Wettability control agent for rock surfaces and evaluation method therefor

MYPI2025004605A0Undetermined Publication Date: 2024-07-31NISSAN CHEM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025004605
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-01-31
Filing Date
2024-01-31
Publication Date
2024-07-31

AI Technical Summary

Technical Problem

Current methods for improving rock surface wettability in enhanced oil recovery (EOR) processes are inadequate, leading to inefficient fluid movement and retention, and existing sensors for evaluating wettability are not effective in saltwater environments.

Method used

A wettability modifier comprising silica particles with a DLS average diameter of 5 to 200 nm, partially coated with a silane compound having hydrophilic organic groups, applied through conformal coating to make rock surfaces hydrophilic, along with a QCM method for evaluating wettability changes.

Benefits of technology

The wettability modifier effectively reduces the contact angle of crude oil on rock surfaces, enhancing fluid storage and flow paths while maintaining salt resistance, allowing for hydrophilic fluid flow without causing blockages in saltwater environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025004605_DRAWING_001
    Figure PI2025004605_DRAWING_001
  • Figure PI2025004605_DRAWING_002
    Figure PI2025004605_DRAWING_002
  • Figure PI2025004605_DRAWING_003
    Figure PI2025004605_DRAWING_003
Patent Text Reader

Abstract

[Problem] To provide a wettability control agent for rock surfaces, which is able to make rock surfaces hydrophilic through conformal coating. [Solution] A wettability control agent for rock surfaces, which makes rock surfaces hydrophilic through conformal coating, comprising silica particles (a) having a DLS average particle diameter of 5 to 200 nm, which is determined by a dynamic light scattering method, and an aqueous medium (b), wherein at least some of the silica particles are coated with a silane compound (c) having a hydrophilic organic group, a method for controlling wettability of rock surfaces using the wettability control agent and a method for evaluating wettability of rock surfaces by applying the wettability control agent. FIG. 1
Need to check novelty before this filing date? Find Prior Art

Description

Wettability control agent for rock surface and its evaluation method

[0001] The present invention relates to a wettability modifier for rock surfaces and a method for evaluating the same, and more particularly to a wettability modifier that hydrophilizes rock surfaces by conformal coating, and a method for evaluating changes in surface wettability (hydrophilization) due to the conformal coating using the QCM (Quartz Crystal Microbalance) method.

[0002] Because silica particles have high hardness and heat resistance, they are widely used as a modifier blended into resins, etc., to impart hardness and heat resistance to the resin. In recent years, silica particles have been used in enhanced oil recovery (EOR) flooding, in which silica particles are injected into an oil reservoir in an inland or offshore oil field to recover crude oil. For example, in anticipation of improving the effectiveness of stripping crude oil from the rock surface, proposals have been made to improve the crude oil recovery rate by blending fine particles such as aqueous silica sol (colloidal silica) into a crude oil recovery solution (Patent Document 1).

[0003] Recently, there has been a demand for more effective means of improving the wettability of rock surfaces to facilitate smoother fluid movement within underground rock masses. Improving the wettability of rock surfaces can contribute not only to fluid movement but also to fluid retention. Known sensors for evaluating wettability include QCM sensors using quartz crystal oscillators.

[0004] A quartz crystal oscillator vibrates when a voltage is applied, resulting in an inverse piezoelectric phenomenon. It is also known that the resonant frequency of the quartz crystal oscillator changes when a substance adheres to the surface of the quartz crystal oscillator or when the adhered substance peels off, causing a change in the weight of the quartz crystal oscillator. A QCM sensor measures the weight and concentration of the adhered substance based on this frequency change. Various sensors utilizing these properties of quartz crystal oscillators have been proposed. For example, a concentration sensor has been disclosed that detects the concentration of a target substance in a mixed solution consisting of a specific target substance dissolved in a specific solvent. The sensor includes a quartz crystal oscillator whose natural frequency changes in response to changes in the target substance concentration, and an oscillation circuit that drives the quartz crystal oscillator. The quartz crystal oscillator is immersed in the mixed solution and oscillated, and the natural frequency of the quartz crystal oscillator is measured to determine the concentration of the target substance in the mixed solution (Patent Document 1).

[0005] International Publication No. 2019 / 054414 JP 6-18394 Publication

[0006] The present invention provides a rock surface wettability control agent that can make rock surfaces hydrophilic by conformal coating. The present invention also provides a rock surface wettability control agent, a method for controlling rock surface wettability using the same, and a method for evaluating the wettability of rock surfaces after application of the wettability control agent.

[0007] The present invention provides, as a first aspect, a wettability control agent for hydrophilizing a rock surface by conformal coating, the wettability control agent for rock surfaces comprising (a) silica particles having a DLS average particle size of 5 to 200 nm as determined by dynamic light scattering and (b) an aqueous medium, at least a portion of the silica particles being coated with (c) a silane compound having a hydrophilic organic group; and, as a second aspect, the wettability control agent for rock surfaces according to the first aspect, wherein the hydrophilic organic group is an epoxy group-containing organic group, an amino group-containing organic group, a hydroxy group-containing organic group, or a carboxy group-containing organic group. As a third aspect, the wettability adjuster for rock surfaces according to the first or second aspect, wherein in a test method in which a sensor having an electrode layer and a quartz layer stacked on a quartz oscillator is resonated in a medium containing salt water containing calcium ions and magnesium ions and a wettability adjuster for the rock surface, a value (F3) obtained by subtracting a ΔF value (F1) indicating a weight change in an accumulation layer containing silica components accumulated on the sensor surface from the start of resonance until 2000 seconds from the start of resonance until 12000 seconds from the start of resonance, is −20 to 20 when the resonance frequency of the quartz oscillator is 25 MHz; As a fourth aspect, the rock surface wettability modifier according to any one of the first to third aspects, wherein, in an evaluation of the wettability of a rock surface by contacting a volume of 0.01 to 1 μL of crude oil with the underside of a rock slab in brine containing the rock surface wettability modifier, the contact angle between the outer surface of the crude oil droplet and the rock slab is reduced by 3° or more compared to the same contact angle evaluated in brine not containing the wettability modifier; As a fifth aspect, the rock surface wettability modifier according to the third or fourth aspect, wherein the brine contains sodium ions and has a salinity of 0.1 to 30 mass %; As a sixth aspect, the rock surface wettability modifier according to the third aspect, wherein the resonant frequency of the quartz crystal oscillator is in the range of 1 MHz to 100 MHz; As a seventh aspect, the rock surface wettability modifier according to the first aspect, which is a wettability modifier for storing fluids in rock masses or ensuring flow paths within rock masses; As an eighth aspect, the wettability adjuster for a rock surface according to the seventh aspect, wherein the fluid is a gas or liquid containing carbon dioxide, an aqueous fluid, or an aqueous fluid containing rock particles of 10 μm or less;As a ninth aspect, there is provided a method for adjusting the surface wettability of rock, comprising adjusting the rock surface wettability adjuster according to any one of the first to eighth aspects in an aqueous medium to a silica particle concentration of 0.1 to 30 mass % and applying the resultant to a rock surface. As a tenth aspect, there is provided a method for evaluating the wettability of a rock surface, comprising contacting a 0.01 to 1 μL volume of crude oil with the bottom of a rock slab in salt water containing the rock surface wettability adjuster according to any one of the first to third aspects, and evaluating the contact angle between the outer surface of the crude oil droplet and the rock slab.

[0008] The rock surface wettability modifier of the present invention can hydrophilize rock surfaces through conformal coating. Furthermore, because the rock surface wettability modifier of the present invention also has excellent salt resistance, it can be used on rock surfaces in saltwater environments. Therefore, the wettability modifier can be injected into underground rock masses in saltwater environments, for example, without aggregation, and is expected to hydrophilize the rock surface through conformal coating. This can be expected to ensure a hydrophilic fluid flow path without risking formation blockage, while contributing to the retention of hydrophobic fluids and the removal of crude oil and other materials from rock surfaces. Furthermore, the wettability evaluation method of the present invention can evaluate the wettability of rock surfaces imparted by the wettability modifier.

[0009] FIG. 1 shows the results of measurement of the frequency change value ΔF, which indicates weight change (weight change of the accumulation layer containing a silica component), detected by a QCM sensor in Examples 1, 2, and 3 (test fluids 1 to 3). FIG. 2 shows the results of measurement of the frequency change value ΔF, which indicates weight change (weight change of the accumulation layer containing a silica component), detected by a QCM sensor in Examples 7, 8, 9, and 10 (test fluids 4 to 7). FIG. 3 shows the results of measurement of the frequency change value ΔF, which indicates weight change (weight change of the accumulation layer containing a silica component), detected by a QCM sensor in Comparative Examples 1 and 2 (test fluids 8 and 9). FIG. 4 shows a schematic diagram of three-state contact angle measurement ( FIG. 4(A) ) and a schematic diagram of wettability ( FIG. 4(B) ). FIG. 5 shows the shapes of crude oil droplets used to measure contact angles (a) obtained with the test fluids (test fluids 1-3, 8, 4-7) of Examples 1-3 and Comparative Example 1, and Examples 7-10 in Evaluation of Wettability Changes of a Substrate (Berea Sandstone) in a Liquid Dispersion Medium-1, as well as the shape of a crude oil droplet of a blank (contact angle (b)). FIG. 6 shows the shapes of crude oil droplets used to measure contact angles (a) obtained with the test fluid (test fluid 1) of Example 4 in Evaluation of Wettability Changes of a Substrate (calcite) in a Liquid Dispersion Medium-2, as well as the shape of a crude oil droplet of a blank (contact angle (b)). FIG. 7 shows the shapes of crude oil droplets used to measure contact angles (a) obtained with the test fluids (test fluids 1 and 2) of Examples 5 and 6 in Evaluation of Wettability Changes of a Substrate (glass slide) in a Liquid Dispersion Medium-3, as well as the shape of a crude oil droplet of a blank (contact angle (b)).

[0010] [Rock Surface Wettability Control Agent] The present invention relates to a rock surface wettability control agent (hereinafter simply referred to as wettability control agent) that makes a rock surface hydrophilic by conformal coating.

[0011] When nanoparticles are coated by adsorption onto a substrate, particle adsorption to the substrate, including particle aggregation, can continue until the supply of nanoparticles is cut off. While this is expected to result in a thicker nanoparticle coating layer and better nanoparticle performance, it is undesirable when coating nanoparticles in narrow flow channels, for example, because it can lead to blockage of the flow channel. In the case of coating with the wettability modifier targeted by the present invention, as described below, results have been obtained suggesting that although nanoparticles (silica particles) adsorb to the rock surface, the amount of adsorption saturates at a certain level, and that further adsorption hardly occurs even when nanoparticles are subsequently supplied. In other words, conformal coating in this invention refers to coating in which the coating agent (wettability modifier) ​​adsorbs to the surface in a uniform, thin layer, such as a monolayer, with the amount of adsorption saturated at a certain level. Examples of rocks that can be hydrophilized by the wettability adjuster of the present invention include sedimentary rocks and igneous rocks, and examples of sedimentary rocks include conglomerate, sandstone, siltstone, mudstone, limestone, carbonate rock, and chert, while examples of igneous rocks include basalt, andesite, dacite, rhyolite, dolerite, porphyrite, quartz porphyry, gabbro, diorite, and granite. Minerals that make up these rocks (quartz, calcite, olivine, pyroxene, amphibole, mica, feldspar, etc.) and glass can also be hydrophilized by the wettability adjuster of the present invention, and for convenience in the present invention, these are also treated as rocks in the broad sense.

[0012] The wettability control agent of the present invention comprises (a) silica particles having an average DLS particle size of 5 to 200 nm as measured by dynamic light scattering (DLS) and (b) an aqueous medium, at least a portion of which is coated with (c) a silane compound having a hydrophilic organic group.

[0013] As an embodiment of the (a) silica particles and (b) aqueous medium, for example, an aqueous silica sol can be used. The aqueous silica sol is a colloidal dispersion system in which an aqueous solvent (i.e., the (b) aqueous medium) is used as a dispersion medium and colloidal silica particles (i.e., the (a) silica particles) are used as a dispersoid, and can be produced by a known method using water glass (aqueous sodium silicate solution) as a raw material.

[0014] In the present invention, the average primary particle diameter of (a) silica particles can be, for example, 5 to 100 nm. As described above, the average primary particle diameter of aqueous silica sol, which is an example of an embodiment of (a) silica particles and (b) aqueous medium, refers to the average primary particle diameter of colloidal silica particles, which are dispersoids. In the present invention, the average primary particle diameter of aqueous silica sol (colloidal silica particles) refers to the specific surface area diameter or Sears method particle diameter measured by the nitrogen adsorption method (BET method), unless otherwise specified. The specific surface area diameter (average particle diameter (specific surface area diameter) D (nm)) measured by the nitrogen adsorption method (BET method) is calculated by multiplying the specific surface area S (m 2 From the particle size (D / g), the particle size is given by the formula D(nm) = 2720 / S. The Sears particle size refers to the average particle size measured based on the literature: G. W. Sears, Anal. Chem. 28(12) 1981, 1956, Rapid Method for Measuring Colloidal Silica Particle Size. Specifically, when 1.5 g of SiO 2 The equivalent diameter (specific surface area diameter) is calculated from the specific surface area of ​​the colloidal silica, which is determined from the amount of 0.1 N NaOH required to titrate colloidal silica equivalent to 100% of the total weight of the colloidal silica from pH 4 to pH 9. In the present invention, the average primary particle diameter of the (a) silica particles, i.e., for example, aqueous silica sol (colloidal silica particles), as determined by the nitrogen adsorption method (BET method) or the Sears method is, for example, 5 to 100 nm, and can also be, for example, 5 to 70 nm, 5 to 60 nm, 5 to 50 nm, or 5 to 30 nm.

[0015] The (a) silica particles in the (b) aqueous medium containing the (a) silica particles of the present invention, i.e., the (a) silica particles in the wettability modifier or in a fluid sample obtained by mixing the wettability modifier with salt water or the like, can be measured by dynamic light scattering to determine their average particle size (DLS average particle size) and their dispersion state (whether the silica particles are dispersed or aggregated). The DLS average particle size represents the average value of the secondary particle size (dispersed particle size), and the DLS average particle size in a completely dispersed state is said to be about twice the average primary particle size (the specific surface area diameter obtained by measurement using the nitrogen adsorption method (BET method) or the Sears method, and represents the average value of the primary particle size). The larger the DLS average particle size, the more it can be determined that the silica particles in the medium are in an aggregated state. For example, an example of an aqueous silica sol is the aqueous silica sol Snowtex (registered trademark) ST-O manufactured by Nissan Chemical Industries, Ltd., which has an average particle size (BET method) of 10 to 11 nm and a DLS average particle size of 15 to 20 nm. As shown in the examples described below, the silica sol (wettability modifier) ​​of a synthetic example prepared using this aqueous silica sol and the test fluid (salt-resistant sample) containing it have a DLS average particle size of 25 nm or less, indicating that the silica particles are substantially dispersed in the medium. In the present invention, the average particle size (DLS average particle size) of (a) the silica particles is 5 to 200 nm, for example, 5 to 100 nm, 1 to 100 nm, 5 to 50 nm, 5 to 30 nm, 5 to 15 nm, or 5 to 70 nm. By making the DLS particles larger than 5 nm, the particles do not aggregate in the aqueous silica sol and become more stable, and by making the DLS particles smaller than 200 nm, they can easily penetrate narrow channels such as the pores of sandstone and carbonate rock present in underground oil field layers.

[0016] Particles with a DLS average particle size larger than 200 nm may not penetrate the narrow flow path and may clog it. Therefore, when considering applications in such narrow flow paths, it is preferable to use an aqueous silica sol that does not contain coarse particles, for example, a silica sol whose cumulative particle size distribution D90 of the average particle size (DLS average particle size) measured by dynamic scattering of silica particles is 5 to 200 nm, e.g., 5 to 150 nm, or e.g., 5 to 100 nm, or e.g., 5 to 70 nm. The D90 is the particle size that represents the cumulative 90% of the cumulative particle size distribution from the fine particle side. In the present invention, for example, the cumulative particle size distribution value can be measured by particle size distribution using image analysis. In measuring particle size distribution using image analysis, the measurement sample is analyzed as a transmission electron microscope image. Methods for analyzing the D value include the number distribution method and the volume distribution method. The number distribution method captures particles as perfect circles with the same area as the particle and measures the percentage of particles with a specific particle size within a certain field of view. In the volume distribution method, assuming that the volume and weight are proportional when the particle density is constant, the mass percentage of particles of a specific particle size present in a given amount of sample is measured. In the present invention, it is preferable to determine the D value (D90) by the volume distribution method.

[0017] The aqueous silica sol can be a commercially available product. Aqueous silica sols with a silica concentration of 5 to 50% by mass are generally commercially available, which is preferred because they are easily available. Aqueous silica sols include alkaline aqueous silica sols and acidic aqueous silica sols, and both can be used, but acidic aqueous silica sols are preferred. Examples of commercially available acidic aqueous silica sols include Snowtex (trade name) ST-OXS, ST-OS, ST-O, and ST-OL.

[0018] In the wettability adjuster of the present invention, the (a) silica particles are at least partially coated with (c) a silane compound having a hydrophilic organic group.

[0019] In the present invention, "coated with a silane compound" refers to an embodiment in which the surface of a silica particle is coated with a silane compound, and also includes an embodiment in which a silane compound is bonded to the surface of a silica particle. "An embodiment in which a silane compound is coated on the surface of a silica particle" may refer to an embodiment in which a silane compound coats at least a portion of the surface of a silica particle, i.e., an embodiment in which the silane compound covers a portion of the surface of a silica particle, and an embodiment in which the silane compound covers the entire surface of a silica particle. This embodiment does not require bonding between the silane compound and the surface of a silica particle. Furthermore, "an embodiment in which a silane compound is bonded to the surface of a silica particle" may refer to an embodiment in which a silane compound is bonded to at least a portion of the surface of a silica particle, i.e., an embodiment in which the silane compound is bonded to a portion of the surface of a silica particle and covers at least a portion of the surface, and an embodiment in which the silane compound is bonded to the entire surface of a silica particle and covers the entire surface.

[0020] The (c) silane compound may be a silane compound having a hydrophilic organic group such as an epoxy group-containing organic group, an amino group-containing organic group, a hydroxy group-containing organic group, or a carboxy group-containing organic group. In addition to the hydrophilic organic group, the (c) silane compound preferably has a hydrolyzable group such as an alkoxy group, an acyloxy group, or a halogen group.

[0021] Specific examples of these (c) silane compounds include silane coupling agents having an epoxy group-containing organic group, an amino group-containing organic group, or an acid anhydride-containing organic group with a protected carboxy group. Examples of the silane coupling agent having an epoxy group-containing organic group include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)propyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)propyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, 2-(3,4-epoxycyclohexyl)methyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)methyltriethoxysilane, 1-(3,4-epoxycyclohexyl)methyltrimethoxysilane, and 1-(3,4-epoxycyclohexyl)methyltriethoxysilane. Examples of silane coupling agents having the amino group-containing organic group include 3-(2-(2-aminoethylamino)ethylamino)propyltriethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrichlorosilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, and N-phenyl-3-aminopropyltriethoxysilane. Examples of the acid anhydride-containing silane coupling agents include [3-(trimethoxysilyl)propyl]succinic anhydride.

[0022] The silica particles according to the present invention, at least a portion of which is coated with a silane compound having a hydrophilic organic group (also referred to as "silica particles surface-treated with a silane compound"), can be obtained, for example, by adding the silane compound to an aqueous silica sol, followed by heat treatment at 50 to 100°C for about 1 to 20 hours. In this case, the amount of the silane compound added relative to the silica particles (silica solid content) in the aqueous silica sol can be, for example, a mass ratio of silane compound / silica particles = 0.1 to 10.0, or for example, 0.1 to 5.0, 0.1 to 2.0, or even 0.1 to 1.0. Furthermore, for example, the amount of the silane compound added relative to the silica particles (silica solid content) in the aqueous silica sol can be set to a mass ratio of silane compound / silica particles = 0.1 to 10.0, or for example, 0.1 to 5.0, 0.1 to 2.0, or even 0.1 to 1.0. 2 Amount of silane compound added per nanometer (pieces / nm 2 The silane compound can be added in a ratio such that the number of particles is about 0.5 to 50, 1.0 to 20, or 2.0 to 10. The amount of surface treatment with the silane compound, that is, the amount of the silane compound bonded to the silica particle surface, is within 1 nm of the silica particle surface. 2 For example, it is preferable that the number of particles is about 0.1 to 12, 0.1 to 8, 0.1 to 4, 0.3 to 4, 0.5 to 4, or 0.5 to 3 per particle.

[0023] As described above, when the wettability modifier of the present invention is applied to a rock surface, nanoparticles (silica particles) are adsorbed onto the rock surface, but the amount of adsorption saturates at a certain level, forming a roughly uniform, thin layer (conformal coating). Whether the wettability modifier of the present invention has conformally coated the rock surface can be confirmed by a measurement method using the QCM method.

[0024] The QCM method is a technique for measuring nanogram-order mass changes from changes in the resonant frequency of a quartz crystal oscillator. Specifically, it is a technique that can measure the amount of substance adsorbed to the surface of a sensor (QCM sensor) containing a quartz crystal oscillator in real time at the nanogram level. In measurements using a QCM sensor, weight changes can be measured from the frequency change value, ΔF value. That is, when the ΔF value when the QCM sensor is contacted with a blank solution containing no drug or other external stimulus is corrected to zero, the ΔF value changes negatively when a substance is adsorbed onto the sensor, and the ΔF value changes positively when the substance is desorbed.

[0025] In the present invention, a sensor having an electrode layer and a quartz layer stacked on a quartz oscillator is resonated in a medium containing saltwater and the wettability modifier of the present invention. The adsorption and desorption (or adhesion and peeling) of silica particles (contained in the wettability modifier) ​​to the quartz layer changes the resonant frequency of the quartz oscillator. This change is utilized, and the change in physical quantity (weight change) is measured by monitoring the amount of change. The saltwater contains calcium ions and magnesium ions, and is preferably composed primarily of sodium ions, with a salt concentration of 0.1 to 30% by mass. The quartz oscillator can be used at a resonant frequency of 100 Hz to 100 MHz, typically 1 MHz to 100 MHz.

[0026] More specifically, a sensor consisting of an electrode layer and a quartz layer stacked on a quartz oscillator is resonated in a medium containing saltwater containing sodium ions as the main component, calcium ions, and magnesium ions, and a wettability adjuster for the rock surface, and the ΔF value, which indicates the frequency change (weight change) of the accumulation layer containing silica components accumulated on the sensor surface, is monitored. The ΔF value is zero-corrected using a value obtained in advance using only the saltwater (blank solution). The sensor uses a quartz oscillator with a diameter of approximately 15 mm, and can be used to measure by resonating it at a resonance frequency of, for example, approximately 25 MHz.

[0027] In the present invention, the amount of change in the ΔF value between 2000 seconds and 12000 seconds after the start of resonance is observed, and the ΔF value (F2), which indicates the weight change in the accumulation layer containing silica components accumulated on the sensor surface between 2000 seconds after the start of resonance and ΔF value (F1), which indicates the weight change in the accumulation layer containing silica components accumulated on the sensor surface between 2000 seconds after the start of resonance, is subtracted to calculate the amount of change (difference) (F3). If the change in this F3 value, i.e., the ΔF value during the observation period, is within a certain range, for example, when the resonant frequency of the quartz oscillator is 25 MHz, the change in the ΔF value is within ±20, for example, F3 is -20 to 15, -20 to 10, -10 to 20, -5 to 20, -5 to 15, -3 to 12, 0 to 15, or 0 to 20, and the weight does not change significantly, then it can be determined that the amount of silica particles adsorbed on the sensor surface (quartz layer) is saturated or close to saturated (the silica particles do not aggregate and saturate at a certain amount), that is, a conformal coating has occurred (nanoparticles (silica particles) are adsorbed to the rock surface, but the amount of adsorption saturates at a certain amount, forming a roughly uniform, thin layer). Since some fluctuations (increases or decreases) in the weight of the accumulation layer containing silica components on the sensor surface are expected depending on the ambient environment, even if the F3 value, which indicates weight loss, is a negative value, if the value is small (-20 to 0, or -10 to 0, for example), it can be considered to be within the range of fluctuation, i.e., that conformal coating is maintained. Regarding the changes between 2000 seconds and 12000 seconds, adhesion to the substrate surface occurs at 0 seconds immediately after resonance, conformal coating is completed around 2000 seconds, and if further aggregates accumulate thereafter, the ΔF value decreases (excess adsorption). This trend continues even after 12000 seconds.

[0028] The hydrophilization of rock surfaces (wettability of rock surfaces) due to the wettability modifier of the present invention can be evaluated by measuring the contact angle between a solid and a liquid (or gas) in a liquid, i.e., a three-state contact angle measurement. In particular, the wettability of rock surfaces can be evaluated in the present invention by placing a predetermined amount of crude oil in contact with (adhering to) the bottom of a rock slab in brine containing the wettability modifier of the present invention, and measuring the contact angle between the outer surface of the crude oil droplet and the rock slab.

[0029] In the present invention, three-state contact angle measurement can be performed using, for example, an apparatus (schematic diagram) shown in FIG. 4 . As shown in FIG. 4(A), the apparatus 1 includes an outer cell 2, a substrate 3 placed at a predetermined distance from the bottom of the outer cell 2, and a capillary needle 4 capable of discharging a fluid onto the underside of the substrate (the side facing the bottom of the outer cell). For measurement, the outer cell 2 (e.g., a quartz cell) is filled with a surrounding liquid 5 (e.g., salt water (blank), a liquid containing the wettability modifier of the present invention, etc.) so that the substrate 3 (e.g., a rock slab such as Berea sandstone) placed inside the outer cell 2 is fully immersed. The capillary needle 4 (made of glass, etc.) is then filled with crude oil (not shown). A predetermined amount (e.g., a volume of 0.01 to 1 μL) of crude oil is then dispensed onto the substrate in the surrounding liquid, and the resulting crude oil droplet d is observed. FIG. 4(B) shows a schematic diagram of wettability, showing an enlarged portion of the substrate 3 and the formed crude oil droplet d. As shown in this figure, the larger the contact angle θ of the crude oil droplet d formed on the substrate 3, the more hydrophobic it is (oil wettability: FIG. 4(B)(i)), and the smaller the contact angle θ, the more hydrophilic it is (water wettability: FIG. 4(B)(ii)). In general, a contact angle of less than 50° can be evaluated as strong water wettability, 50° or more but less than 70° as weak water wettability, and 70° or more but less than 110° as intermediate water wettability.

[0030] The wettability modifier according to the present invention is a wettability modifier that, when used in saltwater containing the wettability modifier to evaluate the wettability of a rock surface by contacting (adhering) a volume of 0.01 to 1 μL of crude oil to the underside of a rock slab, reduces the contact angle between the outer surface of the crude oil droplet and the rock slab by 3° or more compared to the same contact angle evaluated in saltwater containing no wettability modifier, by contacting the underside of the rock slab with crude oil, for example, by 3° to 90°, 3° to 70°, 3° to 50°, 3° to 40°, 3° to 30°, or 5° to 30°. The saltwater used for the measurement preferably contains calcium ions and magnesium ions, and is preferably composed mainly of sodium ions, and has a salt concentration of 0.1 to 30% by mass.

[0031] As described above, the wettability control agent of the present invention can conformally coat the rock surface to make it hydrophilic, and is therefore useful as a wettability control agent for storing fluids in rock masses or for securing flow paths into rock masses. In this case, the fluids can be, for example, gases or liquids containing carbon dioxide, aqueous fluids, or aqueous fluids containing rock particles of 1 μm or less.

[0032] The present invention also relates to a method for adjusting the surface wettability of rock, comprising adjusting the rock surface wettability adjuster in an aqueous medium to a silica particle concentration of 0.1 to 30% by mass, or 0.1 to 20% by mass, or 0.1 to 10% by mass, and applying the adjusted mixture to the rock surface. The wettability adjuster of the present invention can be used for rock surface treatment after being diluted as desired with an aqueous medium such as salt water or river water to adjust the silica particle concentration to 0.1 to 30% by mass, or 0.1 to 20% by mass, or 0.1 to 10% by mass. For example, if the rock is underground, the wettability adjuster can be injected into the bedrock underground using an underground injection well pipe to coat the rock surface and adjust the wettability.

[0033] The present invention also relates to a method for evaluating the wettability of a rock surface, which comprises contacting (adhering) a volume of 0.01 to 1 μL of crude oil to the underside of a rock slab in salt water containing a wettability adjuster for the rock surface, and evaluating the contact angle between the outer surface of the crude oil droplet and the rock slab.

[0034] The present invention will be described in further detail below based on synthesis examples, examples, and comparative examples, but it should be understood that the present invention is not limited to these examples in any way.

[0035] (Measurement Apparatus) The following apparatuses were used to evaluate test fluids 1 to 9 containing wettability modifiers (such as the aqueous silica sols prepared in the Synthesis Examples) used in the Examples and Comparative Examples (the amount of silica particles in the test fluids adsorbed to the substrate, and the change in wettability of the substrate due to the test fluid), the physical properties (DLS average particle diameter) of test fluids 1 to 9, and the physical properties of the wettability modifiers (DLS average particle diameter, D90, pH, electrical conductivity, viscosity). Amount of silica particles adsorbed to the substrate: A QSense Analyzer (manufactured by Biolin Scientific) was used. Wettability of the substrate by the test fluid: A contact angle meter (manufactured by Kyowa Interface Science Co., Ltd.) was used. DLS average particle diameter (dynamic light scattering particle diameter): A Zetasizer Nano (manufactured by the Malvern Division of Spectris K.K.) was used. D90: The particle size with a frequency of 90% was used in the volume distribution of particles detected using a dynamic light scattering particle size measurement device, Zetasizer Nano (manufactured by Spectris Corporation, Malvern Division). Silica specific surface area: Calculated from the amount of nitrogen gas adsorption measured using a MONOSORB (manufactured by Quantachrome Instruments). pH: A pH meter (manufactured by Toa DKK Corporation) was used. Electrical conductivity: An electrical conductivity meter (manufactured by Toa DKK Corporation) was used. Viscosity: A BMII type viscometer (manufactured by Tokyo Keiki Co., Ltd.) was used.

[0036] (Removal of silane not bonded to silica particles) 2 g of the aqueous silica sol prepared in the synthesis example described below and 4 g of pure water were placed in a 15 ml centrifugal filter unit (trade name: Amicon Ultra 15, manufactured by Merck Ltd.), and centrifuged for 20 minutes at a centrifugal force of 2770 G. After centrifugation, the liquid discharged to the bottom of the unit was discarded, and the same mass of pure water as the discarded liquid was added to the aqueous silica sol concentrated on the filter to redisperse it, and then centrifuged again for 20 minutes at a centrifugal force of 2770 G. The above procedure was repeated a total of four times to obtain an aqueous silica sol from which silane not bonded to silica particles had been removed.

[0037] (Measurement of silica specific surface area) The aqueous silica sol or the aqueous silica sol from which the silane not bonded to the silica particles has been removed was dried on a hot plate at 80°C to obtain silica gel, which was then pulverized in a mortar and further dried at 60°C for 3 hours under vacuum to obtain a dried silica powder. The specific surface area (m2) of this powder was measured by the nitrogen adsorption method based on the BET theory. 2 / g) was measured (BET method, i.e., nitrogen gas BET method).

[0038] (Measurement of Silane Bond Amount) The aqueous silica sol from which the silane not bonded to the silica particles had been removed using the above procedure was heated and dried at 100°C, and pulverized in a mortar to obtain a silica sol powder. The carbon amount of the obtained silica sol powder was measured using an organic trace element metal analyzer, and the silane bond amount (surface treatment amount) was calculated from the obtained carbon amount using the following formula: Surface treatment amount = (Cm ÷ Cn ÷ Sc × A) / (Ct × Cs) In the above formula, Cm is the carbon content, Cn is the carbon molecular weight, Sc is the number of carbon atoms in the silane, A is Avogadro's number, Ct is the mass of the silica particles, and Cs is the silica specific surface area. The silane bond amount obtained by measuring the carbon amount is expressed in units of (particles / nm 2 )

[0039] (Evaluation of the amount of adsorption onto the substrate - 1) A standardized used quartz vapor deposition sensor manufactured by Biolin Scientific was prepared (product number: QSX303, a sensor in which a silicon dioxide-containing film was formed on a gold electrode on a quartz oscillator. The quartz oscillator had a diameter of 15 mm). The sensor was immersed in pure water, and using a US CLEANER manufactured by AS ONE Corporation, ultrasonic waves of 33 kHz and 40 kHz were irradiated every minute for a total of 10 minutes. After irradiation, the sensor was removed from the pure water and rinsed with tetrahydrofuran. The rinsed sensor was immersed in toluene and again irradiated with the two types of ultrasonic waves for 10 minutes in the same manner as above. Thereafter, the sensor was removed from toluene, immersed in tetrahydrofuran, and again irradiated with the two types of ultrasonic waves for 10 minutes in the same manner as above. After irradiation, the sensor was removed from tetrahydrofuran and dried on a hot plate at 100°C for 5 minutes. The sensor was placed in a QCM-D chamber, and pure water was pumped into the chamber at a flow rate of 0.1 mL / min using a flow path with a total length of 100 cm on the inlet and outlet sides. After confirming no change in the frequency change (ΔF value) using the QCM-D, a 4% by mass salt solution was pumped at a flow rate of 0.1 mL / min. The salt solution contained 2.4% by mass sodium chloride, 1% by mass magnesium chloride, 0.1% by mass calcium chloride, and 0.5% by mass other salt components. After confirming no change in the ΔF value in the same manner as above, a test fluid (described below) was pumped at a flow rate of 0.1 mL / min and contacted with the sensor. The ΔF value detected by the sensor was quantified due to the interaction caused by contact between the quartz on the sensor and the test fluid. Figures 1 to 3 show the change in ΔF (frequency change) detected when the resonant frequency of the quartz crystal oscillator was 25 MHz over time after the test fluid reached the sensor. When measuring the ΔF value, zero correction was performed using salt water with a salt concentration of 4% by mass (blank solution). The F value (F1) at 2000 seconds from the start of resonance and the ΔF value (F2) at 12000 seconds, as well as the difference F3 between these ΔF values ​​(amount of change: F1-F2), are shown in Tables 1 and 2. The amount of adsorption was also evaluated based on the F3 value using the following criteria. The results of the evaluation of the amount of adsorption are also shown in Tables 1 and 2.<Judgment of adsorption amount> (F3 value) A: The ΔF value is a negative value compared to when resonance started, and the value (F3) obtained by subtracting the ΔF value (F2) at 12,000 seconds from the ΔF value (F1) at 2,000 seconds is -20 or more and less than 20. B: The ΔF value is a negative value compared to when resonance started, and the value (F3) obtained by subtracting the ΔF value (F2) at 12,000 seconds from the ΔF value (F1) at 2,000 seconds is -30 or more and less than -20, or 20 or more and less than 30. C: The ΔF value is a negative value compared to when resonance started, and the value (F3) obtained by subtracting the ΔF value (F2) at 12,000 seconds from the ΔF value (F1) at 2,000 seconds is less than -30, or 30 or more. The evaluation results of adsorption based on the above judgment indicate that A is the most preferable, followed by B and C. The resonant frequency of the quartz crystal resonator at which the above ΔF value was observed was 25 MHz.

[0040] (Evaluation of Change in Wettability of Substrate -1) Evaluation of change in wettability -1 was performed by measuring the contact angle in a three-state system. The three-state kit used for measuring the contact angle in a three-state system was a three-state kit (145 mL) manufactured by Kyowa Interface Science Co., Ltd., with Berea sandstone as the substrate, a glass capillary needle as the needle, and crude oil as the discharged liquid. The Berea sandstone sample was dried at 60°C for one day and measured 7.0 cm in length, 2.8 cm in width, and 0.5 cm in height. The glass capillary needle was a needle obtained by bending a φ50 μm (straight) capillary manufactured by Kyowa Interface Science Co., Ltd. using an alcohol lamp. The crude oil used was Light Sour Russian Urals REBCO Crude Oil purchased from ONTA (see the schematic diagram of three-state contact angle measurement shown in Figure 4(A). As shown in the schematic diagram of wettability in Figure 4(B), a larger contact angle θ between the substrate and the crude oil droplet indicates a more hydrophobic (oil wettability: Figure 4(B)(i)), while a smaller contact angle θ indicates a more hydrophilic (water wettability: Figure 4(B)(ii)). A Berea sandstone sample was immersed in the above-mentioned 4% by mass salt solution (see (Evaluation of Adsorption Amount on Substrate-1) above; the same applies below) in a vacuum chamber, and the pressure inside the chamber was reduced using a vacuum pump to saturate the Berea sandstone sample with the 4% by mass salt solution. The Berea sandstone sample was then placed in a three-state kit and placed in a quartz cell. The quartz cell was then filled with the test fluid. After filling a glass capillary needle with crude oil, it was dispensed onto a Berea sandstone sample in the test fluid. The contact angle (a) was calculated from the angle of the formed oil droplet (crude oil droplet). Taking into account the change in the shape of the oil droplet, the entire process from dispensing the oil droplet to calculating the angle was performed within one hour. A Berea sandstone sample prepared using the same procedure was placed in a three-state kit and placed in a quartz cell. The quartz cell was then filled with the above-mentioned 4% by mass salt solution, and the contact angle (b) (blank) was calculated using the same procedure. The volume of each crude oil droplet formed (discharge volume: μL), the contact angle (a) for each test fluid, the contact angle (b) (blank), and the value of [contact angle (b) - contact angle (a)] are shown in Tables 1 and 2. Figure 5 also shows the shapes of the crude oil droplets used to measure the contact angle (a) obtained with the test fluids of the Examples and Comparative Examples, as well as the shape of the crude oil droplet for the blank (contact angle (b)).The smaller the contact angle (a) is relative to the contact angle (b), and the larger the value obtained by subtracting the contact angle (a) from the contact angle (b) [contact angle (b) - contact angle (a)], the more hydrophilic the Berea sandstone sample substrate is due to the test fluid.

[0041] (Substrate Wettability Change Evaluation-2) Wettability Change Evaluation-2 was performed using the same equipment and procedures as Wettability Change Evaluation-1, except that calcite was used for the substrate. The calcite sample used was Omoshiroishi Calcite (product name) manufactured by Kenis Co., Ltd. The calcite sample was immersed in the above-mentioned 4% by mass salt solution in a vacuum chamber, set in a three-phase kit, and placed in a quartz cell. The quartz cell was then filled with the test fluid. Crude oil was filled into a glass capillary needle and then dispensed onto the calcite sample in the test fluid. The contact angle (a) was calculated from the outer angle of the formed oil droplet. The results are shown in Table 1 and Figure 6. Taking into account the shape change of the oil droplet, the entire process from dispensing the oil droplet to calculating the angle was performed within one hour. The quartz cell was filled with the above-mentioned salt water with a salt concentration of 4% by mass, and the same procedure was performed to obtain the contact angle (b). The smaller the contact angle (a) is, and the larger the value obtained by subtracting the contact angle (a) from the contact angle (b) [contact angle (b) - contact angle (a)], the more hydrophilic the calcite sample substrate becomes due to the test fluid.

[0042] (Substrate Wettability Change Evaluation-3) Wettability Change Evaluation-3 was performed using the same equipment and procedures as Wettability Change Evaluation-1, except that a glass slide was used as the substrate. Matsunami Glass Industry Co., Ltd. (product name) White Edge Polished Frost No. 1 was used as the glass slide sample. After ozone treatment in a vacuum chamber, the glass slide sample was immersed in the above-mentioned 4% by weight salt solution, set in a three-phase kit, and placed in a quartz cell. The quartz cell was then filled with the test fluid. Crude oil was filled into a glass capillary needle and then dispensed onto the glass slide sample in the test fluid. The contact angle (a) was calculated from the outer angle of the formed oil droplet. The results are shown in Table 1 and Figure 7. Considering the shape change of the oil droplet, the operation from dispensing the oil droplet to calculating the angle was performed within one hour. The quartz cell was filled with the above-mentioned salt water with a salt concentration of 4% by mass, and the same procedure was performed to obtain the contact angle (b). The smaller the contact angle (a) is, and the larger the value obtained by subtracting the contact angle (a) from the contact angle (b) [contact angle (b) - contact angle (a)], the more hydrophilic the substrate glass slide sample is due to the test fluid.

[0043] (Salt Tolerance Test Evaluation-1) After placing a stirrer in a 200 mL polystyrene bottle, the wettability adjuster (aqueous silica sols of Synthesis Examples 1 to 6, and aqueous silica sols (ST-O, ST-OXS)) described below, pure water, and salt water with a salt concentration of 4.5% by mass were added while stirring with a magnetic stirrer to prepare 150 g of a mixed solution with a salt concentration of 4.0% by mass (sodium chloride concentration 2.4% by mass, magnesium chloride concentration 1% by mass, calcium chloride concentration 0.1% by mass, other salt component concentration 0.5% by mass) and a silica (solids) concentration of 0.5% by mass, and the solution was stirred for 1 hour. This was used as a saltwater test sample for evaluating the salt resistance of the chemical solution in saltwater. The DLS average particle size of the aqueous silica sol (silica particles) in the obtained saltwater test sample was evaluated. The saltwater test samples were left to stand at room temperature (25°C) for a predetermined time (see Tables 1 and 2), and the appearance of the saltwater test samples and the DLS average particle size of the aqueous silica sol (silica particles) in the samples were evaluated. Salt tolerance was also evaluated by measuring the DLS average particle size of the aqueous silica sol (silica particles) in the samples after holding them at room temperature for a predetermined time (10 hours) and then judging the salt tolerance (see <Judgment of Salt Tolerance> below) based on the results of the measurement, as well as evaluating the appearance. The results obtained are shown in Table 1. <Judgment of Salt Tolerance> A: The ratio of the DLS average particle size after the salt tolerance test to the DLS average particle size before the test was less than 1.5. B: The ratio of the DLS average particle size after the salt tolerance test to the DLS average particle size before the test was 1.5 or more but less than 2.0. C: The ratio of the DLS average particle size after the salt tolerance test to the DLS average particle size before the test was 2.0 or more. Alternatively, the silica sol gelled, resulting in the formation of a white precipitate, making it impossible to measure the DLS average particle size. The salt tolerance test results show that A is the most favorable, followed by B and C in that order.

[0044] Synthesis Example 1: Preparation of Wettability Adjuster Used in Examples 1, 4, 5, and 10 A 2,000 mL glass recovery flask was charged with 1,200 g of aqueous silica sol (Snowtex (trade name) ST-O, manufactured by Nissan Chemical Industries, Ltd., silica concentration = 20.5 mass%, average particle size measured by BET method: 11.0 nm, average particle size measured by DLS method: 17.2 nm) and a magnetic stirrer. While stirring with the magnetic stirrer, 191.0 g of 3-glycidoxypropyltrimethoxysilane (manufactured by Evonik, trade name Dynasylan GLYMO) was added so that the mass ratio of silane compound to silica (colloidal silica particles) in the aqueous silica sol was 0.78. Subsequently, a cooling tube filled with tap water was placed on top of the recovery flask, and the aqueous sol was heated to 60°C while refluxing, maintained at 60°C for 4 hours, and then cooled. After cooling to room temperature, the aqueous sol was removed. Mass ratio of silane compound to silica in aqueous silica sol: 0.78, silica solid content: 21.2 mass%, pH: 2.8, electrical conductivity: 353 μS / cm, DLS average particle size: 23.2 nm, D90: 21.5 nm, silane bond amount: 1.5 particles / nm 2 Thus, 1,391.0 g of an aqueous silica sol (dispersion) surface-treated with a silane compound of Synthesis Example 1 was obtained. The aqueous silica sol of Synthesis Example 1 was used as a wettability adjuster in Examples 1, 4, 5, and 10, and in the subsequent tests.

[0045] Synthesis Example 2: Preparation of Wettability Adjuster Used in Examples 2 and 6 A 1-L glass recovery flask was charged with 400 g of aqueous silica sol (Snowtex (trade name) ST-O, manufactured by Nissan Chemical Industries, Ltd., silica solids concentration = 20.5 mass%, BET average particle size 11.0 nm, DLS average particle size 17.2 nm) and a magnetic stirrer. Then, while stirring with the magnetic stirrer, 91.0 g of lactic acid was added and stirred at room temperature for 30 minutes. Subsequently, while stirring, 52.1 g of N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane (KBM-602, manufactured by Shin-Etsu Chemical Co., Ltd.) was added so that the mass ratio of silane compound to silica (colloidal silica) in the aqueous silica sol was 0.64. Subsequently, a cooling tube through which tap water was flowing was placed on top of the recovery flask, and the aqueous sol was heated to 60°C while refluxing, maintained at 60°C for 4 hours, and then cooled. After cooling to room temperature, the aqueous sol was taken out. The mass ratio of the silane compound to the silica solid content in the aqueous silica sol was 0.64, the silica solid content was 17.5 mass%, the pH was 3.6, the electrical conductivity was 9030 μS / cm, the DLS average particle size was 21.1 nm, D90 was 26.7 nm, and the silane bond amount was 0.7 particles / nm. 2 Thus, 543.1 g of an aqueous silica sol (dispersion) surface-treated with a silane compound of Synthesis Example 2 was obtained. The aqueous silica sol of Synthesis Example 2 was used as a wettability adjuster in Examples 2 and 6, and in the subsequent tests.

[0046] Synthesis Example 3: Preparation of Wettability Adjuster Used in Example 3 A 2,000 mL glass recovery flask was charged with 1,200 g of aqueous silica sol (Snowtex (trade name) ST-OXS manufactured by Nissan Chemical Industries, Ltd., silica concentration = 10.5 mass%, average particle size measured by BET method: 5.0 nm, average particle size measured by DLS method: 8.5 nm) and a magnetic stirrer. Then, while stirring with the magnetic stirrer, 209.1 g of 3-glycidoxypropyltrimethoxysilane (manufactured by Evonik GmbH, trade name Dynasylan GLYMO) was added so that the mass ratio of silane compound to silica (colloidal silica particles) in the aqueous silica sol was 0.78. Subsequently, a cooling tube filled with tap water was placed on top of the recovery flask, and the aqueous sol was heated to 60°C while refluxing, maintained at 60°C for 4 hours, and then cooled. After cooling to room temperature, the aqueous sol was removed. Mass ratio of silane compound to silica in aqueous silica sol: 0.78, silica solid content: 8.9 mass%, pH: 2.9, electrical conductivity: 272 μS / cm, DLS average particle size: 12.7 nm, D90: 21 nm, silane bond amount: 2.0 particles / nm 2 Thus, 1,409.1 g of an aqueous silica sol (dispersion) surface-treated with a silane compound of Synthesis Example 3 was obtained. The aqueous silica sol of Synthesis Example 3 was used as a wettability adjuster in Example 3 and in the subsequent tests.

[0047] Synthesis Example 4: Preparation of Wettability Adjuster Used in Example 7 A 2,000 mL glass recovery flask was charged with 1,200 g of aqueous silica sol (Snowtex (trade name) ST-OL manufactured by Nissan Chemical Industries, Ltd., silica concentration = 20.5 mass%, average particle size measured by BET method: 45.0 nm, average particle size measured by DLS method: 80.5 nm) and a magnetic stirrer. Then, while stirring with the magnetic stirrer, 46.7 g of 3-glycidoxypropyltrimethoxysilane (manufactured by Evonik under the trade name Dynasylan GLYMO) was added so that the mass ratio of silane compound to silica (colloidal silica particles) in the aqueous silica sol was 0.19. Subsequently, a cooling tube through which tap water was flowing was placed on top of the recovery flask, and the aqueous sol was heated to 60°C while refluxing, maintained at 60°C for 4 hours, and then cooled. After cooling to room temperature, the aqueous sol was removed. The aqueous silica sol (dispersion) of Synthesis Example 4, which was surface-treated with a silane compound, was obtained in an amount of 1,246.7 g, and had a mass ratio of the silane compound to the silica in the aqueous silica sol of 0.19, a silica solid content of 22.5 mass%, a pH of 3.2, an electrical conductivity of 310 μS / cm, a DLS average particle size of 79.8 nm, and a D90 of 85.8 nm. The aqueous silica sol of Synthesis Example 4 was used as a wettability adjuster in Example 7 and in the subsequent tests.

[0048] Synthesis Example 5: Preparation of Wettability Adjuster Used in Example 8 A 2,000 mL glass recovery flask was charged with 1,200 g of aqueous silica sol (Snowtex (trade name) ST-O, manufactured by Nissan Chemical Industries, Ltd., silica concentration = 20.5 mass%, average particle size by BET method 11.0 nm, average particle size by DLS method 17.2 nm) and a magnetic stirrer. Then, while stirring with the magnetic stirrer, 211.9 g of [3-(trimethoxysilyl)propyl]succinic anhydride (X-12-967C, manufactured by Shin-Etsu Chemical Co., Ltd.) was added so that the mass ratio of silane compound to silica (colloidal silica particles) in the aqueous silica sol was 0.86. Subsequently, a cooling tube through which tap water was flowing was placed on top of the recovery flask, and the aqueous sol was heated to 60°C while refluxing, maintained at 60°C for 4 hours, and then cooled. After cooling to room temperature, the aqueous sol was removed. The aqueous silica sol (dispersion) of Synthesis Example 1, which was surface-treated with a silane compound, was obtained in an amount of 1,411.9 g, and had a mass ratio of the silane compound to the silica in the aqueous silica sol of 0.86, a silica solid content of 20.7 mass%, a pH of 2.1, an electrical conductivity of 908 μS / cm, a DLS average particle size of 19.0 nm, and a D90 of 18.0 nm. The aqueous silica sol of Synthesis Example 5 was used as a wettability adjuster in Example 8, and was used in the following tests.

[0049] (Synthesis Example 6: Preparation of Wettability Adjuster Used in Example 9) The same procedure as in Synthesis Example 1 was performed, except that 47.8 g of 3-glycidoxypropyltrimethoxysilane (manufactured by Evonik under the trade name Dynasylan GLYMO) was added so that the mass ratio of the silane compound to the silica (colloidal silica particles) in the aqueous silica sol was 0.20, to obtain 1,247.8 g of an aqueous silica sol (dispersion) of Synthesis Example 6 that was surface-treated with a silane compound, having a mass ratio of the silane compound to the silica in the aqueous silica sol of 0.20, a silica solids content of 21.1 mass%, a pH of 2.9, an electrical conductivity of 516 μS / cm, a DLS average particle size of 19.4 nm, and a D90 of 19.0 nm. The aqueous silica sol of Synthesis Example 6 was used as the wettability adjuster in Example 9 and in the subsequent tests.

[0050] (Wettability Adjuster Used in Comparative Example 1) An aqueous silica sol (Snowtex (trade name) ST-O, manufactured by Nissan Chemical Industries, Ltd., silica solid content = 20.5 mass%, BET average particle size = 11.0 nm, DLS average particle size = 18.6 nm, D90 = 21.0 nm) (aqueous silica sol containing uncoated silica particles) was adopted as the wettability adjuster in Comparative Example 1 and used in the subsequent tests.

[0051] (Wettability Adjuster Used in Comparative Example 2) An aqueous silica sol (Snowtex (trade name) ST-OXS manufactured by Nissan Chemical Industries, Ltd., silica solid content concentration = 10.5 mass%, BET average particle size = 5.0 nm, DLS average particle size = 8.6 nm, D90 = 19.1 nm) (aqueous silica sol containing uncoated silica particles) was adopted as the wettability adjuster in Comparative Example 2 and used in the subsequent tests.

[0052] Preparation Example 1 A stirrer was placed in a 120 mL polystyrene bottle, and 2.4 g of the wettability adjuster (the aqueous silica sol produced in Synthesis Example 1) used in Examples 1, 4, and 5 was added. While stirring with a magnetic stirrer, 8.8 g of pure water was added, followed by 88.8 g of brine with a salt concentration of 4.5 mass % to prepare Test Fluid 1 having a silica solids concentration of 0.5 mass % and a salt concentration of 4 mass % (sodium chloride concentration of 2.4 mass %, magnesium chloride concentration of 1 mass %, calcium chloride concentration of 0.1 mass %, and other salt component concentrations of 0.5 mass %, the same applies hereinafter).

[0053] Preparation Example 2 A stirrer was placed in a 120 mL polystyrene bottle, and 2.9 g of the wettability adjuster used in Examples 2 and 6 (the aqueous silica sol produced in Synthesis Example 2) was added. While stirring with a magnetic stirrer, 8.3 g of pure water was added, and then 88.8 g of brine with a salt concentration of 4.5 mass % was added to prepare Test Fluid 2 with a silica solids concentration of 0.5 mass % and a salt concentration of 4 mass %.

[0054] Preparation Example 3 A stirrer was placed in a 120 mL polystyrene bottle, and 5.6 g of the wettability adjuster used in Example 3 (the aqueous silica sol produced in Synthesis Example 3) was added. While stirring with a magnetic stirrer, 5.6 g of pure water was added, and then 88.8 g of brine with a salt concentration of 4.5 mass % was added to prepare Test Fluid 3 with a silica solids concentration of 0.5 mass % and a salt concentration of 4 mass %.

[0055] Preparation Example 4 A stirrer was placed in a 120 mL polystyrene bottle, and 2.2 g of the wettability adjuster used in Example 7 (the aqueous silica sol produced in Synthesis Example 4) was added. While stirring with a magnetic stirrer, 8.9 g of pure water was added, and then 88.8 g of brine with a salt concentration of 4.5 mass % was added to prepare Test Fluid 4 with a silica solids concentration of 0.5 mass % and a salt concentration of 4 mass %.

[0056] Preparation Example 5 A stirrer was placed in a 120 mL polystyrene bottle, and 2.4 g of the wettability adjuster used in Example 8 (the aqueous silica sol produced in Synthesis Example 5) was added. While stirring with a magnetic stirrer, 8.7 g of pure water was added, and then 88.8 g of brine with a salt concentration of 4.5 mass % was added to prepare Test Fluid 5 with a silica solids concentration of 0.5 mass % and a salt concentration of 4 mass %.

[0057] Preparation Example 6 A stirrer was placed in a 120 mL polystyrene bottle, and 2.4 g of the wettability adjuster used in Example 9 (the aqueous silica sol produced in Synthesis Example 6) was added. While stirring with a magnetic stirrer, 8.7 g of pure water was added, and then 88.8 g of brine with a salt concentration of 4.5 mass % was added to prepare Test Fluid 6 with a silica solids concentration of 0.5 mass % and a salt concentration of 4 mass %.

[0058] Preparation Example 7 A stirrer was placed in a 120 mL polystyrene bottle, and 47.2 g of the wettability adjuster used in Example 10 (the aqueous silica sol produced in Synthesis Example 1) was added. While stirring with a magnetic stirrer, 52.8 g of brine with a salt concentration of 4.5 mass % was added to prepare Test Fluid 7 with a silica solids concentration of 10 mass % and a salt concentration of 2.4 mass %.

[0059] Preparation Example 8 A stirrer was placed in a 120 mL polystyrene bottle, and 2.4 g of uncoated aqueous silica sol (Snowtex (registered trademark) ST-O, manufactured by Nissan Chemical Industries, Ltd., silica solids concentration = 20.5 mass%, BET average particle size 11.0 nm, DLS average particle size 17.2 nm) was added as the wettability adjuster used in Comparative Example 1. While stirring with a magnetic stirrer, 8.8 g of pure water was added, and then 88.8 g of brine with a salt concentration of 4.5 mass% was added to prepare test fluid 8 having a silica solids concentration of 0.5 mass% and a salt concentration of 4 mass%.

[0060] Preparation Example 9 A stirrer was placed in a 120 mL polystyrene bottle, and 4.8 g of Snowtex (registered trademark) ST-OXS manufactured by Nissan Chemical Industries, Ltd. was added as the wettability adjuster used in Comparative Example 2. While stirring with a magnetic stirrer, 6.4 g of pure water was added, and then 88.8 g of brine with a salt concentration of 4.5 mass % was added to prepare Test Fluid 9 having a silica solids concentration of 0.5 mass % and a salt concentration of 4 mass %.

[0061] The adsorption amount and wettability of the above test fluids 1 to 9 were evaluated according to (Evaluation of adsorption amount onto substrate - 1) and (Evaluation of change in wettability of substrate (1 to 3)), respectively. In addition, the salt resistance of the wettability adjusters (aqueous silica sols of Synthesis Examples 1 to 6 and aqueous silica sols (ST-O, ST-OXS)) used in the above Examples 1 to 10 and Comparative Examples 1 and 2 was evaluated according to (Salt resistance test evaluation - 1). The obtained results are shown in Tables 1 and 2. 5 shows the shapes of the crude oil droplets used to measure the contact angles (a) obtained with the test fluids (test fluids 1-3, 8, 4-7) of Examples 1-3, Comparative Example 1, and Examples 7-10 in (Evaluation of Changes in Substrate Wettability-1), as well as the shape of the crude oil droplet for the blank (contact angle (b)). FIG. 6 shows the shapes of the crude oil droplets used to measure the contact angles (a) obtained with the test fluid (test fluid 1) of Example 4 in (Evaluation of Changes in Substrate Wettability-2), as well as the shape of the crude oil droplet for the blank (contact angle (b)). FIG. 7 shows the shapes of the crude oil droplets used to measure the contact angles (a) obtained with the test fluids (test fluids 1 and 2) of Examples 5 and 6 in (Evaluation of Changes in Substrate Wettability-3), as well as the shape of the crude oil droplet for the blank (contact angle (b)). In FIGS. 5-7, the black circular or semicircular portions represent the crude oil droplets, and the portions above them represent the substrate. In addition, the contact angle measured in the blank shown in Fig. 5 is indicated as θ. Note that, since a slide glass was used as the substrate in (Evaluation of change in wettability of substrate-3), the substrate (transparent) portion is indicated by a dashed line in Fig. 7.

[0062]

[0063]

[0064] The aqueous silica sol used in the test fluids that obtained satisfactory results in the (Adsorption Amount Evaluation-1) and (Wettability Change Evaluation-1) to (Wettability Change Evaluation-3) evaluations can be said to be useful as wettability modifiers that can conformally coat rock surfaces and hydrophilize them. Furthermore, samples that obtained satisfactory results in the (Salt Tolerance Test Evaluation-1) evaluation can be said to be suitable for injection into underground rock masses. As shown in Table 1, test fluids 1 to 3 containing the wettability modifiers (aqueous silica sols of Synthesis Examples 1 to 3) used in Examples 1 (and Examples 4 and 5), 2 (and Example 6), and 3, and test fluids 4 to 7 containing the wettability modifiers (aqueous silica sols of Synthesis Examples 4 to 6 and 1) used in Examples 7 to 10, as shown in Table 2, showed that the ΔF value (F3) between 2,000 seconds after the start of resonance and 12,000 seconds was in the range of -20 to 20, indicating that the adsorption amount was close to saturation. Furthermore, in all of the tests using test fluids 1 to 3 (Wettability Change Evaluation-1: Berea Sandstone), (Wettability Change Evaluation-2: Calcite), and (Wettability Change Evaluation-3: Glass Slide), and in all of the tests using test fluids 4 to 7 (Wettability Change Evaluation-1: Berea Sandstone), the contact angle (a) was smaller than the contact angle (b) of the blank, and the value of [contact angle (b) - contact angle (a)] was 5.2 to 15.2°, all of which were 3° or more. Test fluids 1 to 7 changed the wettability of these substrates to be more hydrophilic. Furthermore, in the tests using test fluids 1 to 7 (Wettability Change Evaluation-1: Berea Sandstone) and 3 (Wettability Change Evaluation-3: Glass Slide), the contact angle (a) was 30° or less, confirming that the substrate surface had strong wettability. Furthermore, the wettability adjusters used in the test fluids (aqueous silica sols of Synthesis Examples 1 to 6) were also confirmed to be samples with excellent salt resistance. In other words, it was suggested that the wettability adjuster used in the examples is a wettability adjuster that can conformally coat the rock surface to make it hydrophilic, and can also be injected into underground rock masses.When this is injected into underground rock masses, it is expected to have effects such as ensuring a flow path for hydrophilic chemical solutions without causing the risk of clogging the strata.In Comparative Examples 1 and 2, the value of [contact angle (b) - contact angle (a)] was 3° or more in (Wettability change evaluation-1), meaning that an improvement in the wettability of the rock surface is expected. However, in both (Adsorption onto substrate evaluation-1) and (Salt resistance test evaluation-1), the evaluation was C, meaning that good results were not obtained. In other words, if this were injected into underground bedrock, there would be a risk of blockage of the stratum, and there would be a risk of aggregation occurring due to mixing with salt water produced during injection.

[0065] 1 Three-state contact angle measurement apparatus, 2 External cell, 3 Substrate, 4 Capillary needle, 5 Surrounding liquid, d Crude oil droplet

Claims

1. A wettability adjuster for rock surfaces that hydrophilizes the surface by conformal coating, comprising: silica particles (a) having an average DLS particle size of 5 to 200 nm as measured by dynamic light scattering; and an aqueous medium (b), at least a portion of the silica particles being coated with a silane compound (c) having a hydrophilic organic group.

2. The wettability control agent for a rock surface according to claim 1, wherein the hydrophilic organic group is an epoxy group-containing organic group, an amino group-containing organic group, a hydroxyl group-containing organic group, or a carboxyl group-containing organic group.

3. A test method in which a sensor having an electrode layer and a quartz layer laminated on a quartz oscillator is resonated in a medium containing salt water containing calcium ions and magnesium ions and a wettability adjuster for the rock surface, wherein the value (F3) obtained by subtracting the ΔF value (F1) indicating the weight change of the accumulation layer containing silica components accumulated on the sensor surface from the start of resonance until 2000 seconds from the start of resonance until 12000 seconds is -20 to 20 when the resonance frequency of the quartz oscillator is 25 MHz.

4. A rock surface wettability adjuster as claimed in any one of claims 1 to 3, wherein in an evaluation of the wettability of a rock surface in which a volume of 0.01 to 1 μL of crude oil is placed in contact with the underside of a rock slab in salt water containing the rock surface wettability adjuster, the contact angle between the outer surface of the crude oil droplet and the rock slab is reduced by 3° or more compared to the same contact angle evaluated in salt water not containing the wettability adjuster.

5. The wettability adjuster for rock surfaces according to claim 3 or 4, wherein the salt water contains sodium ions and has a salt concentration of 0.1 to 30 mass %.

6. The wettability control agent for a rock surface according to claim 3, wherein the resonant frequency of the quartz crystal oscillator is in the range of 1 MHz to 100 MHz.

7. The wettability control agent for a rock surface according to claim 1, which is a wettability control agent for ensuring the retention of fluid within a rock mass or the formation of a flow path within the rock mass.

8. The wettability control agent for a rock surface according to claim 7, wherein the fluid is a gas or liquid containing carbon dioxide, an aqueous fluid, or an aqueous fluid containing rock particles of 10 μm or less.

9. A method for adjusting the wettability of a rock surface, comprising adjusting the wettability adjuster for a rock surface according to any one of claims 1 to 8 in an aqueous medium to a silica particle concentration of 0.1 to 30 mass % and applying the resulting mixture to the rock surface.

10. A method for evaluating the wettability of a rock surface, comprising contacting the bottom of a rock slab with a volume of 0.01 to 1 μL of crude oil in salt water containing a rock surface wettability regulator as defined in any one of claims 1 to 3, and evaluating the contact angle between the outer surface of the crude oil droplet and the rock slab.