Chloroprene-based polymer latex composition, and dip-molded body
Patent Information
- Application Number
- MYPI2025004707
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-02-20
- Filing Date
- 2024-02-15
- Publication Date
- 2024-08-20
AI Technical Summary
Conventional chloroprene-based polymer latex compositions struggle to achieve a balance between flexibility and tensile strength in dip-molded products, making it difficult to produce articles with both excellent flexibility and mechanical properties similar to those made from natural rubber or polyisoprene.
A chloroprene-based polymer latex composition is developed, incorporating chloroprene polymer latex, metal oxide, vulcanization accelerator, sulfur, and a heteroaromatic ring compound, with specific ratios and processing conditions to achieve a toluene-insoluble content of 50-95% and weight average molecular weights of 5,000 to 80,000, enhancing the tensile strength and flexibility of dip-molded products.
The composition results in dip-molded articles with improved flexibility and tensile strength, suitable for applications such as industrial and medical gloves, balloons, and catheters, offering a balance of mechanical properties and wearing comfort.
Abstract
Description
Chloroprene polymer latex composition and dip-molded product
[0001] The present invention relates to a chloroprene polymer latex composition and a dip-molded article.
[0002] Chloroprene-based polymers are known as materials for dip-molded products such as medical surgical gloves, medical examination gloves, industrial gloves, balloons, catheters, and rubber boots.
[0003] Various technologies have been proposed for chloroprene polymers for use in dip-molded products. Patent Document 1 describes, with respect to vibration-proof rubber applications, that mixing a low-molecular-weight chloroprene polymer with a number-average molecular weight in the range of 500 to 50,000 improves damping performance. Patent Document 2 describes, with respect to dip-molded product applications, a polychloroprene latex with a pH of 7 to 14, containing 100 parts by mass of modified polychloroprene obtained by copolymerizing chloroprene and methacrylic acid, 90 to 150 parts by mass of water, 1 to 5 parts by mass of an emulsifier, and 0.5 to 2.5 parts by mass of potassium ions. Patent Document 3, relating to applications to dip-molded products, describes a mercaptan-modified polychloroprene latex obtained by copolymerizing chloroprene and 2,3-dichloro-1,3-butadiene, in which, in the C-solid-state NMR spectrum of the polychloroprene, the peak area (A) at 126.2 to 127.6 ppm, the peak area (B) at 122.0 to 126.2 ppm, and the peak area (C) at 129.9 to 130.3 ppm are within the ranges represented by the following general formula (I): Patent Document 4, relating to applications to dip-molded products, describes a chloroprene polymer latex that contains high-molecular-weight and low-molecular-weight components, thereby enabling the vulcanized rubber produced by dip molding to have both excellent flexibility and mechanical properties.
[0004]
[0005] Japanese Patent Laid-Open No. 7-292165 Japanese Patent Laid-Open No. 2014-114342 International Publication No. 2019 / 009038 Japanese Patent Laid-Open No. 2019-143002
[0006] Dip-molded articles using chloroprene polymers are required to have high flexibility, similar to dip-molded articles obtained using natural rubber or polyisoprene, and also tend to require high mechanical properties. Improved flexibility is also related to improvements in wearing comfort and texture of the coating. Therefore, a chloroprene polymer latex composition capable of producing dip-molded articles having excellent flexibility and tensile strength at break has been desired.
[0007] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a chloroprene polymer latex composition from which a dip-molded article having excellent flexibility and tensile strength at break can be obtained, which has been difficult to achieve with conventional chloroprene polymer latex compositions.
[0008] Various embodiments of the present invention will be described below as examples, and the embodiments shown below can be combined with each other.
[0009] [1] A chloroprene polymer latex composition comprising a chloroprene polymer latex (A), a metal oxide (B), a vulcanization accelerator (C), sulfur (D), and a heteroaromatic ring compound (E), wherein the chloroprene polymer rubber obtained by freeze-drying the chloroprene polymer latex (A) has a toluene-insoluble content of 50 to 95 mass %, and the chloroprene polymer latex composition contains the metal oxide (B) in an amount of 50 to 95 mass % relative to 100 parts by mass of the solid content of the chloroprene polymer latex (A). 0.3 to 15.0 parts by mass of the vulcanization accelerator (C), 0.02 to 1.50 parts by mass of the sulfur (D), and 0.1 to 10.0 parts by mass of the heteroaromatic ring compound (E), wherein the vulcanization accelerator (C) contains at least one of a thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthogenate-based, and thiazole-based vulcanization accelerator, and the heteroaromatic ring compound (E) is represented by chemical formula (1). (X in the chemical formula (1) represents a hydrogen atom or a metal atom. R 1 ~R 4R represents a hydrogen atom, an alkyl group which may have a substituent, an ether group which may have a substituent, a nitro group, an amino group, or a carboxyl group. 1 ~R 4 and may be the same or different.) [2] The chloroprene polymer latex composition according to [1], containing 0.5 to 10.0 parts by mass of an antioxidant per 100 parts by mass of the solids content of the chloroprene polymer latex (A). [3] The chloroprene polymer latex composition according to [1] or [2], wherein a molecular weight distribution obtained by measuring a tetrahydrofuran-soluble content in the chloroprene polymer latex (A) by gel permeation chromatography has a peak corresponding to a weight average molecular weight of 5,000 to 80,000. [4] The chloroprene polymer latex composition according to any one of [1] to [3], wherein a ratio RB / RA of the total amount RB of peak areas of abietic acid, neoabietic acid, palustric acid, levopimaric acid and salts thereof to the total amount RA of peak areas of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid and salts thereof is 0.10 or more, as determined by gas chromatography of an extract obtained by molding the chloroprene polymer latex composition by a dip coagulation method and drying the resulting product at 140°C for 60 minutes with an ethanol / toluene azeotrope as specified in JIS K 6229. [5] The chloroprene polymer latex composition according to any one of [1] to [4], wherein the dip-molded product obtained by molding the chloroprene polymer latex composition by a dip coagulation method and heating and drying at 140°C for 60 minutes has a modulus at 100% elongation of 0.65 MPa or less and a tensile strength at break of 19.0 MPa or more, as measured in accordance with JIS K 6251. [6] A dip-molded product of the chloroprene polymer latex composition according to any one of [1] to [5]. [7] The dip-molded product according to [6], which is an industrial / general household glove, a medical glove, a balloon, a catheter, or a boot.
[0010] The chloroprene polymer latex composition according to the present invention can provide a dip-molded article having excellent flexibility and tensile strength at break. Furthermore, the obtained dip-molded article can be used as various materials that require flexibility, tensile strength at break, etc., by taking advantage of its properties. Specifically, the dip-molded article can be used as industrial or general household gloves, medical gloves, balloons, catheters, or boots.
[0011] The present invention will be described in detail below by illustrating embodiments of the present invention. The present invention is not limited by these descriptions. The features of the embodiments of the present invention described below can be combined with each other. Furthermore, each feature can be an invention independently.
[0012] 1. Chloroprene Polymer Latex Composition The chloroprene polymer latex composition according to the present invention contains a chloroprene polymer latex (A), a metal oxide (B), a vulcanization accelerator (C), sulfur (D), and a heteroaromatic ring compound (E). Components that may be contained in the chloroprene polymer latex composition according to the present invention will be described below.
[0013] 1.1 Chloroprene Polymer Latex (A) The chloroprene polymer latex (A) according to the present invention contains a chloroprene polymer. The chloroprene polymer according to the present invention means a polymer containing monomer units derived from 2-chloro-1,3-butadiene (hereinafter also referred to as chloroprene).
[0014] <Monomer Units That May Be Included in Chloroprene-Based Polymer> The chloroprene-based polymer according to one embodiment of the present invention may be a copolymer of chloroprene and another monomer that is copolymerizable with chloroprene. Examples of the other monomer include 1-chloro-1,3-butadiene, 2,3-dichloro-1,3-butadiene, isoprene, styrene, methacrylic acid, acrylonitrile, and sulfur. As the other monomer, one of these may be used, or two or more of these may be used in combination.
[0015] A chloroprene-based polymer according to one embodiment of the present invention preferably contains chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units. The chloroprene-based polymer according to one embodiment of the present invention preferably contains 0 to 30% by mass of 2,3-dichloro-1,3-butadiene monomer units, more preferably 8 to 20% by mass, and still more preferably 10 to 17% by mass, relative to 100% by mass of the total of the chloroprene monomer units and the 2,3-dichloro-1,3-butadiene monomer units. The content of the 2,3-dichloro-1,3-butadiene monomer unit is, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or 30% by mass, and may be within a range between any two of the numerical values exemplified here.
[0016] The chloroprene polymer latex (A) according to one embodiment of the present invention may contain 70 to 100% by mass of chloroprene monomer units relative to 100% by mass of the chloroprene polymer contained in the chloroprene polymer latex (A). The content of the chloroprene monomer units may be, for example, 70, 75, 80, 85, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, or 100% by mass, or may be within a range between any two of the values exemplified here.
[0017] The chloroprene polymer latex (A) according to one embodiment of the present invention may contain 0 to 30% by mass of other monomer units than chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units, relative to 100% by mass of the chloroprene polymer contained in the chloroprene polymer latex (A). The content of the other monomer units may be, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or 30% by mass, or may be within a range between any two of the values exemplified here. The chloroprene polymer according to one embodiment of the present invention may be composed of chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units.
[0018] In addition, when the chloroprene polymer latex (A) according to one embodiment of the present invention contains two or more different chloroprene polymers or is a mixture of two or more different chloroprene polymer latexes, the content of each monomer unit means the total amount of each monomer unit in all chloroprene polymers contained in the chloroprene polymer latex (A).
[0019] <Toluene-insoluble content> The chloroprene polymer latex (A) according to the present invention has a toluene-insoluble content of 50 to 95 mass%. The chloroprene polymer latex (A) according to one embodiment of the present invention more preferably has a toluene-insoluble content of 55 to 85 mass%. The toluene-insoluble content is, for example, 50, 55, 60, 65, 70, 75, 80, 85, 90, or 95 mass%, and may be within a range between any two of the values exemplified here.
[0020] The toluene-insoluble content can be calculated by the following formula, specifically by the method described in the Examples: toluene-insoluble content (gel content) = B / A × 100 (%), where Ag is the chloroprene polymer rubber obtained by freeze-drying a chloroprene polymer latex, and Bg is the gel content (insoluble content) separated from the toluene-dissolved mixture.
[0021] The toluene-insoluble content can be controlled by adjusting the production conditions of the chloroprene polymer rubber, for example, the polymerization formulation (formulation such as the type and amount of a chain transfer agent, polymerization temperature, polymerization time, polymerization conversion rate, etc.) contained in the chloroprene polymer latex (A), and by adjusting the type and amount of the polymer blended.
[0022] <Weight Average Molecular Weight> The chloroprene polymer latex (A) according to one embodiment of the present invention can have a peak at a weight average molecular weight of 200,000 to 1,500,000 in the molecular weight distribution obtained by measuring the tetrahydrofuran soluble matter in the chloroprene polymer latex (A) by gel permeation chromatography. Moreover, the chloroprene polymer latex (A) according to one embodiment of the present invention preferably has a peak at a weight average molecular weight of 5,000 to 80,000 in the molecular weight distribution obtained by measuring the tetrahydrofuran soluble matter in the chloroprene polymer latex (A) by gel permeation chromatography. Regarding the chloroprene polymer latex (A) according to one embodiment of the present invention, it is preferred that a peak corresponding to a weight average molecular weight of 200,000 to 1,500,000 and / or a peak corresponding to a weight average molecular weight of 5,000 to 80,000 is detected in a molecular weight distribution obtained by mixing the chloroprene polymer latex (A) with a large amount of methanol, precipitating, filtering, and drying the obtained chloroprene polymer, dissolving the obtained chloroprene polymer in tetrahydrofuran, and measuring the obtained sample by gel permeation chromatography.
[0023] Furthermore, in the chloroprene polymer latex (A) according to one embodiment of the present invention, the chloroprene polymer latex (A) is mixed with a large amount of methanol, precipitated, filtered, and dried. The resulting chloroprene polymer is dissolved in tetrahydrofuran to obtain a sample, and the resulting sample is subjected to gel permeation chromatography. In the molecular weight distribution obtained, a peak corresponding to a weight average molecular weight of 200,000 to 1,500,000 is preferably detected, and more preferably a peak corresponding to a weight average molecular weight of 5,000 to 80,000 is preferably detected. In the molecular weight distribution, a peak corresponding to a weight average molecular weight of 300,000 to 1,500,000 is preferably detected, and more preferably a peak corresponding to a weight average molecular weight of 5,000 to 50,000 is preferably detected. In the molecular weight distribution, a peak corresponding to a weight average molecular weight of 500,000 to 1,500,000 is preferably detected, and more preferably a peak corresponding to a weight average molecular weight of 8,000 to 30,000 is preferably detected.
[0024] The chloroprene polymer latex (A) according to one embodiment of the present invention may contain two or more polymers having different weight-average molecular weights, namely, a chloroprene polymer α and a chloroprene polymer β. The monomer units that the chloroprene polymer α and the chloroprene polymer β may contain and the amounts thereof are as described above for the monomer units that the chloroprene polymer may contain. The chloroprene polymer α according to one embodiment of the present invention may have a weight-average molecular weight different from that of the chloroprene polymer β. The difference between the weight-average molecular weight of the chloroprene polymer α according to one embodiment of the present invention and the weight-average molecular weight of the chloroprene polymer β is preferably 100,000 or more, more preferably 400,000 or more. The difference between the weight-average molecular weight of the chloroprene polymer α and the weight-average molecular weight of the chloroprene polymer β described below is, for example, 100,000, 200,000, 300,000, 400,000, 500,000, 600,000, 700,000, 800,000, 900,000, 1,000,000, 1,200,000, 1,300,000, 1,400,000, or 1,500,000, and may be within a range between any two of the numerical values exemplified here.
[0025] For example, the weight-average molecular weight of the chloroprene polymer α can be smaller than the molecular weight of the chloroprene polymer β. The weight-average molecular weight of the chloroprene polymer α can be 5,000 to 80,000. The weight-average molecular weight of the chloroprene polymer α can be, for example, 5,000, 6,000, 7,000, 8,000, 9,000, 10,000, 11,000, 12,000, 13,000, 14,000, 15,000, 16,000, 17,000, 18,000, 19,000, 20,000, or 21,000. , 22,000, 23,000, 24,000, 25,000, 26,000, 27,000, 28,000, 29,000, 30,000, 35,000, 40,000, 50,000, 60,000, 70,000, 80,000, and may be within a range between any two of the numerical values exemplified here.
[0026] For example, the weight-average molecular weight of the chloroprene polymer β can be greater than the molecular weight of the chloroprene polymer α. The weight-average molecular weight of the chloroprene polymer β can be 200,000 to 1,500,000. The weight-average molecular weight of the chloroprene polymer α can be, for example, 200,000, 300,000, 400,000, 500,000, 600,000, 700,000, 800,000, 900,000, 1,000,000, 1,100,000, 1,200,000, 1,300,000, 1,400,000, or 1,500,000, or can be within a range between any two of the values exemplified here.
[0027] The chloroprene polymer latex (A) according to one embodiment of the present invention preferably contains 5 to 40% by mass of the chloroprene polymer α, relative to 100% by mass of the polymers contained in the chloroprene polymer latex (A). The content of the chloroprene polymer α may be, for example, 5, 10, 15, 20, 25, 30, 35, or 40% by mass, and may be within a range between any two of the values exemplified here.
[0028] The chloroprene polymer latex (A) according to one embodiment of the present invention preferably contains 60 to 95% by mass of the chloroprene polymer β, relative to 100% by mass of the polymer contained in the chloroprene polymer latex (A). The content of the chloroprene polymer β is, for example, 60, 65, 70, 75, 80, 85, 90, or 95% by mass, and may be within a range between any two of the values exemplified here.
[0029] The weight-average molecular weight can be determined, for example, by mixing the chloroprene polymer latex (A) with a large amount of methanol, precipitating, filtering, and drying the resulting chloroprene polymer, dissolving the resulting chloroprene polymer in tetrahydrofuran, and analyzing the resulting sample using gel permeation chromatography (GPC). The GPC measurement conditions can be as described in the Examples. The weight-average molecular weight can be controlled by adjusting the production conditions, specifically, the polymerization formulation of the chloroprene polymer (formulation such as the type and amount of chain transfer agent, polymerization temperature, polymerization time, polymerization conversion rate, etc.).
[0030] 1.2 Method for Producing Chloroprene Polymer Latex (A) The method for producing the chloroprene polymer latex (A) according to the present invention is not particularly limited, and the chloroprene polymer latex (A) can be obtained, for example, by the following method. The method for producing the chloroprene polymer latex (A) according to the first embodiment of the present invention may include a polymerization step of polymerizing raw material monomers containing chloroprene to obtain a chloroprene polymer latex, and the obtained chloroprene polymer latex can be used as the chloroprene polymer latex (A) as is. The method for producing the chloroprene polymer latex (A) according to the second embodiment of the present invention may include a polymerization step of polymerizing raw material monomers containing chloroprene to obtain a chloroprene polymer latex, and a mixing step of mixing two or more types of latexes to obtain the chloroprene polymer latex (A). The method for producing the chloroprene polymer latex (A) according to the third embodiment of the present invention may include: a first polymerization step of polymerizing a chloroprene polymer α by polymerizing a raw material monomer containing chloroprene, and a second polymerization step of polymerizing a chloroprene polymer β in the presence of the chloroprene polymer α; or a first polymerization step of polymerizing a chloroprene polymer β by polymerizing a raw material monomer containing chloroprene, and a second polymerization step of polymerizing the chloroprene polymer α in the presence of the chloroprene polymer β.
[0031]
[0023] Hereinafter, a method for producing the chloroprene polymer latex (A) according to the first embodiment of the present invention will be described. The method for producing the chloroprene polymer latex (A) according to the first embodiment of the present invention may include a polymerization step of polymerizing raw material monomers containing chloroprene to obtain the chloroprene polymer latex.
[0032] In the polymerization step, the raw material monomers include chloroprene and may also include other monomers copolymerizable with chloroprene. The other monomers copolymerizable with chloroprene are as described above. The type and amount of each monomer charged are preferably adjusted so that the type and content of each monomer unit in the resulting polymer fall within the above-described numerical ranges. For example, the copolymerization amount of 2,3-dichloro-1,3-butadiene in the chloroprene polymer contained in the chloroprene polymer latex may be in the range of 0 to 30% by mass relative to 100% by mass of the total of the chloroprene monomer and 2,3-dichloro-1,3-butadiene contained in the chloroprene polymer. In this case, the amount of 2,3-dichloro-1,3-butadiene charged before the start of emulsion polymerization is preferably in the range of 0 to 30 parts by mass relative to 100 parts by mass of the total of the chloroprene monomer and 2,3-dichloro-1,3-butadiene monomer. From the viewpoint of controlling the polymerization, it is more preferable to set the amount of 2,3-dichloro-1,3-butadiene charged to 5 to 25 parts by mass per 100 parts by mass of the total of the chloroprene monomer and the 2,3-dichloro-1,3-butadiene monomer.
[0033] When producing a chloroprene polymer, raw material monomers can be polymerized by a polymerization method such as emulsion polymerization, solution polymerization, suspension polymerization, bulk polymerization, etc. Among these polymerization methods, emulsion polymerization is preferred because it has various advantages such as ease of control, ease of extracting the polymer from a polymerization-finished liquid, and a relatively fast polymerization rate.
[0034] Emulsion polymerization is a type of radical polymerization, in which raw material monomers are charged into a reaction vessel together with a chain transfer agent, water, an alkali (e.g., a metal hydroxide such as potassium hydroxide or sodium hydroxide), an emulsifier (dispersant), a reducing agent (e.g., sodium hydrogen sulfite), a polymerization initiator, and the like, to polymerize them.
[0035] The type of chain transfer agent used in the emulsion polymerization is not particularly limited, and known chain transfer agents generally used in the emulsion polymerization of chloroprene can be used, such as long-chain alkyl mercaptans such as n-dodecyl mercaptan and tert-dodecyl mercaptan, dialkyl xanthogen disulfides such as diisopropyl xanthogen disulfide and diethyl xanthogen disulfide, iodoform, etc. As the chain transfer agent, long-chain alkyl mercaptans are preferred, and n-dodecyl mercaptan is more preferred.
[0036] By adjusting the type and amount of the chain transfer agent, the weight average molecular weight of the resulting chloroprene polymer latex can be adjusted.
[0037] For example, to obtain a chloroprene polymer latex containing a chloroprene polymer β having a weight-average molecular weight of 200,000 to 1,500,000, the amount of chain transfer agent added before the start of emulsion polymerization is preferably 0.01 parts by mass or more per 100 parts by mass of raw material monomers (e.g., 100 parts by mass of chloroprene and 2,3-dichloro-1,3-butadiene in total). From the viewpoint of obtaining a chloroprene polymer latex containing a chloroprene polymer β having a weight-average molecular weight of 200,000 to 1,500,000, the amount of chain transfer agent added is more preferably 0.02 to 0.05 parts by mass, and may be, for example, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09 parts by mass, or less than 0.10 parts by mass, or may be within a range between any two of the values exemplified herein. When the amount of the chain transfer agent, particularly long-chain alkyl mercaptans, added is 0.01 parts by mass or more, the storage stability of the latex is further improved. When the amount is less than 0.10 parts by mass, particularly less than 0.05 parts by mass, the toluene-insoluble matter increases, and the tensile strength at break of the obtained dip-molded product containing the chloroprene polymer latex is further increased.
[0038] As another example, to obtain a chloroprene polymer latex containing a chloroprene polymer α having a peak in the molecular weight distribution exhibiting a weight-average molecular weight of 5,000 to 80,000, the amount of the chain transfer agent added before the start of emulsion polymerization is preferably 1.0 to 10.0 parts by mass per 100 parts by mass of the monomer. In this case, the amount of the chain transfer agent added may be, for example, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, or 10.0 parts by mass, or may be within a range between any two of the values exemplified here.
[0039] In the method for producing the chloroprene polymer latex (A) according to the first embodiment of the present invention, the chloroprene polymer latex obtained in the polymerization step can be used as the chloroprene polymer latex (A) as it is. In this case, it is preferable to obtain a chloroprene polymer latex containing a chloroprene polymer β having a weight-average molecular weight of 200,000 to 1,500,000 in the polymerization step.
[0040] The emulsifier preferably contains rosin acid and / or a rosin acid salt. Examples of rosin acid salts include alkali metal salts such as sodium salts and potassium salts. The amount of rosin acid and rosin acid salt added can be 3.0 to 7.0 parts by mass per 100 parts by mass of the raw material monomer used. The amount of rosin acid and rosin acid salt added can be, for example, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, or 7.0 parts by mass, or can be within a range between any two of the values exemplified here. The use of rosin acids can prevent aggregation of rubber solids and pH fluctuations when blended with the base latex.
[0041] The rosin acid and / or rosin acid salt may contain a conjugated resin acid component and a non-conjugated resin acid component. Examples of the conjugated resin acid component include abietic acid, neoabietic acid, palustric acid, levopimaric acid, and salts thereof. Examples of the non-conjugated resin acid component include dehydroabietic acid, pimaric acid, isopimaric acid, dihydropimaric acid, dihydroabietic acid, and salts thereof.
[0042] The rosin acid and rosin acid salts used in the emulsion polymerization step may have a ratio RB / RA of 0.10 or more and 0.70 or less, where RB is the total peak area of abietic acid, neoabietic acid, palustric acid, levopimaric acid, and their salts relative to RA, the total peak area of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid, and their salts, as determined by gas chromatography analysis of an extract extracted with an ethanol / toluene azeotrope as specified in JIS K 6229. The RB / RA of the rosin acid and rosin acid salt may be, for example, 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, or 0.70, or may be within a range between any two of the values exemplified here. The RB / RA of the dip-molded product of the resulting chloroprene polymer latex composition can be adjusted by adjusting the type and amount of the rosin acid and / or rosin acid salt.
[0043] The emulsifier may also include emulsifiers and dispersants other than rosin acid and rosin acid salts. Examples of emulsifiers and dispersants other than rosin acid and rosin acid salts include cationic, anionic, and nonionic emulsifiers and dispersants. In one embodiment of the present invention, the emulsifier used in the emulsion polymerization process may include rosin acid and / or rosin acid salts, and an anionic emulsifier or dispersant. As anionic emulsifiers and dispersants, sulfate- or sulfonate-based anionic emulsifiers and dispersants are preferably used in combination to stabilize the chloroprene polymer latex when a pH adjuster is added. Specific examples include alkyl sulfonates having 8 to 20 carbon atoms, alkyl aryl sulfates, condensates of sodium β-naphthalene sulfonate and formaldehyde, and sodium alkyl diphenyl ether disulfonates. The amount of anionic emulsifier or dispersant added may be 0.05 to 5 parts by mass per 100 parts by mass of the raw material monomers. The amount of anionic emulsifier or dispersant added is, for example, 0.05, 0.1, 0.2, 0.3, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, or 5.0 parts by mass relative to 100 parts by mass of the raw material monomer, and may be within a range between any two of the numerical values exemplified here.
[0044] The pH of the aqueous emulsion at the start of emulsion polymerization is preferably 10.5 to 13.5. The aqueous emulsion refers to a mixed solution of a chain transfer agent and a monomer (chloroprene, 2,3-dichloro-1,3-butadiene, etc.) immediately before the start of emulsion polymerization, but also includes cases where the composition changes due to the subsequent addition or divided addition of each component. When the pH of the aqueous emulsion at the start of emulsion polymerization is 10.5 or higher, the polymerization reaction can be controlled more stably. When the pH is 13.5 or lower, excessive viscosity increase during polymerization is suppressed, and the polymerization reaction can be controlled more stably.
[0045] The polymerization temperature for emulsion polymerization is preferably within the range of 5 to 55° C. A temperature of 5° C. or higher is preferred because the emulsion does not freeze, and a temperature of 55° C. or lower is preferred because the chloroprene monomer does not evaporate or boil.
[0046] As the polymerization initiator, potassium persulfate, benzoyl peroxide, ammonium persulfate, hydrogen peroxide, etc., which are used in ordinary radical polymerization, can be used.
[0047] The polymerization conversion rate is preferably in the range of 50 to 95%. The polymerization reaction is terminated by adding a polymerization terminator. If the polymerization conversion rate is 50% or higher, the toluene-insoluble content tends to increase, and the tensile strength at break of the resulting dip-molded article tends to be high. This is also advantageous from the viewpoint of production costs. If the polymerization conversion rate is less than 95%, it is possible to avoid a decrease in polymerization reactivity due to a decrease in unreacted monomer, and thus a decrease in productivity.
[0048] Examples of the polymerization terminator include diethylhydroxylamine, thiodiphenylamine, 4-tert-butylcatechol, 2,2'-methylenebis-4-methyl-6-tert-butylphenol, etc. After the emulsion polymerization is completed, unreacted monomers can be removed by a conventional method such as vacuum distillation.
[0049] Furthermore, to the chloroprene polymer latex obtained by the production method according to one embodiment of the present invention, after polymerization, any additive such as a freeze stabilizer, an emulsion stabilizer, a viscosity modifier, an antioxidant, or a preservative may be added, as long as the effects of the present invention are not impaired.
[0050] As an example, in the polymerization step, all of the raw material monomers and chemicals to be used in the polymerization step can be charged into a polymerization vessel before the start of polymerization, and then the polymerization can be started, or at least a portion of the raw material monomers and / or chemicals to be used in the polymerization step can be charged into a polymerization vessel before the start of polymerization, and the remainder can be added in portions after the start of polymerization.
[0051] In the polymerization step, when at least a portion of the raw material monomers and chemicals are charged into a polymerization vessel before the initiation of polymerization, and the remaining raw material monomers and / or chemicals are added after the initiation of polymerization, the remaining raw material monomers and / or chemicals can be added in one or more divided portions, or can be added continuously at a constant flow rate. In one embodiment of the present invention, at least a portion of the raw material monomers can be added in divided portions after the initiation of polymerization. For example, when chloroprene and 2,3-dichloro-1,3-butadiene are used as raw material monomers, a portion of the chloroprene can be added in divided portions after the initiation of polymerization.
[0052] For example, the portionwise addition of the remaining raw material monomers and / or agents can be started when the polymerization rate of the raw material monomers charged before the start of polymerization reaches 50 to 95%. The polymerization rate at which portionwise addition starts can be, for example, 50, 55, 60, 65, 70, 75, 80, 85, 90, or 95%, and may be within a range between any two of the values exemplified here.
[0053] When at least a portion of the raw material monomer is added after the initiation of polymerization, 50 parts by mass or less of 100 parts by mass of all raw material monomers used in the polymerization step can be added after the initiation of polymerization. In this case, the amount of raw material monomer added after the initiation of polymerization can be, for example, 0, 5, 10, 15, 20, 25, 30, 35, 40, 45, or 50 parts by mass, or may be within a range between any two of the values exemplified here. As an example, the raw material monomer, for example, chloroprene, can be added portionwise continuously over a period of 30 to 300 minutes.
[0054] The method for producing the chloroprene polymer latex (A) according to the second embodiment of the present invention will be described below. The method for producing the chloroprene polymer latex (A) according to the second embodiment of the present invention may include a polymerization step and a mixing step.
[0055] The method for producing a chloroprene polymer latex (A) according to the second embodiment of the present invention can include a polymerization step of polymerizing a raw material monomer containing chloroprene to obtain a chloroprene polymer latex. The polymerization step can include a polymerization step of polymerizing a raw material monomer containing chloroprene to obtain a latex containing a chloroprene polymer α, and a polymerization step of polymerizing a raw material monomer containing chloroprene to obtain a latex containing a chloroprene polymer β. In the polymerization step, it is preferable to adjust the amount of a chain transfer agent, etc., depending on the target weight-average molecular weight. The types, amounts used, polymerization conditions, etc. of each agent in the polymerization step of the second embodiment can be the same as those described for the polymerization step of the first embodiment.
[0056] The method for producing a chloroprene polymer latex (A) according to the second embodiment of the present invention may include a mixing step of mixing two or more types of latexes to obtain the chloroprene polymer latex (A). In the mixing step, a latex containing a chloroprene polymer α having a weight-average molecular weight of 5,000 to 80,000 and a latex containing a chloroprene polymer β having a weight-average molecular weight of 200,000 to 1,500,000 are mixed to obtain the chloroprene polymer latex (A). In the mixing step, two or more types of chloroprene polymer latexes may be mixed by a known method. In the mixing step, the chloroprene polymer latex (A) may be obtained by stirring and mixing using a paddle blade at 30 to 300 rpm for 20 seconds to 3 minutes, e.g., at 100 rpm for 1 minute.
[0057] A method for producing the chloroprene polymer latex (A) according to the third embodiment of the present invention will be described below. The method for producing the chloroprene polymer latex (A) according to the third embodiment of the present invention may include: a first polymerization step of polymerizing a chloroprene polymer α by polymerizing raw material monomers containing chloroprene, and a second polymerization step of polymerizing a chloroprene polymer β in the presence of the chloroprene polymer α, or a first polymerization step of polymerizing a chloroprene polymer β by polymerizing raw material monomers containing chloroprene, and a second polymerization step of polymerizing the chloroprene polymer α in the presence of the chloroprene polymer β.
[0058] In the first polymerization step, it is preferable to adjust the amount of the chain transfer agent, etc., depending on the target weight-average molecular weight. In the method for producing a chloroprene polymer latex according to the third embodiment of the present invention, a polymerization terminator may not be used in the first polymerization step. Other details, such as the type, amount of each agent used, and polymerization conditions, in the first polymerization step are as described in the polymerization step of the first embodiment.
[0059] The third embodiment of the present invention may include a second polymerization step of polymerizing the chloroprene polymer β in the presence of the chloroprene polymer α, or a second polymerization step of polymerizing the chloroprene polymer α in the presence of the chloroprene polymer β.
[0060] In the second polymerization step, the chloroprene polymer α (or chloroprene polymer β) may be added to the polymerization solution in any form. For example, the polymerization solution obtained by polymerizing the chloroprene polymer α (or chloroprene polymer β) may be used as is. As an example, when the chloroprene polymer α (or chloroprene polymer β) is polymerized by emulsion polymerization, a latex containing the chloroprene polymer α (or chloroprene polymer β) may be added to the chloroprene polymer β or the polymerization solution of the chloroprene polymer α. Alternatively, for example, the chloroprene polymer α (or chloroprene polymer β) may be precipitated from a polymerization solution obtained by polymerizing the chloroprene polymer α (or chloroprene polymer β), and the precipitated chloroprene polymer α (or chloroprene polymer β) may be added to the polymerization solution of the chloroprene polymer β (or chloroprene polymer α). For example, when the chloroprene polymer α (or the chloroprene polymer β) is polymerized by emulsion polymerization, the chloroprene polymer α (or the chloroprene polymer β) may be precipitated using methanol and added to a polymerization solution of the chloroprene polymer β (or the chloroprene polymer α), or a rubber component (the chloroprene polymer α (or the chloroprene polymer β)) obtained by freeze-drying a latex containing the chloroprene polymer α (or the chloroprene polymer β) may be added to a polymerization solution of the chloroprene polymer β (or the chloroprene polymer α).
[0061] In the second polymerization step, when the chloroprene polymer β is polymerized, the amount of the chloroprene polymer α can be 5.0 to 60.0 parts by mass relative to 100 parts by mass of the chloroprene monomer (or raw material monomer). The amount of the chloroprene polymer α can be, for example, 5.0, 10.0, 15.0, 20.0, 25.0, 30.0, 35.0, 40.0, 50.0, or 60.0 parts by mass, or can be within a range between any two of the values exemplified here. In the second polymerization step, when the chloroprene polymer α is polymerized, the amount of the chloroprene polymer β can be 40.0 to 95.0 parts by mass relative to 100 parts by mass of the chloroprene monomer (or raw material monomer). The amount of the chloroprene polymer β charged is, for example, 40.0, 50.0, 60.0, 65.0, 70.0, 75.0, 80.0, 85.0, 90.0, or 95.0 parts by mass, and may be within a range between any two of the numerical values exemplified here.
[0062] In the second polymerization step, the type and amount of each monomer are preferably adjusted so that the content of each monomer unit in the resulting chloroprene polymer latex (A) falls within the above-mentioned range. Other details such as the type, amount used, and polymerization conditions of each agent in the second polymerization step can be as described in the above-mentioned polymerization step.
[0063] The chloroprene polymer latex containing the chloroprene polymer α having a weight-average molecular weight of 5,000 to 80,000 and / or the chloroprene polymer β having a weight-average molecular weight of 200,000 to 1,500,000 obtained by the above production method can be used as the chloroprene polymer latex (A) according to the present invention.
[0064] 1.3 Metal Oxide (B) The chloroprene polymer latex composition according to the present invention contains 0.3 to 15.0 parts by mass of metal oxide (B) per 100 parts by mass of the solids content of the chloroprene polymer latex (A). The content of metal oxide (B) is, for example, 0.3, 0.5, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, 10.0, 11.0, 12.0, 13.0, 14.0, or 15.0 parts by mass, and may be within a range between any two of the values exemplified here. When the content of metal oxide (B) is equal to or greater than the lower limit, the tensile strength at break is improved due to the crosslinking effect between polymers. Furthermore, when the content of metal oxide (B) is equal to or less than the upper limit, a dip-molded product with excellent flexibility can be obtained.
[0065] The type of metal oxide (B) is not particularly limited and can be at least one of zinc oxide, lead oxide, trilead tetroxide, magnesium oxide, aluminum oxide, iron oxide, beryllium oxide, and titanium oxide. The metal oxide preferably contains zinc oxide. Zinc oxide is generally believed to function as a scavenger for dechlorinated atoms in chloroprene-based polymers. One type of metal oxide (B) may be used, or two or more types may be used in combination.
[0066] 1.4 Vulcanization Accelerator (C) The chloroprene polymer latex composition according to the present invention contains 0.02 to 1.50 parts by mass of a vulcanization accelerator (C) relative to 100 parts by mass of the solid content of the chloroprene polymer latex (A). The content of the vulcanization accelerator (C) is, for example, 0.02, 0.04, 0.06, 0.08, 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, 0.70, 0.80, 0.90, 1.00, 1.10, 1.20, 1.30, 1.40, or 1.50 parts by mass, and may be within a range between any two of the values exemplified here. The chloroprene polymer latex composition according to the present invention contains the vulcanization accelerator (C) in a specific amount that is smaller than that of conventional chloroprene polymer latex compositions, and therefore, it is possible to obtain a dip-molded article having excellent flexibility and tensile strength at break while reducing the risk of allergies and reducing costs.
[0067] The vulcanization accelerator (C) according to the present invention contains at least one of thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthogenate-based, and thiazole-based vulcanization accelerators. One type of vulcanization accelerator (C) may be used, or two or more types may be used in combination.
[0068] The thiourea-based vulcanization accelerator may be a compound having a thiourea structure, such as the compound represented by the following formula:
[0069]
[0070] In the above formula, R 11 ~R 14 can each independently represent hydrogen or an organic group, can represent hydrogen or a hydrocarbon group, and the hydrocarbon group can be an alkyl group or an aryl group. Examples of thiourea compounds include ethylene thiourea, diethyl thiourea (N,N'-diethyl thiourea), trimethyl thiourea, diphenyl thiourea (N,N'-diphenyl thiourea), 1,3-trimethylene-2-thiourea, etc.
[0071] Examples of thiuram vulcanization accelerators include compounds containing one or more structures represented by the following formula:
[0072]
[0073] In the above formula, R 21 , R 22 , R 23 , R 24 R can each independently be an organic group, preferably a hydrocarbon group. The hydrocarbon group can be an alkyl group having 1 to 12 carbon atoms or a cycloalkyl group having 1 to 12 carbon atoms. 21 and R 22 , R 23 and R 24 may be linked to each other to form a cyclic structure (for example, a cycloalkyl group). n can be an integer of 1 or more, and can be 1 to 4, preferably 1 or 2, and more preferably 2.
[0074] Examples of thiuram vulcanization accelerators include tetramethylthiuram disulfide (TMTD), tetraethylthiuram disulfide, tetrabutylthiuram disulfide, tetrakis(2-ethylhexyl)thiuram disulfide, tetramethylthiuram monosulfide, and dipentamethylenethiuram tetrasulfide.
[0075] Examples of dithiocarbamate vulcanization accelerators include compounds composed of ions represented by the following formula and metal ions.
[0076] In the above formula, R 31 ~R 32 can each independently be an organic group or a hydrocarbon group. The hydrocarbon group can be an alkyl group, an aryl group, or an aralkyl group, and R 31 and R 32 may be linked to form a cycloalkyl group. Examples of metal ions include zinc, sodium, copper, iron, nickel, and tellurium. Examples of dithiocarbamate vulcanization accelerators include sodium dibutyldithiocarbamate, zinc dimethyldithiocarbamate, zinc diethyldithiocarbamate, zinc N-ethyl-N-phenyldithiocarbamate, zinc N-pentamethylenedithiocarbamate, copper dimethyldithiocarbamate, ferric dimethyldithiocarbamate, and tellurium diethyldithiocarbamate.
[0077] Examples of guanidine compounds include compounds having a guanidine skeleton, such as 1,3-diphenylguanidine, 1,3-di-o-tolylguanidine, 1-o-tolylbiguanide, and di-o-tolylguanidine salts of dicatechol borate.
[0078] Examples of xanthogenate-based vulcanization accelerators include compounds composed of ions represented by the following formula and metal ions.
[0079]
[0080] In the above formula, R41 can be an organic group or a hydrocarbon group. The hydrocarbon group can be an alkyl group. Examples of metal ions include zinc, sodium, copper, nickel, and tellurium. Examples of xanthogenate-based vulcanization accelerators include zinc butylxanthogenate and zinc isopropylxanthogenate.
[0081] Examples of the thiazole compound include compounds having a thiazole skeleton, and compounds having a benzothiazole skeleton are more preferred. Examples of the thiazole compound include 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, 2-mercaptobenzothiazole zinc salt, cyclohexylamine salt of 2-mercaptobenzothiazole, 2-(4'-morpholinodithio)benzothiazole, N-cyclohexylbenzothiazole-2-sulfenamide, N-cyclohexyl-2-benzothiazolyl sulfenamide, and N-oxydiethylene-2-benzothiazolyl sulfenamide.
[0082] 1.5 Sulfur (D) The chloroprene polymer latex composition according to the present invention contains 0.01 to 0.75 parts by mass of sulfur (D) per 100 parts by mass of the solids content of the chloroprene polymer latex (A). The content of sulfur (D) is, for example, 0.01, 0.02, 0.03, 0.05, 0.10, 0.15, 0.20, 0.25, 0.30, 0.35, 0.40, 0.45, 0.50, 0.55, 0.60, 0.65, 0.70, or 0.75 parts by mass, and may be within a range between any two of the values exemplified here. The chloroprene polymer latex composition according to the present invention contains sulfur (D) in a specific amount that is smaller than that of conventional chloroprene polymer latex compositions, thereby enabling the production of a dip-molded article that has excellent flexibility and tensile strength at break while reducing the risk of allergies and reducing costs.
[0083] 1.6 Heteroaromatic Ring Compound (E) The chloroprene polymer latex composition according to the present invention contains 0.1 to 10.0 parts by mass of a heteroaromatic ring compound (E) per 100 parts by mass of the solid content of the chloroprene polymer latex (A). The heteroaromatic ring compound (E) can be represented by chemical formula (1) and has a benzimidazole structure. Compounds having this structure are sometimes used as secondary antioxidants, mainly in the formulation of rubber compositions.
[0084]
[0085] In chemical formula (1), X of the mercapto group represents a hydrogen atom or a metal atom. X may be a hydrogen atom, and the mercapto group may have a thiol group. X may also be a metal atom, and examples of the metal atom include zinc, sodium, copper, nickel, and tellurium, with zinc being preferred.
[0086] R in chemical formula (1) 1 ~R 4 R represents a hydrogen atom, an alkyl group which may have a substituent, an ether group which may have a substituent, a nitro group, an amino group, or a carboxyl group. 1 ~R 4 may be the same or different. The heteroaromatic ring compounds (E) may be used singly or in combination of two or more.
[0087] Examples of the heteroaromatic ring compound (E) include 2-mercaptobenzimidazole, 5-methyl-2-mercaptobenzimidazole, 4-methyl-2-mercaptobenzimidazole, 5-methoxy-2-mercaptobenzimidazole, 4-methoxy-2-mercaptobenzimidazole, 5-nitro-2-mercaptobenzimidazole, 5-amino-2-mercaptobenzimidazole, 5-carboxy-2-mercaptobenzimidazole, and zinc salts of 2-mercaptobenzimidazole. Among these, 2-mercaptobenzimidazole, 5-methyl-2-mercaptobenzimidazole, 4-methyl-2-mercaptobenzimidazole, 5-methoxy-2-mercaptobenzimidazole, 4-methoxy-2-mercaptobenzimidazole, and zinc salts of 2-mercaptobenzimidazole are preferred.
[0088] The amount of the heteroaromatic ring compound (E) added is preferably 0.1 to 10.0 parts by mass per 100 parts by mass of the solids content of the chloroprene polymer latex (A) contained in the chloroprene polymer latex composition. The content of the heteroaromatic ring compound (E) is, for example, 0.1, 0.2, 0.3, 0.4, 0.5, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, or 10.0 parts by mass, and may be within a range between any two of the values exemplified here. When the content of the heteroaromatic ring compound (E) is equal to or greater than the above-mentioned lower limit, the dip-molded article exhibits extremely high tensile strength at break. When the content of the heteroaromatic ring compound (E) is equal to or less than the above-mentioned upper limit, the stability of the chloroprene polymer latex composition is ensured. By adjusting the content of the heteroaromatic ring compound (E) within the above range, the flexibility and tensile strength at break of the dip-molded article can be highly improved. The heteroaromatic ring compound (E) may be used alone or in combination of two or more.
[0089] 1.7 Antioxidant The chloroprene polymer latex composition according to the present invention may contain 0.5 to 10.0 parts by mass of an antioxidant per 100 parts by mass of the solid content of the chloroprene polymer latex (A). The type of antioxidant is not particularly limited, and phenolic antioxidants, amine-based antioxidants, heat-resistant oxidation (aging) inhibitors, ozone-resistant antioxidants, etc. may be used (however, the heteroaromatic ring compound (E) may be excluded). When the resulting dip-molded article is used as a medical glove, a phenolic antioxidant may be used from the viewpoints of the color tone, texture, and hygiene of the dip-molded article. In particular, a hindered phenolic antioxidant is preferred because of its potent effects. Examples of hindered phenol-based antioxidants include 2,2'-methylenebis(4-ethyl-6-t-butylphenol), 2,2'-methylenebis(4-methyl-6-t-butylphenol), 4,4'-butylidene(3-methyl-6-t-butylphenol), 4,4'-thiobis(3-methyl-6-t-butylphenol), butylated reaction products of p-cresol and dicyclopentadiene, 2,5'-di-t-butylhydroquinone, and 2,5'-di-t-amylhydroquinone. Among these, butylated reaction products of p-cresol and dicyclopentadiene are preferred from the viewpoint of general dispersibility in aqueous materials. One type of antioxidant may be used, or two or more types may be used in combination.
[0090] The content of the antioxidant is preferably 0.5 to 10.0 parts by mass per 100 parts by mass of the solids content of the chloroprene polymer latex (A) contained in the chloroprene polymer latex composition. The content of the antioxidant is, for example, 0.5, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, or 10.0 parts by mass, and may be within a range between any two of the values exemplified here. When the content of the antioxidant is equal to or greater than the lower limit, color change of the dip-molded article can be suppressed. When the amount of the antioxidant is equal to or less than the upper limit, the stability of the chloroprene polymer latex composition can be ensured. Furthermore, from the viewpoint of the balance of physical properties between the flexibility and tensile strength at break of the obtained dip-molded article, the amount of the antioxidant added is more preferably 0.5 to 5.0 parts by mass.
[0091] 2. Physical Properties of Chloroprene Polymer Latex Composition <Toluene Swelling Degree> In the chloroprene polymer latex composition according to one embodiment of the present invention, the chloroprene polymer latex composition is molded by a dip coagulation method, and then subjected to heat drying treatment at 140°C for 60 minutes, and the dip-molded product has a toluene swelling degree of preferably 12.0 or less, and more preferably 10.0 or less. The toluene swelling degree is expressed by formula (1). Formula (1): Toluene swelling index = 1 + (W2 / W1-1)(P1 / P2)(1 / r) In formula (1), W1 represents the mass of the dip-molded article before immersion in toluene, W2 represents the mass of the dip-molded article after immersion in toluene, P1 represents the specific gravity of the chloroprene polymer content in the chloroprene polymer latex (A), P2 represents the specific gravity of toluene, and r represents the mass fraction of the chloroprene polymer content in the dip-molded article. The chloroprene polymer content in the chloroprene polymer latex (A) can be obtained by mixing the chloroprene polymer latex (A) with methanol to cause precipitation, followed by filtration and drying. The specific gravities of the chloroprene polymer content in the chloroprene polymer latex (A) and the specific gravity of toluene can be measured at 20°C, and P2 can be set to 0.867. P1 can be the specific gravity of the chloroprene polymer in the chloroprene polymer latex (A) measured at 20° C., and P1 can be set to 1.23.
[0092] The toluene swelling degree of the dip-molded article of the chloroprene polymer latex composition is, for example, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, 10.0, 11.0, or 12.0, and may be within a range between any two of the numerical values exemplified here. The toluene swelling degree of the dip-molded article of the chloroprene polymer latex composition is thought to be related to the degree of crosslinking of the chloroprene polymer latex, and it is presumed that the higher the degree of crosslinking, the lower the swelling degree tends to be. By setting the toluene swelling degree of the chloroprene polymer latex according to the present invention to 12.0 or less, the dip-molded article can have better tensile strength at break and flexibility.
[0093] The toluene swelling degree can be measured by the method described in Examples. The toluene swelling degree can be adjusted by appropriately selecting a production method for the chloroprene polymer latex composition. For example, a chloroprene polymer latex composition having a toluene swelling degree of 12.0 or less can be obtained by a production method including a polymerization step of polymerizing the chloroprene polymer β (or the chloroprene polymer α) in the presence of the chloroprene polymer α (or the chloroprene polymer β), as described above.
[0094] <Ratio RB / RA of the total amount RB of peak areas of abietic acid, neoabietic acid, palustric acid, levopimaric acid and their salts to the total amount RA of peak areas of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid and their salts> The chloroprene polymer latex composition according to one embodiment of the present invention is obtained by molding a chloroprene polymer latex composition by a dip coagulation method, followed by heating and drying at 140°C for 60 minutes to obtain a dip molded product, and then drying the resulting product in accordance with JIS K The ratio RB / RA, which is the ratio of the total peak area RB of abietic acid, neoabietic acid, palustric acid, levopimaric acid, and their salts to the total peak area RA of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid, and their salts, obtained by gas chromatography analysis of an extract extracted with an ethanol / toluene azeotrope as specified in JIS No. 6229, is preferably 0.10 or more, more preferably 0.10 to 0.70, and even more preferably 0.15 to 0.50. RB / RA may be, for example, 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, or 0.70, or may be within a range between any two of the values exemplified here. By setting RB / RA within the above range, the tensile strength at break of the dip-molded body can be further improved.
[0095] RB / RA can be determined by molding a chloroprene polymer latex composition by a dip coagulation method, heating and drying the resulting dip-molded product at 140°C for 60 minutes, placing the resulting product in a flask equipped with a condenser, extracting the product with an ethanol / toluene azeotrope as specified in JIS K 6229, treating the product with hydrochloric acid, and then analyzing the product with gas chromatography, or by calculating the ratio by the method described in the Examples. RB / RA can be controlled by adjusting the types and blending ratio of rosin acid and rosin acid salt added as emulsifiers during the production of a chloroprene polymer latex.
[0096] In the chloroprene polymer latex composition according to one embodiment of the present invention, a dip-molded product obtained by molding the chloroprene polymer latex composition by a dip coagulation method and then heating and drying the product at 140°C for 60 minutes has a modulus at 100% elongation of preferably 0.65 MPa or less, more preferably 0.60 MPa, as measured in accordance with JIS K 6251. The modulus at 100% elongation is, for example, 0.30, 0.35, 0.4, 0.45, 0.50, 0.55, 0.60, or 0.65 MPa, and may be within a range between any two of the values exemplified here.
[0097] In the chloroprene polymer latex composition according to one embodiment of the present invention, a dip-molded product obtained by molding the chloroprene polymer latex composition by a dip coagulation method and then heating and drying the product at 140°C for 60 minutes has a tensile strength at break of preferably 19.0 MPa or more, more preferably 20.0 MPa, as measured in accordance with JIS K 6251. The tensile strength at break is, for example, 19.0, 20.0, 21.0, 22.0, 23.0, 24.0, or 25.0 MPa, and may be within a range between any two of the values exemplified here.
[0098] The tensile strength at break and the modulus at 100% elongation of the dip-molded product of the chloroprene polymer latex composition can be controlled by adjusting the type and amount of the chloroprene polymer latex composition, as well as the polymerization recipe and conditions, weight-average molecular weight, toluene-insoluble content, etc. of the chloroprene polymer latex used.
[0099] 3. Method for Producing Chloroprene Polymer Latex Composition A method for producing a chloroprene polymer latex composition according to one embodiment of the present invention may include a raw material mixing step of mixing raw materials containing a chloroprene polymer latex (A), a metal oxide (B), a vulcanization accelerator (C), sulfur (D), a heteroaromatic ring compound (E), and other required chemicals. In the mixing step, an aqueous dispersion containing the metal oxide (B), the vulcanization accelerator (C), sulfur (D), a heteroaromatic ring compound (E), and other required chemicals may be prepared in advance, and then the chloroprene polymer latex (A) and the aqueous dispersion may be mixed. The mixing step may be performed using a known mixing device such as a ball mill.
[0100] 4. Dip-molded Articles (Dip-molded Coatings and Films) A dip-molded article according to one embodiment of the present invention is a dip-molded article of the above-described chloroprene polymer latex composition. The dip-molded article according to one embodiment of the present invention is obtained by dip-molding the chloroprene polymer latex composition according to the present invention, either alone or in combination with another chloroprene polymer latex composition. The dip-molded article has a low modulus at 100% elongation, flexibility, and excellent mechanical properties such as strength and elongation. For example, the dip-molded article can have the above-described modulus at 100% elongation and / or tensile strength at break. The dip-molded article can be suitably used as industrial or general household gloves, medical gloves, balloons, catheters, and boots.
[0101] The thickness of the dip-molded article (e.g., the minimum thickness) may be 0.01 to 0.50 mm. The thickness of the dip-molded article may be, for example, 0.01, 0.05, 0.10, 0.20, 0.30, 0.40, or 0.50 mm, and may be within a range between any two of the values exemplified here. The thickness of the dip-molded article can be adjusted by the time for which the mold is immersed in the polymer latex composition, the solids concentration of the chloroprene polymer latex composition, and the like. To reduce the thickness of the dip-molded article, the immersion time may be shortened or the solids concentration of the chloroprene polymer latex composition may be reduced.
[0102] 5. Method for Producing Dip-Molded Article A method for producing a dip-molded article according to one embodiment of the present invention may include a dip-molding step of dip-molding the chloroprene polymer latex composition according to the present invention to obtain a dip-molded article.
[0103] Examples of dip molding methods according to one embodiment of the present invention include the immersion coagulation method, simple immersion method, thermal immersion method, and electrodeposition method. The immersion coagulation method can be used from the viewpoints of ease of production and the ease of obtaining dip-molded bodies of a uniform thickness. Specifically, a ceramic mold coated with a calcium-based coagulation liquid is immersed in a dip-molded body composition, which is then coagulated. After leaching to remove water-soluble impurities, the composition is dried, and then heated and vulcanized to form a dip-molded coating (rubber coating), which is then demolded. This allows for the production of a film-like dip-molded body.
[0104] The method for producing a dip-molded body according to one embodiment of the present invention can include a drying step of heating and drying the dip-molded body.
[0105] The heating and drying temperature may be appropriately set depending on the composition of the chloroprene polymer latex composition, and may be 120 to 180°C. The heating temperature is preferably 120 to 150°C. The heating temperature may be, for example, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, or 220°C, and may be within a range between any two of the values exemplified here. The heating time may be appropriately set depending on the composition of the chloroprene polymer latex composition, the shape of the unvulcanized molded body, and the like, and may be 10 to 300 minutes. The heating time may be, for example, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, or 300 minutes, or may be within a range between any two of the values exemplified here. As an example, a dip-molded body according to one embodiment of the present invention may be one that has been subjected to a heat drying treatment at 140°C for 60 minutes.
[0106] The present invention will be described in more detail below based on examples, but the present invention should not be construed as being limited to these examples.
[0107] First, a method for producing the chloroprene polymer latex used in the examples will be described.
[0108] <Preparation of Chloroprene Polymer Latex A-1> (Polymerization Step of Chloroprene Polymer α-1) To a 30 L polymerization vessel were added 64 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 90 parts by mass of pure water, 4.5 parts by mass of conjugated resin acid-based rosin acid (trade name "Harthall R-WW", manufactured by Harima Chemicals Co., Ltd.), 3.4 parts by mass of n-dodecyl mercaptan, 1.6 parts by mass of potassium hydroxide, 0.5 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "Demol N", manufactured by Kao Corporation), and 0.5 parts by mass of sodium hydrogen sulfite. Polymerization was carried out at a polymerization temperature of 35°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous potassium persulfate solution as a polymerization initiator. When the polymerization rate of the charged monomers reached 80%, 27 parts by mass of chloroprene (monomer) was continuously added over 100 minutes. When the polymerization rate of the initially charged monomers and the continuously added monomers reached 91%, the addition of the aqueous potassium persulfate solution was stopped to terminate the polymerization, thereby obtaining a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and the resulting mixture was concentrated to obtain a latex containing a chloroprene polymer α-1 with a solids concentration of 60% by mass.
[0109] (Precipitation of chloroprene polymer with methanol) The obtained latex containing the chloroprene polymer α-1 was mixed with a large amount of methanol to precipitate the chloroprene polymer α-1, which was then filtered and dried to obtain a chloroprene polymer, which was used in the production of chloroprene polymers β-1 and β-23 and chloroprene polymer latex A-14 described below.
[0110] (Polymerization step of chloroprene polymer β-1) To a 30 L polymerization vessel were added 28.3 parts by mass of the chloroprene polymer precipitated from a latex containing chloroprene polymer α-1, 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 110 parts by mass of pure water, 5.8 parts by mass of conjugated resin acid-based rosin acid (trade name "Harthall R-WW" manufactured by Harima Chemicals Co., Ltd.), 2 parts by mass of potassium hydroxide, 0.5 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "Demol N" manufactured by Kao Corporation), 0.5 parts by mass of sodium hydrogen sulfite, and 0.03 parts by mass of thiourea dioxide. Polymerization was carried out at a polymerization temperature of 14°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous potassium persulfate solution as a polymerization initiator. When the polymerization rate reached 85%, 0.1 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization, yielding a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and the resulting mixture was concentrated to yield a chloroprene polymer latex A-1 having a solids concentration of 60% by mass and containing the chloroprene polymer β-1.
[0111] 50 ml of the chloroprene polymer latex A-1 was sampled, and the remaining chloroprene polymer latex A-1 was used to prepare a dip-molded product for evaluation.
[0112] The sampled chloroprene polymer latex was mixed with a large amount of methanol to precipitate the chloroprene polymer, which was then filtered and dried to obtain a chloroprene polymer sample. The weight-average molecular weight of the chloroprene polymer latex obtained was measured from the obtained sample. Measurement of the weight-average molecular weight of chloroprene polymer latex A-1 confirmed a peak attributable to chloroprene polymer α-1 having a weight-average molecular weight of 5,000 to 80,000, and a peak attributable to chloroprene polymer β-1 having a weight-average molecular weight of 200,000 to 1,500,000. Furthermore, the toluene-insoluble portion of the chloroprene polymer rubber obtained by freeze-drying the chloroprene polymer latex was measured. The respective measurement methods will be described later.
[0113] <Preparation of Chloroprene Polymer Latex A-13> (Synthesis of Chloroprene Polymer β-13) To a 30 L polymerization vessel were added 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 110 parts by mass of pure water, 4.7 parts by mass of conjugated resin acid-based rosin acid (trade name "Harthall R-WW", manufactured by Harima Chemicals Co., Ltd.), 0.02 parts by mass of n-dodecyl mercaptan, 1.6 parts by mass of potassium hydroxide, 0.4 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "Demol N", manufactured by Kao Corporation), and 0.4 parts by mass of sodium hydrogen sulfite. Polymerization was carried out at a polymerization temperature of 40°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous potassium persulfate solution as a polymerization initiator. When the polymerization rate of the charged monomers reached 85%, 0.01 parts by mass of diethylhydroxylamine, a polymerization terminator, was added to terminate the polymerization. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and the mixture was concentrated to obtain a chloroprene polymer latex A-13 containing a chloroprene polymer β-13 having a solids concentration of 60% by mass. The weight average molecular weight and the toluene insoluble matter were analyzed in the same manner as for the chloroprene polymer latex A-1.
[0114] <Preparation of Chloroprene Polymer Latex A-14> (Synthesis of Chloroprene Polymer β-14) To a 30 L polymerization vessel were added 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 110 parts by mass of pure water, 4.7 parts by mass of conjugated resin acid-based rosin acid (trade name "Harthall R-WW", manufactured by Harima Chemicals Co., Ltd.), 0.02 parts by mass of n-dodecyl mercaptan, 1.6 parts by mass of potassium hydroxide, 0.4 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "Demol N", manufactured by Kao Corporation), 0.4 parts by mass of sodium hydrogensulfite, and 0.03 parts by mass of thiourea dioxide. Polymerization was carried out at a polymerization temperature of 14°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous solution of potassium persulfate as a polymerization initiator. When the polymerization rate of the charged monomers reached 85%, 0.01 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and the mixture was concentrated to obtain a latex containing chloroprene polymer β-14 with a solid content of 60% by mass.
[0115] (Preparation of Chloroprene Polymer Latex A-14) The latex containing the chloroprene polymer α-1 and the latex containing the chloroprene polymer β-14 were mixed at a solid content ratio of 25:75 to obtain Chloroprene Polymer Latex A-14. The weight average molecular weight and toluene insoluble matter were analyzed in the same manner as for Chloroprene Polymer Latex A-1.
[0116] <Preparation of Chloroprene Polymer Latex A-15> (Polymerization of Chloroprene Polymer α-15) To a 30 L polymerization vessel were added 64 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 77 parts by mass of pure water, 17.6 parts by mass of a gum rosin-based disproportionated rosin aqueous solution (trade name "LONDIS K-25", solids content 25% by mass, manufactured by Arakawa Chemical Industries, Ltd.), 3.4 parts by mass of n-dodecyl mercaptan, 0.8 parts by mass of potassium hydroxide, 0.5 parts by mass of a sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), and 0.5 parts by mass of sodium hydrogen sulfite. Polymerization was carried out at a polymerization temperature of 35°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous potassium persulfate solution as a polymerization initiator. When the polymerization rate of the charged monomers reached 80%, 27 parts by mass of chloroprene (monomer) was continuously added over 100 minutes. When the polymerization rate of the initially charged monomers and the continuously added monomers reached 91%, the addition of the aqueous potassium persulfate solution was stopped to terminate the polymerization, thereby obtaining a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and the resulting solution was concentrated to obtain a latex containing chloroprene polymer α-15 with a solids concentration of 60% by mass. The obtained latex containing chloroprene polymer α-15 was mixed with a large amount of methanol to precipitate chloroprene polymer α-15, which was then filtered and dried to obtain a chloroprene polymer. This was used to prepare chloroprene polymer β-15, which will be described later.
[0117] (Preparation of Chloroprene Polymer β-15) To a 30 L polymerization vessel were added 28.3 parts by mass of a chloroprene polymer precipitated from a latex containing chloroprene polymer α-15, 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 100 parts by mass of pure water, 18.5 parts by mass of a gum rosin-based disproportionated rosin aqueous solution (trade name "LONDIS K-25", solids content 25% by mass, manufactured by Arakawa Chemical Industries, Ltd.), 0.8 parts by mass of potassium hydroxide, 0.5 parts by mass of a sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), 0.5 parts by mass of sodium hydrogensulfite, and 0.03 parts by mass of thiourea dioxide. Polymerization was carried out at a polymerization temperature of 14°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous potassium persulfate solution as a polymerization initiator. When the polymerization rate reached 85%, 0.1 parts by mass of diethylhydroxylamine, a polymerization terminator, was added to terminate the polymerization, yielding a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and the resulting mixture was concentrated to yield a chloroprene polymer latex A-15 having a solids concentration of 60% by mass and containing the chloroprene polymer β-15. The weight average molecular weight and the toluene insoluble content were analyzed in the same manner as for the chloroprene polymer latex A-1.
[0118] <Preparation of Chloroprene Polymer Latex A-17> (Polymerization of Chloroprene Polymer α-17) To a 30 L polymerization vessel were added 60 parts by mass of chloroprene (monomer), 8 parts by mass of 2,3-dichloro-1,3-butadiene, 90 parts by mass of pure water, 4.5 parts by mass of conjugated resin acid-based rosin acid (trade name "Harthall R-WW", manufactured by Harima Chemicals Co., Ltd.), 3 parts by mass of n-dodecyl mercaptan, 1.5 parts by mass of potassium hydroxide, and 0.5 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "Demol N", manufactured by Kao Corporation). Polymerization was carried out at a polymerization temperature of 40°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous solution of potassium persulfate as a polymerization initiator. When the polymerization rate of the charged monomers reached 65%, 32 parts by mass of chloroprene (monomer) was continuously added over 100 minutes. When the polymerization rate of the initially charged monomer and the continuously added monomer reached 88%, 0.1 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization, thereby obtaining a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and the resulting mixture was concentrated to obtain a latex containing chloroprene polymer α-17 with a solid content of 60% by mass.
[0119] (Polymerization of Chloroprene Polymer β-17) To a 30 L polymerization vessel were added 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 90 parts by mass of pure water, 4.5 parts by mass of conjugated resin acid-based rosin acid (trade name "Harthall R-WW", manufactured by Harima Chemicals Co., Ltd.), 0.02 parts by mass of n-dodecyl mercaptan, 1.5 parts by mass of potassium hydroxide, and 0.5 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "Demol N", manufactured by Kao Corporation). Polymerization was carried out at a polymerization temperature of 25°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous solution of potassium persulfate as a polymerization initiator. When the polymerization rate of the charged monomers reached 82%, 0.01 part by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and concentrated to obtain a latex containing chloroprene polymer β-17 with a solid content of 60% by mass.
[0120] (Preparation of Chloroprene Polymer A-17) A latex containing chloroprene polymer α-17 and a latex containing chloroprene polymer β-17 were mixed at a solid content ratio of 25:75 to obtain chloroprene polymer latex A-17. The weight average molecular weight and toluene insoluble matter were analyzed in the same manner as for chloroprene polymer latex A-1.
[0121] <Preparation of Chloroprene Polymer Latex A-23> (Synthesis of Chloroprene Polymer β-23) A 30 L polymerization vessel was charged with 85 parts by mass of the chloroprene polymer precipitated from a latex containing chloroprene polymer α-1, 9 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 110 parts by mass of pure water, 8.5 parts by mass of conjugated resin acid-based rosin acid (trade name "Harthall R-WW", manufactured by Harima Chemicals Co., Ltd.), 3 parts by mass of potassium hydroxide, 0.7 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (trade name "Demol N", manufactured by Kao Corporation), 0.7 parts by mass of sodium hydrogensulfite, and 0.03 parts by mass of thiourea dioxide. Polymerization was carried out at a polymerization temperature of 14°C under a nitrogen stream by continuously adding a 0.35% by mass aqueous potassium persulfate solution as a polymerization initiator. When the polymerization rate reached 85%, 0.1 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization, yielding a polymerization liquid. The polymerization liquid was distilled under reduced pressure to remove unreacted monomers, and concentrated to obtain a chloroprene polymer latex A-23 containing a chloroprene polymer β-23 having a solids concentration of 60% by mass.
[0122] <Method for Analyzing Chloroprene Polymer Latex> Chloroprene polymer latex was analyzed by the following method. (Measurement of Weight-Average Molecular Weight of Chloroprene Polymer Latex) As described above, the chloroprene polymer latex was precipitated with methanol, filtered, and the dried chloroprene polymer was dissolved in 20 ml of tetrahydrofuran to obtain a sample, which was then subjected to gel permeation chromatography (GPC) under the following measurement conditions. Apparatus: HLC-8320 (manufactured by Tosoh Corporation) Column: Three TSKgel GMHHR-H columns in series Temperature: 40°C Detection: Differential refractive index Solvent: Tetrahydrofuran Calibration curve: Prepared using standard polystyrene (PS).
[0123] (Toluene Insolubles) The obtained chloroprene polymer latex was freeze-dried to obtain a chloroprene polymer rubber, which was then cut into 2 mm squares to obtain a test piece. The test piece was placed in a conical beaker and dissolved in 80 g of toluene for 16 hours. Subsequently, after centrifugation, the gel fraction (insolubles) was separated using a 200-mesh wire netting. The gel fraction was then dried and the mass of the dried product was measured. The toluene insolubles in the chloroprene polymer rubber were calculated using the following formula, where Ag is the chloroprene polymer rubber after freeze-drying and B g is the gel fraction (insolubles) separated from the mixture dissolved in toluene. Toluene insolubles (gel fraction) = B / A x 100 (%)
[0124] Example 1 Preparation of Chloroprene Polymer Latex Composition 2 parts by mass of two types of zinc oxide as the metal oxide (B), 0.5 parts by mass of Noccela BZ as the vulcanization accelerator (C), 0.25 parts by mass of sulfur (D), 2 parts by mass of Nocrac PBK as the antioxidant, 1 part by mass of a heteroaromatic ring compound (E) represented by Chemical Formula 2 as the heteroaromatic ring compound (E), and 0.1 parts by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "Demol N", manufactured by Kao Corporation) were added to water and mixed using a ceramic ball mill at 20°C for 16 hours to prepare an aqueous dispersion. The aqueous dispersion was mixed with chloroprene polymer latex A-1, and water was further added so that the solids concentration was 30% by mass, to prepare a chloroprene polymer latex composition. The obtained chloroprene polymer latex composition contained each agent in the blending amount shown in Table 1 relative to the solid content of the chloroprene polymer latex.
[0125] <Preparation of Dip-Molded Film> A ceramic cylinder (manufactured by Shinko Corporation) with an outer diameter of 50 mm was immersed for 1 second in a coagulation liquid containing 62 parts by mass of water, 35 parts by mass of calcium nitrate tetrahydrate, and 3 parts by mass of calcium carbonate, and then removed. After drying for 3 minutes, the cylinder was immersed for 2 minutes in the chloroprene polymer latex composition prepared by the procedure described above. The cylinder was then washed with running water at 45°C for 1 minute and dried at 140°C for 60 minutes to prepare a dip-molded film (dip-molded coating) for evaluation.
[0126] Examples 2 to 15, Comparative Examples 1 to 8 Chloroprene polymer latex compositions and dip-molded films (dip-molded coatings) for evaluation were prepared in the same manner as in Example 1, except that the types of chloroprene polymer latexes used were as shown in Tables 1 to 3 and the formulation of the aqueous dispersions was adjusted so that the amounts of each agent were as shown in Tables 1 to 3.
[0127] Metal oxide (B) Zinc oxide type 2 Zinc oxide, manufactured by Sakai Chemical Industry Co., Ltd., "Zinc oxide type 2"
[0128] Vulcanization accelerators (C) Noccelaer BZ: zinc dibutyldithiocarbamate, "Noccelaer BZ" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Noccelaer C: N,N'-diphenylthiourea, "Noccelaer C" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Noccelaer TET: tetraethylthiuram disulfide, "Noccelaer TET" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Noccelaer D: 1,3-diphenylguanidine, "Noccelaer D" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Noccelaer TP: sodium dibutyldithiocarbamate, "Noccelaer TP" manufactured by Ouchi Shinko Chemical Industry Co., Ltd.
[0129] Heteroaromatic ring compound (E) Chemical formula 2: Heteroaromatic ring compound represented by chemical formula (2)
[0130]
[0131] Chemical Formula 3: A heteroaromatic ring compound represented by chemical formula (3)
[0132] Chemical Formula 4: A heteroaromatic ring compound represented by chemical formula (4)
[0133] Antioxidant: Antioxidant: Butylated reaction product of p-cresol and dicyclopentadiene, manufactured by Ouchi Shinko Chemical Industry Co., Ltd., Nocrac PBK
[0134] <Evaluation of Dip-Molded Articles> (Film Thickness) The thickness (film thickness) of the dip-molded film for evaluation was measured at three points in the center using a test piece thickness measuring instrument (manufactured by Kobunshi Keiki Co., Ltd., product name: ASKER SDA-12), and the smallest thickness was taken as the thickness of the dip-molded film for evaluation. The results are shown in Tables 1 to 3.
[0135] (Measurement of Tensile Properties) Using the dip-molded film for evaluation, the modulus at 100% elongation and the tensile strength at break were measured in accordance with JIS K 6251. The results are shown in Tables 1 to 3.
[0136] (Toluene Swelling Degree) The dip-molded film for evaluation was cut into a 10 mm x 15 mm piece to obtain a test piece. The mass W1 of the obtained test piece before immersion was measured, and the test piece was then immersed in toluene for 20 hours in an environment of 23°C. After immersion, the test piece was removed from the toluene, the toluene was wiped off the film surface, and the mass W2 after immersion was measured. The toluene swelling degree was calculated from the measured mass W1 before immersion and mass W2 after immersion using the following formula (1). The results are shown in Table 1. Formula (1): Toluene swelling degree = 1 + (W2 / W1-1)(P1 / P2)(1 / r), where P1 is the specific gravity of the chloroprene polymer component in the chloroprene polymer latex (A), P2 is the specific gravity of toluene, and r is the mass fraction of the chloroprene polymer component in the dip-molded product. The calculation was performed assuming P1 to be 1.23 and P2 to be 0.867. The chloroprene polymer content in the chloroprene polymer latex (A) can be obtained by mixing the chloroprene polymer latex (A) according to the Examples and Comparative Examples with methanol to precipitate the chloroprene polymer content, followed by filtration and drying. The specific gravity of the chloroprene polymer content in the chloroprene polymer latex (A) obtained by filtration and drying was calculated by measuring the density of the chloroprene polymer obtained by the above method at room temperature (20°C). The toluene swelling degree of Example 1 was 9.2, and the toluene swelling degree of Example 14 was 13.8.
[0137] A test specimen was obtained by cutting 3 g of the above-mentioned dip-molded film for evaluation into a 2 mm square. The test specimen was placed in a condenser-equipped eggplant-shaped flask, extracted with an ethanol / toluene azeotropic mixture (ETA solution) specified in JIS K 6229, and then treated with hydrochloric acid. Gas chromatography was performed under the following conditions using the extract. From the gas chromatography measurement results, the total amount RA of the peak areas of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid, and their salts was determined. In addition, the total amount RB of the peak areas of abietic acid, neoabietic acid, palustric acid, levopimaric acid, and their salts was determined, and the ratio RB / RA ((conjugated resin acid component b) / (non-conjugated resin acid component a)) of the total amount RB of the peak areas of abietic acid, neoabietic acid, palustric acid, levopimaric acid, and their salts to the total amount RA of the peak areas of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid, and their salts in the dip-molded film for evaluation was calculated.
[0138] [Gas chromatography measurement conditions] Column used: FFAP 0.32 mmφ×25 m (film thickness 0.3 μm) Detector: FID Column temperature: 200° C. (hold for 90 min) → 250° C. Heating rate: 10° C. / min Injection port temperature: 270° C. Detector temperature: 270° C. Injection volume: 2 μL
[0139]
[0140]
[0141]
Claims
1. A chloroprene polymer latex composition comprising a chloroprene polymer latex (A), a metal oxide (B), a vulcanization accelerator (C), sulfur (D), and a heteroaromatic ring compound (E), wherein a toluene insoluble portion of a chloroprene polymer rubber obtained by freeze-drying the chloroprene polymer latex (A) is 50 to 95 mass %, and the chloroprene polymer latex composition contains, relative to 100 mass parts of the solid content of the chloroprene polymer latex (A), 0.3 to 15.0 parts by mass of the metal oxide (B), 0.02 to 1.50 parts by mass of the vulcanization accelerator (C), 0.01 to 0.75 parts by mass of the sulfur (D), and 0.1 to 10.0 parts by mass of the heteroaromatic ring compound (E), The vulcanization accelerator (C) contains at least one of a thiuram-based, a dithiocarbamate-based, a thiourea-based, a guanidine-based, a xanthogenate-based, and a thiazole-based vulcanization accelerator, and the heteroaromatic ring compound (E) is represented by chemical formula (1). (X in the above chemical formula (1) represents a hydrogen atom or a metal atom. R 1 ~R 4 R represents a hydrogen atom, an alkyl group which may have a substituent, an ether group which may have a substituent, a nitro group, an amino group, or a carboxyl group. 1 ~R 4 may be the same or different.) 2. The chloroprene polymer latex composition according to claim 1, which contains 0.5 to 10.0 parts by mass of an antioxidant per 100 parts by mass of the solid content of the chloroprene polymer latex (A).
3. The chloroprene polymer latex composition according to claim 1 or 2, wherein a molecular weight distribution obtained by measuring a tetrahydrofuran soluble portion in the chloroprene polymer latex (A) by gel permeation chromatography has a peak at a weight average molecular weight of 5,000 to 80,000.
4. The chloroprene polymer latex composition according to claim 1 or 2, wherein the ratio RB / RA of the total amount RB of peak areas of abietic acid, neoabietic acid, palustric acid, levopimaric acid and their salts to the total amount RA of peak areas of dehydroabietic acid, pimaric acid, isopimaric acid, dihydroabietic acid and their salts obtained by gas chromatography analysis of an extract extracted from the immersion-coagulation-type immersion-molded body obtained by heating and drying at 140°C for 60 minutes with an ethanol / toluene azeotropic mixture as specified in JIS K 6229 is 0.10 or more.
5. The chloroprene polymer latex composition according to claim 1 or 2, wherein the chloroprene polymer latex composition is molded by a dipping coagulation method, and then heated and dried at 140°C for 60 minutes to obtain a dipping molded product, which has a modulus at 100% elongation of 0.65 MPa or less and a tensile strength at break of 19.0 MPa or more, as measured in accordance with JIS K 6251.
6. A dip-molded product of the chloroprene polymer latex composition according to claim 1 or 2.
7. The dip-molded article according to claim 6, which is an industrial or general household glove, a medical glove, a balloon, a catheter or a boot.