139.8 mm; 3 is a simulation result showing an example of the relationship between the pressing force and bead width during welding for a steel pipe having an outer diameter of 159.8 mm; and 4 is a simulation result showing a state when removal of the outer surface bead is not necessary.
[0018] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. In this specification and drawings, components having substantially the same functional configurations are designated by the same reference numerals, and redundant explanations will be omitted.
[0019] [1. Consideration of Corrosion Resistance Around Welded Zones] Figure 1 is an explanatory diagram showing an example of a welding process for welding both widthwise ends of a cylindrically formed steel plate 3, which is commonly performed in the manufacture of electric resistance welded steel pipes. Electric resistance welded steel pipes are manufactured, for example, as shown in Figure 1 , by passing a cylindrically formed steel plate through a coil 15 through which a high-frequency current 10 flows, heating both widthwise ends 3a, 3b by induction heating, and then welding the molten widthwise ends 3a, 3b by applying pressure with squeeze rolls 20. Furthermore, molten steel is extruded by the pressure applied by the squeeze rolls 20 to form beads on the outer and inner surfaces of a weld 3c joining both widthwise ends 3a, 3b. The beads formed on the outer surfaces are removed, for example, by a tool tool 30.
[0020] In electric resistance welded steel pipes made from galvanized steel sheets, corrosion resistance decreases around welds. As a result of extensive research into the causes of this, the present inventors have found that electric resistance welded steel pipes made from galvanized steel sheets have reduced corrosion resistance around welds due to the following factors:
[0021] First, in electric resistance welded steel pipes, the heat generated during welding locally raises the temperature near both end faces of the plated steel sheet, causing the plating in those areas to evaporate. As a result, in the final product, the amount of plating remaining around the weld is less than in other areas, or even none at all around the weld, resulting in reduced corrosion resistance only around the weld.
[0022] In addition, the beads on the outer surface of steel pipes are removed by cutting with a cutting tool or crushing with a roll, etc. During this process, the plating in the vicinity of the beads is partially removed along with the beads, leaving the bare iron exposed around the weld, which can expand the area where corrosion resistance is reduced. After removing the beads, the reduced corrosion resistance around the weld can be compensated for by performing post-repair work such as thermal spraying the main plating component around the weld, but this does not necessarily restore the corrosion resistance around the repaired weld to the same level as the rest of the area.
[0023] In light of these factors, the present inventors considered that narrowing the bead removal width would reduce the area where bare iron is exposed around the weld and prevent a decrease in corrosion resistance around the weld. They then came up with the idea that optimizing the shape of both widthwise end faces of the plated steel sheet would narrow the bead, thereby narrowing the bead removal width. Specifically, by chamfering the corners between the surface and the end face on only the outer surface side or on both the outer surface side and the inner surface side of each of the first end face and the second end face on both widthwise sides of the plated steel sheet, the bead generated by welding the first end face and the second end face is narrowed.
[0024] FIG. 2 is a schematic diagram showing the pre- and post-welding shapes of the vicinity of a welded portion of an electric resistance welded steel pipe made from a galvanized steel sheet, as viewed in the axial direction. The pre-welding shape shows a state in which a cylindrically formed galvanized steel sheet 5 is heated at both ends in the width direction, a first end face 51 and a second end face 52. The heated portions of the galvanized steel sheet 5 are, from the side nearest the first end face 51 and the second end face 52, a welded portion Q1 and a heat-affected portion Q2. Here, it is assumed that the circumferential widths of the welded portion Q1 and the heat-affected portion Q2 are approximately the same as the plate thickness. The post-welding shape shows a state in which the first end face 51 and the second end face 52 of the galvanized steel sheet 5 are butt-welded together, resulting in an outer bead 53 on the outer surface 5o and an inner bead 54 on the inner surface 5i. Note that FIG. 2 exaggerates the shape of the vicinity of the welded portion for clarity.
[0025] 2 , the first end face 51 and the second end face 52 of the plated steel sheet 5 substantially maintain the sheet shape before being formed into a cylindrical shape and are substantially perpendicular to the outer surface 5o and the inner surface 5i. When the first end face 51 and the second end face 52 of the plated steel sheet 5 are butt-welded together, the base metal of the welded portion Q1 is pushed out toward the outer surface 5o and the inner surface 5i, forming an outer bead 53 and an inner bead 54.
[0026] The end face shape A and the end face shape B in FIG. 2 are examples of the shapes of the first end face 51 and the second end face 52 according to one embodiment of the present invention.
[0027] The end face shape A has chamfered corners on the outer surface 5o and inner surface 5i sides. As shown in FIG. 2 , the end face shape A includes an outer inclined portion 5s that slopes in the thickness direction from the outer surface 5o toward the inner surface 5i and an inner inclined portion 5t that slopes in the thickness direction from the inner surface 5i toward the outer surface 5o, resulting in a shape in which the thickness decreases toward the end face. When the first end face 51 and the second end face 52 have the end face shape A, the amount of base metal in the welded portion Q1 is smaller than in the conventional example by the amount of the corners on the outer surface 5o and inner surface 5i sides. Therefore, when the first end face 51 and the second end face 52 having the end face shape A are butt-welded together, both the outer surface bead 53 and the inner surface bead 54 are smaller than in the comparative example.
[0028] The end face shape B has a chamfered corner on the outer surface 5o side. As shown in FIG. 2 , the end face shape B includes an outer inclined portion 5s that slopes in the thickness direction from the outer surface 5o side toward the inner surface 5i side, resulting in a shape in which the thickness decreases toward the end face. In the example of the end face shape B shown in FIG. 2 , a surface 5r that is approximately perpendicular to the inner surface 5i exists on the inner surface 5i side. However, the end face shape B may have only the outer inclined portion 5s. When the first end face 51 and the second end face 52 have the end face shape B, the amount of base metal in the welded portion Q1 is smaller than in the conventional example by the amount of the corner on the outer surface 5o side. Therefore, when the first end face 51 and the second end face 52 having the end face shape B are butt-welded together, the outer surface bead 53 is smaller than in the comparative example.
[0029] By forming the first end face 51 and the second end face 52 into the end face shape A or the end face shape B, the bead formed after welding can be narrowed, and as a result, the width of the bead to be removed can be narrowed. This narrows the repair width by spraying the main plating component to compensate for the decrease in corrosion resistance, improving the corrosion resistance around the weld.
[0030] In the end face shape B, the inner bead 54 is expected to be approximately the same size as in the conventional example, but the inner bead 54, which is not visible from the outside, may not be removed. For example, in components used in a state where the inner surface is not exposed to the outside, such as guardrail support pipes and guard pipes, the presence of an inner bead does not pose a problem. For this reason, the present invention does not consider the presence or absence of the inner bead 54 to be important, and aims to narrow the outer bead 53.
[0031] [2. Manufacturing Method of Electric-Resistance Welded Steel Pipe Using Coated Steel Sheet as Base Sheet] Hereinafter, a manufacturing method of an electric-resistance welded steel pipe using a coated steel sheet as base sheet according to one embodiment of the present invention will be described. The manufacturing method of an electric-resistance welded steel pipe according to this embodiment includes an end face shaping step of shaping both end faces (first end face and second end face) in the width direction of the coated steel sheet as base sheet, and a pipe making step of butt-welding the formed first end face and second end face together to form a pipe. In the following description, it is assumed that the coated steel sheet as base sheet is a coated steel sheet containing Zn as its main component.
[0032] (End Face Shaping Process) In the end face shaping process, the first end face and the second end face of the plated steel sheet, which is the original sheet, are each shaped into a shape in which the corners between the surface and the end face are chamfered only on the outer surface side or on both the outer surface side and the inner surface side. Specifically, the first end face and the second end face are shaped into a shape having an outer inclined portion 5s, or an outer inclined portion 5s and an inner inclined portion 5t, as shown in end face shape A or end face shape B in FIG. 2 . In this process, the plate thickness is reduced from the center in the width direction of the plated steel sheet toward the end face (first end face or second end face). The outer inclined portion 5s and the inner inclined portion 5t may be flat, as shown in FIG. 2 , or may be curved.
[0033] Although the method for shaping the end face is not particularly limited, it is desirable that the plating on the surface of the plated steel sheet, which is the original sheet, covers the end face after shaping as much as possible. By covering the end face with plating, it is possible to minimize the repair width in which the main plating component is sprayed after welding the first end face and the second end face.
[0034] For example, to form the first end face and the second end face of the plated steel sheet into a shape having an outer inclined portion and an inner inclined portion, respectively, as in the end face shape A shown in Fig. 2, a cutting device having a pair of annular blades 41, 42 with V-shaped cutting edges 41a, 42a as shown in Fig. 3 may be used (see, for example, Patent Document 4). 1 , θ 2 is set to 10° to 120°, and the tip radius R 1 , R 2 The plated steel sheet 5 is passed between the rotating annular blades 41, 42 with a cutting edge of 0.5% to 35.0% of the sheet thickness, and the end portion is cut off. As a result, a tensile force is generated between the cutting edges 41 a, 42 a of the pair of annular blades 41, 42 and the plated steel sheet 5, causing the plating on the surface of the plated steel sheet 5 to penetrate into the cut end surface, and the cut end surface is covered with plating.
[0035] FIG. 4 shows an example of a cut end surface of a plated steel sheet 5 cut by a cutting device having a pair of annular blade portions 41, 42 shown in FIG. 3 . FIG. 4 is a schematic side view of a cross section of the cut end surface of a plated steel sheet 5 in which both surfaces of a base material 5a are coated with a plating 5b. As shown in FIG. 4 , the cut end surface of the plated steel sheet 5 comprises a sag, an inclined surface, and a fracture surface. The upper sag and inclined surface of FIG. 4 are formed by the cutting edge 41a of the annular blade portion 41 in FIG. 3 , and the lower sag and inclined surface of FIG. 4 are formed by the cutting edge 42a of the annular blade portion 42 in FIG. 3 . The inclined surface is covered with the plating 5b that continues from the surface of the plated steel sheet 5. The fracture surface is caused by fracture that originates from cracks generated in the plated steel sheet 5 by the cutting edges 41a, 42a.
[0036] For example, the upper inclined surface in Fig. 4 becomes the outer inclined portion 5s after end face shaping, and the lower inclined surface in Fig. 4 becomes the inner inclined portion 5t after end face shaping. In this way, by cutting both widthwise sides of the plated steel sheet 5 using the cutting device having a pair of annular blades 41, 42 with V-shaped cutting edges 41 a, 42 a shown in Fig. 3, it is possible to form the outer inclined portion 5s and the inner inclined portion 5t covered with the plating 5b on the first end face and the second end face, respectively.
[0037] Furthermore, to form the first and second end faces of the plated steel sheet into a shape with an outwardly inclined portion, as shown in end face shape B in FIG. 2 , a cutting device having a pair of slit blades 61, 62, each of which has a slanted portion P1 and a protruding portion P2, as shown in FIG. 5 , may be used. The slanted portion P1 of the blades 61a, 62a is inclined relative to the pushing direction of the plated steel sheet 5, and the protruding portion P2 protrudes from the slanted portion P1 in the pushing direction. The plated steel sheet 5 is passed between the rotating slit blades 61, 62 to cut its end. This causes the slanted portions P1 of the blades 61a, 62a to compress the plating of the plating layer 5b, including the base material 5a, in the pushing direction (sheet thickness direction) and wrap around the cut end faces. Furthermore, the application of compressive stress delays the cutting timing, allowing the inclined surfaces to be coated with plating. Furthermore, by completely cutting the plated steel sheet 5 with the protruding portions P2 of the blades 61a, 62a, the generation of large burrs can be suppressed.
[0038] FIG. 6 shows an example of a cut end surface of a plated steel sheet 5 cut by a cutting device having a pair of slit blades 61, 62 shown in FIG. 5 . FIG. 6 is a schematic side view of a cross section of the cut end surface of a plated steel sheet 5 in which both surfaces of a base material 5a are coated with a plating 5b. Note that FIG. 6 shows the cut end surface on the side where the surface (top surface) opposite the inclined portion P1 of the slit blade 61 in FIG. 5 is pressed in by the inclined portion P1. As shown in FIG. 6 , the cut end surface of the plated steel sheet 5 has, in order from the top surface, an inclined surface, a shear surface, and a fracture surface. The inclined surface is a surface formed along the inclined portion P1 of the blade portion 61a of the slit blade 61 and is inclined relative to the sheet thickness direction. The shear surface is a smooth surface formed by the movement of the slit blade 61 that has been embedded in the plated steel sheet 5, and is slightly formed. The fracture surface is a surface where the plated steel sheet 5 fractures due to a crack that has occurred in the plated steel sheet 5.
[0039] For example, the inclined surfaces in Fig. 6 become the outer inclined portions 5s after the end face shaping. In this manner, by cutting both sides in the width direction of the plated steel sheet 5 using the cutting device having the pair of slit blades 61, 62 shown in Fig. 5, it is possible to form the outer inclined portions 5s covered with the plating 5b on each of the first end face and the second end face.
[0040] In this way, in the end face forming process, each of the first end face 51 and the second end face 52 of the plated steel sheet 5 is formed into a shape having an outer inclined portion 5s and an inner inclined portion 5t as shown in Figure 4, or a shape having an outer inclined portion 5s as shown in Figure 6.
[0041] Although the outer inclined portion 5s and the inner inclined portion 5t do not necessarily need to be coated with a plating, it is preferable to coat at least a portion of the outer inclined portion 5s with a plating 5b that extends continuously from the outer surface. As described below, when the first end face 51 and the second end face 52 are heated before welding in the pipe-making process, low-melting-point components such as Zn in the plating 5b at the welded portion where the base metal 5a is semi-molten evaporate, but the plating 5b remains molten in the heat-affected zone and solidifies after cooling to coat the base metal 5a. In the end face forming process, coating at least a portion of the outer inclined portion 5s of the first end face 51 and the second end face 52 with a plating 5b that extends continuously from the outer surface can reduce the area where the base metal 5a is exposed to the outside and thus reduces corrosion resistance.
[0042] (Pipe-making process) Next, the first end face 51 and the second end face 52 formed in the end face forming process are butt-welded to form a pipe. The pipe-making process can be performed using, for example, the equipment shown in FIG. 1 . First, the first end face 51 and the second end face 52 are heated and melted. Then, the first end face 51 and the second end face 52 are pressed together to weld them. At this time, the ratio of the width of the weld bead (outer surface bead 53) on the outer surface 5o side to the thickness of the plated steel sheet 5 (hereinafter also referred to as "bead width") is set to 92% or less. The bead width is the portion that needs to be cut after welding and is the circumferential width of the portion that is exposed to the outside from the outer surface 5o of the steel pipe.
[0043] 7 is a schematic diagram showing the shapes of the periphery of the welded portion of the plated steel sheet 5 in the pipe-making process before and after welding as viewed in the axial direction. As an example, FIG. 7 shows a case where the first end face 51 and the second end face 52 have the end face shape A shown in FIG. 2.
[0044] When the first end face 51 and the second end face 52 of a cylindrically formed plated steel sheet 5 are heated, the heated portions of the plated steel sheet 5 are, from the side closest to the first end face 51 and the second end face 52, a welded portion Q1 and a heat-affected portion Q2. The welded portion Q1 is a portion where the base material iron is softened and semi-molten. Because the base material reaches a high temperature of 900°C or higher in the welded portion Q1, low-melting-point components such as Zn among the plating components that cover the surface of the plated steel sheet 5 evaporate. The heat-affected portion Q2 is a portion where the base material iron reaches a high temperature and the plating that covers the surface of the plated steel sheet 5 melts. That is, in the heat-affected portion Q2, the base material is at a temperature of 400°C to 900°C, and some or all of the plating components are melted in part or all of the region. In addition, the portion farther from the end (first end face 51 or second end face 52) than the heat-affected zone Q2 maintains the original plated steel sheet 5, and the outer surface 5o and inner surface 5i are coated with plating.
[0045] In the pipe-making process, the weld Q1 on the first end face 51 and the weld Q1 on the second end face 52 are pressed together to join the first end face 51 and the second end face 52. As the weld Q1 is pressed together, the triangular first end face 51 and the second end face 52, each consisting of an outer inclined portion 5s and an inner inclined portion 5t, are deformed and disappear, and the plated steel sheet 5 becomes tubular (post-welding 1). At this time, molten metal is expelled from the outer surface 5o and the inner surface 5i, forming outer beads 53 and inner beads 54. As the weld Q1 is further pressed together, more metal is expelled from the outer surface 5o and the inner surface 5i, reducing the circumferential width of the joined weld Q1 but increasing the size of the outer beads 53 and inner beads 54 (post-welding 2).
[0046] Of the weld beads created by welding, at least the outer surface bead 53 visible from the outside is removed. In the manufacturing method for electric resistance welded steel pipe according to this embodiment, the bead created after welding is narrowed, and the width of the removed bead is narrowed, thereby narrowing the repair width by spraying the main plating component and improving the corrosion resistance around the weld. To achieve this, the ratio of the bead width of the outer surface bead 53 to the plate thickness of the plated steel sheet 5 is set to 92% or less.
[0047] Here, the width W1 of the weld Q1 (weld width), the width W2 of the heat-affected zone Q2 (heat-affected zone width), and the bead width Wb of the outer surface bead 53 are defined as shown in Figure 8. The weld width W1 is the circumferential length of the weld Q1 on the outer surface 5o. The heat-affected zone width W2 is the circumferential length of the heat-affected zone Q2 on the outer surface 5o. The bead width Wb of the outer surface bead 53 is the circumferential length of the outer surface bead 53 on the outer surface 5o. Note that Figure 8 shows the periphery of the weld on one end face side. In other words, the weld width W1, heat-affected zone width W2, and bead width Wb of the entire steel pipe are twice as large as those in Figure 8.
[0048] Regardless of the shapes of the first end face 51 and the second end face 52 of the plated steel sheet 5, the areas that become the welded zone Q1 and the heat-affected zone Q2 when heated in the pipe-making process are substantially the same. However, if the welded zone Q1 is pressed with the same pressing force during welding, and the end face shape is shaped and chamfered as in end face shape A or end face shape B in Figure 2, the pressing force becomes larger compared to the conventional example because the amount of base metal at the end is less.
[0049] Here, as the pressing force increases, the amount of bare metal of the welded portion Q1 that is expelled from the outer surface 5o of the steel pipe increases, and the bead width Wb of the outer bead 53 increases. However, when the first end face 51 and the second end face 52 are chamfered, the amount of bare metal at the end is less than in the conventional example, so even if the pressing force increases, the amount of bare metal of the welded portion Q1 that is expelled from the outer surface 5o of the steel pipe is also less than in the conventional example. Therefore, by chamfering the first end face 51 and the second end face 52, the bead width Wb of the outer bead 53 can be reduced while increasing the pressing force. By adjusting the pressing force during welding so that the ratio of the bead width Wb to the plate thickness t of the plated steel sheet 5 is 92% or less, the outer bead 53 can be narrowed compared to the conventional example shown in Figure 2.
[0050] Furthermore, by joining the first end face 51 and the second end face 52, a portion of the weld Q1, where low-melting-point components such as Zn among the surface plating components have evaporated, becomes a weld bead (outer surface bead 53 or inner surface bead 54) and is expelled to the outside of the steel pipe. By increasing the pressing amount between the first end face 51 and the second end face 52, it is possible to reduce the amount of the weld Q1 that remains in the final product and causes a decrease in corrosion resistance.
[0051] Furthermore, in the pipe-making process, after the first end face 51 and the second end face 52 are pressed together and joined, a plating may be applied to the welded portion Q1. If no outer bead 53 is formed during welding and the outer surface of the steel pipe is smooth, removing the outer bead 53 is not necessary. However, when the end faces (first end face 51 and second end face 52) of the welded portion Q1 are heated, low-melting-point components of the plating, such as Zn, evaporate. Furthermore, if an outer bead 53 is formed during welding, the outer bead 53 is removed. In the area where the welded portion Q1 or the outer bead 53 has been removed, the base metal is exposed and the plating has disappeared. Therefore, applying a plating to the welded portion Q1 or the area where the outer bead 53 has been removed by, for example, thermal spraying the main plating component, suppresses a decrease in corrosion resistance.
[0052] In this way, in the pipe-making process, the first end face 51 and the second end face 52 formed in the end face forming process are butt-welded to form a pipe. This makes it possible to increase the amount of pressure between the first end face 51 and the second end face 52 while narrowing the bead width of the outer surface bead 53 during welding. This makes it possible to suppress a decrease in corrosion resistance of the weld on the outer surface of the steel pipe after welding.
[0053] When the first end face 51 and the second end face 52 are heated before welding in the pipe-making process, low-melting-point components of the coating 5b, such as Zn, evaporate at the welded portion Q1 where the base metal 5a is semi-molten. Therefore, the base metal and the coating do not intermix at the welded portion Q1, and penetrators generated during electric resistance welding, as feared in Patent Documents 1 and 2, do not remain. Penetrators are often generated in special steels with high Mn and Si contents, but are unlikely to occur in steel sheets used as the base material for the plated steel sheet 5. Furthermore, when welding the plated steel sheet 5, the base metal is coated with a coating, which reduces the time the base metal is exposed to air during welding, thereby suppressing the generation of penetrators due to oxidation of Mn and Si. Therefore, penetrators are not a problem in the present invention.
[0054] The above describes a method for manufacturing an electric resistance welded steel pipe according to this embodiment. According to this embodiment, both end faces (first end face and second end face) in the width direction of a plated steel sheet, which is the base sheet, are chamfered and shaped, and then the shaped first end face and second end face are butt-welded to form a pipe. This narrows the bead formed after welding and reduces the width of the bead to be removed. As a result, the repair width over which the main plating component is sprayed is narrowed, and a decrease in corrosion resistance around the weld can be suppressed.
[0055] The end surface shaping process and the pipe-making process may be performed as a series of processes on the same production line, or may be performed on different production lines. For example, in the end surface shaping process, the first end surface 51 and the second end surface 52 of the original plated steel sheet 5 are shaped, and then the plated steel sheet 5 is wound into a coil. Then, in the pipe-making process, the plated steel sheet 5 wound into a coil in the end surface shaping process may be unwound and used to make a pipe.
[0056] 9 shows an example of an electric resistance welded steel pipe 50 manufactured by the above-described manufacturing method. FIG. 9 is a schematic diagram showing an electric resistance welded steel pipe 50 manufactured by the above-described manufacturing method. As shown in FIG. 9, the electric resistance welded steel pipe 50 has a welded portion Q1 extending in the axial direction (α direction) and a heat-affected portion Q2 extending in the axial direction on both sides of the welded portion Q1 in the circumferential direction (β direction). In such an electric resistance welded steel pipe 50, the circumferential length W of the outer surface 5o of the welded portion Q1 relative to the plate thickness t of the plated steel sheet is 1 The ratio (W 1 / t) is 48% or more. 2 The ratio (W 2 / t) is 40% or less (80% or less for the entire steel pipe).
[0057] The outer surface 5o of the electric resistance welded steel pipe 50 may have a post-plating portion where plating is applied at least along the welded portion Q1 extending in the (α direction). The post-plating portion is a portion where plating is applied by thermal spraying of the main plating component after the outer surface bead 53 is removed. The post-plating portion includes at least the outer surface bead 53 after welding, and may further include a part of the heat-affected zone Q2 adjacent to the welded portion Q1 including the outer surface bead 53 after welding. The circumferential length of the outer surface 5o of the post-plating portion is defined as W. 3 When this is the case, the length of the post-plating part W 3 is the length W of the weld Q1 1 The length W of the post-plating portion relative to the thickness t of the plated steel sheet is equal to or greater than the removed bead width Wb. 3 The ratio (W 3 / t) is 172% or less.
[0058] Such an electric resistance welded steel pipe 50 is prevented from decreasing in corrosion resistance around the welded portion Q1.
[0059] The relationship between the pressing force and the bead width was verified by simulation when the end face shapes of the steel plate were the conventional example shown in Figure 2, end face shape A, and end face shape B. In this verification, simulations were performed on steel pipes with three different outer diameters (114.3 mm, 139.8 mm, and 159.8 mm) and a plate thickness of 4.5 mm. For end face shape A, the inclination angles of the outer inclined portion and the inner inclined portion relative to the plate thickness direction were each 30°, resulting in a vertically symmetrical shape. For end face shape B, the inclination angle of the outer inclined portion relative to the plate thickness direction was 45°, and the ratio of the plate thickness of the outer inclined portion to the plate thickness of the portion approximately perpendicular to the inner surface was 7:3. The tensile strength of the steel plate was assumed to be 400 MPa.
[0060] In the simulation, from the side closest to the end face, a 900°C region simulating the weld, a 300°C region simulating the heat-affected zone, and a 0°C region simulating the part not affected by heating were set. The circumferential widths of the 900°C region and the 300°C region were assumed to be the same as the plate thickness.
[0061] Figures 10 to 12 show the simulation results. Figures 10 to 12 show three conditions for each end face shape: a pressing amount of -1 mm (before welding), a pressing amount of 5 mm (after welding), and a pressing amount of 9 mm (after welding). As shown in Figures 10 to 12, regardless of the steel pipe diameter, the bead width of the outer surface bead after welding for end face shape A and end face shape B was smaller than that of the conventional example. Furthermore, for end face shape B, a larger portion of the end face was chamfered compared to end face shape A, reducing the 900°C region on the outer surface. As a result, it can be seen that, when the pressing amount is the same, end face shape B can reduce the bead width of the outer surface bead and also reduce the 900°C region remaining on the steel pipe compared to end face shape A.
[0062] Table 1 below shows the bead width, weld width, and heat-affected zone width of the outer bead when the pressing amount is 9 mm. Table 2 below also shows the range of the ratio of the outer bead width, weld width, and heat-affected zone width to the plate thickness, calculated based on Table 1. Note that both Tables 1 and 2 are values for one end face, and the values for the entire steel pipe are doubled.
[0063]
[0064]
[0065] The bead width increases as the pressing amount increases. Therefore, the ratio of bead width to plate thickness shown in Table 2 is the maximum possible range. As can be seen from Table 2, the maximum ratio of bead width to plate thickness in the conventional example is 100 to 112% for the entire steel pipe. In contrast, when end face shape A and end face shape B are used, the maximum ratio of bead width to plate thickness is 58 to 92% for the entire steel pipe, which is smaller than the conventional example. In this way, by using end face shape A or end face shape B, the bead width of the outer surface bead can be reduced.
[0066] The weld width becomes smaller as the pressing amount increases. Therefore, the ratio of the weld width to the plate thickness shown in Table 2 is within the range of the minimum value that can be taken. From Table 2, it can be seen that the minimum value of the ratio of the weld width to the plate thickness in the conventional example is 76 to 80% for the entire steel pipe. In contrast, for end face shape A and end face shape B, the minimum value of the ratio of the weld width to the plate thickness is 48 to 80% for the entire steel pipe, which can be a smaller value than the conventional example.
[0067] The width of the heat-affected zone was the same as shown in Tables 1 and 2 above, since there was little change between the conventional example, end face shape A, and end face shape B. Tables 1 and 2 show the results when the pressing amount was 9 mm, and at least in the conventional example, the end was slightly overheated rather than sufficiently heated to avoid poor welding. In actual operation, the end must also be sufficiently heated to avoid poor welding, but it is expected that the width of the heat-affected zone will be the same as or smaller than the results of this verification to avoid overheating. Therefore, it can be considered that the ratio of the width of the heat-affected zone to the plate thickness will be 40% or less for each heat-affected zone (80% or less for the entire steel pipe).
[0068] In addition, if a post-plated portion is present, the ratio of the post-plated portion to the plate thickness can be considered to be 172% or less for the entire steel pipe. The post-plated portion includes at least the outer surface bead after welding and may further include a part of the heat-affected zone adjacent to the weld including the outer surface bead. Therefore, the ratio of the post-plated portion to the plate thickness can be considered to be 172% or less for the entire steel pipe, taking into account the maximum value (92%) of the ratio of the outer surface bead width after welding to the plate thickness for the entire steel pipe, and the maximum value (80%) of the ratio of the heat-affected zone width to the plate thickness.
[0069] Furthermore, Figure 13 shows the state in which removal of the outer surface bead is unnecessary for steel pipes with three different outer diameters (114.3 mm, 139.8 mm, and 159.8 mm) when the conventional example, end face shape A, and end face shape B are used. In this state, the base metal of the weld is expelled from the outer surface after welding, but this does not affect the quality of the product and the bead width is minimized. The pressing amount at which this state occurs is 0 mm for the conventional example, 5.5 mm for end face shape A, and 10.5 mm for end face shape B, regardless of the outer diameter of the steel pipe. In other words, by setting the pressing amount to 5.5 mm for end face shape A and 10.5 mm for end face shape B, the width of the outer surface bead to be removed can be minimized.
[0070] Although the preferred embodiments of the present invention have been described in detail above with reference to the accompanying drawings, the present invention is not limited to these examples. It is clear that a person skilled in the art to which the present invention pertains can conceive of various modifications and alterations within the scope of the technical ideas set forth in the claims, and it is understood that these also naturally fall within the technical scope of the present invention.
[0071] 5 Plated steel sheet 5i Inner surface 5o Outer surface 5s Outer inclined portion 5t Inner inclined portion 10 High frequency current 15 Coil 20 Squeeze roll 30 Bit 41, 42 Annular cutting portion 41a, 42a Cutting edge 50 Electric resistance welded steel pipe 51 First end face 52 Second end face 53 Outer surface bead 54 Inner surface bead 61, 62 Slit blade 61a, 62a Cutting portion Q1 Welded portion Q2 Heat affected zone
Claims
1. A method for manufacturing an electric-resistance welded steel pipe, comprising: an end face shaping process for forming an outer inclined portion that inclines in the plate thickness direction from the outer surface side toward the inner surface side on each of a first end face and a second end face on both sides of the width direction of a plated steel sheet, or for forming the outer inclined portion and an inner inclined portion that inclines in the plate thickness direction from the inner surface side toward the outer surface side, so that the first end face and the second end face have a shape in which the plate thickness decreases from the center in the width direction toward the end faces; and a pipe making process for butt-welding the formed first end face and second end face together to form a pipe.
2. A method for manufacturing an electric welded steel pipe as described in claim 1, wherein in the end face forming process, at least a portion of the outer inclined portion is covered with a plating that continues from the outer surface side.
3. A method for manufacturing an electric welded steel pipe as described in claim 1 or 2, wherein in the pipe making process, the first end face and the second end face are heated and melted, and the first end face and the second end face are pressed together and joined so that the ratio of the width of the weld bead on the outer surface side to the thickness of the plated steel sheet is 92% or less.
4. A method for manufacturing an electric-resistance welded steel pipe as set forth in claim 3, wherein in the pipe-making process, plating is applied to the welded portion where the first end face and the second end face are pressed together and joined.
5. A method for manufacturing an electric welded steel pipe as described in claim 1 or 2, wherein in the end face forming process, after forming the first end face and the second end face, the plated steel sheet is wound into a coil, and in the pipe making process, the plated steel sheet wound into a coil in the end face forming process is discharged and made into a pipe.
6. An electric welded steel pipe made of a galvanized steel sheet, the electric welded steel pipe having a welded portion extending in the axial direction and a heat-affected portion extending in the axial direction on both circumferential sides of the welded portion, the ratio of the outer surface circumferential length of the welded portion to the thickness of the galvanized steel sheet is 48% or more, and the ratio of the outer surface circumferential length of the heat-affected portion to the thickness of the galvanized steel sheet for each of the heat-affected portions is 40% or less.
7. An electric resistance welded steel pipe made of a plated steel sheet, the outer surface of which has a post-plated portion where plating is applied at least along a weld extending in the axial direction, and the ratio of the outer surface circumferential length of the post-plated portion to the thickness of the plated steel sheet is 172% or less.