Wire rod, steel wire, rope, and method for producing rope

MYPI2025004633A0Undetermined Publication Date: 2024-08-03NIPPON STEEL CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025004633
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-02-03
Publication Date
2024-08-03

AI Technical Summary

Technical Problem

Current steel wires used in bridge cables face a trade-off between high strength and good torsional properties, as increasing strength often deteriorates torsional properties, and achieving uniform hardness distribution across the wire diameter is challenging due to differences in cooling rates between the surface and center.

Method used

A wire rod with a chemical composition of C: 0.80-1.10%, Si: 0.10-1.50%, and Mo: 0.02-0.20% is developed, which, when drawn into a steel wire, maintains a mixed structure of ferrite and cementite, ensuring a uniform hardness distribution and improved torsional properties by retarding transformation temperatures, thus achieving high strength and excellent twisting properties.

Benefits of technology

The solution results in steel wires with tensile strengths of 2050 MPa or more and excellent torsional properties, as evidenced by the controlled Vickers hardness differences across the wire cross-section, preventing micro-cracks and maintaining wire integrity during torsion tests.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PI2025004633_DRAWING_001
    Figure PI2025004633_DRAWING_001
Patent Text Reader

Abstract

ABSTRACT WIRE ROD, STEEL WIRE, ROPE, AND METHOD FOR PRODUCING ROPE A wire rod having a chemical composition containing, in % by mass, C: from 0.80 to 1.10%, Si: from 0.10 to 1.50%, Mn: from 0.10 to 1.00%, P: 0.030% or less, S: 0.030% or less, N: 0.0120% or less, O: 0.0100% or less, Al: from 0.005 to 0.070%, and Mo: from 0.02 to 0.20%, with a balance being Fe and impurities, in which a total area ratio of a ferrite structure and a martensite structure at a center portion of a cross section is 5% or less, an average Vickers hardness H, a surface layer Vickers hardness Hs, and a center Vickers hardness Hc in the cross section satisfy the relationships of Formulas (1) to (3) ([C] is a content of C contained in the wire rod in % by mass), and a diameter is 7.0 mm or more, and a steel wire that can be produced from the wire rod, are provided. A rope made of bundled steel wires is also provided. 480 × [C] - 40 < H < 480 × [C] + 40 ...(1) 0 ≤ Hs - H < 30 ...(2) 0 ≤ H - Hc < 30 ...(3)
Need to check novelty before this filing date? Find Prior Art

Description

Wire rod, steel wire, rope, and rope manufacturing method

[0001] The present disclosure relates to wire rods, steel wires, ropes, and methods for manufacturing ropes.

[0002] Steel wires for bridge cables, ropes, and the like are manufactured using steel wires that are obtained by, for example, patenting high-carbon wire rods to form pearlite structures, then drawing and plating them. For example, bridge cables are required to have high strength in order to improve the degree of freedom in cable design, and the steel wires used therefor are also required to have high strength.

[0003] For example, Patent Document 1 discloses a high-strength PC steel wire having a tensile strength of 2000 MPa or more, which contains, by mass, 0.9 to 1.2% C, 0.01 to 1.5% Si, 0.2 to 1.5% Mn, 0.001 to 0.05% Al, and 0.0005 to 0.010% N, with the balance being Fe and unavoidable impurities, and which is composed of 90% or more of drawn pearlite and 10% or less of ferrite and bainite, and which has a tensile strength of 2000 MPa or more, and which has excellent delayed fracture resistance, characterized in that, when the wire diameter of the PC steel wire is D, the ratio (Hv surface / Hv internal) of the surface layer Hv hardness (Hv surface) in a region 0.1D from the surface of the PC steel wire (surface layer portion) to the internal Hv hardness (Hv internal) in a region (internal) inside the surface layer portion is 1.1 or less. However, the problem is that the torsional properties deteriorate as the strength increases.

[0004] As a steel wire intended to improve torsional properties, for example, Patent Document 2 discloses a steel wire containing, by mass%, C: 0.8 to 1.1%, Si: 0.8 to 1.3%, Mn: 0.3 to 0.8%, N: 0.001 to 0.006%, B: 0.0004 to 0.0060%, with solute B being 0.0002% or more, and further containing one or two of Al: 0.005 to 0.1% and Ti: 0.005 to 0.1%, with the balance being Fe and inevitable impurities, with an area ratio of non-pearlite structures in a portion up to a depth of 50 μm from the surface being 10% or less, and a total area ratio of non-pearlite structures in the entire cross section being 5% or less, and with a coating weight of 300 to 500 g / m on the surface. 2The publication discloses a plated steel wire for PWS having excellent twisting properties, characterized by being plated with zinc.

[0005] Patent Document 1: JP 2009-280836 A Patent Document 2: WO 2008 / 093466

[0006] There is a demand for the development of steel wires having high strength and excellent torsional properties, and wire rods suitable for manufacturing steel wires having such properties, for use in bridge cables, etc. Therefore, an object of the present disclosure is to provide wire rods suitable for manufacturing steel wires having high strength and excellent torsional properties by wiredrawing, steel wires having high strength and excellent torsional properties, ropes, and methods for manufacturing ropes.

[0007] The means for solving the above problems include the following aspects. <1> In mass%, C: 0.80 to 1.10%, Si: 0.10 to 1.50%, Mn: 0.10 to 1.00%, P: 0.030% or less, S: 0.030% or less, N: 0.0120% or less, O: 0.0100% or less, Al: 0.005 to 0.070%, Mo: 0.02 to 0.20%, Cr: 0 to 1.00%, Cu: 0 to 0.80%, Sn: 0 to 0.50%, Ni: 0 to 0.50%, V: 0 to 0.15%, Ti: 0 to 0.050%, Nb: 0 to 0.050%, B: 0 to 0.0040%, REM: 0 to 0.030%, the wire rod has a chemical composition comprising Mg: 0 to 0.0040%, Ca: 0 to 0.0040%, Zr: 0 to 0.030%, W: 0 to 0.10%, Te: 0 to 0.030%, and Sb: 0 to 0.030%, with the balance being Fe and impurities; in a cross section perpendicular to the longitudinal direction, a total area ratio of a ferrite structure and a martensite structure in a central portion within 1.0 mm from the center is 5% or less, and the balance is a mixed structure made of ferrite and cementite; when the content of C in mass% contained in the wire rod is [C], the average Vickers hardness H in the cross section satisfies the following formula (1): 480×[C]−40<H<480×[C]+40 ... (1); a surface layer Vickers hardness Hs at a depth of 0.5 to 1.0 mm from the surface and an average Vickers hardness H satisfy the following formula (2); 0≦Hs−H<30 (2) The central Vickers hardness Hc within 1.0 mm from the center and the average Vickers hardness H satisfy the relationship of formula (3), and 0≦H−Hc<30 (3) The wire has a wire diameter of 7.0 mm or more. <2> The wire according to <1>, wherein the chemical composition includes, in mass %, at least one or more selected from the group consisting of Cr: 0.03 to 1.00%, Cu: 0.01 to 0.80%, Sn: 0.001 to 0.50%, Ni: 0.01 to 0.50%, and V: 0.01 to 0.15%.<3> The wire rod according to <1> or <2>, wherein the chemical composition includes, in mass%, one or more elements selected from the group consisting of Ti: 0.002 to 0.050%, Nb: 0.002 to 0.050%, B: 0.0003 to 0.0040%, REM: 0.002 to 0.030%, Mg: 0.0002 to 0.0040%, Ca: 0.0002 to 0.0040%, Zr: 0.002 to 0.030%, W: 0.02 to 0.10%, Te: 0.001 to 0.030%, and Sb: 0.001 to 0.030%. <4> In mass%, C: 0.80 to 1.10%, Si: 0.10 to 1.50%, Mn: 0.10 to 1.00%, P: 0.030% or less, S: 0.030% or less, N: 0.0120% or less, O: 0.0100% or less, Al: 0.005 to 0.070%, Mo: 0.02 to 0.20%, Cr: 0 to 1.00%, Cu: 0 to 0.80%, Sn: 0 to 0.50%, Ni: 0 to 0.50%, V: 0 to 0.15%, Ti: 0 to 0.050%, Nb: 0 to 0.050%, B: 0 to 0.0040%, REM: 0 to 0.030%, It has a chemical composition including Mg: 0 to 0.0040%, Ca: 0 to 0.0040%, Zr: 0 to 0.030%, W: 0 to 0.10%, Te: 0 to 0.030%, and Sb: 0 to 0.030%, with the balance being Fe and impurities; in a cross section parallel to the longitudinal direction and passing through the central axis, a total area ratio of a ferrite structure and a martensite structure in a central portion within 1.0 mm from the center is 5% or less, and the balance is a mixed structure made of ferrite and cementite; the average Vickers hardness h in the cross section perpendicular to the longitudinal direction is 450 to 620; and a surface Vickers hardness hs at a depth of 0.2 to 0.5 mm from the surface and the average Vickers hardness h satisfy the relationship of formula (4), 0≦hs−h<30 (4). A steel wire in which the central Vickers hardness hc within 1.0 mm from the center of the vertical cross section and the average Vickers hardness h satisfy the relationship of formula (5).0≦h−hc<30 (5) <5> The steel wire according to <4>, wherein the chemical composition includes, in mass%, at least one or two or more elements selected from the group consisting of: Cr: 0.03 to 1.00%, Cu: 0.01 to 0.80%, Sn: 0.001 to 0.50%, Ni: 0.01 to 0.50%, and V: 0.01 to 0.15%. <6> The steel wire according to <4> or <5>, wherein the chemical composition includes, in mass%, one or more elements selected from the group consisting of Ti: 0.002 to 0.050%, Nb: 0.002 to 0.050%, B: 0.0003 to 0.0040%, REM: 0.002 to 0.030%, Mg: 0.0002 to 0.0040%, Ca: 0.0002 to 0.0040%, Zr: 0.002 to 0.030%, W: 0.02 to 0.10%, Te: 0.001 to 0.030%, and Sb: 0.001 to 0.030%. <7> The steel wire according to any one of <4> to <6>, the surface of which is plated. <8> A rope comprising a plurality of steel wires according to any one of <4> to <7> bundled together. <9> A method for manufacturing a rope, comprising a step of bundling a plurality of steel wires according to any one of <4> to <7> into a rope.

[0008] According to the present disclosure, there are provided a wire rod suitable for producing a steel wire having high strength and excellent torsional properties by wire drawing, a steel wire having high strength and excellent torsional properties, a rope, and a method for producing a rope.

[0009] 1 is a diagram showing an example of an SEM photograph of each structure of a wire rod, and FIG. 2 is a diagram showing an example of an SEM photograph of a ferrite structure and a martensite structure of a steel wire.

[0010] An embodiment that is an example of the present disclosure will be described below. In this specification, the "surface layer" or "surface layer portion" of a wire rod refers to a range of 0.5 to 1.0 mm deep from the surface (outer peripheral surface) of the wire rod in a cross section perpendicular to the longitudinal direction of the wire rod (a region having a depth of 0.5 mm or more and 1.0 mm or less from the surface), and the "center portion" refers to a range within 1.0 mm from the center of the wire rod in a cross section perpendicular to the longitudinal direction of the wire rod. Meanwhile, the "surface layer" or "surface layer portion" of a steel wire refers to a range of 0.2 to 0.5 mm deep from the surface (outer peripheral surface) of the steel wire in a cross section parallel to or perpendicular to the longitudinal direction of the steel wire (a region having a depth of 0.2 mm or more and 0.5 mm or less from the surface), and the "center portion" refers to a range within 1.0 mm from the center of the steel wire in a cross section parallel to or perpendicular to the longitudinal direction of the steel wire. Furthermore, the "center axis" refers to an imaginary line that passes through the center point of a cross section perpendicular to the axial direction (longitudinal direction) of the wire rod or steel wire and extends in the axial direction. In addition, in this specification, a cross section perpendicular to the longitudinal direction of a wire rod or steel wire may be referred to as a "transverse section," and a cross section parallel to the longitudinal direction and including the central axis may be referred to as a "longitudinal section." In addition, in this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​written before and after "to" as the lower and upper limits. In addition, when "over" or "less than" is added to the numerical values ​​written before and after "to," the numerical range means a range that does not include these numerical values ​​as the lower or upper limit. In the numerical ranges described in stages in this specification, the upper limit of a certain numerical range may be replaced with the upper limit of another numerical range described in stages, or may be replaced with a value shown in the Examples. In the numerical ranges described in stages in this specification, the lower limit of a certain numerical range may be replaced with the lower limit of another numerical range described in stages, or may be replaced with a value shown in the Examples. The content of an element in a chemical composition may be simply expressed as "amount" (e.g., C amount, Si amount, etc.). Regarding the content of an element in a chemical composition, "%" means "mass %." When the lower limit of the content of an element in a chemical composition is "0 to," this means that the element is an optional element and may not be included.Furthermore, the term "process" does not only refer to an independent process, but also includes processes that cannot be clearly distinguished from other processes as long as the intended purpose of the process is achieved.

[0011] [Wire Rod] The wire rod according to the present disclosure contains, in mass %, C: 0.80 to 1.10%, Si: 0.10 to 1.50%, Mn: 0.10 to 1.00%, P: 0.030% or less, S: 0.030% or less, N: 0.0120% or less, O: 0.0100% or less, Al: 0.005 to 0.070%, and Mo: 0.02 to 0.20%, and optionally Cr: 0 to 1.00%, Cu: 0 to 0.80%, Sn: 0 to 0.50%, Ni: 0 to 0.50%, V: 0 to 0.15%, Ti: 0 to 0.050%, Nb: 0 to 0.050%, B: 0 to 0.0040%, It has a chemical composition containing REM: 0 to 0.030%, Mg: 0 to 0.0040%, Ca: 0 to 0.0040%, Zr: 0 to 0.030%, W: 0 to 0.10%, Te: 0 to 0.030%, and Sb: 0 to 0.030%, with the balance being Fe and impurities. Furthermore, in the wire rod according to the present disclosure, in a cross section perpendicular to the longitudinal direction, the total area ratio of ferrite and martensite structures in a central portion within 1.0 mm from the center (sometimes referred to as the "area ratio of ferrite and martensite structures" in the present disclosure) is 5% or less, and the remainder is a mixed structure made of ferrite and cementite, and when the content of C in mass % contained in the wire rod is [C], the average Vickers hardness H in the cross section (sometimes referred to as the "average hardness" in the present disclosure) satisfies formula (1): 480×[C]−40<H<480×[C]+40 ... (1) The surface layer Vickers hardness Hs at a depth of 0.5 to 1.0 mm from the surface (sometimes referred to as the "surface layer hardness" in the present disclosure) and the average Vickers hardness H satisfy the relationship of formula (2): 0≦Hs−H<30 ... (2) The central Vickers hardness Hc (sometimes referred to as "central hardness" in this disclosure) within 1.0 mm from the center and the average Vickers hardness H satisfy the relationship of formula (3): 0≦H−Hc<30 (3) The wire diameter is 7.0 mm or more.

[0012] The inventors of the present disclosure discovered the wire rod and steel wire according to the present disclosure through the following studies. In order to obtain a predetermined wire diameter and strength through wiredrawing while maintaining good torsional properties, it is desirable to use a mixed structure consisting of ferrite and cementite, such as pearlite or bainite, which have excellent work hardening properties, as the main structure. The presence of a structure containing almost no cementite (a ferrite structure or martensite structure) reduces torsional properties. Note that pearlite and bainite are not distinguished in this disclosure because, if the hardness of pearlite and bainite is equivalent, their properties after wiredrawing are similar, and they are difficult to distinguish from each other in photographs. Furthermore, for steel wires used with wire diameters of, for example, 5.0 mm to 7.0 mm, such as steel wires for bridges, the wire diameter of the wire rod often exceeds 7.0 mm. For thick wire rods with a wire diameter exceeding 7.0 mm, it is difficult to uniformly create pearlite and bainite structures within the cross section. Differences in the pearlite transformation temperature and bainite transformation temperature occur between the surface layer, where the cooling rate is high, and the center, where the cooling rate is low. Therefore, the surface layer tends to be harder than the center. The hardness distribution formed in the wire rod is carried over even after wire drawing, and the surface layer of the steel wire also has a hard distribution. In torsion tests, strain is concentrated in the surface layer, so a hard distribution in the surface layer results in poor torsional properties.

[0013] Therefore, the inventors of the present disclosure investigated how to sufficiently delay the transformation so that pearlite transformation or bainite transformation can occur at the same temperature as in the surface layer even in the center where the cooling rate is slow. As a result of extensive investigations, the inventors of the present disclosure found that Mo has the effect of delaying the transformation, and that the addition of Mo improves the uniformity of the hardness distribution in the cross section of the wire rod (the cross section perpendicular to the longitudinal direction of the wire rod), and further confirmed that a steel wire containing a predetermined amount of Mo has good torsional properties even when the tensile strength is 2050 MPa or more.

[0014] <Chemical Composition> The chemical composition (content of each element) of the wire rod according to the present disclosure will be described below.

[0015] C: 0.80 to 1.10% C is a necessary component for increasing the tensile strength of wire rods and steel wires obtained after wire drawing. If the C content is less than 0.80%, the tensile strength is insufficient. On the other hand, if the C content of the wire rod is too high, the wire rod becomes hardened and the torsional properties deteriorate. If the C content of the wire rod exceeds 1.10%, it becomes difficult to suppress the formation of pro-eutectoid cementite, and the target torsional properties cannot be obtained even if other requirements are met. From the viewpoint of tensile strength, the C content is preferably 0.85% or more, and in particular, if it is 0.90% or more, better properties are obtained. On the other hand, from the viewpoint of torsional properties, the C content is preferably 1.05% or less, and in particular, if it is 1.00% or less, better properties are obtained.

[0016] Si: 0.10 to 1.50% Si is an effective component for increasing the tensile strength of wire rods and steel wires obtained after wire drawing. If the Si content of the wire rod is less than 0.10%, the effect of containing Si is not fully obtained. On the other hand, if the Si content of the wire rod exceeds 1.50%, it becomes difficult to suppress the formation of a martensite structure, which is a hard phase, and the target torsional properties cannot be obtained even if other requirements are met. From the viewpoint of tensile strength, the Si content is preferably 0.50% or more, and in particular, 0.70% or more exhibits better properties. On the other hand, from the viewpoint of torsional properties, the Si content is preferably 1.40% or less, and in particular, 1.30% or less exhibits better properties.

[0017] Mn: 0.10 to 1.00% Mn is an effective component for increasing the tensile strength of wire rods and steel wires obtained after wire drawing. Furthermore, Mn fixes S in steel as MnS, suppressing hot brittleness. If the Mn content of the wire rod is less than 0.10%, the effects of Mn inclusion are not fully achieved. On the other hand, if the Mn content of the wire rod exceeds 1.00%, it becomes difficult to suppress the formation of a martensite structure, which is a hard phase, and the desired torsional properties cannot be obtained even if other requirements are met. From the viewpoint of tensile strength, the Mn content is preferably 0.25% or more. On the other hand, from the viewpoint of torsional properties, the Mn content is preferably 0.80% or less.

[0018] P: 0.030% or less P is an element that segregates at the grain boundaries of the wire rod and deteriorates the torsional properties. If the P content of the wire rod is 0.030% or less, the deterioration of the torsional properties is suppressed, and by satisfying other requirements, the target torsional properties can be obtained. The upper limit of the P content is preferably 0.025%, and more preferably 0.020% or less. The lower limit of the P content is not limited, and is preferably 0% (i.e., no P is contained), but from the viewpoint of reducing the dephosphorization cost, it may be more than 0% or may be 0.001% or more.

[0019] S: 0.030% or less S is an element that deteriorates torsional properties. If the S content of the wire rod is 0.030% or less, the target torsional properties can be obtained while satisfying other requirements. A preferable upper limit of the S content is 0.020%. Note that the lower limit of the S content is not limited, but may be more than 0% or may be 0.001% or more from the viewpoint of reducing desulfurization costs.

[0020] N: 0.0120% or less N is an element that deteriorates torsional properties. If the N content of the wire rod is 0.0120% or less, the target torsional properties can be obtained while satisfying other requirements. A preferred upper limit of the N content is 0.0100%, and a more preferred upper limit is 0.0070%. Note that the lower limit of the N content is not limited, but may be more than 0% or may be 0.0001% or more from the viewpoint of reducing refining costs.

[0021] O: 0.0100% or less O is an element that easily forms oxide-based inclusions in a wire rod. If the O content of the wire rod is 0.0100% or less, coarsening of the oxide-based inclusions is suppressed, and deterioration of torsional properties can be suppressed. A preferred upper limit of the O content is 0.0070%, and a more preferred upper limit is 0.0050%. Note that the lower limit of the O content is not limited, but may be more than 0% or may be 0.0001% or more from the viewpoint of reducing refining costs.

[0022] Al: 0.005% to 0.070% Al is an element that has a deoxidizing effect and is necessary for reducing the amount of oxygen in the wire rod. If the Al content of the wire rod is less than 0.005%, it is difficult to obtain the effect of containing Al. On the other hand, Al is an element that easily forms hard oxide-based inclusions. If the Al content of the wire rod exceeds 0.070%, coarse oxide-based inclusions are significantly more likely to form, resulting in a significant decrease in wiredrawability. From the viewpoint of the deoxidizing effect, the Al content is preferably 0.010% or more, and may be 0.020% or more. On the other hand, from the viewpoint of wiredrawability, the Al content is preferably 0.050% or less, and may be 0.040% or less.

[0023] Mo: 0.02 to 0.20%. Mo is an element that can delay pearlite transformation and bainite transformation even in small amounts, and is particularly effective in improving the strength of the central portion of wire rods with a wire diameter of 7.0 mm or more. It also has the effect of increasing the tensile strength of steel wires obtained after wire drawing. If the Mo content of the wire rod is less than 0.02%, the effects of Mo are not fully achieved. On the other hand, if the Mo content of the wire rod exceeds 0.20%, it becomes difficult to suppress the formation of a martensite structure, which is a hard phase, and the target torsional properties cannot be obtained even if other requirements are met. From the viewpoint of tensile strength, a Mo content of 0.025% or more is preferable, and even better properties are obtained when it is 0.03% or more. On the other hand, from the viewpoint of torsional properties, a Mo content of 0.15% or less is preferable, and even better properties are obtained when it is 0.12% or less.

[0024] The wire rod according to the present disclosure may contain, as an optional element, one or more of Cr, Cu, Ni, Sn, V, Ti, Nb, B, REM, Mg, Ca, Zr, W, Te, and Sb in place of a portion of Fe. These optional elements may not be included (i.e., 0%), or may be included within the following ranges. When these optional elements are included, the lower limit of the content may be greater than 0%. For example, one or more elements selected from the group consisting of Cr, Cu, Sn, Ni, and V may be included, or one or more elements selected from the group consisting of Ti, Nb, B, REM, Mg, Ca, Zr, W, Te, and Sb may be included.

[0025] Cr: 0 to 1.00% The inclusion of Cr is optional. Cr has the effect of increasing the tensile strength of the wire rod and the steel wire obtained after wire drawing. To stably obtain this effect, the Cr content is preferably 0.03% or more. If the Cr content exceeds 1.00%, it becomes difficult to suppress the formation of the martensite structure, which is a hard phase, and the torsional properties deteriorate. Therefore, when Cr is intentionally included in the wire rod, the Cr content is preferably within the range of 0.03 to 1.00%. Alternatively, it may be preferably 0.85% or less. More preferably, it is 0.10 to 0.70%.

[0026] Cu: 0 to 0.80% The inclusion of Cu is optional. Cu has the effect of increasing the corrosion resistance of wire rod and the steel wire obtained after wire drawing. In order to stably obtain this effect, it is preferable that the Cu content be 0.01% or more. On the other hand, even if the Cu content of the wire rod exceeds 0.80%, the effect saturates. Therefore, when Cu is intentionally contained in the wire rod, the Cu content is preferably in the range of 0.01 to 0.80%, and more preferably 0.05 to 0.60%.

[0027] Sn: 0 to 0.50% The inclusion of Sn is optional. Sn has the effect of increasing the corrosion resistance of wire rods and steel wires obtained after wire drawing. In order to stably obtain this effect, it is preferable to set the Sn content to 0.005% or more. On the other hand, even if the Sn content of the wire rod exceeds 0.50%, the effect saturates. Therefore, when Sn is intentionally contained in the wire rod, the Sn content is preferably within the range of 0.001 to 0.50%, and more preferably 0.005 to 0.40%.

[0028] Ni: 0 to 0.50% The inclusion of Ni is optional. Ni has the effect of increasing the corrosion resistance of wire rods and steel wires obtained after wire drawing. In order to stably obtain this effect, it is preferable that the Ni content be 0.01% or more. On the other hand, even if the Ni content of the wire rod exceeds 0.50%, the effect saturates. Therefore, when Ni is intentionally contained in the wire rod, the Ni content is preferably within the range of 0.01 to 0.50%. More preferably, it is 0.05 to 0.40%.

[0029] V: 0 to 0.15% The inclusion of V is optional. V has the effect of increasing the tensile strength of the wire rod and the steel wire obtained after wire drawing. In order to stably obtain this effect, it is preferable that the V content of the wire rod be 0.01% or more. On the other hand, if the V content of the wire rod exceeds 0.15%, the torsional properties deteriorate. Therefore, when V is intentionally contained in the wire rod, the V content of the wire rod is preferably 0.02 to 0.15%. It is more preferably 0.03% to 0.13% or less, and even more preferably 0.05% to 0.12%.

[0030] Ti: 0 to 0.050% The inclusion of Ti is optional. Ti forms carbides or carbonitrides in the wire rod, improving the torsional properties. To achieve this effect, the Ti content of the wire rod is preferably 0.002% or more. On the other hand, if the Ti content of the wire rod exceeds 0.050%, coarse carbides or carbonitrides are likely to form, resulting in a deterioration in the torsional properties. Therefore, when Ti is intentionally included in the wire rod, the Ti content of the wire rod is preferably 0.002 to 0.050%. A more preferable Ti content is 0.005 to 0.030%.

[0031] Nb: 0 to 0.050% The inclusion of Nb is optional. Nb forms carbides or carbonitrides in the wire rod, improving the torsional properties. To obtain this effect, the Nb content of the wire rod is preferably 0.002% or more. On the other hand, if the Nb content of the wire rod exceeds 0.050%, coarse carbides or carbonitrides are likely to be formed, resulting in a deterioration in the torsional properties. Therefore, when Nb is intentionally contained in the wire rod, the Nb content of the wire rod is preferably 0.002 to 0.050%. A more preferable Nb content is 0.005 to 0.030%.

[0032] B: 0 to 0.0040% The inclusion of B is optional. B has the effect of suppressing the ferrite structure and improving the torsional properties. To obtain this effect, it is preferable that the B content of the wire rod is 0.0003% or more. On the other hand, if the B content of the wire rod exceeds 0.0040%, coarse carbides are likely to be formed, and the torsional properties deteriorate. Therefore, when B is intentionally contained in the wire rod, the B content of the wire rod is preferably 0.0003 to 0.0040%. A more preferable B content is 0.0006 to 0.0030%.

[0033] REM: 0 to 0.030% The inclusion of REM is optional. The inclusion of REM allows the wire to exhibit high torsional properties more stably. To obtain this effect, it is preferable that the REM content of the wire be 0.002% or more. On the other hand, if the REM content of the wire exceeds 0.030%, the effect saturates. Therefore, when REM is intentionally included, the REM content of the wire is preferably 0.002 to 0.030%. Note that REM refers to a total of 17 elements, including Sc, Y, and lanthanides, and the REM content refers to the content of one type of REM, or the total content of two or more types of REM.

[0034] Mg: 0 to 0.0040% The inclusion of Mg is optional. If Mg is included, high torsional properties can be exhibited more stably. To obtain this effect, it is preferable that the Mg content of the wire rod is 0.0002% or more. On the other hand, if the Mg content of the wire rod exceeds 0.0040%, the effect saturates. Therefore, when Mg is intentionally included in the wire rod, the Mg content of the wire rod is preferably 0.0002 to 0.0040%.

[0035] Ca: 0 to 0.0040% The inclusion of Ca is optional. If Ca is included, high torsional properties can be exhibited more stably. To obtain this effect, it is preferable that the Ca content of the wire rod be 0.0002% or more. On the other hand, if the Ca content of the wire rod exceeds 0.0040%, the effect saturates. Therefore, when Ca is intentionally included in the wire rod, the Ca content of the wire rod is preferably 0.0002 to 0.0040%.

[0036] Zr: 0 to 0.030% The inclusion of Zr is optional. If Zr is included, high torsional properties can be exhibited more stably. To obtain this effect, it is preferable that the Zr content of the wire rod is 0.002% or more. On the other hand, if the Zr content of the wire rod exceeds 0.030%, coarse carbides or carbonitrides are likely to be formed, and the torsional properties will deteriorate. Therefore, when Zr is intentionally included in the wire rod, the Zr content of the wire rod is preferably 0.002 to 0.030%.

[0037] W: 0 to 0.10% The inclusion of W is optional. If W is included, high torsional properties can be exhibited more stably. To obtain this effect, it is preferable that the W content of the wire rod is 0.02% or more. On the other hand, if the W content of the wire rod exceeds 0.10%, the effect saturates. Therefore, when W is intentionally included in the wire rod, the W content of the wire rod is preferably 0.02 to 0.10%.

[0038] Te: 0 to 0.030% The inclusion of Te is optional. If Te is included, high torsional properties can be exhibited more stably. To obtain this effect, it is preferable that the Te content of the wire rod is 0.001% or more. On the other hand, if the Te content of the wire rod exceeds 0.030%, the effect saturates. Therefore, when Te is intentionally included in the wire rod, the Te content of the wire rod is preferably 0.001 to 0.030%.

[0039] Sb: 0 to 0.030% The inclusion of Sb is optional. If Sb is included, high torsional properties can be exhibited more stably. To obtain this effect, it is preferable that the Sb content of the wire rod is 0.001% or more. On the other hand, if the Sb content of the wire rod exceeds 0.030%, the effect saturates. Therefore, when Sb is intentionally included in the wire rod, the Sb content of the wire rod is preferably 0.001 to 0.030%.

[0040] <Metal Structure> Next, the metal structure of the wire rod according to the present disclosure will be described.

[0041] (Total area ratio of ferrite and martensite structures in the center of the cross section) The total area ratio of ferrite and martensite structures in the center of the wire rod's cross section (cross section perpendicular to the longitudinal direction) should be 5% or less. This reduces the torsional properties of the steel wire after wiredrawing. If the total area ratio of ferrite and martensite structures in the center of the wire rod is 5% or less, the total area ratio of ferrite and martensite structures is low, including up to the surface layer, so the center is used as a representative for measurement. The total area ratio of ferrite and martensite structures in the center of the wire rod's cross section may be 4% or less, 2% or less, or 1% or less. Note that either ferrite or martensite structures may be present, or neither may be present. The same applies to the structure in the longitudinal section of the steel wire, which will be described later.

[0042] <Hardness> Next, the hardness of the wire rod according to the present disclosure will be described.

[0043] (Average Vickers Hardness H) The wire rod according to the present disclosure has an average Vickers hardness H in the cross section that satisfies the following formula (1): 480 × [C] - 40 < H < 480 × [C] + 40 (1). The average Vickers hardness H in the cross section depends on the carbon content [C] in mass% contained in the wire rod. If the average Vickers hardness is below "480 × [C] - 40," it is difficult to consistently impart the required tensile strength (e.g., 2050 MPa or more) to the steel wire after wiredrawing. On the other hand, if the average Vickers hardness in the cross section exceeds "480 × [C] + 40," microcracks are likely to occur during wiredrawing. Even if other requirements are met, the steel wire will not have a tensile strength of 2050 MPa or more and will not be able to achieve the target number of twists of 12 or more in the torsion test in the examples described below. The average Vickers hardness H may be in a range that satisfies the following formula (1A) or may be in a range that satisfies the following formula (1B): 480×[C]−30<H<480×[C]+30 (1A) 480×[C]−20<H<480×[C]+20 (1B)

[0044] (Relationship between Surface Layer Vickers Hardness Hs and Average Vickers Hardness H) In the wire rod according to the present disclosure, the surface layer Vickers hardness Hs at a depth of 0.5 to 1.0 mm from the surface and the average Vickers hardness H satisfy the relationship of formula (2): 0≦Hs−H<30 (2). If the surface layer Vickers hardness Hs is 30 or more greater than the average Vickers hardness H, microcracks are likely to occur during a torsion test, and the target torsion test results cannot be obtained even if other requirements are met. On the other hand, it is industrially difficult to make the surface layer Vickers hardness Hs lower than the average Vickers hardness H with ordinary rolled wire rod. The relationship between the surface layer Vickers hardness Hs and the average Vickers hardness H may be within a range that satisfies the following formula (2A) or (2B): 0≦Hs−H<25 (2A) 0≦Hs−H<20 (2B).

[0045] (Relationship between central Vickers hardness Hc and average Vickers hardness H) In the wire rod according to the present disclosure, the central Vickers hardness Hc and the average Vickers hardness H within 1.0 mm from the center of the cross section satisfy the relationship of formula (3). 0≦H−Hc<30 (3) If the central Vickers hardness Hc is 30 or more smaller than the average Vickers hardness H, it is difficult to consistently impart the tensile strength (e.g., 2050 MPa or more) required of the steel wire after wire drawing. It is industrially difficult to make the central Vickers hardness Hc higher than the average Vickers hardness H with ordinary rolled wire rods. The relationship between the central Vickers hardness Hc and the average Vickers hardness H may be in a range that satisfies the following formula (3A) or formula (3B). 0≦H−Hc<25 (3A) 0≦H−Hc<20 (3B)

[0046] <Wire diameter> The wire rod according to the present disclosure has a wire diameter of 7.0 mm or more. If the wire rod has a wire diameter of less than 7.0 mm, the effects of the present disclosure cannot be obtained. On the other hand, there is no particular upper limit to the wire diameter of the wire rod according to the present disclosure, but it is difficult to industrially produce wire rod with a wire diameter of more than 20 mm using a normal manufacturing process. The wire diameter of the wire rod according to the present disclosure may be 7.5 to 18.0 mm or 8.0 to 16.0 mm.

[0047] [Steel Wire] Next, the steel wire according to the present disclosure will be described. The steel wire according to the present disclosure comprises, in mass %, C: 0.80 to 1.10%, Si: 0.10 to 1.50%, Mn: 0.10 to 1.00%, P: 0.030% or less, S: 0.030% or less, N: 0.0120% or less, O: 0.0100% or less, Al: 0.005 to 0.070%, and Mo: 0.02 to 0.20%, and optionally Cr: 0 to 1.00%, Cu: 0 to 0.80%, Sn: 0 to 0.50%, Ni: 0 to 0.50%, V: 0 to 0.15%, Ti: 0 to 0.050%, Nb: 0 to 0.050%, B: 0 to 0.0040%, It has a chemical composition containing REM: 0 to 0.030%, Mg: 0 to 0.0040%, Ca: 0 to 0.0040%, Zr: 0 to 0.030%, W: 0 to 0.10%, Te: 0 to 0.030%, and Sb: 0 to 0.030%, with the balance being Fe and impurities. Furthermore, the steel wire according to the present disclosure is parallel to the longitudinal direction, and in a cross section passing through the central axis, the total area ratio of the ferrite structure and martensite structure in the center is 5% or less, with the remainder being a mixed structure consisting of ferrite and cementite; the average Vickers hardness h in the cross section perpendicular to the longitudinal direction is 450 to 620; the surface Vickers hardness hs at a depth of 0.2 to 0.5 mm from the surface and the average Vickers hardness h satisfy the relationship of formula (4): 0≦hs−h<30 (4); and the central Vickers hardness hc within 1.0 mm from the center in the perpendicular cross section and the average Vickers hardness h satisfy the relationship of formula (5). 0≦h−hc<30 (5) When the wire rod according to the present disclosure is drawn with a wiredrawing strain in the range of 1.0 to 2.5 to control the average Vickers hardness to 450 to 620, the difference (hs−h) between the surface Vickers hardness and the average Vickers hardness, and the difference (h−hc) between the center Vickers hardness and the average Vickers hardness, are each less than 30. By achieving a hardness distribution in which the surface layer is not too hard and the center is not too soft relative to the average hardness, a steel wire can be obtained that achieves high strength and has good torsional properties. The steel wire according to the present disclosure may be plated with zinc or a zinc alloy, or may be subjected to heat input by degreasing.That is, the steel wire according to the present disclosure also includes a steel wire whose surface is plated (plated wire). When the steel wire according to the present disclosure has a plating layer, the chemical composition, metal structure, and hardness in the present disclosure all refer to values ​​of the steel portion. The steel wire according to the present disclosure may contain optional elements similar to those in the chemical composition of the wire rod described above. The wire diameter of the steel wire according to the present disclosure is not particularly limited, but may be, for example, 3.0 to 8.0 mm, or 4.0 to 7.5 mm.

[0048] <Measurement Method> Next, the measurement method and evaluation test method for the area ratio and hardness of the metallographic structure of the wire rod and steel wire according to the present disclosure will be described. Note that the values ​​in the examples described below are measured values ​​obtained by the following measurement methods. In the following description, the diameter of the wire rod or steel wire to be measured is designated as D.

[0049] (Measurement of area ratio of wire structure) The center of the cross section and points 200 μm above, below, left and right from the center were measured with a scanning electron microscope (SEM) using a 2.7 × 10 -3 mm 2Five images were taken from an area of ​​0.045 mm long and 0.060 mm wide. Prior to SEM observation, the cross section was mirror-polished, and then picral was used for etching to reveal the metal structure. Figures 1(A) to 1(D) respectively show a pearlite structure, a martensite structure, a ferrite structure (labeled "ferrite" in Figure 1(C)), and an example of a mixed structure consisting of ferrite and cementite, which are examples of mixed structures containing ferrite and cementite. The ferrite structure and martensite structure do not contain cementite, while mixed structures consisting of ferrite and cementite are pearlite, bainite, etc., in which cementite is mixed in ferrite. For example, in (C), a pearlite structure (an example of a mixed structure of ferrite and cementite) is present, which is a layered structure of ferrite (the dark part) and cementite (the whitish part). However, the area indicated by the arrow does not contain cementite, and is distinguishable from the surrounding pearlite structure, and is therefore determined to be a ferrite structure. On the other hand, in (A), the two arrows indicate a structure in which more ferrite than cementite is present, but fragmented cementite is present in the ferrite, and it is determined to be a mixed structure of ferrite and cementite. The area ratios (%) of the ferrite structure and martensite structure are measured in each SEM photograph. The ferrite structure and martensite structure, which are structures that do not contain cementite, do not necessarily need to be distinguished from each other. Specifically, after printing each SEM image on paper, a transparent sheet such as an OHP (Overhead Projector) sheet is placed on top of the paper, and the structures that do not contain cementite (ferrite structure and martensite structure) are colored. The transparent sheet with the colored ferrite structure and martensite structure is then analyzed by image analysis to measure the total area ratio of the ferrite structure and martensite structure. The area per field of view is 2.7 × 10 -3 mm 2 The dimensions are 0.045 mm long and 0.060 mm wide, and image analysis software (e.g., Luzex AP manufactured by Nireco Corporation) is used for image analysis. The average value is calculated from the total area ratio of the ferrite structure and martensite structure of the five images, and this average value is used as the total area ratio of the ferrite structure and martensite structure of the wire rod.

[0050] (Measurement of area ratio of steel wire structure) The central part of the longitudinal section was measured by a scanning electron microscope (SEM) at 3 × 10 -4 mm 2 Five SEM images were taken at 200 μm intervals (0.015 mm vertical, 0.02 mm horizontal). Prior to SEM observation, the longitudinal cross section of the steel wire was mirror-polished, and then picral was used for etching to reveal the metal structure. Figures 2A and 2B show examples of SEM images of the longitudinal cross section of a steel wire containing a ferrite structure or a martensite structure, and a mixed structure consisting of ferrite and cementite, respectively. Also, (a) is an enlarged view of the arrowed portion in (A), and (b) is an enlarged view of the arrowed portion in (B). The ferrite structure and martensite structure are structures that do not contain cementite, while the mixed structure consisting of ferrite and cementite is a structure that is formed by wiredrawing pearlite, bainite, etc., and cementite is mixed in the ferrite. The area fractions (%) of the ferrite structure and the martensite structure were measured in each SEM image. It is not necessary to distinguish between the ferrite structure and the martensite structure, which are structures that do not contain cementite. Specifically, each SEM image is printed on paper, and then a transparent sheet such as an OHP (Overhead Projector) sheet is placed on the paper to color the ferrite structure and martensite structure. The colored transparent sheet is then analyzed by image analysis to measure the total area ratio of the ferrite structure and martensite structure. The area per field of view is 3 × 10 -4 mm 2 The dimensions are 0.015 mm long and 0.02 mm wide, and image analysis software (e.g., Luzex AP manufactured by Nireco Corporation) is used for image analysis. The average value is calculated from the area ratios of the ferrite structure and martensite structure of the five images, and the average value is used as the total area ratio of the ferrite structure and martensite structure of the steel wire.

[0051] (Wire Hardness Measurement) Using a Vickers tester, an indenter is pressed into the cross section of the wire with a load of 1 kgf. Starting from a position 0.5 mm deep from the surface (outer surface) of the wire, indentations are made at 0.5 mm intervals toward the center. Indentations are made from four directions at 90° intervals. The surface layer is defined as a region within 0.5 to 1.0 mm deep from the surface, and the average value of the Vickers hardness at a total of eight locations indented at distances of 0.5 mm and 1.0 mm from the surface is defined as the surface Vickers hardness Hs. Meanwhile, the center is defined as a region within 1.0 mm from the center (the central axis of the wire) of the cross section, and the average value of the hardness at the center and at distances of 0.5 mm and 1.0 mm from the center, for a total of nine locations, is defined as the central Vickers hardness Hc. In addition, the average value of the Vickers hardness measured over the entire cross section, i.e., from the center and the surface toward the center at 0.5 mm intervals (excluding areas less than 0.3 mm from the center), is defined as the average Vickers hardness. For example, in the case of a wire rod with a wire diameter of 12 mm, the average value of the Vickers hardness measured at one location in the center and 11 locations between a position 0.5 mm from the surface and a position 0.5 mm from the center × 4 directions = 44 locations, for a total of 45 locations, is taken as the average Vickers hardness H. In addition, in the case of a wire rod with a wire diameter of 8.4 mm, the average value of the hardness measured at one location in the center and 7 locations between 0.5 mm and 3.5 mm from the surface (excluding the position 4.0 mm from the surface because it is 0.2 mm from the center) × 4 directions = 28 locations, for a total of 29 locations, is taken as the average Vickers hardness H.

[0052] (Hardness Measurement of Steel Wire) Using a Vickers testing machine, an indenter is pressed into the cross section of a steel wire with a load of 1 kgf. Starting from a position 0.2 mm deep from the surface (outer surface) of the steel wire, indentations are made at 0.2 mm intervals toward the center. Indentations are made from four directions at 90° intervals. For plated steel wire, the starting point is a position 0.2 mm deep from the surface of the steel portion. The average value of the Vickers hardness measured in a depth range of 0.2 to 0.5 mm from the surface of the steel wire is defined as the surface Vickers hardness hs. The average value of the hardness measured within 1 mm from the center is defined as the central Vickers hardness hc. In addition, the average value of the Vickers hardness measured over the entire cross section, i.e., at 0.2 mm intervals from the center and the surface toward the center (excluding areas less than 0.2 mm from the center) in the cross section, is defined as the average Vickers hardness. For example, in the case of a steel wire with a wire diameter of 5.4 mm, the average value of hardness measured at one location in the center and 12 locations between 0.2 mm and 2.4 mm from the surface (the location of 2.6 mm from the surface is excluded because it is 0.1 mm from the center) x 4 directions = 48 locations, for a total of 49 locations, is defined as the average Vickers hardness h.

[0053] (Twisting test of steel wire) The test is evaluated based on the number of twists until the steel wire breaks, and five tests are conducted for each wire, with the minimum value being evaluated. The distance between chucks is 100 × wire diameter D. The rotation speed is 20 rpm. Note that the breakage of the steel wire referred to here includes not only the breakage of the entire steel wire, but also the occurrence of a partial crack in the steel wire. In other words, if a partial crack occurs in the steel wire during the test, the test is evaluated based on the number of twists at that point.

[0054] (Tensile test) The wire rod to be subjected to the tensile test may be straightened by correction. The length of the wire rod is 340 mm, the distance between chucks is 200 mm, and the tensile test is performed at a stroke speed of 10 mm / min. The diameter of the wire rod is measured in two perpendicular directions at the center of the length of the wire rod using a vernier caliper, and the average value is used. The tensile strength is calculated by dividing the maximum load (N) during the tensile test by the cross-sectional area (mm 2 ), Tensile tests and diameter measurements for steel wire can be performed in the same way as for wire rods. In the case of plated wire, the plating is stripped off and the tensile test is performed on the steel wire alone. Plating can be stripped off chemically, such as by immersion in hydrochloric acid, or physically, such as by grinding.

[0055] <Method for manufacturing wire rod and steel wire> The method for manufacturing the wire rod and steel wire according to the present disclosure is not particularly limited, but an example of a suitable manufacturing method will be described below.

[0056] (Casting of Slabs) Slabs having the above-described chemical composition are produced. For example, when continuous casting is performed, slabs can be obtained by melting steel in a converter, thoroughly electromagnetically stirring the molten steel, and then reducing the steel during solidification.

[0057] (Rolling of Cast Slab) The cast slab is heated to 1200 to 1250° C. and then bloomed to obtain a steel slab.

[0058] (Rolling of wire rod) Next, the steel billet is rolled to obtain a rolled wire rod. The heating temperature of the steel billet is 1020°C to 1080°C. If the steel billet is heated to a temperature below 1020°C, the reaction force becomes large and rolling processing becomes difficult. On the other hand, if the temperature exceeds 1080°C, the austenite structure becomes coarse, and when the steel is immersed in a molten salt as described below, untransformed austenite remains, and there is a possibility that martensite may be mixed in.

[0059] The finish rolling delivery temperature (finish rolling temperature) is set to 900 to 1000° C. It is industrially difficult to set the finish rolling temperature below 900° C. On the other hand, if the finish rolling temperature exceeds 1000° C., the austenite structure will become coarse, and when the steel is immersed in a molten salt as described below, untransformed austenite will remain, possibly resulting in the presence of martensite.

[0060] (Cooling before coiling) After finish rolling, the steel sheet is cooled to 800°C to 900°C (temperature before coiling) by water cooling or air cooling. If the temperature is less than 800°C, the steel sheet will have dropped too low before being immersed in molten salt, causing pearlite transformation to start from the surface layer, resulting in softening of the surface layer. If the temperature exceeds 900°C, the austenite structure will become coarse, and when the steel sheet is immersed in molten salt (described later), untransformed austenite will remain, possibly resulting in the presence of martensite.

[0061] (Cooling before immersion in molten salt) Cooling is performed before immersion in molten salt. Before immersion in molten salt, cooling is performed at a rate of 10°C / second or more to a temperature of 740°C to 800°C (temperature before molten salt). If the temperature is less than 740°C, pearlite transformation starts from the surface layer, softening the surface layer. Coarse pearlite reduces torsional properties. If the temperature exceeds 800°C, the temperature of the molten salt rises and pearlite transformation cannot occur at the target temperature. Furthermore, if the cooling rate is less than 10°C / second, the precipitation of pro-eutectoid cementite will reduce torsional properties. There are no particular limitations on the upper limit of the cooling rate, but from a technical standpoint, it may be 50°C / second or less.

[0062] (Immersion in molten salt) After cooling to a temperature of 740°C to 800°C, the wire is transformed into pearlite or bainite by immersion in molten salt. The molten salt bath is set to 540°C to 570°C, and the wire is immersed for 60 to 120 seconds. If the molten salt temperature is less than 540°C, the ferrite structure increases. On the other hand, if the molten salt temperature exceeds 570°C, the cooling rate inside the wire is insufficient, causing softening. Furthermore, if the immersion time in molten salt is less than 60 seconds, untransformed austenite may remain, and martensite may be mixed in. If the wire is immersed for 120 seconds or longer, the cementite may become spheroidized after transformation, resulting in a decrease in strength.

[0063] (Wiredrawing) The wire rod manufactured through the above steps can be subjected to wiredrawing to obtain a steel wire with high strength and excellent torsional properties. The wiredrawing strain ε due to wiredrawing is expressed by the following formula: ε = Ln(D 0 / D) 2 D 0is the diameter before wiredrawing, and D is the diameter after wiredrawing. ε is preferably 1.0 or more and 2.5 or less. If the wiredrawing strain is lower than 1.0, it is difficult to achieve strength, and if it is higher than 2.5, the processing rate becomes too high and the torsional properties deteriorate. Surface lubrication treatment such as zinc phosphate coating or borax coating is preferably performed before wiredrawing. Steel wire with high strength and excellent torsional properties can be manufactured through the above process. After wiredrawing, post-treatment such as plating or degreasing treatment may be performed. Degreasing treatment and zinc or zinc alloy plating treatment are preferably performed within the range of 400 to 530°C. At temperatures below 400°C, the steel hardens due to age hardening and the torsional properties deteriorate. At temperatures above 530°C, softening due to spheroidization of cementite becomes significant, resulting in insufficient strength.

[0064] <Applications> The applications of the steel wire obtained by wiredrawing the wire rod according to the present disclosure are not particularly limited, but are suitable for a variety of applications requiring high strength and torsional properties, such as steel wire for bridge cables and various ropes. The wire rod according to the present disclosure is suitable as a material for the steel wire used in these applications. For example, a rope (strand) can be obtained by bundling multiple steel wires according to the present disclosure. A rope can also be made by bundling multiple plated wires obtained by applying zinc-containing plating to the steel wire according to the present disclosure.

[0065] The wire rod and steel wire of the present disclosure will be described in more detail below with reference to examples, although these examples do not limit the wire rod and steel wire of the present disclosure.

[0066] Example 1 Steel materials having the chemical compositions (units: mass%) shown in Table 1 were prepared, and wire rods were manufactured by the methods (conditions) shown in Table 2. The notation "-" in Table 1 indicates that the content of the element in question is at the impurity level, and it can be determined that the element is not substantially contained. The same applies to the notation "-" in Table 4 described below. The remainder of the chemical compositions in Tables 1 and 4 is Fe and impurities.

[0067]

[0068]

[0069] For wire rods with diameters of 10.0 to 14.0 mm produced by the above-mentioned manufacturing method, the total area ratio of the ferrite and martensite structures in the center, Vickers hardness, and tensile strength were measured using the methods described above. The wire rods were then drawn to produce steel wires with a diameter of 5.0 mm, i.e., a steel wire with a drawing strain of 2.06 for a 14.0 mm diameter wire. After aging at 450°C for 30 seconds, the Vickers hardness and tensile strength were measured using the methods described above. Furthermore, the number of twists was measured using a torsion test. A tensile strength of 2050 MPa or higher was considered good. Furthermore, a steel wire with a twist count of 12 or more was rated as good (marked A), and a wire with a twist count of less than 12 was rated as poor (marked B). The measurement results are shown in Tables 3A and 3B.

[0070]

[0071]

[0072] For wire rods Nos. 1 to 4, high strength (2050 MPa or more) and excellent torsional properties were obtained by wire drawing. For wire rods Nos. 10 and 11, ferrite and martensite structures were mixed in the wire rod, and the area ratio of the ferrite and martensite structures was high, resulting in wire breakage during wire drawing. For wire rod No. 12, the surface hardness and average hardness of the wire rod were small, and the tensile strength of the steel wire after wire drawing was insufficient. For wire rod No. 13, ferrite and martensite structures were mixed in the structure of the wire rod, and the area ratio of the ferrite and martensite structures was high, resulting in wire breakage during wire drawing. For wire rod No. 14, the surface hardness and average hardness of the wire rod were small, and the tensile strength of the steel wire after wire drawing was insufficient. For wire rod No. 15, the average hardness was small due to pearlite transformation at high temperatures, and the tensile strength of the steel wire after wire drawing was insufficient. In No. 16, the difference between the average hardness and the hardness at the center of the wire rod was large due to the temperature difference between the surface and interior of the wire rod, and the torsional properties of the steel wire after wiredrawing were insufficient. In No. 17, the structure of the wire rod contained a mixture of ferrite and martensite, and the area ratio of the ferrite or martensite structure was high, resulting in wirebreakage during wiredrawing. In No. 18, the average hardness of the wire rod was small due to pearlite transformation at high temperatures, and the tensile strength of the steel wire after wiredrawing was insufficient. In No. 19, the structure of the wire rod contained a mixture of ferrite and martensite, and the area ratio of the ferrite or martensite structure was high, resulting in wirebreakage during wiredrawing.

[0073] Example 2 Steel materials having the chemical compositions (unit: mass %) shown in Table 4 were prepared, and wire rods were manufactured under the conditions of manufacturing method A shown in Table 2.

[0074]

[0075] The total area ratio of the ferrite and martensite structures, Vickers hardness, and tensile strength of the produced wire rods were measured by the methods described above. The wire rods were also drawn to produce steel wires with a wire diameter of 5.0 mm, and the total area ratio of the ferrite and martensite structures in the center, Vickers hardness, and tensile strength were measured by the methods described above. Furthermore, the number of twists was measured by a torsion test. The measurement results are shown in Tables 5A and 5B.

[0076]

[0077]

[0078] Wire rods Nos. 20 to 33 satisfied the requirements of the present disclosure, and steel wires with high strength (2050 MPa or more) and excellent torsional properties were obtained by wiredrawing. No. 40 had an insufficient C content, resulting in insufficient tensile strength of the steel wire after wiredrawing. No. 41 had an excessively high C content, resulting in a low average hardness relative to the C content, and the torsional properties of the steel wire after wiredrawing were insufficient. No. 42 had an excessive Si content, resulting in a high area ratio of ferrite and martensite structures in the wire rod, and wire breakage occurred during wiredrawing. No. 43 had an excessive Mn content, resulting in a high area ratio of ferrite and martensite structures in the wire rod, and wire breakage occurred during wiredrawing. In No. 44, the Mo content was too low, so the average hardness relative to the C content was low, and the difference between the average hardness and the hardness at the center and the difference between the hardness at the surface layer and the average hardness were all large, resulting in insufficient tensile strength and torsional properties of the steel wire after wiredrawing. In No. 45, the Mo content was too high, so martensite was mixed in, the area ratio of martensite structure in the wire rod was high, and the average hardness was also small, resulting in wire breakage during wiredrawing. In No. 46, the Al content was too high, so wire breakage occurred during wiredrawing.

[0079] Although the wire rods and the like according to the present disclosure have been described above, the wire rods and the like according to the present disclosure are not limited to the above-described embodiments and examples. For example, the method for manufacturing the wire rod according to the present disclosure is not limited to the method of winding the wire rod and then immersing it in a molten salt. The scope of the present disclosure also includes a case in which the wire rod according to the present disclosure is manufactured by lead patenting, in which the wire rod is heated and then immersed in a lead bath to create a metal structure, and the wire rod is then drawn to manufacture the steel wire according to the present disclosure, and the steel wires are bundled to manufacture a rope (cable).

Claims

1. By mass%, C: 0.80-1.10%, Si: 0.10-1.50%, Mn: 0.10-1.00%, P: 0.030% or less, S: 0.030% or less, N: 0.0120% or less, O: 0.0100% or less, Al: 0.005-0.070%, Mo: 0.02-0.20%, Cr: 0-1.00%, Cu: 0-0.80%, Sn: 0-0.50%, Ni: 0-0.50%, V: 0-0.15%, Ti: 0-0.050%, Nb: 0-0.050%, B: 0-0.0040%, REM: 0-0.030%, the wire has a chemical composition comprising Mg: 0-0.0040%, Ca: 0-0.0040%, Zr: 0-0.030%, W: 0-0.10%, Te: 0-0.030%, and Sb: 0-0.030%, with the balance being Fe and impurities; in a cross section perpendicular to the longitudinal direction, the total area ratio of a ferrite structure and a martensite structure in a central portion within 1.0 mm from the center is 5% or less, and the balance is a mixed structure consisting of ferrite and cementite; when the content of C in mass% contained in the wire is [C], the average Vickers hardness H in the cross section satisfies the following formula (1): 480×[C]-40<H<480×[C]+40 ... (1); 0≦Hs−H<30 (2) The central Vickers hardness Hc within 1.0 mm from the center and the average Vickers hardness H satisfy the relationship of formula (3), and 0≦H−Hc<30 (3) The wire has a wire diameter of 7.0 mm or more.

2. The wire according to claim 1, wherein the chemical composition includes, in mass%, at least one or more elements selected from the group consisting of Cr: 0.03 to 1.00%, Cu: 0.01 to 0.80%, Sn: 0.001 to 0.50%, Ni: 0.01 to 0.50%, and V: 0.01 to 0.15%.

3. The wire according to claim 1 or 2, wherein the chemical composition includes, in mass%, one or more elements selected from the group consisting of Ti: 0.002-0.050%, Nb: 0.002-0.050%, B: 0.0003-0.0040%, REM: 0.002-0.030%, Mg: 0.0002-0.0040%, Ca: 0.0002-0.0040%, Zr: 0.002-0.030%, W: 0.02-0.10%, Te: 0.001-0.030%, and Sb: 0.001-0.030%.

4. By mass: C: 0.80-1.10%, Si: 0.10-1.50%, Mn: 0.10-1.00%, P: 0.030% or less, S: 0.030% or less, N: 0.0120% or less, O: 0.0100% or less, Al: 0.005-0.070%, Mo: 0.02-0.20%, Cr: 0-1.00%, Cu: 0-0.80%, Sn: 0-0.50%, Ni: 0-0.50%, V: 0-0.15%, Ti: 0-0.050%, Nb: 0-0.050%, B: 0-0.0040%, REM: 0-0.030%, The steel has a chemical composition including Mg: 0-0.0040%, Ca: 0-0.0040%, Zr: 0-0.030%, W: 0-0.10%, Te: 0-0.030%, and Sb: 0-0.030%, with the balance being Fe and impurities; the steel is parallel to the longitudinal direction, and in a cross section passing through the central axis, the total area ratio of the ferrite structure and the martensite structure in the central portion within 1.0 mm from the center is 5% or less, and the balance is a mixed structure consisting of ferrite and cementite; the average Vickers hardness h in the cross section perpendicular to the longitudinal direction is 450-620; the surface Vickers hardness hs at a depth of 0.2-0.5 mm from the surface and the average Vickers hardness h satisfy the relationship of formula (4), and 0≦hs-h<30 ... (4) A steel wire in which the central Vickers hardness hc within 1.0 mm from the center in the vertical cross section and the average Vickers hardness h satisfy the relationship of formula (5). 0≦h−hc<30 (5) 5. The steel wire according to claim 4, wherein the chemical composition includes, in mass%, at least one or more elements selected from the group consisting of Cr: 0.03 to 1.00%, Cu: 0.01 to 0.80%, Sn: 0.001 to 0.50%, Ni: 0.01 to 0.50%, and V: 0.01 to 0.15%.

6. A steel wire according to claim 4 or 5, wherein the chemical composition includes, in mass%, one or more elements selected from the group consisting of Ti: 0.002-0.050%, Nb: 0.002-0.050%, B: 0.0003-0.0040%, REM: 0.002-0.030%, Mg: 0.0002-0.0040%, Ca: 0.0002-0.0040%, Zr: 0.002-0.030%, W: 0.02-0.10%, Te: 0.001-0.030%, and Sb: 0.001-0.030%.

7. The steel wire according to any one of claims 4 to 6, the surface of which is plated.

8. A rope comprising a plurality of steel wires according to any one of claims 4 to 7 bound together.