Heat seal paper

MYPI2025004355A0Undetermined Publication Date: 2024-07-31OJI HLDG CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025004355
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-01-31
Filing Date
2024-01-25
Publication Date
2024-07-31

AI Technical Summary

Technical Problem

Heat-seal paper using polylactic acid or polybutylene succinate in the heat-seal layer tends to wrinkle during pillow packaging, leading to poor appearance and tear issues when processed with a pillow packaging machine.

Method used

A heat-seal paper with a thermoplastic resin containing polylactic acid or polybutylene succinate, combined with an inorganic pigment like talc, kaolin, or calcium carbonate, optimized to achieve a specific tear strength to bending resistance ratio, ensuring reduced wrinkle formation and improved tear resistance during pillow packaging.

Benefits of technology

The solution effectively reduces wrinkle occurrence and enhances the suitability of heat-seal paper for pillow packaging by maintaining a high tear strength while minimizing bending resistance, ensuring smooth bag-making processes and maintaining environmental sustainability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The heat seal paper according to one embodiment of the present invention is obtained by adhering a heat seal component containing a thermoplastic resin to at least one surface of a paper substrate having pulp as the main component, wherein the thermoplastic resin contains at least one type of resin selected from the group consisting of polylactic acid and polybutylene succinate, the paper substrate contains an inorganic pigment, and the amount of the inorganic pigment is within a range from 1 to 20% by mass relative to the total mass of the paper substrate.
Need to check novelty before this filing date? Find Prior Art

Description

heat seal paper

[0001] This application claims priority from Japanese Patent Application No. 2023-012730, filed on January 31, 2023, the contents of which are incorporated herein by reference.

[0002] Film-like packaging materials processed into bags (bag-formed bags) are used to package foods, etc. Heat-sealable films having a heat-sealable layer containing a thermoplastic resin on at least one surface of a resin substrate are widely used as such packaging materials, but in recent years, heat-sealable paper having a heat-sealable layer on at least one surface of a paper substrate has also come into use (Patent Documents 1 and 2).

[0003] Japanese Patent Publication No. 2021-188241 Japanese Patent Publication No. 2022-018160

[0004] Because heat-seal paper uses a paper substrate, it has a smaller environmental impact than heat-seal film, which uses a resin substrate. Because polylactic acid and polybutylene succinate are highly biodegradable, using these resins in the heat-seal layer of heat-seal paper can further reduce the environmental impact. However, heat-seal paper using polylactic acid or polybutylene succinate in the heat-seal layer is highly rigid, making it prone to wrinkling during processing, especially during bag formation (pillow processing) using a pillow packaging machine. Pillow packaging is a packaging method using film-like packaging material. In pillow packaging, a roll of packaging material is placed in the pillow packaging machine, unwound from the roll, deformed into a cylindrical shape using a tool called a sailor (former), and heat-sealed and cut to form a pillow-shaped package. If wrinkles occur during bag formation, the package will have a poor appearance.

[0005] An object of the present invention is to provide a heat sealable paper that is less likely to wrinkle even when pillow processed.

[0006] The present invention has the following aspects. [1] A heat-sealable paper having a heat-sealing component containing a thermoplastic resin attached to at least one surface of a paper base material whose main component is pulp, wherein the thermoplastic resin is at least one selected from the group consisting of polylactic acid and polybutylene succinate, and the paper base material contains an inorganic pigment, the content of the inorganic pigment being 1 to 20 mass% relative to the total mass of the paper base material. [2] The heat-sealable paper of [1], wherein the inorganic pigment is at least one selected from the group consisting of talc, kaolin, calcium carbonate, and titanium oxide. [3] The heat-sealable paper of [1] or [2], wherein the content of the thermoplastic resin is 90 mass% or more relative to the total mass of the heat-sealing component. [4] The heat-sealable paper of any one of [1] to [3], wherein the value expressed by T / S is 10 or more, where T is the geometric mean of the tear strength (mN) in each of MD and CD measured in accordance with JIS P 8116:2000, and S is the geometric mean of the bending resistance (mN) in each of MD and CD measured in accordance with JIS P 8125-1:2017. [5] The heat-sealable paper of any one of [1] to [4], wherein the peel strength is 2 N / 15 mm or more when the surfaces of the heat-sealable paper to which the heat-sealing component is attached are heat-sealed under conditions of 140°C, 0.2 MPa, and 1 second, and T-peeled at a tensile speed of 300 mm / min. [6] The heat seal paper according to any one of [1] to [5], wherein the pulp obtained by disintegrating the heat seal paper in accordance with JIS P 8220-1: 2012 has a Canadian standard freeness of 300 to 600 mL as measured in accordance with JIS P 8121-2: 2012. [7] The heat seal paper according to any one of [1] to [6], which is for pillow packaging.

[0007] According to the present invention, it is possible to provide heat seal paper that is less likely to wrinkle even when pillow processed.

[0008] In this specification, "MD" means machine direction. That is, it is the direction parallel to the direction of travel when a paper base material is produced by a papermaking machine, and is also called the machine direction or flow direction. The orientation direction of the fibers of the paper base material can be considered to be MD. If it is unclear which direction is MD, the tensile strength is measured every 22.5 degrees, and the direction showing the strongest tensile strength is considered to be MD. "CD" means cross direction. That is, it is the direction perpendicular to MD, and is also called the cross direction. In this specification, the suffix "to" indicating a numerical range means that the numerical values ​​before and after it are included as the lower and upper limits. The lower and upper limits of the numerical ranges disclosed in this specification can be combined in any way to create a new numerical range.

[0009] <Heat-seal paper> The heat-seal paper according to one embodiment of the present invention comprises a paper substrate and a heat-seal component containing a thermoplastic resin attached to at least one surface of the paper substrate. The paper substrate and the heat-seal component will be described in detail later.

[0010] When the geometric mean of the tear strength (mN) in each of the MD and CD of the heat seal paper is T and the geometric mean of the bending resistance (mN) in each of the MD and CD is S, the value represented by T / S is preferably 10 or more, more preferably 11.5 or more, and even more preferably 13 or more. The upper limit of T / S is not particularly limited, but can be, for example, 50 or less, or 40 or less. Tear strength is measured in accordance with JIS P 8116:2000. Bending resistance is measured in accordance with JIS P 8125-1:2017. After extensive research, the inventors have found that the T / S of heat seal paper affects its suitability for bag formation in a pillow packaging machine. T is an index of tear resistance, and S is an index of hardness. If S is too high (too hard), the paper is likely to tear during bag formation in a pillow packaging machine, even if T is high. By making the T / S ratio 10 or more, the suitability for bag making in a pillow packaging machine is improved, and tearing of the heat seal paper during bag making in the pillow packaging machine can be suppressed. Methods for making the T / S ratio 10 or more include, for example, the following methods. The disintegration freeness will be explained in detail later. - Incorporating 1 to 20 mass% of an inorganic pigment into the paper base material. - Making the disintegration freeness of the heat seal paper 300 to 600 mL.

[0011] The geometric mean T of the tear strength (mN) in each of the MD and CD of the heat-sealable paper is preferably 300 mN or more, more preferably 350 mN or more, and even more preferably 400 mN or more, in order to increase the T / S ratio. The upper limit of T is not particularly limited, but can be, for example, 4000 mN or less, or 3000 mN or less. The geometric mean S of the bending resistance (mN) in each of the MD and CD of the heat-sealable paper is preferably 60 mN or less, more preferably 50 mN or less, and even more preferably 40 mN or less, in order to increase the T / S ratio. The lower limit of S is not particularly limited, but can be, for example, 5 mN or more, or 10 mN or more.

[0012] The heat seal peel strength (hereinafter also referred to as "heat seal peel strength") when the surfaces of the heat seal paper to which the heat seal component is attached are heat sealed under conditions of 140°C, 0.2 MPa, and 1 second, and T-peeled at a tensile speed of 300 mm / min is preferably 2 N / 15 mm or more, more preferably 2.4 N / 15 mm or more, and even more preferably 2.8 N / 15 mm or more. When the heat seal peel strength is above the above-mentioned lower limit, good heat sealing can be achieved during bag formation using a pillow packaging machine, resulting in better pillow packaging suitability. The upper limit of the heat seal peel strength is not particularly limited, but can be, for example, 30 N / 15 mm or less, or 20 N / 15 mm or less. The heat seal peel strength can be adjusted, for example, by the amount of heat seal component attached per unit area and the content of thermoplastic resin relative to the total mass of the heat seal component.

[0013] The amount of heat seal component attached per unit area of ​​the heat seal paper is 2 to 30 g / m2 on one side. 2 is preferred, and 3 to 20 g / m 2 More preferably, 4 to 10 g / m 2 When the amount of the heat-sealing component attached is equal to or greater than the above lower limit, the pillow packaging suitability is better. When the amount of the heat-sealing component attached is equal to or less than the above upper limit, blocking and staining during the process are easily suppressed.

[0014] When the amount of heat-sealing component adhered is within the above range, the thickness of the heat-sealing component adhered to the fiber surface of the paper substrate is considered to be approximately 4 μm or less, but is not particularly limited. The thickness of the heat-sealing component on the fiber surface of the paper substrate can be confirmed by microscopic observation of the fiber cross-section. In a cross-section perpendicular to the plane of the heat-sealing paper, a heat-sealing layer consisting of the heat-sealing component may be observed, but it is thought that such a heat-sealing layer may not always be clearly observed.

[0015] In the heat-seal paper, the heat-sealing component may be attached to one side or both sides of the paper substrate. In terms of further reducing production costs, it is preferable that the heat-sealing component be attached to one side of the paper substrate. In the heat-seal paper, the heat-sealing component may be attached uniformly to the paper substrate, or may be attached unevenly in a dotted, linear, or mesh-like pattern when viewed from above.

[0016] The Canadian Standard Freeness (hereinafter also referred to as "disintegrated freeness") of the pulp obtained by disintegrating the heat-sealable paper in accordance with JIS P 8220-1, as measured in accordance with JIS P 8121-2:2012, is preferably 300 to 600 mL, more preferably 350 to 550 mL, and even more preferably 400 to 500 mL. When the disintegrated freeness of the heat-sealable paper is within the above range, the tear strength of the heat-sealable paper tends to be higher.

[0017] The basis weight of heat seal paper is 20 to 200 g / m 2 is preferred, and 35 to 150 g / m 2 More preferably, 40 to 100 g / m 2 is more preferable. When the basis weight of the heat-sealable paper is equal to or greater than the lower limit, the tear strength of the heat-sealable paper tends to be higher. When the basis weight of the heat-sealable paper is equal to or less than the upper limit, the bending resistance of the heat-sealable paper tends to be lower. The basis weight of the heat-sealable paper is measured in accordance with JIS P 8124:2011.

[0018] The thickness of the heat-seal paper is preferably 20 to 300 μm, more preferably 35 to 220 μm, and even more preferably 40 to 150 μm. When the thickness of the heat-seal paper is equal to or greater than the lower limit, the tear strength of the heat-seal paper tends to be higher. When the thickness of the heat-seal paper is equal to or less than the upper limit, the bending resistance of the heat-seal paper tends to be lower. The thickness of the heat-seal paper is measured in accordance with JIS P 8118:2014.

[0019] (Paper base material) The paper base material is composed primarily of pulp. Here, "composed primarily of pulp" means that the pulp content is 70% by mass or more relative to the mass of the paper base material. In this embodiment, the paper base material contains 1 to 20% by mass of an inorganic pigment. Therefore, the pulp content is in the range of 80 to 99% by mass relative to the mass of the paper base material. The pulp content is preferably 85 to 97% by mass, more preferably 90 to 95% by mass relative to the mass of the paper base material.

[0020] The paper substrate may be any commonly used paper, for example, a paper substrate mainly composed of wood pulp. Specific examples of the paper substrate include bleached kraft paper, unbleached kraft paper, fine paper, paperboard, liner paper, coated paper, one-side glazed paper, glassine paper, and graphene paper. Among these, bleached kraft paper, unbleached kraft paper, coated paper, and one-side glazed paper are preferred in terms of the heat sealability of the heat seal paper.

[0021] Examples of pulp include chemical pulps such as bleached hardwood kraft pulp (LBKP), bleached softwood kraft pulp (NBKP), bleached hardwood sulfite pulp (LBSP), and bleached softwood sulfite pulp (NBSP). Other examples include unbleached pulp, semi-bleached pulp, and bleached pulp such as stone ground pulp (GP), pressurized stone ground pulp (PGW), refiner ground pulp (RGP), chemi-ground pulp (CGP), thermomechanical pulp (TMP), and chemi-thermomechanical pulp (CTMP). Other examples include sulfite pulp and recycled paper pulp.

[0022] In order to improve printability, the pulp preferably contains hardwood pulp such as bleached hardwood kraft pulp (LBKP) or bleached hardwood sulfite pulp (LBSP). The content of the hardwood pulp is preferably 50% by mass or more, more preferably 70% by mass or more, and may be 100% by mass, based on the total mass of the pulp.

[0023] In order to increase tear strength, the pulp preferably contains softwood pulp such as bleached softwood kraft pulp (NBKP) or bleached softwood sulfite pulp (NBSP). The content of the softwood pulp is preferably 10% by mass or more, more preferably 20% by mass or more, and may be 100% by mass, based on the total mass of the pulp.

[0024] Hardwood pulp and softwood pulp may be used in combination. When hardwood pulp and softwood pulp are used in combination, the hardwood pulp content is preferably 50 to 90 mass% and the softwood pulp content is 10 to 50 mass%, and more preferably 70 to 90 mass% and 10 to 30 mass% of the softwood pulp content, based on the total mass of the pulp.

[0025] The paper substrate contains an inorganic pigment. When the paper substrate contains an inorganic pigment, the ash content of the paper substrate increases and the tensile modulus decreases. The bending resistance of the paper substrate is proportional to the tensile modulus multiplied by the cube of the thickness. By lowering the tensile modulus, the bending resistance of the paper substrate and, in turn, the bending resistance of the heat-sealable paper is reduced, making it less likely to wrinkle during pillow processing. In addition, the suitability for pillow packaging is improved.

[0026] Examples of inorganic pigments include talc, kaolin, calcium carbonate, titanium oxide, barium sulfate, calcium sulfate, zinc oxide, silicic acid, silicates, colloidal silica, satin white, etc. Among these, from the viewpoint of economy, at least one selected from the group consisting of talc, kaolin, calcium carbonate and titanium oxide is preferred.

[0027] The content of the inorganic pigment is 1 to 20% by mass, preferably 3 to 15% by mass, and more preferably 5 to 10% by mass, based on the total mass of the paper base material. If the content of the inorganic pigment is above the lower limit, bending resistance tends to be low. If the content of the inorganic pigment is below the upper limit, paper dust generation is low.

[0028] The paper base material may further contain internal additives other than inorganic pigments, such as sizing agents, fillers, paper strength agents, retention aids, pH adjusters, drainage aids, water-resistant agents, softeners, antistatic agents, antifoaming agents, slime control agents, dyes, and pigments (excluding inorganic pigments).

[0029] The paper substrate may further include an optional layer, such as a clay coating layer, on at least a portion of one or both sides of the paper substrate. The clay coating layer serves to fill and smooth the paper substrate. Examples of clay include kaolin, talc, and mica.

[0030] The density (tightness) of the paper base material is 0.60 to 1.00 g / cm 3 is preferred, and 0.65 to 0.95 g / cm 3 More preferably, 0.70 to 0.90 g / cm 3 is more preferable. When the density of the paper substrate is equal to or higher than the lower limit, excessive penetration of the heat-sealing components into the paper substrate is suppressed, and the heat-sealing peel strength tends to be high. When the density of the paper substrate is equal to or lower than the upper limit, the heat-sealing paper does not become hard and tends to be less likely to tear. The density of the paper substrate is determined by dividing the basis weight of the paper substrate by its thickness. The method for measuring the basis weight and thickness of the paper substrate is the same as the method for measuring the basis weight and thickness of the heat-sealing paper.

[0031] (Heat-sealing component) The heat-sealing component contains a thermoplastic resin. Therefore, the heat-sealing paper exhibits heat-sealing properties within a practical heating temperature range. The thermoplastic resin contains at least one selected from the group consisting of polylactic acid and polybutylene succinate (hereinafter also referred to as "PBS"). Hereinafter, polylactic acid and PBS will be collectively referred to as "Resin I." Resin I has excellent biodegradability, so the heat-sealing paper has a low environmental impact.

[0032] The polylactic acid may be a homopolymer of L-lactic acid, a homopolymer of D-lactic acid, a copolymer of L-lactic acid and D-lactic acid, or a copolymer of a monomer copolymerizable with L-lactic acid or D-lactic acid. Examples of monomers copolymerizable with L-lactic acid or D-lactic acid include glycolic acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 4-hydroxyvaleric acid, 5-hydroxyvaleric acid, and 6-hydroxycaproic acid. Commercially available polylactic acid may be used. Examples of commercially available polylactic acid include Randy PL-1000 and Randy PL-3000 (aqueous dispersions of polylactic acid) manufactured by Miyoshi Oil & Fats Co., Ltd., and Resem Y225 (aqueous dispersion of polylactic acid) manufactured by Chukyo Oil & Fats Co., Ltd. Resin I may be used alone or in combination of two or more types. Polylactic acid is preferred as Resin I due to its ease of availability.

[0033] The content of resin I, that is, the total content of polylactic acid and PBS, is preferably 50% by mass or more, more preferably 70% by mass or more, and may be 100% by mass, based on the total mass of the thermoplastic resin.

[0034] The thermoplastic resin may further contain another thermoplastic resin other than Resin I. Examples of the other thermoplastic resin include biodegradable resins other than Resin I, polyethylene, polypropylene, olefin-unsaturated carboxylic acid copolymers, acrylic resins, ethylene vinyl alcohol, polystyrene resins, polycarbonate resins, polyacetal resins, polyester resins, polyamides, styrene-butadiene latex, polyvinyl alcohol, and polyvinylidene chloride. The other thermoplastic resin may be a non-petroleum-derived resin. One type of the other thermoplastic resin may be used alone, or two or more types may be used in combination.

[0035] Examples of other biodegradable resins include polybutylene succinate adipate (PBSA), polybutylene adipate terephthalate (PBAT), and poly(3-hydroxybutyrate-co-hydroxyhexanoate) (PHBH). One type of other biodegradable resin may be used alone, or two or more types may be used in combination.

[0036] Olefin-unsaturated carboxylic acid copolymers are copolymers of olefins and unsaturated carboxylic acid monomers. Examples of olefins include ethylene and propylene. Olefins may be used singly or in combination of two or more. Unsaturated carboxylic acid monomers include unsaturated carboxylic acids, their salts, and esters. Specific examples of unsaturated carboxylic acid monomers include unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, cinnamic acid, itaconic acid, fumaric acid, maleic acid, and butenetricarboxylic acid; unsaturated polycarboxylic acid alkyl esters having at least one carboxyl group, such as itaconic acid monoethyl ester, fumaric acid monobutyl ester, and maleic acid monobutyl ester; and unsaturated sulfonic acid monomers and salts thereof, such as acrylamidopropanesulfonic acid, acrylate sulfoethyl sodium salt, and methacrylate sulfopropyl sodium salt. Unsaturated carboxylic acid monomers may be used singly or in combination of two or more.

[0037] The olefin-unsaturated carboxylic acid copolymer can be obtained, for example, by emulsion polymerization of an olefin such as ethylene and an unsaturated carboxylic acid monomer. A commercially available product may be used as the olefin-unsaturated carboxylic acid copolymer. An example of a commercially available olefin-unsaturated carboxylic acid copolymer is ZAIXXEN AC (aqueous dispersion of ethylene-acrylic acid copolymer ammonium salt, copolymerization ratio of acrylic acid: 20 mol%), manufactured by Sumitomo Seika Chemicals Co., Ltd. One type of olefin-unsaturated carboxylic acid copolymer may be used alone, or two or more types may be used in combination.

[0038] The non-petroleum-derived resin is not particularly limited, and various thermoplastic resins can be used. Examples include biomass-derived polyolefin, biomass-derived polyester, biomass-derived polyamide, biomass-derived polyurethane, and biomass-derived cellulose acetate. Biomass is preferably derived from plants. Examples include corn-derived biomass and sugarcane-derived biomass. One type of non-petroleum-derived resin can be used alone, or two or more types can be used in combination.

[0039] Examples of biomass-derived polyolefins include polymers of various olefins such as ethylene and propylene, and copolymers of these olefins. Among these, biomass-derived polypropylene and biomass-derived polyethylene are preferred, and biomass-derived polyethylene is more preferred.

[0040] Commercially available biomass-derived polyolefins may be used, including, for example, Braskem products SBC818 (biomass low-density polyethylene) and SGF4950 (biomass high-density polyethylene).

[0041] In biomass-derived polyesters, either one or both of the alcohol units and the carboxylic acid units are derived from biomass. Examples of alcohols include diols. Examples include ethylene glycol, propanediol, butanediol, pentanediol, hexanediol, neopentyl glycol, 1,4-cyclohexanedimethanol, decanediol, and 2-ethyl-butyl-1-propanediol. However, the alcohols are not limited to these examples. Furthermore, one type of alcohol may be used alone, or two or more types may be used in combination.

[0042] Examples of carboxylic acids include aromatic dicarboxylic acids, aliphatic dicarboxylic acids, and derivatives thereof. Examples of aromatic dicarboxylic acids include terephthalic acid, isophthalic acid, and phthalic acid. Examples of aromatic dicarboxylic acid derivatives include lower alkyl esters of aromatic dicarboxylic acids (e.g., methyl ester, ethyl ester, propyl ester, butyl ester, etc.). Examples of aliphatic dicarboxylic acids include linear or alicyclic dicarboxylic acids having 2 to 40 carbon atoms. Examples include oxalic acid, succinic acid, glutaric acid, 2,6-naphthalenedicarboxylic acid, adipic acid, sebacic acid, dodecanedioic acid, dimer acid, azelaic acid, dodecadicarboxylic acid, and cyclohexanedicarboxylic acid. Examples of aliphatic dicarboxylic acid derivatives include lower alkyl esters of aliphatic dicarboxylic acids (e.g., methyl ester, ethyl ester, propyl ester, butyl ester, etc.). Acid anhydrides of aliphatic dicarboxylic acids such as succinic anhydride are also included. However, the carboxylic acids are not limited to these examples. The carboxylic acids may be used alone or in combination of two or more.

[0043] As the biomass-derived polyester, a commercially available product may be used. An example of a commercially available biomass-derived polyester is CB602AB (biopolyethylene terephthalate) manufactured by FENC.

[0044] From the viewpoint of environmental friendliness, the other thermoplastic resin is preferably at least one selected from the group consisting of other biodegradable resins and non-petroleum-derived resins.

[0045] When the thermoplastic resin has a melting point, the melting point is preferably 80 to 180°C, more preferably 100 to 170°C, and even more preferably 110 to 160°C. When the melting point of the thermoplastic resin is within the above range, it can be heat-sealed well when making bags using a pillow packaging machine. The melting point of the thermoplastic resin is measured using a differential scanning calorimeter (DSC). When the heat-sealing component contains two or more types of thermoplastic resins, the mass average value measured for a mixture of multiple thermoplastic resins is taken as the melting point of the thermoplastic resin. The melting point of polylactic acid is, for example, 145 to 180°C. The melting point of PBS is, for example, 100 to 120°C.

[0046] The content of the thermoplastic resin in the heat-sealing component is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 85% by mass or more, particularly preferably 90% by mass or more, and may even be 100% by mass, relative to the total mass of the heat-sealing component. When the content of the thermoplastic resin in the heat-sealing component is equal to or greater than the above-mentioned lower limit, good heat sealing can be achieved during bag formation using a pillow packaging machine, and the pillow packaging suitability is superior. When the heat-sealing component contains components other than the thermoplastic resin, the content of the thermoplastic resin in the heat-sealing component can be, for example, 99% by mass or less, 98% by mass or less, 98.5% by mass or less, or 97% by mass or less, relative to the total mass of the heat-sealing component.

[0047] The heat-sealing component may further contain a salt of an acrylic acid polymer to enhance the adhesive strength of the heat-sealing paper after heat sealing. Examples of the acrylic acid polymer include polyacrylic acid, acrylic acid-maleic acid copolymer, and acrylic acid-sulfonic acid copolymer. Examples of the salt include sodium salt, potassium salt, and ammonium salt.

[0048] When the heat-sealing component contains a salt of an acrylic acid polymer, the content of the salt of the acrylic acid polymer is preferably 0.1 to 3 mass%, more preferably 0.2 to 2 mass%, and even more preferably 0.5 to 1.5 mass%, relative to the mass of the thermoplastic resin in the heat-sealing component. When the content of the salt of the acrylic acid polymer is equal to or greater than the above-mentioned lower limit, good heat-sealing properties are likely to be obtained. When the content of the salt of the acrylic acid polymer is equal to or less than the above-mentioned upper limit, an improvement in heat-sealing properties commensurate with the amount added is obtained.

[0049] The heat-sealing component may optionally contain various auxiliary agents in addition to the thermoplastic resin and the salt of the acrylic acid polymer. Examples of the auxiliary agents include antifoaming agents, thickeners, thickening polysaccharides, neutralizing agents, plasticizers, preservatives, pH adjusters, crosslinking agents, antiblocking agents, lubricants, dyes, and pigments. Examples of the pigments include the inorganic pigments described above. However, the auxiliary agents are not limited to these examples.

[0050] (Method for Producing Heat-Sealable Paper) Heat-sealable paper can be produced by producing the above-mentioned paper base material and attaching the above-mentioned heat-sealable component to at least one surface of the paper base material.

[0051] The paper substrate can be produced, for example, by making a pulp slurry containing an inorganic pigment using a paper machine and drying the resulting wet paper. The paper machine is not particularly limited. Examples include a Fourdrinier paper machine, a gap former paper machine, a cylinder paper machine, and a short wire paper machine. From the standpoint of economy, a paper machine equipped with an on-machine coater is preferred.

[0052] To prepare a pulp slurry for papermaking, the pulp is preferably disaggregated and beaten using a refiner or beater to impart appropriate flexibility and fluffiness to the pulp. However, the pulp beating method is not particularly limited. As described above, the disaggregated freeness, which is an index of the degree of beating of the pulp, is preferably 300 to 600 mL, more preferably 350 to 550 mL, and even more preferably 400 to 500 mL. The beaten pulp may be mixed with an inorganic pigment and, if necessary, other internal additives such as a sizing agent and a paper strength agent, and dispersed in water to prepare a pulp slurry of a concentration suitable for papermaking.

[0053] The wet paper obtained by the paper machine is preferably dried using a multistage cylinder dryer, an air dryer or a Yankee dryer.

[0054] A method for attaching a heat-sealing component to at least one surface of a paper substrate includes, for example, applying a coating liquid containing the heat-sealing component to at least one surface of the paper substrate and drying the coating liquid. The coating liquid is preferably an aqueous dispersion (e.g., an aqueous emulsion) containing a thermoplastic resin. The coating liquid may further contain, in addition to the thermoplastic resin, a salt of an acrylic acid polymer or an auxiliary as an optional component.

[0055] The method for applying the coating liquid is not particularly limited. Various commonly available coating machines can be used. Examples of coating machines include blade coaters, air knife coaters, roll coaters, reverse roll coaters, bar coaters, curtain coaters, slot die coaters, gravure coaters, champlex coaters, brush coaters, slide bead coaters, two-roll size press coaters, pond size press coaters, rod metering size press coaters, blade metering size press coaters, short dwell coaters, gate roll coaters, and nip coaters using a calendar. Among these, on-machine coating machines are preferred in terms of productivity. Examples of on-machine coating machines that are preferred include blade coaters, bar coaters, gate roll coaters, rod metering size press coaters, blade metering size press coaters, and pond size press coaters.

[0056] The heat seal paper may be subjected to a smoothing treatment as needed. The smoothing treatment can be carried out on-machine or off-machine using a normal smoothing treatment device such as a super calender, gloss calender, or soft calender. The paper substrate may be subjected to a smoothing treatment before the coating liquid is applied, as long as the effects of the invention are not impaired.

[0057] The resulting heat-sealable paper is wound into a roll, and then both ends of the roll may be removed by a slitter to adjust the width of the heat-sealable paper to the width of a processing machine in a subsequent process.

[0058] In the heat seal paper described above, the paper base material contains 1 to 20% by mass of inorganic pigment, so wrinkles are less likely to occur during pillow processing (bag production using a pillow packaging machine). Furthermore, the heat seal paper has excellent pillow packaging suitability, and is less likely to tear when continuously producing bags using a pillow packaging machine. It also has good heat sealability and printability.

[0059] The uses of the heat seal paper are not particularly limited. For example, it can be used as a packaging material in various fields such as paper products, food (e.g., confectionery), medical supplies, electronic components, sanitary products, agricultural materials, and building materials. When the heat seal paper is used as a packaging material, known packaging methods can be applied, such as pillow packaging, gusset packaging, tube packaging, three-side seal packaging, four-side seal packaging, stick packaging, pouch packaging, and deep-draw packaging. Because of the above effects, the heat seal paper is suitable for pillow packaging.

[0060] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following descriptions. "Parts" and "%" represent "parts by mass" and "% by mass", respectively.

[0061] Example 1 An aqueous coating solution was prepared by mixing 90 parts of an aqueous emulsion of polylactic acid ("Rezem Y225" manufactured by Chukyo Yushi Co., Ltd., polylactic acid melting point 150°C), 8.5 parts of kaolin ("Barisurf HX" manufactured by Imerys Co., Ltd.), 1 part of a polyacrylic acid sulfonate ("SN Thickener 615" manufactured by San Nopco), and 0.5 parts of a mineral oil-based defoamer ("Noptum 777F" manufactured by San Nopco). 100 parts of hardwood pulp (LBKP) was beaten and blended with 5.5% talc, 1.5% aluminum sulfate (self-made), 0.55% rosin sizing agent (Size Pine G manufactured by Arakawa Chemical Co., Ltd.), and 0.5% cationized starch (GELTRON 18 manufactured by Oji Cornstarch Co., Ltd.) as internal additives to obtain a pulp slurry. The blending amount (%) of each component is the ratio when the mass of the pulp is 100%. This pulp slurry was applied to the heat seal paper with a basis weight of 50 g / m 2The paper substrate was obtained by papermaking so that the heat seal component adhered to one side. The degree of beating of the pulp was adjusted so that the resulting heat seal paper had a disintegration freeness of 500 mL. The aqueous dispersion was applied on-machine to the felt surface of the resulting paper substrate using a rod metering size press coater, and then dried to obtain a heat seal paper having a heat seal component adhered to one side.

[0062] Example 2 A heat seal paper having a heat seal component attached to one side thereof was obtained in the same manner as in Example 1, except that titanium oxide was used instead of talc.

[0063] Examples 3 and 4 Heat-sealable papers with heat-sealing components attached to one side were obtained in the same manner as in Example 1, except that the amount of talc added was changed so that the content of the inorganic pigment in the paper base material was the value shown in Table 1.

[0064] <Examples 5 and 6> Heat seal papers having a heat seal component attached to one side were obtained in the same manner as in Example 1, except that the beating degree of the pulp was adjusted so that the disintegration freeness of the paper base material was the value shown in Table 1.

[0065] Example 7 A heat seal paper having a heat seal component attached to one side was obtained in the same manner as in Example 1, except that an aqueous emulsion of polylactic acid ("Rezem Y225" manufactured by Chukyo Yushi Co., Ltd.) was used as the aqueous coating liquid.

[0066] Example 8 A heat seal paper having a heat seal component attached to one side was obtained in the same manner as in Example 1, except that 60 parts of hardwood pulp (LBKP) and 40 parts of softwood pulp (NBKP) were used as the pulp.

[0067] Example 9 An aqueous coating liquid was prepared by mixing 70 parts of an aqueous emulsion of polylactic acid (Rezem Y225, manufactured by Chukyo Yushi Co., Ltd.; melting point of polylactic acid: 150°C), 28.5 parts of kaolin (Barisurf HX, manufactured by Imerys), 1 part of a polyacrylic acid sulfonate (SN Thickener 615, manufactured by San Nopco), and 0.5 parts of a mineral oil-based defoamer (Noptum 777F, manufactured by San Nopco). Except for using this aqueous coating liquid, heat seal paper having a heat seal component adhered to one side was obtained in the same manner as in Example 1.

[0068] Example 10 The degree of beating of the pulp was adjusted so that the disintegration freeness of the paper base material was 280 mL, and the basis weight of the paper base material was 40 g / m 2 A heat seal paper having a heat seal component attached to one side was obtained in the same manner as in Example 1, except that the above-mentioned

[0069] Comparative Example 1 A heat seal paper having a heat seal component attached to one side was obtained in the same manner as in Example 1, except that a styrene-butadiene latex ("LX407-S12" manufactured by Nippon Zeon Co., Ltd.) was used instead of the aqueous emulsion of polylactic acid.

[0070] <Comparative Example 2> A heat-sealable paper having a heat-sealing component attached to one side was obtained in the same manner as in Example 1, except that the degree of beating of the pulp was adjusted so that the disintegration freeness of the paper base material was 200 mL and talc was not added.

[0071] Comparative Example 3 A heat seal paper having a heat seal component attached to one side was obtained in the same manner as in Example 1, except that talc was not blended.

[0072] Comparative Example 4 A heat-sealable paper having a heat-sealing component attached to one side was obtained in the same manner as in Example 1, except that the amount of talc added was changed so that the talc content was 25% by mass relative to the mass of the paper base material.

[0073] <Measurement and Evaluation> (Basis Weight) The basis weight of the heat seal paper was measured in accordance with JIS P 8124: 2011. (Disintegrated Freeness) The heat seal paper was disintegrated in accordance with JIS P 8220-1, and the Canadian Standard Freeness of the obtained pulp was measured in accordance with JIS P 8121-2: 2012, and the value was taken as the disintegrated freeness.

[0074] (Tear strength of heat seal paper) In accordance with JIS P 8116:2000, an Elmendorf tear tester was used to measure the tear strength (mN) of the heat seal paper in each of the MD and CD directions, and the geometric mean T was calculated. (Bending resistance of heat seal paper) In accordance with JIS P 8125-1:2017, the bending resistance (mN) of the heat seal paper in each of the MD and CD directions was measured, and the geometric mean S was calculated.

[0075] (Heat seal peel strength) Two sheets of heat seal paper of each example were stacked so that the surfaces with the heat seal component attached faced each other, and heat sealed using a heat seal tester ("TP-701-B" manufactured by Tester Sangyo Co., Ltd.) under conditions of 140 ° C, 0.2 MPa, and 1 second to obtain a test specimen. The obtained test specimen was left to stand for 4 hours or more in a room at a temperature of 23 ° C ± 1 ° C and a humidity of 50% ± 2%. Subsequently, the test specimen was cut to a width of 15 mm and subjected to T-peel at a tensile speed of 300 mm / min using a tensile tester, and the recorded maximum load was taken as the heat seal peel strength.

[0076] (Printability) The wire side of the heat seal paper of each example was printed with a water-based gravure ink ("Surf WH Process Ink" manufactured by DIC Corporation) using a gravure printing tester (manufactured by Kumagai Riki Kogyo Co., Ltd.) under conditions of a printing pressure of 30 kg / cm and a speed of 60 m / min. The printed surface was visually observed, and the printability was evaluated according to the following criteria. A: No missing dots, good appearance. B: Missing dots, some faded.

[0077] (Heat sealability) Using a high-speed horizontal pillow packaging machine FW3410 / B (manufactured by Fujikikai Co., Ltd.), bags were made from the heat seal paper of each example at a speed of 100 bags / minute, and the heat sealability was evaluated according to the following criteria. A: When the adhesive was applied at a sealing temperature of 150°C and the adhesive was peeled off, the paper substrate was destroyed (material breakage). B: When the adhesive was applied at a sealing temperature of 180°C and the adhesive was peeled off, the paper substrate was destroyed (material breakage). C: When the adhesive was applied at a sealing temperature of 180°C and the adhesive was peeled off, the paper substrate was not destroyed (interface peeling or non-adhesion).

[0078] (Wrinkles during bag making) Using a high-speed horizontal pillow packaging machine FW3410 / B (manufactured by Fuji Machinery Co., Ltd.), bags were made from the heat seal paper of each example, and the occurrence of wrinkles in the sailor of the bag making machine (wrinkles during bag making) was evaluated according to the following criteria: A: No wrinkles occurred. B: Light wrinkles occurred. C: Obvious wrinkles occurred, poor appearance.

[0079] (Bag making suitability) Bags were made from the heat seal paper of each example using a high-speed horizontal pillow packaging machine FW3410 / B (manufactured by Fujikikai Co., Ltd.), and the bag making suitability was evaluated according to the following criteria. Bag making suitability indicates suitability for continuous production of bags. If defects such as tearing occur that impair the performance of the bag, continuous production becomes difficult. A: Production is possible without problems. B: Production is possible, although the bag making speed must be reduced to ensure stable bag making. C: Defects such as tearing occur, making continuous production difficult.

[0080] <Results> The measurement results and evaluation results for each example are shown in Tables 1 and 2. In Tables 1 and 2, "PLA" represents polylactic acid.

[0081]

[0082]

[0083] The heat-sealable papers of Examples 1 to 10 suppressed the occurrence of wrinkles during bag making. They also had sufficient heat-sealing properties and excellent printability. The heat-sealable papers of Examples 1 to 9, which had a disintegration freeness of 300 to 600 mL, also had excellent bag-making suitability. On the other hand, Comparative Example 1, which used a thermoplastic resin other than Resin I as the heat-sealing component, was inferior in terms of environmental impact. Comparative Examples 2 and 3, in which the paper substrate did not contain an inorganic pigment, showed obvious wrinkles during bag making. They also had poor bag-making suitability. Comparative Example 4, in which the paper substrate contained 25% inorganic pigment, had poor heat-sealing properties and was not suitable as heat-sealable paper. It also had poor bag-making suitability.

[0084] According to the present invention, it is possible to provide heat seal paper that is less likely to wrinkle even when pillow processed.

Claims

1. A heat seal paper having a heat seal component containing a thermoplastic resin attached to at least one side of a paper base material whose main component is pulp, said thermoplastic resin containing at least one type selected from the group consisting of polylactic acid and polybutylene succinate, said paper base material containing an inorganic pigment, and the content of said inorganic pigment being 1 to 20 mass % relative to the total mass of said paper base material.

2. The heat seal paper according to claim 1, wherein the inorganic pigment is at least one selected from the group consisting of talc, kaolin, calcium carbonate and titanium oxide.

3. A heat seal paper as described in claim 1 or 2, wherein the content of the thermoplastic resin is 90 mass% or more based on the total mass of the heat seal components.

4. A heat seal paper according to claim 1 or 2, in which the value expressed by T / S is 10 or more, where T is the geometric mean of the tear strength (mN) in MD and CD measured in accordance with JIS P 8116:2000, and S is the geometric mean of the bending resistance (mN) in MD and CD measured in accordance with JIS P 8125-1:2017.

5. A heat seal paper as described in claim 1 or 2, in which the surfaces of the heat seal paper to which the heat seal component is attached are heat sealed under conditions of 140°C, 0.2 MPa, and 1 second, and the peel strength when T-peeled at a tensile speed of 300 mm / min is 2 N / 15 mm or more.

6. The heat seal paper according to claim 1 or 2, wherein the pulp obtained by disintegrating the heat seal paper in accordance with JIS P 8220-1:2012 has a Canadian standard freeness of 300 to 600 mL as measured in accordance with JIS P 8121-2:2012.

7. The heat seal paper according to claim 1 or 2, which is for pillow packaging.