AI Technical Summary
Non-aqueous secondary battery separators face challenges in achieving strong adhesion to electrodes during wet heat pressing at low temperatures and pressures, which is crucial for preventing battery short circuits as batteries increase in size.
A separator comprising a porous layer with inorganic particles and a binder resin, combined with a phenyl group-containing acrylic resin and a butadiene-acrylonitrile resin in the adhesive layer, ensuring excellent adhesion by wet heat pressing at low temperature and low pressure.
The separator provides excellent adhesion to electrodes, enhancing the reliability and safety of non-aqueous secondary batteries by maintaining strong bonding during the manufacturing process, even at reduced temperature and pressure conditions.
Smart Images

Figure PI2025004666_DRAWING_001 
Figure PI2025004666_DRAWING_002
Abstract
Description
Separator for non-aqueous secondary battery and non-aqueous secondary battery
[0001] The present disclosure relates to a separator for a non-aqueous secondary battery and a non-aqueous secondary battery.
[0002] Patent Document 1 discloses an adhesive for bonding components that constitute a lithium ion secondary battery together, the adhesive containing a particulate polymer having a core-shell structure.
[0003] Patent Documents 2 and 3 disclose separators for non-aqueous secondary batteries, which include an adhesive layer provided on one or both sides of a laminate of a porous substrate and a porous layer, and in which adhesive resin particles are adhered to the laminate.
[0004] International Publication No. WO 2015 / 005145 International Publication No. WO 2019 / 130994 International Publication No. WO 2020 / 246497
[0005] To prevent short circuits in batteries, separators are required to have good adhesion to electrodes. To achieve stronger adhesion, batteries are manufactured by placing a separator impregnated with an electrolyte on the electrodes and then heat-pressing them (this is called "wet heat pressing"). As batteries become larger, the heat-pressing equipment for wet heat pressing becomes more complex. Therefore, there is a need for separators that have excellent adhesion to electrodes even when wet heat pressing is performed at relatively low temperatures and pressures.
[0006] The present disclosure has been made under the above circumstances, and an object of the present disclosure is to provide a separator for a non-aqueous secondary battery that has excellent adhesion to electrodes when wet-heat pressed at low temperature and low pressure.
[0007] Specific means for solving the above problems include the following aspects. <1> A separator for a non-aqueous secondary battery comprising: a porous layer containing inorganic particles and a binder resin; and an adhesive layer containing a phenyl group-containing acrylic resin and a butadiene-acrylonitrile resin, wherein the amount of butadiene units in the resins is 3 mol % to 50 mol % of the total amount of acrylic units, styrene units, butadiene units, and acrylonitrile units. <2> The separator for a non-aqueous secondary battery according to <1>, further comprising a porous substrate, wherein the porous layer is provided on one or both sides of the porous substrate, and the adhesive layer is provided on one or both sides of a laminate of the porous substrate and the porous layer. <3> The separator for a non-aqueous secondary battery according to <1> or <2>, wherein the adhesive layer contains resin particles, wherein the resin particles contain at least one of a phenyl group-containing acrylic resin and a butadiene-acrylonitrile resin. <4> The separator for a non-aqueous secondary battery according to <3>, wherein the average primary particle size of all resin particles contained in the adhesive layer is 0.1 μm to 1.0 μm. <5> The separator for a non-aqueous secondary battery according to any one of <1> to <4>, wherein the mass ratio of the phenyl group-containing acrylic resin to the butadiene-acrylonitrile resin contained in the adhesive layer is 60:40 to 95:5. <6> The separator for a non-aqueous secondary battery according to any one of <1> to <5>, wherein the phenyl group-containing acrylic resin has a styrene-based unit and an acrylic unit, and the molar ratio of the styrene-based unit to the acrylic unit is 30:70 to 50:50. <7> The separator for a non-aqueous secondary battery according to any one of <1> to <6>, wherein the glass transition temperature of all resins contained in the adhesive layer is 58°C to 100°C. <8> The adhesive layer has a basis weight of 0.05 g / m per one side of the nonaqueous secondary battery separator. 2 ~1.0 g / m 2<9> The separator for a nonaqueous secondary battery according to any one of <1> to <8>, wherein the inorganic particles contained in the porous layer have an average primary particle size of 0.01 μm to 1.0 μm. <10> The separator for a nonaqueous secondary battery according to any one of <1> to <9>, wherein the binder resin contains at least one resin selected from the group consisting of polyamide-based resins, acrylic-based resins, fluorine-based resins, and styrene-butadiene-based resins. <11> A nonaqueous secondary battery comprising a positive electrode, a negative electrode, and the separator for a nonaqueous secondary battery according to any one of <1> to <10> disposed between the positive electrode and the negative electrode, and wherein an electromotive force is generated by doping and undoping of lithium ions.
[0008] According to the present disclosure, a separator for a non-aqueous secondary battery is provided that exhibits excellent adhesion to electrodes when subjected to low-temperature, low-pressure wet heat pressing.
[0009] FIG. 1 is a schematic cross-sectional view of an example of a separator according to the present disclosure. FIG. 2 is a schematic cross-sectional view of an example of a separator according to the present disclosure. FIG. 3 is a schematic cross-sectional view of an example of a separator according to the present disclosure. FIG. 4 is a schematic cross-sectional view of an example of a separator according to the present disclosure. FIG. 5 is a schematic cross-sectional view of an example of a separator according to the present disclosure.
[0010]
[0023] The following describes embodiments of the present disclosure. These descriptions and examples are intended to illustrate the embodiments and are not intended to limit the scope of the embodiments.
[0011] In the present disclosure, a numerical range indicated using "to" indicates a range that includes the numerical values before and after "to" as the minimum and maximum values, respectively. In the numerical ranges described in stages in the present disclosure, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. Furthermore, in the numerical ranges described in the present disclosure, the upper or lower limit value of that numerical range may be replaced with a value shown in an example.
[0012] In the present disclosure, the term "step" includes not only an independent step but also a step that cannot be clearly distinguished from other steps as long as the purpose of the step is achieved.
[0013] In the present disclosure, when referring to the amount of each component in a composition, if the composition contains multiple substances corresponding to each component, the total amount of the multiple substances present in the composition is referred to unless otherwise specified. In the present disclosure, multiple types of particles corresponding to each component may be included. If the composition contains multiple types of particles corresponding to each component, the particle size of each component refers to the value for a mixture of the multiple types of particles present in the composition, unless otherwise specified.
[0014] In this disclosure, MD (Machine Direction) refers to the longitudinal direction of a separator manufactured in a long shape, and TD (Transverse Direction) refers to the direction perpendicular to the MD in the plane direction of the separator. In this disclosure, TD is also referred to as the "width direction."
[0015] In the present disclosure, when the stacking relationship of each layer constituting a separator is expressed as "upper" and "lower," the layer closer to the porous substrate is referred to as "lower," and the layer farther from the porous substrate is referred to as "upper."
[0016] In the present disclosure, the volume of the porous layer excluding pores is referred to as the "solid content volume."
[0017] In the present disclosure, performing a heat press treatment after impregnating a separator with an electrolyte solution is referred to as "wet heat press," and performing a heat press treatment without impregnating a separator with an electrolyte solution is referred to as "dry heat press."
[0018] In the present disclosure, the term "(meth)acrylic" means either "acrylic" or "methacrylic."
[0019] In the present disclosure, the "monomer unit" of a polymer or resin means a constituent unit of the polymer or resin, which is a constituent unit formed by polymerization of a monomer. In the present disclosure, a constituent unit formed by polymerization of an acrylic monomer is referred to as an "acrylic unit," a constituent unit formed by polymerization of a styrene monomer is referred to as a "styrene unit," a constituent unit formed by polymerization of butadiene is referred to as a "butadiene unit," and a constituent unit formed by polymerization of acrylonitrile is referred to as an "acrylonitrile unit."
[0020] <Separator for Non-Aqueous Secondary Battery> The separator for a non-aqueous secondary battery according to the present disclosure (also simply referred to as "separator" in the present disclosure) includes a porous layer containing inorganic particles and a binder resin, and an adhesive layer containing a phenyl group-containing acrylic resin and a butadiene-acrylonitrile resin, in which the amount of butadiene units relative to the total amount of acrylic units, styrene units, butadiene units, and acrylonitrile units contained in both resins is 3 mol % to 50 mol %.
[0021] The phenyl group-containing acrylic resin and the butadiene-acrylonitrile resin may be contained in the adhesive layer as two types of resins as separate molecules, or may be contained in the adhesive layer in a linked state.
[0022] The separator of the present disclosure contains a phenyl group-containing acrylic resin and a butadiene-acrylonitrile resin, and has an adhesive layer in which the amount of butadiene units relative to the total amount of acrylic units, styrene units, butadiene units, and acrylonitrile units contained in these resins is 3 mol % to 50 mol %, thereby providing excellent adhesion to electrodes using low-temperature, low-pressure wet heat pressing.The mechanism behind this is presumed to be as follows.
[0023] Phenyl group-containing acrylic resins are resins that easily bond to electrodes when heat is applied. On the other hand, butadiene-acrylonitrile resins are resins that have excellent affinity with electrolyte solutions. It is believed that the amount of butadiene units in the total amount of acrylic units, styrene units, butadiene units, and acrylonitrile units contained in both resins is 3 mol % to 50 mol %, which allows the two resins to mix without separating. It is believed that the mixture of both resins contained in the adhesive layer allows the adhesive layer to adhere well to the electrode even when subjected to a low-temperature, low-pressure wet heat press.
[0024] If the amount of butadiene units relative to the total amount of acrylic units, styrene units, butadiene units, and acrylonitrile units contained in the phenyl group-containing acrylic resin and the butadiene-acrylonitrile resin is less than 3 mol%, the adhesive layer has low affinity for the electrolyte. From the viewpoint of sufficiently impregnating the adhesive layer with the electrolyte, the amount of butadiene units is 3 mol% or more, preferably 3.2 mol% or more, and more preferably 3.5 mol% or more. If the amount of butadiene units relative to the total amount of acrylic units, styrene units, butadiene units, and acrylonitrile units contained in the phenyl group-containing acrylic resin and the butadiene-acrylonitrile resin exceeds 50 mol%, the phenyl group-containing acrylic resin and the butadiene-acrylonitrile resin are difficult to mix. From the viewpoint of thoroughly mixing the two resins, the amount of butadiene units is 50 mol% or less, preferably 40 mol% or less, and more preferably 30 mol% or less.
[0025] The types and molar ratios of the monomer units contained in the phenyl group-containing acrylic resin and the butadiene-acrylonitrile resin are identified by nuclear magnetic resonance (NMR). Specifically, the following measurements are carried out.
[0026] The adhesive layer peeled off from the separator or the resin material used to form the adhesive layer is used as a sample. If the resin material used to form the adhesive layer is a resin particle dispersion, the resin particle dispersion is air-dried to prepare the sample. After swelling the sample with deuterated chloroform, it is measured at room temperature at 600 MHz using an NMR device (JNM-ECA600 manufactured by JEOL Ltd.) and a semi-solid probe (FGMAS probe manufactured by JEOL Ltd.). 1 H-NMR spectrum (MAS rotation speed 6 kHz, observation width 15 ppm, number of points 32 k, pulse repetition waiting time 4 seconds) was measured at 150 MHz. 13 The C-NMR spectrum is measured. 13 The C-NMR spectrum is accumulated approximately 33,000 times in quantitative mode (inverse gate decoupling method, MAS rotation speed 6 kHz, observation width 250 ppm, number of points 32 k, pulse repetition waiting time 12 seconds).
[0027] In the above measurement, it does not matter whether the acrylic units, styrene units, butadiene units, and acrylonitrile units are contained in the phenyl group-containing acrylic resin or the butadiene-acrylonitrile resin. For example, if the butadiene-acrylonitrile resin contains styrene units, the styrene units are also quantified. In the above measurement, acrylonitrile units are not included in the acrylic units. That is, acrylonitrile units are not quantified in duplicate as acrylic units. In the above measurement, styrene units may not be detected. For example, if the phenyl group-containing acrylic resin is a resin that contains phenyl (meth)acrylate units and does not contain styrene units, and the butadiene-acrylonitrile resin is a resin that does not contain styrene units, styrene units will not be detected.
[0028] The separator of the present disclosure may have only a porous layer and an adhesive layer, or may further have a porous substrate. From the viewpoint of increasing the mechanical strength of the separator and imparting a shutdown function to the separator, the separator of the present disclosure preferably has a porous substrate. The porous substrate is a sheet that does not contain inorganic particles, and is distinguished from the porous layer in that it does not contain inorganic particles.
[0029] When the separator of the present disclosure includes a porous substrate, the separator includes a porous layer on one or both sides of the porous substrate, and an adhesive layer on one or both sides of a laminate of the porous substrate and the porous layer.
[0030] In the separator of the present disclosure, the adhesive layer is preferably an adhesive layer containing resin particles from the viewpoint of ion permeability. The resin particles may be attached to the porous layer or porous substrate due to the adhesiveness of the resin particles, or may be included in the adhesive layer together with a binder resin. That is, the adhesive layer may be an adhesive layer in which resin particles are attached to the porous layer or porous substrate, or an adhesive layer containing resin particles and a binder resin.
[0031] When the adhesive layer contains resin particles, the resin particles preferably contain at least one of a phenyl group-containing acrylic resin and a butadiene-acrylonitrile resin. That is, the resin particles may be any of phenyl group-containing acrylic resin particles, butadiene-acrylonitrile resin particles, resin particles containing a phenyl group-containing acrylic resin and a butadiene-acrylonitrile resin, or a combination of two or three of these resin particles.
[0032] The layer structure of the separator of the present disclosure will be described with reference to the drawings.
[0033] 1 to 7 are schematic cross-sectional views of examples of embodiments of the separator of the present disclosure. These cross-sectional views are primarily for explaining the stacking order of layers, and the structure of each layer is omitted or simplified. In FIGS. 1 to 7, layers having similar functions are denoted by the same reference numerals.
[0034] The separator 101 shown in FIG. 1 is a separator in which an adhesive layer 50 is disposed on one surface of a porous layer 30 .
[0035] The separator 102 shown in Fig. 2 is a separator in which adhesive layers 50 are disposed on both sides of a porous layer 30. One adhesive layer 50 and the other adhesive layer 50 may be the same or different in components and / or composition.
[0036] 3 is a separator in which a porous layer 30 is disposed on one side of a porous substrate 20, and an adhesive layer 50 is disposed on one side of a laminate 40 of the porous substrate 20 and one porous layer 30. In the separator 103, the adhesive layer 50 is disposed on the surface of the porous layer 30.
[0037] 4 is a separator in which a porous layer 30 is disposed on one surface of a porous substrate 20, and an adhesive layer 50 is disposed on one surface of a laminate 40 of the porous substrate 20 and one porous layer 30. In the separator 104, the adhesive layer 50 is disposed on the surface of the porous substrate 20.
[0038] 5 is a separator in which a porous layer 30 is disposed on one side of a porous substrate 20, and adhesive layers 50 are disposed on both sides of a laminate 40 of the porous substrate 20 and one porous layer 30. One adhesive layer 50 and the other adhesive layer 50 may be the same or different in components and / or composition.
[0039] 6 is a separator in which porous layers 30 are disposed on both sides of a porous substrate 20, and an adhesive layer 50 is disposed on one side of a laminate 40 of the porous substrate 20 and two porous layers 30. One porous layer 30 and the other porous layer 30 may be the same or different in components and / or composition.
[0040] The separator 107 shown in Fig. 7 is a separator in which porous layers 30 are disposed on both sides of a porous substrate 20, and adhesive layers 50 are disposed on both sides of a laminate 40 of the porous substrate 20 and two porous layers 30. One porous layer 30 and the other porous layer 30 may be the same or different in components and / or composition. One adhesive layer 50 and the other adhesive layer 50 may be the same or different in components and / or composition.
[0041] From the viewpoint of adhering the separator to both opposing electrodes, it is preferable that both surfaces of the separator are adhesive layers 50. From this viewpoint, separators 102, 105 and 107 are preferable.
[0042] In the separators 103 to 107, the porous layer 30 is a layer disposed on the surface of the porous substrate 20. The porous layer 30 may be present on only one surface of the porous substrate 20, or on both surfaces of the porous substrate 20. When the porous layer 30 is present on both surfaces of the porous substrate 20, the heat resistance of the separator is superior, and the safety of the battery can be further improved. In addition, the separator is less likely to curl, and handling during battery production is excellent. When the porous layer 30 is present on only one surface of the porous substrate 20, the ion permeability of the separator is superior. In addition, the overall thickness of the separator can be reduced, and a battery with a higher energy density can be produced.
[0043] The adhesive layer 50 is a layer disposed on the surface of the porous substrate 20 or the porous layer 30, and exists as the outermost layer of the separator.
[0044] From the viewpoint of ion permeability, the adhesive layer 50 is preferably a layer containing resin particles 52. From the viewpoint of superior adhesion to the electrode, the adhesive layer 50 preferably has a structure in which a large number of resin particles 52 are arranged adjacent to each other on the surface of the porous substrate 20 or the porous layer 30, and from the viewpoint of increasing the energy density of the battery, it is preferable that the resin particles 52 have a single layer structure in the thickness direction. However, the structure of the adhesive layer 50 is not limited to the above structure, and the adhesive layer 50 may have a structure in which a large number of resin particles 52 are scattered on the surface of the porous substrate 20 or the porous layer 30, or a structure in which multiple layers of resin particles 52 are stacked in the thickness direction.
[0045] In a separator adhered to an electrode, the resin particles 52 contained in the adhesive layer 50 may melt partially or completely when heat is applied to adhere the separator to the electrode, causing adjacent resin particles 52 to connect to each other, and some or all of the resin particles may not retain their particle shape.
[0046] The porous substrate, porous layer, and adhesive layer of the separator of the present disclosure will be described in detail below.
[0047] [Porous substrate] In the present disclosure, the term "porous substrate" refers to a substrate having pores or gaps therein. Examples of such substrates include microporous membranes; porous sheets made of fibrous materials, such as nonwoven fabrics and paper; and composite porous sheets obtained by laminating one or more other porous layers on these microporous membranes or porous sheets. In the present disclosure, microporous membranes are preferred from the viewpoint of thinning and strength of the separator. The term "microporous membrane" refers to a membrane having a large number of micropores therein, a structure in which the micropores are connected, and which allows gas or liquid to pass from one surface to the other.
[0048] The material of the porous substrate is preferably an electrically insulating material.
[0049] The porous substrate preferably contains a thermoplastic resin to impart a shutdown function to the porous substrate. The shutdown function refers to a function in which, when the battery temperature rises, the constituent materials dissolve and block the pores of the porous substrate, thereby blocking the movement of ions and preventing thermal runaway of the battery. The thermoplastic resin preferably has a melting point of less than 200°C. Examples of the thermoplastic resin include polyesters such as polyethylene terephthalate; polyolefins such as polyethylene and polypropylene; and polyolefins are particularly preferred.
[0050] The porous substrate is preferably a microporous membrane containing polyolefin (referred to as a "polyolefin microporous membrane" in the present disclosure). Examples of polyolefin microporous membranes include those used in conventional battery separators, and it is preferable to select one having sufficient mechanical properties and ion permeability from these.
[0051] From the viewpoint of exhibiting a shutdown function, the polyolefin microporous membrane is preferably a microporous membrane containing polyethylene, and the polyethylene content is preferably 95% by mass or more based on the total mass of the polyolefin microporous membrane.
[0052] The polyolefin microporous film is preferably a microporous film containing polypropylene, from the viewpoint of heat resistance that prevents the film from easily breaking when exposed to high temperatures.
[0053] From the viewpoint of providing a shutdown function and heat resistance that does not easily rupture when exposed to high temperatures, the polyolefin microporous membrane is preferably a polyolefin microporous membrane containing polyethylene and polypropylene. An example of a polyolefin microporous membrane containing polyethylene and polypropylene is a microporous membrane in which polyethylene and polypropylene are mixed in one layer. From the viewpoint of achieving both the shutdown function and heat resistance, the microporous membrane preferably contains 95% by mass or more of polyethylene and 5% by mass or less of polypropylene. Also, from the viewpoint of achieving both the shutdown function and heat resistance, a polyolefin microporous membrane having a laminate structure of two or more layers, at least one layer containing polyethylene and at least one layer containing polypropylene, is preferred.
[0054] The polyolefin contained in the polyolefin microporous membrane preferably has a weight-average molecular weight (Mw) of 100,000 to 5,000,000. When the Mw of the polyolefin is 100,000 or more, the microporous membrane can be imparted with sufficient mechanical properties. On the other hand, when the Mw of the polyolefin is 5,000,000 or less, the microporous membrane has good shutdown properties and is easy to mold.
[0055] Examples of methods for producing a polyolefin microporous membrane include a method in which a molten polyolefin resin is extruded through a T-die to form a sheet, which is crystallized, stretched, and then heat-treated to form a microporous membrane; and a method in which a molten polyolefin resin together with a plasticizer such as liquid paraffin is extruded through a T-die, cooled to form a sheet, stretched, the plasticizer is extracted, and then heat-treated to form a microporous membrane.
[0056] Examples of porous sheets made of fibrous materials include porous sheets such as nonwoven fabrics and papers made of fibrous materials such as polyesters such as polyethylene terephthalate; polyolefins such as polyethylene and polypropylene; heat-resistant resins such as wholly aromatic polyamide, polyamideimide, polyimide, polyethersulfone, polysulfone, polyetherketone, and polyetherimide; and cellulose.
[0057] In the present disclosure, a heat-resistant resin refers to a resin having a melting point of 200° C. or higher, or a resin having no melting point and a decomposition temperature of 200° C. or higher. In other words, a heat-resistant resin in the present disclosure refers to a resin that does not melt or decompose in a temperature range below 200° C.
[0058] Examples of composite porous sheets include sheets in which a functional layer is laminated on a porous sheet made of a microporous membrane or a fibrous material. Such composite porous sheets are preferred because the functional layer allows for additional functionality to be added. For example, from the viewpoint of imparting heat resistance, the functional layer may be a porous layer made of a heat-resistant resin. Examples of heat-resistant resins include one or more heat-resistant resins selected from wholly aromatic polyamides, polyamideimides, polyimides, polyethersulfones, polysulfones, polyetherketones, and polyetherimides. Examples of composite methods include coating a functional layer on a microporous membrane or porous sheet, bonding a microporous membrane or porous sheet and a functional layer with an adhesive, and thermocompression bonding a microporous membrane or porous sheet and a functional layer.
[0059] The surface of the porous substrate may be subjected to various surface treatments to improve wettability with the coating liquid for forming the porous layer, as long as the properties of the porous substrate are not impaired. Examples of surface treatments include corona treatment, plasma treatment, flame treatment, and ultraviolet irradiation treatment.
[0060] -Characteristics of porous substrate- From the viewpoint of increasing the energy density of the battery, the thickness of the porous substrate is preferably 15 μm or less, more preferably 12 μm or less, and even more preferably 10 μm or less, and from the viewpoint of the separator production yield and the battery production yield, the thickness is preferably 3 μm or more, more preferably 5 μm or more, and even more preferably 7 μm or more.
[0061] The thickness of the porous substrate is determined by measuring 20 points within a 10 cm square area with a contact type thickness meter and averaging the measurements.
[0062] The air permeability of the porous substrate is preferably 30 seconds / 100 mL or more, more preferably 50 seconds / 100 mL or more, and even more preferably 70 seconds / 100 mL or more from the viewpoint of suppressing short-circuiting of the battery. The air permeability of the porous substrate is preferably 200 seconds / 100 mL or less, more preferably 180 seconds / 100 mL or less, and even more preferably 160 seconds / 100 mL or less from the viewpoint of ion permeability and suppressing clogging of the porous structure at the boundary between the porous substrate and the porous layer or adhesive layer when exposed to high temperatures.
[0063] The air permeability (seconds / 100 mL) of the porous substrate is measured using a digital Oken air permeability tester in accordance with JIS P8117:2009.
[0064] [Porous Layer] The porous layer has a structure in which many micropores are connected inside, and is a layer that allows gas or liquid to pass from one surface to the other.
[0065] When the separator of the present disclosure includes a porous substrate, the porous layer may be present on only one side of the porous substrate or on both sides of the porous substrate. When the porous layer is present on both sides of the porous substrate, the separator is less likely to curl, resulting in excellent handling during battery production. When the porous layer is present on only one side of the porous substrate, the separator has better ion permeability. Furthermore, the overall thickness of the separator can be reduced, allowing batteries with higher energy density to be produced.
[0066] The porous layer included in the separator of the present disclosure contains at least inorganic particles and a binder resin.
[0067] - Inorganic Particles - Examples of inorganic particles include metal hydroxide particles, metal oxide particles, metal sulfate particles, metal carbonate particles, metal nitride particles, and clay mineral particles.
[0068] Examples of metal hydroxides constituting metal hydroxide particles include magnesium hydroxide, aluminum hydroxide, calcium hydroxide, chromium hydroxide, zirconium hydroxide, cerium hydroxide, nickel hydroxide, boron hydroxide, etc., with magnesium hydroxide being preferred. Examples of metal oxides constituting metal oxide particles include silica, alumina, boehmite (alumina monohydrate), titania, zirconia, magnesium oxide, barium oxide, etc., with alumina being preferred. Examples of metal sulfates constituting metal sulfate particles include barium sulfate, calcium sulfate, etc., with barium sulfate being preferred. Examples of metal carbonates constituting metal carbonate particles include calcium carbonate, magnesium carbonate, barium carbonate, etc. Examples of metal nitrides constituting metal nitride particles include boron nitride, aluminum nitride, etc. Clay mineral particles include calcium silicate, talc, etc.
[0069] The inorganic particles may be surface-modified with a silane coupling agent or the like.
[0070] The inorganic particles may be used alone or in combination of two or more kinds.
[0071] The inorganic particles are preferably at least one type selected from the group consisting of metal hydroxide particles, metal oxide particles, and metal sulfate particles, from the viewpoints of stability in the electrolyte and electrochemical stability.
[0072] The particle shape of the inorganic particles is not limited, and may be any of spherical, elliptical, plate-like, needle-like, and amorphous. From the viewpoint of suppressing short circuits in the battery, the inorganic particles contained in the porous layer are preferably plate-like particles or non-aggregated primary particles.
[0073] The average primary particle size of all the inorganic particles contained in the porous layer is preferably 0.01 μm or more, more preferably 0.02 μm or more, and even more preferably 0.03 μm or more, from the viewpoint of ion permeability of the porous layer. The average primary particle size of all the inorganic particles contained in the porous layer is preferably 1.0 μm or less, more preferably 0.9 μm or less, and even more preferably 0.8 μm or less, from the viewpoint of suppressing interlayer delamination between the porous layer and the porous substrate or adhesive layer and maintaining adhesion of the separator to the electrode.
[0074] The average primary particle size of the inorganic particles is determined by measuring the long diameters of 100 randomly selected inorganic particles in observation using a scanning electron microscope (SEM) and averaging the long diameters of the 100 particles. The sample used for SEM observation is inorganic particles that are the material forming the porous layer, or inorganic particles extracted from the porous layer. There are no limitations on the method for extracting the inorganic particles from the porous layer. Examples of such methods include a method in which the porous layer peeled off from the separator is immersed in an organic solvent that dissolves the binder resin, thereby dissolving the binder resin with the organic solvent and extracting the inorganic particles; and a method in which the porous layer peeled off from the separator is heated to about 800°C to remove the binder resin and extract the inorganic particles.
[0075] From the viewpoint of achieving a good balance between the heat resistance and ion permeability of the porous layer, and the adhesion of the porous layer to the porous substrate, the content of the inorganic particles is preferably 60% by mass to 99% by mass, more preferably 65% by mass to 98% by mass, and even more preferably 68% by mass to 96% by mass, relative to the total mass of the porous layer.
[0076] When porous layers are present on both sides of the porous substrate, the type or amount of inorganic particles contained in one porous layer may be the same as or different from the type or amount of inorganic particles contained in the other porous layer.
[0077] -Organic Particles- The porous layer may contain organic particles. Examples of organic particles include particles made of crosslinked polymers such as crosslinked poly(meth)acrylic acid, crosslinked poly(meth)acrylic acid ester, crosslinked polysilicone, crosslinked polystyrene, crosslinked polydivinylbenzene, styrene-divinylbenzene copolymer crosslinked product, melamine resin, phenol resin, and benzoguanamine-formaldehyde condensate; and particles made of heat-resistant polymers such as polysulfone, polyacrylonitrile, aramid, and polyacetal. The resin constituting the organic particles may be a mixture, modified product, derivative, copolymer (random copolymer, alternating copolymer, block copolymer, graft copolymer), or crosslinked product of the above-mentioned exemplified materials.
[0078] The organic particles may be used alone or in combination of two or more kinds.
[0079] - Binder Resin - The binder resin contained in the porous layer has the function of binding the inorganic particles contained in the porous layer together, as well as the function of adhering the porous layer to the porous substrate, the function of adhering the porous layer to the electrode, and the function of improving the heat resistance of the porous layer.
[0080] When porous layers are present on both sides of the porous substrate, the type or amount of binder resin contained in one porous layer may be the same as or different from the type or amount of binder resin contained in the other porous layer.
[0081] Examples of binder resins include polyamide resins, acrylic resins, fluorine-based resins, styrene-butadiene resins, homopolymers or copolymers of vinyl nitrile compounds (such as acrylonitrile and methacrylonitrile), carboxymethyl cellulose, hydroxyalkyl cellulose, polyvinyl alcohol, polyvinyl butyral, polyvinyl pyrrolidone, polyethers (such as polyethylene oxide and polypropylene oxide), polysulfone, polyketone, polyether ketone, polyether sulfone, and mixtures thereof.
[0082] As the binder resin, from the viewpoint of suppressing interlayer delamination between the porous layer and the adhesive layer, a resin having excellent affinity with the adhesive layer is preferred, and specifically, at least one resin selected from the group consisting of polyamide-based resins, acrylic-based resins, fluorine-based resins, and styrene-butadiene-based resins is preferred.
[0083] From the viewpoint of the heat resistance of the porous layer, the binder resin is preferably a polyamide-based resin. Examples of polyamide-based resins include wholly aromatic polyamide, polyamideimide, poly-N-vinylacetamide, polyacrylamide, copolymerized polyether polyamide, polyimide, and polyetherimide. These resins may be used alone or in combination of two or more.
[0084] Among polyamide resins, fully aromatic polyamides are preferred from the viewpoint of durability. Fully aromatic polyamides refer to polyamides whose main chains are composed only of benzene rings and amide bonds. However, a small amount of aliphatic monomers may be copolymerized in fully aromatic polyamides. Fully aromatic polyamides are also called aramids.
[0085] The wholly aromatic polyamide may be meta-type or para-type. Among wholly aromatic polyamides, meta-type wholly aromatic polyamide (also known as meta-type aramid) is preferred from the viewpoint of ease of forming a porous layer and excellent oxidation-reduction resistance in electrode reactions. Specifically, the wholly aromatic polyamide is preferably polymetaphenylene isophthalamide or polyparaphenylene terephthalamide, and more preferably polymetaphenylene isophthalamide.
[0086] When the porous layer contains a wholly aromatic polyamide, the content of the wholly aromatic polyamide is preferably 85% by mass to 100% by mass, more preferably 90% by mass to 100% by mass, and even more preferably 95% by mass to 99% by mass, relative to the total amount of all resins contained in the porous layer.
[0087] Examples of the acrylic resin include a homopolymer or copolymer of an acrylic monomer, and a copolymer of an acrylic monomer and a styrene monomer. These resins may be used alone or in combination of two or more.
[0088] Examples of acrylic monomers for acrylic resins include (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, isobornyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. Preferred acrylic monomers are alkyl (meth)acrylates. The alkyl group at the ester moiety of the alkyl (meth)acrylate is preferably an alkyl group having 1 to 10 carbon atoms, and more preferably an alkyl group having 1 to 8 carbon atoms. One type of acrylic monomer may be used alone, or two or more types may be used in combination.
[0089] Examples of styrene-based monomers for acrylic resins include styrene and α-methylstyrene; alkyl-substituted styrenes such as 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-ethylstyrene, 3-ethylstyrene, and 4-ethylstyrene; halogen-substituted styrenes such as 2-chlorostyrene, 3-chlorostyrene, and 4-chlorostyrene; and fluorine-substituted styrenes such as 4-fluorostyrene and 2,5-difluorostyrene. As the styrene-based monomer, styrene and α-methylstyrene are preferred, and styrene is more preferred. One type of styrene-based monomer may be used alone, or two or more types may be used in combination.
[0090] As the fluorine-based resin, for example, polyvinylidene fluoride resin can be mentioned.As the polyvinylidene fluoride resin, for example, vinylidene fluoride homopolymer (i.e., polyvinylidene fluoride); copolymer of vinylidene fluoride and halogen-containing monomer such as hexafluoropropylene, tetrafluoroethylene, trifluoroethylene, chlorotrifluoroethylene, vinyl fluoride, trichloroethylene; copolymer of vinylidene fluoride and other monomers other than halogen-containing monomers; copolymer of vinylidene fluoride, halogen-containing monomers, and other monomers other than halogen-containing monomers; mixtures thereof; can be mentioned.These resins can be used alone or in combination of two or more.
[0091] Styrene-butadiene resins are copolymers of styrene monomers and butadiene. Examples of styrene monomers include styrene and α-methylstyrene; alkyl-substituted styrenes such as 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-ethylstyrene, 3-ethylstyrene, and 4-ethylstyrene; halogen-substituted styrenes such as 2-chlorostyrene, 3-chlorostyrene, and 4-chlorostyrene; and fluorine-substituted styrenes such as 4-fluorostyrene and 2,5-difluorostyrene. Preferred styrene monomers are styrene and α-methylstyrene, with styrene being more preferred. One type of styrene monomer may be used alone, or two or more types may be used in combination.
[0092] The styrene-butadiene resin may be copolymerized with a small amount of an acrylic monomer. The acrylic monomer is preferably a (meth)acrylic acid alkyl ester. The alkyl group at the ester moiety of the (meth)acrylic acid alkyl ester is preferably an alkyl group having 1 to 10 carbon atoms, and more preferably an alkyl group having 1 to 8 carbon atoms. Specific examples of the acrylic monomer include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. One type of acrylic monomer may be used alone, or two or more types may be used in combination.
[0093] From the viewpoint of achieving a good balance between the heat resistance and ion permeability of the porous layer, and the adhesion of the porous layer to the porous substrate, the content of the binder resin is preferably 1% by mass to 40% by mass, more preferably 2% by mass to 35% by mass, and even more preferably 4% by mass to 32% by mass, relative to the total mass of the porous layer.
[0094] - Other Components - The porous layer may contain additives such as a dispersant such as a surfactant, a wetting agent, an antifoaming agent, and a pH adjuster. The dispersant is added to the coating liquid for forming the porous layer for the purpose of improving dispersibility, coatability, or storage stability. The wetting agent, antifoaming agent, and pH adjuster are added to the coating liquid for forming the porous layer for the purpose of, for example, improving compatibility with the porous substrate, suppressing air entrapment in the coating liquid, or adjusting the pH.
[0095] -Characteristics of Porous Layer- From the viewpoint of heat resistance, the thickness of each porous layer is preferably 0.5 μm or more, more preferably 1.0 μm or more, and even more preferably 1.5 μm or more. From the viewpoint of ion permeability and the energy density of the battery, the thickness is preferably 5.0 μm or less, more preferably 4.0 μm or less, and even more preferably 3.5 μm or less.
[0096] When the porous layer is present on both sides of the porous substrate, the thickness of the porous layer is preferably 1.0 μm or more, more preferably 2.0 μm or more, and even more preferably 2.5 μm or more, as the total thickness of both sides, and is preferably 10.0 μm or less, more preferably 8.0 μm or less, and even more preferably 6.0 μm or less.
[0097] The thickness of the porous layer is the thickness of the flat membrane after removing the adhesive layer from the separator minus the thickness of the porous substrate. The thickness of the flat membrane after peeling the adhesive layer from the separator is measured at 20 points within a 10 cm square using a contact thickness meter and the average is calculated.
[0098] [Adhesive Layer] The adhesive layer is a layer disposed on the surface of the porous layer or porous substrate, and exists as the outermost layer of the separator. The adhesive layer has numerous gaps or micropores, allowing gas or liquid to pass from one surface to the other.
[0099] From the viewpoint of ion permeability, the adhesive layer is preferably an adhesive layer containing resin particles. The adhesive layer containing resin particles has excellent ion permeability due to the presence of gaps between the resin particles. The resin particles preferably maintain their shape in the electrolyte and are electrochemically stable.
[0100] The resin particles preferably contain at least one of a phenyl group-containing acrylic resin and a butadiene-acrylonitrile resin, i.e., the resin particles may be any of phenyl group-containing acrylic resin particles, butadiene-acrylonitrile resin particles, resin particles containing a phenyl group-containing acrylic resin and a butadiene-acrylonitrile resin, or a combination of two or three of these resin particles.
[0101] When the adhesive layer contains resin particles, the adhesive layer may further contain a non-granular resin. The resin functions, for example, as a binder resin between the resin particles, or between the resin particles and the porous layer or porous substrate. The resin is preferably at least one of a phenyl group-containing acrylic resin and a butadiene-acrylonitrile resin.
[0102] When the adhesive layer contains resin particles, the average primary particle size of all the resin particles contained in the adhesive layer is preferably 0.1 μm or more, more preferably 0.2 μm or more, and even more preferably 0.3 μm or more, from the viewpoint of ion permeability of the adhesive layer. The average primary particle size of all the resin particles contained in the adhesive layer is preferably 1.0 μm or less, more preferably 0.9 μm or less, and even more preferably 0.8 μm or less, from the viewpoint of preventing the resin particles from falling off.
[0103] The average primary particle size of the resin particles is determined by measuring the long diameters of 100 randomly selected resin particles in observation with a scanning electron microscope (SEM) and averaging the long diameters of the 100 particles. The sample used for SEM observation is resin particles that are a material for forming the adhesive layer, or resin particles removed from the adhesive layer.
[0104] The adhesive layer contains a phenyl group-containing acrylic resin and a butadiene-acrylonitrile resin. The phenyl group-containing acrylic resin and the butadiene-acrylonitrile resin contained in the adhesive layer may be two types of resin in the form of separate molecules, two types of resin in the form of linked molecules, or a mixture thereof.
[0105] The phenyl group-containing acrylic resin and butadiene-acrylonitrile resin contained in the adhesive layer have a butadiene unit content of 3 mol% to 50 mol%, preferably 3.2 mol% to 40 mol%, and more preferably 3.5 mol% to 30 mol%, of the total amount of acrylic units, styrene units, butadiene units, and acrylonitrile units contained in both resins.
[0106] The mass ratio of the phenyl group-containing acrylic resin to the butadiene-acrylonitrile resin contained in the adhesive layer (phenyl group-containing acrylic resin:butadiene-acrylonitrile resin) is preferably 60:40 to 95:5, more preferably 55:45 to 92:8, and even more preferably 51:49 to 90:10, from the viewpoint of facilitating adhesion of the adhesive layer to the electrode by wet heat pressing.
[0107] - Phenyl Group-Containing Acrylic Resin - The polymerization component that provides the phenyl group in the phenyl group-containing acrylic resin is not limited. Examples of the polymerization component that provides the phenyl group include phenyl (meth)acrylate and styrene-based monomers.
[0108] The phenyl group-containing acrylic resin preferably contains a styrene unit from the viewpoint of facilitating adhesion of the resin to an electrode by wet heat pressing. That is, the phenyl group-containing acrylic resin preferably contains at least an acrylic monomer and a styrene monomer as polymerization components.
[0109] When the phenyl group-containing acrylic resin contains an acrylic monomer and a styrene monomer as polymerization components, it may be a random copolymer, an alternating copolymer, a block copolymer, or a graft copolymer of these two monomers. For example, the phenyl group-containing acrylic resin may be a block copolymer or a graft copolymer of an acrylic monomer and a styrene monomer, and the acrylic unit may be arranged in the core of the phenyl group-containing acrylic resin particle, and the styrene unit may be arranged in the shell.
[0110] The acrylic monomer is preferably at least one selected from the group consisting of (meth)acrylic acid, (meth)acrylates, and (meth)acrylic acid esters. One acrylic monomer may be used alone, or two or more acrylic monomers may be used in combination.
[0111] Examples of (meth)acrylate salts include sodium (meth)acrylate, potassium (meth)acrylate, magnesium (meth)acrylate, zinc (meth)acrylate, etc. Examples of (meth)acrylic acid esters include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, isobornyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-(diethylamino)ethyl (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, and phenyl (meth)acrylate.
[0112] The acrylic monomer is preferably a (meth)acrylic acid alkyl ester. The alkyl group at the ester moiety of the (meth)acrylic acid alkyl ester is preferably an alkyl group having 1 to 10 carbon atoms, and more preferably an alkyl group having 1 to 8 carbon atoms.
[0113] Specific examples of the acrylic monomer include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. These acrylic monomers may be used alone or in combination of two or more.
[0114] Examples of styrene-based monomers include styrene, α-methylstyrene, alkyl-substituted styrenes such as 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-ethylstyrene, 3-ethylstyrene, and 4-ethylstyrene, halogen-substituted styrenes such as 2-chlorostyrene, 3-chlorostyrene, and 4-chlorostyrene, and fluorine-substituted styrenes such as 4-fluorostyrene and 2,5-difluorostyrene. One type of styrene-based monomer may be used alone, or two or more types may be used in combination.
[0115] As the styrene-based monomer, styrene and α-methylstyrene are preferred, and styrene is more preferred.
[0116] The phenyl group-containing acrylic resin preferably has a styrene unit and an acrylic unit, and the molar ratio of the two units (styrene unit:acrylic unit) is preferably 30:70 to 50:50, more preferably 35:65 to 45:55, and even more preferably 37:63 to 43:57, from the viewpoint of ease of adhesion of the resin to electrodes by wet heat pressing. The molar ratio is determined by nuclear magnetic resonance (NMR). Details of NMR are as described above.
[0117] The phenyl group-containing acrylic resin may contain a monomer other than the acrylic monomer and the styrene monomer as a polymerization component. Examples of such monomers include acid group-containing monomers. Examples of acid group-containing monomers include: carboxyl group-containing monomers such as crotonic acid, maleic acid, fumaric acid, and itaconic acid; sulfonic acid group-containing monomers such as vinyl sulfonic acid, methyl vinyl sulfonic acid, (meth)allyl sulfonic acid, (meth)acrylic acid-2-ethyl sulfonate, 2-acrylamido-2-methylpropanesulfonic acid, and 3-allyloxy-2-hydroxypropanesulfonic acid; phosphate group-containing monomers such as 2-(meth)acryloyloxyethyl phosphate, methyl-2-(meth)acryloyloxyethyl phosphate, and ethyl-(meth)acryloyloxyethyl phosphate; and hydroxyl group-containing monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. The acid group-containing monomer may be used alone or in combination of two or more kinds.
[0118] The phenyl group-containing acrylic resin may contain a crosslinkable monomer as a polymerization component. Examples of the crosslinkable monomer include polyfunctional monomers having two or more polymerizable groups. Examples of polyfunctional monomers include divinyl compounds such as divinylbenzene; di(meth)acrylic acid ester compounds such as diethylene glycol dimethacrylate, ethylene glycol dimethacrylate, diethylene glycol diacrylate, and 1,3-butylene glycol diacrylate; tri(meth)acrylic acid ester compounds such as trimethylolpropane trimethacrylate and trimethylolpropane triacrylate; and ethylenically unsaturated monomers containing epoxy groups such as allyl glycidyl ether and glycidyl methacrylate. One type of polyfunctional monomer may be used alone, or two or more types may be used in combination.
[0119] -Butadiene-acrylonitrile-based resin- The butadiene-acrylonitrile-based resin may be a resin composed only of butadiene units and acrylonitrile units, or may be a resin composed of butadiene units, acrylonitrile units, and other monomer units. In other words, the butadiene-acrylonitrile-based resin may be a binary copolymer of butadiene and acrylonitrile, or a copolymer of butadiene, acrylonitrile, and other monomers. Examples of other monomers include styrene-based monomers and acrylic-based monomers.
[0120] Examples of styrene-based monomers include styrene and α-methylstyrene; alkyl-substituted styrenes such as 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 2-ethylstyrene, 3-ethylstyrene, and 4-ethylstyrene; halogen-substituted styrenes such as 2-chlorostyrene, 3-chlorostyrene, and 4-chlorostyrene; and fluorine-substituted styrenes such as 4-fluorostyrene and 2,5-difluorostyrene. Preferred styrene-based monomers are styrene and α-methylstyrene, and styrene is more preferred. One type of styrene-based monomer may be used alone, or two or more types may be used in combination.
[0121] Examples of acrylic monomers include (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, isobornyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. Preferred acrylic monomers are alkyl (meth)acrylates. The alkyl group at the ester moiety of the alkyl (meth)acrylate is preferably an alkyl group having 1 to 10 carbon atoms, and more preferably an alkyl group having 1 to 8 carbon atoms. One type of acrylic monomer may be used alone, or two or more types may be used in combination.
[0122] The molar ratio of butadiene units to acrylonitrile units (butadiene units:acrylonitrile units) contained in the butadiene-acrylonitrile resin is preferably 60:40 to 1:99, more preferably 50:50 to 10:90, from the viewpoint of excellent affinity with the phenyl group-containing acrylic resin. The molar ratio is determined by nuclear magnetic resonance (NMR). Details of NMR are as described above.
[0123] -Other Resins- The adhesive layer may contain other resins in addition to the phenyl group-containing acrylic resin and the butadiene-acrylonitrile resin. Examples of other resins include polyvinylidene fluoride resins, fluorine-containing rubbers, homopolymers or copolymers of vinyl nitrile compounds (such as acrylonitrile and methacrylonitrile), carboxymethyl cellulose, hydroxyalkyl cellulose, polyvinyl alcohol, polyvinyl butyral, polyvinyl pyrrolidone, polyethers (such as polyethylene oxide and polypropylene oxide), and mixtures of two or more of these. These resins may be contained in the form of resin particles or as a binder resin for the resin particles.
[0124] The mass proportion of other resins in the total resin of the adhesive layer is preferably 10 mass% or less, more preferably 5 mass% or less, even more preferably 1 mass% or less, and particularly preferably substantially none. The mass proportion of the total of the phenyl group-containing acrylic resin and the butadiene-acrylonitrile resin in the total resin of the adhesive layer is preferably 90 mass% or more, more preferably 95 mass% or more, even more preferably 99 mass% or more, and particularly preferably 100 mass%.
[0125] Although the detailed mechanism is unknown, from the viewpoint of excellent adhesion to the electrode, the glass transition temperature of the entire resin contained in the adhesive layer is preferably 58° C. or higher, more preferably 58.5° C. or higher, and even more preferably 59° C. or higher. There is no upper limit to the glass transition temperature of the entire resin contained in the adhesive layer, but it is preferably 100° C. or lower, more preferably 95° C. or lower, and even more preferably 94° C. or lower.
[0126] The glass transition temperature of the resin can be controlled by adjusting the types and copolymerization ratio of the monomers that are the polymerization components, using the FOX formula as a guideline.
[0127] The glass transition temperature of a resin is determined from a differential scanning calorimetry (DSC) curve obtained by DSC measurement. In the DSC curve, the intersection of the low-temperature baseline and the tangent to the curve of the stepwise change portion is defined as intersection (1), and the intersection of the high-temperature baseline and the tangent to the curve of the stepwise change portion is defined as intersection (2). The glass transition temperature is determined as the temperature midway between intersection (1) and intersection (2).
[0128] -Other Components- The adhesive layer may contain additives such as a dispersant such as a surfactant, a wetting agent, an antifoaming agent, and a pH adjuster. The dispersant is added, for example, to the resin particle dispersion for forming the adhesive layer for the purpose of improving dispersibility, coatability, or storage stability. The wetting agent, antifoaming agent, and pH adjuster are added, for example, to the resin particle dispersion for forming the adhesive layer for the purpose of improving compatibility with the porous layer or porous substrate, for the purpose of suppressing air entrapment in the resin particle dispersion, or for the purpose of adjusting the pH.
[0129] - Characteristics of adhesive layer - The basis weight (mass per unit area) of the adhesive layer is set to 0.05 g / m per side of the separator from the viewpoint of adhesion to the electrode. 2 More than 0.07 g / m 2 More preferably, 0.1 g / m or more 2 The weight of the adhesive layer is more preferably 1.0 g / m per one side of the separator from the viewpoint of ion permeability. 2 Preferably, 0.8 g / m or less 2 More preferably, 0.6 g / m or less 2 The following is even more preferred:
[0130] When the adhesive layer is on both sides of the separator, the total weight of the adhesive layer on both sides is 0.1 g / m 2 ~2.0 g / m 2 is preferred, and 0.14 g / m 2 ~1.6g / m 2 More preferably, 0.2 g / m 2 ~1.2g / m 2 is more preferred.
[0131] The basis weight of the adhesive layer is determined by cutting a separator into a 20 cm x 20 cm piece, measuring the mass of the layer corresponding to the adhesive layer, and dividing the mass by the area to determine the total for both sides. When adhesive layers are formed in equal amounts on both sides of the separator, half of the total for both sides is calculated as the basis weight (g / m) per side. 2 )
[0132] [Separator Characteristics] The thickness of the separator is preferably 5 μm or more, more preferably 7 μm or more, and even more preferably 9 μm or more from the viewpoint of the mechanical strength of the separator, and is preferably 22 μm or less, more preferably 20 μm or less, and even more preferably 18 μm or less from the viewpoint of the energy density of the battery.
[0133] The thickness of the separator is determined by measuring 20 points within a 10 cm square area with a contact type thickness meter and averaging the measurements.
[0134] From the viewpoint of suppressing short circuits in the battery, the separator has an air permeability of preferably 60 sec / 100 mL or more, more preferably 70 sec / 100 mL or more, and even more preferably 80 sec / 100 mL or more. From the viewpoint of ion permeability, the separator has an air permeability of preferably 260 sec / 100 mL or less, more preferably 250 sec / 100 mL or less, and even more preferably 240 sec / 100 mL or less.
[0135] The air permeability (seconds / 100 mL) of the separator is measured using a digital Oken air permeability tester in accordance with JIS P8117:2009.
[0136] [Method for manufacturing separator] The separator of the present disclosure is manufactured, for example, by the following manufacturing method A or manufacturing method B. Manufacturing methods A and B are methods for manufacturing a separator including a porous substrate. By replacing the porous substrate in manufacturing methods A and B with a release sheet and peeling off the release sheet at an appropriate time, it is possible to manufacture a separator including only a porous layer and an adhesive layer.
[0137] In the manufacturing method A and the manufacturing method B, the porous layer is formed on the porous substrate by a wet coating method. In the present disclosure, the wet coating method is a method in which the coating layer is solidified in a coagulation liquid, and the dry coating method is a method in which the coating layer is solidified by drying.
[0138] Production method A (discontinuous production method): A porous layer is formed on a porous substrate unwound from a roll to obtain a laminate of the porous substrate and the porous layer, and the laminate is then temporarily wound up on another roll. Next, an adhesive layer is formed on the laminate unwound from the roll to obtain a separator, and the completed separator is then wound up on another roll.
[0139] Manufacturing method B (continuous manufacturing method): A porous layer and an adhesive layer are formed continuously or simultaneously on a porous substrate unwound from a roll, and the completed separator is wound up on another roll.
[0140] The manufacturing method B may be any of the following modes B-1 to B-4.
[0141] Configuration B-1: A porous layer-forming coating liquid is applied onto a porous substrate, the substrate is immersed in a coagulation liquid to solidify the coating layer, the substrate is pulled out of the coagulation liquid, washed with water, and dried, and then a resin particle dispersion liquid is applied onto the substrate and dried.
[0142] Configuration B-2: A porous layer-forming coating liquid is applied onto a porous substrate, the coating layer is solidified by immersion in a coagulation liquid, the substrate is pulled out of the coagulation liquid and washed with water, and then a resin particle dispersion liquid is applied onto the substrate and dried.
[0143] Configuration B-3: Two layers, a coating liquid for forming a porous layer and a resin particle dispersion liquid, are simultaneously coated onto a porous substrate, the substrate is immersed in a coagulating liquid to solidify the former coating layer, and the substrate is then removed from the coagulating liquid, washed with water, and dried.
[0144] Configuration B-4: A coating liquid for forming a porous layer is applied onto a porous substrate, the coating layer is solidified by immersion in a coagulation liquid, the substrate is removed from the coagulation liquid, and the substrate is transported through a water bath containing resin particles to wash with water and allow the resin particles to adhere, and the substrate is removed from the water bath and dried.
[0145] The steps included in the production method will be described in detail below, taking Production Method B of Form B-1 as an example.
[0146] In the manufacturing method B of the embodiment B-1, a porous layer is formed on at least one surface of a porous substrate by a wet coating method to obtain a laminate of the porous substrate and the porous layer, and then an adhesive layer is formed on at least one surface of the laminate by a dry coating method. The manufacturing method B of the embodiment B-1 includes the following steps (1) to (7), which are carried out in order.
[0147] Step (1): Preparation of Porous Layer-Forming Coating Liquid The porous layer-forming coating liquid (hereinafter referred to as "coating liquid" in the description of the production method) is prepared by dissolving or dispersing the binder resin and inorganic particles of the porous layer in a solvent. If necessary, other components besides the binder resin and inorganic particles may be dissolved or dispersed in the coating liquid.
[0148] The solvent used in preparing the coating liquid includes a solvent that dissolves the binder resin of the porous layer (hereinafter also referred to as a "good solvent"). Examples of the good solvent include polar amide solvents such as N-methylpyrrolidone, dimethylacetamide, dimethylformamide, and dimethylformamide.
[0149] From the viewpoint of forming a porous layer having a good porous structure, the solvent used in preparing the coating liquid preferably contains a phase separation agent that induces phase separation. Therefore, the solvent used in preparing the coating liquid is preferably a mixed solvent of a good solvent and a phase separation agent. The phase separation agent is preferably mixed with the good solvent in an amount that ensures a viscosity appropriate for coating. Examples of the phase separation agent include water, methanol, ethanol, propyl alcohol, butyl alcohol, butanediol, ethylene glycol, propylene glycol, and tripropylene glycol.
[0150] As the solvent used for preparing the coating liquid, from the viewpoint of forming a good porous structure, a mixed solvent of a good solvent and a phase separation agent is preferred, which mixed solvent contains 60% by mass or more of the good solvent and 5% by mass to 40% by mass of the phase separation agent.
[0151] The resin concentration in the coating liquid is preferably 1% by mass to 20% by mass from the viewpoint of forming a good porous structure, and the inorganic particle concentration in the coating liquid is preferably 0.5% by mass to 50% by mass from the viewpoint of forming a good porous structure.
[0152] Step (2): Preparation of Resin Particle Dispersion The resin particle dispersion is prepared by dispersing resin particles in a suitable dispersion medium (e.g., water). A surfactant may be added to the resin particle dispersion to enhance the dispersibility of the resin particles in the dispersion medium. The resin particle dispersion may be a commercially available product or a diluted solution of a commercially available product.
[0153] From the viewpoint of coating suitability, the concentration of the resin particles in the resin particle dispersion is preferably 1% by mass to 60% by mass.
[0154] Step (3): Coating of coating liquid The coating liquid is coated on at least one surface of the porous substrate to form a coating layer on the porous substrate. Methods for applying the coating liquid to the porous substrate include knife coating, Mayer bar coating, die coating, reverse roll coating, roll coating, gravure coating, screen printing, inkjet printing, and spraying. When forming a porous layer on both sides of the porous substrate, it is preferable from the viewpoint of productivity to coat the coating liquid on both sides of the porous substrate simultaneously.
[0155] Step (4): Solidification of the Coating Layer The porous substrate with the coating layer formed thereon is immersed in a coagulation liquid to induce phase separation in the coating layer while solidifying the binder resin, thereby forming a porous layer containing the binder resin and inorganic particles, thereby obtaining a laminate consisting of the porous substrate and the porous layer.
[0156] The coagulation liquid generally contains the good solvent and phase separation agent used in preparing the coating liquid, as well as water. From a productivity perspective, it is preferable that the mixing ratio of the good solvent and the phase separation agent be the same as the mixing ratio of the mixed solvent used in preparing the coating liquid. From the viewpoints of forming a porous structure and productivity, the water content in the coagulation liquid is preferably 40% by mass to 90% by mass. The temperature of the coagulation liquid is, for example, 20°C to 50°C.
[0157] Step (5): Washing and drying of coating layer The laminate is lifted out of the coagulating solution and washed with water. By washing with water, the coagulating solution is removed from the laminate. Furthermore, by drying, water is removed from the laminate. Washing with water is carried out, for example, by transporting the laminate in a water washing bath. Drying is carried out, for example, by transporting the laminate in a high-temperature environment, by blowing air on the laminate, or by bringing the laminate into contact with a heat roll. The drying temperature is preferably 40°C to 80°C.
[0158] Step (6): Coating of Resin Particle Dispersion The resin particle dispersion is coated on at least one surface of the laminate. Examples of methods for coating the resin particle dispersion include knife coating, gravure coating, Mayer bar coating, die coating, reverse roll coating, roll coating, screen printing, inkjet printing, and spraying.
[0159] Step (7): Drying of Resin Particle Dispersion The resin particle dispersion on the laminate is dried to adhere the resin particles to the surface of the laminate. Drying is performed, for example, by transporting the laminate in a high-temperature environment or by blowing air onto the laminate. The drying temperature is preferably 40°C to 100°C.
[0160] The production method A or the production method B of Forms B-2 to B-4 can be carried out by partially omitting or modifying the above steps (1) to (7).
[0161] The nonaqueous secondary battery according to the present disclosure is a nonaqueous secondary battery that generates electromotive force by doping and dedoping lithium ions, and includes a positive electrode, a negative electrode, and the separator according to the present disclosure. "Doping" refers to occlusion, support, adsorption, or insertion, and refers to the phenomenon in which lithium ions enter the active material of an electrode such as a positive electrode.
[0162] The nonaqueous secondary battery of the present disclosure has a structure in which, for example, a battery element in which a negative electrode and a positive electrode face each other with a separator interposed therebetween is enclosed in an exterior material together with an electrolyte solution. The nonaqueous secondary battery of the present disclosure is suitable for nonaqueous electrolyte secondary batteries, particularly lithium ion secondary batteries.
[0163] The nonaqueous secondary battery of the present disclosure has excellent productivity in terms of battery productivity, since the separator of the present disclosure is well bonded to the electrodes by low-temperature, low-pressure wet heat pressing.
[0164] Hereinafter, examples of the positive electrode, negative electrode, electrolyte, and exterior material included in the nonaqueous secondary battery of the present disclosure will be described.
[0165] An example of the positive electrode is a structure in which an active material layer containing a positive electrode active material and a binder resin is formed on a current collector. The active material layer may further contain a conductive additive. Examples of the positive electrode active material include lithium-containing transition metal oxides, specifically LiCoO 2 , LiNiO 2 , LiMn 1/2 Ni 1/2 O 2 , LiCo 1/3 Mn 1/3 Ni 1/3 O 2 , LiMn 2 O 4 , LiFePO 4 , LiCo 1/2 Ni 1/2 O 2 , LiAl 1/4 Ni 3/4 O 2 Examples of binder resins include polyvinylidene fluoride resins and styrene-butadiene copolymers. Examples of conductive additives include carbon materials such as acetylene black, ketjen black, and graphite powder. Examples of current collectors include aluminum foil, titanium foil, and stainless steel foil, each having a thickness of 5 μm to 20 μm.
[0166] An example of an embodiment of the negative electrode includes a structure in which an active material layer containing a negative electrode active material and a binder resin is formed on a current collector. The active material layer may further include a conductive additive. Examples of negative electrode active materials include materials capable of electrochemically absorbing lithium ions, such as carbon materials; alloys of lithium with silicon, tin, aluminum, etc.; and Wood's alloy. Examples of binder resins include polyvinylidene fluoride resins and styrene-butadiene copolymers. Examples of conductive additives include carbon materials such as acetylene black, ketjen black, graphite powder, and ultrafine carbon fibers. Examples of current collectors include copper foil, nickel foil, stainless steel foil, and the like, each having a thickness of 5 μm to 20 μm. Alternatively, a metallic lithium foil may be used as the negative electrode instead of the above-described negative electrode.
[0167] The electrolyte is a solution in which a lithium salt is dissolved in a non-aqueous solvent. Examples of the lithium salt include LiPF 6 , LiBF 4 , LiClO 4 Examples of non-aqueous solvents include cyclic carbonates such as ethylene carbonate, propylene carbonate, fluoroethylene carbonate, difluoroethylene carbonate, and vinylene carbonate; chain carbonates such as dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, and fluorine-substituted derivatives thereof; and cyclic esters such as γ-butyrolactone and γ-valerolactone; which may be used alone or in combination. A suitable electrolyte solution is a solution in which a cyclic carbonate and a chain carbonate are mixed in a mass ratio (cyclic carbonate:chain carbonate) of 20:80 to 40:60, and a lithium salt is dissolved in the range of 0.5 mol / L to 1.5 mol / L.
[0168] Examples of the exterior packaging include aluminum laminate film packs, metal cans, etc. The shape of the battery may be rectangular, cylindrical, coin-shaped, etc., and the separator of the present disclosure is suitable for any shape.
[0169] The nonaqueous secondary battery of the present disclosure can be produced by producing a laminate in which the separator of the present disclosure is disposed between a positive electrode and a negative electrode, and then using this laminate by, for example, Production Method 1 or Production Method 2 described below.
[0170] Manufacturing method 1: The laminate is dry-heat pressed to temporarily bond the electrodes and separator, then housed in an exterior packaging (e.g., an aluminum laminate film pack; the same applies hereinafter), and an electrolyte solution is poured into it. The laminate is then wet-heat pressed from above the exterior packaging to bond the electrodes and separator and seal the exterior packaging.
[0171] Manufacturing method 2: The laminate is placed in an exterior packaging material, and an electrolyte solution is poured into the packaging material. The laminate is then wet heat pressed onto the exterior packaging material to bond the electrodes and separator together and seal the exterior packaging material.
[0172] In Production Method 1 and Production Method 2, the pressing temperature of the wet heat press is preferably 50° C. to 80° C., more preferably 60° C. to 70° C. The pressing pressure of the wet heat press is preferably 40 kPa to 200 kPa, more preferably 50 kPa to 100 kPa. The pressing time of the wet heat press is preferably adjusted according to the pressing temperature and pressing pressure, and is adjusted, for example, within the range of 8 hours to 20 hours.
[0173] When manufacturing a laminate in which a separator is disposed between a positive electrode and a negative electrode, the method of disposing the separator between the positive electrode and the negative electrode may be a method of stacking at least one layer of a positive electrode, a separator, and a negative electrode in this order (so-called stack method), or a method of stacking a positive electrode, a separator, a negative electrode, and a separator in this order and winding them in the length direction.
[0174] The separator and nonaqueous secondary battery of the present disclosure will be described in more detail below with reference to examples. The materials, amounts used, ratios, processing procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present disclosure. Therefore, the scope of the separator and nonaqueous secondary battery of the present disclosure should not be construed as being limited by the specific examples shown below.
[0175] In the following description, syntheses, treatments, manufacturing, etc. were carried out at room temperature (25° C.±3° C.) unless otherwise specified.
[0176] <Measurement Methods and Evaluation Methods> The measurement methods and evaluation methods used in the examples and comparative examples are as follows.
[0177] [Air Permeability of Separator and Porous Substrate] The air permeability (seconds / 100 mL) of the separator and porous substrate was measured according to JIS P8117:2009 using a digital Oken air permeability tester (Asahi Seiko Co., Ltd., EGO1-55-1MR).
[0178] [Thickness of Separator and Porous Substrate] The thickness of the separator and porous substrate was measured at 20 points within a 10 cm square using a contact thickness meter (Mitutoyo Corporation, LITEMATIC VL-50S) and the average was calculated. A spherical probe with a sphere radius of 10 mm (Mitutoyo Corporation) was used as the measurement terminal, and the measurement was adjusted so that a load of 0.19 N was applied during measurement.
[0179] [Porous Layer Thickness] The thickness of the porous substrate was subtracted from the thickness of the flat membrane obtained by removing the adhesive layer from the separator. The thickness of the flat membrane was measured at 20 points within a 10 cm square using a contact thickness meter (Mitutoyo Corporation, LITEMATIC VL-50S) and the average was calculated. A spherical probe with a sphere radius of 10 mm (Mitutoyo Corporation) was used as the measurement terminal, and the measurement was adjusted so that a load of 0.19 N was applied during measurement.
[0180] [Weight per unit area of adhesive layer] The separator was cut into a piece of 20 cm x 20 cm, the mass of the layer portion corresponding to the adhesive layer was measured, and the mass was divided by the area to obtain the total weight per unit area of both sides (g / m 2 In all examples and comparative examples, the adhesive layer was formed in equal amounts on both sides of the separator, so the basis weight per side (g / m) was calculated by dividing half of the total basis weight on both sides. 2 )
[0181] [Average Primary Particle Size of Inorganic Particles] The inorganic particles used to form the porous layer were used as samples and observed with a scanning electron microscope (SEM) to determine the average primary particle size. Specifically, the major axes of 100 randomly selected inorganic particles were measured during SEM observation, and the average value of the major axes of the 100 particles was taken as the average primary particle size (μm).
[0182] [Average Primary Particle Size of Resin Particles] A dried sample of the resin particle dispersion liquid used to form the adhesive layer was observed under an SEM to determine the average primary particle size. Specifically, the major axes of 100 randomly selected resin particles were measured during the SEM observation, and the average of the major axes of the 100 particles was taken as the average primary particle size (μm).
[0183] [Glass Transition Temperature of Resin] Differential scanning calorimetry (DSC) was performed on a dried sample of the resin particle dispersion used to form the adhesive layer. A Q200 Differential Scanning Calorimeter (TA Instruments) was used as the DSC device, and the sample weight was 5 mg. The sample was heated from -65°C to 150°C at a heating rate of 10°C / min, quenched, and then heated again at the same heating rate to obtain a DSC curve. In the obtained DSC curve, the intersection point (1) between the low-temperature baseline and the tangent to the curve of the stepwise change portion, and the intersection point (2) between the high-temperature baseline and the tangent to the curve of the stepwise change portion were determined, and the temperature midway between the intersection points (1) and (2) was taken as the glass transition temperature (Tg, °C).
[0184] [Resin Composition] The monomer units contained in the resin constituting the adhesive layer were quantified by NMR. The dried resin particle dispersion used to form the adhesive layer was used as a sample. The sample was swollen with deuterated chloroform, and then measured at 600 MHz at room temperature using an NMR device (JNM-ECA600 manufactured by JEOL Ltd.) and a semi-solid probe (FGMAS probe manufactured by JEOL Ltd.). 1 H-NMR spectrum (MAS rotation speed 6 kHz, observation width 15 ppm, number of points 32 k, pulse repetition waiting time 4 seconds) was measured at 150 MHz. 13 The C-NMR spectrum was measured. 13 The C-NMR spectrum was accumulated approximately 33,000 times in quantitative mode (inverse gate decoupling method, MAS rotation speed 6 kHz, observation width 250 ppm, number of points 32 k, pulse repetition waiting time 12 seconds).
[0185] [Adhesion Strength] A test secondary battery, as described below, was prepared. A compression bending test (three-point bending measurement) was performed on the battery. The measurement was performed using a Tensilon (A&D Co., Ltd., STB-1225S) equipped with a compression bending test jig. The distance between the support stands was 4 cm, and the battery was placed on the support stand so that the short side of the battery was parallel to the long direction of the indenter and the compression position during measurement was at the center of the long direction of the electrode in the battery. The measurement was started by setting the displacement at 0 when the indenter was lowered until a load of 0.1 N was applied. The compression rate during measurement was 2 mm / min, and measurements were performed up to a displacement of 2 mm. The yield point load (N) in the load-displacement curve obtained from this result was taken as the adhesive strength. When the yield point load could not be observed, the maximum load (N) was taken as the adhesive strength. The results are shown in Table 3.
[0186] [Heat Resistance] A test secondary battery as described below was prepared. The battery was charged at a constant current and constant voltage of 0.2 C and 4.2 V at room temperature. The battery was then placed in an oven at a temperature of 150°C, and a weight of approximately 500 g was placed on the battery. After 60 minutes, the battery was removed from the oven and allowed to cool to room temperature. The battery voltage was measured, and a short circuit was judged to have occurred when it was 3.5 V or less. The number of short circuits out of five batteries was classified as follows. The results are shown in Table 3. A: 0 B: 1 to 2 C: 3 to 5
[0187] <Preparation of Separator and Battery> [Example 1] -Preparation of Separator- A mixed solvent of dimethylacetamide (DMAc) and tripropylene glycol (TPG) (DMAc:TPG = 80:20 [mass ratio]) was prepared. Meta-aramid (polymetaphenylene isophthalamide, Teijin, Conex) was dissolved in the mixed solvent to a resin concentration of 4 mass% to obtain a resin solution. Magnesium hydroxide particles (average primary particle size 0.8 μm) were added to the resin solution in an amount such that the magnesium hydroxide particles:meta-aramid ratio was 70:30 [mass ratio], and the mixture was stirred and mixed to obtain coating solution (1).
[0188] Resin particle dispersion (1) (dispersion medium: water, solid content concentration: 7% by mass) was prepared. The dried resin particle dispersion (1) was used as a sample, and the particle size of the resin particles, Tg of the resin, and composition of the resin were analyzed by SEM observation, DSC, and NMR. The results are shown in Table 2.
[0189] An appropriate amount of coating liquid (1) was placed on a pair of Mayer bars, and a polyethylene microporous membrane (thickness 9 μm, air permeability 95 sec / 100 mL) was passed between the Mayer bars to coat both sides with equal amounts of coating liquid (1). The membrane was immersed in a coagulation liquid (DMAc:TPG:water = 30:8:62 [mass ratio], liquid temperature 40°C) to solidify the coating layer, and then washed in a water washing tank at 40°C and dried. The membrane was then passed between a pair of bar coaters on which an appropriate amount of resin particle dispersion liquid (1) was placed, to coat both sides with equal amounts of resin particle dispersion liquid (1), and then dried. In this way, a separator was obtained in which a porous layer and an adhesive layer were formed on both sides of the polyethylene microporous membrane. When the obtained separator was observed with an SEM, the porous layer had a large number of micropores inside, a structure in which the micropores were connected, and a layer that allowed gas or liquid to pass from one side to the other.
[0190] - Preparation of Positive Electrode - 89.5 parts by mass of lithium cobalt oxide powder as the positive electrode active material, 4.5 parts by mass of acetylene black as the conductive additive, 6 parts by mass of polyvinylidene fluoride as the binder resin, and an appropriate amount of N-methyl-2-pyrrolidone were mixed by stirring in a twin-arm mixer to prepare a positive electrode slurry. The positive electrode slurry was applied to one or both sides of a 20 μm thick aluminum foil, dried, and pressed to obtain a positive electrode having a positive electrode active material layer on one or both sides.
[0191] - Preparation of Negative Electrode - 300 parts by mass of artificial graphite as the negative electrode active material, 7.5 parts by mass of an aqueous dispersion containing 40% by mass of a modified styrene-butadiene copolymer as the binder resin, 3 parts by mass of carboxymethyl cellulose as a thickener, and an appropriate amount of water were mixed by stirring using a twin-arm mixer to prepare a negative electrode slurry. The negative electrode slurry was applied to one or both sides of a 10 μm thick copper foil, dried, and pressed to obtain a negative electrode having a negative electrode active material layer on one or both sides.
[0192] - Preparation of battery for adhesive strength evaluation - The double-sided positive electrode and double-sided negative electrode were each cut into a rectangle of 30 mm x 70 mm. The separator was cut into a rectangle of TD 35 mm x MD 75 mm. These were stacked so that the positive and negative electrodes alternated and the separator was sandwiched between the positive and negative electrodes, to prepare a laminate consisting of three positive electrodes, three negative electrodes, and five separators. The laminate was inserted into a pack made of aluminum laminate film, and an electrolyte (1 mol / L LiPF 6 A mixture of ethylene carbonate and ethyl methyl carbonate (mass ratio 3:7) was poured into the laminate, allowing the electrolyte to soak into the laminate. The laminate was then heat-pressed (wet heat press) along the stacking direction of the pack using a heat press machine to bond the electrodes and separators. The heat press conditions were a press temperature of 60°C, a press pressure of 50 kPa, and a press time of 17 hours. The test secondary battery thus obtained was subjected to the aforementioned adhesive strength test.
[0193] - Preparation of battery for heat resistance evaluation - A single-sided positive electrode and a single-sided negative electrode were each cut into a rectangle of 14 mm x 20 mm. A separator was cut into a rectangle of 20 mm TD x 26 mm MD. These were stacked so that the positive electrode active material layer and the negative electrode active material layer faced each other and the separator was sandwiched between the positive electrode and the negative electrode to prepare a laminate consisting of one positive electrode, one negative electrode, and one separator. The laminate was inserted into a pack made of aluminum laminate film, and an electrolyte (1 mol / L LiPF 6 A mixture of ethylene carbonate and ethyl methyl carbonate (mass ratio 3:7) was poured into the laminate, allowing the electrolyte to soak into the laminate. The laminate was then heat-pressed (wet heat press) along the stacking direction of the pack using a heat press machine to bond the electrodes and separators. The heat press conditions were a press temperature of 60°C, a press pressure of 50 kPa, and a press time of 17 hours. The test secondary batteries thus obtained were subjected to the heat resistance evaluation described above.
[0194] [Example 2] Resin particle dispersion (2) (dispersion medium: water, solid content concentration: 7% by mass) was prepared. The dried resin particle dispersion (2) was used as a sample, and the particle size of the resin particles, Tg of the resin, and composition of the resin were analyzed by SEM observation, DSC, and NMR as described above. The results are shown in Table 2.
[0195] A separator was produced in the same manner as in Example 1, except that resin particle dispersion liquid (1) was replaced with resin particle dispersion liquid (2). The basis weight of the adhesive layer is as shown in Table 2. When the obtained separator was observed with an SEM, it was found that the porous layer had a large number of micropores therein, a structure in which the micropores were connected, and a layer through which gas or liquid could pass from one surface to the other.
[0196] Comparative Example 1: Resin particle dispersion (3) (dispersion medium: water, solid content concentration: 7% by mass) was prepared. The dried resin particle dispersion (3) was used as a sample, and the particle size of the resin particles, Tg of the resin, and composition of the resin were analyzed by SEM observation, DSC, and NMR. The results are shown in Table 2.
[0197] A separator was produced in the same manner as in Example 1, except that the resin particle dispersion liquid (1) was changed to the resin particle dispersion liquid (3). The basis weight of the adhesive layer is as shown in Table 2.
[0198] Comparative Example 2 A separator was produced in the same manner as in Example 1, except that the resin particle dispersion (1) was changed to a liquid butadiene-acrylonitrile copolymer (hereinafter referred to as liquid NBR). The basis weight of the adhesive layer is as shown in Table 2.
[0199] Comparative Example 3 A separator was produced in the same manner as in Example 1, except that the resin particle dispersion (1) was replaced with a mixture of the resin particle dispersion (1) and liquid NBR. The mixing ratio was 15:85 (mass ratio) of solids in the resin particle dispersion (1) to the liquid NBR. The resin particles in the resin particle dispersion (1) and the liquid NBR separated, and an adhesive layer could not be formed. In this example, the glass transition temperature was not measured. The particle diameters of the resin particles listed in Table 2 are measured values for the resin particle dispersion (1). The types and amounts of the monomer units listed in Table 2 are based on the measurement results for the resin particle dispersion (1) and the liquid NBR.
[0200] Example 3 A separator was produced in the same manner as in Example 1, except that the magnesium hydroxide particles were replaced with barium sulfate particles (average primary particle size 0.03 μm). The composition of the porous layer and the basis weight of the adhesive layer are as shown in Tables 1 and 2. When the obtained separator was observed with an SEM, it was found that the porous layer had a large number of micropores therein, a structure in which the micropores were connected, and a layer through which gas or liquid could pass from one surface to the other.
[0201] Comparative Example 4 A separator was produced in the same manner as in Example 3, except that resin particle dispersion (1) was changed to resin particle dispersion (3). The composition of the porous layer and the basis weight of the adhesive layer are as shown in Tables 1 and 2.
[0202] [Example 4] A separator was produced in the same manner as in Example 1, except that the meta-aramid was replaced with an acrylic resin and the magnesium hydroxide particles were replaced with alumina particles (average primary particle size 1.0 μm). The composition of the porous layer and the basis weight of the adhesive layer are as shown in Tables 1 and 2. When the obtained separator was observed with an SEM, it was found that the porous layer had a large number of micropores therein, a structure in which the micropores were connected, and a layer through which gas or liquid could pass from one surface to the other.
[0203] Comparative Example 5 A separator was produced in the same manner as in Example 4, except that resin particle dispersion (1) was changed to resin particle dispersion (3). The composition of the porous layer and the basis weight of the adhesive layer are as shown in Tables 1 and 2.
[0204] [Example 5] A separator was produced in the same manner as in Example 1, except that the meta-aramid was replaced with an acrylic resin and the magnesium hydroxide particles were replaced with boehmite particles (average primary particle size 1.0 μm). The composition of the porous layer and the basis weight of the adhesive layer are as shown in Tables 1 and 2. When the obtained separator was observed with an SEM, it was found that the porous layer had a large number of micropores therein, a structure in which the micropores were connected, and a layer through which gas or liquid could pass from one surface to the other.
[0205] The acrylic resin used to form the porous layer in Example 4, Comparative Example 5, and Example 5 was an n-butyl methacrylate / acrylonitrile copolymer.
[0206] The abbreviations in Tables 1 and 2 have the following meanings: PE: polyethylene St: styrene MMA: methyl methacrylate BMA: n-butyl methacrylate EHMA: 2-ethylhexyl methacrylate Bt: butadiene AN: acrylonitrile
[0207]
[0208]
[0209]
[0210] All publications, patent applications, and technical standards mentioned in this specification are herein incorporated by reference to the same extent as if each individual publication, patent application, or technical standard was specifically and individually indicated to be incorporated by reference.
[0211] The disclosure of Japanese Application No. 2023-028672, filed on February 27, 2023, is incorporated herein by reference in its entirety.
[0212] 101, 102, 103, 104, 105, 106, 107 Separator 20 Porous substrate 30 Porous layer 40 Laminate 50 Adhesive layer 52 Resin particles
Claims
1. A non-aqueous secondary battery separator comprising: a porous layer containing inorganic particles and a binder resin; and an adhesive layer containing a phenyl group-containing acrylic resin and a butadiene-acrylonitrile resin, the amount of butadiene units being 3 mol % to 50 mol % of the total amount of acrylic units, styrene units, butadiene units and acrylonitrile units contained in both resins.
2. The separator for a non-aqueous secondary battery according to claim 1, further comprising a porous substrate, the porous layer being provided on one or both sides of the porous substrate, and the adhesive layer being provided on one or both sides of a laminate of the porous substrate and the porous layer.
3. The separator for a non-aqueous secondary battery according to claim 1, wherein the adhesive layer contains resin particles, and the resin particles contain at least one of a phenyl group-containing acrylic resin and a butadiene-acrylonitrile resin.
4. The separator for a non-aqueous secondary battery according to claim 3, wherein the average primary particle size of all the resin particles contained in said adhesive layer is 0.1 μm to 1.0 μm.
5. The separator for a non-aqueous secondary battery according to claim 1, wherein the mass ratio of the phenyl group-containing acrylic resin to the butadiene-acrylonitrile resin contained in the adhesive layer is 60:40 to 95:
5.
6. The separator for a non-aqueous secondary battery according to claim 1, wherein the phenyl group-containing acrylic resin has a styrene unit and an acrylic unit, and a molar ratio of the styrene unit to the acrylic unit is 30:70 to 50:
50.
7. The separator for a non-aqueous secondary battery according to claim 1, wherein the glass transition temperature of the entire resin contained in said adhesive layer is 58°C to 100°C.
8. The adhesive layer has a basis weight of 0.05 g / m on one side of the nonaqueous secondary battery separator. 2 ~1.0g / m 2 The separator for a non-aqueous secondary battery according to claim 1 , 9. The separator for a nonaqueous secondary battery according to claim 1, wherein the average primary particle size of all the inorganic particles contained in said porous layer is 0.01 μm to 1.0 μm.
10. The separator for a nonaqueous secondary battery according to claim 1, wherein the binder resin comprises at least one resin selected from the group consisting of polyamide resins, acrylic resins, fluorine resins, and styrene-butadiene resins.
11. A non-aqueous secondary battery comprising: a positive electrode; a negative electrode; and the separator for a non-aqueous secondary battery according to any one of claims 1 to 10, which is disposed between the positive electrode and the negative electrode; and which obtains an electromotive force by doping and dedoping lithium ions.