Bonding wire

MYPI2025004557A0Undetermined Publication Date: 2024-07-31TATSUTA ELECTRICWIRE & CABLE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025004557
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-01-31
Filing Date
2024-01-29
Publication Date
2024-07-31

AI Technical Summary

Technical Problem

Bonding wires with a silver (Ag) core and gold (Au) coating face challenges in forming a free air ball (FAB) with good sphericity and achieving a circular shape for the first joint, due to Ag sulfidation defects and high costs associated with Au-based wires.

Method used

A bonding wire with a core material primarily composed of Ag and a coating layer primarily composed of Au, along with optional Pd, In, and Bi, where the coating layer's thickness is between 0.0014 and 0.0048 times the core diameter, and the specific resistance ratio of the core to the coating layer is between 85% and 115%, enhancing sphericity and circularity of the FAB and first joint.

Benefits of technology

The solution allows for the stable formation of a FAB with high sphericity and a circular first joint, while maintaining corrosion resistance and long-term reliability, and reducing the specific resistance of the Ag core to match Au's resistance, thus overcoming Ag sulfidation issues and cost concerns.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025004557_DRAWING_001
    Figure PI2025004557_DRAWING_001
Patent Text Reader

Abstract

There is provided a bonding wire including a core material containing Ag as a main component and a covering layer containing Au as a main component disposed on a surface of the core material, in which a FAB having high sphericity and a good shape can be formed. The bonding wire of the present invention is a bonding wire W including a core material 10 containing Ag as a main component and a covering layer 12 that is disposed on a surface of the core material 10 and contains Au as a main component. In this bonding wire, the core material 10 contains one or two or more selected from the group consisting of Au, Pd, and In. The ratio of the film thickness of the covering layer 12 to the diameter of the core material 10 is 0.0014 or more and 0.0048 or less, and the ratio of the resistivity of the core material 10 to the resistivity of the covering layer 12 is 85% or more and 115% or less. Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Bonding Wire

[0001] The present invention relates to a bonding wire in which the surface of a bonding wire mainly composed of Ag (silver) is coated with a coating layer mainly composed of Au (gold).

[0002] Bonding wires used for connecting electrodes on semiconductor elements to electrodes on substrates are generally very thin and are therefore made of metal materials that have good conductivity and excellent workability. In particular, bonding wires primarily composed of Au have been widely used because of their chemical stability and ease of handling in the atmosphere.

[0003] However, bonding wires primarily composed of Au contain 99% or more of Au by mass and are very expensive. Therefore, bonding wires primarily composed of Ag instead of Au have been proposed (for example, Patent Documents 1 and 2 listed below).

[0004] Although Ag is cheaper than Au, Ag-based bonding wires are more likely to have poor bonding to electrodes due to sulfurization of the wire surface compared to Au-based bonding wires. In order to prevent poor bonding due to Ag sulfurization, bonding wires have been proposed in which the surface of a core material primarily composed of Ag is coated with a coating layer primarily composed of Au (see, for example, Patent Documents 3 to 5 listed below).

[0005] Patent No. 5616165 Patent No. 5529992 Patent No. 2016-517623 International Publication WO2013 / 129253 International Publication WO2021 / 205674

[0006] When a coating layer mainly composed of Au is provided on the surface of a core material mainly composed of Ag, it is difficult to stably form a free air ball (hereinafter abbreviated as FAB) with a good shape and high sphericity when ball bonding to an electrode, and it is also difficult to form a good circular shape at the first joint formed when the FAB is brought into contact with an electrode and crushed.

[0007] The present invention has been made in consideration of the above circumstances, and aims to provide a bonding wire in which a coating layer mainly composed of Au is provided on the surface of a core material mainly composed of Ag, which can form a FAB with a good shape and high sphericity, and can make the shape of the first joint a good circle.

[0008] In order to solve the above problems, the bonding wire of the present invention is a bonding wire having a core material containing Ag as its main component and a coating layer provided on the surface of the core material and containing Au as its main component, wherein the core material contains one or more elements selected from Au, Pd (palladium), and In (indium), the ratio of the film thickness of the coating layer to the diameter of the core material is 0.0014 or more and 0.0048 or less, and the ratio of the resistivity of the core material to the resistivity of the coating layer is 85% or more and 115% or less.

[0009] In the bonding wire according to the present invention, the core material may contain at least one of Au and Pd.

[0010] In the bonding wire according to the present invention, the core material may contain Au and Pd, with the Au content being greater than the Pd content.

[0011] In the bonding wire according to the present invention, the core material may contain Bi (bismuth) in an amount of 1 ppm by mass or more and 50 ppm by mass or less.

[0012] In the bonding wire according to the present invention, the core material may contain 0.1 mass % or more and 1.0 mass % or less of In.

[0013] In the bonding wire of the present invention, a bonding wire having a coating layer mainly composed of Au on the surface of a core material mainly composed of Ag can form a FAB with a good shape and high sphericity, and the shape of the first joint can be made to be a good circle.

[0014] 1 is a cross-sectional view of a bonding wire according to an embodiment of the present invention.

[0015] (1) Configuration of Bonding Wire W Hereinafter, a bonding wire W according to one embodiment of the present invention will be described with reference to the drawings.

[0016] The bonding wire W of this embodiment is a bonding wire for connecting electrodes (e.g., Al alloy electrodes, nickel-palladium-gold coated electrodes, Au-coated electrodes, etc.) on semiconductor elements in semiconductor devices (power ICs, LSIs, transistors, BGAs (Ball Grid Array packages), QFNs (Quad Flat Non-lead packages), LEDs (light-emitting diodes), etc.) to conductor wiring (electrodes) on circuit wiring boards (lead frames, ceramic substrates, printed circuit boards, etc.) 2 by a ball bonding method. Note that the bonding wire W of this embodiment can be used as a bonding wire in various forms other than semiconductor devices.

[0017] As shown in Figure 1, the bonding wire W of this embodiment comprises a core material 10 mainly composed of Ag and a coating layer 12 mainly composed of Au, and the coating layer 12 covers the entire outer surface of the core material 10 so that there are no exposed portions.

[0018] Specifically, the core material 10 contains 90% by mass or more, preferably 95% by mass or more, of Ag. The Ag constituting the core material 10 may contain impurities such as Fe (iron) that are inevitably present during purification, and it is preferable to produce an Ag alloy constituting the bonding wire W using Ag with a purity of 99.9% by mass or more.

[0019] The core material 10 contains one or more elements selected from the group consisting of Au, Pd, and In in addition to Ag, and the resistivity ρ1 of the core material 10 is adjusted. In other words, the contents of Au, Pd, and In in the core material 10 are adjusted so that the ratio β (=ρ1 / ρ2) of the resistivity ρ1 of the core material 10 to the resistivity ρ2 of the coating layer 12 is 85% or more and 115% or less, preferably 90% or more and 110% or less.

[0020] As an example of the resistivity of the core material 10 and the covering layer 12, the resistivity of the core material 10 can be set to 1.95 μΩ·cm or more and 3.26 μΩ·cm or less, and the resistivity of the covering layer 12 can be set to 2.30 μΩ·cm or more and 2.83 μΩ·cm or less.

[0021] When the resistivity of the coating layer 12 is 2.3 μΩ cm, the core material 10 contains only one element selected from the group consisting of Au, Pd, and In, and in order to set the ratio β of the resistivity ρ1 of the core material 10 to the resistivity ρ2 of the coating layer 12 to 85% or more and 115% or less, the core material 10 can contain 1.3 mass% or more and 4.0 mass% or less of Au, 0.7 mass% or more and 2.1 mass% or less of Pd, and 0.2 mass% or more and 0.6 mass% or less of In.

[0022] Furthermore, the diameter φ of the core material 10 and the thickness t of the coating layer 12 of the bonding wire W are set so that the ratio α (= t / φ) of the thickness t of the coating layer 12 to the diameter φ of the core material 10 is 0.0014 or more and 0.0048 or less. The diameter of the core material 10 may be various sizes depending on the application of the bonding wire. For example, the diameter (wire diameter) φ of the core material 10 can be 15 μm or more and 150 μm or less. The thickness t of the coating layer 12 is preferably 0.15 μm or more and 0.50 μm or less.

[0023] For the resistivity of the core material 10, three evaluation samples are prepared, and the resistivity of each of the three evaluation samples is measured at room temperature using the four-terminal method, and the average value of the measurement results is defined as the resistivity of the core material 10. For the resistivity of the coating layer 12, three evaluation samples are prepared from a bonding wire made with the same alloy composition as the coating layer 12, and the resistivity of each of the three evaluation samples is measured at room temperature using the four-terminal method, as with the core material 10, and the average value of the measurement results is defined as the resistivity of the core material 10.

[0024] The diameter φ of the core material 10 and the thickness t of the coating layer 12 were determined by irradiating X-rays using a fluorescent X-ray thickness meter and converting the intensity of the fluorescent X-rays generated into the thickness of the coating layer.

[0025] The bonding wire W preferably contains Au and preferably Pd in ​​the core material 10. When the core material 10 contains both Au and Pd, the Au content is preferably greater than the Pd content. When the core material 10 contains both Au and Pd, the total Au and Pd content is preferably 0.6% by mass or more and 3.0% by mass or less.

[0026] The core material 10 may contain 0.1% by mass or more and 1.0% by mass or less of In. When the core material 10 contains 0.1% by mass or more of In, the corrosion resistance of the first bonded portion formed when the FAB is pressed against the electrode and crushed is improved, thereby improving long-term reliability. When the In content in the core material 10 is 1.0% by mass or less, the specific resistance of the wire is maintained within an appropriate range.

[0027] Furthermore, the core material 10 may contain 1 mass ppm or more and 50 mass ppm or less of Bi in addition to one or more elements selected from the group consisting of Au, Pd, and In.

[0028] In the present invention, in addition to the above-mentioned Au, Pd, Bi, and In, one or two elements selected from Ca and Cu may be further contained. If the total content of Ca and Cu is 100 ppm by mass or less, the strength of the wire can be improved without impairing the above-mentioned effects achieved by adding Au, Pd, Bi, and In. When Ca and / or Cu are added, the total content of Ca and Cu is preferably 1 ppm by mass or more and 100 ppm by mass or less, and more preferably 5 ppm by mass or more and 85 ppm by mass or less.

[0029] The coating layer 12 contains 95% by mass or more, preferably 99% by mass or more, of gold, with gold being the main component. The coating layer 12 may be made of pure gold (gold content of 99.9% or more), or may be made of a gold alloy containing gold and an additive element. The gold alloy constituting the coating layer 12 may contain at least one element selected from the group consisting of Ag, Pd, Bi, Pt (platinum), Ni (nickel), Co (cobalt), and Sb (antimony).

[0030] (2) Manufacturing Method of Bonding Wire W Next, an example of a manufacturing method of the bonding wire W having the above-described configuration will be described.

[0031] First, an element selected from Au, Pd, and In is added to Ag having a purity of 99.9% by mass or more, and Bi, Ca, and Cu are added as necessary to contain 95% by mass or more of Ag, thereby casting an Ag alloy having a resistivity of 85% to 115% of the resistivity ρ2 of the coating layer 12, and then a rod-shaped ingot of a predetermined diameter is produced by a continuous casting method.

[0032] Next, the rod-shaped ingot is drawn to reduce its diameter to a predetermined diameter of the core material 10. Thereafter, a coating layer 12 containing Au is formed on the entire outer periphery of the core material 10. The coating layer 12 can be formed by known means such as electroplating, electroless plating, or vapor deposition.

[0033] The core material 10 on which the coating layer 12 is formed is further drawn to reduce its diameter to a predetermined value, thereby obtaining a bonding wire W having a ratio α of the thickness t of the coating layer 12 to the diameter φ of the core material 10 of 0.0014 to 0.0048, and a ratio β of the specific resistance ρ1 of the core material 10 to the specific resistance ρ2 of the coating layer 12 of 85% to 115%.

[0034] If necessary, heat treatment may be performed on the bonding wire W during or after the wire drawing process. As an example of the heat treatment, continuous annealing treatment can be performed at 300 to 1000°C for 0.1 to 60 seconds in an air atmosphere, a nitrogen gas atmosphere, or a mixed gas atmosphere of 5% hydrogen and 95% nitrogen.

[0035] (3) Effect In the bonding wire W of this embodiment, a coating layer 12 containing gold as its main component is provided on the outer surface of the core material 10, which improves the corrosion resistance of the bonding wire W and provides good bonding strength to metals that constitute electrodes, such as Al (aluminum), Au, Ag, and alloys thereof.

[0036] In the bonding wire W, by setting the film thickness t of the coating layer 12 to 0.0014 times or more the wire diameter φ of the core material 10, the corrosion resistance of the bonding wire W is exhibited, ball bonding in the atmosphere becomes possible, and good bonding strength is obtained with respect to the metal constituting the electrode. Furthermore, by setting the film thickness t of the coating layer 12 to 0.0048 times or less the wire diameter φ of the core material 10, the balance of the surface tension of the bonding wire W melted during FAB formation can be well maintained, and a FAB with a good shape and high sphericity can be formed.

[0037] In the bonding wire W, by setting the ratio of the resistivity ρ1 of the core material 10 to the resistivity ρ2 of the coating layer 12 to be 85% or more and 115% or less, when the tip of the bonding wire W is discharge-heated, the discharged electricity flows uniformly through the tip of the bonding wire W, the tip of the bonding wire W melts from all directions, and the FAB grows uniformly. Therefore, it is possible to form a FAB with a good shape and high sphericity, and to make the shape of the first bonded portion a good circle.

[0038] In the bonding wire W, since the core material 10 contains Au, when an FAB is formed at the tip of the bonding wire W by discharge heating or the like, the Au in the coating layer 12 is less likely to diffuse into the core material 10, and an FAB with a good shape and high sphericity can be formed more stably.

[0039] Since Pd has a higher resistivity than Au, by containing Pd together with Au in the core material 10, the total content of Au and Pd can be reduced while the resistivity of the core material 10, which is mainly composed of Ag, can be made closer to the resistivity of Au. Furthermore, when the core material 10 contains both Au and Pd, the content of Au is greater than that of Pd, so that a FAB with a good shape and high sphericity can be formed, and the shape of the first joint can be made to be a good circle.

[0040] In the bonding wire W, when the core material 10 contains Bi in an amount of 1 mass ppm or more and 50 mass ppm or less, a FAB having a good shape and high sphericity can be stably formed.

[0041] In the bonding wire W, if the core material 10 contains 0.1 mass % or more of In, the corrosion resistance of the first bonded portion formed when the FAB is pressed against the electrode and crushed is improved, thereby improving long-term reliability. If the In content in the core material 10 is 1.0 mass % or less, the specific resistance of the wire is maintained within an appropriate range, and a FAB with a good shape and high sphericity can be formed.

[0042] Although the embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments can be embodied in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included within the scope and spirit of the invention, as well as within the scope of the inventions described in the claims and their equivalents.

[0043] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to these examples.

[0044] Using an Ag raw material with a purity of 99.9% by mass or more, an Ag alloy having the composition shown in Table 1 below was melted and a rod-shaped ingot was produced by continuous casting. The rod-shaped ingot was then subjected to wire drawing to reduce the diameter of the core material 10 to 105 μm, and then electroplated to form a coating layer 12 made of an Au alloy having the composition shown in Table 1 below on the outer surface of the core material 10. Thereafter, the core material 10 on which the coating layer 12 was formed was further wiredrawn to reduce the diameter to a wire diameter φ of 20 μm and a coating layer 12 thickness t of approximately 57 nm. Then, continuous annealing (heat treatment) was performed at 400 to 600 ° C. for 0.4 to 0.5 seconds in a mixed gas atmosphere of 5% hydrogen and 95% nitrogen, to obtain bonding wires of Examples 1 to 21 and Comparative Examples 1 to 7.

[0045] In addition, using the same method as above, except that the outer surface of the core material 10 was not coated with Au, wires consisting only of the core material 10 of the bonding wires of Examples 1 to 21 and Comparative Examples 1 to 7, and wires consisting of the same alloy composition as the coating layer 12 of the bonding wires of Examples 1 to 21 and Comparative Examples 1 to 7 were produced.

[0046] Then, for the bonding wires of Examples 1 to 21 and Comparative Examples 1 to 7, the diameter φ of the core material 10 and the thickness t of the coating layer 12 were measured using the above-mentioned measurement method, and the ratio α of the thickness t of the coating layer 12 to the diameter φ of the core material 10 was calculated from these measurement results.

[0047] In addition, using a wire consisting only of the core material 10 and a wire having the same alloy composition as the coating layer 12, the resistivity ρ1 of the core material 10 and the resistivity ρ2 of the coating layer 12 were measured by the above-mentioned measurement method. From the obtained resistivity ρ1 of the core material 10 and the resistivity ρ2 of the coating layer 12, the ratio β of the resistivity ρ1 of the core material 10 to the resistivity ρ2 of the coating layer 12 was calculated.

[0048] In the bonding wires of Examples 1 to 21 and Comparative Examples 1 to 7, the diameter φ of the core material 10, the film thickness t of the coating layer 12, the ratio α, the specific resistance ρ1 of the core material 10, the specific resistance ρ2 of the coating layer 12, and the ratio β are as shown in Table 1 below.

[0049] The resulting bonding wires of Examples 1 to 21 and Comparative Examples 1 to 7 were evaluated for the following (1) to (4). Specific evaluation methods are as follows. (1) FAB sphericity (formability) FABs 1.9 to 2.1 times the wire diameter were produced in an atmosphere using a wire bonder (UTC-5000NeoCu, manufactured by Shinkawa Co., Ltd.). To evaluate FAB sphericity (formability), 100 FABs were produced for each bonding wire of the Examples and Comparative Examples, and then the appearance was observed using a general-purpose electron microscope (JEOL Ltd., JSM-6510LA), and the lengths of the produced FABs in the directions parallel to and perpendicular to the wire were measured. If the average value of the ratio (X / Y) of the length X of the FAB parallel to the wire to the length Y of the FAB perpendicular to the wire was within 100±5%, it was judged to have "sphericity" and was rated "A." If the average value of the ratio (X / Y) was 92% or more but less than 95% or more than 105% but less than 108%, it was rated "B." If the average value of the ratio (X / Y) was 90% or more but less than 92% or more than 108% but less than 110%, it was rated "C." If it was not visually circular, it was rated "D." (2) Shape Stability of the First Bond: Using the wire bonder used in (1) above, 100 FABs prepared in an atmospheric gas atmosphere were pressed against the electrode and bonded so that the diameter of the first bond was 1.4 times the diameter of the FAB. The center-to-center distance between the center of the first bond and the chamfer diameter of the capillary attached to the wire bonder was measured using a three-dimensional microscope (Olympus compact measuring microscope, STM6). If the center-to-center distance for all 100 FABs was 2.5 μm or less, it was rated "A." If the incidence of first bonded portions greater than 2.5 μm and less than 5 μm was less than 20%, it was rated "B." If the incidence of first bonded portions greater than 2.5 μm and less than 5 μm was 20% or more, it was rated "C." If even one first bonded portion exceeded 5 μm, it was considered to have low circularity and was unsuitable for fine-pitch applications, and it was rated "D." (3) High-Temperature Storage Test (Long-Term Reliability) After bonding in an air atmosphere using the wire bonder used in (1) above, semiconductor samples were prepared and sealed with epoxy resin. The semiconductor samples prepared using a commercially available thermostatic chamber were held at 150°C for 1,000 hours, after which electrical measurements were performed to evaluate conductivity.The number of wires evaluated was 500, and a defect rate of 1% or less was given an "A," a defect rate of more than 1% but less than 3% was given a "B," and a defect rate of more than 3% was given a "D" due to low resistance. (4) Overall Evaluation In the evaluation items (1) to (3) above, if all received an A rating, the rating was "A," if there were one or two A ratings, the rating was "B," if there were no A ratings, the rating was "C," and if there was at least one D rating, the rating was "D."

[0050] The results are shown in Table 1, and Examples 1 to 21 obtained good results in all of the evaluations (1) to (4) above.

[0051] On the other hand, in Comparative Examples 1 to 3, where the ratio α of the thickness t of the coating layer 12 to the diameter φ of the core material 10 was outside the range of 0.0014 to 0.0048, a circular FAB was not formed, and the sphericity of the FAB and the shape of the first bonded portion were deteriorated. Also, in Comparative Examples 4 to 7, where the ratio β of the specific resistance ρ1 of the core material 10 to the specific resistance ρ2 of the coating layer 12 was outside the range of 85% to 115%, the shape of the first bonded portion was deteriorated.

[0052] 10...core material, 12...covering layer, W...bonding wire

Claims

1. A bonding wire having a core material containing Ag as its main component and a coating layer containing Au as its main component and provided on the surface of the core material, wherein the core material contains one or more elements selected from the group consisting of Au, Pd and In, the ratio of the thickness of the coating layer to the diameter of the core material is 0.0014 or more and 0.0048 or less, and the ratio of the resistivity of the core material to the resistivity of the coating layer is 85% or more and 115% or less.

2. The bonding wire according to claim 1, wherein the core material contains at least one of Au and Pd.

3. The bonding wire according to claim 2, wherein the core material contains Au and Pd, with the Au content being greater than the Pd content.

4. A bonding wire according to any one of claims 1 to 3, wherein the core material contains Bi in an amount of 1 ppm by mass or more and 50 ppm by mass or less.

5. A bonding wire according to any one of claims 1 to 3, wherein the core material contains 0.1 mass % or more and 1.0 mass % or less of In.