Liquid quick-setting agent and shotcrete

MYPI2025004751A0Undetermined Publication Date: 2024-08-08DENKA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
MYPI2025004751
Authority / Receiving Office
MY · MY
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-02-08
Filing Date
2024-02-06
Publication Date
2024-08-08

AI Technical Summary

Technical Problem

Conventional liquid quick-setting agents used in shotcrete have lower quick-setting properties compared to powder agents, leading to poor finish quality and uneven concrete surfaces.

Method used

A liquid quick-setting agent containing specific amounts of aluminum, sulfur, and silicon oxides, along with calcium, optimized for chemical composition and pH, is used in combination with a powder quick-setting agent containing calcium aluminate to enhance rapid setting, strength development, and finishing properties.

Benefits of technology

The solution provides excellent quick-setting properties, strength development, and improved finish quality, while ensuring worker safety and reducing environmental impact.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A liquid quick-setting agent containing aluminum, sulfur, and silicon in amounts of 2.5 to 21.0 mass%, 7.5 to 30.0 mass%, and 50 to 15,000 mass ppm in terms of oxide, respectively.
Need to check novelty before this filing date? Find Prior Art

Description

Liquid quick-setting agent, shotcrete

[0001] The present invention relates to a liquid quick-setting admixture and a shotcrete.

[0002] Conventionally, to prevent the collapse of exposed ground such as in tunnel excavation, a method of spraying quick-setting concrete, in which an accelerator is mixed into the concrete, has been used. In this method, materials are measured and mixed in a measuring plant installed at the excavation site to prepare the shotcrete, which is then pumped out and mixed with accelerator pumped in from the other side of the confluence pipe, and sprayed onto the ground surface until it reaches a specified thickness.

[0003] The quick-setting admixtures used in the spraying method can be broadly classified into two types: powder quick-setting admixtures whose main components are calcium aluminate or alkali metal aluminate, and liquid quick-setting admixtures whose main components are alkali metal aluminate or aluminum sulfate.

[0004] In recent years, from the perspective of ensuring the health of workers engaged in tunnel construction sites, etc., there has been a demand for the use of acidic liquid quick-setting admixtures whose main component is aluminum salt, which produce less dust when sprayed and are free from the risk of alkaline chemical burns.

[0005] On the other hand, liquid quick-setting admixtures have a problem in that they have lower quick-setting properties than powder quick-setting admixtures. To address this problem, measures have been taken to improve quick-setting properties by increasing the sulfate ion concentration, as shown in Patent Document 1, for example.

[0006] Furthermore, as a measure to improve strength, a liquid quick-setting admixture comprising aluminum fluoride, an acidic or basic solution of aluminum containing aluminum hydrofluoric acid as a component, lithium silicate, or lithium aluminate has been proposed, as in Patent Document 2. Alternatively, a liquid quick-setting admixture comprising a fluoride-containing water-soluble aluminum salt obtained by the reaction of aluminum sulfate with hydrofluoric acid, aluminum hydroxide, and lithium hydroxide, lithium carbonate, lithium sulfate, or the like has been proposed, as in Patent Document 3.

[0007] Japanese Patent Application Laid-Open No. 2006-193388 Japanese Patent Application Laid-Open No. 2001-130935 Japanese Patent Application Laid-Open No. 2005-89276

[0008] However, while the above-mentioned techniques improve strength characteristics, they have the problem that the concrete surface after spraying may become rough and uneven, resulting in poor finish.

[0009] In view of the above, an object of the present invention is to provide a liquid quick-setting admixture that has excellent quick-setting properties, strength development, and finish properties.

[0010] As a result of intensive research conducted by the present inventors in light of the above-mentioned problems, they found that a liquid quick-setting admixture containing specific amounts of aluminum, sulfur, and silicon calculated as oxides can solve the above-mentioned problems, and thus completed the present invention.

[0011] [1] A liquid quick-setting admixture containing aluminum, sulfur, and silicon in amounts of 2.5 to 21.0 mass%, 7.5 to 30.0 mass%, and 50 to 15,000 mass ppm, respectively, calculated as oxides. [2] The liquid quick-setting admixture according to [1] above, further containing calcium in an amount of 1 to 4,000 mass ppm, calculated as oxides. [3] The liquid quick-setting admixture according to [1] above, measured under the following conditions: 27 The liquid quick-setting admixture according to the above [1] or [2], which has a peak in the chemical shift range of 0 ppm to 2.0 ppm in a spectrum obtained by Al-NMR. (Conditions) Observation nucleus: 27 Al Sample tube rotation speed: 12 Hz Measurement temperature: 25°C Pulse width: 5 μsec (45° pulse) Waiting time: 5 seconds External standard: aluminum chloride aqueous solution [4] The liquid quick-setting admixture according to any one of the above [1] to [3], wherein the half-width of the peak in the chemical shift range of 0 ppm to 2.0 ppm is 2.0 ppm or less. [5] The mass ratio of the aluminum and the silicon in terms of their oxides (Al 2 O 3 / SiO 2 [6] The liquid quick-setting admixture according to any one of the above [1] to [4], wherein the pH is 4.0 or less. [7] Shotcrete, which is a combination of the liquid quick-setting admixture according to any one of the above [1] to [6] and a powder quick-setting admixture containing calcium aluminate as a main component.

[0012] According to the present invention, it is possible to provide a liquid quick-setting admixture that has excellent quick-setting properties, strength development, and finish properties.

[0013] Hereinafter, an embodiment of the present invention (the present embodiment) will be described in detail, but the present invention is not limited to this embodiment. In addition, "%" in this specification is based on mass unless otherwise specified.

[0014] [1. Liquid quick-setting admixture] The liquid quick-setting admixture according to this embodiment is a liquid quick-setting admixture containing aluminum, sulfur, and silicon in amounts of 2.5 to 21.0 mass%, 7.5 to 30.0 mass%, and 50 to 15,000 mass ppm, respectively, calculated as oxides.

[0015] The liquid quick-setting admixture contains aluminum in oxide equivalent (Al 2 O 3 The aluminum oxide-equivalent content in the liquid quick-setting admixture is 2.5 to 21.0 mass %, preferably 3.5 to 18.0 mass %, more preferably 4.5 to 15.0 mass %, and even more preferably 5.0 to 12.0 mass %. If the aluminum oxide-equivalent content in the liquid quick-setting admixture is less than 2.5 mass %, quick-setting properties may not be exhibited, whereas if it exceeds 21.0 mass %, strength development and finish may be poor.

[0016] The liquid quick-setting admixture contains sulfur in oxide equivalent (SO 3 The sulfur oxide-equivalent content in the liquid quick-setting admixture is 7.5 to 30.0 mass %, preferably 8.5 to 28.0 mass %, more preferably 12.0 to 27.0 mass %, and even more preferably 13.5 to 20.0 mass %. If the sulfur oxide-equivalent content in the liquid quick-setting admixture is less than 7.5 mass %, strength development may not be achieved, whereas if it exceeds 30.0 mass %, quick-setting properties and strength development may be poor.

[0017] Liquid quick-setting admixture contains silicon in oxide equivalent (SiO 2 The liquid quick-setting admixture contains 50 to 15,000 ppm by mass, preferably 150 to 9,000 ppm by mass, more preferably 500 to 7,000 ppm by mass, and even more preferably 1,000 to 5,000 ppm by mass, calculated as silicon oxide. If the amount of silicon oxide in the liquid quick-setting admixture is less than 50 ppm by mass or exceeds 15,000 ppm by mass, the finish may be poor.

[0018] The liquid quick-setting admixture further contains calcium, calculated as an oxide (CaO), in an amount of preferably 1 to 4,000 ppm by mass, more preferably 100 to 3,800 ppm by mass, and even more preferably 750 to 3,500 ppm by mass. When the amount of calcium calculated as an oxide in the liquid quick-setting admixture is within the above range, quick-setting properties, strength development, and finish are likely to be good.

[0019] The mass ratio of aluminum and silicon in the liquid quick-setting admixture in terms of oxide (Al 2 O 3 / SiO 2 ) is preferably 3 to 1,000, more preferably 5 to 500, and even more preferably 10 to 150. 2 O 3 / SiO 2 When the viscosity is within the above range, the quick setting property, strength development property, and finish property tend to be good.

[0020] Liquid Accelerator 27 In the spectrum obtained by Al-NMR, it is preferable that the spectrum has a peak in the chemical shift range of 0 ppm to 2.0 ppm. The half-value width of the peak is, for example, preferably 2.0 ppm or less, more preferably 1.8 ppm or less, and even more preferably 1.5 ppm or less. This can improve the storage stability of the quick-setting admixture. The half-value width may be, for example, 0.1 ppm or more.

[0021] Here, the liquid accelerator 27 The Al-NMR measurement can be performed using a commercially available measuring device, for example, a superconducting nuclear magnetic resonance device (ECX-400) manufactured by JEOL Ltd., under the following conditions: (Conditions) Observation nuclei: 27 Al Sample tube rotation speed: 12 Hz Measurement temperature: 25°C Pulse width: 5 μsec (45° pulse) Waiting time: 5 seconds External standard: aluminum chloride aqueous solution

[0022] The pH of the liquid quick-setting admixture is preferably 4.0 or less, and more preferably 3.5 or less. A pH of 4.0 or less can reduce the environmental load and suppress adverse effects on the human body. The pH is preferably 1.5 or more. The pH of the liquid quick-setting admixture can be measured using a pH meter.

[0023] From the viewpoint of reducing elution of fluoride ions, the fluoride ion concentration in the liquid quick-setting admixture is preferably 1.0 to 500 ppm, more preferably 1.0 to 450 ppm, and even more preferably 1.0 to 350 ppm. When the fluoride ion concentration is within the above range, false setting due to rapid hydration caused by the addition of the quick-setting admixture is easily alleviated, and good workability is easily obtained.

[0024] Total alkali content R in liquid quick-setting admixture 2 From the viewpoint of worker safety, the total alkali content R is preferably 1.0% by mass or less, more preferably 0.8% by mass or less, and even more preferably 0.5% by mass or less. In addition, the total alkali content R may be 0% by mass or more. 2 By using a raw material with a low concentration of O, the total alkali content R in the liquid quick-setting admixture 2 The total alkali content R in the liquid quick-setting admixture can be set within the above range. 2 O can be measured by atomic absorption spectrometry.

[0025] From the viewpoint of preventing steel corrosion, the chloride ion concentration in the liquid quick-setting admixture is preferably 5.0% by mass or less, more preferably 3.0% by mass or less, and even more preferably 2.0% by mass or less. When preparing the liquid quick-setting admixture, the chloride ion concentration in the liquid quick-setting admixture can be within the above range, for example, by using raw materials with a low chloride ion concentration. The chloride ion concentration in the liquid quick-setting admixture can be measured using a commercially available analyzer, for example, an ion chromatograph (ICS2100) manufactured by Thermo Scientific. For analysis, the measurement can be performed by diluting the liquid in advance so that the chloride ions are within the calibration curve.

[0026] Liquid quick-setting admixtures can be obtained by mixing aluminum-containing raw materials such as aluminum sulfate, aluminum hydroxide, various alums, ground granulated blast furnace slag, and aluminum dross ash, sulfur-containing raw materials such as sulfuric acid, and silicon-containing raw materials such as fly ash, silica fume, ground granulated blast furnace slag, amorphous silica, and aluminum dross ash, and then reacting them at high heat. Calcium-containing raw materials such as calcium oxide, calcium hydroxide, ground granulated blast furnace slag, and carbide slag can also be used. The heating temperature is preferably 70 to 100°C, more preferably 85 to 100°C, and even more preferably 85 to 95°C. The reaction time is preferably 30 to 150 minutes, more preferably 60 to 150 minutes, and even more preferably 90 to 120 minutes. For example, the liquid quick-setting admixture can be prepared by mixing aluminum hydroxide, sulfuric acid, and ground granulated blast furnace slag and heating at 85 to 95°C for 90 to 120 minutes. The liquid quick-setting admixture 27 The peak position and half-width in the spectrum obtained by Al-NMR are affected by the ratio of aluminum content, sulfur content, and silicon content of the raw materials. For example, in the ratio of aluminum content raw material to sulfur content raw material, if the ratio of aluminum content raw material is increased, the chemical shift is likely to fall within the desired range, and if the ratio of sulfur content raw material is increased, the half-width is likely to become smaller.

[0027] In addition to the components described above, the liquid quick-setting admixture may contain various additives within the range that does not impair the effects of the present invention. However, from the viewpoint of ease of handling, it is preferable that the liquid quick-setting admixture does not contain sodium aluminum dioxide.

[0028] [2. Shotcrete] The shotcrete according to this embodiment preferably uses a combination of the liquid quick-setting admixture of the present invention and a powder quick-setting admixture containing calcium aluminate as the main component.

[0029] In practice, cement is used in sprayed concrete, and examples of cement that can be used in this sprayed concrete include various types of Portland cement, such as normal, early strength, extra early strength, low heat, and medium heat; various mixed cements in which blast furnace slag, fly ash, or silica is mixed with these Portland cements; filler cements in which limestone powder or pulverized slowly cooled blast furnace slag powder is mixed; and environmentally friendly cements (ecocements) made from municipal waste incineration ash and sewage sludge incineration ash as raw materials.

[0030] Shotcrete actually uses aggregate, but the type of aggregate is not particularly limited; however, aggregates with low water absorption and high aggregate strength are preferred. The maximum size of the aggregate is not particularly limited as long as it can be sprayed. River sand, mountain sand, sea sand, lime sand, silica sand, etc. can be used as fine aggregate, and river gravel, mountain gravel, lime gravel, etc. can be used as coarse aggregate, and crushed sand and crushed stone can also be used.

[0031] The powder quick-setting admixture is preferably one containing calcium aluminate as the main component. By containing calcium aluminate as the main component, good quick-setting properties and improved strength development can be achieved. Here, "containing calcium aluminate as the main component" means that the content (by mass) of calcium aluminate is the highest among the quick-setting admixture components in the powder quick-setting admixture.

[0032] The calcium aluminate content in the powder quick-setting admixture is 30% or more, preferably 30 to 80%, and more preferably 45 to 60%. When it is 30% or more, good setting properties are easily obtained. When it is 80% or less, good long-term strength development is easily obtained.

[0033] Calcium aluminate is a compound of CaO and Al 2 O 3 It is a general term for compounds that have hydration activity and contain CaO and / or Al as the main components. 2 O 3or a compound in which a part of the above is replaced with an alkali metal oxide, an alkaline earth metal oxide, silicon oxide, titanium oxide, iron oxide, an alkali metal halide, an alkaline earth metal halide, an alkali metal sulfate, an alkaline earth metal sulfate, or the like, or a compound in which CaO and Al 2 O 3 It is a substance in which these are dissolved in small amounts as a solid solution in a substance mainly composed of these, and calcium aluminate may be either crystalline or amorphous.

[0034] Specific examples of crystalline materials include CaO, C, and Al. 2 O 3 A, R 2 O(Na 2 O.K. 2 O, Li 2 O) is R, then C 3 A and C, which is a solid solution of alkali metals 14 R.A. 5 , C.A., C. 12 A 7 Or C 11 A 7 CaF 2 , C 4 A.Fe 2 O 3 , and C 3 A 3 CaSO 4 Among these, amorphous calcium aluminate is preferred because of its quick setting property. In the case of amorphous calcium aluminate, the vitrification rate is preferably 80% or more.

[0035] Calcium aluminate CaO / Al 2 O 3 The molar ratio is not particularly limited, but in consideration of the very early and long-term strength development, the molar ratio is preferably 2.0 to 3.0, more preferably 2.1 to 2.8. A molar ratio of 2.0 or more can improve the very early setting properties, and a molar ratio of 3.0 or less makes it easier to obtain good long-term strength development.

[0036] Calcium aluminate can be obtained by combining CaO raw materials such as calcium carbonate and calcium hydroxide with Al raw materials such as bauxite. 2 O 3Examples of the method include heat treating the raw materials in a rotary kiln, an electric furnace, etc. Specifically, the raw materials are mixed in a predetermined ratio, heated and melted in an electric furnace, etc., and then quenched by contacting with compressed air or water. By adjusting the ratio of the raw materials, the above CaO / Al 2 O 3 The molar ratio can be adjusted, and the vitrification rate can be adjusted by the temperature during heating and melting and the cooling method.

[0037] The Blaine specific surface area of ​​calcium aluminate is 4,000 to 8,000 cm 2 / g, and 5,000 to 7,000 cm 2 / g. 2 / g, early strength development is easily achieved and the handleability of the mortar and / or concrete at the time of spraying can be improved. The Blaine specific surface area is measured based on the specific surface area test described in JIS R 5201:2015 "Physical Testing Methods for Cement."

[0038] The amount of liquid quick-setting admixture added to the shotcrete can be adjusted so that the aluminum content in the liquid quick-setting admixture is preferably 0.1 to 20 parts by mass per 100 parts by mass of cement in the shotcrete. The amount of powder quick-setting admixture added can be adjusted so that the calcium aluminate content in the powder quick-setting admixture is preferably 1 to 15 parts by mass per 100 parts by mass of cement. The amounts of liquid quick-setting admixture and powder quick-setting admixture added can be adjusted as described above depending on the required strength of the shotcrete, thereby improving the initial and long-term compressive strength of the shotcrete. Regarding the blending ratio of the liquid quick-setting admixture to the powder quick-setting admixture, for example, when the natural ground is in poor condition, adding a larger amount of powder quick-setting admixture can improve the early strength of the shotcrete, while when the natural ground is stable, the amounts of both quick-setting admixtures can be reduced.

[0039] The present invention will be explained in more detail below using examples and comparative examples, but the present invention is not limited to the following examples as long as it does not deviate from the gist of the invention.

[0040] [Experimental Example 1 (Experiment Nos. 1-1 to 1-19)] <Preparation of Liquid Quick-Set Admixture> The aluminum, sulfur, silicon, and calcium oxide equivalents were calculated as shown in Table 1 below. 2 O 3 Conversion, SO 3 Conversion, SiO 2 The various raw materials were adjusted and mixed so as to be equivalent to 1000 kJ / kg of sintered body and 1000 kJ / kg of CaO, and heated at 90° C. for 2 hours to prepare a liquid quick-setting admixture.

[0041] <Raw materials used> Aluminum raw material: aluminum hydroxide, industrial grade. Sulfur raw material: sulfuric acid, industrial grade. Silicon raw material: amorphous silica, industrial grade. Calcium raw material: hydrated lime, industrial grade. Solvent: pure water.

[0042] < 27 The prepared liquid quick-setting admixture was analyzed using a JEOL superconducting nuclear magnetic resonance spectrometer (ECX-400) under the following conditions to measure the chemical shift and half-width of the peak. The results are shown in Table 1 below.

[0043] < 27 Al-NMR measurement conditions> Observation nuclei: 27 Al Sample tube rotation speed: 12 Hz Measurement temperature: 25°C Pulse width: 5 μsec (45° pulse) Waiting time: 5 seconds External standard: aluminum chloride aqueous solution

[0044] <Concrete spraying test> Concrete prepared according to the mix conditions shown in Table 2 below was sprayed using a concrete pump "MKW-25SMT" (manufactured by Shintech Co., Ltd.) with a pump discharge setting of 10 m 3 / hr, and each liquid quick-setting admixture with the composition shown in Table 1 below was pumped in fixed amounts from a separate system just before spraying, and mixed with the concrete so that it accounted for 10 mass % of the cement in the concrete.Then, the concrete was sprayed onto each of the objects to be tested for setting property, compressive strength, and finished evaluation, as shown below.

[0045] <Materials used> Ordinary Portland cement: commercially available product, Blaine value 3,200 cm 2 / g Fine aggregate: Himekawa River water system sand, Itoigawa City, Niigata Prefecture, maximum size 5 mm or less, density 2.62 g / cm 3Coarse aggregate: Niigata Prefecture Itoigawa No. 6 crushed stone, maximum size 15 mm, density 2.67 g / cm 3 ・Water: Tap water. ・Water reducing agent: Commercially available, high-performance water reducing agent.

[0046] <Setting test> Concrete was sprayed into a wooden frame of 30 cm length x 30 cm width x 10 cm depth, and the Proctor penetration resistance value of the sprayed concrete was measured over time using a Proctor penetration tester (spring type). 2 The time when this occurs is called the starting time, or 28.0 N / mm 2 The time when this occurred was defined as the final setting time. The results are shown in Table 1 below.

[0047] <Compressive strength test (3 hours and 1 day old)> Compressive strength was measured at 3 hours and 1 day old in accordance with JSCE-G 561-2010 "Test method for early strength of shotcrete by pull-out method." The results are shown in Table 1 below.

[0048] <Finish evaluation and compressive strength test (28 days old)> Concrete was sprayed into a wooden frame measuring 30 cm long x 50 cm wide x 20 cm deep, and from the concrete sprayed at 28 days old, five φ100 x 200 mm specimens were cored so that they were lined up on a horizontal line passing through the center of the concrete in accordance with JIS A 1107:2022 "Method for extracting cores from concrete and compressive strength test method." The underside of each specimen was polished with a specimen edge finishing machine (manufactured by Marui Co., Ltd.), and the height of the specimen on a φ100 mm circumference centered on the center of the top surface of the five cored specimens was measured using a digital caliper (manufactured by Mitutoyo Co., Ltd.) with an accuracy of 1 / 100 mm. The height of the specimen on the circumference was measured at 6 points x 5 points every 60 °, for a total of 30 points, and the standard deviation of the height was calculated. If the standard deviation value was small, it was judged that the finish had small unevenness and was good. After the evaluation of the finish, the top surface of the specimen was polished and the compressive strength at 28 days was measured in accordance with JIS A 1107:2022 "Method for extracting cores from concrete and testing compressive strength" and JIS A 1132:2020 "Method for preparing specimens for strength tests of concrete."

[0049]

[0050]

[0051] The results shown in Table 1 confirm that liquid quick-setting admixtures containing specific amounts of aluminum, sulfur, and silicon, calculated as oxides, are excellent in quick-setting properties, strength development, and finish. Furthermore, it was confirmed that when the liquid quick-setting admixture further contains specific amounts of calcium, calculated as oxides, the quick-setting properties, strength development, and finish can be further improved.

[0052] [Experimental Example 2 (Experiment No. 2-1 to 2-3)] <Concrete spraying test> Immediately before spraying, calcium aluminate powder (CaO / Al 2 O 3 Molar ratio 2.3, Blaine value 6,000 cm 2 A concrete spraying test was carried out in the same manner as in Experimental Example 1, except that the liquid quick-setting admixture used in Experimental Example 1 was mixed together so that the concentration of the liquid quick-setting admixture was 5% by mass and 7% by mass, respectively, relative to the cement in the concrete, and various evaluations were carried out. The results are also shown in Table 1.

[0053] The results shown in Table 1 confirm that shotcrete made using a combination of a liquid quick-setting admixture and a powder quick-setting admixture mainly composed of calcium aluminate exhibits excellent quick-setting properties, strength development, and finish.

[0054] The liquid quick-setting admixture of the present invention can be suitably used for cement concrete to be sprayed onto exposed natural ground surfaces such as tunnels for roads, railways, and waterways, and slopes.

Claims

1. A liquid quick-setting admixture containing, in terms of oxide, 2.5 to 21.0 mass %, 7.5 to 30.0 mass %, and 50 to 15,000 mass ppm of aluminum, sulfur, and silicon, respectively.

2. The liquid quick-setting admixture according to claim 1, further comprising 1 to 4,000 ppm by mass of calcium calculated as oxide.

3. Measured under the following conditions: 27 The liquid quick-setting admixture according to claim 1 or 2, which has a peak in a chemical shift range of 0 ppm to 2.0 ppm in a spectrum obtained by Al-NMR. (Conditions) Observation nucleus: 27 Al Sample tube rotation speed: 12 Hz Measurement temperature: 25°C Pulse width: 5 μsec (45° pulse) Waiting time: 5 seconds External standard: Aluminum chloride aqueous solution 4. The liquid quick-setting admixture according to claim 1 or 2, wherein the half-width of the peak in the chemical shift range of 0 ppm to 2.0 ppm is 2.0 ppm or less.

5. The mass ratio of the aluminum and silicon in terms of their oxides (Al 2 O 3 / SiO 2 3. The liquid quick-setting admixture according to claim 1, wherein the molecular weight of the liquid quick-setting admixture is 3 to 1,000.

6. The liquid quick-setting admixture according to claim 1 or 2, having a pH of 4.0 or less.

7. A sprayed concrete comprising a liquid quick-setting admixture as set forth in claim 1 or 2 in combination with a powder quick-setting admixture containing calcium aluminate as a main component.