Method for manufacturing thermoplastic fiber-reinforced resin wheel
Patent Information
- Application Number
- MYPI2025004775
- Authority / Receiving Office
- MY · MY
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-02-08
- Filing Date
- 2024-01-22
- Publication Date
- 2024-08-08
AI Technical Summary
Current methods for manufacturing automobile wheels with integrated rim and disc portions using thermoplastic fiber-reinforced resin face challenges in achieving precise molding in a short time, balancing molding speed and product performance, and restricting rim width due to anisotropy issues and high forming loads.
A method combining deep drawing of sheet-like materials and compression molding of billet-like materials, where both are heated to a temperature higher than the resin's melting point and molded at a temperature lower than the melting point, allowing for the formation of wide rim sections with reduced anisotropy and forming loads, and integrated into a wheel in a short cycle time.
Enables the rapid production of wheels with good moldability and mechanical performance, allowing for wide rim portions and reducing the cycle time to minutes while maintaining mechanical strength by controlling the flow of reinforcing fibers.
Smart Images

Figure PI2025004775_DRAWING_001 
Figure PI2025004775_DRAWING_002 
Figure PI2025004775_DRAWING_003
Abstract
Description
Method for manufacturing thermoplastic fiber reinforced resin wheels
[0001] The present invention relates to a manufacturing method for molding an automobile wheel having an integrated rim portion and disk portion from a thermoplastic fiber reinforced resin.
[0002] Automobile wheels with an integrated rim and disc structure are generally formed by first aligning all or part of the material, i.e., fiber-reinforced plastics (e.g., FRP (Fiber Reinforced Plastics) or SMC (Sheet Molding Compound)) or a fiber-based material, along the inner surface of a mold. However, because a wheel is made up of an integrated rim and disc, which have different shapes and orientations, the multiple materials that make up at least these parts must be shaped differently and positioned in different positions.
[0003] The wheel disclosed in Patent Document 1 below is made of a thermosetting resin and is manufactured as follows: The material for the rim portion is a sheet-shaped molding compound (SMC) with a high resin content, which is formed into a cylindrical shape and held inside a rim-molding mold. The material for the disk portion is a sheet-shaped molding compound (SMC) with a high fiber volume fraction, which is placed between a lower mold and an upper mold that mold the disk portion. In this example, the cylindrical material for the rim portion is wrapped around the outer periphery of the material for the disk portion to form the resin material for processing.
[0004] The resin material to be processed is placed in a heated mold and then compression molded (heat and cool molding). After heating for a specified time, the resin matrix of the material solidifies through a chemical reaction, and then the material is cooled to complete the molding process.
[0005] Because the wheels are manufactured in this way, it takes time to properly position and shape the material inside the mold and for the resin to harden, making it impossible to complete the molding process in just a few minutes, including the preparation stage.
[0006] A technology for high-speed molding of sheet material made of thermoplastic fiber-reinforced resin rather than thermosetting fiber-reinforced resin is disclosed in the following non-patent document 1. This aims to shorten the cycle time while ensuring sufficient moldability, and employs a method in which the sheet material is heated to a temperature higher than the melting point of the resin matrix, and then sandwiched and molded in a mold set at a temperature lower than the melting point of the resin matrix. Manufacturing wheels from thermoplastic fiber-reinforced resin is disclosed in the following non-patent document 2. This uses thermoplastic fiber-reinforced resin, whose reinforcing fibers are chopped material, as the raw material, heated to a predetermined processing temperature, and then placed in a mold for compression molding.
[0007] In this method, a punch is pressed into the blank to compress and form the disk portion, while extruding a portion of the blank into a cylindrical shape to form the rim portion. Because the diameter of the rim portion increases as it extends upward, a larger volume of blank is required to ensure the required thickness. This requires the disk portion to have a larger volume than necessary. Furthermore, for wider rims, the punch must be pressed deeper and harder, dramatically increasing the forming load. Furthermore, because the rim portion is formed by extrusion, the reinforcing fibers tend to align in a specific direction. This increases anisotropy, preventing high strength, making it difficult to mold wheels with wide rims. In other words, even if the reinforcing fibers are isotropic in the blank before molding, their anisotropy increases as they flow upward into the rim, leading to axial strength variations and strength reduction. This imposes limitations on the width of the rim portion.
[0008] To reduce anisotropy, it is conceivable to slow down the molding speed to slow down the flow rate of the reinforcing fibers, but this would increase the molding time and also hinder moldability due to the rapid drop in resin temperature during molding. Thus, while the technology of Non-Patent Document 1 seems to enable molding in a short time with a single compression operation, it is difficult to balance molding speed and molded product performance to satisfy both, and there are also restrictions on the product shape.
[0009] In addition to the quick form molding as in Non-Patent Document 2, there is also a technique called HP-RTM (High Pressure Resin Transfer Molding) molding (for example, Patent Document 2).
[0010] In this molding method, for example, dry fiber substrates or fiber substrate laminates that have not been impregnated with resin are manually placed in a molding die and shaped. After the molding die is closed, the pressure inside the die is reduced and a thermosetting resin such as epoxy resin is injected under pressure to impregnate the fiber substrate. The die is then heated to harden the thermosetting resin. Multiple fiber substrates are prepared depending on the application area and manually placed, which has the advantage of ensuring the wheel's strength by increasing the number of layers in areas that need reinforcement.
[0011] However, the process of arranging and shaping the fiber substrate takes time, and a high level of know-how is required to obtain a uniform product.
[0012] As a result, the pre-molding process and molding require a considerable amount of time that cannot be measured in minutes, and the wheels produced in this way are very expensive and can only be used on certain special vehicles such as supercars.
[0013] Japanese Patent Publication No. 6-51308 Patent No. 6652523
[0014] Sachihiro Isogawa, Yoshio Enomoto, Hisao Kobayashi, Shougo Nasu, “High cycle deep drawing of PA6 matrix carbon fiber reinforced thermoplastics by servo-driven screw press,” “Procedia Manufacturing,” Available online August 11, 2018, Version of Record August 11, 2018., Volume 15, pp. 1722-1729. “Carbon Fiber Reinforced Plastic (CFRTP) Automobile Tire Wheels,” Rapit Co., Ltd., Product Catalog, [Retrieved October 3, 2022], Internet <URL: https: / / www.ipros.jp / catalog / detail / 498804>
[0015] The main object of this invention is to enable the manufacture of wheels made of thermoplastic fiber reinforced resin with good formability in a short time, while also ensuring mechanical performance and enabling the manufacture of wheels with wide rim portions.
[0016] The means for achieving this is a method for manufacturing a thermoplastic fiber reinforced resin wheel, in which a material made of thermoplastic fiber reinforced resin is molded in a mold to produce a wheel in which the rim portion and disc portion are integrated, the mold being set to a temperature lower than the melting point of the resin matrix which is a constituent element of the material, and the billet-shaped material and sheet-shaped material as the material are heated to a temperature higher than the melting point of the resin matrix which is a constituent element of those materials, and then the billet-shaped material is held in a mold surrounded by a disk outer surface mold and a rim outer diameter mold, while the sheet-shaped material is held on the surface of the rim outer diameter mold on the punch die side opposite to the disk outer surface mold and the outer periphery of the sheet-shaped material is pressed with a wrinkle suppression plate, the sheet-shaped material is deep drawn with the punch die and the rim outer diameter mold to form the rim portion of the wheel, while a part of the sheet-shaped material is pressed against the billet-shaped material to join them, and the billet-shaped material is compression molded with the disk outer surface mold, the rim outer diameter mold and the punch die to form the disc portion of the wheel.
[0017] In this configuration, the sheet-shaped material and billet-shaped material, which have different shapes, are plastically deformed in a manner that is minimally strained and matches their respective shapes, and are simultaneously joined and integrated with each other during plastic deformation. Deep drawing of the sheet-shaped material enables the formation of a wide rim portion, while compression molding of the billet-shaped material does not require the formation of a rim portion, eliminating the need for excessive volume or molding load. Furthermore, the sheet-shaped material and billet-shaped material are heated to a temperature higher than the melting point of the resin matrix, and as their temperature decreases, they are rapidly plastically deformed into the desired shape within a mold whose temperature is lower than the melting point of the resin matrix.
[0018] According to this invention, deep drawing of a sheet-like material and compression molding of a billet-like material are organically combined to smoothly form and integrate the rim and disc portions in a single operation, allowing the wheel to be formed in a very short time of minutes, with good formability. Furthermore, each material is formed in a relatively smooth manner that matches the shape of the material. This makes it easy to control the flow of the material during the formation of the rim and disc portions, and by preventing the reinforcing fibers from becoming excessively anisotropic, mechanical performance can be ensured. Furthermore, because the rim portion is formed by deep drawing of a sheet-like material, a wide rim portion can also be formed.
[0019] Schematic diagram of a method for manufacturing a thermoplastic fiber reinforced resin wheel. Front view of the wheel and its A-A cross section. Perspective view of a sheet-shaped material and a billet-shaped material. Plan view showing the structure of a continuous fiber laminated quasi-isotropic cross sheet. Half-sectional view of a billet-shaped material. Cross-sectional view showing the structure of a mold. Cross-sectional view of a material held in a mold. Cross-sectional view showing the molding process. Cross-sectional view of the molded state. Cross-sectional view showing a molding state for reinforcing the rim portion, as another example. Perspective views showing the state before and after molding of a material in which additional sheet-shaped material is laminated. Half-sectional view of a billet-shaped material with a reinforcing sheet, as another example. Plan view of a billet-shaped material with a reinforcing sheet. Cross-sectional view showing the molding state using a reinforcing sheet. Front view of a molded product with a reinforcing sheet. Front view of a wheel with a reinforcing sheet.
[0020] An embodiment of the present invention will be described below with reference to the drawings.
[0021] This invention is for manufacturing an automobile wheel (hereinafter referred to as "wheel") having an integrated rim portion and disk portion by molding, and uses a thermoplastic fiber reinforced resin as the molding material (intermediate substrate).
[0022] Thermoplastic fiber reinforced resins include SMC (Sheet Molding Compound), BMC (Bulk Molding Compound), also known as Forged Carbon Sheet or Forged Carbon Fiber Sheet, FRP (Fiber Reinforced Plastic) such as Carbon Fiber Reinforced Plastic, stampable sheets, etc., and are mainly composed of a resin matrix (base material) and reinforcing fibers (reinforcement material).
[0023] Figure 1 shows an outline of the main components of a method for manufacturing an automobile wheel. In this manufacturing method, a prepared material 11 is heated and then molded in a mold 31 to obtain a wheel-shaped molded product. The molded product is then removed from the mold 31 and subjected to post-processing such as cutting to obtain an intermediate wheel product 71 (hereinafter also referred to as "wheel 71") as shown in Figure 2.
[0024] First, the material 11 will be described.
[0025] The material 11 is used in two shapes as shown in Fig. 3. One is a sheet shape, and the other is a billet or bulk shape.
[0026] The sheet-like material 11 (sheet-like material 11a) mainly constitutes the rim portion 72 of the wheel 71, and has a thickness equal to or greater than that of the rim portion 72, and is formed in a disk shape that expands in the surface direction. A through-hole 12 that penetrates through in the thickness direction is formed in the center of the surface. The material is formed by deep drawing. The through-hole 12 may have a circular shape as shown in the example.
[0027] The sheet material 11a may be made of a single sheet material, or may be made of a plurality of stacked sheets.
[0028] The billet-shaped or bulk-shaped material 11 (billet-shaped material 11b) mainly constitutes the disk portion 73 of the wheel 71, and is a lump of a size suitable for compression molding, or a shape of a predetermined size, volume, and bulk. Specifically, it has a predetermined thickness and a predetermined diameter to fit the cavity of the mold, and is formed into a short cylindrical shape with a through-hole 13 in the center. It is compression molded during molding. This through-hole 13 may also have a circular shape as in the illustrated example, or may have any other shape.
[0029] The reinforcing fibers 14 of the raw material 11 can be made of chopped material (chopped fiber), chopped sheets, continuous fiber cloth (woven) sheets, etc., with carbon fiber or glass fiber being preferred. In particular, for the sheet-like raw material 11a, although chopped material or chopped sheets can be used, it is preferable to use continuous fibers as the reinforcing fibers 14. A continuous fiber cross sheet is more preferable. Considering shear deformation and fiber misalignment of the woven fabric during deep drawing, as shown in Figure 4, it is preferable to use a continuous fiber laminated quasi-isotropic cross sheet 15, in which the directionality of continuous fiber cross sheets 14a is changed by a certain angle α while being stacked, to improve strength and deformation isotropy. In the example of Figure 4, the continuous fiber laminated quasi-isotropic cross sheet 15 is formed by stacking the required number of continuous fiber cross sheets 14a, each consisting of warp and weft threads, while rotating them by 22.5 degrees at a time.
[0030] Taking into consideration formability during compression molding, the billet-shaped material 11b is made quasi-isotropic and has chopped material (chopped fiber) or chopped sheet as the reinforcing fibers 14. Considering the rigidity of the molded product in addition to formability, it is more desirable to form the billet-shaped material 11b by stacking multiple SMC 16 sheets, which are quasi-isotropic random sheet materials having chopped sheet as the reinforcing fibers 14, in the thickness direction as shown in Fig. 5. The thickness direction of the SMC 16 is the compression direction during compression molding.
[0031] The resin matrices of the sheet material 11a and the billet material 11b may be any resin that is compatible with each other and can be mixed with each other, and generally the same resin is used, such as a thermoplastic epoxy resin or polyamide.
[0032] Next, the apparatus used in the manufacturing method will be described.
[0033] The manufacturing method involves heating the billet-shaped material 11b and the sheet-shaped material 11a to a temperature higher than the melting point of the resin matrix that constitutes them, and then molding them at high speed in a mold 31 that is set to a temperature lower than the melting point of the resin matrix.
[0034] 1, the apparatus includes not only a mold 31 for forming but also heating devices 51 and 52 for heating the sheet-shaped material 11a and the billet-shaped material 11b. The heating devices 51 and 52 may be of any suitable heating type, but from the viewpoint of achieving ideal heating without uneven heating inside and outside in a short time, it is preferable to use an IR (infrared) heating type.
[0035] The heating device 51 that heats the sheet material 11a has heaters 53 on the top and bottom, and has an inlet 54 that serves as an entrance to the conveyance path between the heaters 53, and an outlet 55 that serves as an exit. The sheet material 11a is conveyed from inlet to outlet by an automatic conveyance device.
[0036] The heating device 52 that heats the billet-shaped material 11b is the same as the heating device 51 that heats the sheet-shaped material 11a. A plurality of sheet materials (SMC16) that will form a billet when stacked are heated while being conveyed. A heat-retaining pot 56 is provided downstream of the heating device 52. The heat-retaining pot 56 contains the billet-shaped material 11b, which is made by stacking the sheet materials (SMC16), and ensures uniform heating.
[0037] The heating temperature of the sheet-shaped material 11a and the billet-shaped material 11b is higher than the melting point of their resin matrix. If the resin matrix is, for example, polyamide, it is recommended to heat it to about 280°C. This temperature takes into consideration the temperature drop during molding, and is about 30°C to 70°C higher than the melting point.
[0038] The mold 31 used for molding is composed of a disk outer surface mold 32, a rim outer diameter mold 33, and a punch mold 34. The disk outer surface mold 32 is a lower mold that mainly molds the outer surface of the disk portion 73 of the wheel 71. The rim outer diameter mold 33 moves radially on the top surface of the disk outer surface mold 32 to form the outer peripheral surface of the rim portion 72 of the wheel 71, and is divided into multiple parts in the circumferential direction. The punch mold 34 is an upper mold that mainly forms the inner peripheral surface of the rim portion 72 and the inner surface of the disk portion 73, and is supported on the rim outer diameter mold 33 from the side opposite the disk outer surface mold 32 so that it can move up and down toward the disk outer surface mold 32.
[0039] A wrinkle suppression plate 35 that moves up and down similarly to the punch die 34 is provided above the rim outer diameter die 33 when it is closed. The wrinkle suppression plate 35 presses down on the outer periphery of the sheet material 11a placed on the upper surface of the rim outer diameter die 33 while allowing it to be pulled in, thereby preventing wrinkles from occurring in the sheet material 11a during deep drawing.
[0040] The structure of the mold 31 will now be described. Wheels 71 come in a variety of shapes, including whether the outer surface of the disk is convex, flat, or concave, as in the case of inset, zero set, or outset, depending on the distance from the center line of the wheel (rim width) to the mounting surface. The mold 31 also comes in a variety of shapes depending on the wheel shape, and the mold 31 shown in the illustration is one example. The manufacturing method of the present invention is not limited to the illustrated shape.
[0041] 1 and 6, the disk outer diameter mold 32 is roughly flat and has a vertically upwardly facing shaft portion 36 formed in the center. The shaft portion 36 is located in a position corresponding to the center bore 74 of the wheel 71, and the entire circumference of the shaft portion 36 has an undulating surface 37 that corresponds to the outer surface of the disk portion 73. The portion further outward from this is a support surface 38 that supports the rim outer diameter mold 33.
[0042] The tip end of the shank 36 is a fitting portion 36a that fits into the punch die 34, and is formed as the thinnest portion of the shank 36. A large diameter portion 36c is formed below the fitting portion 36a, with a step portion 36b interposed between them. The diameter of the large diameter portion 36c is smaller than the diameter of the through hole 13 in the billet-shaped material 11b. The large diameter portion 36c has a base portion, i.e., a sloped portion 36d at the bottom outer periphery, that has a diameter that increases downward like a mountain foot. The diameter of the sloped portion 36d at its bottom end is larger than the diameter of the through hole 13 in the billet-shaped material 11b.
[0043] The rim outer diameter mold 33 has a recess 39 at its lower end which forms the portion where the outer flange 75 of the wheel 71 and the outer portion of the tire are assembled. Above the recess 39, an uneven portion 41 which flows in and out along the shape of the rim portion 72 is formed, and at the upper end above the portion 41a which forms the inner flange 76 of the wheel 71, a rounded corner portion 42 is formed.
[0044] The wrinkle suppressor plate 35 is a plate-like plate that presses down on the upper surface of the rim outer diameter mold 33, that is, the outer peripheral portion of the rounded corner portion 42, and is formed in an annular shape as a whole.
[0045] The punch die 34 has a fitting recess 43 in the centre of its underside that fits with the fitting portion 36a of the shaft portion 36 of the disc outer surface die 32. It also has an outer peripheral surface 44 shaped to fit inside the rim outer diameter die 33 in the closed state, with a corner gap corresponding to the thickness of the rim portion 72. Of the outer peripheral surface 44, the portion 44a that forms the inner flange 76 of the wheel 71 is particularly shaped so as to form a molding space of the desired shape that takes mechanical performance into consideration between it and the corresponding portion of the rim outer diameter die 33.
[0046] The depth of the fitting recess 43 is set so that a gap d1 is formed between the bottom of the fitting recess 43 and the tip of the shank 36 even when the punch 34 is at the bottom dead center. The dimensions of the periphery of the shank 36 are also designed so that an escape portion 45 that will not reach the billet material 11b when the punch 34 reaches the bottom dead center is formed near the rim of the fitting recess 43.
[0047] The portion outer than the fitting recess 43 is an annular recess 46 that forms the portion outer than the center bore 74 of the wheel 71, and the portion further outer than that is an overhang 47 that forms the spokes 77 of the wheel 71 and the portions corresponding to the window portions 78 between the spokes 77. The overhang 47 protrudes downward from the annular recess 46. The portion of the overhang 47 that corresponds to the window portions 78 is formed so that its thickness after molding is thin between the undulating surface 37 of the disk outer surface mold 32.
[0048] Such a mold 31 is equipped with a temperature control mechanism (not shown) that controls the temperature of the mold 31 to a constant value. The temperature control mechanism is configured with a flow path for flowing a medium such as water, and is configured to maintain a predetermined temperature by monitoring and adjusting the medium flow rate and temperature. The temperature control mechanism can also be configured by inserting a cartridge heater into the mold 31.
[0049] The temperature of the mold 31 is lower than the melting point of the resin matrix of the sheet-shaped material 11a and the billet-shaped material 11b, and preferably lower than the glass transition temperature. When the resin matrix is a thermoplastic epoxy resin, the temperature is specifically 100°C to 130°C, particularly 120°C or lower, and may be 80°C or lower, or around 50°C. As long as the temperature is above a certain required temperature, a lower temperature is preferable because it can suppress adhesion of the resin matrix to the mold 31 and shorten the holding time, thereby shortening the cycle time.
[0050] The above-described apparatus manufactures the wheel 71 by forming the sheet material 11a and the billet material 11b as follows.
[0051] The mold 31 is kept closed and its temperature is set to a predetermined temperature lower than the melting point of the resin matrix of the material.
[0052] While these preparations are being made, a thermoplastic fiber reinforced resin is cut using a water jet or the like to prepare the sheet material 11a and the sheet material (SMC16) for forming the billet material 11b. These are heated to a predetermined temperature using heating devices 51 and 52, and the heated sheet material (SMC16) for the billet material 11b is stacked and heated uniformly in a heat-retaining pot 56.
[0053] 7, the punch die 34 is raised to open the die 31, and the billet-shaped material 11b is introduced into the die 31. At this time, the shaft portion 36 and the inclined portion 36d of the disk outer surface die 32 align the center of the billet-shaped material 11b with the center of the disk outer surface die 32.
[0054] Immediately after this, the sheet material 11a is placed on the upper surface of the rim outer diameter mold 33, and the wrinkle suppression plate 35 is lowered to press down the outer periphery of the sheet material 11a. This wrinkle suppression plate 35 is heated and kept at a temperature lower than that of the sheet material.
[0055] At this time, since the temperature of the mold 31 is lower than the heating temperature of the sheet-like material 11a and the billet-like material 11b, the temperatures of the sheet-like material 11a and the billet-like material 11b, which decrease in temperature as they leave the heating device 51 and the thermal insulation pot 56, decrease further.
[0056] High-speed forming can be achieved by lowering the punch 34 as shown in Figure 8 immediately after the sheet-like material 11a and billet-like material 11b are set in the die 31. That is, as the punch 34 descends, the lower end of its protruding portion 47 first comes into contact with the upper surface of the sheet-like material 11a and presses down the abutting portion. As the punch 34 descends, the sheet-like material 11a is deep-drawn while being drawn into the die 31, and a rim portion 72 is gradually formed along the rim outer diameter die 33 and the punch 34. At this time, the rim portion 72 cools and solidifies.
[0057] The inner peripheral portion of the sheet material 11a pressed down by the lower end of the overhanging portion 47 comes into contact with the upper surface of the billet material 11b from above and is pressed against the billet material 11b by the punch 34. As a result, the sheet material 11a and the billet material 11b are joined together and continue to deform, and when the punch 34 reaches the bottom dead center, the desired forming of the sheet material 11a and the billet material 11b is completed as shown in FIG.
[0058] At this time, the tip of the shaft portion 36 of the disk outer surface die 32 does not come into contact with the bottom of the fitting recess 43 of the punch die 34, and a space that the compression-molded billet-shaped material 11b does not reach, i.e., an escape portion 45, is formed near the edge of the fitting recess 43. Therefore, although the molding load increases especially after the sheet-shaped material 11a comes into contact with the billet-shaped material 11b, an extreme increase in the molding load can be avoided.
[0059] Molding using such a mold 31 can be completed in less than one minute, even if the molded product is held at bottom dead center for 15 seconds, depending on the size of the molded product. Moreover, holding the material 11 in the mold 31 can be done easily and quickly, unlike operations that require precise placement of many materials. Therefore, the molding process, including removal of the molded product, can be completed in less than one minute.
[0060] The molded product removed from the mold 31 is cooled by leaving it to stand at room temperature, and then post-processing is performed, such as cutting out excess parts such as the part that protrudes beyond the inner flange 76 and the window part 78, to form the wheel 71 (see Figure 2).
[0061] As described above, in the molding process using the mold 31, the sheet material 11a is deep-drawn, and the billet material 11b is compression-molded, and they are joined together during the molding process. Moreover, the sheet material 11a is formed into a cylindrical shape by pressing down on the inner peripheral portion, so the desired rim portion 72 can be obtained without difficulty, and the rim portion 72 can also be made wider. With the billet material 11b, only the disk portion 73 is formed, and there is no need to form the rim portion 72, so excessive volume and molding load are not required. As for the molding load, the provision of the relief portion 45 reliably prevents a sudden increase in the molding load.
[0062] This type of molding is essentially an organic combination of deep drawing of the sheet material 11a and compression molding of the billet material 11b, smoothly molding and joining the rim portion 72 and disc portion 73 in a single operation. This allows the wheel 71 to be molded in a very short time, on the order of minutes, with good moldability. Furthermore, since molding is performed in a manner that matches the respective shapes of the sheet material 11a and billet material 11b with minimal strain, the flow of the materials during molding is easily controlled. By preventing the reinforcing fibers 14 from excessively increasing anisotropy, the mechanical performance of the wheel can be ensured.
[0063] Furthermore, since there is no excessive deformation during molding and the flow of the material is easily controlled, it is possible to reinforce parts, etc., thereby obtaining sufficient mechanical properties.
[0064] For example, in molding, in order to make the thickness of the portion of the rim portion 72 corresponding to the inner flange 76 thicker than other portions of the rim portion 72 and to improve the strength, the following procedure is carried out.
[0065] That is, as shown in Figure 10, an additional sheet material 11c is used, which is laminated to a portion of the sheet material 11a. Depending on the purpose, the additional sheet material 11c can be one having chopped material as reinforcing fibers, a continuous fiber cross sheet 14a, or a continuous fiber laminated quasi-isotropic cross sheet 15. To increase strength, it is better to use a fiber-reinforced resin sheet having a continuous fiber cross sheet as the additional sheet material 11c. Note that for convenience, the illustration of the wrinkle suppression plate 35 is omitted in Figure 10.
[0066] The additional sheet material 11c is formed in a circular ring shape of an appropriate width. Its stacking position is set at a position on the top surface of the sheet material 11a where, due to deformation during deep drawing, it should move to a portion where thickness, rigidity, or strength should be increased after forming compared to other portions, such as the portion 41a that forms the inner flange 76. The additional sheet material 11c can be stacked on the sheet material 11a not only on the top surface, but also inside the sheet material 11a, i.e., between the sheets that make up the sheet material 11a, or on the bottom surface of the sheet material 11a.
[0067] When molding is performed using this sheet material 11a, the laminated additional sheet material 11c is deep-drawn while being pulled in integrally with the sheet material 11a, and reaches the portion 41a that forms the inner flange 76. It then flows as shown by the arrows and is molded into the desired final shape with a thick wall. Therefore, even if the inner flange 76 portion is thicker than the other portions, it can be molded sufficiently, and if the additional sheet material 11c has a continuous fiber cross sheet, the laminated sheet materials 11a, 11c can be used to improve rigidity and strength.
[0068] Another example of the additional sheet material 11c is shown in Figure 11. This additional sheet material 11c is intended to reduce the change in fiber orientation during deep drawing and improve strength in the circumferential and width directions.
[0069] That is, the additional sheet material 11c is a sheet material having a continuous fiber cross sheet as a reinforcing fiber, and a notch 23 that widens toward the outer periphery is formed at a position at 45 degrees to the longitudinal and transverse directions in which the fibers extend in a peripheral edge portion 22 surrounding the central portion 21. The contour lines 24 that form the notch 23 are shaped to join together during deep drawing.
[0070] Specifically, the additional sheet material 11c is formed to a size that fits into the disk-shaped sheet material 11a, and its shape roughly resembles open petals. In other words, the additional sheet material 11c has notches 23 formed at equal intervals around the periphery of the disk, and has petal-like portions 25 divided by the notches 23. A through-hole 26 similar to the through-hole 12 in the sheet material 11a is formed in the center.
[0071] The notches 23 in the peripheral edge portion 22 are roughly fan-shaped, with two contour lines that radiate outward from a position near the center portion 21 where the corners of the fan are located. If the warp and weft directions in which the fibers extend are considered to be east, west, north, and south, the arrangement of the notches 23 of this shape is between these positions, i.e., northeast, southeast, southwest, and northwest. The two opposing contour lines 24 that form the four notches 23 are formed in accordance with the shape of the rim so that they will join together, that is, butt or overlap each other, during deep drawing.
[0072] When this additional sheet material 11c is layered on top of the sheet material 11a and molded, the layered additional sheet material 11c is deep-drawn while being pulled together with the sheet material 11a. At this time, the petal-shaped portions 25 of the additional sheet material 11c that were separated by the notches 23 approach each other, and the outlines 24 are joined together. This joint is pressed down by the surrounding material to ensure strength. In Figure 11, 27 is the joint line where the outlines 24 are joined together.
[0073] The fibers of the continuous fiber cross sheet as reinforcing fibers constituting the additional sheet-like material 11c extend in the circumferential and width directions, improving strength in those directions. During deep drawing, the petal-shaped portions 25 are deformed by folding along the rim outer diameter mold 33, so the crossing angle of the fibers of the continuous fiber cross sheet hardly changes. This results in high strength.
[0074] Even in the molding of the disk portion 73, since there is no complicated or excessive deformation, the flow of the billet-shaped material 11b is easy to control, and sufficient mechanical performance can be partially ensured.
[0075] For example, when reinforcing the area between the spokes 77 of the disk portion 73 and the outer flange 75 during molding, the following procedure is carried out.
[0076] That is, when the billet-shaped material 11b is formed by laminating a plurality of SMC 16 sheets, which are quasi-isotropic random sheet materials having chopped sheets as the reinforcing fibers 14, in the thickness direction, a reinforcing sheet 17 is provided between the SMC 16 sheets, as shown in Fig. 12. The reinforcing sheet 17 may be formed of a continuous fiber cross sheet. Alternatively, a braided sheet (quasi-isotropic fabric) such as "QISO" (registered trademark) by A&P Technology may be used as the reinforcing fiber.
[0077] The reinforcing sheet 17 has the same thickness as the SMC 16 and is sandwiched between the SMC 16 .
[0078] This reinforcing sheet 17 moves in the outer circumferential direction as the billet-shaped material 11b is deformed during compression molding, and to enable this movement, it is located on the outer circumferential side of the billet-shaped material 11b and is divided in the circumferential direction.
[0079] FIG. 12(a) shows an example in which the reinforcing sheet 17 is provided on the outer surface side of the disk portion 73, and FIG. 12(b) shows an example in which the reinforcing sheet 17 is provided on both the outer surface side and the inner surface side.
[0080] Specifically, as shown in Figure 13, the reinforcing sheets 17 of the billet-shaped material 11b are formed in an approximately fan shape, with multiple reinforcing sheets 17 arranged at equal intervals to match the number of spokes 77. When the billet-shaped material 11b is placed in the mold 31, the circumferential direction is determined so that the spokes 77 are formed in the portion having the reinforcing sheets 17. This can be easily achieved by providing a regulating structure between the shaft 36 and the through-holes 13 of the billet-shaped material 11b, since the disk outer surface mold 32 has a shaft 36.
[0081] Then, when forming is performed, as shown in Figure 14, when the billet-shaped material 11b is compressed and deformed to expand in the outer and inner circumferential directions, the reinforcing sheet 17 moves in the outer circumferential direction and becomes positioned between the outer flange 75 and the outer peripheral end of the spoke 77. Note that Figure 14 illustrates an example in which the billet-shaped material 11b shown in Figure 12(a) has been formed.
[0082] Figure 15 shows a front view of molded product 18. In post-processing of molded product 18, the portion corresponding to window portion 78, including reinforcing sheet 17, is cut to open window portion 78. As a result, as shown in Figure 16, reinforcing sheet 17, which is T-shaped when viewed from the front, remains connecting outer flange 75 and spoke 77, improving the strength of this portion.
[0083] The above configuration is one embodiment for carrying out the present invention, and the present invention is not limited to only the above configuration, and other configurations can also be adopted.
[0084] For example, in order to build up or reinforce a portion of the rim portion 72, the additional sheet material 11c may not be annular as described above, but may be discontinuous in the circumferential direction to provide partial reinforcement. Strength can be increased by using an additional sheet material 11c that extends elongatedly in the rim width direction after molding. The additional sheet material 11c may also have a shape that combines a discontinuous portion in the circumferential direction with a continuous portion in the circumferential direction.
[0085] The billet-shaped material 11b may be provided with a reinforcing sheet (not shown) that is not intended to move during molding. The reinforcing sheet may be a continuous fiber cross sheet 14a or a continuous fiber laminated quasi-isotropic cross sheet 15. In this case, since the reinforcing sheet is not intended to move, it may be formed into a circumferentially continuous annular shape.
[0086] In the above example, the sheet material 11a was disk-shaped, but the sheet material 11a may have other shapes. For example, similar to the additional sheet material 11c illustrated in FIG. 11, the sheet material 11a may have a shape with notches having outlines that join the sheets together during deep drawing, i.e., a shape resembling open petals. When using a sheet material 11a having such a shape, the additional sheet material 11c can be omitted. Also, in this case, similar to the continuous fiber laminated quasi-isotropic cloth sheet 15 illustrated in FIG. 4, it is preferable to stack multiple sheets of the open-petal-shaped sheet material with their orientations offset by a certain angle, or 45 degrees in the case of the sheet material illustrated in FIG. 11, from the viewpoint of strengthening the joints.
[0087] DESCRIPTION OF SYMBOLS 11...Material 11a...Sheet-shaped material 11b...Billet-shaped material 11c...Additional sheet-shaped material 13...Through-hole 14...Reinforcing fiber 14a...Continuous cross sheet 15...Continuous fiber laminated cross sheet 16...SMC 17...Reinforcing sheet 31...Mold 32...Disc outer surface mold 33...Rim outer diameter mold 34...Punch mold 35...Wrinkle suppression plate 36...Shaft portion 71...Wheel intermediate product 72...Rim portion 73...Disc portion
Claims
1. A method for manufacturing a thermoplastic fiber reinforced resin wheel, in which a material made of thermoplastic fiber reinforced resin is molded in a mold to produce a wheel having an integrated rim portion and disk portion, comprising the steps of: setting the mold to a temperature lower than the melting point of the resin matrix which is a constituent element of the material; heating the billet-like material and sheet-like material as the material to a temperature higher than the melting point of the resin matrix which is a constituent element of the material; holding the billet-like material in a mold surrounded by a disk outer surface mold and a rim outer diameter mold; holding the sheet-like material on the surface of the rim outer diameter mold on the punch die side opposite to the disk outer surface mold and holding the outer periphery of the sheet-like material with a wrinkle suppression plate; deep drawing the sheet-like material with the punch die and the rim outer diameter mold to form the rim portion of the wheel, while pressing a part of the sheet-like material against the billet-like material to join them, and compression molding the billet-like material with the disk outer surface mold, the rim outer diameter mold, and the punch die to form the disk portion of the wheel.
2. The method for manufacturing a thermoplastic fiber reinforced resin wheel as set forth in claim 1, wherein the billet-shaped material has a through hole in the center, and the through hole is inserted into and held in place by a shaft provided in the center of the disk outer surface mold.
3. A method for manufacturing a thermoplastic fiber reinforced resin wheel according to claim 1 or 2, wherein the sheet material is a sheet material having a continuous fiber cross sheet as reinforcing fiber.
4. A method for manufacturing a thermoplastic fiber reinforced resin wheel according to claim 1 or 2, wherein the sheet material is a sheet material having continuous fiber laminated quasi-isotropic cloth sheets as reinforcing fibers.
5. A method for manufacturing a thermoplastic fiber reinforced resin wheel according to claim 1 or 2, wherein the sheet material has chopped material as reinforcing fibers.
6. A method for manufacturing a thermoplastic fiber reinforced resin wheel as described in claim 1 or claim 2, wherein the sheet material is a material in which an additional sheet material made of thermoplastic fiber reinforced resin is laminated to a portion thereof, and the lamination position of the additional sheet material is set to a position where, due to deformation during deep drawing, the additional sheet material will move to a portion where thickness, rigidity or strength should be increased compared to other portions after molding.
7. A method for manufacturing a thermoplastic fiber reinforced resin wheel as set forth in claim 6, wherein the additional sheet material is a sheet material having a continuous fiber cross sheet as a reinforcing fiber, and a notch that widens toward the outer periphery is formed at a position at 45 degrees to the vertical and horizontal directions in which the fibers extend in the peripheral portion surrounding the center of the additional sheet material, and the contour lines forming the notch are shaped to join together during the deep drawing molding.
8. A method for manufacturing a thermoplastic fiber reinforced resin wheel as described in claim 1 or claim 2, in which the billet-shaped material is made by stacking multiple sheet materials having chopped sheets as reinforcing fibers in the direction of compression by the punch die.
9. The method for manufacturing a thermoplastic fiber reinforced resin wheel according to claim 8, further comprising providing a reinforcing sheet made of a continuous fiber cross sheet between the sheet materials, and moving the reinforcing sheet in the outer circumferential direction during compression molding.