Bonding sheet, bonded assembly and preparation methods therefor

MYPI2025004586A0Undetermined Publication Date: 2024-08-22THE UNIVERSITY OF HONG KONG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025004586
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-02-22
Filing Date
2024-02-21
Publication Date
2024-08-22

AI Technical Summary

Technical Problem

Existing solders cannot function stably at high operating temperatures, resulting in reduced welding reliability of high-power components, and the porous structure of the nanometal particle layer results in poor thermal and electrical conductivity and insufficient shear strength.

Method used

The welding piece is made of a copper matrix and a nanometal layer. The yield strength of the copper base is not higher than 100MPa through annealing treatment. Combined with hot pressure welding technology, the welding piece undergoes local plastic deformation during the welding process to fit the surface of the component to be welded. , improve the effective welding area and shear strength.

Benefits of technology

The shear strength and reliability of the welded components are improved, the roughness tolerance of the surface to be welded is enhanced, and the welding pieces can be processed twice to adapt to application requirements of different sizes and shapes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025004586_DRAWING_001
    Figure PI2025004586_DRAWING_001
  • Figure PI2025004586_DRAWING_002
    Figure PI2025004586_DRAWING_002
  • Figure PI2025004586_DRAWING_003
    Figure PI2025004586_DRAWING_003
Patent Text Reader

Abstract

The present invention relates to a bonding sheet, a bonded assembly, and preparation methods therefor. The bonding sheet comprises: a copper substrate having opposing first and second surfaces; and at least one nano-metal layer deposited on at least one of the first and second surfaces of the copper substrate, the yield strength of the bonding sheet is not greater than 100 MPa. The bonded assembly comprises: a first substrate; a second substrate; and a bonding portion located between the first substrate and the second substrate to connect the two, the bonding portion comprises a copper substrate, a first bonded interface on a first side of the copper substrate, and a second bonded interface on a second side of the copper substrate opposite to the first side, the first bonded interface and the second bonded interface are formed by bonding nano-metal on opposite sides of the copper substrate to the first substrate and the second substrate, respectively; and the shear strength of the bonded assembly is not less than 40 MPa. Fig. 9
Need to check novelty before this filing date? Find Prior Art

Description

Welding sheet, welding assembly and preparation method thereof Technical Field

[0001] The present invention relates to a solder sheet that can be used to encapsulate high-power components to be soldered, comprising a copper substrate and a nanometal layer deposited on at least one outer surface of the copper substrate. The present invention also relates to a solder assembly formed by soldering the solder sheet, and methods for preparing the solder sheet and the solder assembly. Background Art

[0002] As high-power components are increasingly becoming more functionally diverse and miniaturized, their packaging faces significant challenges. The US Department of Energy projects that the energy per unit volume of automotive high-power components will rise from 18kW / L in 2020 to 100kW / L by 2025. This increase in power density directly leads to higher operating temperatures for these components. To meet this increased power density, high-power components have evolved from first-generation silicon-based semiconductors to third-generation wide-bandgap silicon carbide semiconductors, with operating temperatures correspondingly increasing from 100°C to 175°C, with further increases expected in the future. This poses a challenge for traditional solders, which cannot withstand these high operating temperatures, thus limiting the increase in power density for high-power components. For example, current device packaging uses tin-based solder paste with a melting point of 250°C. This traditional solder can only withstand device operating temperatures below 150°C. Above this temperature, the reliability of tin-based solder interconnects is significantly reduced, leading to premature device failure and short circuits. To this end, new high-temperature resistant solders based on nano-silver and nano-copper are gradually replacing traditional solders and entering the mainstream market.

[0003] CN110640354 A describes a preformed solder comprising a preformed metal substrate and a nanoparticle film coated on the outer surface of the substrate; the nanoparticle film primarily contains nanometal particles and is prebaked and coated on the preformed surface, and the melting point of the nanometal particles is lower than that of the metal substrate. Because the nanoparticle film itself has a loose structure and uniform pores, it can better compensate for the flatness and surface roughness of the components to be welded (e.g., a chip, a copper-clad ceramic substrate, or a radiator surface), allowing pressure to be more evenly transmitted to each weld area during the welding process. Furthermore, internal stress generated during welding or during drying can be absorbed by the pores and does not accumulate within the nanoparticle film. However, it is worth noting that the loose nature of the nanometal particle structure itself results in excessive pores in the final weld, which not only leads to poor thermal and electrical conductivity but also compromises the shear strength of the welded assembly. Furthermore, because the prebaked nanoparticle layer cannot undergo elastic deformation and has poor adhesion to the substrate, the solder cannot be subjected to secondary processing to improve its shape, resulting in inconvenience in use.

[0004] WO2022 / 127776A1 describes a method for low-temperature soldering using a nano-copper layer, which involves depositing a nano-copper layer on the surface of one or more structures to be soldered, wherein the nano-copper layer has a thickness of 10nm to 10μm and a grain size of 5 to 500nm. Compared with CN110640354 A, the coating is dense and pore-free, eliminating the pore defects of the nano-metal particle structure and improving electrical and thermal conductivity. However, the inventors found that in order to obtain high shear strength, the flatness of the parts to be soldered must be very high.

[0005] In view of the foregoing, there remains a need for improved solders to increase the shear strength of soldered assemblies.

[0006] Summary of the Invention

[0007] The present invention is made in view of the above problems existing in the prior art.

[0008] A first aspect of the present invention provides a welding sheet that enables a final welded assembly to have a high effective welding area and shear strength, thereby improving welding reliability, when the porosity of the surface coating is low and the surface flatness requirements of the components to be welded are not high.

[0009] The soldering sheet of the present invention comprises:

[0010] a copper substrate having opposing first and second surfaces; and

[0011] at least one nanometal layer deposited on at least one of the first and second surfaces of the copper substrate,

[0012] Wherein, the yield strength of the welding piece is not greater than 100 MPa.

[0013] The soldering surfaces of components to be welded, such as chips, often have uneven surfaces without special treatment, meaning they are relatively rough. While preparing solder sheets, the inventors discovered that when using solder sheets made by depositing a dense nano-copper layer on a conventional substrate, the shear strength of the components welded using them was insufficient. The inventors discovered that this is because the dense nano-copper layer cannot, like a nano-particle layer, rely on particle misalignment or pore deformation to synchronously deform the copper layer. Consequently, it cannot compensate for the surface unevenness of the components to be welded, resulting in significant misalignment. This reduces the effective welding area, and as a result, only partial welding can be achieved between the components to be welded, resulting in low shear strength.

[0014] To overcome this drawback, wet polishing can be used to improve the flatness of the surface to be welded, thereby effectively increasing the weld area and thus improving shear strength. However, this operation is not only expensive but also causes some damage to the welded components, making it a less preferred method for improving the shear strength of welded assemblies.

[0015] To this end, the present invention seeks to find a solution for improving the shear strength of welded assemblies without requiring special treatment of the surfaces to be welded (e.g., wet polishing). Using a copper substrate as the soldering pad substrate, the present invention models the surface morphology of the component to be welded (e.g., a chip), where the vertical difference between the highest and lowest points on the outer surface of the component to be welded when placed horizontally can be as high as 200 nm (i.e., a rough surface). The yield strength corresponding to the yield point of the copper substrate under the pressure used for hot-press welding (15-40 MPa) is calculated. This serves as the basis for selecting a copper substrate that allows the soldering pad to undergo at least partial plastic deformation during hot-press welding. The present inventors' theoretical research and experimental verification have shown that the yield strength of the soldering pad should not exceed 100 MPa. During hot-press welding, the solder tab contacts the raised portion on the chip surface. Because the contact area is small and the pressure is high, the yield strength of the solder tab can be reached more easily, allowing the solder tab to undergo local plastic deformation centered on the raised portion. This allows the recessed portion on the chip surface to contact the deformed solder tab and undergo diffusion welding, thereby increasing the effective welding area and improving the shear strength of the final welded assembly. If the yield strength of the solder tab exceeds 100 MPa, the solder tab cannot or rarely undergoes plastic deformation, making it difficult to compensate for the significant difference in surface flatness of the components to be welded. Consequently, the effective welding area cannot be significantly increased, and the shear strength is low. Therefore, the present invention requires that the yield strength of the solder tab be no greater than 100 MPa. Preferably, the yield strength of the solder tab is within the range of 18 to 100 MPa, more preferably, within the range of 18 to 67.5 MPa, more preferably, within the range of 20 to 46.5 MPa, and even more preferably, within the range of 23 to 36 MPa.

[0016] Preferably, the average grain size of the copper matrix is ​​in the range of 30 to 140 μm, preferably in the range of 50 to 140 μm, more preferably in the range of 75 to 122.5 μm, and even more preferably in the range of 90 to 115 μm.

[0017] Preferably, the elongation of the welding piece is not less than 11.5%, preferably, not less than 23%, further preferably, in the range of 27.5% to 36%, and more preferably, in the range of 29% to 34%.

[0018] Preferably, the solder sheet is in a thin sheet form, allowing it to be cut into the desired size or shape after secondary cutting. Compared to a nanoparticle layer that is applied and then dried, cutting or bending the sheet does not cause the nanometal layer on the sheet to peel off, thereby improving the integrity of the sheet and expanding its application scenarios.

[0019] Preferably, the average grain size of the nanometal layer is in the range of 5 to 500 nm, more preferably in the range of 5 to 100 nm, to achieve low-temperature soldering and improve soldering performance between the interfaces to be soldered. Preferably, the average thickness of the nanometal layer is 100 nm to 10 μm, more preferably 500 nm to 5 μm. Preferably, the metal of the nanometal layer can be selected from the group consisting of copper, gold, nickel, silver, platinum, and titanium. Preferably, the nanometal layer is a nanocopper layer.

[0020] A second aspect of the present invention provides a method for preparing a solder sheet, comprising the following steps:

[0021] Step A: providing a copper substrate having a first surface and a second surface opposite to each other;

[0022] Step B: annealing the copper substrate under vacuum to obtain a soft copper substrate, wherein the average grain size of the soft copper substrate is in the range of 30 to 140 μm;

[0023] Step C: depositing at least one nanometal layer on at least one of the first surface and the second surface of the soft copper substrate to obtain the soldering sheet.

[0024] The process involved in this method is simple and does not require complicated or expensive equipment.

[0025] Preferably, the copper substrate is a common industrial-grade electroplated copper foil or rolled copper foil, typically having a yield strength in the range of 140 to 250 MPa. The present invention first anneals the copper foil to fully recrystallize it to an average grain size of 30 to 140 μm, thereby obtaining a soft copper foil. The yield strength of the soft copper foil is no greater than 100 MPa, ensuring that the yield strength of the resulting solder sheet is no greater than 100 MPa.

[0026] It is well known that at the same annealing temperature, the longer the holding time, the larger the final average grain size. At the same holding time, the higher the annealing temperature, the larger the final average grain size. Therefore, depending on the target average grain size of 30 to 140 μm, various heat treatment conditions can be expected. Preferably, in step B, the vacuum degree is 1.0×10 -3Torr, the annealing temperature is 400-850°C, and the holding time is 2-16 hours; preferably, the annealing temperature is 500-800°C, and the holding time is 6-12 hours. For low annealing temperatures, such as 400°C, if the annealing time is too short, it will not be enough to grow the average grain size to 30μm, so a minimum holding time of 2 hours is required. Relatively speaking, for high annealing temperatures, such as 850°C, if the annealing time is too long, the average grain size will exceed the expected range, which is not conducive to the shear strength of the final device. Therefore, the holding time is required to be no more than 16 hours, which is also conducive to shortening the entire operation process and improving the yield of the production line.

[0027] Preferably, a cleaning step is included before step C: the soft copper substrate is cleaned with a mixture of dilute hydrochloric acid and deionized water with a volume fraction of 1:1 for 30 seconds to remove the surface oxide layer, followed by ultrasonic cleaning in deionized water and drying, for example, by blowing dry with a nitrogen gun at room temperature.

[0028] Preferably, the deposition of the nanometal layer on the copper substrate is carried out by methods such as electroplating, evaporation, vapor deposition (such as magnetron sputtering), ion plating, to obtain a relatively uniform and dense nanometal layer of thickness and grain size. The thickness and grain size of the nanometal layer are selected to not significantly change the yield strength of the entire soldering sheet after being deposited on the copper substrate, thereby ensuring that the yield strength of the entire soldering sheet is dominated by the copper substrate and is no more than 100MPa. Therefore, if it is desired to use a thicker nanometal layer, such as a 10 μm nanometal layer, a copper substrate that is thicker and has a low yield strength (i.e., a large grain size) should be selected to ensure that the yield strength of the entire soldering sheet obtained after depositing the nanometal layer is no more than 100MPa.

[0029] Preferably, the average thickness of the nanometal layer is 100 nm to 10 μm, more preferably 500 nm to 5 μm. Preferably, the average grain size of the nanometal layer is in the range of 5 to 500 nm, more preferably 5 to 100 nm, to achieve low-temperature welding and promote welding performance between the interfaces to be welded.

[0030] Preferably, the average thickness of the copper matrix is ​​at least 10 times, preferably 50 to 600 times, and further preferably 100 to 400 times, the average thickness of the nanometal layer and the average grain size of the copper matrix is ​​at least 60 times, preferably at least 100 times, the average grain size of the nanometal layer, so as to ensure that the yield strength of the solder tab is dominated by the copper matrix.

[0031] Preferably, the metal of the nano-metal layer can be selected from the group consisting of copper, gold, nickel, silver, platinum, and titanium. Preferably, the nano-metal layer is a nano-copper layer.

[0032] Preferably, the nano copper layer is deposited by electroplating as follows: the electrolytic solution contains 100-150 g / L of anhydrous copper sulfate, 80-150 g / L of 98% mass fraction concentrated sulfuric acid, 50-150 mg / L of sodium chloride, 350-480 mg / L of PEG20000, and 20-40 mg / L of Janus Green B. Preferably, the current density of the electroplating deposition is 0.05-0.15 A / cm 2 , and the deposition time is 10 to 300 seconds.

[0033] A third aspect of the present invention is a welding assembly comprising:

[0034] a first substrate;

[0035] a second substrate; and

[0036] A welding portion located between the first substrate and the second substrate to connect the two, wherein the welding portion includes a copper substrate, a first welding interface on a first side of the copper substrate, and a second welding interface on a second side of the copper substrate opposite to the first side, the first welding interface and the second welding interface being formed by bonding nanometal on opposite sides of the copper substrate to the first substrate and the second substrate, respectively.

[0037] Wherein, the shear strength of the welding assembly is not less than 40 MPa.

[0038] Preferably, the average grain size of the copper matrix is ​​in the range of 30 to 140 μm, preferably in the range of 50 to 140 μm, preferably in the range of 75 to 122.5 μm, and further preferably in the range of 92 to 115 μm.

[0039] Preferably, the first substrate and / or the second substrate may be a chip, a copper-clad ceramic substrate, a heat sink or other components.

[0040] Preferably, the effective welding area of ​​the first welding interface and / or the second welding interface is not less than 67.5% of the entire interface area, preferably, not less than 76%, preferably, not less than 86%, preferably, not less than 92.5%.

[0041] Preferably, the shear strength of the welded assembly is not less than 45 MPa, more preferably, the shear strength is not less than 50 MPa, and even more preferably, the shear strength is not less than 55 MPa.

[0042] A fourth aspect of the present invention is a method for producing a welded assembly, comprising:

[0043] Step A: Providing a first substrate having a first outer surface, a second substrate having a second outer surface, and a soldering pad, wherein the soldering pad comprises: a copper substrate having a first surface and a second surface opposite to each other; a first nanometal layer on the first surface of the copper substrate; and a second nanometal layer on a second surface of the copper substrate opposite to the first surface, wherein the yield strength of the soldering pad is no greater than 100 MPa;

[0044] Step B: placing the first nano-metal layer of the soldering sheet in surface contact with the first outer surface of the first substrate and placing the second nano-metal layer of the soldering sheet in surface contact with the second outer surface of the second substrate to form a stacked structure;

[0045] Step C: performing hot-press welding on the stacked structure to weld the first substrate, the second substrate and the welding piece together, thereby obtaining a welded assembly, wherein the shear strength of the welded assembly is not less than 40 MPa.

[0046] Preferably, in step C, hot-press welding is performed as follows: in a helium-protected environment, at a temperature of 250-350° C., pressurizing the stacked structure from both the top and bottom, with a pressure of 15-40 MPa, for a welding time of 10-30 minutes. Further preferably, the welding temperature is 250-300° C., or the pressure is 20-30 MPa, or the welding time is 10-20 minutes.

[0047] Preferably, when the first substrate and / or the second substrate are placed horizontally, the vertical difference between the highest point and the lowest point on the first outer surface and the second outer surface can be as high as 200 nm, eliminating the need for additional surface processing to obtain high flatness.

[0048] The description and preferred embodiments of the soldering tab in relation to the first aspect of the present invention are applicable to the second, third and fourth aspects of the present invention.

[0049] In summary, compared with the prior art, the present invention achieves the following technical effects:

[0050] 1) The present invention controls the yield strength of the solder sheet by softening the copper matrix. This allows the solder sheet to increase the effective soldering area of ​​the solder interface without requiring smoothing (e.g., wet polishing) of the rough soldering surface (i.e., the vertical difference between the highest and lowest points of the soldering surface when placed horizontally can be as much as 200nm), thereby enhancing the shear strength after soldering and improving soldering reliability. Therefore, the solder sheet of the present invention has improved tolerance to surface roughness and achieves higher shear strength.

[0051] 2) Compared with the soldering sheet prepared from nano copper particle film, the surface nano metal layer of the present invention has a high density, which improves the thermal conductivity and electrical conductivity of the soldering assembly; and

[0052] 3) The copper substrate of the soldering sheet of the present invention and the nanometal layer thereon have better adhesion, so that the soldering sheet can be subjected to secondary processing (such as cutting) to obtain a size and shape for a specific application to adapt to the expected application scenario, without the nanometal layer peeling off as in the case of nano-copper particle film. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] Exemplary embodiments of the present invention will now be described with reference to the accompanying drawings, in which:

[0054] FIG1 shows the height variation of the surface to be bonded of an example chip measured by an atomic force microscope in a direction perpendicular to the surface, wherein y is the height in the vertical direction and x is the length in the horizontal direction;

[0055] FIG2 shows the morphology comparison of the chip model and the solder tab model before and after pressurization in welding simulation 1;

[0056] FIG3 shows the morphology comparison of the chip model and the solder tab model before and after pressurization in welding simulation 2;

[0057] FIG4 shows the morphology comparison of the chip model and the solder tab model before and after pressurization in welding simulation 3;

[0058] FIG5 shows a comparison of the morphologies of the chip model and the solder tab model before and after pressurization in welding simulation 4;

[0059] FIG6 shows a scanning electron microscope (SEM) image of the surface morphology of the soft copper substrate of Sample 1 of Example S1;

[0060] FIG7 shows a scanning acoustic microscope image of the solder pad and chip of Sample 1 of Example S1 after soldering;

[0061] FIG8 shows an SEM image of the surface morphology of the soft copper substrate of Sample 1 of Example S2;

[0062] FIG9 shows an SEM cross-sectional view of the solder piece of sample 1 of example S2, wherein the W—Pt layer is a protective layer used for focused ion beam sample preparation and is not included in the original structure;

[0063] FIG10 shows a surface morphology SEM image of the nano-copper layer of the solder sheet of sample 1 of example S2;

[0064] FIG11 shows a scanning acoustic microscope image of the solder pad and chip of Sample 1 of Example S2 after soldering;

[0065] FIG12 shows an SEM image of the surface morphology of the soft copper substrate of Sample 1 of Example S3;

[0066] FIG13 shows a scanning acoustic microscope image of Sample 1 of Example S3 after soldering the solder pad to the chip;

[0067] FIG14 shows an SEM image of the surface morphology of the soft copper substrate of Sample 1 of Example S4;

[0068] FIG15 shows a scanning acoustic microscope image of Sample 1 of Example S4 after soldering the solder pad to the chip;

[0069] FIG16 shows an SEM image of the surface morphology of the soft copper substrate of Sample 1 of Example S5;

[0070] FIG17 shows a scanning acoustic microscope image of Sample 1 of Example S5 after soldering the solder pad to the chip;

[0071] FIG18 shows an SEM image of the surface morphology of the soft copper substrate of Sample 1 of Example S6;

[0072] FIG19 shows a scanning acoustic microscope image of Sample 1 of Example S6 after soldering the solder pad to the chip;

[0073] FIG20 shows an SEM image of the surface morphology of the soft copper substrate of Sample 1 of Example S7;

[0074] FIG21 shows a scanning acoustic microscope image of the solder pad and chip of Sample 1 of Example S7 after soldering;

[0075] FIG22 shows an SEM image of the surface morphology of the copper substrate of Sample 1 of Comparative Example C1;

[0076] FIG23 shows a scanning acoustic microscope image of Sample 1 of Comparative Example C1 after soldering the solder pad to the chip;

[0077] FIG24 shows an SEM image of the surface morphology of the copper substrate of Sample 1 of Comparative Example C2;

[0078] FIG25 shows a scanning acoustic microscope image of the soldering pad and chip of Sample 1 of Comparative Example C2 after soldering; and

[0079] FIG26 shows the relationship between the average yield strength of the solder piece and the average shear strength of the solder assembly (a), the average effective solder area ratio (b), the average grain size of the copper matrix (c), and the average elongation of the solder piece (d). DETAILED DESCRIPTION

[0080] The present invention will be described in more detail below with reference to exemplary embodiments. The following examples or experimental data are intended to illustrate the present invention by way of example, and it should be clear to those skilled in the art that the present invention is not limited to these examples or experimental data. Features or elements described in conjunction with or with respect to one embodiment are applicable to all embodiments, unless there is incompatibility of features. One or more features or elements from one embodiment may be incorporated into or combined with any other embodiment disclosed herein, and may include the features or elements extracted from the one embodiment to supplement or replace one or more features or elements of the other embodiments. The features or combination of features of the embodiments disclosed herein may be extracted in isolation from the other features of the embodiment. Alternatively, the features or combination of features of the embodiment may be omitted from the embodiment.

[0081] Those skilled in the art will understand that any range or value within each interval herein is applicable to the present invention. For example, a yield strength of a soldering piece within the range of 18-100 MPa means that the yield strength can be any range or any specific value within the range, for example, a yield strength of 18-95 MPa, 21-90 MPa, 28-90 MPa, 20-80 MPa, 22-70 MPa, 19-60 MPa, 20-55 MPa, 22-64 MPa, 25-42 MPa, 25-60 MPa, 28-82 MPa, or 23-58 MPa, and a yield strength of 23 MPa, 25 MPa, 26 MPa, 30 MPa, 35 MPa, 40 MPa, 42 MPa, 48 MPa, 55 MPa, 60 MPa, 65 MPa, 70 MPa, 76 MPa, 80 MPa, 88 MPa, 94 MPa, and the like.

[0082] In this document, the terms yield strength, tensile strength, and elongation are generally understood in the art. Specifically, yield strength refers to the limit of a sample's elastic behavior and the onset of plastic deformation, i.e., the stress at which a sample undergoes 0.2% deformation. Tensile strength refers to the stress at which a sample undergoes maximum uniform plastic deformation. Elongation is the material's ability to deform before fracture, representing the ratio of the total deformation ΔL of the gauge length after fracture to the original gauge length L.

[0083] In this article, the shear fracture test method is as follows: The welded assembly consists of a first substrate and a solder tab welded together, with the weld interface measuring 10 x 10 mm. The unwelded surface of the solder tab is fixed to a test platform with resin. A movable mechanical component presses against the side of the first substrate and applies a shear force parallel to the welded assembly at a speed of 1 mm / min. Five samples of each welded assembly are tested, and the average value is calculated.

[0084] In this paper, the effective welding area ratio is measured as follows: an acoustic scanning test is performed on a welded assembly with a welding area of ​​10×10 mm, where the dark area is the effective welding area and the light area is the delamination area, that is, the unsuccessful welding area. The effective welding area ratio is obtained by the ratio of the effective welding area to the overall area.

[0085] The present invention controls the yield strength of the welding piece so that the welding piece can undergo local yield deformation during the welding process to fit the welding surface of the component to be welded, thereby increasing the effective welding area and increasing the welding strength, solving the problem that the dense metal layer cannot adapt to the surface roughness of the component to be welded, resulting in low shear strength.

[0086] Specifically, in order to solve the above problems, the present invention simulates and estimates the yield strength required for the soldering sheet. Taking a conventional chip as an example of a component to be soldered, the inventors used an atomic force probe to measure the roughness of the surface to be soldered of different chips. The results showed that there were periodic wavy ups and downs in the direction perpendicular to the surface to be soldered of the chip, with a roughness Ra of 20 to 52 nm and a vertical difference between the highest point and the lowest point of 56 to 150 nm. Figure 1 shows the height fluctuation of the surface to be soldered of an example chip in a direction perpendicular to it. In order to quantify such fluctuations, the vertical value of the wavy fluctuations shown in Figure 1 can be simplified and simulated as the following curve:

[0087] Wherein, y represents the surface undulation in the thickness direction of the chip (ie, perpendicular to the welding interface); x represents the length along the interface to be welded.

[0088] To simulate hot-press welding, the maximum measured roughness was used as a reference, i.e., Ra = 52nm, with a vertical difference of approximately 150nm between the highest and lowest points. To increase product tolerance, the vertical difference between the highest and lowest points in the simulation was set to 200nm, i.e., a roughness greater than Ra = 52nm, with a period length of 10μm, resulting in the following curve:

[0089] The above curve is used to simulate the undulations of the surface of the chip to be soldered.

[0090] The welding simulation steps are as follows:

[0091] 1) A chip model and a solder pad model were constructed using the SolidWorks modeling software. The surface to be soldered on the chip model was rough, with a vertical difference of 200 nm between the highest and lowest points. The solder pad model consisted of a copper substrate and a nano-copper layer disposed on the copper substrate. The simulation assumed that diffusion and soldering would occur as long as the chip and solder pad models fit together. Therefore, the yield strength of the solder pad was considered as a whole.

[0092] 2) The nanocopper layer of the soldering pad model was brought into contact with the surface to be soldered of the chip model, simulating the initial state before hot pressing. At this point, because the surface to be soldered is rough, only the protruding portions of the surface to be soldered contact the nanocopper layer, resulting in an unbonded area between the two, which is shown in white in the figures.

[0093] 3) In the initial state, finite element simulation is used in the software to apply pressure in the vertical direction, and the stress and strain near the welding interface of the solder joint model and the chip model under the action of the vertical pressure are calculated. This is used to determine the yield strength range required to produce sufficient plastic deformation under the same pressure to match the surface roughness of the chip.

[0094] The chip model used in all simulations uses the same material parameters as the metal material in the database. The solder joint model uses copper material parameters with yield strength and tensile strength adjusted by annealing. The pressure range used in the simulated welding is based on the commonly used copper sintering welding pressure, which is 15 to 40 MPa.

[0095] Simulation 1: The yield strength of the solder pad model is 258 MPa. A pressure equivalent to 15 MPa was applied to the bottom of the solder pad model in the direction shown in Figure 2 (i.e., perpendicular to the surface to be bonded), while the top of the chip was restrained for static stress analysis. Figure 2 shows a comparison of the solder interface morphology before and after pressure application. The left image shows a white region between the nanocopper layer of the solder pad model and the surface to be bonded of the chip model, indicating that the two are not bonded. The right image also shows a white region at the same location, indicating that the region that was not bonded before pressure application remains unbonded after pressure application. The right image also shows the stress distribution in the system after pressure application. The grayscale scale on the far right compared to the grayscale of the solder pad region shows that the stress at the contact area between the chip surface to be bonded and the solder pad at the solder interface ranges from 9 to 13.6 MPa, far below the yield strength of the solder pad model (258 MPa). Therefore, the solder pad model cannot undergo plastic deformation to compensate for the fluctuations on the chip surface. It can be determined that under a welding pressure of 15 MPa, the yield strength of the welding piece must be at least less than 13.6 MPa in order for the welding piece to yield and fit the surface of the chip to be welded.

[0096] Simulation 2: The yield strength of the solder pad model is 258 MPa. A pressure equivalent to 40 MPa is applied to the bottom of the solder pad model in the direction shown (i.e., perpendicular to the surface to be bonded), while the top of the chip is restrained for static stress analysis. Figure 3 shows a comparison of the solder interface morphology before and after pressure application. Similar to Figure 2, there is no significant change in the unbonded portion before and after pressure application. Furthermore, the stress distribution in the system after pressure application (right figure) shows that the stress at the contact area between the chip surface to be bonded and the solder pad at the solder interface ranges from 76.8 to 152 MPa, far below the yield strength of the solder pad model (258 MPa). Therefore, the solder pad cannot undergo plastic deformation to compensate for the roughness fluctuations on the chip. Similarly, it can be determined that under a soldering pressure of 40 MPa, the yield strength of the solder pad must be at least less than 152 MPa for the solder pad to yield and conform to the chip surface to be bonded.

[0097] Simulation 3: The yield strength of the solder tab model is 18 MPa. A pressure equivalent to 15 MPa is applied to the bottom of the solder tab model in the direction shown (i.e., perpendicular to the surface to be soldered). The top of the chip is restrained for static stress analysis. The morphology of the solder interface before and after pressurization is shown in Figure 4. Compared to the state before pressurization (left figure), the unbonded portion in the state after pressurization (right figure) is significantly reduced, accounting for less than 10% of the entire solder interface. The solder tab model undergoes significant deformation at the solder interface. The stress distribution in the system after pressurization (right figure) shows that the stress in the contact area between the chip surface to be soldered and the solder tab at the solder interface ranges from 15 to 28 MPa, which is higher than the yield strength of the solder tab (18 MPa). This theoretically proves that a solder tab with a yield strength of 18 MPa can undergo plastic deformation to fit the chip under a pressure of 15 MPa.

[0098] Simulation 4: The yield strength of the solder tab model is 100 MPa. A pressure equivalent to 40 MPa is applied to the bottom of the solder tab model in the direction shown (i.e., perpendicular to the surface to be soldered). The top of the chip is restrained for static stress analysis. The morphology of the solder interface before and after pressurization is shown in Figure 5. Compared to the state before pressurization (left figure), the unbonded portion in the state after pressurization (right figure) is significantly reduced, accounting for less than 10% of the entire solder interface. The solder tab model undergoes significant deformation at the solder interface. The stress distribution in the system after pressurization (right figure) shows that the stress in the contact area between the chip surface to be soldered and the solder tab at the solder interface ranges from 84 to 146 MPa, which is higher than the yield strength of the solder tab (100 MPa). This theoretically proves that a solder tab with a yield strength of 100 MPa can undergo plastic deformation to fit the chip under a pressure of 40 MPa.

[0099] Based on the above simulation, the inventors found that by controlling the yield strength of the solder sheet to no more than 100 MPa, under different sintering pressures in the range of 15 to 40 MPa, the solder sheet can undergo local yielding to at least partially compensate for the roughness of the chip, thereby increasing the effective welding area and solving the problem of low shear strength caused by the low fit between the solder sheet and the surface of the chip to be welded. Preferably, the solder sheet as a whole still maintains a certain strength, thereby ensuring the welding strength while increasing the effective welding area. This is because the shear strength of the welding area is affected by the tensile strength of the solder sheet, and the tensile strength of the material is generally positively correlated with the yield strength, so a solder sheet with a higher yield strength should be used while ensuring that the solder sheet can undergo local yielding to fit the chip. Therefore, the present invention preferably requires that the yield strength of the solder sheet be no less than 18 MPa.

[0100] The improvement of the welding assembly by the welding sheet of the present invention will be described below with reference to specific examples.

[0101] The copper substrate of the solder sheet in each of Examples S1-S7 and Comparative Example C1 was obtained from a commercially available rolled copper foil having a thickness of 100 μm, a yield strength of 156 MPa, a tensile strength of 350 MPa, and an elongation of 7.8%. The copper substrate of the solder sheet in Comparative Example C2 was obtained from a commercially available rolled copper foil having a thickness of 100 μm, a yield strength of 202 MPa, a tensile strength of 380 MPa, and an elongation of 5.4%.

[0102] Preparation of solder pads

[0103] 1. Heat Treatment Step: The copper substrates of Examples S1-S7 were heat treated according to the parameters listed in Table 1 to obtain soft copper substrates. Samples of the obtained soft copper substrates were taken and photographed using a scanning electron microscope (see Figures 6, 8, 12, 14, 16, 18, and 20). The average grain sizes were measured according to methods known in the art and are listed in Table 1. The copper substrates of Comparative Examples C1-C2 were not heat treated. Their surface morphologies are shown in Figures 22 and 24. The average grain sizes of Comparative Examples C1-C2 were also measured according to methods known in the art and are listed in Table 1. In addition, for each Example and Comparative Example, the yield strength of five samples was tested and the average results were reported in Table 2.

[0104] Table 1 Heat treatment conditions of copper substrates of S1-S7 and C1-C2

[0105] 2. Deposition step: Electroplating is schematically used to deposit nano-copper layers on both surfaces of the soft copper substrates of S1-S7 and the copper substrates of C1-C2. Taking sample 1 of example S2 as an example, the electrolytic solution schematically used includes 120 g / L of anhydrous copper sulfate, 110 g / L of 98% mass fraction concentrated sulfuric acid, 100 mg / L of sodium chloride, 420 mg / L of PEG20000, and 25 mg / L of Janus Green B. The current density of the electroplating deposition is 0.08 A / cm 2 , the deposition time is 30 seconds, and the thickness of the obtained single-sided nano-copper layer is about 300nm, as shown in Figure 9, and the average grain size is about 30nm, as shown in Figure 10. Since the nano-copper layers of each sample of S1-S7 and C1-C2 are deposited on the corresponding copper substrate using the same process as sample 1 of S2, they will not be repeatedly characterized here. Alternatively, the nano-copper layer can be deposited only on a single side of the soft copper substrate / copper substrate. Optionally, at least two nano-metal layers can be deposited on at least one surface of the soft copper substrate, and the metal of the nano-metal layer can be selected from: copper, gold, nickel, silver, platinum, and titanium.

[0106] After deposition, solder sheets S1-S7 and C1-C2 were obtained, respectively. For each example and comparative example, five samples were tested and the average values ​​were calculated. The corresponding average yield strength, average tensile strength, and average elongation are listed in Table 2. Compared to the average yield strength of the copper substrate, the average yield strength of the solder sheets was only slightly higher than that of the copper substrate. This indicates that the average yield strength of the solder sheets is controlled by the copper substrate. Therefore, the expected yield strength of the solder sheets can be achieved by controlling the yield strength of the copper substrate.

[0107] Each soldering pad of S1-S7 includes: a copper substrate having a first and a second opposing surface; and two nano-copper layers deposited on the first and second surfaces of the copper substrate, respectively. The yield strength of the soldering pad is no greater than 100 MPa (see Table 2 for details). Similarly, each soldering pad of C1-C2 includes: a copper substrate having a first and a second opposing surface; and two nano-copper layers deposited on the first and second surfaces of the copper substrate, respectively. The yield strengths of the soldering pads are 157 MPa and 203 MPa, respectively.

[0108] Table 2 Properties of copper substrates and solder sheets of S1-S7 and C1-C2

[0109] Preferably, before deposition, the surfaces of the soft copper substrates of S1-S7 and the copper substrates of Comparative Examples C1-C2 were cleaned with dilute hydrochloric acid in a ratio of HCl:H₂O = 1:1 to remove any scale, etc. It will be appreciated that other methods can be used to deposit a nanometal layer on the surface of the copper substrate, such as evaporation, vapor deposition (e.g., magnetron sputtering), ion plating, etc. It will also be appreciated that the present invention is not limited to nanocopper layers; nanogold layers, nanosilver layers, nanonickel layers, nanotitanium layers, and nanoplatinum layers may also be deposited.

[0110] Preparation of welded assemblies

[0111] Soldering steps: First, the nano-copper layers of the solder pads S1-S7 and C1-C2 are placed face-to-face with the surfaces to be soldered of the two chips (which have not been subjected to additional treatment to obtain high flatness, so the vertical difference between the highest point and the lowest point on the surface to be soldered can be as high as 200nm); then hot pressing welding is performed in a direction perpendicular to the surface to be soldered, wherein the welding vacuum degree is 1×10 -3 Torr (for example, in a helium atmosphere), a welding temperature of 280°C, a welding time of 15 minutes, and a welding pressure of 25 MPa, thereby obtaining a welded assembly according to the present invention. It will be understood that the welding parameters are not limited thereto; for example, the welding temperature may be 250-350°C, the pressure may be 15-40 MPa, and the welding time may be 10-30 minutes. Further preferably, the welding temperature is 250-300°C, or the pressure is 20-30 MPa, or the welding time is 10-20 minutes.

[0112] Each soldering assembly of S1-S7 includes: a first chip; a second chip; and a soldering portion located between the first chip and the second chip to connect the two, wherein the soldering portion includes a copper substrate, a first soldering interface on a first side of the copper substrate, and a second soldering interface on a second side of the copper substrate opposite to the first side, the first soldering interface and the second soldering interface being formed by bonding the nanometal on opposite sides of the copper substrate to the first chip and the second chip, respectively, wherein the shear strength of the soldering assembly is not less than 40 MPa (see Table 3). It will be understood that the chips in the soldering assembly can be replaced by other components, such as a copper-clad ceramic substrate, a heat sink, and the like.

[0113] To test the effective soldering area between the solder tab and the component to be soldered and the shear strength of the soldered assembly, a single chip and solder tab were soldered according to the above method (hereinafter referred to as a single-sided soldered assembly). The following effective soldering area ratio and shear strength test samples are single-sided soldered assemblies (i.e., only one soldering interface) to avoid the inability to accurately determine the unsoldered area on each side due to overlapping soldering areas in double-sided soldering. It will be understood that the measurement results of the single-sided soldered assembly will apply to each soldering interface of the double-sided soldered assembly.

[0114] Effective welding area rate: Taking sample 1 of S1 as an example, the welding position (welding interface 10×10mm) of the single-sided welded component obtained therefrom was subjected to acoustic scanning detection. Figure 7 shows the scanning results of sample 1 of S1, where the box indicates the welding position. Within the box, the dark part is the effective welding area, and the area circled by the irregular dotted edge is the delamination area, that is, the area where no welding (non-bonding) occurred. Based on the proportion of the unwelded area to the entire weld area, the effective welding area rate was calculated to be 94.8% and is listed in Table 3. Similarly, the effective welding area rate was measured for 5 single-sided welded components of S1-S7 and C1-C2 to obtain the average value, which is listed in Table 3.

[0115] Shear strength test: According to the shear strength test method described in this article, the five samples of the single-sided welded assemblies of S1-S7 and C1-C2 were tested to obtain the average shear strength values, which are listed in Table 3.

[0116] Table 3 Effective welding area ratio and shear strength of single-sided welded assemblies AS1-AS7 and AC1-AC2 welded by S1-S7 and C1-C2

[0117] The yield strength of the soldering pads S1-S7 of the present invention ranges from 18 to 100 MPa. In comparison, the yield strengths of the soldering pads C1 and C2 are 157 MPa and 203 MPa, respectively. The welded assemblies AS1-AS7 obtained using the S1-S7 soldering pads have an average effective weld area ratio of no less than 69% (AS7), an increase of at least 44% compared to AC1 and over 70% compared to AC2. Furthermore, the average shear strength is no less than 40.2 MPa, an increase of at least 28% compared to AC1 and more than double that of AC2. Thus, by controlling the yield strength of the soldering pads, the present invention effectively addresses the issues of small effective weld area and low shear strength at the weld interface of welded assemblies, which arise without additional surface treatment to achieve high flatness.

[0118] For AS1-AS7, as the yield strength increases, the shear strength of the final welded assembly first increases to 57.3 MPa, and then gradually decreases to 40.2 MPa. The effective weld area ratio shows a similar pattern. Based on the experimental data, the relationship between the average yield strength of the weld and the average shear strength of the welded assembly, the average effective weld area ratio, the average grain size of the copper matrix of the weld, and the average elongation of the weld was fitted, as shown in Figure 26. The goodness of fit of each curve R 2 The values ​​are all close to 1, indicating a good fit. The following analysis combines the fitting curves with various examples.

[0119] Overall, by controlling the yield strength of the solder tab to 18-100 MPa, the shear strength of the resulting welded assembly is no less than 40 MPa, and the effective welding area ratio is no less than 67.5%. Correspondingly, the present invention controls the yield strength of the solder tab by controlling the yield strength of the copper substrate of the solder tab. Preferably, the yield strength of the copper substrate can be controlled by controlling the grain size of the copper substrate. In this case, in order to control the yield strength of the solder tab to 18-100 MPa, the average grain size of the copper substrate is in the range of 30-140 μm, and correspondingly, the elongation of the solder tab is no less than 11.5%.

[0120] Comparing Figures 17, 19, and 21 (AS5-AS7) with Figures 7, 11, 13, and 15 (AS1-AS4), it can be seen that the unwelded areas in AS5-AS7 are larger than those in AS1-AS4 and occur primarily at the edges of the solder interface. This is because the solder tabs used in AS5-AS7 have a higher yield strength. While localized plastic deformation can occur during soldering, the uneven stress at the edges, compared to the uniform stress in the center, makes it difficult for the relatively high-yield-strength solder tabs to undergo proper plastic deformation, resulting in a poor conformity to the rough surface of the chip in these areas. Unwelded areas at the edges are more likely to become failure initiation points than unwelded areas not at the edges. Therefore, in order to minimize the unwelded area from the edges of the solder interface to ensure a shear strength of no less than 45 MPa, based on the fitting curve, the yield strength of the solder tab is preferably set between 18 and 67.5 MPa. This results in an effective solder area ratio of no less than 76%. Correspondingly, preferably, in order to control the yield strength of the solder piece to be 18-67.5 MPa, the average grain size of the copper matrix is ​​in the range of 50-140 μm, and the elongation of the solder piece is not less than 23%.

[0121] Comparing AS1 (Figure 7) and AS4 (Figure 15), although the weld area of ​​AS1 is significantly larger than that of AS4 (increased by approximately 12.4%), the shear strength of the two is almost the same. This is because, as can be observed from Figure 7, the unwelded area of ​​AS1 is long, crescent-shaped and extends continuously along the diagonal of the weld area. In contrast, the unwelded area of ​​AS4, as can be seen in Figure 15, is scattered and does not have a continuous, long, unwelded area. Therefore, under the same shear test, the unwelded area of ​​AS1 that extends continuously along the diagonal of the weld area weakens the effect of the increased weld area, resulting in a final shear strength that is almost the same as that of AS4. The long, crescent-shaped unwelded area is due to the low yield strength of the weld sheet, which leads to excessive deformation or even tearing in the local area. The presence of cracks is not conducive to shear strength and also poses a threat to the reliability of subsequent use. Therefore, to further avoid continuous unwelded areas such as long crescent-shaped areas and increase the shear strength to no less than 50 MPa, based on the fitting curve, the yield strength of the solder tab is preferably set between 20 and 46.5 MPa. This results in an effective solder area ratio of no less than 86%. Correspondingly, preferably, the average grain size of the copper matrix is ​​controlled within the range of 75 to 122.5 μm to achieve a solder tab yield strength of 20 to 46.5 MPa, with an elongation of 27.5 to 36%.

[0122] The effective weld area ratio and shear strength of AS2 and AS3 are significantly higher than those of the other examples, making them the preferred solutions in the present invention. Compared to AS2, while AS3 has a similar effective weld area ratio, its shear strength is approximately 4.6% higher. The shear strength of AS3 is superior to AS2 because the yield strength of the solder pad used in AS3 is increased from 24.3 MPa, the 24.3 MPa of the S2 pad, to 31.1 MPa. This not only meets the deformation requirements of local yielding under the current sintering pressure (25 MPa), but also brings about a simultaneous increase in tensile strength through the increased yield strength, thereby increasing the strength of the solder pad and, in turn, the shear strength of the weld area. In other words, while achieving a similar effective weld area, selecting a higher yield strength, i.e., a higher tensile strength, can result in higher shear strength. Therefore, to further improve the shear strength to no less than 55 MPa, based on the fitting curve, it is preferred that the yield strength of the solder pad be 23 to 36 MPa, thereby achieving an effective weld area ratio of no less than 92.5%. Preferably, the average grain size of the copper matrix is ​​controlled within the range of 90 to 115 μm to obtain a solder sheet yield strength of 23 to 36 MPa, and an elongation of 29 to 34%.

[0123] In view of the above, the present invention controls the yield strength of the welding piece so that it can undergo local deformation during the welding process, thereby improving the fit between the welding piece and the welding surface of the component to be welded that does not require additional flattening, thereby increasing the effective welding area of ​​the welding interface and improving the shear strength of the resulting welded assembly and its service stability.

[0124] The above embodiments and experimental data are intended to illustrate the present invention by way of example. It should be clear to those skilled in the art that the present invention is not limited to these embodiments, and various modifications may be made without departing from the scope of protection of the present invention.

Claims

1. A welding sheet, comprising: a copper substrate having opposing first and second surfaces; and at least one nanometal layer deposited on at least one of the first surface and the second surface of the copper substrate, Wherein, the yield strength of the welding piece is not greater than 100 MPa.

2. The soldering sheet according to claim 1, wherein: The yield strength of the welding piece is in the range of 18 to 100 MPa, preferably in the range of 18 to 67.5 MPa, preferably in the range of 20 to 46.5 MPa, and more preferably in the range of 23 to 36 MPa.

3. The soldering sheet according to claim 1 or 2, wherein: The average grain size of the copper matrix is ​​in the range of 30 to 140 μm, preferably in the range of 50 to 140 μm, preferably in the range of 75 to 122.5 μm, and more preferably in the range of 92 to 115 μm.

4. The soldering sheet according to claim 1 or 2, wherein: The elongation of the welding piece is not less than 11.5%, preferably not less than 23%, preferably in the range of 27.5% to 36%, and more preferably in the range of 29% to 34%.

5. The soldering sheet according to claim 1 or 2, wherein: The average grain size of the nanometal layer is in the range of 5 to 500 nm, preferably in the range of 5 to 100 nm; and the average thickness of the nanometal layer is in the range of 100 nm to 10 μm, preferably in the range of 500 nm to 5 μm.

6. The soldering sheet according to claim 1 or 2, wherein: The metal of the nano-metal layer may be selected from: copper, gold, nickel, silver, platinum, and titanium, wherein at least two stacked nano-metal layers are provided on at least one of the first surface and the second surface.

7. A method for preparing a solder sheet, comprising: Step A: providing a copper substrate having a first surface and a second surface opposite to each other; Step B: annealing the copper substrate under vacuum to obtain a soft copper substrate, wherein the average grain size of the soft copper substrate is in the range of 30 to 140 μm; Step C: depositing at least one nanometal layer on at least one of the first surface and the second surface of the soft copper substrate to obtain the soldering sheet.

8. The method according to claim 7, wherein: The yield strength of the soft copper matrix is ​​not higher than 100 MPa and the yield strength of the solder sheet is in the range of 18 to 100 MPa, preferably in the range of 18 to 67.5 MPa, preferably in the range of 20 to 46.5 MPa, and more preferably in the range of 23 to 36 MPa; wherein the average grain size of the copper matrix is ​​in the range of 50 to 140 μm, preferably in the range of 75 to 122.5 μm, and more preferably in the range of 92 to 115 μm.

9. The method according to claim 7 or 8, wherein: In step B, the vacuum degree is 1.0×10 -3 Preferably, the annealing temperature is 400-850°C, and the holding time is 2-16 hours; more preferably, the annealing temperature is 500-800°C, and the holding time is 6-12 hours.

10. The method according to claim 7 or 8, wherein: The average grain size of the nanometal layer is in the range of 5 to 500 nm, preferably in the range of 5 to 100 nm.

11. The method according to claim 7 or 8, comprising depositing at least two superimposed nanometal layers on at least one of the first surface and the second surface, wherein: The metal of the nanometal layer can be selected from: copper, gold, nickel, silver, platinum, and titanium.

12. The method according to claim 7 or 8, wherein: The nanometal layer is a nanocopper layer, which is deposited by electroplating as follows: the electrolytic solution contains 100-150 g / L of anhydrous copper sulfate, 80-150 g / L of 98% mass fraction concentrated sulfuric acid, 50-150 mg / L of sodium chloride, 350-480 mg / L of PEG20000, and 20-40 mg / L of Janus Green B, wherein the current density of the electroplating deposition is 0.05-0.15 A / cm 2 , the deposition time is 10 to 300 seconds.

13. A welding assembly comprising: a first substrate; a second substrate; as well as A welding portion located between the first substrate and the second substrate to connect the two, wherein the welding portion includes a copper substrate, a first welding interface on a first side of the copper substrate, and a second welding interface on a second side of the copper substrate opposite to the first side, the first welding interface and the second welding interface are formed by bonding the nanometal on the opposite sides of the copper substrate to the first substrate and the second substrate, respectively. Wherein, the shear strength of the welding assembly is not less than 40MPa.

14. The welding assembly according to claim 13, wherein: The average grain size of the copper matrix is ​​in the range of 30 to 140 μm, preferably in the range of 50 to 140 μm, preferably in the range of 75 to 122.5 μm, and more preferably in the range of 92 to 115 μm.

15. The welding assembly according to claim 13 or 14, wherein: The effective welding area of ​​the first welding interface and / or the second welding interface is not less than 67.5% of the entire interface area, preferably, not less than 76%, and more preferably, not less than 86%.

16. The welding assembly according to claim 13 or 14, wherein: The shear strength of the welded assembly is not less than 45 MPa, preferably, the shear strength is not less than 50 MPa, and more preferably, not less than 55 MPa.

17. A method of producing a welded assembly, comprising: Step A: providing a first substrate having a first outer surface, a second substrate having a second outer surface, and a soldering sheet, wherein the soldering sheet comprises: a copper substrate having a first surface and a second surface opposite to each other; a first nanometal layer on the first surface of the copper substrate; and a second nanometal layer on the second surface of the copper substrate, wherein the yield strength of the soldering sheet is not greater than 100 MPa; Step B: placing the first nano-metal layer of the soldering sheet in surface contact with the first outer surface of the first substrate and placing the second nano-metal layer of the soldering sheet in surface contact with the second outer surface of the second substrate to form a stacked structure; Step C: hot-pressing the stacked structure to weld the first substrate, the second substrate and the welding sheet together, thereby obtaining a welded assembly, wherein the shear strength of the welded assembly is not less than 40 MPa.

18. The method according to claim 17, wherein: In step C, the hot pressing welding is performed as follows: in a helium protective environment at a temperature of 250 to 350° C., pressurizing is performed from the top and bottom of the stacked structure, the pressure is 15 to 40 MPa, and the heat preservation time is 10 to 30 minutes.

19. The method according to claim 17, wherein: When the first substrate and / or the second substrate is placed horizontally, the vertical difference between the highest point and the lowest point on the first outer surface and the second outer surface does not exceed 200 nm.

20. The method according to any one of claims 17 to 19, wherein: The yield strength of the solder sheet is in the range of 18 to 100 MPa, preferably in the range of 18 to 67.5 MPa, preferably in the range of 20 to 46.5 MPa, and more preferably in the range of 23 to 36 MPa; wherein the average grain size of the copper matrix is ​​in the range of 30 to 140 μm, preferably in the range of 50 to 140 μm, preferably in the range of 75 to 122.5 μm, and more preferably in the range of 92 to 115 μm.