Mold release film and method for manufacturing semiconductor package

MYPI2025004388A0Undetermined Publication Date: 2024-08-03AGC INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025004388
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-02-03
Filing Date
2024-01-31
Publication Date
2024-08-03

AI Technical Summary

Technical Problem

The existing methods for manufacturing semiconductor packages face challenges with poor visibility of laser markings due to surface scratches and dirt, which affect appearance quality, and increased risk of dielectric breakdown from electrostatic discharge (ESD), especially with narrower semiconductor device lines.

Method used

A release film comprising a release layer, an antistatic layer, and a base material is used, with specific surface characteristics such as an abundance fraction of 10 to 35 degrees and a surface resistivity of 1×10^7 to 1×10^11 Ω/□, to enhance antistatic properties and releasability, while optimizing the surface roughness for improved laser marking visibility.

Benefits of technology

The solution provides semiconductor packages with excellent antistatic properties, improved releasability, and enhanced laser marking visibility, reducing the visibility of scratches and resin flow marks, and effectively suppressing ESD-related issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025004388_DRAWING_001
    Figure PI2025004388_DRAWING_001
  • Figure PI2025004388_DRAWING_002
    Figure PI2025004388_DRAWING_002
  • Figure PI2025004388_DRAWING_003
    Figure PI2025004388_DRAWING_003
Patent Text Reader

Abstract

The present invention provides a mold release film comprising a mold release layer, an antistatic layer, and a substrate in this order. The average thickness of the mold release layer exceeds 0.1 μm. When unevenness of a surface of a face in contact with curable resin is measured by a laser microscope and a surface angle distribution of an angle (θ) formed between the normal vector of the unevenness and the normal line of a principal surface of the mold release film is obtained, the existence fraction (Φ) in a range of 10-35° is 0.12 or more. This mold release film can be used for the manufacture of a semiconductor package in which a curing-agent resin is used to seal a semiconductor device so as to form a resin sealed portion. Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Release film and method for manufacturing semiconductor package

[0001] The present invention relates to a method for producing a release film and a semiconductor package.

[0002] Semiconductor packages have a resin encapsulation portion that protects the semiconductor element. A curable resin, such as a thermosetting epoxy resin, is widely used to form the resin encapsulation portion. Known methods for encapsulating semiconductor elements include compression molding and transfer molding, in which a substrate on which a semiconductor element is mounted is placed in a mold cavity and a curable resin is filled into the cavity to form the resin encapsulation portion. In these encapsulation methods, a release film is typically placed on the cavity surface of the mold to prevent adhesion between the resin encapsulation portion and the mold. In such cases, the surface shape of the release film is transferred to the surface of the resin encapsulation portion.

[0003] In addition, to ensure subsequent tracking, identification information such as the manufacturer name, product name, and lot number is laser marked on the surface of the sealed semiconductor package. If the visibility of the markings is poor, problems may arise, such as the manufacturer and users being unable to identify the product.

[0004] In light of this situation, for example, Patent Document 1 proposes a release film having a surface condition with a surface smoothness (Ra) of 0.1 to 0.5 μm and a mean irregularity spacing (RSm) of 90 to 125 μm. Use of this release film is said to increase the contrast between the non-marking area and the marking area, resulting in excellent visibility of the marking area.

[0005] Japanese Patent Application Publication No. 2014-179593

[0006] However, scratches, dirt, etc. on the surface of a semiconductor package can cause problems in terms of appearance quality. To make such small scratches less noticeable, the surface of a semiconductor package is made slightly rough, rather than mirror-finished, to create a matte finish. Increasing the contrast between the non-marking area and the marking area, as in Patent Document 1, tends to make scratches, etc. on the non-marking area more noticeable, reducing appearance quality. Furthermore, these scratches, etc. may cause the identification information to be read incorrectly.

[0007] Furthermore, in recent years, semiconductor elements have become increasingly narrow in line width, making them more susceptible to dielectric breakdown due to electrostatic discharge (ESD) caused by slight static electricity, which was previously not a problem. When manufacturing a semiconductor package by encapsulating a semiconductor element using a release film, the curable resin is cured to form a resin encapsulation portion, and then the release film is peeled off from the resin encapsulation portion. It is necessary to suppress ESD even during this peeling process.

[0008] The present disclosure provides a release film that is excellent in antistatic properties and releasability from a semiconductor package and that can form a semiconductor package surface that has excellent laser marking visibility, and a method for manufacturing a semiconductor package using this release film.

[0009] Specific means for achieving the above-mentioned object are as follows. <1> A release film comprising a release layer, an antistatic layer, and a substrate in this order, wherein the average thickness of the release layer is greater than 0.1 μm, and when unevenness on the surface of the release film on the release layer side is measured using a laser microscope to determine a surface angle distribution of the angle (θ) between the normal vector of the unevenness and the normal to the main surface of the release film, the abundance fraction (Φ) in the range of 10 to 35° is 0.12 or more. <2> The release film according to <1>, wherein the arithmetic mean height Sa of at least one surface of the substrate is 0.9 μm or more. <3> The release film according to <2>, wherein the arithmetic mean height Sa of the surface of the substrate on the antistatic layer side is 1.2 μm or more. <4> The release film according to any one of <1> to <3>, wherein the particle content in the release layer is 25% by volume or less. <5> The release film according to any one of <1> to <4>, wherein the base material contains a fluororesin. <6> The release film according to <5>, wherein the fluororesin contains an ethylene-tetrafluoroethylene copolymer. <7> The release film according to <5>, wherein the surface on the release layer side has a surface resistivity of 1×10 7 ~1 x 10 11<1> The release film according to any one of <1> to <6>, having a resistivity of Ω / □. <8> The release film according to any one of <1> to <7>, which is disposed between a curable resin and a surface of a mold in the manufacture of a semiconductor package. <9> The release film according to <8>, wherein a surface of the release film on the release layer side is in contact with the curable resin. <10> A method for manufacturing a semiconductor package having a semiconductor element and a resin encapsulation part formed from a curable resin and encapsulating the semiconductor element, comprising: placing a substrate on which the semiconductor element is mounted in a cavity of a mold; placing the release film according to any one of <1> to <9>, which comprises a release layer, an antistatic layer, and a base, on a cavity surface of the mold on which the substrate is not mounted, with the surface on the release layer side facing the space within the cavity; filling the cavity with the curable resin, and curing the curable resin in contact with the release film to form a resin encapsulation part that encapsulates the semiconductor element.

[0010] According to the present disclosure, there can be provided a release film that is excellent in antistatic properties and releasability from a semiconductor package, and that can form a semiconductor package surface that has excellent laser marking visibility, and a method for manufacturing a semiconductor package using this release film.

[0011] FIG. 1 is a diagram illustrating the surface angle distribution and the abundance fraction (Φ) in the range of 10 to 35°. FIG. 2 is a diagram illustrating the angle (θ) between the normal vector of the irregularities on the surface of a release film and the normal to the main surface of the release film. FIG. 3 is a cross-sectional view schematically illustrating a compression molding method as an example of a method for manufacturing a semiconductor package according to the present disclosure. FIG. 4 is a cross-sectional view schematically illustrating a compression molding method as an example of a method for manufacturing a semiconductor package according to the present disclosure. FIG. 5 is a cross-sectional view schematically illustrating a compression molding method as an example of a method for manufacturing a semiconductor package according to the present disclosure. FIG. 6 is a cross-sectional view schematically illustrating a transfer molding method as an example of a method for manufacturing a semiconductor package according to the present disclosure. FIG. 7 is a cross-sectional view schematically illustrating a transfer molding method as an example of a method for manufacturing a semiconductor package according to the present disclosure. FIG. 8 is a cross-sectional view schematically illustrating a transfer molding method as an example of a method for manufacturing a semiconductor package according to the present disclosure. FIG. 9 is a cross-sectional view schematically illustrating a transfer molding method as an example of a method for manufacturing a semiconductor package according to the present disclosure. 10 and 11 are cross-sectional views schematically illustrating an outline of a transfer molding method as an example of a method for manufacturing a semiconductor package according to the present disclosure.

[0012] Embodiments of the present disclosure are described in detail below. However, the present disclosure is not limited to the following embodiments. In the following embodiments, components (including elementary steps, etc.) are not essential unless otherwise specified. The same applies to numerical values ​​and their ranges, and do not limit the present disclosure. In this disclosure, the term "process" includes not only processes that are independent of other processes, but also processes that cannot be clearly distinguished from other processes as long as the purpose of the process is achieved. In this disclosure, numerical ranges indicated using "to" include the numerical values ​​before and after "to" as the minimum and maximum values, respectively. In numerical ranges described in stages in this disclosure, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another numerical range described in stages. Furthermore, in numerical ranges described in this disclosure, the upper or lower limit of that numerical range may be replaced with a value shown in the examples. In this disclosure, each component may contain multiple corresponding substances. When a composition contains multiple substances corresponding to each component, the content or amount of each component refers to the total content or amount of the multiple substances present in the composition, unless otherwise specified. In the present disclosure, the particles corresponding to each component may contain multiple types of particles. When a composition contains multiple types of particles corresponding to each component, the particle size of each component refers to the value for a mixture of the multiple types of particles present in the composition, unless otherwise specified. In the present disclosure, the term "layer" includes cases where the layer is formed over the entire area when observing the area where the layer exists, as well as cases where the layer is formed only in a portion of the area. When describing with reference to drawings, the present disclosure is not limited to the drawings. The sizes of components in the drawings are conceptual, and the relative size relationships between components are not limited thereto.

[0013] "(Meth)acrylate" is a general term for acrylate and methacrylate. "Acrylic polymer" is a polymer having units based on (meth)acrylate. The acrylic polymer may contain one type of (meth)acrylate-based unit or two or more types of units. The acrylic polymer may further have units based on other monomers other than the units based on (meth)acrylate. In the present disclosure, units based on a monomer may be expressed by adding the unit name to the monomer name, for example, as an ethylene unit.

[0014] In this disclosure, "laser marking visibility" refers to the visibility during automatic visualization inspection (AVI), in which light incident at a specific angle to the horizontal plane of the semiconductor package surface is detected as brightness by a detector positioned at 90°.

[0015] In the present disclosure, the arithmetic mean height Sa is measured in accordance with ISO-25178-2: 2012. A laser microscope is used for the measurement, and the environmental temperature is set to 23 to 25°C.

[0016] <Release Film> The release film of the present disclosure is a release film comprising a release layer, an antistatic layer, and a substrate in this order, wherein the average thickness of the release layer exceeds 0.1 μm, and when the irregularities on the surface of the release film on the release layer side are measured using a laser microscope to determine the surface angle distribution of the angle (θ) between the normal vector of the irregularities and the normal line of the main surface of the release film, the abundance fraction (Φ) of angles in the range of 10 to 35° is 0.12 or more.

[0017] The reason why the above configuration makes it possible to form a semiconductor package surface that has excellent antistatic properties, releasability from the semiconductor package, and laser marking visibility is believed to be as follows, but the present invention is not limited to the following belief.

[0018] When an antistatic layer is provided on a release film from the viewpoint of suppressing ESD, a release layer is often provided on the antistatic layer to improve releasability from the encapsulating resin. If this release layer is too thin, the release property from the resin encapsulation portion tends to be insufficient. The release film of the present disclosure has excellent antistatic properties by comprising, in order from the side in contact with the curable resin, a release layer, an antistatic layer, and a substrate, and the average thickness of the release layer is more than 0.1 μm, thereby ensuring releasability.

[0019] Furthermore, when the unevenness of the surface of the release film of the present disclosure on the release layer side (the surface of the release film on the side where the release layer is present relative to the substrate; hereinafter also referred to as the "first surface") is measured using a laser microscope and the surface angle distribution of the angle (θ) between the normal vector of the unevenness and the normal to the main surface of the release film is determined, the abundance fraction (Φ) in the range of 10 to 35° is 0.12 or more. Note that when an antistatic layer and a release layer are formed by coating on a substrate having an uneven surface to produce a release film, the properties of the angle of the surface unevenness change before and after coating. Because the coating liquid tends to accumulate in the recesses of the substrate, when each layer is formed on the substrate by coating, the change before and after coating tends to be that the surface angle is gentler in the recesses than in the protrusions. Since visibility is affected by the overall surface shape of the uneven surface, it is preferable that the release film of the present disclosure produced by this production method optimizes the overall surface shape of the recesses and protrusions by controlling the surface roughness of the substrate and the average thicknesses of the antistatic layer and the release layer, and as a result, the abundance fraction (Φ) in the range of 10 to 35° is set to 0.12 or more, thereby improving the visibility of the laser marking.

[0020] First, the method for determining the abundance fraction (Φ) will be described. The surface shape of the release film is measured using a laser microscope in accordance with ISO-25178-2:2012 at an ambient temperature of 23 to 25°C, with both the X and Y coordinates measured in 0.25 μm increments. The normal vector of the irregularities at each point is determined using the surfnorm function in MATLAB® R2022b for the obtained X, Y, and Z coordinate (height) data. The angle (θ) between the normal vector of the irregularities at each point and the normal to the main surface of the release film is determined, and a histogram is created in 0.1° increments to determine the surface angle distribution. FIG. 1 shows an example of the surface angle distribution. In the graph of the surface angle distribution in FIG. 1, the proportion of the area occupied by the angle (θ) in the range of 10 to 35° relative to the total area of ​​all angles from 0 to 90° is determined as the abundance fraction (Φ) of the range of 10 to 35°.

[0021] Here, the angle (θ) between the normal vector of the irregularities on the first surface of the release film and the normal to the main surface of the release film will be described using Figure 2. As shown in Figure 2, in the release film 30, the angle between the normal N to the main surface S having the irregularities 32 and the normal vector L to the irregularities 32 is θ. The main surface S is a surface that extends in a direction perpendicular to the thickness direction of the release film, and the normal N to the main surface S can also be said to be the thickness direction of the release film.

[0022] Therefore, the abundance fraction (Φ) in the range of 10 to 35° means the proportion of angles between 10 and 35° among the angles that the normal vector of the irregularities on the surface of the release film has with respect to the normal to the main surface of the release film. For example, when observing light from above the release film, i.e., from the normal direction to the main surface of the release film, light incident at an angle of 20° with respect to the normal to the main surface of the release film will be observed as reflected by a surface with an angle (θ) of 10°. Furthermore, light incident at an angle of 70° with respect to the normal direction to the main surface of the release film will be observed as reflected by a surface with an angle (θ) of 35°. Therefore, when the angle (θ) is 10 to 35°, light incident at an angle of 20 to 70° with respect to the normal direction to the main surface of the release film will be reflected in the normal direction to the main surface of the release film, making such light more visible from above the release film. The irregular shape of the surface of the release film is transferred to the surface of the semiconductor package. The surface of a semiconductor package has an inverted uneven shape of the surface of the release film, and the angle between the normal vector of the unevenness on the surface of the semiconductor package and the normal to the horizontal plane of the semiconductor package surface is the same as the angle (θ) at the corresponding location on the surface of the release film. Therefore, it is believed that the visibility of light on the surface of the semiconductor package coincides with the visibility of light on the surface of the release film. The inventors have experimentally found that when the fraction (Φ) of the angle (θ) in the range of 10 to 35° in the release film is 0.12 or more, the visibility of the laser-marked inscription on the surface of the semiconductor package is excellent when inspected using an AVI equipped with a detector positioned at 90° relative to the horizontal plane of the semiconductor package surface.

[0023] The fraction (Φ) of the angle in the range of 10 to 35° is 0.12 or more, and from the viewpoint of improving the appearance quality by making traces of resin flow (flow marks) on the surface of the semiconductor package and scratches on the package surface less noticeable while maintaining the visibility of the laser marking, it is preferably 0.14 or more, and more preferably 0.15 or more. Furthermore, from the viewpoint of further improving the visibility of the laser marking, the fraction (Φ) of the angle in the range of 10 to 35° is preferably 0.66 or less, more preferably 0.65 or less, and even more preferably 0.64 or less.

[0024] The release film of the present disclosure can be used, for example, by being disposed between a curable resin and a surface of a mold in the manufacture of a semiconductor package. It is preferable that the surface (first surface) of the release film on the release layer side be in contact with the curable resin. In the manufacture of the semiconductor package, a semiconductor element is placed in a mold, and the semiconductor element is encapsulated with a curable resin to form a resin encapsulation portion.

[0025] (Substrate) The material (composition) constituting the substrate is not particularly limited, and known materials such as resins used in release films can be used. The resin used in the substrate preferably contains a resin having releasability, in order to ensure excellent releasability of the release film from the mold after sealing. A resin having releasability refers to a resin in which a layer consisting of only the resin has releasability. Examples of resins having releasability include fluororesin, polymethylpentene, syndiotactic polystyrene, polycycloolefin, silicone rubber, polyester elastomer, polyethylene terephthalate, polybutylene terephthalate, and unstretched nylon. In terms of releasability from the mold, heat resistance at the mold temperature (e.g., 180°C) during sealing, strength capable of withstanding the flow and pressure of the curable resin, and elongation at high temperatures, fluororesin, polymethylpentene, syndiotactic polystyrene, polycycloolefin, and the like are preferred, and fluororesin is particularly preferred in terms of excellent releasability. That is, the substrate preferably contains a fluororesin. These resins may be used alone or in combination of two or more.

[0026] The content of the fluororesin in all resins contained in the substrate is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, particularly preferably 99% by mass or more, and may even be 100% by mass. As the fluororesin, a fluoroolefin-based polymer is preferred in terms of excellent releasability and heat resistance. The fluoroolefin-based polymer is a polymer having units based on a fluoroolefin. The fluoroolefin-based polymer may further have units other than units based on a fluoroolefin.

[0027] Examples of fluoroolefins include tetrafluoroethylene (hereinafter also referred to as "TFE"), vinyl fluoride, vinylidene fluoride, trifluoroethylene, hexafluoropropylene, and chlorotrifluoroethylene. One type of fluoroolefin may be used alone, or two or more types may be used in combination. Examples of fluoroolefin polymers include ethylene-tetrafluoroethylene copolymer (ETFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-perfluoro(alkyl vinyl ether) copolymer (PFA), and tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymer (THV). One type of fluoroolefin polymer may be used alone, or two or more types may be used in combination. ETFE is particularly preferred as the fluoroolefin polymer because of its large elongation at high temperatures. ETFE is a copolymer having TFE units and ethylene units (hereinafter also referred to as "E units"). That is, ETFE is preferred as the fluororesin contained in the substrate.

[0028] ETFE may have units based on a third monomer in addition to TFE units and E units. The third monomer may be used alone or in combination of two or more. The third monomer may be a monomer having a fluorine atom or a monomer not having a fluorine atom.

[0029] Examples of the monomer having a fluorine atom include the following monomers (a1) to (a5): Monomer (a1): Fluoroolefins having 2 or 3 carbon atoms. Monomer (a2): X(CF 2 ) n CY=CH 2 (wherein X and Y each independently represent a hydrogen atom or a fluorine atom, and n represents an integer of 2 to 8.) Monomer (a3): Fluorovinyl ethers. Monomer (a4): Functional group-containing fluorovinyl ethers. Monomer (a5): Fluorine-containing monomers having an aliphatic ring structure.

[0030] Examples of the monomer (a1) include fluoroethylenes (trifluoroethylene, vinylidene fluoride, vinyl fluoride, chlorotrifluoroethylene, etc.), fluoropropylenes (hexafluoropropylene (hereinafter also referred to as "HFP"), 2-hydropentafluoropropylene, etc.), and the like.

[0031] As the monomer (a2), a monomer in which n is 2 to 6 is preferred, and a monomer in which n is 2 to 4 is particularly preferred. A monomer in which X is a fluorine atom and Y is a hydrogen atom, i.e., (perfluoroalkyl)ethylene, is particularly preferred. Specific examples of the monomer (a2) include the following compounds: CF 3 CF 2 CH=CH 2 , C.F. 3 CF 2 CF 2 CF 2 CH=CH 2 ((Perfluorobutyl)ethylene, hereinafter also referred to as "PFBE"), CF 3 CF 2 CF 2 CF 2 CF=CH 2 , C.F. 2 HCF 2 CF 2 CF=CH 2 , C.F. 2 HCF 2 CF 2 CF 2 CF=CH 2 etc.

[0032] Specific examples of the monomer (a3) ​​include the following compounds. Among the following, diene monomers are cyclopolymerizable monomers. CF 2 = CFOCF 3 , C.F. 2 = CFOCF 2 CF 3 , C.F. 2 = CFO (CF 2 ) 2 CF 3 (perfluoro(propyl vinyl ether). hereinafter also referred to as "PPVE"), CF 2 = CFOCF 2CF (CF 3 ) O(CF 2 ) 2 CF 3 , C.F. 2 = CFO (CF 2 ) 3 O (CF 2 ) 2 CF 3 , C.F. 2 = CFO (CF 2 CF (CF 3 ) O) 2 (CF 2 ) 2 CF 3 , C.F. 2 = CFOCF 2 CF (CF 3 ) O(CF 2 ) 2 CF 3 , C.F. 2 = CFOCF 2 CF = CF 2 , C.F. 2 = CFO (CF 2 ) 2 CF = CF 2 etc.

[0033] Specific examples of the monomer (a4) include the following compounds: CF 2 = CFO (CF 2 ) 3 CO 2 CH 3 , C.F. 2 = CFOCF 2 CF (CF 3 ) O(CF 2 ) 3 CO 2 CH 3 , C.F. 2 = CFOCF 2 CF (CF 3 ) O(CF 2 ) 2 SO 2 F etc.

[0034] Specific examples of the monomer (a5) include perfluoro(2,2-dimethyl-1,3-dioxole), 2,2,4-trifluoro-5-trifluoromethoxy-1,3-dioxole, and perfluoro(2-methylene-4-methyl-1,3-dioxolane).

[0035] Examples of the monomer not having a fluorine atom include the following monomers (b1) to (b4): Monomer (b1): olefins, Monomer (b2): vinyl esters, Monomer (b3): ​​vinyl ethers, Monomer (b4): unsaturated acid anhydrides. Specific examples of the monomer (b1) include propylene and isobutene. Specific examples of the monomer (b2) include vinyl acetate. Specific examples of the monomer (b3) include ethyl vinyl ether, butyl vinyl ether, cyclohexyl vinyl ether, and hydroxybutyl vinyl ether.

[0036] Specific examples of the monomer (b4) include maleic anhydride, itaconic anhydride, citraconic anhydride, and 5-norbornene-2,3-dicarboxylic anhydride.

[0037] As the third monomer, the monomer (a2), HFP, PPVE, and vinyl acetate are preferred because they are easy to adjust the degree of crystallinity and have excellent tensile strength and elongation at high temperatures (particularly around 180°C), and HFP, PPVE, and CF 3 CF 2 CH=CH 2 , PFBE is more preferred, and PFBE is even more preferred.

[0038] In ETFE, the molar ratio of TFE units to E units (TFE units / E units) is preferably 80 / 20 to 40 / 60, more preferably 70 / 30 to 45 / 55, and particularly preferably 65 / 35 to 50 / 50. When the TFE units / E units is within the above range, the ETFE has excellent heat resistance and mechanical strength. The proportion of units based on a third monomer in ETFE is preferably 0.01 to 20 mol%, more preferably 0.10 to 15 mol%, and particularly preferably 0.20 to 10 mol%, relative to the total of all units constituting ETFE (100 mol%). When the proportion of units based on the third monomer is within the above range, the ETFE has excellent heat resistance and mechanical strength.

[0039] When the units based on the third monomer contain PFBE units, the proportion of the PFBE units is preferably 0.5 to 4.0 mol%, more preferably 0.7 to 3.6 mol%, and particularly preferably 1.0 to 3.6 mol%, relative to the total (100 mol%) of all units constituting ETFE. When the proportion of the PFBE units is within the above range, the tensile strength and elongation at high temperatures (particularly around 180°C) are improved.

[0040] The melting point of ETFE is preferably 190°C or higher, more preferably 200°C or higher, even more preferably 210°C or higher, and particularly preferably 220°C or higher. The upper limit of the melting point of ETFE is not particularly limited, but is, for example, 270°C. When the melting point of ETFE is within this range, the release film tends to have excellent tensile strength and elongation at high temperatures (particularly around 180°C). "Melting point" means the temperature corresponding to the maximum value of the melting peak measured by differential scanning calorimetry (DSC). The melt flow rate (MFR) of ETFE is preferably 2 to 40 g / 10 min, more preferably 3 to 30 g / 10 min, and particularly preferably 5 to 20 g / 10 min. When the MFR of ETFE is within this range, the release film tends to have large elongation at high temperatures and tends to have excellent conformability to the mold. The MFR of ETFE is a value measured under a load of 49 N at 297°C in accordance with ASTM D3159.

[0041] The substrate may further contain other components other than the resin. Examples of the other components include a lubricant, an antioxidant, an antistatic agent, a plasticizer, and a mold release agent. In terms of preventing mold contamination, the content of the other components in the substrate is preferably 5% by mass or less, more preferably 1% by mass or less, even more preferably 0.5% by mass, and particularly preferably 0% by mass (absence of other components).

[0042] From the viewpoint of improving the appearance quality by making scratches on the surface of the semiconductor package obtained using the release film less noticeable and suppressing wrinkles of the film on the mold surface during the sealing process of the semiconductor package, the arithmetic mean height Sa of at least one surface of the substrate is preferably 0.9 μm or more, more preferably 1.1 μm or more, and even more preferably 1.2 μm or more. From the viewpoint of laser marking visibility on the surface of the semiconductor package, the arithmetic mean height Sa of at least one surface of the substrate is preferably 2.7 μm or less, more preferably 2.6 μm or less, and even more preferably 2.5 μm or less. From the viewpoint of improving the laser marking visibility and the appearance quality by making resin flow marks (flow marks) on the surface of the semiconductor package and scratches on the package surface less noticeable, the arithmetic mean height Sa of the substrate surface on the first surface side (antistatic layer side) is preferably 0.05 μm or more, more preferably 0.9 μm or more, even more preferably 1.2 μm or more, particularly preferably 1.4 μm or more, and extremely preferably 1.5 μm or more. From the viewpoint of laser marking visibility, the arithmetic mean height Sa of the substrate surface on the first surface side is preferably 2.7 μm or less, more preferably 2.6 μm or less, and even more preferably 2.5 μm or less.

[0043] Furthermore, from the viewpoint of suppressing wrinkles on the mold surface during the sealing process of the semiconductor package and releasability from the mold, the arithmetic mean height Sa of the substrate surface on the release layer side of the release film (the surface of the release film on the side where the substrate is present relative to the release layer; hereinafter also referred to as the "second surface") is preferably 0.03 μm or more, more preferably 0.05 μm or more, and even more preferably 0.1 μm or more. From the viewpoint of suppressing wrinkles on the mold surface during the sealing process of the semiconductor package, the arithmetic mean height Sa of the substrate surface on the second surface side is preferably 0.9 μm or more, more preferably 1.2 μm or more, even more preferably 1.3 μm or more, and particularly preferably 1.5 μm or more. From the viewpoint of laser marking visibility on the surface of the semiconductor package, the arithmetic mean height Sa of the substrate surface on the second surface side is preferably 2.7 μm or less, more preferably 2.6 μm or less, and even more preferably 2.5 μm or less. When the arithmetic mean height Sa of the substrate surface on the second surface side is equal to or less than the upper limit, the shape of the substrate surface on the second surface side is less likely to affect the surface of the semiconductor package. Note that the arithmetic mean height Sa of the substrate surface on the second surface side may be less than 0.03 μm, may be equal to or less than 0.02 μm, or may be a mirror finish.

[0044] The arithmetic mean height Sa of the surface of the substrate may be measured after removing the release layer, antistatic layer, and other layers from the release film using methyl ethyl ketone.

[0045] In the substrate, the surface shape having an arithmetic mean height Sa of 0.9 μm or more may be a shape in which at least one of a plurality of convex portions and concave portions is randomly distributed, or a shape in which at least one of a plurality of convex portions and concave portions is regularly arranged. The shapes of the plurality of convex portions may be the same or different. Furthermore, the sizes of the plurality of convex portions may be the same or different. The sizes of the plurality of concave portions may be the same or different.

[0046] Examples of the convex portions include long convex portions extending on the surface of the release film, scattered protrusions, etc., and examples of the concave portions include long grooves extending on the surface of the release film, scattered holes, etc. Examples of the shape of the convex portions or grooves include straight lines, curved lines, bent lines, etc. On the surface of the release film, multiple convex portions or grooves may exist in parallel to form stripes. Examples of the cross-sectional shape of the convex portions or grooves in a direction perpendicular to the longitudinal direction include polygons such as triangles (V-shapes), semicircles, etc. Examples of the shape of the protrusions or holes include polygonal pyramids such as triangular pyramids, quadrangular pyramids, and hexagonal pyramids, cones, hemispheres, polyhedrons, and various other irregular shapes.

[0047] The method for producing a substrate having a surface with an arithmetic mean height Sa of 0.9 μm or more is not particularly limited, and any known production method can be used. For example, a method of transferring the unevenness of a master mold to the surface of a resin film by thermal processing can be used. From the viewpoint of productivity, the following methods (i) and (ii) are preferred, with method (ii) being particularly preferred.

[0048] (i) A method in which a resin film is passed between two rolls, and the irregularities formed on the surface of the rolls are continuously transferred to the resin film. (ii) A method in which a resin extruded from a die of an extruder is passed between two rolls, and the resin is formed into a film while the irregularities formed on the surface of the rolls are continuously transferred to the surface of the resin film.

[0049] By using one of the two rolls as a roll having an uneven surface (hereinafter also referred to as a mold roll) and the other as a roll without unevenness, a substrate having unevenness on one side is produced. By using both of the two rolls as mold rolls, a substrate having unevenness on both sides is produced. Note that one of the two rolls usually has the function of pressing the resin film and is called a pressing roll. When a roll without unevenness on its surface is used, the roll without unevenness is usually used as a cooling roll, and when both of the two rolls are mold rolls, one of them is used as a cooling roll. Note that a roll without unevenness on its surface also means a roll having a surface that can form a substantially smooth surface.

[0050] The unevenness on the surface of the mold roll is an inverted shape of a specific unevenness on the substrate, and is the same shape as the unevenness formed on the surface of the resin-sealed portion of the semiconductor package. Methods for forming unevenness on the surface of the mold roll include cutting, etching, and the like. In the case of a rubber-wrapped roll, a mold roll having an uneven surface can be obtained by blending particles into the rubber sheet wound on the surface. In this case, the depth direction of the roughness, i.e., Sa, can be adjusted by the size of the particles blended into the rubber sheet. In the case of a resin-wrapped roll, Sa can also be adjusted by a similar method.

[0051] In methods (i) and (ii), the arithmetic mean height Sa of the substrate surface can be adjusted by adjusting the processing speed, the melt flow rate (MFR) of the substrate resin, the pressure of the roll, the distance between the die and the roll, and the like, in addition to the unevenness of the roll surface.

[0052] The average thickness of the substrate is preferably 35 to 100 μm, more preferably 35 to 75 μm. When the thickness of the substrate is 35 μm or more, the release film tends to have excellent releasability. When the thickness of the substrate is 75 μm or less, the release film is easily deformable and has excellent mold followability. When the thickness of the substrate is 100 μm or less, the release film is easy to handle (for example, roll-to-roll handling), and wrinkles are less likely to occur when the release film is stretched and placed to cover the cavity of a mold.

[0053] The average thickness of the substrate is measured in accordance with ISO 4591:1992 (JIS K7130:1999, Method B1, a method for measuring thickness by a mass method of a sample taken from a plastic film or sheet). In this case, the average thickness of the substrate may be measured after removing the release layer, antistatic layer, and other layers from the release film using methyl ethyl ketone.

[0054] (Antistatic Layer) The material of the antistatic layer is not particularly limited as long as it has an antistatic function. The antistatic layer preferably contains an antistatic agent. Examples of antistatic agents include ionic liquids, conductive polymers, metal ion conductive salts, and conductive metal oxides. A conductive polymer is a polymer in which electrons move and diffuse along the polymer skeleton (polymer skeleton). Examples of conductive polymers include polyaniline-based polymers, polyacetylene-based polymers, polyparaphenylene-based polymers, polypyrrole-based polymers, polythiophene-based polymers, and polyvinylcarbazole-based polymers. Examples of metal ion conductive salts include lithium salt compounds. Examples of conductive metal oxides include tin oxide, tin-doped indium oxide, antimony-doped tin oxide, phosphorus-doped tin oxide, zinc antimonate, and antimony oxide.

[0055] The antistatic layer preferably contains a resin binder. When the antistatic layer contains a resin binder and an antistatic agent, the antistatic agent is preferably dispersed in the resin binder. The resin binder is preferably heat-resistant enough to withstand the heat (e.g., 180°C) in the sealing step, and examples thereof include acrylic resin, silicone resin, urethane resin, polyester resin, polyamide resin, vinyl acetate resin, ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, chlorotrifluoroethylene-vinyl alcohol copolymer, and tetrafluoroethylene-vinyl alcohol copolymer.

[0056] The resin binder may be crosslinked. A crosslinked resin binder has better heat resistance than a non-crosslinked resin binder. Examples of such a resin binder include a carboxy group-containing (meth)acrylic polymer and a hydroxy group-containing acrylic polymer. Examples of the crosslinking agent include a polyfunctional aziridine compound and a polyfunctional epoxy compound in the case of a carboxy group-containing acrylic polymer, and a polyfunctional isocyanate compound in the case of a hydroxy group-containing acrylic polymer.

[0057] The surface resistivity of the antistatic layer is 1×10 10 Ω / □ or less is preferable, and 1×109 The lower limit of the surface resistivity of the antistatic layer is not particularly limited, but is preferably 1×10 7 The content of the antistatic agent in the antistatic layer is appropriately set so that the surface resistivity of the antistatic layer falls within the above range.

[0058] The average thickness of the antistatic layer is preferably 0.05 to 3 μm, more preferably 0.05 to 2 μm, from the viewpoint of reducing the surface resistivity of the first surface of the release film while maintaining releasability. The method for measuring the average thickness of the antistatic layer and the average thickness of the release layer described below is not particularly limited. For example, the average thickness of the antistatic layer and the average thickness of the release layer described below may be determined by removing the release layer and the antistatic layer from the release film using methyl ethyl ketone, measuring the mass before and after removal of each layer, and using the reduced mass and the density of each layer. The average thickness of the antistatic layer and the average thickness of the release layer described below may also be determined by observing the cross section of the release film using a focused ion beam scanning electron microscope (FIB-SEM). With FIB-SEM, layer boundaries can be determined from the difference in contrast between layers, and the thickness of each layer can be measured. Such measurements are performed at 30 randomly selected locations, or at least 30 locations between the concave and convex portions if surface irregularities are observed, and the average thickness of each layer can be determined by averaging the measurement results. In addition, when there is no difference in contrast between the antistatic layer and the release layer during cross-sectional observation with an FIB-SEM and it is difficult to distinguish the boundary between the layers, the boundary between the layers can be distinguished using a scanning transmission electron microscope (STEM-EDX) based on the presence or absence of elements characteristic of the antistatic layer (particularly the antistatic agent contained in the antistatic layer) and the release layer.

[0059] The method for forming the antistatic layer is not particularly limited, and a method of coating the antistatic layer composition on one side of the substrate and drying it is preferred. As the coating method, various known wet coating methods can be used, such as gravure coating, die coating, and bar coating. The drying temperature and time are appropriately adjusted depending on the type and content of the liquid medium.

[0060] The antistatic layer composition may contain other components in addition to the antistatic agent. Examples of other components include a liquid medium such as a solvent or water. The solid content of the antistatic layer composition is appropriately adjusted in consideration of coatability. To enhance wettability, it is preferable to subject the surface of the substrate to a corona treatment before applying the antistatic layer composition. It is preferable to perform the corona treatment so that the wetting tension based on ISO 8296:1987 (JIS K6768:1999) is 40 mN / m or more.

[0061] (Release Layer) The material of the release layer is not limited as long as it has releasability. The release layer may or may not have adhesive properties. The release layer preferably contains a reaction cured product of a hydroxyl group-containing acrylic polymer and a polyfunctional isocyanate compound.

[0062] The hydroxyl group contained in the hydroxyl group-containing acrylic polymer is a crosslinking functional group that reacts with the isocyanate group in the polyfunctional isocyanate compound. The hydroxyl value of the hydroxyl group-containing acrylic polymer is preferably 1 to 100 mgKOH / g, particularly preferably 29 to 100 mgKOH / g. The hydroxyl value is measured by the method specified in JIS K0070:1992.

[0063] The hydroxy group-containing acrylic polymer may or may not have a carboxy group. Like the hydroxy group, the carboxy group is a crosslinking functional group that reacts with the isocyanate group in the polyfunctional isocyanate compound. The acid value of the hydroxy group-containing acrylic polymer is preferably 0 to 100 mgKOH / g, particularly preferably 0 to 30 mgKOH / g. The acid value, like the hydroxyl value, is measured by the method specified in JIS K0070:1992.

[0064] The crosslinking functional group equivalent weight (total equivalent weight of hydroxy groups and carboxy groups) of the hydroxy group-containing acrylic polymer is 2,000 g / mol or less, preferably 500 to 2,000 g / mol, and particularly preferably 600 to 1,000 g / mol. The "total equivalent weight of hydroxy groups and carboxy groups" means the total mass of hydroxy groups and carboxy groups per mole of the hydroxy group-containing acrylic polymer.

[0065] The crosslinking functional group equivalent corresponds to the molecular weight between crosslinking points and is a physical property that governs the elastic modulus after crosslinking (elastic modulus of the reaction-cured product). When the crosslinking functional group equivalent is 2,000 g / mol or less, the elastic modulus of the reaction-cured product is sufficiently high, and the release layer has excellent releasability from the resin-sealed portion and excellent peelability from the semiconductor chip, source electrode, or seal glass. Furthermore, when the crosslinking functional group equivalent is 2,000 g / mol or less, migration to the resin-sealed portion (adhesive residue) is suppressed.

[0066] The mass average molecular weight (Mw) of the hydroxy group-containing acrylic polymer is preferably 100,000 to 1,200,000, more preferably 200,000 to 1,000,000, and particularly preferably 200,000 to 700,000. When the mass average molecular weight is 100,000 or more, the releasability from the resin encapsulation portion and the removability from the semiconductor chip, source electrode, or seal glass are superior. When the mass average molecular weight is 1,200,000 or less, the adhesion to the semiconductor chip, source electrode, or seal glass is superior. The mass average molecular weight of the hydroxy group-containing acrylic polymer is a polystyrene-equivalent value obtained by measurement by gel permeation chromatography using a calibration curve prepared using standard polystyrene samples of known molecular weight.

[0067] The glass transition temperature (Tg) of the hydroxy group-containing acrylic polymer is preferably 20°C or lower, particularly preferably 0°C or lower. If Tg is equal to or higher than the lower limit of the above range, the release layer exhibits sufficient flexibility even at low temperatures, and is easily peeled from the substrate. The lower limit of Tg is not particularly limited, but is preferably -60°C or higher within the above-mentioned molecular weight range. In the present disclosure, Tg refers to the midpoint glass transition temperature measured by differential scanning calorimetry (DSC).

[0068] The polyfunctional isocyanate compound is a compound having two or more isocyanate groups, preferably a compound having 3 to 10 isocyanate groups. Examples of polyfunctional isocyanate compounds include hexamethylene diisocyanate (HDI), tolylene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), naphthalene diisocyanate (NDI), tolidine diisocyanate (TODI), isophorone diisocyanate (IPDI), xylylene diisocyanate (XDI), triphenylmethane triisocyanate, and tris(isocyanatophenyl)thiophosphate. Other examples include isocyanurate compounds (trimers) and biuret compounds of these polyfunctional isocyanate compounds, and adducts of these polyfunctional isocyanate compounds and polyol compounds. It is preferable for the polyfunctional isocyanate compound to have an isocyanurate ring, as the planarity of the ring structure allows the reaction-cured product (release layer) to exhibit a high elastic modulus. Examples of polyfunctional isocyanate compounds having an isocyanurate ring include isocyanurates of HDI (isocyanurate-type HDI), isocyanurates of TDI (isocyanurate-type TDI), and isocyanurates of MDI (isocyanurate-type MDI).

[0069] The release layer may contain other components, such as crosslinking catalysts (e.g., amines, metal compounds, acids, etc.), reinforcing fillers, coloring dyes, pigments, antistatic agents, etc. As the antistatic agent, those listed for the antistatic layer may be used.

[0070] The crosslinking catalyst may be any substance that functions as a catalyst for the reaction (urethanization reaction) between a hydroxy group-containing acrylic copolymer and a crosslinking agent when a polyfunctional isocyanate compound is used as the crosslinking agent, and a general urethanization reaction catalyst can be used, including, for example, amine compounds such as tertiary amines, organotin compounds, organolead compounds, organozinc compounds, and other organometallic compounds. Examples of tertiary amines include trialkylamines, N,N,N',N'-tetraalkyldiamines, N,N-dialkylaminoalcohols, triethylenediamine, morpholine derivatives, and piperazine derivatives. Examples of organotin compounds include dialkyltin oxides, fatty acid salts of dialkyltins, and fatty acid salts of stannous.

[0071] As the crosslinking catalyst, an organic tin compound is preferred, with dioctyltin oxide, dioctyltin dilaurate, dibutyltin laurate, and dibutyltin dilaurate being particularly preferred. Alternatively, a dialkylacetylacetone tin complex catalyst can be used, which is synthesized by reacting a dialkyltin ester with acetylacetone in a solvent and has a structure in which two acetylacetone molecules are coordinated to one dialkyltin atom. The amount of the crosslinking catalyst used is preferably 0.01 to 0.5 parts by mass per 100 parts by mass of the hydroxyl group-containing acrylic polymer.

[0072] The release layer may contain particles. The particles may be used to adjust the fraction of the release film in the range of 10 to 35° on the first surface of the release film. Alternatively, a substrate having an uneven surface may be used, and particles may be further added to the release layer to adjust the fraction of the release film in the range of 10 to 35° on the first surface of the release film. When a substrate having an uneven surface is used, the release layer does not need to contain particles.

[0073] The material of the particles contained in the release layer is not particularly limited, and may be, for example, organic particles or inorganic particles. Examples of organic particles include acrylic resin particles, polyolefin resin particles, polystyrene resin particles, polyacrylonitrile resin particles, and silicone resin particles. Examples of inorganic particles include silica particles and alumina particles.

[0074] The average particle size of the particles is preferably 2.0 μm or more, more preferably 2.5 μm or more, and even more preferably 3.0 μm or more. In such a case, the resin flow marks (flow marks) in the formed resin sealing portion can be made less noticeable. Furthermore, the average particle size of the particles is preferably 10 μm or less, more preferably 7.5 μm or less, and even more preferably 5 μm or less. In such a case, detachment of particles from the release layer can be easily suppressed.

[0075] When the release layer contains particles, the content of particles in the release layer is preferably 3.0% by volume or more, more preferably 3.9% by volume or more, and even more preferably 5.0% by volume or more, from the viewpoint of making the resin flow marks (flow marks) of the formed resin sealing portion less noticeable.The content of particles in the release layer is preferably 25% by volume or less, more preferably 20% by volume or less, and even more preferably 16.5% by volume or less, from the viewpoint of making it easier to suppress particle detachment from the release layer.In addition, when using a substrate with an uneven surface structure, the content of particles in the release layer is preferably 16.5% by volume or less, more preferably 10% by volume or less, and even more preferably 4.9% by volume or less, from the viewpoint of making it easier to suppress particle detachment from the release layer, and may be 0% by volume, that is, may not contain particles.

[0076] The particle content can be calculated as the proportion of resin particles per unit volume, for example, by observing the cross section of the release layer with a scanning electron microscope (SEM). Specifically, it can be calculated by the following method. First, the cross section of the target release layer is observed with an SEM, and the number and particle diameter of resin particles contained in an arbitrary area (hereinafter also referred to as the "target area") in this cross section are measured. Furthermore, an arbitrary volume (hereinafter also referred to as the "target volume") is set based on the target area, and the number of resin particles contained in this target volume is calculated. Furthermore, the volume per resin particle is calculated based on the particle diameter of the resin particles. The total volume of resin particles contained in the target volume is then calculated from the calculated number of resin particles and volume per resin particle, and the layer volume of this resin particle is divided by the target volume to calculate the volume content of resin particles contained in the target release layer.

[0077] From the viewpoint of the releasability of the release film, the average thickness of the release layer is more than 0.1 μm, preferably 0.15 μm or more, more preferably 0.17 μm or more, and even more preferably 0.2 μm or more. Because the thickness of the release layer is more than 0.1 μm, the releasability is ensured. Furthermore, from the viewpoint of the antistatic properties of the release film, the thickness of the release layer is preferably 2.3 μm or less, more preferably 2.2 μm or less, and even more preferably 2.1 μm or less. When the thickness of the release layer is 2.3 μm or less, the antistatic properties are better.

[0078] The method for forming the release layer is preferably a method in which a composition for the release layer containing each component of the release layer and a liquid medium is coated on the antistatic layer and then dried. As the coating method, various known wet coating methods can be used, such as gravure coating, die coating, and bar coating. The temperature and time of drying are appropriately adjusted depending on the type and content of the liquid medium.

[0079] (Other Layers) The release film may have other layers. The other layers may be provided between the base layer and the antistatic layer, or between the antistatic layer and the release layer, or may be provided on the side of the base layer opposite the antistatic layer, or may be provided on the side of the release layer opposite the antistatic layer. For example, the other layers may be the first surface of the release film. Examples of the other layers include a gas barrier layer and a colored layer. Any one of these layers may be used alone, or two or more types may be used in combination. The average thickness of each of the other layers is preferably 0.05 to 3 μm, more preferably 0.05 to 2 μm.

[0080] (Physical Properties of the Release Film) The arithmetic mean height Sa of the first surface of the release film is preferably 1.0 μm or more, more preferably 1.1 μm or more. In such a case, the resin flow marks (flow marks) formed in the resin sealing portion are not noticeable, which is preferable. Furthermore, when the release layer does not contain particles, the arithmetic mean height Sa of the first surface of the release film is preferably 2.3 μm or less, more preferably 2.2 μm or less, and even more preferably 2.1 μm or less. In such a case, the laser marking visibility on the surface of the semiconductor package formed using the release film is more excellent. When the release layer contains particles, the arithmetic mean height Sa of the first surface of the release film is preferably 3.0 μm or less, more preferably 2.9 μm or less, and even more preferably 2.7 μm or less. In such a case, the laser marking visibility is more excellent.

[0081] The surface resistivity of the first surface of the release film is 1×10 11 Ω / □ or less is preferable, and 2×10 10 The surface resistivity of the first surface of the release film is preferably 1×10 Ω / □ or less. In this case, damage to the semiconductor chip due to discharge during peeling can be effectively prevented. The lower limit of the surface resistivity of the first surface of the release film is not particularly limited, but is preferably 1×10 7 The surface resistivity may be Ω / □ or more. The surface resistivity is measured in accordance with IEC 60093, double ring electrode method.

[0082] The electrostatic potential of the first surface of the release film is preferably from |0 to 50| V, more preferably from |0 to 30| V, and even more preferably from |0 to 25| V. The electrostatic potential is measured with a surface electrometer.

[0083] <Method for manufacturing a semiconductor package> The method for manufacturing a semiconductor package of the present disclosure is a method for manufacturing a semiconductor package having a semiconductor element and a resin sealing portion that seals the semiconductor element and is formed from a curable resin, and includes the steps of: placing a substrate that includes the semiconductor element in a cavity of a mold; placing a release film of the present disclosure that includes a release layer, an antistatic layer, and a substrate on the cavity surface of the mold on which the substrate is not placed, with the surface on the release layer side facing the space in the mold cavity; filling the cavity with the curable resin; and curing the curable resin in contact with the release film to form a resin sealing portion that seals the semiconductor element.

[0084] The method for manufacturing a semiconductor package according to the present disclosure can employ known manufacturing methods, except for using the release film according to the present disclosure. For example, methods for forming a resin encapsulation portion include compression molding and transfer molding, and known compression molding or transfer molding devices can be used as the apparatus used in these methods. The manufacturing conditions can also be the same as those in known semiconductor package manufacturing methods. Below, compression molding and transfer molding are described as representative examples with reference to figures, but the semiconductor package manufacturing method according to the present disclosure is not limited to these figures. Furthermore, in the following description, a semiconductor package having a so-called MAP-BGA shape is shown as an example of a semiconductor package, but the shape of the semiconductor package is not limited to this.

[0085] 3 and 4 are cross-sectional views that schematically illustrate an outline of the compression molding method. The compression molding method shown in FIG. 3 uses a mold having a fixed upper mold 20, a cavity bottom member 22, and a frame-shaped movable lower mold 24 arranged on the periphery of the cavity bottom member 22. The fixed upper mold 20 is formed with a vacuum vent (not shown) for sucking air between the substrate 10 and the fixed upper mold 20, thereby adsorbing the substrate 10 to the fixed upper mold 20. In addition, the cavity bottom member 22 is formed with a vacuum vent (not shown) for sucking air between the release film 30 and the cavity bottom member 22, thereby adsorbing the release film 30 to the cavity bottom member 22.

[0086] A release film 30 is placed on the movable lower mold 24 so as to cover the upper surface of the cavity bottom member 22. At this time, the release film 30 is placed with its first surface facing upward (the opposite direction to the cavity bottom member 22). The release film 30 is fed from an unwinding roll (not shown) and taken up by a take-up roll (not shown). The release film 30 is pulled by the unwinding roll and the take-up roll, and is therefore placed on the movable lower mold 24 in a stretched state.

[0087] Separately, a vacuum is applied through a vacuum vent (not shown) in the cavity bottom member 22 to reduce the pressure in the space between the upper surface of the cavity bottom member 22 and the release film 30, stretching and deforming the release film 30 and vacuum-adhering it to the upper surface of the cavity bottom member 22. Furthermore, the frame-shaped movable lower die 24 arranged around the periphery of the cavity bottom member 22 is tightened to pull the release film 30 in all directions, placing it in a tensed state. Note that the release film 30 may not always adhere tightly to the cavity surface, depending on the strength and thickness of the release film 30 in a high-temperature environment and the shape of the recess formed by the upper surface of the cavity bottom member 22 and the inner side surface of the movable lower die 24. During the vacuum adsorption stage, a small gap may remain between the release film 30 and the cavity surface, as shown in FIG. 3 .

[0088] 3, an appropriate amount of curable resin 40 is filled onto the release film 30 in the cavity 26 using an applicator (not shown). Separately, vacuum is applied through a vacuum vent (not shown) of the fixed upper mold 20, and the substrate 10 on which multiple semiconductor chips 12 are mounted is vacuum-adsorbed onto the lower surface of the fixed upper mold 20. Various curable resins used in the manufacture of semiconductor packages may be used as the curable resin 40. Thermosetting resins such as epoxy resin and silicone resin are preferred, with epoxy resin being particularly preferred.

[0089] 4, with the hardening resin 40 filled on the release film 30 in the cavity 26, the cavity bottom member 22 and the movable lower die 24 are raised and clamped to the fixed upper die 20. Next, as shown in FIG. 5, only the cavity bottom member 22 is raised and the die is heated to harden the hardening resin 40 and seal the semiconductor chip 12.

[0090] The pressure generated when the cavity bottom member 22 is raised further presses the curable resin 40 filled in the cavity 26 into the cavity surface. This causes the release film 30 to be stretched and deformed, and it adheres to the cavity surface. As a result, a resin sealing portion having a shape corresponding to the shape of the cavity 26 is formed. At this time, the irregularities on the first surface of the release film 30 are transferred to the surface of the resin sealing portion.

[0091] Then, the fixed upper die 20, the cavity bottom member 22, and the movable lower die 24 are opened, and the encapsulated body is removed. The encapsulated body is released from the die, and the used portion of the release film 30 is sent to a take-up roll (not shown), and the unused portion of the release film 30 is sent from an unwinding roll (not shown).

[0092] The substrate 10 and the resin sealing portion of the blanket sealed body removed from the mold are cut (diced) so as to separate the plurality of semiconductor chips 12, thereby obtaining an individual sealed body having the substrate 10, at least one semiconductor chip 12, and a resin sealing portion that seals the semiconductor chip 12. The individualization can be performed by a known method, such as a dicing method.

[0093] A semiconductor package is obtained by printing any desired information by laser marking on the upper surface of the resin-sealed portion of the obtained singulated sealed body (the surface that was in contact with the first surface of release film 30). A semiconductor package manufactured using the release film of the present disclosure has excellent visibility of characters when the characters are printed by laser marking.

[0094] 6 to 11 are cross-sectional views that schematically illustrate the transfer molding method. The transfer molding method shown in FIG. 6 uses a mold having an upper mold 50 and a lower mold 52. The upper mold 50 is formed with a cavity 54 shaped to correspond to the shape of the resin encapsulation portion 14, and a recessed resin inlet portion 60 that guides the curable resin 40 into the cavity 54. The lower mold 52 is formed with a substrate mounting portion 58 for mounting the substrate 10 on which the semiconductor chip 12 is mounted, and a resin mounting portion 62 for mounting the curable resin 40. A plunger 64 is also provided within the resin mounting portion 62, which pushes the curable resin 40 into the resin inlet portion 60 of the upper mold 50.

[0095] 7, the release film 30 is placed so as to cover the cavity 54 of the upper mold 50. The release film 30 is preferably placed so as to cover the entire cavity 54 and the resin introducing portion 60. The release film 30 is pulled by an unwinding roll (not shown) and a take-up roll (not shown), and therefore is placed so as to cover the cavity 54 of the upper mold 50 in a stretched state.

[0096] Then, as shown in FIG. 8 , vacuum suction is applied through a groove (not shown) formed on the outside of the cavity 54 of the upper mold 50, reducing the pressure in the space between the release film 30 and the cavity surface 56 and the space between the release film 30 and the inner wall of the resin introduction section 60, stretching and deforming the release film 30 so that it is vacuum-adsorbed to the cavity surface 56 of the upper mold 50.

[0097] 9, the substrate 10 on which the plurality of semiconductor chips 12 are mounted is placed on the substrate placement section 58, and the upper mold 50 and the lower mold 52 are clamped together to place the plurality of semiconductor chips 12 at predetermined positions within the cavity 54. Furthermore, a curable resin 40 is placed in advance on the plunger 64 of the resin placement section 62. Examples of the curable resin 40 include the same curable resin 40 as that mentioned in the compression molding method.

[0098] 10 , the plunger 64 of the lower mold 52 is pushed up, and the hardening resin 40 is filled into the cavity 54 through the resin introduction portion 60. Next, the mold is heated to harden the hardening resin 40, thereby forming the resin sealing portion 14 that seals the multiple semiconductor chips 12. As the hardening resin 40 is filled into the cavity 54, the resin pressure presses the release film 30 further toward the cavity surface 56, and the release film 30 is stretched and deformed, thereby adhering to the cavity surface 56. As a result, the resin sealing portion 14 is formed in a shape corresponding to the shape of the cavity 54.

[0099] 11, the blanket sealed body 1A is removed from the mold. At this time, a cured product 19 formed by curing the curable resin 40 in the resin introduction portion 60 is removed from the mold together with the blanket sealed body 1A in a state of adhering to the resin sealing portion 14 of the blanket sealed body 1A. Therefore, the cured product 19 adhering to the removed blanket sealed body 1A is cut away to obtain the blanket sealed body 1A.

[0100] The substrate 10 and resin sealing portion 14 of the obtained blanket sealed body 1A are cut (singled) so as to separate the semiconductor chips 12, thereby obtaining singulated sealed bodies each having the substrate 10, at least one semiconductor chip 12, and a resin sealing portion that encapsulates the semiconductor chip 12. The subsequent steps are the same as those in the compression molding method. The method for manufacturing a semiconductor package using the release film of the present disclosure can form a semiconductor package surface that has excellent laser marking visibility.

[0101] <Semiconductor Package> A semiconductor package manufactured using the release film of the present disclosure by the semiconductor package manufacturing method of the present disclosure may be any semiconductor package manufactured through collective sealing and singulation, and examples thereof include semiconductor packages using a MAP (Molded Array Packaging) method or a WL (Wafer Label Packaging) method. The semiconductor package manufactured using the release film of the present disclosure has a surface with excellent laser marking visibility.

[0102] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. Among examples 1 to 27, examples 1 to 13 and 23 to 27 are examples, and examples 14 to 22 are comparative examples. The evaluation methods and materials used in each example are shown below.

[0103] [Evaluation Method] (Thickness) The average thickness (μm) of the substrate was measured in accordance with ISO 4591:1992 (JIS K7130:1999, B1 method, thickness measurement method by mass method of sample taken from plastic film or sheet). The average thickness (μm) of the antistatic layer and the release layer was determined by removing each layer from the release film using methyl ethyl ketone, measuring the mass before and after removing each layer, and using the mass reduction and the density of each layer.

[0104] (Arithmetic mean height Sa) The arithmetic mean height Sa of both surfaces of the substrate and the first surface (surface in contact with the curable resin) of the release film was measured based on JIS B0601:2013 (ISO 4287:1997, Amd.1:2009). An Olympus laser microscope (LEXT OLS 4000) was used for the measurement, and the ambient temperature was set to 23 to 25°C. The measurement sample was attached to a metal substrate to eliminate the influence of a large tilt of the measurement sample itself. The main setting conditions for the laser microscope were as follows:

[0105] Objective lens: MPLAPON50LEXT (magnification: 50x, numerical aperture: 0.95, immersion type: air, mechanical lens barrel length: ∞, cover glass thickness: 0, field of view: FN18) Optical zoom magnification: 1x Scanning mode: XYZ high precision Captured image size [number of pixels]: 259 μm horizontal x 259 μm vertical [1024 x 1024] DIC: Off Multilayer: Off Laser intensity: 100 Offset: 0 Confocal level: 0 Beam diameter aperture: Off Image averaging: 1 time Noise reduction: On Brightness unevenness correction: On Optical noise filter: On Cutoff: None (λc, λs, λf all absent) Filter: Gaussian filter Noise removal: Pre-measurement processing Tilt correction: Not performed

[0106] (Surface angle distribution) Under the same conditions as in the measurement of the arithmetic mean height Sa, the surface shape of the first surface of the release film was measured using an Olympus laser microscope (LEXT OLS 4000) in accordance with ISO-25178-2:2012. The measurement location was changed and the number of measurements was 12. The normal vector of the unevenness at each point was determined using the surfnorm function in MATLAB (registered trademark) R2022b for the X coordinate, Y coordinate, and Z coordinate (height) data obtained at each point in increments of 0.25 μm. The angle (θ) between the normal vector of the unevenness at each point and the normal to the main surface of the release film was determined, and the angle was plotted in increments of 0.1° to determine the surface angle distribution. In the surface angle distribution, the area ratio of the angle (θ) range of 10 to 35° to the total area of ​​all angles from 0 to 90° was calculated as the abundance fraction (Φ) of the range of 10 to 35°.

[0107] (Surface Resistivity) The surface resistivity (Ω / □) of the first surface (the surface in contact with the curable resin) of the release film was measured in accordance with the double ring electrode method of IEC 60093. The measuring instrument used was an ultra-high resistance meter R8340 (manufactured by Advantec) and a resistivity chamber 12704A as the electrode, and the measurement was performed at an applied voltage of 500 V for 1 minute.

[0108] (Releasability) A 13 cm x 13 cm x 100 μm thick aluminum foil (AIN30P according to JIS H4000:2006) was placed on a 13 cm x 13 cm first stainless steel plate. A 125 μm thick polyimide film (Upilex 125S, manufactured by Ube Industries, Ltd.) with a 10 cm x 12 cm to 8 cm x 10 cm hollowed out was placed on top of it as a spacer. Furthermore, an appropriate amount of semiconductor encapsulation epoxy resin (SUMIKON EME G770H typeF ver.GR (manufactured by Sumitomo Bakelite Co., Ltd.)) was spread as a curable resin in the hollowed-out portion of the polyimide film. A release film cut to 13 cm x 13 cm was previously neutralized and placed on top of it so that the first surface was in contact with the curable resin. Finally, a 13 cm x 13 cm second stainless steel plate was placed on top of it.

[0109] The sample prepared by the above procedure was pressed in a press at a temperature of 180°C, a pressure of 1 MPa, and a time of 3 minutes. After removing from the press, the entire sample was placed on a hot plate at 180°C, the second stainless steel plate was removed, and the release film was peeled off by hand over 5 seconds. The evaluation criteria for releasability are as follows: A (good): Easily peeled off. B (poor): Unable to peel off the entire surface.

[0110] (Charging Property) For samples with a release property rating of A, the charging voltage of the first surface of the release film was measured immediately after peeling. A surface electrometer MP-520-1 (manufactured by Midori Anzen Co., Ltd.) was used as the device for measuring charging voltage, and the distance between the release film and the measuring terminal was fixed at 3 cm. The measured value was calculated by rounding off to the nearest 1 V (the upper measurement limit of the device is 2,000 V). The evaluation criteria for charging property are as follows: A (Good): |0 to 30| V B (Fair): Over |30| V, |50| V or less C (Poor): Over |50| V

[0111] (Adhesive Residue) For samples rated A for releasability, after peeling, the surface of the cured resin was observed with an optical microscope (magnification 100x) to see if there was any transfer from the release film. The evaluation criteria for adhesive residue are as follows: A (Good): No transfer was observed on the surface of the cured product. B (Poor): Transfer was observed on the surface of the cured product.

[0112] (Laser marking visibility evaluation) <Preparation of sealed body> The sealed body used for the laser marking visibility evaluation was prepared according to the following procedure, using the film of each example as the release film, a semiconductor sealing epoxy resin (SUMIKON EME G770H typeF ver. GR (manufactured by Sumitomo Bakelite Co., Ltd.)) as the curable resin, and a transfer molding machine (G-LINE Manual System, Apic Yamada Co., Ltd.) as the sealing device.

[0113] The mold temperature was set to 175°C, and a 70mm x 230mm copper lead frame and a 190mm wide release film roll were set in a roll-to-roll configuration. After placing the lead frame in the lower mold, the release film was vacuum-adsorbed onto the upper mold, the mold was closed, and the curable resin was injected. After applying pressure for 5 minutes, the mold was opened and the sealed package was removed. Note that for the film rated B in the above-mentioned mold releasability evaluation, a portion of the cured encapsulating resin and the release film did not release from the mold when the mold was opened, resulting in a separation abnormality, while for the film rated A in mold releasability, no separation abnormality occurred.

[0114] <Laser Marking> A discoloration pattern (printed characters) was formed on the laser marking layer using a 1064 nm wavelength laser marker (product name: MD-X1000) manufactured by Keyence Corporation. The laser marking conditions were: number of prints: 1, scan speed: 1000 mm / s, frequency: 100 kHz, laser power: 20%, print thickness: 0.3 mm, number of lines: 5, and spot variable: -20. The printed characters were 10 alphabet characters (ABCDEFGHIJ), printed with a height of 2.0 mm, a width of 1.5 mm, and a character spacing of 0.5 mm. The visibility of the laser-marked portion (printed characters) produced in this manner was evaluated.

[0115] <Visibility of Marking> Fifty packages on which 10 alphabetical characters (ABCDEFGHIJ) were printed by laser marking were evaluated, and a reading test was conducted on all packages, i.e., 500 characters. The visibility evaluation criteria are as follows: A (Good): All 500 characters were readable, with a reading rate of 100%. B (Fair): One or two characters could not be read, with a reading rate of 99.8 or 99.6%. C (Poor): Three or more characters could not be read, with a reading rate of 99.4% or less.

[0116] Note that "readable" refers to a reading score of 80 to 99, and a reading score of less than 80 is considered unreadable. A high-speed, high-capacity flexible image processing system manufactured by KEYENCE was used for the evaluation of the reading score. The device used for the evaluation is not limited, as long as the incident angle of the red LED is set to 20° to 70° relative to the horizontal plane of the package surface and the detection camera is perpendicular to the horizontal plane of the package. The basic conditions below reproduce the conditions used in typical laser visibility evaluation devices, such as the ICOS component inspection devices CI-9X50 and CI-G10 manufactured by KLA Corporation.

[0117] Measuring equipment: High-capacity controller: XG-X2700, 16x speed 21 megapixel monochrome camera: CA-H2100M, 4 / 3-inch 50mm lens: CA-LHE50 (depth of focus ±2.5mm), red lighting dome Φ152: CA-DDR15, application: XG-X2000 Series Ver. 2.2

[0118] Measurement conditions Measurement area per data: 6.48 μm × 6.48 μm (42 μm 2) Distance between sample and lens: A temporary distance of 170 mm was used to monitor the brightness of the non-marked area, and the position showing maximum brightness was determined. This position was then shortened by 1.0 mm. A red LED lighting dome was installed so that the angle of incidence on the package surface was between 20° and 70°, and the camera was set perpendicular to the package surface. The camera sensitivity was 3.0, the shutter speed was 20 msec, the lighting brightness was 511, and the shading level was 14. The lens aperture was set to 2.8.

[0119] Readability score: The readability score was determined using OCR2 in the XG-X2000 Series Ver. 2.2 application. Ten characters A, B, C, D, E, F, G, H, I, and J (character size: 2.0 mm vertical, 1.5 mm horizontal, 0.5 mm character spacing) of good products with no visibility issues were registered in advance in a rectangular area that fit the characters perfectly, and then the characters laser-marked on each package sample were read. A readability score (a readability score of 99 is optimal) was determined by comparing the registered characters of good products with the characters on the surface of the package.

[0120] (Brightness of non-marking portion) A sealed body was prepared in the same manner as in the laser marking visibility evaluation, and the brightness of the sealed body was measured using the above-mentioned high-speed, high-capacity flexible image processing system manufactured by KEYENCE Co., Ltd. The measurement area was 1.5 mm × 16 mm = 24 mm 2 The test was carried out under the same conditions as the visibility evaluation, except that the brightness was expressed as a value ranging from 0 to 255, with 0 corresponding to the dark side and 255 corresponding to the bright side. The measurement area was divided into sections of 6.48 μm x 6.48 μm, and the brightness of each section was measured. Therefore, the brightness was determined as the brightness distribution within the measurement area. The average value was calculated from the brightness distribution within the obtained measurement area and used as the average brightness. The average brightness of the laser-marked area was 160.

[0121] [Materials Used] (Base Material) ETFE film: An ETFE film was produced using the following ETFE (1) or ETFE (2). The method for producing the ETFE film is described in each example. ETFE (1): Fluon (registered trademark) ETFE C-88AXP (manufactured by AGC) ETFE (2): Fluon (registered trademark) LM-ETFE LM-720AP (manufactured by AGC)

[0122] PMP (polymethylpentene) film: X-88BMT4 manufactured by Mitsui Chemicals Tohcello Co., Ltd., 50 μm thick, double-sided embossed type (the arithmetic mean height Sa of each surface was 2.5 μm and 1.4 μm, respectively). PET (polyethylene terephthalate) film: S-38 (LS) manufactured by Unitika Ltd., a 38 μm thick biaxially stretched polyethylene terephthalate film was used, and a so-called sand matting treatment was performed by spraying sand onto one side of the film to form irregularities. The arithmetic mean height Sa of each surface was 1.6 μm and 0.1 μm, respectively.

[0123] SPS (syndiotactic polystyrene) film: Xarek (registered trademark) 142ZE (manufactured by Idemitsu Kosan Co., Ltd.) was fed into an extruder equipped with a T-die, taken up between mirror-finished metal rolls, and simultaneously stretched in the machine direction and the direction perpendicular to the machine direction to produce a 50 μm thick film. The extruder and T-die temperatures were 270°C, the cooling roll temperature was 100°C, the stretching temperature was 115°C, the stretching ratio was 3.3 times in both the machine direction and the direction perpendicular to the machine direction, and the stretching speed was 500% / min. After the stretching process, the film was heat-treated at 215°C. Furthermore, to create irregularities on one side of the film, a so-called sand matting process was performed by spraying sand onto the film. The arithmetic mean heights Sa of the respective surfaces were 1.9 μm and 0.1 μm.

[0124] For each film, the surface with the higher arithmetic mean height Sa was subjected to corona treatment so that the wetting tension based on ISO 8296: 1987 (JIS K6768: 1999) was 40 mN / m or more. When the arithmetic mean height Sa of both surfaces was the same, corona treatment was applied to one surface.

[0125] (Antistatic Layer Liquid) 10 parts by mass of an acrylic resin-containing polythiophene-based conductive polymer dispersion (ALACOAT (registered trademark) AS601D (solid content 4 mass%, manufactured by Arakawa Chemical Industries, Ltd.)) and 1 part by mass of a polyfunctional aziridine compound curing agent (ALACOAT (registered trademark) CL910 (solid content 10 mass%, manufactured by Arakawa Chemical Industries, Ltd.)) were mixed. The resulting mixture was diluted with a mixed solvent of isopropanol / toluene / water = 50 / 40 / 10 (mass ratio) to obtain the solid content concentration of each example, thereby obtaining an antistatic layer liquid. Note that the surface resistivity of the antistatic layer itself after formation of the antistatic layer described below was 7 × 10 7 It was Ω / □.

[0126] (Release layer liquid) Release layer liquid (1): 100 parts by mass of Nissetsu (registered trademark) KP2562 (manufactured by Nippon Carbide Industries Co., Ltd., solid content 35% by mass, hydroxyl group-containing (meth)acrylic polymer (hydroxyl value 70 mg KOH / g, crosslinking functional group equivalent 801 g / mol)), 6 parts by mass of Nissetsu (registered trademark) CK157 (manufactured by Nippon Carbide Industries Co., Ltd., solid content 100% by mass, trifunctional isocyanate compound (isocyanurate-type hexamentylene diisocyanate)), and 21 parts by mass of Nissetsu (registered trademark) CK-939 (manufactured by Nippon Carbide Industries Co., Ltd., solid content 0.5% by mass, acetylacetone solution of dioctyltin dilaurate) were mixed. The resulting mixture was diluted with ethyl acetate to obtain the solid content concentration of each example, to obtain a release layer liquid.

[0127] Release layer liquid (2-1): 10 parts by mass of Tuftic FH-S005 (manufactured by Toyobo Co., Ltd., product name, acrylic particles, average particle size 5 μm) resin particles were added to the mixture of release layer liquid (1) before dilution with ethyl acetate solvent, and mixed. The mixture was diluted with ethyl acetate to a solids concentration of 26% by mass to obtain a release layer liquid. The content of acrylic particles contained in the release layer formed from this release layer liquid was equivalent to 16.9% by volume. Release layer liquid (2-2): A release layer liquid was obtained using the same procedure as for release layer liquid (2-1), except that the amount of Tuftic FH-S005 was changed to 2 parts by mass. The content of acrylic particles contained in the release layer formed from this release layer liquid was equivalent to 3.9% by volume.

[0128] Release layer liquid (3-1): 10 parts by mass of Sunsphere H-31 (manufactured by AGC Si-Tech Co., Ltd., silica particles, average particle diameter 3 μm) as resin particles were added to the mixture of release layer liquid (1) before dilution with ethyl acetate solvent, and mixed. The mixture was diluted with ethyl acetate to a solids concentration of 20% by mass to obtain a release layer liquid. The content of silica particles contained in the release layer formed from this release layer liquid was equivalent to 11.9% by volume. Release layer liquid (3-2): A release layer liquid was obtained using the same procedure as for release layer liquid (3-1), except that the amount of Sunsphere H-31 (trade name, silica particles, average particle diameter 3 μm, manufactured by AGC Si-Tech Co., Ltd.) was changed to 3.5 parts by mass. The content of silica particles contained in the release layer formed from this release layer liquid was equivalent to 4.5% by volume.

[0129] [Example 1] ETFE (1) was fed into an extruder, and melt-extruded at 320°C using the extruder with the lip opening adjusted so that the film thickness would be 50 μm. The film-forming speed was adjusted using two master rolls with uneven surfaces, and the film was taken up to produce an ETFE film having an uneven structure on both surfaces. The arithmetic mean heights Sa of both surfaces were 2.5 μm and 2.5 μm, respectively. Furthermore, one surface of the ETFE film was subjected to a corona treatment. An antistatic layer solution with a solid content concentration of 4.0 mass% was applied to the corona-treated surface of the ETFE film using a gravure coater, and dried to form an antistatic layer with a thickness of 0.25 μm. Coating was performed by a direct gravure method using a Φ100 mm x 250 mm wide lattice 150#-depth 40 μm roll as a gravure plate, and the coating speed was 4 m / min. Drying was carried out at 100°C for 1 minute, passing through a roll-supported drying oven, and an air flow rate of 15 m / s. A release layer solution (1) with a solids concentration of 13% by mass was applied to the antistatic layer using a gravure coater, and then dried to form a release layer with a thickness of 1.0 μm. Coating was carried out by a direct gravure method, using a Φ100 mm x 250 mm wide grating 150#-depth 40 μm roll as a gravure plate. Drying was carried out at 100°C for 1 minute, passing through a roll-supported drying oven, and an air flow rate of 19 m / s. The film was then aged at 40°C for 120 hours to obtain a release film.

[0130] [Example 2] In the same manner as in Example 1, except that one of the master rolls was changed to adjust the film-forming speed, an ETFE film having an arithmetic mean height Sa of 1.9 μm and 1.3 μm on both surfaces was produced, and the surface with the higher arithmetic mean height Sa was subjected to corona treatment, and further an antistatic layer was formed using an antistatic layer solution with a solid content concentration of 3.2 mass%, to obtain a release film.

[0131] [Example 3] In the same manner as in Example 2, except that ETFE (2) is used as resin, and the film-forming speed is adjusted, an ETFE film having a thickness of 60 μm and an arithmetic mean height Sa of both surfaces of 2.0 μm and 1.4 μm is produced, and the surface of the film having a higher arithmetic mean height Sa is subjected to corona treatment, and further an antistatic layer is formed using an antistatic layer solution with a solid content concentration of 4.0 mass%, and subsequently a release layer is formed using a release layer solution (1) with a solid content concentration of 16 mass%, to obtain a release film.

[0132] [Example 4] In the same manner as in Example 2, except that film-forming speed is adjusted, the ETFE film of which the arithmetic mean height Sa of both surfaces is 1.7 μ m and 1.7 μ m is produced, and the surface that is subjected to corona treatment is formed with the antistatic layer solution of 2.4 mass % solid content, and then the release layer is formed with the release layer solution (1) of 29 mass % solid content, thereby obtaining release film.

[0133] [Example 5] In the same manner as in Example 1, except that one of the master rolls is not used, and the film-forming speed is adjusted, the ETFE film that the arithmetic mean height Sa of both surfaces is 1.6 μm and less than 0.05 μm is produced, and the surface that has the higher arithmetic mean height Sa is subjected to corona treatment, and further, an antistatic layer and a release layer are formed, thereby obtaining a release film.

[0134] Example 6 A release film was obtained in the same manner as in Example 3, except that an antistatic layer liquid having a solid content of 6.9% by mass and a release layer liquid (1) having a solid content of 10% by mass were used.

[0135] Example 7 A release film was obtained in the same manner as in Example 6, except that a release layer liquid (1) having a solid content concentration of 2.6% by mass was used.

[0136] [Example 8] In the same manner as in example 3, except that film-forming speed is adjusted, produce the ETFE film of film thickness 70 μ m, and the arithmetic mean height Sa of both surfaces is 1.4 μ m, 1.0 μ m respectively. The surface of the side with higher arithmetic mean height Sa is subjected to corona treatment, and further, use the antistatic layer solution of solid content concentration 5.0 mass % to form antistatic layer, then use the release layer solution (1) of solid content concentration 2.5 mass % to form release layer, thereby obtain release film.

[0137] Example 9 A release film was obtained in the same manner as in Example 8, except that a release layer liquid (1) having a solid content concentration of 5.6% by mass was used.

[0138] Example 10 A release film was obtained in the same manner as in Example 8, except that a release layer liquid (1) having a solid content concentration of 7.2% by mass was used.

[0139] Example 11 A release film was obtained in the same manner as in Example 1, except that a PMP film was used in place of the ETFE film.

[0140] Example 12 A release film was obtained in the same manner as in Example 1, except that a PET film was used instead of the ETFE film and a release layer liquid (1) having a solid content concentration of 7.8% by mass was used.

[0141] Example 13 A release film was obtained in the same manner as in Example 12, except that an SPS film was used in place of the ETFE film.

[0142] Example 14 A release film was obtained in the same manner as in Example 8, except that an antistatic layer solution having a solid content of 4.2% by mass and a release layer solution (1) having a solid content of 1.3% by mass were used.

[0143] [Example 15] In the same manner as in example 1, but adjust film-forming speed to produce the ETFE film that the arithmetic mean height Sa of both surfaces is 1.6 μ m, 1.6 μ m, respectively, and use the release layer liquid (1) of solid content concentration 31 mass% to obtain release film.

[0144] Example 16 A release film was obtained in the same manner as in Example 3, except that an antistatic layer liquid having a solid content of 6.9% by mass and a release layer liquid (1) having a solid content of 36% by mass were used.

[0145] Example 17 A release film was obtained in the same manner as in Example 8, except that a release layer liquid (1) having a solid content concentration of 31% by mass was used.

[0146] [Example 18] In the same manner as in Example 5, an antistatic layer was formed using an antistatic layer liquid having a solid content concentration of 1.6% by mass, and then a release layer was formed using a release layer liquid (1) having a solid content concentration of 20% by mass, thereby obtaining a release film.

[0147] Example 19 A release film was obtained in the same manner as in Example 8, except that the antistatic layer and the release layer were not formed.

[0148] Example 20 A release film was obtained in the same manner as in Example 1, except that no release layer was formed.

[0149] Example 21 A release film was obtained in the same manner as in Example 3, except that no release layer was formed.

[0150] Example 22 A release film was obtained in the same manner as in Example 8, except that no release layer was formed.

[0151] [Example 23] In the same manner as in Example 5, except that the release layer liquid (2-1) was used instead of the release layer liquid (1), the corona treatment was performed on the surface side having a lower arithmetic mean height Sa, and an antistatic layer and a release layer were further formed to obtain a release film.

[0152] Example 24 A release film was obtained in the same manner as in Example 1, except that the release layer liquid (2-1) was used instead of the release layer liquid (1).

[0153] Example 25 A release film was obtained in the same manner as in Example 1, except that the release layer liquid (2-2) was used instead of the release layer liquid (1).

[0154] Example 26 A release film was obtained in the same manner as in Example 1, except that the release layer liquid (3-1) was used instead of the release layer liquid (1).

[0155] Example 27 A release film was obtained in the same manner as in Example 1, except that the release layer liquid (3-2) was used instead of the release layer liquid (1).

[0156] The release films of Examples 1 to 27, the sealed articles produced using these release films, and the sealed articles that had been laser marked were subjected to the above evaluations. The results are shown in Tables 1 to 3.

[0157]

[0158]

[0159]

[0160] As shown by the above results, the release films of Examples 1 to 13 and 23 to 27, which included a release layer, an antistatic layer, and a substrate, and in which the average thickness of the release layer exceeded 0.1 μm and the abundance fraction (Φ) in the range of 10 to 35° on the surface of the first side was 0.12 or more, had excellent releasability and antistatic properties. Furthermore, the sealed bodies produced using the release films of Examples 1 to 13 and 23 to 27 had surfaces that were excellent in laser marking visibility while suppressing brightness abnormalities due to resin flow marks (flow marks) on the surface of the semiconductor package and scratches on the package surface.

[0161] One characteristic of visibility is that a large difference in the average brightness between the laser-marked and non-marked areas creates contrast, improving visibility. From the above evaluation results, it was found that, from the perspective of increasing contrast, the average brightness of the non-marked areas is preferably 100 or less, and more preferably 95 or less. On the other hand, since a phenomenon occurs in which the brightness of a portion of the non-marked area is high due to traces of resin flow (flow marks) on the package surface or scratches on the package surface, reducing the readability, it was found that the average brightness of the non-marked area is preferably 55 or more, and more preferably 60 or more.

[0162] Although the present invention has been described in detail and with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on a Japanese patent application (Patent Application No. 2023-015583) filed on February 3, 2023, the contents of which are incorporated herein by reference.

[0163] The release film of the present disclosure has excellent semi-antistatic properties and releasability from a semiconductor package, and can form a semiconductor package surface that has excellent laser marking visibility.Using the release film of the present disclosure, a semiconductor package having a surface that has excellent laser marking visibility can be produced.

[0164] DESCRIPTION OF SYMBOLS 1A Bulk sealing body, 10 Substrate, 12 Semiconductor chip (semiconductor element), 19 Cured product, 20 Fixed upper mold, 22 Cavity bottom member, 24 Movable lower mold, 26 Cavity, 30 Release film, 32 Unevenness on surface of release film, 40 Curable resin, 50 Upper mold, 52 Lower mold, 54 Cavity, 56 Cavity surface, 58 Substrate placement section, 60 Resin introduction section, 62 Resin placement section, 64 Plunger

Claims

1. A release film comprising a release layer, an antistatic layer, and a substrate in this order, wherein the average thickness of the release layer exceeds 0.1 μm, and when the irregularities on the surface of the release film on the release layer side are measured with a laser microscope and the surface angle distribution of the angle (θ) between the normal vector of the irregularities and the normal line of the main surface of the release film is calculated, the fraction (Φ) of angles in the range of 10 to 35° is 0.12 or more.

2. The release film according to claim 1, wherein the arithmetic mean height Sa of at least one surface of the substrate is 0.9 μm or more.

3. The release film according to claim 2, wherein the arithmetic mean height Sa of the surface of the substrate on the antistatic layer side is 1.2 μm or more.

4. The release film according to any one of claims 1 to 3, wherein the particle content in the release layer is 25 volume % or less.

5. The release film according to claim 1 or 2, wherein the substrate comprises a fluororesin.

6. The release film according to claim 5, wherein the fluororesin comprises an ethylene-tetrafluoroethylene copolymer.

7. The surface resistivity of the surface on the release layer side is 1×10 7 ~1×10 11 The release film according to claim 1 or 2, having a resistance to deformation (shearing) of Ω / □.

8. The release film according to claim 1 or 2, which is disposed between a curable resin and a surface of a mold in the manufacture of a semiconductor package.

9. The release film according to claim 8, wherein the surface of the release film facing the release layer is in contact with the curable resin.

10. A method for manufacturing a semiconductor package having a semiconductor element and a resin sealing portion formed from a curable resin that seals the semiconductor element, comprising the steps of: placing a substrate having the semiconductor element in a cavity of a mold; placing a release film according to claim 1 or 2, which comprises a release layer, an antistatic layer, and a base material, on a cavity surface of the mold on which the substrate is not placed, with the surface on the release layer side facing the space within the cavity; filling the cavity with the curable resin, and curing the curable resin in contact with the release film to form a resin sealing portion that seals the semiconductor element.