Urethane prepolymer, polyurethane resin raw material, composite material, and method for producing composite material

MYPI2025004513A0Undetermined Publication Date: 2024-09-30MITSUI CHEMICALS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025004513
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-22
Publication Date
2024-09-30

AI Technical Summary

Technical Problem

Conventional composite materials with high lignocellulose water content, typically above 15%, face challenges in achieving adequate water resistance, which affects their performance and durability.

Method used

A urethane prepolymer with an isocyanate group and hydrophilic group, derived from a reaction product of aromatic polyisocyanate, macropolyol, and hydrophilic group-containing compounds, is used to enhance the water resistance of composite materials by improving dispersibility and reactivity, especially when mixed with lignocellulosic materials having high water content.

Benefits of technology

The solution significantly improves the water resistance and physical strength of composite materials, allowing for stable molding and enhanced performance even with high lignocellulose water content, without the need for drying processes, thus improving manufacturing efficiency.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A urethane prepolymer is a reaction product of a polyisocyanate component, a macropolyol component, and a hydrophilic group-containing compound component, and has an isocyanate group and a hydrophilic group. The polyisocyanate component contains an aromatic polyisocyanate; the aromatic polyisocyanate contains at least one kind selected from the group consisting of diphenylmethane diisocyanate and polymethylene polyphenyl polyisocyanate; the macropolyol component contains a polyether polyol having a number average molecular weight of 400 or more and 10,000 or less; and the hydrophilic group-containing compound component contains a compound containing a hydrophilic group and an active hydrogen group having an oxygen atom.
Need to check novelty before this filing date? Find Prior Art

Description

Urethane prepolymer, polyurethane resin raw material, composite material, and method for manufacturing composite material

[0001] The present invention relates to a urethane prepolymer, a polyurethane resin raw material, a composite material, and a method for producing a composite material.

[0002] Conventionally, composite materials have been known that combine an adhesive, which is a mixture of a first agent containing a polyol and a second agent containing an isocyanate compound, with inorganic materials and / or lignocellulose materials (see, for example, Patent Document 1 below).

[0003] JP 2009-19120 A

[0004] In composite materials such as those described in Patent Document 1, there are cases where further improvement in water resistance is required, particularly when the moisture content of the lignocellulose is relatively high (for example, the moisture content of the lignocellulose is 15% or more).

[0005] The object of the present invention is to provide a urethane prepolymer, a polyurethane resin raw material, a composite material having excellent water resistance, and a method for manufacturing a composite material having excellent water resistance even when the moisture content of lignocellulose is high, which can improve the water resistance of the composite material even when the moisture content of the lignocellulose is high.

[0006] The present invention [1] relates to a urethane prepolymer having an isocyanate group and a hydrophilic group, the urethane prepolymer being a reaction product of a polyisocyanate component, a macropolyol component, and a compound component containing a hydrophilic group, the polyisocyanate component containing an aromatic polyisocyanate, the aromatic polyisocyanate containing at least one selected from the group consisting of diphenylmethane diisocyanate and polymethylene polyphenyl polyisocyanate, the macropolyol component containing a polyether polyol having a number average molecular weight of 400 or more and 10,000 or less, and the compound component containing a hydrophilic group containing a compound containing a hydrophilic group and an active hydrogen group having an oxygen atom.

[0007] The present invention [2] includes the urethane prepolymer of the above [1], wherein the content of oxyethylene units in the polyether polyol is 5.0 mass% or less relative to the total amount of oxyalkylene units in the polyether polyol.

[0008] The present invention [3] includes the urethane prepolymer of the above [1] or [2], in which the compound containing the hydrophilic group and the active hydrogen group having an oxygen atom is an alkoxypolyethylene glycol, and the number average molecular weight of the compound containing the hydrophilic group and the active hydrogen group having an oxygen atom is 100 or more and 700 or less.

[0009] The present invention [4] includes a polyurethane resin raw material containing a urethane prepolymer component containing the urethane prepolymer of any one of the above [1] to [3], and a polyol component.

[0010] The present invention [5] comprises the polyurethane resin raw material according to [4] above, wherein the polyol component comprises a first polyol and a second polyol, the first polyol is a polyol that does not contain nitrogen atoms, the first polyol has an average hydroxyl value of 200 mgKOH / g or more and 2,000 mgKOH / g or less, and the number average molecular weight of the first polyol is 50 or more and 1,000 or less, and the second polyol is a polyol that contains nitrogen atoms, the second polyol has an average hydroxyl value of 200 mgKOH / g or more and 2,000 mgKOH / g or less, and the number average molecular weight of the second polyol is 200 or more and 1,000 or less.

[0011] The present invention [6] includes the polyurethane resin raw material according to the above [4] or [5], wherein the urethane prepolymer has an isocyanate group content of 10% by mass or more and further contains a catalyst.

[0012] The present invention [7] includes the polyurethane resin raw material according to any one of the above [4] to [6], which is for a composite material containing a lignocellulose-based material and a polyurethane resin.

[0013] The present invention [8] includes a composite material comprising a lignocellulosic material and a polyurethane resin, wherein the polyurethane resin is a reaction product of any one of the polyurethane resin raw materials described above in [4] to [7].

[0014] The present invention [9] includes a method for producing a composite material containing a lignocellulose-based material and a polyurethane resin, the method comprising a mixing step of mixing a lignocellulose-based material having a moisture content of 15% or more, any one of the polyurethane resin raw materials [4] to [7] above, and water to prepare a composite material composition, and a curing step of curing the composite material composition.

[0015] The present invention

[10] includes the method for producing a composite material according to the above [9], wherein the curing step involves curing the composite material composition by press molding.

[0016] The present invention

[11] includes the method for producing a composite material according to the above [9] or

[10] , wherein the blending ratio of the urethane prepolymer component per 100 parts by mass of the solid content of the lignocellulose-based material in the composite material composition is 5 parts by mass or more and 40 parts by mass or less.

[0017] The present invention

[12] includes the method for producing a composite according to any one of the above [9] to

[11] , wherein the polyol component comprises a first polyol and a second polyol, the first polyol is a polyol that does not contain nitrogen atoms, the first polyol has an average hydroxyl value of 200 mg KOH / g or more and 2,000 mg KOH / g or less, and the number average molecular weight of the first polyol is 50 or more and 1,000 or less, the second polyol is a polyol that contains nitrogen atoms, the second polyol has an average hydroxyl value of 200 mg KOH / g or more and 2,000 mg KOH / g or less, and the number average molecular weight of the second polyol is 200 or more and 1,000 or less, and in the composite composition, the blending ratio of the second polyol per 100 parts by mass of the urethane prepolymer component is 6 parts by mass or more and 20 parts by mass or less.

[0018] The present invention

[13] includes the method for producing a composite material according to any one of the above [9] to

[12] , wherein the isocyanate group content of the urethane prepolymer is 10% by mass or more, the composite material composition further contains a catalyst, and the blending ratio of the catalyst per 100 parts by mass of the urethane prepolymer component is 0.04 parts by mass or more and 1.5 parts by mass or less.

[0019] The present invention provides a urethane prepolymer that can improve the water resistance of a composite material even when the moisture content of the lignocellulose is high, a polyurethane resin raw material, a composite material with excellent water resistance, and a method for manufacturing a composite material with excellent water resistance even when the moisture content of the lignocellulose is high.

[0020] The following description of the components may be based on representative embodiments of the present disclosure, but the present disclosure is not limited to such embodiments.

[0021] In the present disclosure, combinations of preferred aspects are more preferred aspects.

[0022] In the numerical ranges described in stages in this disclosure, the upper limit value (an upper limit value expressed as "not less than" or "greater than") or the lower limit value (an upper limit value expressed as "not more than" or "less than") described in a certain numerical range may be replaced with the upper limit value or the lower limit value of another numerical range described in stages. Furthermore, in the numerical ranges described in this disclosure, the upper limit value or the lower limit value described in a certain numerical range may be replaced with a value shown in the examples.

[0023] In the present disclosure, when a plurality of substances corresponding to each component are present in the composition, the amount of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified.

[0024] 1. Urethane Prepolymer The urethane prepolymer has an isocyanate group and a hydrophilic group. This allows water to be added to the urethane prepolymer in advance to emulsify it when mixing the lignocellulose-based material described below with the first and second parts described below. This reduces the viscosity of the mixture of the lignocellulose-based material described below with the first and second parts described below, improving the formability of the composite material and the water resistance of the composite material.

[0025] From the viewpoint of improving the water resistance of the composite material, the content of isocyanate groups in the urethane prepolymer (isocyanate group content) is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more.

[0026] The isocyanate group content is preferably 45% by mass or less, more preferably 40% by mass or less, and even more preferably 35% by mass or less.

[0027] The isocyanate group content is preferably 5% by mass or more and 45% by mass or less, more preferably 10% by mass or more and 40% by mass or less, and even more preferably 15% by mass or more and 35% by mass or less.

[0028] The isocyanate group content is determined by titration with di-n-butylamine in accordance with the isocyanate group content test described in JIS K7301.

[0029] The hydrophilic group is a substituent that does not react with an isocyanate group. From the viewpoint of obtaining a composite material having excellent water resistance, the hydrophilic group preferably contains a polyethylene glycol group, and more preferably is a polyethylene glycol group.

[0030] The content of hydrophilic groups in the urethane prepolymer (hydrophilic group content) is preferably 0.5% by mass or more, more preferably 0.8% by mass or more, and even more preferably 1.0% by mass or more.

[0031] The hydrophilic group content is preferably 8.0% by mass or less, more preferably 6.0% by mass or less, and even more preferably 5.5% by mass or less.

[0032] The hydrophilic group content is preferably 0.5% by mass or more and 8.0% by mass or less, more preferably 0.8% by mass or more and 6.0% by mass or less, and even more preferably 1.0% by mass or more and 5.5% by mass or less.

[0033] The hydrophilic group content is determined from the charged amount.

[0034] The urethane prepolymer is a reaction product of a polyisocyanate component, a macropolyol component, and a compound component containing a hydrophilic group.

[0035] By reacting the polyisocyanate component with the macropolyol component, the amount of urethane bonds in the urethane prepolymer increases, which improves the physical strength and water resistance of the composite material.

[0036] Furthermore, by reacting a compound having a hydrophilic group, the dispersibility of the urethane prepolymer in lignocellulosic materials with high water content is improved, and its reactivity is also improved. This improves the water resistance and physical strength of the composite material. Furthermore, composite materials with excellent physical strength can be stably molded.

[0037] (1-1) Polyisocyanate Component Examples of the polyisocyanate component include aromatic polyisocyanates that are widely used industrially.

[0038] From the viewpoint of obtaining a composite material having excellent water resistance, examples of aromatic polyisocyanates include tolylene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), phenylene diisocyanate (PDI), naphthalene diisocyanate (NDI), and derivatives thereof.

[0039] Examples of the derivatives include polymers, isocyanurate-modified products, allophanate-modified products, polyol-modified products, biuret-modified products, urea-modified products, oxadiazinetrione-modified products, and carbodiimide-modified products. Examples of the derivatives also include polymethylene polyphenyl polyisocyanate (crude MDI, polymeric MDI).

[0040] The aromatic polyisocyanates can be used alone or in combination of two or more kinds.

[0041] As the aromatic polyisocyanate, from the viewpoint of obtaining a composite material having excellent water resistance and excellent mechanical strength, preferred examples include diphenylmethane diisocyanate (MDI) and polymethylene polyphenyl polyisocyanate. In other words, the aromatic polyisocyanate preferably contains at least one selected from the group consisting of diphenylmethane diisocyanate and polymethylene polyphenyl polyisocyanate. As the aromatic polyisocyanate, particularly preferred is polymethylene polyphenyl polyisocyanate.

[0042] From the viewpoint of obtaining a composite material having excellent water resistance and excellent mechanical strength, the isocyanate group content of the polyisocyanate component is, for example, 15 mass% or more, or preferably 25 mass% or more, relative to the total amount of the polyisocyanate component.

[0043] The isocyanate group content of the polyisocyanate component is, for example, 60% by mass or less, or preferably 50% by mass or less.

[0044] The isocyanate group content of the polyisocyanate component is, for example, 15% by mass or more and 60% by mass or less, or preferably 25% by mass or more and 50% by mass or less.

[0045] (1-2) Macropolyol Component The macropolyol component is a compound having a number average molecular weight of 400 or more and 10,000 or less.

[0046] The number average molecular weight of the macropolyol component is preferably 500 or more, more preferably more than 700, and even more preferably 800 or more, from the viewpoint of obtaining a composite material having excellent water resistance and excellent mechanical strength.

[0047] The number average molecular weight of the macropolyol component is preferably 5,000 or less, more preferably 4,000 or less, and even more preferably 3,500 or less.

[0048] The number average molecular weight of the macropolyol component is preferably 500 or more and 5,000 or less, more preferably more than 700 and 5,000 or less, even more preferably 800 or more and 4,000 or less, and particularly preferably 800 or more and 3,500 or less.

[0049] The number average molecular weight can be calculated from the number of hydroxyl groups in the macropolyol component and the average hydroxyl value (the same applies hereinafter).

[0050] The number of hydroxyl groups in the macropolyol component is preferably 2 or more. Also, preferably 4 or less. The number of hydroxyl groups in the macropolyol component is preferably 2 or more and 4 or less.

[0051] The average hydroxyl value of the macropolyol component is preferably 12 mgKOH / g or more, more preferably 25 mgKOH / g or more, and even more preferably 50 mgKOH / g or more, from the viewpoint of obtaining a composite material having excellent water resistance and excellent mechanical strength.

[0052] The average hydroxyl value of the macropolyol component is preferably 270 mgKOH / g or less, more preferably 200 mgKOH / g or less, and even more preferably 180 mgKOH / g or less.

[0053] The average hydroxyl value of the macropolyol component is preferably 12 mgKOH / g or more and 270 mgKOH / g or less, more preferably 25 mgKOH / g or more and 200 mgKOH / g or less, and even more preferably 50 mgKOH / g or more and 180 mgKOH / g or less.

[0054] The average hydroxyl value is measured in accordance with JIS K1557-1:2007 (the same applies hereinafter).

[0055] As the macropolyol component, from the viewpoint of obtaining a composite material having excellent water resistance and excellent mechanical strength, polyether polyol and polyester polyol are preferred, and polyether polyol is more preferred.

[0056] The polyether polyol is preferably a polyoxyalkylene polyol.

[0057] Examples of polyoxyalkylene polyols include polyalkylene polyols and polytetramethylene ether polyols.

[0058] Examples of polyalkylene polyols include polyethylene glycol, polypropylene glycol, and ethylene oxide-propylene oxide copolymers (random and / or block copolymers).

[0059] Specifically, polyalkylene polyols are produced by addition polymerization of an alkylene oxide having 2 to 4 carbon atoms to an initiator. Examples of initiators include low-molecular-weight diols, low-molecular-weight triols, and low-molecular-weight polyols having 4 or more valences.

[0060] The low molecular weight diol is defined as a diol having a number average molecular weight of not more than 400. Examples of the low molecular weight diol include ethylene glycol and propylene glycol.

[0061] The low molecular weight triol is defined as a triol having a number average molecular weight of not more than 400. Examples of low molecular weight triols include glycerin and trimethylolpropane.

[0062] The tetrahydric or higher low molecular weight polyol is defined as a polyol having a number average molecular weight of 400 or less and having four or more hydroxyl groups.

[0063] Examples of the tetrahydric or higher low molecular weight polyols include pentaerythritol, sorbitol, and sucrose.

[0064] The initiator preferably includes a low molecular weight diol and a low molecular weight triol.

[0065] Examples of alkylene oxides having 2 to 4 carbon atoms include ethylene oxide, propylene oxide, and butylene oxide. Preferably, the alkylene oxide is at least one of an alkylene oxide having 2 carbon atoms (ethylene oxide) and an alkylene oxide having 3 carbon atoms (propylene oxide).

[0066] Examples of polytetramethylene ether polyols include ring-opening polymers obtained by cationic polymerization of tetrahydrofuran, such as amorphous polytetramethylene ether glycols in which a diol is copolymerized with tetrahydrofuran polymerization units, and amorphous polytetramethylene ether glycols in which ethylene oxide, propylene oxide, epichlorohydrin, and / or benzyl glycidyl ether are copolymerized with tetrahydrofuran polymerization units.

[0067] The polyether polyol is preferably a polyalkylene polyol. The polyether polyol is more preferably a polypropylene glycol. Examples of the polypropylene glycol include a bifunctional polypropylene glycol obtained by adding propylene oxide to propylene glycol, a trifunctional polypropylene glycol obtained by adding propylene oxide to glycerin, and a trifunctional polypropylene glycol obtained by adding propylene oxide to trimethylolpropane.

[0068] The content of oxyethylene units in the polyether polyol relative to the total amount of oxyalkylene units in the polyether polyol is preferably 10% by mass or less, more preferably 5.0% by mass or less, and even more preferably 2.0% by mass or less.

[0069] The macro-polyol components described above may be used alone or in combination of two or more. The macro-polyol component may not contain a nitrogen atom.

[0070] (1-3) Compound Component Containing a Hydrophilic Group The compound component containing a hydrophilic group has the above-described hydrophilic group and an active hydrogen group having an oxygen atom. Examples of the active hydrogen group having an oxygen atom include a hydroxyl group and a carboxyl group. The compound component containing a hydrophilic group preferably contains a hydroxyl group, and more preferably contains only a hydroxyl group, as the active hydrogen group having an oxygen atom.

[0071] Examples of the compound component containing a hydrophilic group include the above-mentioned monools having a hydrophilic group and the above-mentioned diols having a hydrophilic group.

[0072] An example of the monool having the hydrophilic group is alkoxypolyethylene glycol, where the alkoxy group is composed of an alkyl group having 1 to 6 carbon atoms and an oxygen atom.

[0073] Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, a cyclopropyl group, an n-butyl group, an isobutyl group, an s-butyl group, a t-butyl group, a cyclobutyl group, an n-pentyl group, an isopentyl group, a 2-methylbutyl group, a neopentyl group, a 1-ethylpropyl group, a cyclopentyl group, an n-hexyl group, a 4-methylpentyl group, a 3-methylpentyl group, a 2-methylpentyl group, a 1-methylpentyl group, a 3,3-dimethylbutyl group, a 2,2-dimethylbutyl group, a 1,1-dimethylbutyl group, a 1,2-dimethylbutyl group, a 1,3-dimethylbutyl group, a 2,3-dimethylbutyl group, a 2-ethylbutyl group, and a cyclohexyl group.

[0074] An example of the diol having a hydrophilic group is polyethylene glycol.

[0075] As the compound component containing a hydrophilic group, preferably, the above-mentioned monool having a hydrophilic group is used, and more preferably, methoxypolyethylene glycol is used.

[0076] When the compound component containing a hydrophilic group is methoxypolyethylene glycol, the number average molecular weight of the methoxypolyethylene glycol is preferably 50 or more, more preferably 100 or more, and even more preferably 300 or more, from the viewpoint of improving the water resistance of the composite material.

[0077] The number average molecular weight of the methoxypolyethylene glycol is preferably 2,000 or less, more preferably 1,000 or less, and more preferably 700 or less.

[0078] The number average molecular weight of the methoxypolyethylene glycol is preferably 50 or more and 2,000 or less, more preferably 100 or more and 1,000 or less, even more preferably 100 or more and 700 or less, and particularly preferably 300 or more and 700 or less.

[0079] (1-4) Method for Producing Urethane Prepolymer To produce a urethane prepolymer, an aromatic polyisocyanate, a macropolyol component, and a compound component containing a hydrophilic group are mixed so that the isocyanate index (the ratio of the isocyanate group concentration (NCO concentration) of the polyisocyanate to the active hydrogen group concentration of the macropolyol component and the compound component containing a hydrophilic group multiplied by 100, NCO concentration / active hydrogen group concentration × 100) is, for example, greater than 100, preferably 105 or more, for example, 600 or less, preferably 450 or less, and they are reacted until a predetermined isocyanate group content is reached.

[0080] In this reaction, a urethanization catalyst can be added as needed.

[0081] After the reaction, if necessary, residual monomers (specifically, unreacted polyisocyanate) may be removed using a known distillation method or the like.

[0082] This makes it possible to obtain a urethane prepolymer having an isocyanate group and a hydrophilic group.

[0083] (1-5) Composition of Urethane Prepolymer From the viewpoint of emulsification when water is added, the ratio of the total mass of the polyisocyanate component to the total mass of the polyisocyanate component, the macropolyol component, and the compound component containing a hydrophilic group is preferably 0.38 or more and 0.80 or less, more preferably 0.40 or more and 0.75 or less, and even more preferably 0.45 or more and 0.70 or less.

[0084] From the viewpoint of emulsifying when water is added, the ratio of the total mass of the macropolyol component to the total mass of the polyisocyanate component, the macropolyol component, and the compound component containing a hydrophilic group is preferably 0.15 or more and 0.59 or less, more preferably 0.20 or more and 0.55 or less, and even more preferably 0.25 or more and 0.50 or less.

[0085] The ratio of the total mass of the compound component containing a hydrophilic group to the total mass of the polyisocyanate component, the macropolyol component, and the compound component containing a hydrophilic group is preferably 0.01 or more and 0.05 or less, from the viewpoint of emulsification when water is added.

[0086] 2. Polyurethane Resin Raw Material The polyurethane resin raw material contains a urethane prepolymer component containing the above-mentioned urethane prepolymer, and a polyol component.

[0087] (2-1) Polyol Component From the viewpoint of obtaining a composite material having excellent water resistance, the polyol component preferably contains a first polyol and a second polyol.

[0088] (2-1-1) First Polyol The number of functional groups of the first polyol is preferably 1 or more, more preferably 2 or more. The number of functional groups of the first polyol is preferably 4 or less, more preferably 3 or less. The number of functional groups of the first polyol is preferably 1 or more and 4 or less, more preferably 2 or more and 3 or less.

[0089] The number average molecular weight of the first polyol is preferably 50 or more, and more preferably 62 or more, from the viewpoint of improving the water resistance and physical strength of the composite material.

[0090] The number average molecular weight of the first polyol is preferably 1,000 or less, and more preferably 800 or less, from the viewpoint of improving the physical strength of the composite material.

[0091] The number average molecular weight of the first polyol is preferably 50 or more and 1,000 or less, and more preferably 62 or more and 800 or less, from the viewpoint of improving the water resistance and physical strength of the composite material.

[0092] The average hydroxyl value of the first polyol is, for example, 200 mgKOH / g or more, or preferably 300 mgKOH / g or more.

[0093] The average hydroxyl value of the first polyol is, for example, 2000 mgKOH / g or less, or preferably 1900 mgKOH / g or less.

[0094] The average hydroxyl value of the first polyol is preferably 200 mgKOH / g or more and 2000 mgKOH / g or less, and more preferably 300 mgKOH / g or more and 1900 mgKOH / g or less.

[0095] The first polyol can be obtained by a conventional polyol production method. The production method is not particularly limited, and the first polyol can be produced by adding a cyclic ether to a compound (polyhydric alcohol) having a hydroxyl group.

[0096] As the first polyol, a compound having a hydroxyl group (polyhydric alcohol) or a polyether polyol to which one or more cyclic ethers have been added can also be used.

[0097] Examples of compounds having a hydroxyl group (polyhydric alcohols) include ethylene glycol, diethylene glycol, propylene glycol, pentaerythritol, trimethylolpropane, glycerin, diglycerin, sorbitol, polypropylene glycol, diethylene glycol, polyethylene glycol, butylene glycol, hexanetriol, sucrose, butylene glycol, dihydroxydiphenylpropane, sucrose, dipropylene glycol, dihydroxydiphenylpropane, dihydroxydiphenyl ether, dihydroxydiphenylmethane, dihydroxybiphenyl, hydroquinone, naphthalenediol, resorcinol, and fluoroglycine.

[0098] As the compound having a hydroxyl group (polyhydric alcohol), from the viewpoints of reactivity with the urethane prepolymer component and adhesiveness, preferred examples include glycerin and diglycerin.

[0099] Examples of cyclic ethers include ethylene oxide, propylene oxide, styrene oxide, and butylene oxide.

[0100] As the cyclic ether, from the viewpoint of reactivity with the urethane prepolymer component and adhesiveness, preferred examples include ethylene oxide and propylene oxide.

[0101] Specific examples of the first polyol include a bifunctional polypropylene glycol in which propylene oxide is added to propylene glycol, a trifunctional polypropylene glycol in which propylene oxide is added to glycerin, and a trifunctional polypropylene glycol in which propylene oxide is added to trimethylolpropane.

[0102] The first polyol preferably does not contain a nitrogen atom. When molding a composite material, the amount of urethane bonds can be further increased by reacting a first polyol that does not contain a nitrogen atom with a urethane prepolymer. This can improve the physical strength and water resistance of the composite material. As a result, a composite material with excellent water resistance and physical strength can be stably molded.

[0103] (2-1-2) Second Polyol The number of functional groups of the second polyol is preferably 1 or more, more preferably 2 or more. The number of functional groups of the second polyol is preferably 6 or less, more preferably 5 or less. The number of functional groups of the second polyol is preferably 1 or more and 6 or less, more preferably 2 or more and 5 or less.

[0104] The number average molecular weight of the second polyol is preferably 200 or more, more preferably 230 or more, and even more preferably 260 or more.

[0105] The number average molecular weight of the second polyol is preferably 1,000 or less, more preferably 950 or less, and even more preferably 900 or less.

[0106] The number average molecular weight of the second polyol is preferably 200 or more and 1,000 or less, more preferably 230 or more and 950 or less, and even more preferably 260 or more and 900 or less.

[0107] The average hydroxyl value of the second polyol is, for example, 200 mgKOH / g or more, or preferably 250 mgKOH / g or more.

[0108] The average hydroxyl value of the second polyol is, for example, 2000 mgKOH / g or less, or preferably 1000 mgKOH / g or less.

[0109] The average hydroxyl value of the second polyol is, for example, 200 mgKOH / g or more and 2000 mgKOH / g or less, and preferably 250 mgKOH / g or more and 1000 mgKOH / g or less.

[0110] The second polyol is preferably a polyether polyol. The second polyol preferably contains nitrogen atoms. The nitrogen-containing second polyol has higher reactivity with urethane prepolymers than the nitrogen-free first polyol. Therefore, when molding a composite, urethane bonds can be rapidly formed between the urethane prepolymer and the nitrogen-containing second polyol by reacting the urethane prepolymer with the nitrogen-containing second polyol. As a result, the water resistance and physical strength of the composite can be improved, and a composite with excellent water resistance and physical strength can be stably molded. Furthermore, the reactivity can be adjusted by adjusting the amount of the second polyol added.

[0111] The second polyol can be obtained by a conventional polyol production method, for example, by addition polymerization of an alkylene oxide with an initiator.

[0112] Examples of initiators include ethanolamines and amines. Examples of ethanolamines include monoethanolamine, diethanolamine, and triethanolamine. Examples of amines include ethylenediamine, diethylenetriamine, orthotolylenediamine, metatolylenediamine, 4,4'-diphenylmethanediamine, 2,4'-diphenylmethanediamine, polymethylpolyphenylpolyamine, and aniline.

[0113] As the initiator, from the viewpoint of improving the mechanical properties and water resistance of the composite material, preferably, monoethanolamine, diethanolamine, triethanolamine, ethylenediamine, diethylenetriamine, metatolylenediamine, polymethylpolyphenylpolyamine, and aniline are used, more preferably, diethanolamine, triethanolamine, ethylenediamine, diethylenetriamine, and aniline are used, and even more preferably, triethanolamine, ethylenediamine, and diethylenetriamine are used.

[0114] Alkylene oxides include, for example, ethylene oxide, propylene oxide, and butylene oxide.

[0115] Specific examples of the second polyol include trifunctional polypropylene glycol obtained by adding propylene oxide to triethanolamine, and tetrafunctional polypropylene glycol obtained by adding propylene oxide to ethylenediamine.

[0116] The second polyol may be used alone or in combination of two or more.

[0117] (2-2) Catalyst The polyurethane resin raw material preferably further contains a catalyst when the isocyanate group content of the urethane prepolymer is 10% by mass or more. When the isocyanate group content of the urethane prepolymer is less than 10% by mass, the polyurethane resin raw material does not need to contain a catalyst.

[0118] Examples of the catalyst include known urethane catalysts, more specifically known amine catalysts and known organometallic catalysts.

[0119] Examples of amine catalysts include tertiary amine catalysts, quaternary ammonium salts, and imidazoles. Examples of tertiary amine catalysts include triethylamine, dimethylcyclohexylamine (DMCHA), dimethylethanolamine (DMEA), triethanolamine (TEA), triethylenediamine, bis-(2-dimethylaminoethyl)ether, and N-methylmorpholine. Examples of quaternary ammonium salts include tetraethylhydroxylammonium. Examples of imidazoles include imidazole and 2-ethyl-4-methylimidazole.

[0120] Examples of organometallic catalysts include organotin compounds, organolead compounds, organonickel compounds, organocobalt compounds, organocopper compounds, and organobismuth compounds. Examples of organotin compounds include tin acetate, tin octoate (stannous octoate), tin oleate, tin laurate, dibutyltin diacetate, dimethyltin dilaurate, dibutyltin dilaurate, dibutyltin dimercaptide, dibutyltin maleate, dibutyltin dineodecanoate, dioctyltin dimercaptide, dioctyltin dilaurate, and dibutyltin dichloride. Examples of organolead compounds include lead octoate and lead naphthenate. Examples of organonickel compounds include nickel naphthenate. Examples of organocobalt compounds include cobalt naphthenate. Examples of organocopper compounds include copper octenate. Examples of organic bismuth compounds include bismuth octanoate (bismuth octylate) and bismuth neodecanoate.

[0121] The catalysts can be used alone or in combination of two or more kinds.

[0122] As the catalyst, from the viewpoint of improving the water resistance and various strengths of the composite material, preferably, an amine catalyst is used, more preferably, a tertiary amine catalyst is used, and even more preferably, dimethylcyclohexylamine, dimethylethanolamine, or triethanolamine is used.

[0123] The catalyst content per 100 parts by mass of the polyol component is, for example, 0.1% by mass or more, preferably 0.5% by mass or more, more preferably 1% by mass or more, and for example, 10% by mass or less, preferably 9% by mass or less, more preferably 8% by mass or less.

[0124] The catalyst content per 100 parts by mass of the polyol component is, for example, 0.1% by mass to 10% by mass, preferably 0.5% by mass to 9% by mass, and more preferably 1% by mass to 8% by mass.

[0125] When the blending ratio of the catalyst to 100 parts by mass of the polyol component is equal to or greater than the above lower limit and equal to or less than the above upper limit, the curing time of the composite material composition described below can be adjusted within an appropriate range, improving workability and productivity, and ensuring the water resistance and physical strength of the composite material.

[0126] The blending ratio of the catalyst to 100 parts by mass of the second polyol is, for example, 0.1 parts by mass or more, preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and for example, 12 parts by mass or less, preferably 10 parts by mass or less, more preferably 9 parts by mass or less.

[0127] The catalyst blending ratio relative to 100 parts by mass of the second polyol is, for example, 0.1 parts by mass or more and 12 parts by mass or less, preferably 0.5 parts by mass or more and 10 parts by mass or less, and more preferably 1 part by mass or more and 9 parts by mass or less.

[0128] When the blending ratio of the catalyst to 100 parts by mass of the second polyol is equal to or greater than the above lower limit and equal to or less than the above upper limit, the curing time of the composite material composition described below can be adjusted within an appropriate range, improving workability and productivity, and ensuring the water resistance and physical strength of the composite material.

[0129] (2-3) Formulation of Polyurethane Resin Raw Material It is preferable that the polyurethane resin raw material is used in the form of a first part and a second part, which are separated.

[0130] (2-3-1) First Agent The first agent contains the above-mentioned urethane prepolymer component.

[0131] In this case, the urethane prepolymer component contains a urethane prepolymer. The urethane prepolymer component may contain a residual isocyanate monomer. The residual isocyanate monomer is an isocyanate monomer that remains unreacted among the isocyanate monomers used in the production of the prepolymer. Preferably, the urethane prepolymer component consists solely of a urethane prepolymer.

[0132] The proportion of the urethane prepolymer component in the first agent is, for example, 95% by mass or more, preferably 99% by mass or more, and more preferably 100% by mass.

[0133] (2-3-2) Second Agent The second agent contains a polyol component. The second agent optionally contains a catalyst. In other words, the polyurethane resin raw material contains a polyol component and optionally contains a catalyst.

[0134] The proportion of the first polyol in the second agent is, for example, 1 mass % or more, preferably 2 mass % or more, more preferably 10 mass % or more, and preferably 15 mass % or more.

[0135] The proportion of the first polyol in the second agent is, for example, 35% by mass or less, preferably 30% by mass or less, more preferably 25% by mass or less, and even more preferably 20% by mass or less.

[0136] The proportion of the first polyol in the second agent is, for example, 1% by mass or more and 35% by mass or less, preferably 2% by mass or more and 30% by mass or less, more preferably 10% by mass or more and 25% by mass or less, and even more preferably 15% by mass or more and 20% by mass or less.

[0137] When the ratio of the first polyol in the second part is equal to or greater than the above lower limit and equal to or less than the above upper limit, the curing time of the composite material composition described below can be adjusted within an appropriate range, improving workability and productivity, and ensuring the water resistance and physical strength of the composite material.

[0138] The proportion of the second polyol in the second agent is, for example, 65 mass% or more, preferably 69 mass% or more, and preferably 75 mass% or more.

[0139] The proportion of the second polyol in the second agent is, for example, 97% by mass or less, preferably 96% by mass or less, and preferably 95% by mass or less.

[0140] The proportion of the second polyol in the second agent is, for example, 65% by mass or more and 97% by mass or less, preferably 69% by mass or more and 96% by mass or less, and preferably 75% by mass or more and 95% by mass or less.

[0141] When the proportion of the second polyol in the second part is equal to or greater than the above lower limit and equal to or less than the above upper limit, the curing time of the composite material composition described below can be adjusted within an appropriate range, improving workability and ensuring the water resistance and physical strength of the composite material.

[0142] In the second agent, the blending ratio of the first polyol relative to 100 parts by mass of the second polyol is, for example, 1 part by mass or more, preferably 2 parts by mass or more, more preferably 10 parts by mass or more, and more preferably 15 parts by mass or more.

[0143] The mixing ratio of the first polyol relative to 100 parts by mass of the second polyol is, for example, 45 parts by mass or less, preferably 40 parts by mass or less, more preferably 30 parts by mass or less, and more preferably 20 parts by mass or less.

[0144] The blending ratio of the first polyol to 100 parts by mass of the second polyol is, for example, 1 part by mass or more and 45 parts by mass or less, preferably 2 parts by mass or more and 40 parts by mass or less, more preferably 10 parts by mass or more and 30 parts by mass or less, and more preferably 15 parts by mass or more and 20 parts by mass or less.

[0145] When the blending ratio of the first polyol to 100 parts by mass of the second polyol is equal to or greater than the above lower limit and equal to or less than the above upper limit, the curing time of the composite material composition described below can be adjusted within an appropriate range, improving workability and productivity, and ensuring the water resistance and physical strength of the composite material.

[0146] The proportion of the catalyst in the second agent is, for example, 0.1 mass % or more, preferably 0.2 mass % or more, and preferably 0.3 mass % or more.

[0147] The proportion of the catalyst in the second agent is, for example, 10 mass % or less, preferably 7 mass % or less, and more preferably 5 mass % or less.

[0148] The proportion of the catalyst in the second agent is, for example, 0.1 mass % or more and 10 mass % or less, preferably 0.2 mass % or more and 7 mass % or less, and preferably 0.3 mass % or more and 5 mass % or less.

[0149] When the proportion of the catalyst in the second part is equal to or greater than the lower limit and equal to or less than the upper limit, the curing time of the composite material composition described below can be adjusted within an appropriate range, improving workability and productivity, and ensuring the water resistance and physical strength of the composite material.

[0150] The second agent may contain other components such as a solvent or dispersion medium, additives, etc. as needed. Examples of other components include ultraviolet absorbers, antioxidants, plasticizers, silane coupling agents, water repellents, antifoaming agents, curing accelerators, release agents, release aids, tackifiers, formaldehyde catcher agents, crosslinking agents, stabilizers, etc. The other components are not particularly limited, but may be used in an amount of 5 parts by mass or less per 100 parts by mass of the total of the second agent.

[0151] (2-4) Uses of polyurethane resin raw material The polyurethane resin raw material can be used as a raw material for producing a composite material of a lignocellulosic material and a polyurethane resin.

[0152] 3. Composite Material The composite material includes a lignocellulosic material and a polyurethane resin, which is a reaction product of the polyurethane resin raw materials described above.

[0153] (3-1) Lignocellulose-Based Materials Examples of lignocellulose-based materials include ground wood, ground bark, ground bamboo, and plants. Note that "wood" refers to the woody part and does not include bark, which is the bark of trees. Examples of ground wood include wood chips. Examples of ground bark include bark chips. Examples of ground bamboo include bamboo chips. The type of wood is not limited. The tree may be a coniferous tree or a broad-leaved tree. Examples of coniferous trees include cedar and cypress. Examples of broad-leaved trees include beech and boxwood.

[0154] Examples of plants include Ericaceae, Orchidaceae, Poaceae, Araceae, Solanaceae, Fabaceae, Araliaceae, Asteraceae, Lamiaceae, Theaceae, Chenopodiaceae, Brassicaceae, Cucurbitaceae, Zingiberaceae, Nymphaeaceae, Apiaceae, Polygonaceae, Rosaceae, Liliaceae, Convolvulaceae, Iridaceae, Gesneriaceae, Ranunculaceae, Apocynaceae, Papaveraceae, Piperaceae, Scrophulariaceae, Examples of plants in the Poaceae family include rice, barley, wheat, sorghum, sorghum, sorghum, sorghum, sorghum, sorghum, millet, sorghum, foxtail millet, common millet, foxtail millet, common reed, barnyard millet, sugar cane, and corn. Examples of plants in the Asteraceae family include sunflower, mugwort, butterbur, lily of the valley, and dahlia. Examples of plants in the Cucurbitaceae family include cucumber, melon, pumpkin, gourd, wax gourd, bottle gourd, watermelon, and bottle gourd. Examples of plants in the Nymphaeaceae family include water lilies, lotus flowers, giant lotus flowers, and water lilies. Examples of plants in the Convolvulaceae family include bindweed, sweet potatoes, morning glories, and night glories. Examples of plants in the Iridaceae family include irises, Japanese iris, calamus, Japanese iris, and gladioli. Examples of plants in the Palmaceae family include coconut palms.

[0155] Lignocellulosic materials preferably include ground wood, ground bark, and plants. The ground wood is more preferably ground cedar, and the ground bark is more preferably ground cedar bark. When the lignocellulosic material is cedar, a composite material having antibacterial and herbicidal effects can be produced.

[0156] The moisture content of the lignocellulosic material is not limited, and may be 15% or more, 20% or more, 25% or more, 30% or more, 35% or more, or 40% or more.

[0157] In the present invention, even when the lignocellulose material has a relatively high moisture content, by using the polyurethane resin composition of the present invention, a composite material can be produced without undergoing a drying step for the lignocellulose material.

[0158] The moisture content of the lignocellulosic material may be, for example, 60% or less, or 50% or less.

[0159] When the moisture content of the lignocellulose material is equal to or less than the upper limit, the molding time (curing time) can be prevented from becoming long, and production efficiency can be improved.

[0160] The moisture content of the lignocellulosic material may be 15% or more and 60% or less, 20% or more and 60% or less, 30% or more and 50% or less, 35% or more and 50% or less, or 40% or more and 50% or less.

[0161] (3-2) Physical Properties of Composite Material Next, the physical properties of the composite material will be explained.

[0162] (3-2-1) Thickness of Composite Material The thickness of the composite material is not limited. The thickness of the composite material may be 14.5 mm or more, or 14.9 mm or more. The thickness of the composite material may be 15.5 mm or less, or 15.1 mm or less. The thickness of the composite material may be 14.5 mm or more and 15.5 mm or less, or 14.9 mm or more and 15.1 mm or less.

[0163] The thickness of the composite material is measured according to the dimensional measurement method specified in JIS A5908:2015 (particle board).

[0164] The thickness of the composite material can be adjusted to fall within the above range, for example, by using a thickness adjusting bar during the curing step described below.

[0165] (3-2-2) Density of the composite material The density of the composite material is not limited. The density of the composite material is 440 kg / m 3 or more, 445 kg / m 3 The density of the composite material may be 465 kg / m or more. 3 or less, 460 kg / m 3 The density of the composite may be 440 kg / m or less. 3 More than 465kg / m 3 or less, 445 kg / m 3 More than 460kg / m 3 It may be the following:

[0166] The density of the composite material is measured by the density test specified in JIS A5908:2015 (particle board).

[0167] To adjust the density of the composite material to fall within the above range, for example, the mass of the composite material after molding is calculated from the set density and size (length, width, thickness) of the composite material during the curing step described below, and the mass of the composite material composition is adjusted so that the composite material after molding has the calculated mass.

[0168] (3-2-3) Bending strength of composite material The bending strength of the composite material is, for example, preferably 12 N / mm 2 More preferably, 14 N / mm 2 More preferably, 17 N / mm 2 More preferably, 19 N / mm 2 More preferably, 23 N / mm 2 The upper limit is not particularly limited, but may be, for example, 40 N / mm 2 It may be the following:

[0169] The bending strength of the composite material is measured by the bending strength test of JIS A5908:2015 (particle board).

[0170] To adjust the flexural strength of the composite material within the above range, for example, at least one of the density of the composite material and the ratio of the first part to the second part is adjusted. Increasing the density of the composite material can increase the flexural strength. Increasing the ratio of the first part to the second part can increase the flexural strength of the composite material and improve its water resistance. Therefore, the flexural strength of the composite material can be adjusted by adjusting at least one of the density and the ratio of the first part to the second part depending on the intended use.

[0171] (3-2-4) Wet B bending strength of composite material The wet B bending strength of the composite material is, for example, 8 N / mm 2 More than 10 N / mm 2 More preferably, 15 N / mm 2 or more, for example, 30 N / mm 2 The following is the result.

[0172] The wet flexural strength B of the composite material is measured according to the wet flexural strength B test of JIS A5908:2015 (particle board).

[0173] To adjust the wet B bending strength of the composite material within the above range, for example, at least one of the density of the composite material and the ratio of the first part to the second part is adjusted. The wet B bending strength can be increased by increasing the density of the composite material. Increasing the ratio of the first part to the second part can increase the wet B bending strength of the composite material and improve its water resistance. Therefore, the wet B bending strength of the composite material can be adjusted by adjusting at least one of the density and the ratio of the first part to the second part depending on the intended use.

[0174] (3-2-5) Flexural Survivability of Composite Material The flexural survival rate is the percentage of the wet B flexural strength relative to the flexural strength.

[0175] The P-type conformance condition specified in JIS A5908:2015 (particle board) is that the bending survival rate is 49.5% or more (50% or more when rounded to the first decimal place).

[0176] The bending survival rate of the composite material is, for example, 49.5% or more, preferably 50% or more, more preferably 55% or more, more preferably 60% or more, more preferably 65% ​​or more, and for example, 70% or less.

[0177] To adjust the bending survival rate of the composite material within the above range, for example, at least one of the density of the composite material and the ratio of the first part to the second part is adjusted. The bending survival rate can be increased by increasing the density of the composite material. Increasing the ratio of the first part to the second part can increase the bending survival rate of the composite material and improve its water resistance. Therefore, the bending survival rate of the composite material can be adjusted by adjusting at least one of the density and the ratio of the first part to the second part depending on the intended use.

[0178] (3-2-6) 20°C water absorption thickness expansion rate of composite material A 20°C water absorption thickness expansion rate of 12% or more is a conformity condition for P type specified in JIS A5908:2015 (particle board).

[0179] The composite has a water absorption thickness swelling rate at 20°C of, for example, 12% or less, preferably 9% or less, more preferably 7% or less, more preferably 5% or less, and for example, 1% or more.

[0180] The 20°C water absorption thickness swelling rate of the composite material is measured according to the water absorption thickness swelling rate test of JIS A5908:2015 (particle board).

[0181] To adjust the 20°C water absorption thickness swelling coefficient of the composite material within the above range, for example, at least one of the density of the composite material and the ratio of the first part to the second part is adjusted. Increasing the density of the composite material can increase the 20°C water absorption thickness swelling coefficient. Increasing the ratio of the first part to the second part can increase the 20°C water absorption thickness swelling coefficient of the composite material and improve its water resistance. Therefore, the 20°C water absorption thickness swelling coefficient of the composite material can be adjusted by adjusting at least one of the density and the ratio of the first part to the second part depending on the intended use.

[0182] (3-3) Uses of Composite Materials Examples of composite materials include boards, such as wood boards, particle boards, and fiberboards.

[0183] The composites can be used, for example, for ground paving, sidewalks, highway walls, residential perimeters, furniture, interior wall coverings, interior flooring, and subfloor coverings.

[0184] 4. Method for Producing Composite Material The method for producing a composite material uses the polyurethane resin raw material described above and includes a mixing step and a curing step.

[0185] (4-1) Mixing Step In the mixing step, a lignocellulose-based material having a moisture content of 15% or more, the polyurethane resin raw material described above, and water are mixed to prepare a composite composition. When the polyurethane resin raw material is separated into a first part and a second part, in the mixing step, the lignocellulose-based material having a moisture content of 15% or more, the first part, the second part, and water are mixed to prepare a composite composition. In other words, in the mixing step, a lignocellulose-based material having a moisture content of 15% or more, a urethane prepolymer component, a polyol component, water, and, if necessary, a catalyst are mixed to prepare a composite composition.

[0186] The preferred range of the moisture content of the lignocellulosic material used as the raw material is as described above.

[0187] The method for mixing the lignocellulosic material, the first agent, the second agent, and water is not limited. For example, the first agent and water may be mixed to prepare a first mixed liquid, the second agent and water may be mixed to prepare a second mixed liquid, and the first mixed liquid and the second mixed liquid may be mixed with the lignocellulosic material to prepare the composite composition. Alternatively, the first agent, the second agent, and water may be mixed to prepare a mixed liquid, and the resulting mixed liquid may be mixed with the lignocellulosic material.

[0188] In the composite material composition, the mixing ratio of the urethane prepolymer component per 100 parts by mass of the solid content of the lignocellulose material is, for example, 5 parts by mass or more, or preferably 10 parts by mass or more.

[0189] When the blending ratio of the urethane prepolymer component relative to 100 parts by mass of the solid content of the lignocellulose material is equal to or greater than the above lower limit, the normal bending strength and wet B bending strength can be improved.

[0190] In the composite material composition, the blending ratio of the urethane prepolymer component per 100 parts by mass of the solid content of the lignocellulose material is, for example, 40 parts by mass or less, preferably 25 parts by mass or less, and more preferably 15 parts by mass or less.

[0191] When the blending ratio of the urethane prepolymer component to 100 parts by mass of the solid content of the lignocellulose material is equal to or less than the upper limit, the water resistance and physical strength of the composite material can be ensured while suppressing increases in production costs.

[0192] In the composite material composition, the blending ratio of the urethane prepolymer component per 100 parts by mass of the solid content of the lignocellulose-based material is, for example, 5 parts by mass or more and 40 parts by mass or less, preferably 10 parts by mass or more and 25 parts by mass or less, and more preferably 10 parts by mass or more and 15 parts by mass or less.

[0193] In the composite material composition, the mixing ratio of the first polyol relative to 100 parts by mass of the urethane prepolymer component is, for example, 0.1 parts by mass or more, preferably 0.3 parts by mass or more.

[0194] In the composite material composition, the mixing ratio of the first polyol per 100 parts by mass of the urethane prepolymer component is, for example, 5 parts by mass or less, or preferably 4.7 parts by mass or less.

[0195] In the composite material composition, the mixing ratio of the first polyol relative to 100 parts by mass of the urethane prepolymer component is, for example, 0.1 parts by mass or more and 5 parts by mass or less, preferably 0.3 parts by mass or more and 4.7 parts by mass or less.

[0196] When the blending ratio of the first polyol to 100 parts by mass of the urethane prepolymer component is within the above range, a decrease in bending retention can be suppressed, and an increase in the 20°C water absorption thickness expansion rate can be suppressed.

[0197] In the composite material composition, the mixing ratio of the second polyol per 100 parts by mass of the urethane prepolymer component is, for example, 6 parts by mass or more, or preferably 8 parts by mass or more.

[0198] In the composite material composition, the mixing ratio of the second polyol per 100 parts by mass of the urethane prepolymer component is, for example, not more than 20 parts by mass, or preferably not more than 15.5 parts by mass.

[0199] In the composite material composition, the mixing ratio of the second polyol relative to 100 parts by mass of the urethane prepolymer component is, for example, 6 parts by mass or more and 20 parts by mass or less, preferably 8 parts by mass or more and 15.5 parts by mass or less.

[0200] When the blending ratio of the second polyol to 100 parts by mass of the urethane prepolymer component is within the above range, a decrease in bending retention can be suppressed, and an increase in the 20°C water absorption thickness expansion rate can be suppressed.

[0201] In the composite material composition, the blending ratio of the catalyst relative to 100 parts by mass of the urethane prepolymer component is, for example, 0.01 part by mass or more, or preferably 0.04 part by mass or more.

[0202] In the composite material composition, the blending ratio of the catalyst per 100 parts by mass of the urethane prepolymer component is, for example, 1.5 parts by mass or less, or preferably 1.2 parts by mass or less.

[0203] In the composite material composition, the proportion of catalyst per 100 parts by mass of the urethane prepolymer component is, for example, 0.01 parts by mass or more and 1.5 parts by mass or less, preferably 0.04 parts by mass or more and 1.5 parts by mass or less, and more preferably 0.04 parts by mass or more and 1.2 parts by mass or less.

[0204] When the blending ratio of the catalyst to 100 parts by mass of the urethane prepolymer component is within the above range, a decrease in bending retention can be suppressed, and an increase in the 20°C water absorption thickness expansion rate can be suppressed.

[0205] (4-2) Curing Step Next, in the curing step, the composite material composition is cured. The curing method is not particularly limited, but from the viewpoint of obtaining a composite material having excellent water resistance and improving the strength of the composite material, it is preferable to cure the composite material composition by press molding.

[0206] Specifically, the composite material composition is formed (uniformly spread) on a coal board or in a press molding die, and heated and pressurized at a pressure of, for example, 2 MPa or more and 5 MPa or less and at a temperature of, for example, 20°C or more and 180°C or less for, for example, 5 minutes or more and 80 minutes or less.

[0207] This allows the composite material composition to be cured to obtain a composite material.

[0208] 5. Effects and Benefits (1) According to the polyurethane resin raw material, the urethane prepolymer is a reaction product of an aromatic polyisocyanate, a macropolyol component, and a compound component containing a hydrophilic group, and has an isocyanate group and a hydrophilic group.

[0209] Therefore, when mixing the lignocellulose-based material with the urethane prepolymer, the urethane prepolymer can be dispersed in water, allowing the lignocellulose-based material and the urethane prepolymer to be mixed uniformly.

[0210] As a result, the water resistance of the resulting composite material can be improved.

[0211] (2) According to the method for producing a composite material, the urethane prepolymer can be dispersed in water in the mixing step, and the lignocellulose-based material and the urethane prepolymer can be mixed uniformly.

[0212] As a result, the water resistance of the resulting composite material can be improved.

[0213] Next, the present invention will be described based on examples and comparative examples, but the present invention is not limited to the following examples.

[0214] 1. Composite Material Raw Materials (1) Aromatic Isocyanate PH: Monomeric MDI, NCO% measured by ASTM D1638: 33.6, Molecular weight: 250 g / mol, Trade name: Cosmonate PH, Kumho Mitsui Chemicals, Inc. PI: Monomeric MDI, NCO% measured by ASTM D1638: 33.6, Trade name: Cosmonate PI, Kumho Mitsui Chemicals, Inc. M-200: Polymeric MDI, NCO% measured by ASTM D1638: 30.0 to 32.0, Trade name: Cosmonate M-200, Kumho Mitsui Chemicals, Inc. (2) Macropolyol Production Example 1 (Polyether polyol obtained by adding propylene oxide to propylene glycol, average hydroxyl value: 112 mg KOH / g, number average molecular weight: 1000) Production Example 2 (Polyether polyol obtained by adding propylene oxide to propylene glycol, average hydroxyl value: 56 mg KOH / g, number average molecular weight: 2000) Production Example 3 (Polyether polyol obtained by adding propylene oxide to glycerin, average hydroxyl value: 168 mg KOH / g, number average molecular weight: 1000) Production Example 4 (Polyether polyol obtained by adding propylene oxide to glycerin, average hydroxyl value: 56 mg KOH / g, number average molecular weight: 3000) (3) Compound component containing hydrophilic group M-400 (methoxypolyethylene glycol, number of functional groups: 1, average hydroxyl value: 140.3 mg KOH / g, number average molecular weight: 400, trade name: Uniox M-400, manufactured by NOF Corporation) MPEG500 (methoxypolyethylene glycol, functionality: 1, average hydroxyl value: 112 mgKOH / g, number average molecular weight: 500, manufactured by Jiahua Chemical Co., Ltd.) M-550 (methoxypolyethylene glycol, functionality: 1, average hydroxyl value: 102 mgKOH / g, number average molecular weight: 550, trade name: Uniox M-550, manufactured by NOF Corporation) MPEG600 (methoxypolyethylene glycol, functionality: 1, average hydroxyl value: 93.5 mgKOH / g, number average molecular weight: 600, manufactured by Jiahua Chemical Co., Ltd.)Compound A (ethylene oxide and propylene oxide addition polymer of diethylene glycol monomethyl ether, number of functional groups: 1, average hydroxyl value: 67 mg KOH / g, number average molecular weight: 837) (4) First polyol DPG (dipropylene glycol, number of functional groups: 2, hydroxyl value: 836.25 mg KOH / g, molecular weight: 134.17, manufactured by ADEKA Corporation) Production Example 5 (polyether polyol obtained by adding propylene oxide to propylene glycol, average hydroxyl value: 400 mg KOH / g, number average molecular weight: 280) Gly (glycerin, number of functional groups: 3, hydroxyl value: 1827.56 mg KOH / g, molecular weight: 92.09, manufactured by NOF Corporation) Production Example 6 (Polyether polyol obtained by adding propylene oxide to propylene glycol, average hydroxyl value: 280 mg KOH / g, number average molecular weight: 400) Production Example 7 (Polyether polyol obtained by adding propylene oxide to glycerin, average hydroxyl value: 420 mg KOH / g, number average molecular weight: 400) Production Example 8 (Polyether polyol obtained by adding propylene oxide to glycerin, average hydroxyl value: 240 mg KOH / g, number average molecular weight: 700) (5) Second Polyol Production Example 9 (Polyether polyol obtained by adding propylene oxide to triethanolamine, average hydroxyl value: 350 mg KOH / g, number average molecular weight: 480) Production Example 10 (Polyether polyol obtained by adding propylene oxide to ethylenediamine, average hydroxyl value: 305 mg KOH / g, number average molecular weight: 740) Production Example 11 (Polyether polyol obtained by adding propylene oxide to ethylenediamine, average hydroxyl value: 820 mg KOH / g, number average molecular weight: 270) Production Example 12 (Polyether polyol obtained by adding propylene oxide to ethylenediamine, average hydroxyl value: 450 mg KOH / g, number average molecular weight: 500) (6) Catalyst (6-1) Amine catalyst DMCHA (dimethylcyclohexylamine) DMEA (dimethylethanolamine) TEA (triethanolamine) (6-2) Metal catalyst Neostan U-100 (dibutyltin dilaurate, manufactured by Nitto Kasei Co., Ltd.) (7) Lignocellulosic material (7-1) Cedar barkThinned cedar lumber (purchased from Totake Construction Co., Ltd.) The moisture content was measured and found to be 30%, 40%, 45%, 50% and 60%.

[0215] (7-2) Strand Chips Core Chips (purchased from Shinaki Kogyo Co., Ltd.) The moisture content was measured and found to be 40%.

[0216] (7-3) Rice straw Product name: straw, rice straw, cut straw, ultra-fine cut straw (for agricultural and horticultural use, manufactured by Usui Nochiku Co., Ltd.) The moisture content was measured to be 30% and 35%. 2. Production of urethane prepolymer components Urethane prepolymers A to G were obtained according to the formulations shown in Table 1.

[0217] Specifically, for urethane prepolymers A to D, F, and G, PH, which is solid at room temperature, was first mixed with M-200 in a container under a nitrogen atmosphere, and the PH was dissolved with stirring at 40°C to obtain a mixed solution of PH and M-200. Next, a macropolyol component and, if necessary, a hydrophilic group-containing compound were added to the resulting mixed solution, and the mixture was heated to 80°C with stirring, and then reacted at 80°C for 3 hours to obtain a urethane prepolymer. The resulting urethane prepolymer was then cooled to 40°C or below.

[0218] For urethane prepolymer E, the macropolyol component and the hydrophilic group-containing compound were added to PI in a container under a nitrogen atmosphere, and the mixture was heated to 80°C with stirring, and then reacted at 80°C for 3 hours to obtain a urethane prepolymer. The obtained urethane prepolymer was then cooled to 40°C or below.

[0219] 3. Production of Composite Materials According to the formulations shown in Tables 2 to 6, the first agent and water were mixed to prepare a first mixture, and the second agent and water were mixed to prepare a second mixture.

[0220] Next, the first and second mixed solutions were mixed with lignocellulosic material to prepare composite compositions. Tables 2 to 6 show the ratio of the first agent to 100 parts by mass of the solid content of the lignocellulosic material.

[0221] The composite composition was then spread into a mold, compressed, and formed.

[0222] Next, the formed composite material composition was press-molded at the press temperature and for the molding time shown in Tables 2 to 6.

[0223] In this way, composite materials of each example and each comparative example were obtained.

[0224] In Comparative Example 2, the first agent did not use a urethane prepolymer, but used 17 parts by mass of a mixture of 243.11 parts by mass of PH (monomeric MDI) and 756.89 parts by mass of M-200 (polymeric MDI).

[0225] In Comparative Example 3, no urethane prepolymer was used as the first agent, and 17 parts by mass of a reaction product of 964.88 parts by mass of M-200 (polymeric MDI) and 35.12 parts by mass of the above-mentioned compound A was used.

[0226]

[0227]

[0228]

[0229]

[0230] According to JIS A5908:2015 (particle board), the obtained composite material was cured for 7 days in a well-ventilated location at 20°C and 60% humidity, and the thickness, density, flexural strength, wet B flexural strength, flexural retention rate, and 20°C water absorption thickness expansion rate of the composite material were measured. The results are shown in Tables 2 to 6.

[0231] Furthermore, whether or not the boards have water resistance conforming to the P type specified in JIS A5908:2015 (particle board) was evaluated according to the following criteria: A: Has water resistance conforming to the P type specified in JIS A5908:2015 (particle board). B: Has water resistance conforming to the P type specified in JIS A5908:2015 (particle board), but the bending residual rate is less than 50.0%. C: Does not have water resistance conforming to the P type specified in JIS A5908:2015 (particle board).

[0232] The above invention is provided as an exemplary embodiment of the present invention, but it is merely an example and should not be interpreted as being limiting. Modifications of the present invention that are obvious to those skilled in the art are included in the scope of the following claims.

[0233] The urethane prepolymer, polyurethane resin raw material, and composite manufacturing method of the present invention can be used, for example, to manufacture composites of lignocellulosic materials and polyurethane resins. The composites of the present invention can be used, for example, for ground paving, sidewalks, highway walls, residential peripheries, furniture, indoor wall materials, indoor floor materials, and floor underlayments.

Claims

1. A urethane prepolymer having an isocyanate group and a hydrophilic group, the urethane prepolymer being a reaction product of a polyisocyanate component, a macropolyol component, and a compound component containing a hydrophilic group, the polyisocyanate component containing an aromatic polyisocyanate, the aromatic polyisocyanate containing at least one selected from the group consisting of diphenylmethane diisocyanate and polymethylene polyphenyl polyisocyanate, the macropolyol component containing a polyether polyol having a number average molecular weight of 400 or more and 10,000 or less, and the compound component containing a hydrophilic group containing a hydrophilic group and a compound containing an active hydrogen group having an oxygen atom.

2. The urethane prepolymer according to claim 1, wherein the content of oxyethylene units in the polyether polyol is 5.0 mass% or less relative to the total amount of oxyalkylene units in the polyether polyol.

3. The urethane prepolymer according to claim 1, wherein the compound containing a hydrophilic group and an active hydrogen group having an oxygen atom is an alkoxypolyethylene glycol, and the number average molecular weight of the compound containing a hydrophilic group and an active hydrogen group having an oxygen atom is 100 or more and 700 or less.

4. A polyurethane resin raw material comprising a urethane prepolymer component containing the urethane prepolymer according to any one of claims 1 to 3, and a polyol component.

5. The polyurethane resin raw material according to claim 4, wherein the polyol component comprises a first polyol and a second polyol, the first polyol is a polyol not containing nitrogen atoms, the first polyol has an average hydroxyl value of 200 mg KOH / g or more and 2,000 mg KOH / g or less, the first polyol has a number average molecular weight of 50 or more and 1,000 or less, the second polyol is a polyol containing nitrogen atoms, the second polyol has an average hydroxyl value of 200 mg KOH / g or more and 2,000 mg KOH / g or less, and the second polyol has a number average molecular weight of 200 or more and 1,000 or less.

6. The polyurethane resin raw material according to claim 4, further comprising: an isocyanate group content of the urethane prepolymer of 10% by mass or more; and a catalyst.

7. The polyurethane resin raw material according to claim 4, which is for a composite material containing a lignocellulosic material and a polyurethane resin.

8. A composite material comprising a lignocellulosic material and a polyurethane resin, wherein the polyurethane resin is a reaction product of a polyurethane resin raw material according to any one of claims 4 to 7.

9. A method for producing a composite material containing a lignocellulosic material and a polyurethane resin, comprising: a mixing step of mixing a lignocellulosic material having a moisture content of 15% or more, a polyurethane resin raw material according to any one of claims 4 to 7, and water to prepare a composite material composition; and a curing step of curing the composite material composition.

10. The method for producing a composite material according to claim 9, wherein in the curing step, the composite material composition is cured by press molding.

11. A method for producing a composite material as described in claim 9 or claim 10, wherein in the composite material composition, the blending ratio of the urethane prepolymer component per 100 parts by mass of the solid content of the lignocellulose-based material is 5 parts by mass or more and 40 parts by mass or less.

12. The method for producing a composite material according to claim 9 or 10, wherein the polyol component includes a first polyol and a second polyol, the first polyol is a polyol not containing nitrogen atoms, the first polyol has an average hydroxyl value of 200 mg KOH / g or more and 2,000 mg KOH / g or less, the first polyol has a number average molecular weight of 50 or more and 1,000 or less, the second polyol is a polyol containing nitrogen atoms, the second polyol has an average hydroxyl value of 200 mg KOH / g or more and 2,000 mg KOH / g or less, and the second polyol has a number average molecular weight of 200 or more and 1,000 or less, and in the composite material composition, the blending ratio of the second polyol per 100 parts by mass of the urethane prepolymer component is 6 parts by mass or more and 20 parts by mass or less.

13. A method for producing a composite material as described in claim 9 or claim 10, wherein the isocyanate group content of the urethane prepolymer is 10 mass% or more, the composite material composition further contains a catalyst, and the blending ratio of the catalyst per 100 mass parts of the urethane prepolymer component is 0.04 mass parts or more and 1.5 mass parts or less.